A gallium oxide-based MIS-HEMT device and a method for preparing the same
By using δ-doped barrier layer and groove gate etching technology in normally-off gallium oxide-based MIS-HEMT devices, the problem that normally-on high electron mobility transistors cannot be turned off is solved, and the device's Normally off operation and performance improvements.
Patent Information
- Application Number
- CN202111021113.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-01
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-09-01
Smart Images

Figure CN113745333B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of semiconductor devices, and in particular relates to a normally-off gallium oxide-based MIS-HEMT device containing a delta-doped barrier layer and a preparation method thereof. Background Art
[0002] Today, the growing demand for power electronics technology applications has put forward higher performance requirements for power semiconductor devices in terms of voltage resistance, high temperature resistance, efficiency, power and reliability. High electron mobility transistor (HEMT), also known as modulation doped field effect transistor (MODFET) or heterojunction field effect transistor (HFET), which uses the two-dimensional electron gas (2DEG) at the heterojunction interface as the conductive channel, has the characteristics of high electron mobility and high carrier density in device performance because it realizes the separation of donor impurities and electrons in space and avoids the scattering of ionized impurities. These characteristics enable high electron mobility transistors to work well in high-frequency and high-power applications, and also make them an integral part of power semiconductor devices.
[0003] β-Ga2O3 is considered to be an ideal material for preparing a new generation of high-voltage and high-temperature resistant high electron mobility transistors due to its large bandgap (4.9eV), high electron mobility (300cm2 / V·s), ultra-high breakdown field strength (8MV / cm), and low-cost single crystal growth technology. (Advantages of β-Ga2O3 materials) High electron mobility transistors are divided into two types according to their working mode: normally-on (depletion mode) and normally-off (enhancement mode). In the zero bias state, due to the presence of two-dimensional electron gas, high electron mobility transistors are usually normally-on. For normally-on high electron mobility transistors, the device can only be turned off under external negative bias conditions. This will cause additional power loss on the one hand, and make the design of the drive circuit more complicated on the other hand, which not only increases the design cost, but also poses a safety hazard. The normally-off high electron mobility transistor can overcome the above shortcomings, so it has a high application value in practice. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a normally-off gallium oxide-based MIS-HEMT device containing a delta-doped barrier layer and a preparation method thereof in view of the deficiencies in the prior art.
[0005] In order to solve the above technical problems, a normally-off gallium oxide-based MIS-HEMT device containing a δ-doped barrier layer of the present invention comprises a substrate and a buffer layer stacked on one end surface of the substrate, and further comprises: a channel layer, a spacer layer, a δ-doped layer, a barrier layer, a source electrode, a drain electrode, a dielectric layer and a gate electrode;
[0006] The delta-doped layer is arranged on the end surface of the spacer layer away from the channel layer, so as to avoid the generation of parallel conductive channels.
[0007] As a possible implementation method, further,
[0008] The channel layer and the spacer layer are stacked in sequence on the end surface of the buffer layer away from the substrate, the source electrode and the drain electrode are respectively arranged on both sides of the end surface of the channel layer away from the buffer layer, the spacer layer is arranged on the end surface of the channel layer between the source electrode and the drain electrode, the barrier layer is arranged on the end surface of the δ-doped layer away from the spacer layer, the dielectric layer is integrated and divided into three parts, which are respectively arranged across the barrier layer, the source electrode and the drain electrode, and its edge extends downward to cover the barrier layer, the source electrode, the drain electrode and the channel layer, the source electrode and the drain electrode are inverted T-shaped structures, and the upper ends of the inverted T-shaped structures pass through the dielectric layer and expose the dielectric layer; the gate electrode is a T-shaped structure and is connected to the dielectric layer.
[0009] As a possible implementation method, further,
[0010] The substrate layer and the buffer layer have the same width; the upper left and upper right sides of the channel layer are etched to form a table; the widths of the channel layer table, the spacer layer, the delta-doped layer and the barrier layer are the same and smaller than the width of the buffer layer; the middle position on the upper side of the barrier layer is etched to form a groove, and the distance between the groove position and the left side of the barrier layer is smaller than the right side; the dielectric layer forms a groove surrounded by the barrier layer groove.
[0011] As a possible implementation method, further,
[0012] A first cap layer is disposed between the source electrode and the channel layer, one end of which is in contact with an end surface of the channel layer away from the buffer layer, and the other end of which is in contact with the source electrode;
[0013] A second cap layer is disposed between the drain electrode and the channel layer, one end of which is in contact with the end surface of the channel layer away from the buffer layer, and the other end of which is in contact with the drain electrode;
[0014] The upper edges of the first capping layer, the barrier layer and the second capping layer are aligned.
[0015] As a possible implementation method, further,
[0016] The delta-doped layer includes a first delta-doped layer and a second delta-doped layer, the spacer layer includes a first spacer layer and a second spacer layer, and the barrier layer includes a first barrier layer and a second barrier layer;
[0017] The first barrier layer, the first delta doped layer, the first spacer layer, the channel layer, the second spacer layer, the second delta doped layer and the second barrier layer are sequentially stacked from bottom to top on the end surface of the buffer layer away from the substrate, and the dielectric layer is arranged on the second barrier layer.
[0018] The substrate layer, the buffer layer, the first barrier layer, the first delta-doped layer and the first spacer layer have the same width; the channel layer, the second spacer layer, the second delta-doped layer and the second barrier layer have the same width and are smaller than the first spacer layer.
[0019] A method for preparing a normally-off gallium oxide-based MIS-HEMT device containing a delta-doped barrier layer comprises the following steps:
[0020] S01, taking a substrate of preset specifications and pre-treating its surface;
[0021] S02, forming a buffer layer by homoepitaxial growth on one end surface of the substrate;
[0022] S03, homoepitaxially growing a channel layer on the end surface of the buffer layer away from the substrate, and etching steps on both sides of the end surface of the channel layer away from the buffer layer to form a table shape with the same height difference on both sides;
[0023] S04, epitaxially growing a spacer layer on the terrace of the channel layer;
[0024] S05, epitaxially growing a delta-doped layer on the end surface of the spacer layer;
[0025] S06, epitaxially growing a barrier layer on the end surface of the δ-doped layer away from the spacer layer;
[0026] S07. Preparation of source electrode and drain electrode: depositing a metal layer on the etched regions on both sides of the channel layer to obtain the source electrode and drain electrode; or, epitaxially growing a first cap layer and a second cap layer on the etched regions on both sides of the channel layer, and then depositing a metal layer thereon to obtain the source electrode and drain electrode;
[0027] S08, wrapping a dielectric layer with a thickness of 3 to 7 nm at least on the channel layer, the barrier layer, the source electrode and the drain electrode;
[0028] S09, depositing two layers of metal in the groove surrounded by the dielectric layer to form a gate electrode and a MIS structure;
[0029] S10, etching the dielectric layer on the surface of the source electrode and the drain electrode, and then evaporating and depositing source and drain electrode metal pads to form source and drain electrodes, thereby completing the preparation of the device.
