Cathode electrode compositions for battery applications
By using electrode materials formed by carbon nanostructures, the problem of insufficient conductivity of cathode materials in lithium-ion batteries is solved, and the high energy density and low temperature performance are improved, reducing the use and cost of conductive additives.
Patent Information
- Application Number
- CN202080036991.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-22
- Filing Date
- 2020-02-21
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-02-21
AI Technical Summary
The low conductivity of cathode materials and the use of conductive additives in lithium-ion batteries leads to battery failure, and the dispersion of traditional carbon nanotubes is insufficient and costly, which affects battery performance.
The composition prepared from carbon nanostructures (CNS) is used as the electrode material, and the polymerized structure is formed by interleaving, branching, and crosslinking to improve conductivity and reduce the amount of conductive additives used.
Improve the conductivity and battery performance of the electrode under low conductive additives, reduce the risk of battery failure, and achieve higher energy density and low temperature performance due to the high dispersion and low cost of CNS.
Smart Images

Figure CN113841267B_ABST
Abstract
Description
[0001] Related Applications
[0002] This application claims the benefit under 35 USC 119(e) of U.S. Provisional Application No. 62 / 822,097, filed on March 22, 2019, which is hereby incorporated by reference in its entirety. Background Art
[0003] Lithium-ion batteries are a common source of electrical energy for numerous applications ranging from electronic devices to electric vehicles. A lithium-ion battery (LIB) typically includes a negative (electro) electrode and a positive (electro) electrode, which are arranged to allow lithium ions and electrons to move in and out of the electrodes during charge and discharge. An electrolyte solution in contact with the electrodes provides a conductive medium in which ions can move. To prevent direct reactions between the electrodes, an ion-permeable separator is used to physically and electrically isolate the electrodes. During operation, electrical contact is made to the electrodes, allowing electrons to flow through the device to provide power, and lithium ions move from one electrode to the other through the electrolyte.
[0004] In many cases, the negative electrode is constructed of graphite. The positive electrode typically includes a conductive substrate that supports a mixture (e.g., applied as a paste) of at least an electroactive material, a binder, and a conductive additive. The electroactive material, such as a lithium transition metal oxide, can receive and release lithium ions. Binders, such as polyvinylidene fluoride (PVDF), are used to provide mechanical integrity and stability to the electrode. Because the electroactive material and binder often show poor conductive properties or insulating properties, materials such as graphite and carbon (carbon) black (carbon black) are often added to enhance the conductivity of the electrode. Summary of the invention
[0005] Some cathode materials used in lithium-ion batteries, such as LFP, NCM, and NCA, can exhibit low electrical conductivity (conductivity), e.g. -9 Siemens / cm (S / cm)-10 -4 S / cm. To avoid battery failure, this performance can be enhanced by building a cathode with a conductive network. Some materials with the potential to enhance performance and avoid battery failure include conductive carbon black (CB) (e.g., with a grape-like morphology), and carbon nanotubes (CNTs).
[0006] Since conductive additives and binders generally do not participate in the electrochemical reactions that produce electrical energy, these materials can negatively impact certain performance characteristics of the battery (e.g., capacity and energy density) because they actually reduce the amount of electroactive material that can be contained in the volume available for the positive electrode.
[0007] To build a conductive cathode network, the amount of CB required is relatively high, typically exceeding 2 weight percent (wt%). In addition, volume expansion and contraction of the cathode can lead to loss of contact between CB particles, resulting in battery failure.
[0008] CNT can be considered as a material with the potential attractiveness to reduce the amount of additives to be introduced into the cathode composition relative to the amount of CB. Some difficulties encountered when utilizing CNT include limited dispersibility and insufficient purity in some media. It is believed that at least some of these problems are caused by strong van der Waals forces that occur between individual carbon nanotubes, thereby causing them to agglomerate into bundles or entanglements. Such performance can lead to lower than expected property enhancement and / or inconsistent performance. In some cases, relative to the enhancement expected when using original carbon nanotubes, the technology that can be used to debundle carbon nanotubes into individual, well-dispersed members can adversely affect the desired property enhancement.
[0009] Often, the low dispersion of CNTs is addressed by using an excess (i.e., more than the theoretical amount) of CNTs. However, this approach increases manufacturing costs, introduces impurities (e.g., iron and cobalt catalysts used to make CNTs), and can reduce battery capacity by reducing the battery volume available for electroactive materials.
