Capacitive deionization selective adsorption electrode and preparation method thereof
By preparing a capacitive deionization selective adsorption electrode, using cross-linking treatment and Ti3C2Tx and other materials, the problem of high calcium and magnesium ion removal costs and pollution in the existing technology has been solved, and high-efficiency, low-energy consumption calcium and magnesium ion adsorption effects have been achieved. , suitable for seawater desalination and hard water softening.
Patent Information
- Application Number
- CN202110764500.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-06
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-07-06
AI Technical Summary
Existing capacitive deionization technology is costly and produces secondary pollution when removing calcium and magnesium ions, and lacks a selective removal method with high efficiency and low energy consumption.
A method of preparing a capacitive deionization selective adsorption electrode is used, by cross-linking chitosan, polyvinyl alcohol and glutaraldehyde in a glacial acetic acid solution, combining Ti3C2Tx, conductive carbon black and polyvinyl alcohol, and scraping onto graphite Selective adsorption electrodes are prepared on paper to achieve highly selective adsorption of calcium and magnesium ions.
It realizes the selective removal of calcium and magnesium ions with high efficiency and low energy consumption, reduces the preparation cost, is suitable for seawater desalination and hard water softening, has no secondary pollution, and is suitable for industrial production.
Smart Images

Figure BDA0003150605480000041
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wastewater treatment, and in particular to a capacitive deionization selective adsorption electrode and a preparation method thereof. Background Art
[0002] In recent years, with the development of supercapacitor materials, capacitive deionization technology has attracted more and more attention due to its many advantages such as low energy consumption, high efficiency, low operating cost and environmental friendliness. Capacitive deionization technology uses a pair of parallel porous carbon electrodes. After applying a DC voltage, the ions in the solution will be adsorbed onto the plates with opposite voltage and stored in the pores inside the porous carbon material. When adsorption saturation is reached, the ions will be released from the electrodes by removing or reversing the voltage, and the electrodes will restore their initial ion absorption capacity. Under a specific voltage, there is no chemical reaction in the capacitive deionization process. It is a purely physical process, and no chemical agents are required. There is no secondary pollution, which is conducive to the long-term use of the equipment and reduces maintenance costs.
[0003] Because capacitive deionization technology removes a small number of salt ion compounds in water from a mixed solution, while other methods extract the majority phase (water) of the mixture from the salt solution, capacitive deionization technology has high energy efficiency for low-salinity or medium-salinity seawater with a salt concentration below 10g / L, and has been tried in the fields of brackish water desalination and hard water softening.
[0004] Calcium and magnesium ions in water affect human health, the efficiency of detergents, and the heating efficiency and safety of boilers and heat exchangers. When industrial wastewater is treated with high-salt wastewater, membrane technology is generally used, and the presence of calcium and magnesium ions can easily lead to scaling on the surface of the separation membrane. Therefore, selective removal of calcium and magnesium ions has a wide range of application scenarios.
[0005] The performance of the adsorption electrode is the key parameter that determines the performance of the electrode in capacitive deionization technology. The performance of the electrode material determines the energy consumption of capacitive deionization, as well as the type and valence of the adsorbed ions. At present, the electrode materials used in capacitive deionization technology mainly include: activated carbon, graphene, carbon aerogel, etc. These carbon materials have poor selective adsorption capacity for different metal ions.
[0006] Ti 3 C 2 Tx is a two-dimensional layered metal carbide, commonly known as MXene, whose structure is very similar to the sheet structure of graphene, has a large specific surface area and good electrical conductivity, and is only a few atomic layers thick. 3 C 2 Tx exhibits excellent properties in many aspects, such as electrical properties, optical properties, mechanical properties and thermal stability, so it has been widely used in the fields of energy storage and adsorption. 3C 2 Tx has been used as an electrode material for capacitive deionization technology, but there have been no reports on its application in the field of selective ion adsorption.
[0007] At present, the removal of calcium and magnesium ions in industry usually adopts precipitation method, ion exchange method, etc. These methods are costly and will produce secondary pollution. It is imperative to develop a high-efficiency, low-energy consumption, and secondary-pollution-free calcium and magnesium ion selective removal technology. Summary of the invention
[0008] In order to solve the above technical problems, the present invention provides a capacitive deionization selective adsorption electrode and a preparation method thereof.