[0030] As a possible implementation method, further, it includes the following specific steps:
[0031] S01. Pre-treating the surface of a semi-insulating or high-resistance β-Ga2O3 substrate in a reaction chamber, wherein the doping element of the substrate includes any one of Mg, Fe, Zn, N, and P, the molar percentage of the doping is 0.05 to 0.06, and the thickness is 400 to 700 μm;
[0032] S02, homoepitaxially growing a non-intentionally doped β-Ga2O3 buffer layer with a thickness of 6 to 12 μm on the substrate layer, wherein the epitaxial growth method is one of MOCVD, MBE, PLD and HVPE;
[0033] S03, homoepitaxially growing a non-intentionally doped β-Ga2O3 channel layer with a thickness of 250 to 700 nm on the buffer layer, wherein the epitaxial growth method adopts one of MOCVD, MBE, PLD and HVPE, and after the epitaxial growth is completed, dry etching is performed on the upper left and upper right sides thereof to form a mesa;
[0034] S04. Heteroepitaxially grow an intrinsic (AlGa)2O3 spacer layer with a thickness of 15 to 35 nm above the channel layer terrace, wherein the Al composition is 0.15 to 0.26. The epitaxial growth method is one of MOCVD, MBE, PLD and HVPE;
[0035] S05, a delta doped layer grown on the spacer layer, the doping element type includes any one of Si, Sn, and Ge, and the growth method adopts one of MOCVD and MBE;
[0036] S06. Epitaxially grow an (AlGa)2O3 barrier layer with a thickness of 30 to 50 nm on the δ-doped layer, wherein the Al component is 0.14 to 0.28, and the epitaxial growth method is one of MOCVD, MBE, PLD and HVPE; after the epitaxial growth of the barrier layer is completed, dry etching is performed on the middle of the upper side near the left edge to form a groove, and the remaining barrier layer thickness below the groove is 0 to 6 nm;
[0037] S07, depositing three metal layers of Ti, Al and Au with thicknesses of 60 nm, 80 nm and 200 nm respectively on the upper left and upper right sides of the channel layer by electron beam evaporation to form source and drain electrodes respectively, and then annealing them at high temperature to obtain good ohmic contact;
[0038] S08, depositing a dielectric layer with a thickness of 3 to 7 nm that wraps the channel layer, the barrier layer, the source electrode, and the drain electrode, wherein the dielectric layer comprises any one of Al2O3, SiO2, Si3N4, and HfO2;
[0039] S09, using electron beam evaporation to sequentially deposit two metal layers of Ni and Au with thicknesses of 60 nm and 250 nm respectively at the groove surrounded by the dielectric layer to form a T-type gate electrode and a MIS structure;
[0040] S10, dry-etching the dielectric layer on the surface of the source electrode and the drain electrode to form a metal interconnection window. At this time, the dielectric layer is divided into three parts, and then the source and drain electrode metal pads are deposited by electron beam evaporation to form inverted T-shaped source and drain electrodes to complete the preparation of the device.
[0041] As a possible implementation method, further, it includes the following specific steps:
[0042] S01. Pre-treating the surface of a semi-insulating or high-resistance β-Ga2O3 substrate in a reaction chamber, wherein the doping element of the substrate includes any one of Mg, Fe, Zn, N, and P, the molar percentage of the doping is 0.05 to 0.06, and the thickness is 400 to 700 μm;
[0043] S02, homoepitaxially growing a non-intentionally doped β-Ga2O3 buffer layer with a thickness of 6 to 12 μm on the substrate layer, wherein the epitaxial growth method is one of MOCVD, MBE, PLD and HVPE;
[0044] S03, homoepitaxially growing a non-intentionally doped β-Ga2O3 channel layer with a thickness of 250 to 700 nm on the buffer layer, wherein the epitaxial growth method adopts one of MOCVD, MBE, PLD and HVPE, and after the epitaxial growth is completed, dry etching is performed on the upper left and upper right sides thereof to form a mesa;
[0045] S04. Heteroepitaxially grow an intrinsic (AlGa)2O3 spacer layer with a thickness of 15 to 35 nm above the channel layer terrace, wherein the Al composition is 0.15 to 0.26. The epitaxial growth method is one of MOCVD, MBE, PLD and HVPE;
[0046] S05, a delta doped layer grown on the spacer layer, the doping element type includes any one of Si, Sn, and Ge, and the growth method adopts one of MOCVD and MBE;
[0047] S06. Epitaxially grow an (AlGa)2O3 barrier layer with a thickness of 30 to 50 nm on the δ-doped layer, wherein the Al component is 0.14 to 0.28, and the epitaxial growth method is one of MOCVD, MBE, PLD and HVPE; after the epitaxial growth of the barrier layer is completed, dry etching is performed on the middle of the upper side near the left edge to form a groove, and the remaining barrier layer thickness below the groove is 0 to 6 nm;
[0048] S07. Homoepitaxially grow a first capping layer and a second capping layer of heavily n-type β-Ga2O3 on the etched portions on the upper left and upper right sides of the channel layer, respectively, wherein the epitaxial growth method adopts one of MOCVD, MBE, PLD and HVPE; the doping element type includes any one of Si, Sn, Ge, F and Cl, the doping concentration is 1×1018 to 5×1019 cm-3, and the thickness is 60 to 120 nm; three layers of metals, Ti, Al and Au, with thicknesses of 60 nm, 80 nm and 200 nm, respectively, are sequentially deposited on the first capping layer and the second capping layer by electron beam evaporation to form source and drain electrodes, respectively, and then subjected to high temperature annealing to obtain good ohmic contact;
[0049] S08, depositing a dielectric layer with a thickness of 3 to 7 nm that wraps the channel layer, the first cap layer, the source electrode, the barrier layer, the drain electrode, and the second cap layer, wherein the dielectric layer comprises any one of Al2O3, SiO2, Si3N4, and HfO2;
[0050] S09, using electron beam evaporation to sequentially deposit two metal layers of Ni and Au with thicknesses of 60 nm and 250 nm respectively at the groove surrounded by the dielectric layer to form a T-type gate electrode and a MIS structure;
[0051] S10, dry-etching the dielectric layer on the surface of the source electrode and the drain electrode to form a metal interconnection window. At this time, the dielectric layer is divided into three parts, and then the source and drain electrode metal pads are deposited by electron beam evaporation to form inverted T-shaped source and drain electrodes to complete the preparation of the device.
[0052] A method for preparing a normally-off gallium oxide-based MIS-HEMT device containing a delta-doped double barrier layer comprises the following steps:
[0053] S01, taking a substrate of preset specifications and pre-treating its surface;
[0054] S02, forming a buffer layer by homoepitaxial growth on one end surface of the substrate;
[0055] S03, epitaxially growing a first barrier layer on the end surface of the buffer layer away from the substrate;
[0056] S04, epitaxially growing a first delta-doped layer on an end surface of the first barrier layer;
[0057] S05, epitaxially growing a first spacer layer on an end surface of the first δ-doped layer;
[0058] S06, epitaxially growing a channel layer on an end surface of the first spacer layer;
[0059] S07, epitaxially growing a second spacer layer on the end surface of the channel layer;
[0060] S08, epitaxially growing a second delta-doped layer on an end surface of the second spacer layer;
[0061] S09, epitaxially growing a second barrier layer on an end surface of the second δ-doped layer;
[0062] S10, epitaxially growing a first cap layer and a second cap layer in the regions etched on both sides of the first spacer layer;
[0063] S11, depositing a metal layer on the first cap layer and the second cap layer to obtain a source electrode and a drain electrode;
[0064] S12, wrapping a dielectric layer on the first cap layer, the source electrode, the second barrier layer, the drain electrode and the second cap layer;
[0065] S13, depositing two layers of metal in the groove surrounded by the dielectric layer to form a gate electrode and a MIS structure;
[0066] S14, etching the dielectric layer on the surface of the source electrode and the drain electrode, and then evaporating and depositing the source and drain electrode metal pads to form the source and drain electrodes, and completing the preparation of the device.