[0010] Another difficulty is that the small size of individual carbon nanotubes raises concerns about their environmental health and safety. Also, the cost of manufacturing individual carbon nanotubes can be prohibitive for some commercial applications.
[0011] Therefore, there is a need for conductive additives that can address at least some of these problems. For example, there is a need for additives that can be used in batteries characterized by high energy density. Materials that can maintain good conductivity even when added at levels of 1 wt% or less are particularly desirable.
[0012] In some of its aspects, the present invention relates to compositions prepared from carbon nanostructures (CNS). In turn, the compositions can be used to prepare electrode compositions, such as cathode compositions for lithium ion batteries.
[0013] As used herein, the term "carbon nanostructure" or "CNS" refers to a plurality of carbon nanotubes (CNTs) that can exist as a polymeric structure by interlacing, branching, crosslinking and / or sharing a common wall with each other, in many cases, multi-walled (also referred to as multi-walled) carbon nanotubes (MWCNTs). Therefore, CNS can be considered to be the basic monomer unit of its polymeric structure with CNT such as MWCNT. Typically, CNS is grown under CNS growth conditions on a substrate (e.g., a fiber material). In such a case, at least a portion of the CNTs in the CNS can be substantially parallel to each other orientations, which is very similar to the parallel CNT orientations seen in conventional carbon nanotube bundles.
[0014] The CNS may be provided as loose particles (eg, in the form of pellets, flakes, granules, etc.) or dispersed in a suitable dispersant.
[0015] In some embodiments, the present invention relates to an electrode composition comprising an electroactive material and at least one material selected from the group consisting of carbon nanostructures, fragments of carbon nanostructures, and disrupted carbon nanotubes such as disrupted MWCNTs. In many cases, the electroactive material is a lithium transition metal compound.
[0016] One method for preparing an electrode composition includes combining a dispersion containing carbon nanostructures with an electroactive material, such as a lithium transition metal compound. Another method for preparing an electrode composition includes introducing the carbon nanostructures into a slurry containing an electroactive material, such as a lithium transition metal compound.
[0017] Further embodiments relate to electrodes and / or batteries comprising CNS, CNS fragments (which may be derived from CNS) and / or disrupted CNTs such as MWCNTs (which are derived from CNS and retain the structural features of carbon nanotube branching and a common wall).
[0018] In one implementation, a lithium battery comprises: a cathode comprising a lithium transition metal compound and a first carbon conductive additive; and an anode comprising an active anode material selected from graphite, silicon or lithium titanate and a second carbon conductive additive. The first and optionally the second carbon conductive additive are selected from: carbon nanostructures, fragments of carbon nanostructures and broken carbon nanotubes such as broken MWCNTs.
[0019] In some cases, conductive additives including one or more of CNS, CNS fragments and / or ruptured CNTs impart desired electrical properties even when the additive is introduced in relatively low amounts, such as 1 weight % (wt%) or less. It is believed that this effect is at least partially due to the formation of fragments as follows: the fragments maintain branching, thereby allowing better connectivity between them and producing enhanced electrical conductivity (conductivity) connections. In other cases, additives such as those described herein bring such cathode capacity and internal resistance: typically, when conventional additives such as CB are used, they can only be achieved at higher loadings. Relative to comparative electrode compositions (containing, for example, CB, CNT, or graphene as conductive additives), electrode additives according to the principles described herein typically will not need to use higher amounts to achieve the same or substantially the same electrical properties; in many cases, the required levels of CNS-based additives will be lower than those required when using traditional carbon additives.
[0020] In other words, the use of compositions prepared from CNS starting materials will result in electrodes that exhibit at least the same, and often improved, electrical properties relative to comparative electrode compositions formulated with conventional carbon additives such as CB, CNT, graphene, etc. at the same level of loading.
[0021] Thus, practicing aspects of the present invention can reduce the amount of conductive additive necessary to achieve certain performance, thereby enabling the manufacture of electrodes containing higher amounts of active electrode material (and lower amounts of conductive additive) in a given electrode volume. In some embodiments, the CNS used produces fragments (including partially fragmented CNS) and / or broken CNTs. These structures can provide improved connectivity between each other, thereby enhancing conductivity in the electrode.
