Secondary battery and device containing the secondary battery

By using artificial graphite as the negative electrode active material in secondary batteries, and combining it with the optimization of cell size and structure, the problems of fast charging and long cycle life under high energy density are solved, thereby improving the electrochemical performance and safety of the battery.

CN113767498BActive Publication Date: 2026-11-17CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202080005570.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-04-02
Publication Date
2026-11-17
Estimated Expiration
2040-04-02

AI Technical Summary

Technical Problem

How to balance the fast charging performance and long cycle life of secondary batteries while improving high-temperature storage performance, under the premise of high energy density.

Method used

Artificial graphite is used as the negative electrode active material. By rationally designing the size and structural parameters of the battery cell, the uniform wetting and reflux of the electrolyte in the negative electrode membrane are ensured, the pore structure of the negative electrode membrane is optimized, and the reduction and precipitation of active ions are reduced.

Benefits of technology

This technology enables secondary batteries to exhibit excellent fast-charging performance, cycle life, and high-temperature storage performance at high energy density, while reducing the reduction and precipitation of active ions caused by poor electrolyte wetting, thus improving battery safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113767498B_ABST
    Figure CN113767498B_ABST
Patent Text Reader

Abstract

This application discloses a secondary battery and an apparatus containing the secondary battery. The secondary battery includes an electrode assembly, which includes a cell and tabs extending from the cell. The cell includes a negative electrode sheet, which includes a negative current collector and a negative electrode film disposed on at least one surface of the negative current collector and comprising a negative electrode active material. The negative electrode active material comprises artificial graphite, which comprises secondary particles. The cell satisfies the following conditions: a ≤ 15 cm; where a is the maximum dimension of the cell in the tab extension direction, in cm; and b is the maximum dimension of the cell in a direction perpendicular to the tab extension direction, in cm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of secondary battery technology, specifically relating to a secondary battery and an apparatus containing the secondary battery. Background Technology

[0002] Secondary batteries primarily rely on the reciprocating movement of active ions between the positive and negative electrodes for reversible charging and discharging. Due to their advantages such as high energy density, high output voltage, good safety, and the absence of pollution and memory effect, they have been widely used in various consumer electronics products and electric vehicles. Furthermore, with the increasing popularity of electric vehicles, the demand for secondary batteries is expected to experience explosive growth.

[0003] As the application range of rechargeable batteries becomes increasingly wide, customer demand for them is also growing. However, how to achieve high energy density while simultaneously maintaining good other electrochemical performance remains a challenge in the development of rechargeable batteries. Summary of the Invention

[0004] A first aspect of this application provides a secondary battery comprising an electrode assembly, the electrode assembly including a cell and tabs extending from the cell, the cell including a negative electrode sheet, the negative electrode sheet including a negative current collector and a negative electrode film disposed on at least one surface of the negative current collector and including a negative electrode active material, wherein:

[0005] The negative electrode active material includes artificial graphite, and the artificial graphite includes secondary particles;

[0006] And the battery cell satisfies: And a≤15cm; where,

[0007] 'a' represents the maximum dimension of the battery cell in the direction of the tab extension, in cm;

[0008] b is the maximum dimension of the battery cell in the direction perpendicular to the direction of the electrode extension, in cm.

[0009] Surprisingly, the negative electrode active material of the secondary battery provided in this application includes artificial graphite, and the artificial graphite comprises secondary particles aggregated from primary particles. This allows the battery cell to meet specific size designs, enabling the secondary battery to achieve high energy density while also maintaining good fast-charging performance and a long cycle life. Furthermore, the battery also exhibits good high-temperature storage performance.

[0010] In any embodiment of this application, the proportion of secondary particles in the artificial graphite is S≥30%. Secondary particles help maintain unobstructed channels within the porous electrode, enabling the negative electrode to maintain high active ion liquid-phase conductivity during pressure (such as cold pressing or cyclic expansion force), thereby further improving the battery's fast-charging and cycle performance. In some embodiments, 50%≤S≤80%. A suitable proportion of secondary particles in the artificial graphite helps the secondary battery simultaneously achieve high fast-charging performance, cycle performance, and high-temperature storage performance.

[0011] In any embodiment of this application, the battery cell satisfies: Optionally, Optimized cell size design enables secondary batteries to better balance energy density, fast charging performance, and cycle life.

[0012] In any embodiment of this application, 6cm ≤ a ≤ 13cm; optionally, 7cm ≤ a ≤ 12cm. When a is within the given range, the electrolyte wettability of the entire negative electrode film, including the central region, can be further improved, thereby further improving the cycle life of the secondary battery. Furthermore, when a is within an appropriate range, it can also ensure a high proportion of positive and negative electrode active materials in the entire battery, thus giving the battery a high energy density. In addition, as a gradually increases within the given range, the battery can have a suitable temperature rise during charging and discharging, further improving the battery's fast charging performance.

[0013] In any embodiment of this application, the particle size distribution D of the artificial graphite v 10 satisfies: 5.2μm≤D v 10 ≤ 8.3 μm, optionally, 6.6 μm ≤ D v 10≤7.8μm. The presence of a suitable amount of smaller particles in artificial graphite can improve the fast-charging performance of batteries.

[0014] In any embodiment of this application, the average particle size D of the artificial graphite v 50 satisfies: 6μm≤D v 50≤15μm, optionally, 8μm≤D v 50≤13μm. The D of artificial graphite v Within an appropriate range, 50 can further improve the fast charging performance and cycle performance of secondary batteries.

[0015] In any embodiment of this application, the particle size distribution D of the artificial graphite v 90 satisfies: 13μm≤D v 90≤30μm, optionally, 15μm≤D v90≤25μm. An appropriate content of large particles in artificial graphite can further improve the fast charging performance of the battery.

[0016] In any embodiment of this application, the specific surface area SSA of the artificial graphite satisfies: 0.6 m² / s². 2 / g≤SSA≤2.5m 2 / g, optionally, 0.9m 2 / g≤SSA≤1.7m 2 / g. When the specific surface area of ​​artificial graphite is within an appropriate range, it enables batteries to achieve both high fast-charging performance and long cycle life.

[0017] In any embodiment of this application, the compacted density of artificial graphite powder under 2 tons of pressure is 1.5 g / cm³. 3 ~1.7g / cm 3 The option is 1.53g / cm³. 3 ~1.65g / cm 3 Artificial graphite has an appropriate powder compaction density, which enables the negative electrode film using it to have a high compaction density while also having porosity suitable for full electrolyte wetting and reflux. This allows the battery to simultaneously achieve high energy density, fast charging performance, and cycle life.

[0018] In any embodiment of this application, at least a portion of the surface of the artificial graphite has a coating layer.

[0019] In any embodiment of this application, the specific capacity of the artificial graphite is 343 mAh / g to 359 mAh / g, optionally 350 mAh / g to 355 mAh / g. While possessing a high specific capacity, artificial graphite also exhibits a short active ion migration path and facilitates the maintenance of a porous structure within the negative electrode film that allows for electrolyte wetting and reflux, thereby enabling the battery to simultaneously achieve high energy density, fast charging performance, and cycle life.

[0020] In any embodiment of this application, the areal density CW of the negative electrode film satisfies: 7.1 mg / cm³ 2 ≤CW≤10.4mg / cm 2 ;Optional, 7.8 mg / cm 2 ≤CW≤9.1mg / cm 2 When the areal density of the negative electrode film is within an appropriate range, the energy density, fast charging performance, and cycle life of the battery can be further improved.