[0067] As a possible implementation method, further, it includes the following specific steps:
[0068] S01. Pre-treating the surface of a semi-insulating or high-resistance β-Ga2O3 substrate in a reaction chamber, wherein the doping element of the substrate includes any one of Mg, Fe, Zn, N, and P, the molar percentage of the doping is 0.05 to 0.06, and the thickness is 400 to 700 μm;
[0069] S02, homoepitaxially growing a non-intentionally doped β-Ga2O3 buffer layer with a thickness of 6 to 12 μm on the substrate layer, wherein the epitaxial growth method is one of MOCVD, MBE, PLD and HVPE;
[0070] S03, epitaxially growing a first (AlGa)2O3 barrier layer with a thickness of 30-50 nm on the buffer layer, wherein the Al composition is 0.14-0.28, and the epitaxial growth method is one of MOCVD, MBE, PLD and HVPE;
[0071] S04, epitaxially growing a first delta-doped layer on the first barrier layer, wherein the doping element type includes any one of Si, Sn, and Ge, and the growth method adopts one of MOCVD and MBE;
[0072] S05, epitaxially growing a first spacer layer of i-(AlGa)2O3 with a thickness of 15-35 nm on the first delta-doped layer, wherein the Al composition is 0.15-0.26. The epitaxial growth method is one of MOCVD, MBE, PLD and HVPE;
[0073] S06. epitaxially growing a UID β-Ga2O3 channel layer with a thickness of 100 to 200 nm at a middle position above the first spacer layer, wherein the epitaxial growth method is one of MOCVD, MBE, PLD and HVPE;
[0074] S07, epitaxially growing a second i-(AlGa)2O3 spacer layer with a thickness of 15 to 35 nm on the channel layer, wherein the Al composition is 0.15 to 0.26, and the epitaxial growth method is one of MOCVD, MBE, PLD and HVPE;
[0075] S08, epitaxially growing a second delta-doped layer on the second spacer layer, wherein the doping element type includes any one of Si, Sn, and Ge, and the growth method adopts one of MOCVD and MBE;
[0076] S09, epitaxially growing a second barrier layer of (AlGa)2O3 with a thickness of 30 to 50 nm on the second δ-doped layer, wherein the Al component is 0.14 to 0.28, and the epitaxial growth method is one of MOCVD, MBE, PLD and HVPE. After the epitaxial growth of the second barrier layer is completed, dry etching is performed on the middle of the upper side near the left edge to form a groove, and the thickness of the remaining second barrier layer below the groove is 0 to 6 nm;
[0077] S10, epitaxially growing a first cap layer and a second cap layer of heavily n-type β-Ga2O3 on the left and right sides above the first spacer layer, respectively, wherein the epitaxial growth method adopts one of MOCVD, MBE, PLD and HVPE, the doping element type includes any one of Si, Sn, Ge, F and Cl, the doping concentration is 1×1018 to 5×1019 cm-3, and the thickness is 200 to 400 nm;
[0078] S11, depositing three metal layers of Ti, Al and Au with thicknesses of 60nm, 80nm and 200nm respectively on the first cap layer and the second cap layer by electron beam evaporation to form source and drain electrodes respectively, and then annealing them at high temperature to obtain good ohmic contact;
[0079] S12, depositing a dielectric layer with a thickness of 3 to 7 nm that wraps the first cap layer, the source electrode, the second barrier layer, the drain electrode, and the second cap layer, wherein the dielectric layer comprises any one of Al2O3, SiO2, Si3N4, and HfO2;
[0080] S13, using electron beam evaporation to sequentially deposit two metal layers of Ni and Au with thicknesses of 60 nm and 250 nm respectively at the groove surrounded by the dielectric layer to form a T-type gate electrode and a MIS structure;
[0081] S14. Dry-etching the dielectric layer on the surface of the source electrode and the drain electrode to form a metal interconnection window. At this time, the dielectric layer is divided into three parts, and then the source and drain electrode metal pads are deposited by electron beam evaporation to form inverted T-shaped source and drain electrodes to complete the preparation of the device.
[0082] The present invention adopts the above technical scheme, and has the following beneficial effects: the present invention adopts groove gate etching technology to cut off the conductive channel composed of 2DEG to realize the normally-off operation of HEMT, and the groove gate etching technology has the advantages of mature process, low cost, good uniformity and repeatability. More importantly, the present invention designs a δ-doped (planar doped) barrier layer, and the specific method is that after the (AlGa)2O3 spacer layer is grown, a donor impurity layer with a thickness of several atomic layers is grown thereon, that is, a δ-doped layer, and then an undoped (AlGa)2O3 barrier layer is grown. The present invention adopts a δ-doped barrier layer structure to replace the barrier layer structure in which the entire layer is uniformly doped. On the one hand, it can avoid the generation of parallel conductive channels and overcome the shortcomings of the device transconductance and breakdown voltage reduction, radio frequency characteristic function reduction and switching characteristic deterioration caused by it. On the other hand, it can weaken the trap effect, increase the 2DEG concentration in the channel, and improve the breakdown voltage and reliability of the device. The groove gate etching technology used by the present invention to realize the normally-off operation of the device has the advantages of mature process, low cost, good uniformity and repeatability. BRIEF DESCRIPTION OF THE DRAWINGS
[0083] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:
[0084] Figure 1 A schematic diagram of the structure of a normally-off gallium oxide-based MIS-HEMT device containing a δ-doped single barrier layer provided in Example 1 of the present invention;
[0085] Figure 2 Schematic diagram of the conduction band of the normally-off gallium oxide-based MIS-HEMT device containing a δ-doped single barrier layer in Example 1 at different barrier layer thicknesses;
[0086] Figure 3 A flow chart for preparing a normally-off gallium oxide-based MIS-HEMT device containing a δ-doped single barrier layer provided in Example 1 of the present invention;
[0087] Figure 4 A schematic diagram of the structure of a normally-off gallium oxide-based MIS-HEMT device including a cap layer and a delta-doped single barrier layer provided in Example 2 of the present invention;
[0088] Figure 5 Schematic diagram of the conduction band of the normally-off gallium oxide-based MIS-HEMT device containing a cap layer and a δ-doped single barrier layer in Example 2 at different barrier layer thicknesses;
[0089] Figure 6 A flow chart for preparing a normally-off gallium oxide-based MIS-HEMT device including a cap layer and a delta-doped single barrier layer provided in Example 2 of the present invention;
[0090] Figure 7 A schematic diagram of the structure of a normally-off gallium oxide-based MIS-HEMT device including a cap layer and a delta-doped double barrier layer provided in Example 3 of the present invention;
[0091] Figure 8 Schematic diagram of the conduction band of the normally-off gallium oxide-based MIS-HEMT device containing a cap layer and a δ-doped double barrier layer in Example 3 at different barrier layer thicknesses;
[0092] Fig. 9 This is a flow chart for preparing a normally-off gallium oxide-based MIS-HEMT device containing a cap layer and a delta-doped double barrier layer provided in Example 3 of the present invention. DETAILED DESCRIPTION
[0093] In order to make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.
[0094] Example 1
[0095] The structure of a normally-off gallium oxide-based MIS-HEMT device containing a δ-doped single barrier layer of the present invention is as follows: Figure 1 As shown, from bottom to top, it includes:
[0096] The substrate 11 , the buffer layer 12 , the channel layer 13 , the spacer layer 14 , the delta-doped layer 15 , the barrier layer 16 , the source electrode 17 , the drain electrode 18 , the dielectric layer divided into three parts 19 ( 1 ), 19 ( 2 ) and 19 ( 3 ) and the gate electrode 20 .