[0022] The CNS can be provided in a form that is easy to handle and, in some embodiments, forms a stable dispersion in a desired solvent.The compositions and techniques described herein also address other problems encountered with the use of separate CNTs and / or CBs.
[0023] Cathode electrodes prepared using CNS were found to show improved low temperature performance when compared to cathodes made with pristine MWCNTs. Advantages in low temperature performance may also be associated with providing the CNS via a dispersion.
[0024] The above and other features of the present invention will now be described in more detail with reference to the accompanying drawings, including various details of the construction and combination of the parts, and other advantages, and which are pointed out in the claims. It will be understood that the specific methods and devices embodying the present invention are given as examples rather than limitations of the present invention. The principles and features of the present invention can be embodied in countless embodiments without departing from the scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In the accompanying drawings, reference numerals refer to the same parts in different figures. The drawings are not necessarily to scale; instead, emphasis is placed on illustrating the principles of the invention. In the drawings:
[0026] Figure 1A and 1B Figure 1 is a diagram illustrating the difference between Y-shaped MWCNTs and branched MWCNTs. Y-shaped MWCNTs are not in or derived from carbon nanostructures ( Figure 2A ); branched MWCNT ( Figure 2B ) in carbon nanostructures;
[0027] Figure 2A and 2B TEM images showing features that characterize multi-walled carbon nanotubes found in carbon nanostructures;
[0028] Figure 2C and 2D This is a SEM image showing the presence of multiple branches in a carbon nanostructure.
[0029] Figure 3A is an illustrative depiction of a carbon nanostructure sheet material after separation of the carbon nanostructure from a growth substrate;
[0030] Figure 3B is a SEM image of an illustrative carbon nanostructure obtained as a thin-sheet material;
[0031] Figure 4 series of graphs showing the resistance of cathodes prepared with no greater than 1.5 wt % CNS loading compared to the resistance of cathodes prepared with 2 wt % and 4 wt % CB loading;
[0032] Figure 5 A series of graphs comparing the discharge capacities of electrodes prepared with 0.25 wt % CNS, 2 % CB, and 4 % CB;
[0033] Figure 6 A series of graphs showing the direct current internal resistance (DCIR) obtained at different states of charge (SOC) for coin cell cells made with cathodes containing 0.25 wt % CNS and comparative 2 wt % and 4 wt % carbon additives;
[0034] Figure 7 The in-plane resistance and thru plane conductivity of NCM622 cathodes containing 0.5% CNS, 0.5% CNT or 1% carbon black (CB) are shown.
[0035] Figure 8Graph showing the electrode vertical resistivity obtained from cathode sheets on aluminum foil prepared with selected CCA types and coated on aluminum foil as a function of CCA weight % ranging from 0.1 wt % to 1.0 wt %;
[0036] Fig. 9 is a graph showing the vertical resistivity of selected NCM electrodes coated on aluminum foil containing 0.5 wt % of the conductive additive disclosed herein;
[0037] Fig.10 Graphs showing 0.5C and 2C discharge capacity and HPPC DC-IR at 50% state of charge (SOC) of half coin cell cells with NCM622 cathodes using the conductive additives disclosed herein;
[0038] Fig.11 Graph showing retention of 1C discharge capacity at -10°C relative to 1C discharge capacity at +25°C for half coin cell cells having NCM622 cathodes using the conductive additives disclosed herein. DETAILED DESCRIPTION
[0039] The present invention will be described more fully hereinafter with reference to the accompanying drawings in which illustrative embodiments of the present invention are shown. However, the present invention can be embodied in many different forms and should not be construed as limited to the description set forth herein; on the contrary, these embodiments are provided so that this disclosure will be thorough and complete and will fully convey the scope of the invention to those skilled in the art.
[0040] In general, the present invention relates to compositions useful for making electrodes for batteries, methods for making the compositions, and uses of the compositions in electrodes (e.g., cathodes) and batteries. In many of its aspects, the present invention relates to compositions suitable for lithium-ion batteries. In one example, the battery of interest is a rechargeable lithium-ion battery.
[0041] Examples of various types of lithium-ion batteries (according to the acronyms of the electroactive materials used (often intercalation compounds)) include: LCO (lithium cobalt oxide), LMO (lithium manganese oxide), NCM (lithium nickel cobalt manganese oxide), NCA (lithium nickel cobalt aluminum oxide), LCP (lithium cobalt phosphate), LFP (lithium iron phosphate), LFSF (lithium fluoroferric sulfate), LTS (lithium titanium sulfide), and others as known in the art or as developed in the future. Materials such as these are collectively referred to herein as "lithium transition metal compounds", such as "lithium transition metal oxides".