[0021] In any embodiment of this application, the compaction density PD of the negative electrode film satisfies: 1.4 g / cm³ 3 ≤PD≤1.7g / cm 3 Optionally, 1.45 g / cm³3 ≤PD≤1.65g / cm 3 When the compaction density of the negative electrode film is within an appropriate range, it can further improve the battery's energy density, fast charging performance, and cycle life.

[0022] In any embodiment of this application, the porosity P of the negative electrode film a Satisfying: 23% ≤ P a ≤42%; optionally, 28% ≤P a ≤37%. When the porosity of the negative electrode film is within the given range, the secondary battery can better balance energy density, fast charging performance, and cycle life.

[0023] In any embodiment of this application, the OI value of the negative electrode film satisfies: 10 ≤ OI ≤ 30; optionally, 14 ≤ OI ≤ 25. When the OI value of the negative electrode film is within the given range, the energy density, fast charging performance, and cycle life of the secondary battery can be further improved.

[0024] In any embodiment of this application, the battery cell further satisfies: 0.3 ≤ a / b ≤ 0.8; optionally, 0.4 ≤ a / b ≤ 0.6. When the a / b ratio of the battery cell is within an appropriate range, it facilitates uniform wetting of the electrolyte within the battery cell and also ensures balanced expansion and contraction of the negative electrode sheet in both the horizontal and vertical directions during rapid charging and discharging, which is beneficial to the stability of the electrode interface. Therefore, the fast charging performance and cycle life of the secondary battery are further improved.

[0025] In any embodiment of this application, the battery cell includes a positive electrode sheet, which includes a positive current collector and a positive electrode film disposed on at least one surface of the positive current collector and comprising a positive active material, wherein the positive active material includes one or more of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. This enables the battery to achieve a higher energy density.

[0026] A second aspect of this application provides an apparatus comprising the secondary battery described in the first aspect of this application.

[0027] The device of this application includes the aforementioned secondary battery, and therefore has at least the same advantages as the aforementioned secondary battery. Attached Figure Description

[0028] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the embodiments of this application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the drawings without creative effort.

[0029] Figure 1This is a scanning electron microscope (SEM) image of one embodiment of the negative electrode active material.

[0030] Figure 2 This is an SEM image of another embodiment of the negative electrode active material.

[0031] Figure 3 The cell dimensions a and b of a secondary battery are shown.

[0032] Figure 4 The cell dimensions a and b of another secondary battery are shown.

[0033] Figure 5 The cell dimensions a and b of another secondary battery are shown.

[0034] Figure 6 This is a schematic diagram of one embodiment of a secondary battery.

[0035] Figure 7 yes Figure 6 The exploded diagram.

[0036] Figure 8 This is a schematic diagram of one embodiment of the battery module.

[0037] Figure 9 This is a schematic diagram of one embodiment of the battery pack.

[0038] Figure 10 yes Figure 9 The exploded diagram.

[0039] Figure 11 This is a schematic diagram of one embodiment of a device that uses a secondary battery as a power source. Detailed Implementation

[0040] To make the inventive objectives, technical solutions, and beneficial technical effects of this application clearer, the following detailed description is provided in conjunction with embodiments. It should be understood that the embodiments described in this specification are merely illustrative and not intended to limit the scope of this application.

[0041] For simplicity, this paper only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an undefined range; and any lower limit can be combined with other lower limits to form an undefined range, just as any upper limit can be combined with any other upper limit to form an undefined range. Furthermore, although not explicitly stated, every point or individual value between the endpoints of a range is included within that range. Therefore, each point or individual value can serve as its own lower or upper limit and be combined with any other point or individual value, or with other lower or upper limits, to form an undefined range.

[0042] In the description of this article, it should be noted that, unless otherwise stated, "above" and "below" include the number itself, and "several" in "one or several" means two or more.

[0043] The foregoing description of this invention is not intended to describe every disclosed embodiment or implementation. Instead, the following description provides more specific examples of exemplary embodiments. Throughout the application, guidance is provided through a series of embodiments that can be used in various combinations. The examples listed are merely representative and should not be construed as exhaustive.

[0044] Secondary batteries

[0045] During the charging and discharging process of a secondary battery, the electrolyte is squeezed out and returns to the membrane pores as the active material expands and contracts. This phenomenon is defined as the "breathing phenomenon" of the membrane. Because the interlayer spacing of the negative electrode material changes significantly during the insertion and extraction of active ions, the "breathing phenomenon" is particularly evident in the negative electrode membrane.

[0046] After the electrolyte is extruded from the membrane, it takes time for it to return to the membrane pores. This process can lead to "breathing problems," resulting in poor local wetting of the membrane, causing active ions to be reduced and deposited on the membrane surface, and deteriorating the conductivity of active ions. This directly affects the electrochemical performance of the battery.

[0047] Through extensive research, the applicant has discovered that by using specific negative electrode active materials and rationally designing the cell size parameters, it is possible to effectively ensure that the battery can "breathe smoothly" during cycling. This allows the rechargeable battery to achieve both high energy density and good fast-charging performance, as well as a long cycle life. Furthermore, the battery also exhibits good high-temperature storage performance.

[0048] Therefore, a first aspect of this application provides a secondary battery comprising an electrode assembly, the electrode assembly including a cell and tabs extending from the cell, the cell including a negative electrode sheet, the negative electrode sheet including a negative current collector and a negative electrode film disposed on at least one surface of the negative current collector and including a negative electrode active material, wherein: the negative electrode active material includes artificial graphite, the artificial graphite comprising secondary particles; the cell satisfies: And a≤15cm; where a is the maximum dimension of the battery cell in the direction of the tab extension, in cm; b is the maximum dimension of the battery cell in the direction perpendicular to the direction of the tab extension, in cm.

[0049] In this application, "secondary particle" has a well-known meaning in the art, referring to aggregated particles formed by the aggregation of two or more primary particles. For example... Figure 1 and Figure 2 As shown.

[0050] In this application, the battery cell can be a wound structure formed by a winding process of a positive electrode, a negative electrode, and a separator, or a stacked structure formed by a stacking process. The separator is located between the positive and negative electrode sheets and serves as a separator. The electrode assembly also includes two tabs (i.e., a positive tab and a negative tab) extending from the battery cell. Typically, the positive active material is coated on the coated area of ​​the positive electrode, and the positive tab is formed by stacking multiple uncoated areas extending from the coated area of ​​the positive electrode. Similarly, the negative active material is coated on the coated area of ​​the negative electrode, and the negative tab is formed by stacking multiple uncoated areas extending from the coated area of ​​the negative electrode. Further, the two tabs can be electrically connected to corresponding electrode terminals (which can be disposed on the top cover of the battery packaging) via adapter tabs, thereby extracting the electrical energy from the battery cell.

[0051] The two tabs can extend from the same side of the battery cell, or from opposite sides of the battery cell. For example... Figure 3 and Figure 4 Two different electrode assemblies 52 are shown as examples, each with two tabs 522 extending from the same side of the cell 521. Figure 5 Another electrode assembly 52 is shown as an example, with two tabs 522 extending from opposite sides of a cell 521. a is the maximum dimension of the cell 521 in the direction in which the tabs 522 extend (X direction in the figure); b is the maximum dimension of the cell 521 in a direction perpendicular to the direction in which the tabs 522 extend (Y direction in the figure).