[0097] Among them, the substrate 11 is a semi-insulating or high-resistance β-Ga2O3, and the doping element type is any one of Mg, Fe, Zn, N, and P, but not limited thereto. The molar percentage of doping is 0.05-0.06, and the thickness is 400-700μm. Above the substrate 11 is a UIDβ-Ga2O3 buffer layer 12, and its thickness is 6-12μm. The main function of this layer is to reduce the defect density of the epitaxial layer and reduce the influence of impurities from the reaction chamber or substrate on the channel electrons, and prevent substrate electrons from entering the buffer layer and interfering with the modulation effect of the gate on the channel electrons. Above the buffer layer 12 is a UIDβ-Ga2O3 channel layer 13, and its upper left and upper right sides are etched (etching thickness is 300 μm, respectively). Figure 121 and 27 in the figure), so it is in the shape of a table. The thickness of the channel layer 13 before being etched is 250 to 700 nm. The function of this layer is to gather 2DEG (25) and serve as an electron transport channel. The purpose of etching the upper left and upper right sides of the channel layer 13 is to increase the oxygen vacancy defects on the surface of the channel layer and increase the carrier concentration at the interface, thereby reducing the ohmic contact resistance. Above the table of the channel layer 13 is the i-(AlGa)2O3 spacer layer 14, which has a thickness of 15 to 35 nm and an Al component of 0.15 to 0.26. The function of this layer is to separate the ionized donor impurities and electrons in the δ-doped layer in space, reduce the influence of ionized impurity scattering on the channel electrons, thereby improving the mobility of electrons, and secondly, to contact with the channel layer to form a triangular potential well, thereby gathering 2DEG (25). Above the spacer layer 14 is a delta-doped layer 15, which is essentially a very thin donor impurity layer, doped with any one of Si, Sn, Ge, but not limited thereto, and serves to provide electrons to the channel layer to form 2DEG (25). Above the delta-doped layer 15 is an (AlGa)2O3 barrier layer 16 etched in the middle of the upper side near the left edge, with a thickness of 30 to 50 nm and an Al component of 0.14 to 0.28. The thickness of the remaining portion (i.e. Figure 1 The thickness shown in 22 is 0-6nm. The functions of the barrier layer 16 are, first, to ensure that the channel region outside the groove has a sufficiently large concentration of 2DEG, second, to be one of the components of the MIS, and third, to be an etched region to achieve the normally-off operation of the device. Above the etched areas on the upper left and upper right sides of the channel layer 13 are the inverted T-shaped source electrode 17 and the drain electrode 18, which are composed of three layers of metals of Ti, Al and Au with thicknesses of 60nm, 80nm and 200nm respectively. The dielectric layer wraps the channel layer 13, the barrier layer 16, the source electrode 17 and the drain electrode 18 and is divided into three parts 19(1), 19(2) and 19(3) by the inverted T-shaped source electrode 17 and the drain electrode 18. The material of the dielectric layer can be any one of Al2O3, SiO2, Si3N4 and HfO2, but is not limited thereto. The thickness is 3-7nm. Its function is to reduce the damage caused by etching and reduce the gate leakage current. Above the groove 23 surrounded by the dielectric layer 19 (2) is a T-shaped gate electrode 20, which is composed of two metal layers of Ni and Au with thicknesses of 60nm and 250nm respectively. The T-shaped gate electrode 20, the dielectric layer 19 (2) and the barrier layer 16 constitute the metal-insulator-semiconductor (MIS) structure of the device.
[0098] For the normally-off gallium oxide-based MIS-HEMT device containing a δ-doped single barrier layer, the recessed gate etching technology is used to realize the normally-off operation of the device. The object of this technology is the barrier layer 16, and the thickness of the portion directly below the gate electrode 20 is reduced to achieve the purpose of the device being normally-off. Since this technology forms a groove by etching the barrier layer 16, a recess 23 surrounded by the dielectric layer 19 (2) is formed when the dielectric layer 19 (2) is deposited, and the gate electrode 20 is recessed into the recess 23 during the manufacturing process, and finally a groove 23 is formed as shown in FIG. Figure 1 The T-shaped groove gate structure shown in (20) is therefore called groove gate etching technology.
[0099] Combination Figure 2 The schematic diagram of the conduction band with different barrier layer thicknesses shown in FIG. 1 explains the mechanism of using the groove gate etching technology to cut off the conductive channel formed by 2DEG to achieve the normally-off operation of the device. As for the barrier layer 16, due to being etched, it can be divided into two types according to its position and thickness. One is the thinner part located below the groove 23 after being etched (i.e. Figure 1 The other is the thicker part outside the groove 23 that has not been etched. The conduction band of the barrier layer 16 located in the thinner part below the groove 23 (i.e., the remaining etched part), the delta-doped layer 15, the spacer layer 14, and the channel layer 13 is as follows: Figure 2 As shown in (a), at this time, due to the thin barrier layer 16, the position of the triangular potential well at the heterojunction interface is raised, so that it is located above the Fermi level, and at the same time, the channel electrons located below the groove 23 are completely depleted (i.e. Figure 1 There is no 2DEG at 24 in the figure). The barrier layer 16 is not etched and the conduction bands of the thicker parts outside the groove 23, the delta-doped layer 15, the spacer layer 14 and the channel layer 13 are as shown in FIG. Figure 2 As shown in (b), at this time, due to the thick barrier layer 16, the position of the triangular potential well at the heterojunction interface is reduced, so that it is located below the Fermi level, so that electrons gather on the surface of the channel layer outside the groove 23 (i.e. Figure 1 For the entire device, when the gate electrode 20 is not biased and only a bias voltage is applied between the source electrode 17 and the drain electrode 18, due to the channel layer interface below the groove 23 (i.e. Figure 1 24) in the circuit has no 2DEG, which causes the conductive channel between the source electrode 17 and the drain electrode 18 formed by the 2DEG to be cut off, thereby disconnecting the source electrode 17 and the drain electrode 18, and no leakage current is output, so the device works in a normally-off state.
[0100] Reference Figure 3 The present invention provides a method for preparing a normally-off gallium oxide-based MIS-HEMT device containing a δ-doped single barrier layer:
[0101] A β-Ga2O3 substrate 11 with a thickness of 600 μm and doped with Fe and a molar percentage of 0.055 was prepared, a β-Ga2O3 buffer layer 12 with a thickness of 8 μm, a UIDβ-Ga2O3 channel layer 13 with a thickness of 600 nm, an i-(AlGa)2O3 spacer layer 14 with a thickness of 25 nm and an Al component of 0.16, a δ-doped layer 15 doped with Si element, and an (AlGa)2O3 barrier layer 16 with a thickness of 45 nm and an Al component of 0.24 (the remaining A normally-off gallium oxide-based MIS-HEMT device containing a delta-doped single barrier layer is provided, wherein the residual barrier layer thickness 22 is 3 nm), a source electrode 17 and a drain electrode 18 are composed of three metal layers of Ti, Al and Au with thicknesses of 60 nm, 80 nm and 200 nm respectively, a Si3N4 dielectric layer with a thickness of 4 nm (composed of three parts 19(1), 19(2) and 19(3)), and a gate electrode 20 is composed of two metal layers of Ni and Au with thicknesses of 60 nm and 250 nm respectively, the steps of which are as follows:
[0102] (1) Prepare an Fe-doped high-resistance or semi-insulating β-Ga2O3 substrate 11 and pretreat it. Specifically, the substrate is first cleaned with acetone and isopropanol for 40 to 60 seconds, then cleaned with deionized water, and finally dried with a nitrogen gun. Figure 3 (a).
[0103] (2) Placing the substrate 11 in a metal organic chemical vapor deposition (MOCVD) reaction chamber to homoepitaxially grow a buffer layer 12, such as Figure 3 (b) The epitaxial growth conditions are as follows: triethylgallium (TEGa) is used as the gallium source with a flow rate of 40 sccm; argon is used as the carrier gas to transport the gallium source to the reaction chamber; high-purity oxygen is used as the reactant with a flow rate of 45 sccm; the growth temperature is 650°C, and O2 / TEGa (the ratio of O2 to gallium source flow rate) is 900.
[0104] (3) homoepitaxially grow the channel layer 13 on the buffer layer 12, and etch the upper left and upper right sides thereof to form a mesa, as shown in FIG. Figure 3(c). MOCVD technology is used for epitaxial growth, and the conditions are as follows: triethylgallium (TEGa) is used as the gallium source, and its flow rate is 30sccm; the carrier gas is argon; the flow rate of the reactant high-purity oxygen is 55sccm; the growth temperature is 720°C, and O2 / TEGa is 920. After the growth of the channel layer 13 is completed, the middle position of the upper surface of the channel layer 13 is protected by photoresist and photolithography, and then the upper left and upper right areas of the channel layer 13 that are not protected by the photoresist are etched by inductively coupled plasma (ICP) to form a mesa. The etching conditions are as follows: the etching gas used is BCl3, and its flow rate is 40sccm; the ignition power is 450W; the entire etching process is divided into two steps, the first step is the main etching process, and the etching power used is 30W; the second step needs to be completed at low power to reduce surface etching damage, and the etching power used is 15W.