[0042] Some embodiments relate to a composition consisting of, consisting essentially of, or comprising a conductive additive. The composition is combined with an active electrode material (e.g., NCM or NCA) with or without a binder to form an electrode composition in the form of a slurry, typically a paste, which can be applied to a current collector to form an electrode. The electrode can be used to make a battery.
[0043] In many of its aspects, the present invention relates to compositions prepared using: carbon nanostructures (multiple CNS, single CNS), which is a term used herein to refer to a plurality of carbon nanotubes (CNTs) cross-linked into a polymeric structure by branching (e.g., in dendritic form), interlacing, entanglement, and / or sharing a common wall with each other. The operations performed to prepare the compositions, electrodes, and / or batteries described herein may produce CNS fragments and / or ruptured CNTs. Fragments of CNS are derived from CNSs and, like larger CNSs, include a plurality of CNTs cross-linked into a polymeric structure by branching, interlacing, entanglement, and / or sharing a common wall. Ruptured CNTs are derived from CNSs that are branched and share a common wall with each other.
[0044] Highly entangled CNS is visible to the naked eye in size and can be considered to have carbon nanotubes (CNTs) as the basic monomer units of its polymeric structure. For many CNTs in the CNS structure, at least a portion of the CNT sidewall is shared with other CNTs. Although it is generally understood that each carbon nanotube in the CNS does not necessarily need to be branched, crosslinked or share a common wall with other CNTs, at least a portion of the CNTs in the carbon nanostructure can be interlaced with each other and / or with branched, crosslinked, or co-walled carbon nanotubes in the carbon nanostructure of the remainder.
[0045] As is known in the art, a carbon nanotube (a CNT or a plurality of CNTs) is a nanotube comprising at least one sheet of sp 2 Carbonaceous material of hybridized carbon atoms: they are bonded to each other to form a honeycomb lattice that forms a cylindrical or tubular structure. Carbon nanotubes can be single-walled carbon nanotubes (SWCNTs) or multi-walled carbon nanotubes (MWCNTs). SWCNTs can be considered sp similar to fullerenes. 2 Allotropes of hybridized carbon. The structure is a cylindrical tube comprising a six-membered carbon ring. On the other hand, similar MWCNTs have several tubes in the form of concentric cylinders. The number of these concentric walls can vary, for example, from 2 to 25 or more. Typically, MWNTs can have a diameter of 10 nm or more, compared to a typical SWNT of 0.7-2.0 nm.
[0046] In many CNS used in the present invention, the CNT is a MWCNT having, for example, at least 2 coaxial carbon nanotubes. The number of walls present, as determined, for example, by transmission electron microscopy (TEM) at a magnification sufficient to analyze the number of walls in a particular case, can range from about 2-30, for example: 4-30; 6-30; 8-30; 10-30; 12-30; 14-30; 16-30; 18-30; 20-30; 22-30; 24-30; 26-30; 28-30; or 2-28; 4-28; 6-28; 8-28 ; 10-28; 12-28; 14-28; 16-28; 18-28; 20-28; 22-28; 24-28; 26-28; or 2-26; 4-26; 6-26; 8-26; 10-26; 12-26; 14-26; 16-26; 18-26; 20-26; 22-26; 24-26; or 2-24; 4-24; 6-24; 8-24; 10-24; 12-24; 14-24 ; 16-24; 18-24; 20-24; 22-24; or 2-22; 4-22; 6-22; 8-22; 10-22; 12-22; 14-22; 16-22; 18-22; 20-22; or 2-20; 4-20; 6-20; 8-20; 10-20; 12-20; 14-20; 16-20; 18-20; or 2-18; 4-18; 6-18; 8-18; 10-18; 12 -18; 14-18; 16-18; or 2-16; 4-16; 6-16; 8-16; 10-16; 12-16; 14-16; or 2-14; 4-14; 6-14; 8-14; 10-14; 12-14; or 2-12; 4-12; 6-12; 8-12; 10-12; or 2-10; 4-10; 6-10; 8-10; or 2-8; 4-8; 6-8; or 2-6; 4-6; or 2-4.