[0052] In the secondary battery of this application, (Denoteed as R) is used to characterize the longest path for the electrolyte to flow back to the negative electrode membrane. The inventors discovered that, under the same conditions, the energy density of a secondary battery increases with the increase of R or the cell dimensions a and b. Furthermore, when R is larger, the battery will experience a certain temperature rise during charging, which can reduce the electrochemical impedance of the battery, improve the conductivity of active ions, and thus improve the fast charging performance of the battery. However, if R or a and b are too large, the electrolyte flow and wetting of the negative electrode membrane will be difficult, and active ions will be more easily reduced and precipitated on the membrane surface, thus affecting the fast charging performance and reducing the cycle life and high-temperature storage performance of the secondary battery. Through extensive research, the inventors further discovered that when the negative electrode active material includes artificial graphite, and the artificial graphite contains secondary particles, and the cell size is controlled within a certain range, the pore structure in the negative electrode film can be effectively improved and the electrolyte backflow resistance reduced, while maintaining a high proportion of active material and an appropriate charging temperature rise in the secondary battery. Simultaneously, the reasonable combination of these two elements can effectively reduce cell expansion during rapid charging and discharging, thereby enhancing fast charging performance and improving cycle performance while maintaining high energy density. Furthermore, their synergy can also improve the problem of excessively high local SOC (State of Charge) in the cell caused by poor electrolyte wetting, thus improving the battery's high-temperature storage performance. Therefore, the secondary battery of this application can achieve both high energy density and good fast charging performance and long cycle life. Furthermore, the battery also exhibits good high-temperature storage performance.

[0053] In addition, the negative electrode film has good electrolyte reflux and wetting performance, which results in good active ion transport performance. This reduces the phenomenon of active ions being reduced and deposited on the surface of the negative electrode film (such as lithium plating), and thus enables the battery to have high safety performance.

[0054] In some optional embodiments, the battery cell satisfies 7cm ≤ R ≤ 15cm; alternatively, 9cm ≤ R ≤ 13cm. For example, the battery cell satisfies R = 8cm, 8.5cm, 9cm, 9.5cm, 10cm, 10.5cm, 11cm, 11.5cm, 12cm, 12.2cm, 12.5cm, 12.8cm, 13cm, 13.5cm, 14cm, or 14.5cm. Optimized cell size design enables secondary batteries to better balance energy density, fast charging performance, and cycle life.

[0055] In some alternative embodiments, 6cm ≤ a ≤ 13cm; alternatively, 7cm ≤ a ≤ 12cm. For example, a can be 6.5cm, 7cm, 8cm, 8.5cm, 9cm, 9.5cm, 10cm, 10.2cm, 10.5cm, 11cm, 11.5cm, 12cm, or 12.5cm.

[0056] The inventors discovered that when 'a' is within a given range, the electrolyte wettability of the entire negative electrode film, including the central region, can be further improved, making it easier for the electrolyte to wet and flow back into the entire negative electrode film, thereby further improving the cycle life of the secondary battery. Furthermore, within an appropriate range, 'a' can also ensure a higher effective height for both the positive and negative electrode films while maintaining proper tab welding. This is beneficial for increasing the proportion of positive and negative electrode active materials in the entire battery, thus resulting in a higher energy density. Moreover, as 'a' gradually increases within the given range, the battery can achieve a suitable temperature rise during charging and discharging, further improving the battery's fast-charging performance.

[0057] In some optional embodiments, the width b of the battery cell satisfies 10cm≤b≤35cm; optionally, 18cm≤b≤25cm; and further optionally, 20cm≤b≤24cm. For example, b can be 15cm, 17cm, 19cm, 20cm, 21cm, 22cm, 23cm, 24cm, 25cm, 27cm, or 30cm.

[0058] The inventors further discovered that controlling the cell width within an appropriate range facilitates uniform wetting and reflux of the electrolyte throughout the negative electrode film, preventing the reduction and precipitation of active ions caused by difficulties in electrolyte wetting in the central area of ​​the negative electrode film during rapid charging and discharging. It also avoids interface wrinkling caused by the continuous contraction and expansion of the negative electrode sheet during charging and discharging, thereby further improving the fast-charging performance and cycle life of the secondary battery. Furthermore, a cell width within an appropriate range also improves the lateral space utilization of the cell, resulting in a higher energy density for the battery.

[0059] In some alternative embodiments, the height 'a' and width 'b' of the battery cell satisfy 0.3 ≤ a / b ≤ 0.8. Optionally, 0.35 ≤ a / b ≤ 0.7. Further alternatively, 0.4 ≤ a / b ≤ 0.6. For example, a / b = 0.3, 0.35, 0.4, 0.42, 0.45, 0.46, 0.48, 0.5, 0.55, 0.6, or 0.65.

[0060] The inventors discovered that when a / b is within an appropriate range, the electrolyte is less affected by its own gravity, which is beneficial for its uniform wetting within the battery cell. Furthermore, an appropriate a / b value also ensures balanced expansion and contraction of the negative electrode in both the horizontal and vertical directions during rapid charging and discharging, contributing to the stability of the electrode interface. Therefore, the fast-charging performance and cycle life of the secondary battery are further improved.

[0061] In the secondary battery of this application, the negative electrode active material includes artificial graphite, and the artificial graphite comprises secondary particles. This improves the pore structure inside the negative electrode film while also giving the negative electrode sheet high active ion solid-phase diffusion performance. In particular, the secondary particles disperse the cyclic expansion during charge and discharge in different directions, thereby maintaining a good pore structure in the negative electrode film and reducing the cyclic expansion force. This significantly reduces the resistance to electrolyte extrusion from and return to the negative electrode film. Therefore, the fast charging performance and cycle performance of the secondary battery are correspondingly improved.

[0062] In some optional embodiments, the proportion S of secondary particles in artificial graphite satisfies 20% ≤ S ≤ 100%; alternatively, S ≥ 30%; further alternatively, S ≥ 50%. For example, the proportion S of secondary particles in artificial graphite can be 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 90%, or 100%. During the compression of the negative electrode sheet (such as cold pressing or cyclic expansion force), the secondary particles can play a good role in channel support, effectively preventing the problem of local, especially surface, pore closure of the negative electrode film caused by particle slippage. This maintains the unobstructed channels inside the porous electrode sheet, allowing the negative electrode sheet to maintain high active ion liquid phase conductivity, thereby further improving the battery's fast charging performance and cycle performance. However, the inventors further discovered that as the content of secondary particles increases, a large number of new interfaces are added to the negative electrode active material during the cold pressing process, thereby increasing the side reactions between the negative electrode active material and the electrolyte, which to some extent affects the battery's high-temperature storage performance. Therefore, in order to further balance and improve the above three performance aspects, optionally, 50% ≤ S ≤ 80%.

[0063] Through in-depth research, the inventors have discovered that when the negative electrode active material of the secondary battery of this application includes artificial graphite, and the artificial graphite includes secondary particles, and the battery cell meets a specific size design, if the artificial graphite also meets one or more of the following parameters, the performance of the secondary battery can be further improved.

[0064] In some optional embodiments, the average particle size D of the artificial graphite v 50 satisfies: 6μm≤D v 50 ≤ 15 μm. Optionally, 8 μm ≤ Dv 50≤13μm, and optionally, 10μm≤D v 50≤12.5μm. The D of artificial graphite v Within a suitable range, 50 can shorten the transport paths of active ions and electrons in the particles, while also reducing the interfacial resistance of the negative electrode. Furthermore, it facilitates the fabrication of uniformly distributed artificial graphite negative electrode films, thereby improving the kinetic performance of the negative electrode film, reducing polarization, and further enhancing the fast-charging and cycle performance of the secondary battery. In addition, appropriate D... v 50 can also reduce electrolyte side reactions and further improve the cycle life of secondary batteries.