[0105] (4) epitaxially growing a spacer layer 14 on the mesa of the channel layer 13, such as Figure 3 (d). MOCVD technology was used for epitaxial growth under the following conditions: triethylgallium (TEGa) was used as the gallium source, trimethylaluminum (TMAl) was used as the aluminum source, the molar number of the aluminum source was represented by moral (TMAl), the molar number of the gallium source and the aluminum source was represented by moral (TEGa + TMGa), and the ratio of the two during the reaction (moral (TMAl) / moral (TEGa + TMGa)) was 0.23; the carrier gas was argon; the flow rate of the reactant high-purity oxygen was 55 sccm; the growth temperature was 800 ° C, and O2 / (TEGa + TMGa) (the ratio of the O2 flow rate to the sum of the gallium source and aluminum source flows) was 940.
[0106] (5) epitaxially growing a delta-doped layer 15 on the spacer layer 14, such as Figure 3 (e) MOCVD technology was used for epitaxial growth under the following conditions: silane was used as a precursor with a molar flow rate of 40 nmol / min; argon was used as a carrier gas, the flow rate of the reactant O2 was 650 sccm, and the growth temperature was 800°C.
[0107] (6) epitaxially grow a barrier layer 16 on the delta-doped layer 15 and dry-etch the middle of the upper side near the left edge to form a trench, such as Figure 3(f). MOCVD technology is used for epitaxial growth, and the conditions are as follows: triethylgallium (TEGa) is used as the gallium source, trimethylaluminum (TMAl) is used as the aluminum source, and moral (TMAl) / moral (TEGa + TMGa) is 0.26; the carrier gas is argon; the flow rate of the reactant high-purity oxygen is 52sccm; the growth temperature is 850°C, and O2 / (TEGa + TMGa) is 960. After the epitaxial growth of the barrier layer 16 is completed, the barrier layer 16 is protected outside the groove by photoresist and photolithography, and then the barrier layer is not protected by the photoresist. The area is etched by ICP to form a groove. The etching conditions are as follows: the etching gas used is BCl3, and its flow rate is 35sccm; the ignition power is 380W; the entire etching process is divided into two steps, the first step is the main etching process, and the etching power used is 28W, and the second step needs to be completed at low power to reduce surface etching damage, and the etching power used is 12W.
[0108] (7) Depositing source electrode 17 and drain electrode 18 above the etched portions on the upper left and upper right sides of the channel layer 13, as shown in FIG. Figure 3 (g) Electron beam evaporation technology is used to deposit three metal layers of Ti, Al, and Au in sequence under high vacuum and 550 W process conditions. After the source electrode 17 and the drain electrode 18 are deposited, annealing is performed in a nitrogen atmosphere at a temperature of 480°C for 65 seconds.
[0109] (8) Depositing a dielectric layer 19, such as Figure 3 (h) The deposition technology used was plasma enhanced chemical vapor deposition (PECVD) with the following conditions: ammonia flow rate of 4 sccm, nitrogen flow rate of 920 sccm, silane flow rate of 280 sccm, temperature of 450°C, and power of 25W.
[0110] (9) Depositing a T-shaped gate electrode 20, such as Figure 3 (i) Electron beam evaporation technology is used to deposit two layers of gate metal, Ni and Au, in sequence under high vacuum and 450W power conditions.
[0111] (10) Dry-etching the dielectric layer on the surface of the source electrode 17 and the drain electrode 18 to form a metal interconnection window, and then depositing metal pads of the source electrode 17 and the drain electrode 18 by electron beam evaporation to form an inverted T-shaped source electrode 17 and drain electrode 18, as shown in FIG. Figure 3 (j). Dry etching uses ICP etching, and the conditions are as follows: the etching gas is a mixed gas composed of CF4 and O2, with flow rates of 75 sccm and 5 sccm respectively; the ignition power is 450 W; and the etching power is 75 W. The deposition method and conditions of the source electrode 17 and the drain electrode 18 are the same as those of step (7) of Example 1.
[0112] Example 2
[0113] A normally-off gallium oxide-based MIS-HEMT device comprising a cap layer and a delta-doped single barrier layer according to the present invention is Figure 4 As shown, from bottom to top, it includes:
[0114] The substrate 31, the buffer layer 32, the channel layer 33, the spacer layer 34, the delta-doped layer 35, the barrier layer 36, the first cap layer 37, the second cap layer 38, the source electrode 39, the drain electrode 40, the dielectric layer divided into three parts 41(1), 41(2) and 41(3), and the gate electrode 42.
[0115] The substrate 31, the buffer layer 32, the channel layer 33, the spacer layer 34, the delta doped layer 35, and the barrier layer 36 are respectively Figure 1 The substrate 11, buffer layer 12, channel layer 13, spacer layer 14, delta doped layer 15, and barrier layer 16 in FIG. 43 and 48 respectively represent the thickness of the upper left and upper right sides of the channel layer 33 etched, and the value ranges are respectively Figure 1 21 and 26 are the same. 44 represents the thickness of the remaining barrier layer, which is Figure 1 The value range of 22 in is the same. The first cap layer 37 and the second cap layer 38 located above the etched portion on the upper left and upper right sides of the channel layer 33 are n-type heavily doped β-Ga2O3, and the doping element type is any one of Si, Sn, Ge, F, and Cl, but not limited thereto, and the doping concentration is 1×1018~5×1019cm-3, and the thickness is 60~120nm. The role of the first cap layer 37 and the second cap layer 38 is to reduce the process difficulty while obtaining good ohmic contact. The source electrode 39 and the drain electrode 40 are respectively Figure 1 The source electrode 17 and the drain electrode 18 in the same manner correspond to each other. 41(1), 41(2) and 41(3) as one of the components of the dielectric layer are respectively Figure 1 19(1), 19(2) and 19(3) correspond to each other. Above the groove 45 surrounded by the dielectric layer 41(2) is a T-shaped gate electrode 42. Figure 1 The MIS structure of the device is formed by a T-type gate electrode 42, a dielectric layer 41 (2) and a barrier layer 36.
[0116] Schematic diagram of the conduction band of a normally-off gallium oxide-based MIS-HEMT device with a cap layer and a δ-doped single barrier layer at different barrier layer thicknesses. Figure 5 As shown, due to Figure 5 The barrier layer 36, the delta-doped layer 35, the spacer layer 34 and the channel layer 33 are respectively Figure 2The barrier layer 16, the δ-doped layer 15, the spacer layer 14 and the channel layer 13 in the device correspond to each other, so the normally-off type gallium oxide-based MIS-HEMT device containing the cap layer and the δ-doped single barrier layer also realizes the normally-off operation of the device by cutting off the conductive channel composed of 2DEG using the groove gate etching technology. Its mechanism is exactly the same as that of the normally-off type gallium oxide-based MIS-HEMT device containing the δ-doped single barrier layer. The thickness of the barrier layer 36 located below the groove 45 is thinned by using the groove gate etching technology to deplete the electrons in the channel layer 33 located directly below the groove 45, that is, there is no 2DEG at 46 (at Figure 5 (a) shows that the triangular potential well in the channel 33 is located above the Fermi level EF), and at the same time, it is ensured that the area of the channel layer 33 outside the groove 45 can gather a certain concentration of electrons, that is, there is a 2DEG at 47 (at Figure 5 (b) shows that the triangular potential well in the channel 33 is located below the Fermi level EF), which ultimately makes the source electrode 39 and the drain electrode 40 disconnected when the gate electrode 42 is not biased because the conductive channel connecting the two formed by 2DEG is cut off, completing the normally-off operation of the device.