[0047] Since CNS are polymeric, highly branched and cross-linked networks of CNTs, some of the chemical properties observed for individualized CNTs can also be realized on CNS. In addition, some of the attractive properties often associated with the use of CNTs are also displayed in materials incorporating CNS. These include, for example, electrical conductivity; attractive physical properties including: good tensile strength, thermal stability (sometimes comparable to that of diamond crystals or in-plane graphene sheets) and / or chemical stability, to name a few, when incorporated into composites such as thermoplastic or thermosetting compounds (compounds).
[0048] However, as used herein, the term "CNS" is not synonymous with individualized, unentangled structures such as "monomeric" fullerenes (the term "fullerene" refers broadly to hollow spheres, tubes such as carbon nanotubes, and other shaped allotropes of carbon). In fact, many embodiments of the present invention highlight observed or expected differences and advantages when using CNS as opposed to using its CNT building blocks. Without wishing to be bound by a specific explanation, it is believed that the combination of branching, crosslinking, and common walls between carbon nanotubes in CNS reduces or minimizes van der Waals forces, which are often problematic when individual carbon nanotubes are used in a similar manner.
[0049] In addition or alternatively, with respect to performance properties, CNTs that are part of or derived from a CNS may be characterized by a number of features, at least some of which may be relied upon to distinguish them from nanomaterials such as ordinary CNTs (i.e., CNTs that are not derived from a CNS and may be provided as individualized, pristine or fresh CNTs).
[0050] In many cases, CNTs present in or derived from the CNS have a typical diameter of 100 nanometers (nm) or less, such as in the range of about 5 to about 100 nm, such as in the range of about 10 to about 75, about 10 to about 50, about 10 to about 30, about 10 to about 20 nm.
[0051] In various embodiments, at least one of the CNTs has a length equal to or greater than 2 microns, as determined by SEM. For example, at least one of the CNTs has a length in the following ranges: 2-2.25 microns; 2-2.5 microns; 2-2.75 microns; 2-3.0 microns; 2-3.5 microns; 2-4.0 microns; or 2.25-2.5 microns; 2.25-2.75 microns; 2.25-3 microns; 2.25-3.5 microns; 2.25-4 microns; or 2.5-2.75 microns; 2.5-3 microns; 2.5-3.5 microns; 2.5-4 microns; or 3-3.5 microns; 3-4 microns; 3.5-4 microns or more. In some embodiments, more than one, e.g., a portion, e.g., at least about 0.1%, at least about 1%, at least about 10%, at least about 15%, at least about 20%, at least about 25%, at least about 30%, at least about 35%, at least about 40, at least about 45%, at least about 50%, or even more than half, of the CNTs may have a length greater than 2 microns, e.g., within the above ranges, as determined by SEM.
[0052] The morphology of CNTs present in CNS, in fragments of CNS, or in ruptured CNTs derived from CNS will generally be characterized by a high aspect ratio, wherein the length is typically greater than 100 times the diameter, and in some cases even higher. For example, in CNS (or CNS fragments), the aspect ratio of the length to the diameter of the CNTs may be in the range of about 200 to about 1000, such as 200-300; 200-400; 200-500; 200-600; 200-700; 200-800; 200-900; or 300-400; 300-500; 300-600; 300-700; 300-800; 300-900; 300-1000; or 400-500 0; 400-600; 400-700; 400-800; 400-900; 400-1000; or 500-600; 500-700; 500-800; 500-900; 500-1000; or 600-700; 600-800; 600-900; 600-1000; 700-800; 700-900; 700-1000; or 800-900; 800-1000; or 900-1000.
[0053] It has been found that in CNS, and in structures derived from CNS (e.g., in fragments of CNS or in broken CNTs), at least one feature of CNTs is a certain "branch density". As used herein, the term "branch" refers to a feature in which a single carbon nanotube branches into multiple (two or more), connected multi-walled carbon nanotubes. An embodiment has the following branch density: according to the branch density, along the 2 micron length of the carbon nanostructure, there are at least two branches, as determined by SEM. Three or more branches may also occur.
[0054] Further features (detected using, for example, TEM or SEM) can be used to characterize the type of branching found in CNS relative to structures not derived from CNS, such as Y-shaped CNTs. For example, while Y-shaped CNTs have catalyst particles at or near branching regions (points), such catalyst particles are not present at or near branching regions that occur in CNSs, fragments of CNSs, or broken CNTs.