[0009] The present invention is achieved through the following technical solutions.
[0010] A method for preparing a capacitive deionization selective adsorption electrode comprises the following steps:
[0011] S1. Add chitosan and polyvinyl alcohol in a mass ratio of 1:(0.1-5) to a 1-4% glacial acetic acid solution and stir to dissolve;
[0012] S2. Add glutaraldehyde solution to the mixed solution obtained in step S1, and cross-link for 12-16h; wash with deionized water to remove free glutaraldehyde, and dry to obtain a selective material;
[0013] S3. Ti 3 C 2 Tx, the selective material obtained in step S2, conductive carbon black and polyvinyl alcohol are mixed in a mass ratio of 8:1:1:1, ground and then scraped on graphite paper, and dried to obtain a selective adsorption electrode.
[0014] Furthermore, in step S1, the mass ratio of chitosan to polyvinyl alcohol is 1:1.
[0015] Furthermore, in step S2, the concentration of the glutaraldehyde solution is 5%.
[0016] Furthermore, in step S3, the drying conditions are 40-80° C. vacuum drying for 6-10 hours.
[0017] A capacitive deionization selective adsorption electrode prepared by the above method.
[0018] This application has the following beneficial effects.
[0019] The electrode prepared by the method of the present application has good regeneration performance, high desalination rate, high selectivity for high-valent ions such as calcium and magnesium, and is suitable for seawater desalination, hard water softening, separation and enrichment of different ions, etc. The preparation process of the present application is simple, the conditions are mild, and the preparation cost is low, and it is easy to realize large-scale industrial production. DETAILED DESCRIPTION
[0020] This application's 3 C 2 Tx was purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., product number 102475.
[0021] Example 1
[0022] A method for preparing a capacitive deionization selective adsorption electrode comprises the following steps:
[0023] S1. Weigh 1.0g chitosan, add it to 100mL 1% glacial acetic acid aqueous solution, stir and dissolve to obtain a transparent solution; weigh 0.1g polyvinyl alcohol, add it to 2ml deionized water, stir and dissolve to obtain a transparent solution; under vigorous stirring, add the polyvinyl alcohol solution to the chitosan solution;
[0024] S2. Under vigorous stirring, 4 mL of 5% glutaraldehyde aqueous solution was added dropwise. After the addition was completed, the mixture was shaken on a shaker for 16 h to obtain a gel-like material. The mixture was washed with a large amount of deionized water to remove free glutaraldehyde, and then dried in vacuum at 60 ° C to obtain a selective material.
[0025] S3. Weigh 8g Ti 3 C 2 Tx, 1g selective material, 1g conductive carbon black, 40g 2.5% polyvinyl alcohol solution, add 50mL deionized water, mix well and grind to obtain slurry, then scrape and coat on graphite paper, and vacuum dry at 40°C for 10h to obtain a selective adsorption electrode.
[0026] Example 2
[0027] A method for preparing a capacitive deionization selective adsorption electrode comprises the following steps:
[0028] S1. Weigh 1.0 g of chitosan, add it to 25 mL of 4% glacial acetic acid aqueous solution, stir and dissolve to obtain a transparent solution; weigh 5.0 g of polyvinyl alcohol, add it to 100 ml of deionized water, stir and dissolve to obtain a transparent solution; under vigorous stirring, add the polyvinyl alcohol solution to the chitosan solution;
[0029] S2. Under vigorous stirring, 6 mL of 5% glutaraldehyde aqueous solution was added dropwise. After the addition was completed, the mixture was shaken on a shaker for 12 h to obtain a gel-like material. The mixture was washed with a large amount of deionized water to remove free glutaraldehyde, and then dried in vacuum at 60 ° C to obtain a selective material.
[0030] S3. Weigh 8g Ti 3 C 2 Tx, 1g selective material, 1g conductive carbon black, 40g 2.5% polyvinyl alcohol solution, add 50mL deionized water, mix well and grind to obtain slurry, then scrape and coat on graphite paper, vacuum dry at 80°C for 6h to obtain a selective adsorption electrode.