[0117] Reference Figure 6 The present invention is based on a method for preparing a normally-off gallium oxide-based MIS-HEMT device containing a cap layer and a delta-doped single barrier layer:
[0118] A β-Ga2O3 substrate 31 with a thickness of 600 μm and doped with Fe and a molar percentage of 0.055 is prepared, a β-Ga2O3 buffer layer 32 with a thickness of 8 μm, a UIDβ-Ga2O3 channel layer 33 with a thickness of 600 nm, an i-(AlGa)2O3 spacer layer 34 with a thickness of 25 nm and an Al component of 0.16, a δ-doped layer 35 doped with Si element, a (AlGa)2O3 barrier layer 36 with a thickness of 45 nm and an Al component of 0.24 (the remaining barrier layer thickness 44 is 3 nm), a 70 nm thick, doped element A normally-off gallium oxide-based MIS-HEMT device including a capping layer and a delta-doped single barrier layer is provided, wherein the first capping layer 37 and the second capping layer 38 have concentrations of Si and 1×1019cm-3, respectively, a Si3N4 dielectric layer having a thickness of 4nm (composed of three parts 41(1), 41(2) and 41(3)), a source electrode 39 and a drain electrode 40 composed of three metal layers of Ti, Al and Au with thicknesses of 60nm, 80nm and 200nm, respectively, and a gate electrode 42 composed of two metal layers of Ni and Au with thicknesses of 60nm and 250nm, respectively. The steps are as follows:
[0119] (1) Prepare an Fe-doped high-resistance or semi-insulating β-Ga2O3 substrate 31 and pretreat it. Specifically, the substrate is first cleaned with acetone and isopropanol for 40 to 60 seconds, then cleaned with deionized water, and finally dried with a nitrogen gun. Figure 6 (a).
[0120] (2) Placing the substrate 31 in a metal organic chemical vapor deposition (MOCVD) reaction chamber to homoepitaxially grow a β-Ga2O3 buffer layer 32, such as Figure 6 (b) The conditions for epitaxial growth are the same as those in step (2) of Example 1.
[0121] (3) Homoepitaxially grow the channel layer 33 on the buffer layer 32, and etch the upper left and upper right sides thereof to form a mesa, as shown in FIG. Figure 6 (c). The epitaxial growth method and conditions are the same as those of step (3) in Example 1. After the growth of the channel layer 33 is completed, the middle position of the surface of the channel layer 33 is protected by photoresist and photolithography, and then the upper left and upper right areas of the channel layer 33 that are not protected by the photoresist are etched by inductively coupled plasma (ICP) to form a mesa. The etching method and conditions are the same as those of step (3) in Example 1.
[0122] (4) epitaxially grow a spacer layer 34 on the mesa of the channel layer 33, such as Figure 6 (d) The epitaxial growth method and conditions are the same as those in step (4) of Example 1.
[0123] (5) epitaxially grow a delta-doped layer 35 on the spacer layer 34, such as Figure 6 (e) The epitaxial growth method and conditions are the same as those in step (5) of Example 1.
[0124] (6) epitaxially grow a barrier layer 36 on the delta-doped layer 35 and dry-etch the middle of the upper side near the left edge to form a trench, such as Figure 6 (f). The epitaxial growth method and conditions are the same as those of step (6) in Example 1. After the epitaxial growth of the barrier layer 36 is completed, the barrier layer 36 is protected in the area outside the groove by photoresist and photolithography, and then the barrier layer is etched by ICP in the area not protected by the photoresist to form a groove. The etching method and conditions are the same as those of step (6) in Example 1.
[0125] (7) Epitaxially grow a first cap layer 37 and a second cap layer 38 above the etched portions on the upper left and upper right sides of the channel layer 33, as shown in FIG. Figure 6 (g) MOCVD technology was used for epitaxial growth under the following conditions: triethylgallium (TEGa) was used as the gallium source with a flow rate of 35 sccm; silane (SiH4) was used as the dopant; argon was used as the carrier gas; the flow rate of high-purity oxygen as the reactant was 60 sccm; the growth temperature was 600°C, and O2 / TEGa was 970.
[0126] (8) Depositing a source electrode 39 and a drain electrode 40 on the first cap layer 37 and the second cap layer 38, as shown in FIG. Figure 6 (h) The deposition method and conditions are the same as those in step (7) of Example 1. After the source electrode 39 and the drain electrode 39 are deposited, they are annealed. The annealing conditions are the same as those in step (7) of Example 1.
[0127] (9) Depositing a dielectric layer 41, such as Figure 6 (i) The deposition method and conditions are the same as those in step (8) of Example 1.
[0128] (10) Depositing a T-shaped gate electrode 20, such as Figure 6 (j) The deposition method and conditions are the same as those in step (9) of Example 1.
[0129] (11) Dry-etching the dielectric layer on the surface of the source electrode 39 and the drain electrode 40 to form a metal interconnection window, and then depositing metal pads of the source electrode 39 and the drain electrode 40 by electron beam evaporation to form an inverted T-shaped source and drain electrode, such as Figure 6 (k) The method and conditions of dry etching are the same as those of step (10) of Example 1. The method and conditions of deposition of source electrode 39 and drain electrode 40 are the same as those of step (10) of Example 1.
[0130] Example 3
[0131] A normally-off gallium oxide-based MIS-HEMT device comprising a cap layer and a delta-doped double barrier layer according to the present invention is Figure 7 As shown, from bottom to top, it includes:
[0132] The substrate 51, the buffer layer 52, the first barrier layer 53, the first δ-doped layer 54, the first spacer layer 55, the channel layer 56, the second spacer layer 57, the second δ-doped layer 58, the second barrier layer 59, the first cap layer 60, the second cap layer 61, the source electrode 62, the drain electrode 63, the dielectric layer divided into three parts 64(1), 64(2) and 64(3), and the gate electrode 65.
[0133] The substrate 51 and the buffer layer 52 are Figure 2 The substrate 31 and the buffer layer 32 in the figure correspond to each other. The first barrier layer 53 (AlGa)2O3 is located above the buffer layer 52. The thickness of the first barrier layer 53 is 30-50nm, and the Al component is 0.14-0.28. The first barrier layer 53 and the first spacer layer 55 act as a wide bandgap semiconductor to form a heterojunction with the narrow bandgap semiconductor β-Ga2O3, thereby exhausting the electrons in the first δ-doped layer 54. The first barrier layer 53 is located above the first δ-doped layer 54, which is connected to the first δ-doped layer 54. Figure 4 The first delta-doped layer 54 is provided with a first spacer layer 55 of i-(AlGa)2O3, which is the same as 35 in FIG. Figure 4 The first spacer layer 55 is located in the middle of the UIDβ-Ga2O3 channel layer 56, and its thickness is 100-200nm. The channel layer 56 is located above the second spacer layer 57, which is the same as the first spacer layer 55. The second spacer layer 57 is located above the second δ-doped layer 58, which is the same as the first δ-doped layer 54. Figure 4 The second barrier layer 59 having the same thickness as 36 in FIG. 3 is etched to a thickness of Figure 7 67 in the range of Figure 4 44 in . On the left and right sides above the first spacer layer 55 are respectively the first cap layer 60 and the second cap layer 61 of heavily n-type β-Ga2O3, the doping element type is any one of Si, Sn, Ge, F, Cl, but not limited thereto, the doping concentration is 1×1018~5×1019cm-3, and the thickness is 200~400nm. On the first cap layer 60 and the second cap layer are respectively the source electrode 62 and the drain electrode 63, which are respectively connected to Figure 4 The source electrode 39 and the drain electrode 40 in the same manner correspond to each other. 64(1), 64(2) and 64(3) as one of the components of the dielectric layer are respectively Figure 4 41(1), 41(2) and 41(3) are exactly the same. Above the groove 68 surrounded by the dielectric layer 64(2) is a T-shaped gate electrode 65, which is Figure 4 The MIS structure of the device is formed by the T-type gate electrode 65, the dielectric layer 64(2) and the second barrier layer 59.