[0055] Additionally or alternatively, the number of walls observed at a branching region (point) in a CNS, a fragment of a CNS, or a ruptured CNT varies from one side of the branch (e.g., before the branching point) to the other side of the region (e.g., after or past the branching point). Such a variation in the number of walls, also referred to herein as "asymmetry" in the number of walls, is not observed for normal Y-shaped CNTs (where the same number of walls is observed in both the region before the branching point and the region after the branching point).
[0056] Figure 1A and 1B A diagram illustrating these features is provided in . Figure 1A 1 is an exemplary Y-shaped CNT 11 that is not derived from a CNS. The Y-shaped CNT 11 includes a catalyst particle 13 at or near a branch point 15. Regions 17 and 19 are located before and after the branch point 15, respectively. In the case of a Y-shaped CNT such as Y-shaped CNT 11, both regions 17 and 19 are characterized by the same number of walls, i.e., two walls in this figure.
[0057] In contrast, in the CNS, the CNT building block 111 that branches at branch point 115 does not include catalyst particles at or near that point, as seen in catalyst-free region 113. In addition, the number of walls present in region 117, located before, in front of (or on a first side of) branch point 115, is different from the number of walls in region 119, located past, after, or on the other side of branch point 115. In more detail, the three-wall feature found in region 117 is not carried through to region 119, which is located after branch point 115. Figure 1B ), resulting in the asymmetry mentioned above.
[0058] exist Figure 2A and 2B TEM images and Figure 2C-2D These features are highlighted in the SEM images of the .
[0059] In more detail, Figure 2A The TEM area 40 of the CNS branching shows the absence of any catalyst particles. Figure 2B In the TEM of FIG. 1 , the first channel 50 and the second channel 52 show the asymmetry in the number of walls that is characteristic of branched CNS, while arrows 54 indicate regions showing shared walls. Figure 2C and 2D Multiple branches are seen in SEM areas 60 and 62, respectively.
[0060] One, more than one, or all of these attributes may be encountered in the compositions (eg, dispersions, slurries, pastes, solid or dried compositions, etc.), electrodes, and / or batteries described herein.
[0061] In some embodiments, a CNS exists as part of a tangle and / or interconnected network of CNSs. Such an interconnected network may contain bridges between CNSs.
[0062] Suitable techniques for preparing CNS are described, for example, in U.S. Patent Application Publication No. 2014 / 0093728A1, published on April 3, 2014; U.S. Patent Nos. 8,784,937B2; 9,005,755B2; 9,107,292B2; and 9,447,259B2. The entire contents of these documents are incorporated herein by reference.
[0063] As described in these documents, CNS can be grown on a suitable substrate, for example, on a catalyst-treated fiber material. The product can be a fiber-containing CNS material. In some cases, the CNS is separated from the substrate to form a sheet.
[0064] As seen in US2014 / 0093728A1, the carbon nanostructure obtained as a thin sheet material (that is, discrete particles with limited scale) exists as a three-dimensional microstructure due to the entanglement and crosslinking of its highly oriented carbon nanotubes. This orientation morphology reflects the formation of carbon nanotubes under fast carbon nanotube growth conditions (for example, several micrometers / second, for example, about 2 micrometers / second-about 10 micrometers / second) on the growth substrate, thereby causing substantially vertical carbon nanotube growth from the growth substrate. Not subject to any theory or mechanism constraints, it is believed that the fast carbon nanotube growth rate on the growth substrate can at least partially contribute to the complex structural morphology of the carbon nanostructure. In addition, by adjusting the carbon nanostructure growth conditions, including, for example, by changing the concentration of the transition metal nanoparticle catalyst particles arranged on the growth substrate to cause carbon nanotube growth, the packing density of CNS can be regulated to some extent.
[0065] The flakes may be further processed, for example by cutting or fluffing (operations that may involve mechanical milling, grinding, blending, etc.), chemical processing, or any combination thereof.