[0065] In some embodiments, the particle size distribution D of artificial graphite v 10 satisfies: 5.2μm≤D v 10 ≤ 8.3 μm. Optionally, 6.6 μm ≤ D v 10≤7.8μm. The presence of a suitable amount of smaller particles in the artificial graphite improves the packing performance between particles of the negative electrode active material, further enhancing the solid-phase diffusion performance of active ions in the negative electrode film, thereby improving the battery's fast-charging performance. Simultaneously, this artificial graphite also has a smaller specific surface area, reducing electrolyte side reactions and improving cycle life.

[0066] In some embodiments, the particle size distribution D of artificial graphite v 90 satisfies 13μm ≤ Dv90 ≤ 30μm. Optionally, 15μm ≤ Dv90. v 90 ≤ 25 μm. Alternatively, 18 μm ≤ D v 90≤22μm. An appropriate content of large particles in artificial graphite can improve the transport rate of active ions and electrons in the negative electrode, thereby further improving the fast charging performance of the battery.

[0067] In some embodiments, the specific surface area SSA of artificial graphite satisfies 0.6 m². 2 / g≤SSA≤2.5m 2 / g. Optionally, 0.9m 2 / g≤SSA≤1.7m 2 / g. The specific surface area of ​​artificial graphite is within an appropriate range, which can meet the electrochemical kinetic performance requirements of the battery while reducing side reactions, thus enabling the battery to achieve both high fast charging performance and cycle life.

[0068] In some embodiments, the compaction density of the negative electrode active material powder under 2 tons of pressure is 1.5 g / cm³. 3 ~1.7g / cm 3 The option is 1.53g / cm³. 3 ~1.65g / cm 3Artificial graphite has an appropriate powder compaction density, which enables the negative electrode film using it to have a high compaction density while also having porosity suitable for full electrolyte wetting and reflux. This allows the battery to simultaneously achieve high energy density, fast charging performance, and cycle life.

[0069] In some embodiments, the specific capacity of the artificial graphite can be selected from 343 mAh / g to 359 mAh / g, and may also be selected from 350 mAh / g to 355 mAh / g. This artificial graphite, while possessing a high specific capacity, also exhibits a short active ion migration path and high structural stability, which is beneficial for maintaining the porous structure within the negative electrode film that facilitates electrolyte wetting and reflux. This allows the battery to simultaneously achieve high energy density, fast charging performance, and cycle life.

[0070] In some embodiments, at least a portion of the surface of the artificial graphite has a coating layer. Optionally, 80% to 100% of the surface of the artificial graphite is covered with a coating layer. Further, 90% to 100% of the surface of the artificial graphite may be covered with a coating layer. Optionally, the coating layer covers 100% of the surface of the artificial graphite.

[0071] The coating layer can be a conductive coating layer, and more preferably an amorphous carbon coating layer. Partially or completely surface-coated modified artificial graphite can exhibit higher electronic conductivity and reduce side reactions of the electrolyte on the material surface, thereby further improving the fast-charging performance and cycle life of the secondary battery. Optionally, the coating layer may include one or more of coke, carbon black, soft carbon, and hard carbon.

[0072] The artificial graphite used in this application is commercially available.

[0073] In the secondary battery of this application, the negative electrode active material may optionally contain other active materials that can be used as the negative electrode of the secondary battery. As an example, other active materials may include, but are not limited to, one or more of natural graphite, hard carbon, soft carbon, silicon-based materials, and tin-based materials. Silicon-based materials may be selected from one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, and silicon alloys. Tin-based materials may be selected from one or more of elemental tin, tin oxide compounds, and tin alloys.

[0074] In the secondary battery of this application, the negative electrode film may optionally contain a conductive agent. The conductive agent may be selected from conductive materials known in the art that can be used as the negative electrode of a secondary battery. As an example, the conductive agent in the negative electrode film may include one or more of superconducting carbon, acetylene black, conductive carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0075] In the secondary battery of this application, the negative electrode membrane may optionally contain an adhesive. The adhesive may be selected from adhesive materials known in the art that can be used for the negative electrode of a secondary battery. As an example, the adhesive in the negative electrode membrane may include one or more of styrene-butadiene rubber (SBR), polyvinyl alcohol (PVA), aqueous acrylic resin, sodium alginate (SA), and carboxymethyl chitosan (CMCS).

[0076] In the secondary battery of this application, the negative electrode film may optionally contain a thickener. The thickener may include, but is not limited to, sodium carboxymethyl cellulose (CMC-Na).

[0077] The inventors have also discovered that when the negative electrode active material of the secondary battery of this application includes artificial graphite, and the artificial graphite includes secondary particles, and the cell meets a specific size design, the battery performance can be further improved if the negative electrode film also meets one or more of the following parameters.

[0078] In some alternative embodiments, the porosity P of the negative electrode membrane a Satisfying 23% ≤ P a ≤42%. Alternatively, 28% ≤P a ≤37%. Further, alternatively, 30% ≤P a ≤35%. When the porosity of the negative electrode film is within the given range, the secondary battery can better balance energy density, fast charging performance, and cycle life.

[0079] In some optional embodiments, the OI value of the negative electrode film satisfies 10 ≤ OI ≤ 30. Alternatively, 14 ≤ OI ≤ 25. Further optional, 15 ≤ OI ≤ 20. When the OI value of the negative electrode film is within the given range, good electrical contact is formed between the negative electrode active material particles, while the electrolyte flow driven by volume changes during charging and discharging is relatively small, i.e., the "breathing phenomenon" is weak, which is beneficial for maintaining a good reaction interface, thereby further improving the energy density, fast charging performance, and cycle life of the secondary battery.

[0080] In some optional embodiments, the areal density CW of the negative electrode film satisfies 7.1 mg / cm³. 2 ≤CW≤10.4mg / cm 2 Alternatively, 7.8 mg / cm³ 2 ≤CW≤9.1mg / cm 2 When the areal density of the negative electrode film is within an appropriate range, the negative electrode can achieve a high energy density while reducing the transport impedance of active ions and electrons, thereby further improving the battery's energy density, fast charging performance, and cycle life.

[0081] In some optional embodiments, the compaction density PD of the negative electrode film satisfies 1.4 g / cm³.3 ≤PD≤1.7g / cm 3 Alternatively, 1.45 g / cm³ 3 ≤PD≤1.65g / cm 3 When the compaction density of the negative electrode film is within an appropriate range, the negative electrode sheet can have both high energy density and high low-cycle expansion performance and kinetic performance, thereby further improving the battery's energy density, fast charging performance and cycle life.

[0082] In the secondary battery of this application, the negative electrode current collector can be made of a material with good conductivity and mechanical strength, such as copper foil, but is not limited to this.

[0083] In the secondary battery of this application, the cell further includes a positive electrode sheet, which includes a positive current collector and a positive electrode film disposed on at least one surface of the positive current collector and including a positive active material.

[0084] The positive current collector can be made of a material with good conductivity and mechanical strength. In some optional embodiments, the positive current collector can be aluminum foil, but it is not limited to this.