[0134] Schematic diagram of the conduction band of a normally-off gallium oxide-based MIS-HEMT device with a cap layer and a δ-doped double barrier layer at different barrier layer thicknesses. Figure 8 As shown. Since the narrow bandgap channel layer 56 is flanked by the symmetrical wide bandgap first spacer layer 55 and the second spacer layer 57, an approximately square potential well consisting of two triangular potential wells appears at the channel layer 56. The normally-off gallium oxide-based MIS-HEMT device containing a cap layer and a δ-doped double barrier layer also achieves the normally-off operation of the device by cutting off the conductive channel formed by 2DEG using the recessed gate etching technology. Its mechanism is similar to that of the normally-off gallium oxide-based MIS-HEMT device containing a cap layer and a δ-doped single barrier layer, in that the thickness of the second barrier layer 59 located below the recess 68 is thinned by the recessed gate etching technology to deplete the electrons in the channel layer 56 located directly below the recess 68, that is, there is no 2DEG at 69 (at Figure 8 (a) shows that the square potential well in the channel 56 is located above the Fermi level EF), and at the same time, it is ensured that the area of the channel layer 56 outside the groove 68 can gather a certain concentration of electrons, that is, there is a 2DEG at 66 (at Figure 8(b) shows that the square potential well in the channel 56 is located below the Fermi level EF), so that when the gate electrode is not biased, the source electrode 62 and the drain electrode 63 are disconnected because the conductive channel connecting the two formed by 2DEG is cut off, completing the normally-off operation of the device.
[0135] Reference Fig. 9 The present invention is based on a method for preparing a normally-off gallium oxide-based MIS-HEMT device containing a cap layer and a delta-doped double barrier layer:
[0136] A β-Ga2O3 substrate 51 with a thickness of 600 μm and doped with Fe and a molar percentage of 0.055 is prepared, a β-Ga2O3 buffer layer 52 with a thickness of 8 μm, a first (AlGa)2O3 barrier layer 53 with a thickness of 45 nm and an Al component of 0.24, a first δ-doped layer 54 doped with Si element, a first i-(AlGa)2O3 spacer layer 55 with a thickness of 25 nm and an Al component of 0.16, a β-Ga2O3 channel 56 with a thickness of 180 nm, an i-(AlGa)2O3 second spacer layer 57 with a thickness of 25 nm and an Al component of 0.16, a second δ-doped layer 58 doped with Si element, a first δ-doped layer 59 with a thickness of 45 nm and an Al component of 0.24 A normally-off gallium oxide-based MIS-HEMT device comprising a (AlGa)2O3 second barrier layer 59 (the remaining barrier layer thickness 67 is 3 nm), a first cap layer 60 and a second cap layer 61 with a thickness of 250 nm and doped with Si and 1×1019 cm-3, respectively, a Si3N4 dielectric layer with a thickness of 4 nm (composed of three parts 64(1), 64(2) and 64(3)), a source electrode 62 and a drain electrode 63 composed of three metal layers of Ti, Al and Au with thicknesses of 60 nm, 80 nm and 200 nm, respectively, and a gate electrode 65 composed of two metal layers of Ni and Au with thicknesses of 60 nm and 250 nm, respectively, containing a cap layer and a delta-doped double barrier layer, wherein the steps are as follows:
[0137] (1) Prepare an Fe-doped high-resistance or semi-insulating β-Ga2O3 substrate 51 and pretreat it. Specifically, the substrate is first cleaned with acetone and isopropanol for 40 to 60 seconds, then cleaned with deionized water, and finally dried with a nitrogen gun. Fig. 9 (a).
[0138] (2) Placing the substrate 51 in a metal organic chemical vapor deposition (MOCVD) reaction chamber to homoepitaxially grow a buffer layer 52, such as Fig. 9 (b) The conditions for epitaxial growth are the same as those in step (2) of Example 2.
[0139] (3) epitaxially growing a first barrier layer 53 on the buffer layer 52, such as Fig. 9(c) The epitaxial growth method and conditions are the same as those in step (6) of Example 2.
[0140] (4) epitaxially growing a first delta-doped layer 54 on the first barrier layer 53, such as Fig. 9 (d) The epitaxial growth method and conditions are the same as those in step (5) of Example 2.
[0141] (5) epitaxially grow a first spacer layer 55 on the first delta-doped layer 54, such as Fig. 9 (e) The epitaxial growth method and conditions are the same as those in step (4) of Example 2.
[0142] (6) epitaxially grow a channel layer 56 at a middle position above the first spacer layer, such as Fig. 9 (f) MOCVD technology was used for epitaxial growth under the following conditions: triethylgallium (TEGa) was used as the gallium source with a flow rate of 30 sccm; the carrier gas was argon; the flow rate of the reactant high-purity oxygen was 55 sccm; the growth temperature was 720°C, and the O2 / TEGa ratio was 920.
[0143] (7) epitaxially grow a second spacer layer 57 on the channel layer 56, such as Fig. 9 (g) The epitaxial growth method and conditions are the same as those in step (4) of Example 2.
[0144] (8) epitaxially grow a second delta-doped layer 58 on the second spacer layer 57, such as Fig. 9 (h) The epitaxial growth method and conditions are the same as those in step (5) of Example 2.
[0145] (9) epitaxially grow a second barrier layer 59 on the second δ-doped layer, such as Fig. 9 (i). The epitaxial growth method and conditions are the same as step (6) in Example 2. After the epitaxial growth of the barrier layer 36 is completed, the barrier layer 59 is protected in the area outside the groove by photoresist and photolithography, and then the barrier layer is etched by ICP in the area not protected by the photoresist to form a groove. The etching method and conditions are the same as step (6) in Example 2.
[0146] (10) A first capping layer 60 and a second capping layer 61 are epitaxially grown on the left and right sides of the first spacer layer 55, respectively. Fig. 9 (j) MOCVD technology was used for epitaxial growth under the following conditions: triethylgallium (TEGa) was used as the gallium source with a flow rate of 35 sccm; silane (SiH4) was used as the dopant; argon was used as the carrier gas; the flow rate of high-purity oxygen as the reactant was 60 sccm; the growth temperature was 600°C, and the O2 / TEGa ratio was 970.
[0147] (11) Depositing a source electrode 62 and a drain electrode 63 on the first cap layer 60 and the second cap layer 61, as shown in FIG. Fig. 9 (k) The deposition method and conditions are the same as those in step (8) of Example 2. After the source electrode 62 and the drain electrode 63 are deposited, they are annealed. The annealing conditions are the same as those in step (8) of Example 2.
[0148] (12) Depositing a dielectric layer 64, such as Fig. 9 (l) The deposition method and conditions are the same as those in step (9) of Example 2.
[0149] (13) Depositing a T-shaped gate electrode 65, such as Fig. 9 (m) The deposition method and conditions are the same as those in step (10) of Example 2.
[0150] (14) Dry etching the dielectric layer on the surface of the source electrode 62 and the drain electrode 63 to form a metal interconnection window, and then depositing the metal pads of the source electrode 62 and the drain electrode 63 by electron beam evaporation to form an inverted T-shaped source electrode 62 and drain electrode 63, as shown in FIG. Fig. 9 (n) The method and conditions of dry etching are the same as those of step (11) of Example 2. The method and conditions of deposition of source electrode 62 and drain electrode 63 are the same as those of step (11) of Example 2.
[0151] The above are embodiments of the present invention. For ordinary technicians in this field, according to the teachings of the present invention, all equivalent changes, modifications, substitutions and variations made within the scope of the patent application of the present invention without departing from the principles and spirit of the present invention should fall within the scope of the present invention.
Claims
1. A normally-off gallium oxide-based MIS-HEMT device containing a delta-doped barrier layer, comprising a substrate layer and a buffer layer stacked on one end surface of the substrate layer, characterized in that: It also includes: a channel layer, a spacer layer, a delta doping layer, a barrier layer, a source electrode, a drain electrode, a dielectric layer and a gate electrode; Wherein, the delta doped layer is arranged on the end surface of the spacer layer away from the channel layer, so as to avoid the generation of parallel conductive channels; The delta-doped layer includes a first delta-doped layer and a second delta-doped layer, the spacer layer includes a first spacer layer and a second spacer layer, and the barrier layer includes a first barrier layer and a second barrier layer; The first barrier layer, the first delta-doped layer, the first spacer layer, the channel layer, the second spacer layer, the second delta-doped layer and the second barrier layer are sequentially stacked from bottom to top on the end surface of the buffer layer away from the substrate layer, and the dielectric layer is arranged on the second barrier layer; The substrate layer, the buffer layer, the first barrier layer, the first delta-doped layer and the first spacer layer have the same width; the channel layer, the second spacer layer, the second delta-doped layer and the second barrier layer have the same width and are smaller than the first spacer layer.