[0031] Example 3
[0032] A method for preparing a capacitive deionization selective adsorption electrode comprises the following steps:
[0033] S1. Weigh 1.0g chitosan, add it to 50mL 2% glacial acetic acid aqueous solution, stir and dissolve to obtain a transparent solution; weigh 1.0g polyvinyl alcohol, add it to 20ml deionized water, stir and dissolve to obtain a transparent solution; under vigorous stirring, add the polyvinyl alcohol solution to the chitosan solution;
[0034] S2. Under vigorous stirring, 5 mL of 5% glutaraldehyde aqueous solution was added dropwise. After the addition was completed, the mixture was shaken on a shaker for 12 h to obtain a gel-like material. The mixture was washed with a large amount of deionized water to remove free glutaraldehyde, and then dried in vacuum at 60 ° C to obtain a selective material.
[0035] S3. Weigh 8g Ti 3 C 2 Tx, 1g selective material, 1g conductive carbon black, 40g 2.5% polyvinyl alcohol solution, add 50mL deionized water, mix well and grind to obtain slurry, then scrape and coat on graphite paper, and vacuum dry at 60°C for 8h to obtain a selective adsorption electrode.
[0036] Comparative Example 1
[0037] A method for preparing an activated carbon adsorption electrode comprises the following steps:
[0038] Weigh 8 g of activated carbon, 1 g of conductive carbon black, and 40 g of 2.5% polyvinyl alcohol solution, add 50 mL of deionized water, mix well and grind to obtain a slurry, then apply it on graphite paper and vacuum dry it at 60°C for 8 h to obtain an activated carbon adsorption electrode.
[0039] Desalination performance test
[0040] The prepared electrodes were assembled into a device, the selective electrode prepared in Example 3 plus a cation exchange membrane was connected to the negative electrode, and the commercial activated carbon electrode plus an anion exchange membrane was connected to the positive electrode of the power supply. The charge and discharge test was carried out in a mixed solution consisting of 200 mg / L calcium chloride, 200 mg / L magnesium chloride and 150 mg / L sodium chloride. The voltage was controlled at 1.2 V, short-circuit discharge desorption, and the adsorption time and desorption time were both 30 min. The concentration change during the desalination process was detected in real time by a conductivity meter. The mixed solution after adsorption was measured by an atomic absorption spectrometer for Ca 2+ and Mg 2+ As a comparison, a device composed of an activated carbon electrode (prepared in Comparative Example 1) was also tested for desalination under the same conditions. The experimental results are shown in Table 1.
[0041] Table 1 Performance of electrode materials for selective adsorption and removal of ions
[0042]
[0043] It can be seen from Table 1 that, relative to the activated carbon electrode, the selective adsorption electrode has obvious selective adsorption performance for calcium and magnesium ions.
[0044] The embodiments of this specific implementation method are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a capacitive deionization selective adsorption electrode, characterized in that: The following steps are involved: S1. Add chitosan and polyvinyl alcohol in a mass ratio of 1:(0.1-5) to a 1-4% glacial acetic acid solution and stir to dissolve; S2. Add glutaraldehyde solution to the mixed solution obtained in step S1, and cross-link for 12-16h; wash with deionized water to remove free glutaraldehyde, and dry to obtain a selective material; S3. Ti3C2Tx, the selective material obtained in step S2, conductive carbon black and polyvinyl alcohol are mixed in a mass ratio of 8:1:1:1, grind and apply on graphite paper, and dry to obtain a selective adsorption electrode; the drying conditions are vacuum drying at 40-80°C for 6-10h.
2. The method for preparing a capacitive deionization selective adsorption electrode according to claim 1, characterized in that: In step S1, the mass ratio of chitosan to polyvinyl alcohol is 1:
1.
3. The method for preparing a capacitive deionization selective adsorption electrode according to claim 1, characterized in that: In step S2, the concentration of the glutaraldehyde solution is 5%.
4. A capacitive deionization selective adsorption electrode prepared by the method according to any one of claims 1 to 3.
Citation Information
Patent Citations
A mercury ion adsorbent
CN102284277A
Preparation method and application of chitosan and polyvinyl alcohol mixed film
CN102671555A
Preparation method of capacitance deionized selective adsorption electrode
CN105948189A
Porous carbon material for treating organic dye and fluoride-containing waste water, and preparation method thereof
CN107715855A
Photothermal-photochemical synergistic conversion hydrogel material as well as preparation method and application thereof
CN113042077A