[0085] This application does not limit the specific type of positive electrode active material. Any active material known in the art that can be used as the positive electrode of a secondary battery can be used. Those skilled in the art can select according to actual needs.

[0086] In some embodiments, the positive electrode active material may include one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and lithium phosphates with an olivine structure, as well as materials modified from the above materials. The lithium phosphates with an olivine structure may include one or more of lithium iron phosphate, lithium iron phosphate and carbon composites, lithium manganese phosphate, and lithium manganese phosphate and carbon composites. To further improve the energy density of the battery, the positive electrode active material may optionally include one or more of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. The modification may be doping and / or coating modification of the above materials.

[0087] In some embodiments, the positive electrode membrane may optionally include an adhesive. This application does not specifically limit the type of adhesive, and those skilled in the art can select one according to actual needs. As an example, the adhesive in the positive electrode membrane may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylic acid (PAA), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0088] In some embodiments, the positive electrode film may optionally include a conductive agent. This application does not impose specific limitations on the type of conductive agent, and those skilled in the art can select one according to actual needs. As an example, the conductive agent in the positive electrode film may include one or more of graphite, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0089] It is understood that the positive current collector has two surfaces opposite each other in its thickness direction, and the positive electrode membrane can be laminated on either or both of the two opposite surfaces of the positive current collector. The negative current collector has two surfaces opposite each other in its thickness direction, and the negative electrode membrane can be laminated on either or both of the two opposite surfaces of the negative current collector.

[0090] It should be noted that the parameters of the positive and negative electrode films given in this application refer to the parameter range of a single-sided film. When the positive and negative electrode films are disposed on two surfaces of the current collector, the film parameters on either surface that meet the requirements of this application are considered to fall within the protection scope of this application. Furthermore, the film thickness, compaction density, areal density, OI value, porosity, and other ranges mentioned in this application refer to the parameter range after cold pressing and compaction and for use in assembling secondary batteries.

[0091] In this paper, the percentage of secondary particles in the negative electrode active material has a well-known meaning in the art and can be tested using methods known in the art. For example, a negative electrode active material (e.g., artificial graphite) is laid and adhered to conductive adhesive to form a sample with a length × width of 6 cm × 1.1 cm; the particle morphology is tested using a scanning electron microscope and energy dispersive spectroscopy (e.g., ZEISS Sigma300). The test can be referenced in JY / T010-1996. To ensure the accuracy of the test results, 20 different regions can be randomly selected from the sample for scanning tests, and at a certain magnification (e.g., 1000x), the ratio of the number of secondary particles to the total number of particles in each region is counted, which is the percentage of secondary particles in that region; the average of the test results of the 20 test regions is taken as the percentage of secondary particles in the artificial graphite. Among them, agglomerated particles formed by the adhesion of two or more primary particles are considered secondary particles.

[0092] The specific capacity of the negative electrode active material has a meaning known in the art and can be tested using methods known in the art. An example test method may include: mixing artificial graphite, conductive agent Super P, and binder PVDF in a mass ratio of 91.6:1.8:6.6 with solvent NMP (N-methylpyrrolidone) to form a slurry; coating the slurry onto a copper foil current collector and drying it in an oven for later use. A lithium metal sheet is used as the counter electrode, and a polyethylene (PE) film is used as the separator. Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and then LiPF6 is uniformly dissolved in the above solution to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L. A CR2430 coin cell is assembled in an argon-protected glove box. After the obtained button cells were left to stand for 12 hours, they were discharged at a constant current of 0.05C to 0.005V, left to stand for 10 minutes, and then discharged at a constant current of 50μA to 0.005V. After leaving to stand for 10 minutes, they were discharged at a constant current of 10μA to 0.005V. Then, they were charged at a constant current of 0.1C to 2V, and the charging capacity was recorded. The ratio of the charging capacity to the mass of the artificial graphite is the specific capacity of the artificial graphite.

[0093] D of negative electrode active material v 10. D v 50. D v 90 has a meaning known in the art and can be determined using instruments and methods known in the art. For example, it can be conveniently determined using a laser particle size analyzer (such as the Malvem Mastersizer 3000) according to GB / T 19077-2016 Particle Size Distribution Laser Diffraction Method. Wherein, D v The physical definition of 90 is the particle size corresponding to a material's cumulative volumetric distribution percentage reaching 90%; D v The physical definition of 50 is the particle size corresponding to a material's cumulative volumetric distribution percentage reaching 50%; D v The physical definition of 10 is the particle size corresponding to a cumulative volume distribution percentage of 10% in a material.

[0094] The specific surface area (SSA) of the negative electrode active material is a well-known concept in the art and can be tested using methods known in the art. For example, it can be tested using the nitrogen adsorption specific surface area analysis method according to GB / T 19587-2017, and calculated using the BET (Brunauer Emmett Teller) method. The nitrogen adsorption specific surface area analysis can be performed using a Tri-Star 3020 specific surface area and pore size analyzer from Micromeritics, Inc.

[0095] The compaction density of the negative electrode active material powder is a well-known concept in the art and can be tested using methods known in the art. For example, it can be tested using an electronic pressure testing machine (such as UTM7305) according to GB / T 24533-2009: a certain amount of powder is placed on a special compaction mold, different pressures are set, and the thickness of the powder under different pressures can be read on the equipment, and the compaction density under different pressures can be calculated.

[0096] It should be noted that all the parameter tests for the above-mentioned negative electrode active material can be performed by sampling from the cold-pressed negative electrode film. As an example of obtaining the negative electrode active material from the cold-pressed negative electrode film, the cold-pressed negative electrode film can be placed in deionized water, and the negative electrode active material will naturally detach. The negative electrode active material is then filtered, dried, and then fired at 400℃ for 2 hours to remove the binder and conductive carbon, thus obtaining the negative electrode active material.

[0097] The areal density of the negative electrode film is a well-known concept in the art and can be measured using instruments and methods known in the art. For example, take a negative electrode sheet that has been coated on one side and cold-pressed (if it is a double-sided coated negative electrode sheet, the negative electrode film on one side can be wiped off first), cut it into small circular pieces with an area of ​​S1, weigh them, and record their weight as M1. Then wipe off the negative electrode film of the weighed negative electrode sheet, weigh the negative current collector, and record it as M0. The areal density of the negative electrode film = (weight of the negative electrode sheet M1 - weight of the negative current collector M0) / S1.

[0098] The thickness of the negative electrode film is a term known in the art and can be measured using instruments and methods known in the art. For example, a 4-digit micrometer can be used.

[0099] The compaction density of the negative electrode membrane is a well-known concept in the art and can be measured using instruments and methods known in the art. The compaction density of the negative electrode membrane = the areal density of the negative electrode membrane / the thickness of the negative electrode membrane.

[0100] The porosity of the negative electrode membrane has a well-known meaning in the art and can be determined using instruments and methods known in the art. An exemplary test method is as follows: A small circular sample with a diameter of 14 mm is cut from a negative electrode sheet with a negative electrode membrane on one side; the thickness of the negative electrode membrane is measured (thickness of the negative electrode sheet - thickness of the negative electrode current collector); the apparent volume V of the negative electrode membrane is calculated according to the formula for the volume of a cylinder. 表 The true volume of the negative electrode sheet is determined using a gas displacement method with an inert gas such as helium or nitrogen as the medium, measured by a true density meter (such as the Micromeritics AccuPyc II 1340). The test can be referenced in GB / T 24586-2009. The true volume of the negative electrode membrane, V, is obtained by subtracting the volume of the negative current collector from the true volume of the negative electrode sheet. 真The porosity of the negative electrode film = (V 表 -V 真 ) / V 表 ×100%. Multiple electrode samples (e.g., 30) can be tested, and the average value of the results can be taken to improve the accuracy of the test results.