2. A normally-off gallium oxide-based MIS-HEMT device containing a δ-doped barrier layer according to claim 1, characterized in that: The channel layer and the spacer layer are stacked in sequence on the end face of the buffer layer away from the substrate layer, the source electrode and the drain electrode are respectively arranged on both sides of the end face of the channel layer away from the buffer layer, the spacer layer is arranged on the end face of the channel layer between the source electrode and the drain electrode, the barrier layer is arranged on the end face of the δ-doped layer away from the spacer layer, the dielectric layer is integrated and divided into three parts, which are respectively arranged across the barrier layer, the source electrode and the drain electrode, and its edge extends downward to cover the barrier layer, the source electrode, the drain electrode and the channel layer, the source electrode and the drain electrode are inverted T-shaped structures, and the upper ends of the inverted T-shaped structures pass through the dielectric layer and expose the dielectric layer; the gate electrode is a T-shaped structure and is connected to the dielectric layer.
3. The normally-off gallium oxide-based MIS-HEMT device containing a δ-doped barrier layer according to claim 1, characterized in that: The substrate layer and the buffer layer have the same width; the upper left and upper right sides of the channel layer are etched to form a table; the table, the spacer layer, the delta-doped layer and the barrier layer have the same width and are smaller than the width of the buffer layer; the middle position on the upper side of the barrier layer is etched to form a groove, and the distance between the groove position and the left side of the barrier layer is smaller than the right side; the dielectric layer forms a groove surrounded by the barrier layer groove.
4. The normally-off gallium oxide-based MIS-HEMT device containing a δ-doped barrier layer according to claim 1, characterized in that: It also includes: A first cap layer is disposed between the source electrode and the channel layer, one end of which is in contact with an end surface of the channel layer away from the buffer layer, and the other end of which is in contact with the source electrode; A second cap layer is disposed between the drain electrode and the channel layer, one end of which is in contact with the end surface of the channel layer away from the buffer layer, and the other end of which is in contact with the drain electrode; The upper edges of the first capping layer, the barrier layer and the second capping layer are aligned.
5. A method for preparing a normally-off gallium oxide-based MIS-HEMT device containing a δ-doped double barrier layer, characterized in that: The steps include: S01, taking a substrate layer with preset specifications and pre-treating its surface; S02, forming a buffer layer by homoepitaxial growth on one end surface of the substrate layer; S03, epitaxially growing a first barrier layer on the end surface of the buffer layer away from the substrate layer; S04, epitaxially growing a first delta-doped layer on an end surface of the first barrier layer; S05, epitaxially growing a first spacer layer on an end surface of the first δ-doped layer; S06, epitaxially growing a channel layer on an end surface of the first spacer layer; S07, epitaxially growing a second spacer layer on the end surface of the channel layer; S08, epitaxially growing a second delta-doped layer on an end surface of the second spacer layer; S09, epitaxially growing a second barrier layer on an end surface of the second δ-doped layer; S10, epitaxially growing a first cap layer and a second cap layer in the regions etched on both sides of the first spacer layer; S11, depositing a metal layer on the first cap layer and the second cap layer to obtain a source electrode and a drain electrode; S12, wrapping a dielectric layer on the first cap layer, the source electrode, the second barrier layer, the drain electrode and the second cap layer; S13, depositing two layers of metal in the groove surrounded by the dielectric layer to form a gate electrode and a MIS structure; S14, etching the dielectric layer on the surface of the source electrode and the drain electrode, and then evaporating and depositing the source and drain electrode metal pads to form the source and drain electrodes, and completing the preparation of the device.
6. The method for preparing a normally-off gallium oxide-based MIS-HEMT device containing a δ-doped double barrier layer according to claim 5, characterized in that: It includes the following specific steps: S01. Pre-treating the surface of a semi-insulating or high-resistance β-Ga2O3 substrate layer in a reaction chamber, wherein the doping element type of the substrate layer includes any one of Mg, Fe, Zn, N, and P, the molar percentage of the doping is 0.05 to 0.06, and the thickness is 400 to 700 μm; S02, homoepitaxially growing a non-intentionally doped β-Ga2O3 buffer layer with a thickness of 6 to 12 μm on the substrate layer, wherein the epitaxial growth method is one of MOCVD, MBE, PLD and HVPE; S03, epitaxially growing a first (AlGa)2O3 barrier layer with a thickness of 30-50 nm on the buffer layer, wherein the Al composition is 0.14-0.28, and the epitaxial growth method is one of MOCVD, MBE, PLD and HVPE; S04, epitaxially growing a first delta-doped layer on the first barrier layer, wherein the doping element type includes any one of Si, Sn, and Ge, and the growth method adopts one of MOCVD and MBE; S05, epitaxially growing a first i-(AlGa)2O3 spacer layer with a thickness of 15 to 35 nm on the first delta-doped layer, wherein the Al composition is 0.15 to 0.26, and the epitaxial growth method is one of MOCVD, MBE, PLD and HVPE; S06. epitaxially growing a UID β-Ga2O3 channel layer with a thickness of 100 to 200 nm at a middle position above the first spacer layer, wherein the epitaxial growth method is one of MOCVD, MBE, PLD and HVPE; S07, epitaxially growing a second i-(AlGa)2O3 spacer layer with a thickness of 15 to 35 nm on the channel layer, wherein the Al composition is 0.15 to 0.26, and the epitaxial growth method is one of MOCVD, MBE, PLD and HVPE; S08, epitaxially growing a second delta-doped layer on the second spacer layer, wherein the doping element type includes any one of Si, Sn, and Ge, and the growth method adopts one of MOCVD and MBE; S09, epitaxially growing a second barrier layer of (AlGa)2O3 with a thickness of 30 to 50 nm on the second δ-doped layer, wherein the Al component is 0.14 to 0.28, and the epitaxial growth method is one of MOCVD, MBE, PLD and HVPE. After the epitaxial growth of the second barrier layer is completed, dry etching is performed on the middle of the upper side near the left edge to form a groove, and the thickness of the remaining second barrier layer below the groove is 0 to 6 nm; S10, epitaxially growing a first cap layer and a second cap layer of heavily n-type β-Ga2O3 on the left and right sides above the first spacer layer, respectively, wherein the epitaxial growth method adopts one of MOCVD, MBE, PLD and HVPE, the doping element type includes any one of Si, Sn, Ge, F and Cl, the doping concentration is 1×1018 to 5×1019 cm-3, and the thickness is 200 to 400 nm; S11, depositing three metal layers of Ti, Al and Au with thicknesses of 60nm, 80nm and 200nm respectively on the first cap layer and the second cap layer by electron beam evaporation to form source and drain electrodes respectively, and then annealing them at high temperature to obtain good ohmic contact; S12, depositing a dielectric layer with a thickness of 3 to 7 nm that wraps the first cap layer, the source electrode, the second barrier layer, the drain electrode, and the second cap layer, wherein the dielectric layer comprises any one of Al2O3, SiO2, Si3N4, and HfO2; S13, using electron beam evaporation to sequentially deposit two metal layers of Ni and Au with thicknesses of 60 nm and 250 nm respectively at the groove surrounded by the dielectric layer to form a T-type gate electrode and a MIS structure; S14. Dry-etching the dielectric layer on the surface of the source electrode and the drain electrode to form a metal interconnection window. At this time, the dielectric layer is divided into three parts, and then the source and drain electrode metal pads are deposited by electron beam evaporation to form inverted T-shaped source and drain electrodes to complete the preparation of the device.