[0101] The OI value of the negative electrode sheet has a well-known meaning in the art and can be determined using instruments and methods known in the art. For example, it can be obtained using an X-ray powder diffractometer (such as the PANalytical X'pert PRO type) according to the general rules of X-ray diffraction analysis JISK0131-1996 and the method for determining the lattice parameters of graphite JB / T4220-2011; the OI value of the negative electrode film = C 004 / C 110 , where C 004 C represents the peak area of ​​the characteristic diffraction peak 004 in the X-ray diffraction pattern of the negative electrode. 110 This represents the peak area of ​​the characteristic diffraction peak 110 in the X-ray diffraction pattern of the negative electrode sheet.

[0102] In X-ray diffraction analysis, a copper target can be used as the anode target, with CuKα rays as the radiation source, and the ray wavelength... The scanning 2θ angle range is 20° to 80°, and the scanning rate is 4° / min. The 2θ angle corresponding to the 004 crystal plane of graphite is 53.5° to 55.5°; the 2θ angle corresponding to the 110 crystal plane of graphite is 76.5° to 78.5°.

[0103] In the secondary battery of this application, the cell also includes a separator. The separator is disposed between the positive electrode and the negative electrode, serving as a separator. This application does not impose any particular limitation on the type of separator; any known porous structure separator with good chemical and mechanical stability can be selected. For example, the separator may include glass fiber membrane, non-woven fabric membrane, polyethylene membrane, polypropylene membrane, polyvinylidene fluoride membrane, and their multilayer composite films.

[0104] The secondary battery of this application also includes an electrolyte. The electrolyte comprises an organic solvent and an electrolyte salt dispersed in the organic solvent. The types of organic solvent and electrolyte salt, as well as the composition of the electrolyte, are not specifically limited and can be selected according to requirements.

[0105] As an example, the organic solvent may include one or more of ethylene carbonate (EC), propylene carbonate (PC), methyl ethyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butyl carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS), and diethyl sulfone (ESE).

[0106] As an example, the electrolyte salt is a lithium salt, which may include one or more of the following: LiPF6 (lithium hexafluorophosphate), LiBF4 (lithium tetrafluoroborate), LiClO4 (lithium perchlorate), LiAsF6 (lithium hexafluoroarsenate), LiFSI (lithium bis(fluorosulfonyl)imide), LiTFSI (lithium bis(trifluoromethanesulfonyl)imide), LiTFS (lithium trifluoromethanesulfonate), LiDFOB (lithium difluorooxalate borate), LiBOB (lithium dioxalate borate), LiPO2F2 (lithium difluorophosphate), LiDFOP (lithium difluorodioxalate phosphate), and LiTFOP (lithium tetrafluorooxalate phosphate).

[0107] In some embodiments, the electrolyte may optionally include additives. There are no specific limitations on the types of additives; they can be selected according to requirements. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature performance, and additives that improve battery low-temperature performance.

[0108] The secondary battery of this application also includes an outer packaging. The outer packaging is used to encapsulate the electrode assembly and electrolyte. There are no particular limitations on the type of outer packaging for the secondary battery of this application; it can be selected according to actual needs. In some embodiments, the outer packaging of the secondary battery can be a soft pack, such as a pouch-type soft pack. The material of the soft pack can be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS). The outer packaging of the secondary battery can also be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell.

[0109] Secondary batteries can be prepared using methods known in the art. For example, a secondary battery can be prepared by dispersing a negative electrode active material and optional conductive agents, binders, and thickeners in a solvent (e.g., water) to form a uniform negative electrode slurry; coating the negative electrode slurry onto a negative electrode current collector, and obtaining a negative electrode sheet after drying, cold pressing, and other processes. Negative electrode tabs are obtained in the uncoated areas of the negative electrode current collector by punching or laser die-cutting. Similarly, a positive electrode active material and optional conductive agents and binders are dispersed in a solvent (e.g., N-methylpyrrolidone, NMP) to form a uniform positive electrode slurry; coating the positive electrode slurry onto a positive electrode current collector, and obtaining a positive electrode sheet after drying, cold pressing, and other processes. Positive electrode tabs are obtained in the uncoated areas of the positive electrode current collector by punching or laser die-cutting. The positive electrode sheet, separator, and negative electrode sheet can be formed into an electrode assembly through a winding or stacking process, with the separator acting as a separator between the positive and negative electrode sheets. The electrode assembly is placed in the outer packaging, electrolyte is injected and the packaging is sealed. The secondary battery is then produced through processes such as formation.

[0110] This application does not impose any particular limitation on the shape of the secondary battery; it can be cylindrical, square, or any other arbitrary shape. Figure 6 This is an example of a square-structured secondary battery 5.

[0111] Reference Figure 6 and Figure 7 The outer packaging may include a housing 51 and a cover 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover 53 can be placed over the opening to close the receiving cavity. Electrode assemblies 52 are encapsulated within the receiving cavity. Electrolyte is immersed in the cell. The secondary battery 5 may contain one or more electrode assemblies 52, which can be adjusted according to requirements.

[0112] In some embodiments, secondary batteries can be assembled into battery modules, and the number of secondary batteries contained in a battery module can be multiple, the specific number of which can be adjusted according to the application and capacity of the battery module.

[0113] Figure 8 This is battery module 4, used as an example. (See reference...) Figure 8 In battery module 4, multiple secondary batteries 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple secondary batteries 5 can be fixed in place using fasteners.

[0114] Optionally, the battery module 4 may also include a housing with a receiving space in which a plurality of secondary batteries 5 are received.

[0115] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be adjusted according to the application and capacity of the battery pack.

[0116] Figure 9 and Figure 10 This is battery pack 1 as an example. (See reference...) Figure 9 and Figure 10 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0117] Device

[0118] A second aspect of this application provides an apparatus comprising a secondary battery as described in the first aspect of this application. The secondary battery can be used as a power source for the apparatus or as an energy storage unit. The apparatus may be, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.

[0119] The device can be configured to use a secondary battery, battery module, or battery pack, depending on its usage requirements.

[0120] Figure 11 This is an example device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. To meet the device's requirements for high power and high energy density in its secondary batteries, a battery pack or battery module can be used.

[0121] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a rechargeable battery as their power source.

[0122] Example

[0123] The following embodiments describe the disclosure of this application in more detail. These embodiments are merely illustrative, as various modifications and variations will be apparent to those skilled in the art within the scope of the disclosure of this application. Unless otherwise stated, all parts, percentages, and ratios reported in the following embodiments are based on weight, and all reagents used in the embodiments are commercially available or synthesized by conventional methods and can be used directly without further processing, and the instruments used in the embodiments are commercially available.

[0124] Example 1

[0125] 1) Preparation of positive electrode sheet

[0126] LiNi, a positive electrode active material, is a lithium nickel cobalt manganese oxide (LiNi). 0.6 Co 0.2 Mn 0.2 O2 (NCM622), conductive carbon nanotubes (CNTs), conductive carbon black (Super P), and binder PVDF were thoroughly mixed in an appropriate amount of NMP at a mass ratio of 97.5:0.5:0.9:1.1 to form a uniform positive electrode slurry. The positive electrode slurry was then coated onto a positive electrode current collector aluminum foil. The coated current collector was then transferred to an oven for drying, followed by cold pressing and slitting to obtain the positive electrode sheet. Positive electrode tabs were punched off the uncoated areas of the current collector. The compacted density of the positive electrode sheet was 3.4 g / cm³. 3 Its surface density is 14.1 mg / cm³. 2 .

[0127] 2) Preparation of negative electrode sheet

[0128] Artificial graphite (negative electrode active material), Super P (conductive agent), sodium carboxymethyl cellulose (CMC-Na) (thickener), and styrene-butadiene rubber (SBR) (binder) were mixed in a mass ratio of 94.5:1.5:1.5:2.5. Deionized water was added as a solvent, and the mixture was stirred under vacuum until homogeneous to obtain a negative electrode slurry. The negative electrode slurry was uniformly coated onto a copper foil current collector. After drying the coated current collector at room temperature, it was transferred to an oven for further drying. Following cold pressing and slitting, the negative electrode sheet was obtained. Negative electrode tabs were punched off the uncoated areas of the current collector. The compaction density of the negative electrode sheet was 1.50 g / cm³. 3 Its surface density is 8.44 mg / cm³. 2 .

[0129] 3) Separating membrane

[0130] Polyethylene film was selected as the separator.

[0131] 4) Preparation of electrolyte

[0132] Ethyl carbonate (EC), dimethyl carbonate (DMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1. The thoroughly dried lithium salt LiPF6 was dissolved in the mixed organic solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0133] 5) Preparation of secondary batteries

[0134] The positive electrode, separator, and negative electrode are stacked in sequence, and a reference electrode is added between the separator and the negative electrode (the reference electrode is used for subsequent performance testing of the battery sample; it can be a lithium sheet, lithium metal wire, etc., and should be separated by the separator to prevent contact with either the positive or negative electrode). After winding, an electrode assembly is obtained, wherein the winding width corresponds to the cell size b. The electrode assembly is then placed in an outer packaging. The positive and negative electrode tabs can be electrically connected to the corresponding electrode terminals (located on the top cover of the battery packaging) via adapters. The prepared electrolyte is added and the package is sealed to obtain a secondary battery.

[0135] Examples 2-19 and Comparative Examples 1-5

[0136] Similar to Example 1, except that the relevant preparation parameters of the negative electrode sheet were changed, as detailed in Table 1; and in Table 1,

[0137] The positive electrode active material in Examples 1-16 and Comparative Examples 1-5 was NCM622, with a specific capacity of 185 mAh / g; the positive electrode active material in Example 17 was LiNi. 0.5 Co 0.2 Mn 0.3 O2 (NCM523), with a specific capacity of 175 mAh / g; the positive electrode active material in Example 18 is LiNi. 0.8 Co 0.1 Mn 0.1 O2 (NCM811) has a specific capacity of 200 mAh / g; the positive electrode active material in Example 19 is lithium iron phosphate (LFP) with a specific capacity of 144 mAh / g.

[0138] The areal density and compacted density of the positive electrode films in Examples 1-16 and Comparative Examples 1-5 are the same as those in Example 1; the compacted density of the positive electrode film in Example 17 is 3.45 g / cm³. 3 The areal density is 14.9 mg / cm³. 2 The compaction density of the positive electrode film in Example 18 was 3.5 g / cm³. 3 The areal density is 13.1 mg / cm³. 2 The compaction density of the positive electrode film in Example 19 was 2.35 g / cm³. 3 The areal density is 18.2 mg / cm³. 2 The compaction density and areal density of the negative electrode film in Example 2 are the same as those in Example 1; the compaction density of the negative electrode films in Examples 3-19 and Comparative Examples 1-5 is 1.5 g / cm³. 3 The areal density is 8.39 mg / cm³. 2 .

[0139] Test section

[0140] (1) Cyclic performance test

[0141] At 25°C, the secondary batteries prepared in the above embodiments and comparative examples were charged at a constant current rate of 1C to the charging cutoff voltage V1, then charged at a constant voltage until the current ≤0.05C, allowed to stand for 5 minutes, and then discharged at a constant current rate of 0.33C to the discharge cutoff voltage V2, allowed to stand for 5 minutes. This constitutes one charge-discharge cycle. The batteries were subjected to cyclic charge-discharge tests according to this method until the battery capacity decreased to 80%. The number of cycles at this point is the cycle life of the battery at 25°C.

[0142] (2) Fast charging performance test

[0143] At 25°C, the secondary batteries prepared in the above embodiments and comparative examples were charged and discharged for the first time with a current of 1C (i.e., the current value at which the theoretical capacity is completely discharged within 1 hour). Specifically, the batteries were charged at a constant current of 1C to the charging cutoff voltage V1, then charged at a constant voltage until the current ≤0.05C, left to stand for 5 minutes, and then discharged at a constant current of 0.33C to the discharge cutoff voltage V2. The actual capacity was recorded as C0.

[0144] Then, the battery is sequentially charged at constant currents of 2.8C0, 3C0, 3.2C0, 3.5C0, 3.8C0, 4.1C0, 4.4C0, 4.7C0, 5C0, 5.3C0, 5.6C0, and 5.9C0 until it reaches either the full-cell charging cutoff voltage V1 or the 0V negative electrode cutoff potential (whichever comes first). After each charge, it is discharged at 1C0 until it reaches the full-cell discharge cutoff voltage V2. The negative electrode potentials corresponding to 10%, 20%, 30%, ..., 80% SOC (State of Charge) are recorded at different charging rates. The charging rate-negative electrode potential curves under different SOC states are plotted. After linear fitting, the charging rate corresponding to a negative electrode potential of 0V under different SOC states is obtained. This charging rate is the charging window under that SOC state, denoted as C. 20%SOC C 30%SOC C 40%SOC C 50%SOC C 60%SOC C 70%SOC C 80%SOC According to the formula (60 / C) 20%SOC +60 / C 30%SOC +60 / C 40%SOC +60 / C 50%SOC +60 / C 60%SOC +60 / C 70%SOC +60 / C 80%SOCThe charging time T, in minutes, is calculated by multiplying the battery's state of charge (SOC) by 10%. The shorter this time, the better the battery's fast charging performance.

[0145] (3) High-temperature storage performance test

[0146] At 25°C, the secondary batteries prepared in the above embodiments and comparative examples were charged at a 1C rate to the charging cutoff voltage V1, then charged at a constant voltage to a current of 0.05C, allowed to stand for 5 minutes, and then discharged at a constant current rate of 0.33C to the discharge cutoff voltage V2 to obtain the initial capacity of the battery. Then, at 25°C, the battery was charged at a 1C rate to the charging cutoff voltage V1, then charged at a constant voltage to a current of 0.05C. At this point, the battery was fully charged. The fully charged battery was stored in a constant temperature chamber at 60°C. Every 7 days, the battery was removed and discharged at a 0.33C rate to the discharge cutoff voltage V2 at 25°C, allowed to stand for 5 minutes, then charged at a 1C rate to the charging cutoff voltage V1, then charged at a constant voltage to a current of 0.05C, allowed to stand for 5 minutes, and then discharged at a constant current rate of 0.33C. The capacity of the battery at this time was tested. This process continued until the capacity decayed to 80% of the initial capacity, and the number of days of storage was recorded. (It should be noted that after each capacity test, the battery should be charged at a 1C rate to the charging cutoff voltage V1, then charged at a constant voltage to a current of 0.05C to keep the battery fully charged, and then stored in a 60℃ constant temperature chamber.)

[0147] The charge / discharge cutoff voltage range can be the battery's nominal voltage range. In the above tests,

[0148] The charge / discharge cutoff voltage range V1 to V2 of the battery using NCM622 cathode material is 2.8V to 4.35V.

[0149] The charge / discharge cutoff voltage range V1 to V2 of the battery using NCM523 cathode material is 2.8V to 4.25V.

[0150] The charge / discharge cutoff voltage range V1 to V2 of the battery using NCM811 cathode material is 2.8V to 4.2V.

[0151] The charge / discharge cutoff voltage range V1 to V2 of batteries using LFP cathode material is 2.5V to 3.65V.

[0152] Table 1

[0153]

[0154] As can be seen from the results of Examples 1 to 17, the negative electrode active material of the secondary battery provided in this application includes artificial graphite, and the artificial graphite includes secondary particles. At the same time, the cell meets a specific size design, so that the secondary battery can have a high energy density while also taking into account good fast charging performance, cycle life and high temperature storage performance.

[0155] The results of comparative examples 1 to 5 show that when the secondary battery does not simultaneously meet the technical solution of this application, the secondary battery cannot simultaneously achieve good fast charging performance, cycle life and high temperature storage performance.

[0156] The above description is merely a specific embodiment of this application, but the scope of protection of this application is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the technical scope disclosed in this application, and these modifications or substitutions should all be covered within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.

Claims

1. A secondary battery, comprising an electrode assembly, the electrode assembly including a cell and tabs extending from the cell, the cell including a negative electrode sheet, the negative electrode sheet including a negative current collector and a negative electrode film disposed on at least one surface of the negative current collector and including a negative electrode active material, wherein: The negative electrode active material includes artificial graphite, and the artificial graphite includes secondary particles; The battery cell meets the following requirements: 9cm ≤ 0.5× ≤ 15cm, 0.3 ≤ a / b ≤ 0.8, and a ≤15cm, 10cm<b ≤ 35cm; where, a is the maximum dimension of the battery cell in the direction of the tab extension, in cm; b is the maximum dimension of the battery cell in the direction perpendicular to the direction of the electrode extension, in cm; The proportion of the secondary particles in the artificial graphite satisfies 30% ≤ S ≤ 80%.

2. The secondary battery according to claim 1, wherein, The proportion of the secondary particles in the artificial graphite satisfies 50% ≤ S ≤ 80%.

3. The secondary battery according to claim 1, wherein, The battery cell meets the following requirement: 9cm ≤ 0.5× ≤13cm.

4. The secondary battery according to claim 1, wherein, 6cm ≤ a ≤ 13cm.

5. The secondary battery according to claim 1, wherein, 7cm ≤ a ≤ 12cm.

6. The secondary battery according to claim 4, wherein, 7cm ≤ a ≤ 12cm.

7. The secondary battery according to claim 1, wherein, 18cm ≤ b ≤ 25cm.

8. The secondary battery according to claim 1, wherein, 20cm ≤ b ≤ 24cm.

9. The secondary battery according to any one of claims 1-6, wherein, The artificial graphite also satisfies one or more of the following (1) to (6): (1) The particle size distribution D of the artificial graphite v 10 satisfies: 5.2μm ≤ D v 10 ≤ 8.3μm; (2) The average particle size D of the artificial graphite v 50 satisfies: 6μm ≤ Dv50 ≤ 15μm; (3) The particle size distribution D of the artificial graphite v 90 satisfies: 13μm ≤ Dv90 ≤ 30μm; (4) The specific surface area SSA of the artificial graphite satisfies: 0.6 m² 2 / g ≤ SSA ≤ 2.5 m 2 / g; (5) The compacted density of the artificial graphite powder under 2 tons of pressure is 1.5 g / cm³. 3 ~ 1.7 g / cm 3 ; (6) At least a portion of the surface of the artificial graphite has a coating layer.

10. The secondary battery according to any one of claims 1-6, wherein, The artificial graphite also satisfies one or more of the following (1) to (6): (1) The particle size distribution D of the artificial graphite v 10 satisfies: 6.6μm ≤ D v 10 ≤ 7.8 μm; (2) The average particle size D of the artificial graphite v 50 satisfies: 8μm ≤ D v 50≤ 13μm; (3) The particle size distribution Dv90 of the artificial graphite satisfies: 15μm ≤ D v 90≤ 25μm; (4) The specific surface area SSA of the artificial graphite satisfies: 0.9 m² 2 / g ≤ SSA ≤ 1.7 m 2 / g; (5) The compacted density of the artificial graphite powder under 2 tons of pressure is 1.53 g / cm³. 3 ~ 1.65 g / cm 3 ; (6) At least a portion of the surface of the artificial graphite has a coating layer.

11. The secondary battery according to any one of claims 1-6, wherein, The specific capacity of the artificial graphite is 343 mAh / g ~ 359 mAh / g.

12. The secondary battery according to any one of claims 1-6, wherein, The specific capacity of the artificial graphite is 350 mAh / g ~ 355 mAh / g.

13. The secondary battery according to any one of claims 1-6, wherein, The negative electrode film satisfies one or more of the following (1) to (4): (1) The areal density CW of the negative electrode film satisfies: 7.1 mg / cm³ 2 ≤ CW ≤ 10.4mg / cm 2 ; (2) The compaction density PD of the negative electrode film satisfies: 1.4 g / cm³ 3 ≤ PD ≤ 1.7g / cm 3 ; (3) The porosity Pa of the negative electrode membrane satisfies: 23% ≤ Pa ≤ 42%; (4) The OI value of the negative electrode film satisfies: 10 ≤ OI ≤ 30.

14. The secondary battery according to any one of claims 1-6, wherein, The negative electrode film satisfies one or more of the following (1) to (4): (1) The areal density CW of the negative electrode film satisfies: 7.8 mg / cm³ 2 ≤ CW ≤ 9.1mg / cm 2 ; (2) The compaction density PD of the negative electrode film satisfies: 1.45 g / cm³ 3 ≤ PD ≤ 1.65g / cm 3 ; (3) The porosity Pa of the negative electrode membrane satisfies: 28% ≤ Pa ≤ 37%; (4) The OI value of the negative electrode film satisfies: 14 ≤ OI ≤ 25.

15. The secondary battery according to any one of claims 1-6, wherein, The battery cell also satisfies the following condition: 0.35 ≤ a / b ≤ 0.

7.

16. The secondary battery according to any one of claims 1-6, wherein, The battery cell also satisfies the following condition: 0.4 ≤ a / b ≤ 0.

6.

17. The secondary battery according to claim 1, wherein, The battery cell also satisfies the following condition: 0.4 ≤ a / b ≤ 0.

6.

18. The secondary battery according to any one of claims 1-6, wherein, The battery cell includes a positive electrode sheet, which includes a positive current collector and a positive electrode film disposed on at least one surface of the positive current collector and including a positive active material. The positive active material includes one or more of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide and their respective modified compounds.

19. An apparatus comprising a secondary battery according to any one of claims 1-18.

Citation Information

Patent Citations

  • Lithium ion battery

    CN104779413A

  • Simulated analysis method for internal distribution characteristics of lithium ion battery of multi-layer laminated structure

    CN108169683A

  • Electrode material and secondary battery

    CN109461934A

  • Electrode material and secondary battery

    CN109704323A