[0066] In some embodiments, the CNS employed is a "coated", also referred to herein as "sizing", or "encapsulated" CNS. In a typical sizing process, a coating is applied to the CNTs that form the CNS. The sizing process can form a partial or complete coating that is non-covalently bound to the CNTs and can act as a binder in some cases. In addition, or alternatively, a sizing agent can be applied to the already formed CNS in a post-coating process. In the case of using a sizing agent with adhesive properties, the CNS can be formed into larger structures, such as granules or pellets. In other embodiments, the granules or pellets are formed independently of the sizing function.
[0067] The amount of coating can vary. For example, the coating layer can be in the range of about 0.1 wt % to about 10 wt % (e.g., in the range of about 0.1% to about 0.5%; about 0.5% to about 1%; about 1% to about 1.5%; about 1.5% to about 2%; about 2% to about 2.5%; about 2.5% to about 3%; about 3% to about 3.5%; about 3.5% to about 4%; about 4% to about 4.5%; about 4.5% to about 5%; about 5% to about 5.5%; about 5.5% to about 6%; about 6% to about 6.5%; about 6.5% to about 7%; about 7% to about 7.5%; about 7.5% to about 8%; about 8% to about 8.5%; about 8.5% to about 9%; about 9% to about 9.5%; or about 9.5% to about 10% by weight, relative to the total weight of the coated CNS material.
[0068] In many cases, controlling the amount of coating (or sizing agent) reduces or minimizes the undesirable effects on the properties of the CNS material itself. Low coating levels, for example, are more likely to maintain the electrical properties brought about by introducing CNS or CNS-derived materials (e.g., CNS fragments of broken CNTs) materials into the cathode composition.
[0069] Can select various types of coating layer.In many cases, also can utilize the sizing solution commonly used when coating carbon fiber or glass fiber to coat CNS.The specific example of coating material includes but is not limited to fluorinated polymer such as poly (vinyl difluoride) (PVDF), poly (vinyl difluoride-co-hexafluoropropylene) (PVDF-HFP), poly (tetrafluoroethylene) (PTFE), polyimide, and water-soluble binder such as polyoxy (ethylene), polyvinyl alcohol (PVA), cellulose, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone (PVP), and copolymers and mixtures thereof.In many implementations, the CNS used is polyurethane (PU), thermoplastic polyurethane (TPU) or is processed with polyethylene glycol (PEG).
[0070] In some cases, polymers such as epoxy resins, polyesters, vinyl esters, polyetherimides, polyetherketoneketones, polyphthalamides, polyetherketones, polyetheretherketones, polyimides, phenol-formaldehyde, bismaleimide, acrylonitrile-butadiene styrene (ABS), polycarbonates, polyethyleneimines, polyurethanes, polyvinyl chlorides, polystyrenes, polyolefins, polypropylenes, polyethylenes, polytetrafluoroethylenes, elastomers such as polyisoprene, polybutadiene, butyl rubbers, nitrile rubbers, ethylene-vinyl acetate polymers, silicone polymers, and fluorinated silicone polymers, combinations thereof, or other polymers or polymer blends may also be used. To enhance conductivity, conductive polymers such as polyanilines, polypyrroles, and polythiophenes may also be used.
[0071] Some implementations employ coating materials that can assist in stabilizing the dispersion of CNS in a solvent. In one example, the coating layer is selected to promote and / or stabilize the dispersion of CNS in a medium comprising, consisting essentially of, or consisting of: N-methylpyrrolidone (NMP), acetone, a suitable alcohol, water, or any combination thereof.
[0072] Many embodiments described herein use CNS materials having a CNT purity of 97% or higher. Typically, anionic, cationic, or metallic impurities are very low, for example, in the range of several parts per million (ppm). Often, the CNS used herein do not require further additives to counteract van der Waals forces.
[0073] The CNS may be provided in the form of loose particulate material (as, for example, CNS flakes, granules, pellets, etc.) or in a composition further comprising a liquid medium, such as a dispersion, slurry, paste, or in other forms. In many implementations, the CNS employed does not contain any growth substrate.
[0074] In some embodiments, the CNS is provided in the form of a flake material after removal from a growth substrate on which the carbon nanostructures are initially formed. As used herein, the term "flake material" refers to discrete particles having a finite size. Figure 1A is an illustrative depiction of a CNS flake material after separating the CNS from the growth substrate. The flake structure 100 may have a first dimension 110 in the range of about 1 nm to about 35 μm thick, particularly about 1 nm to about 500 nm thick, including any value between and any portion thereof. The flake structure 100 may have a second dimension 120 in the range of about 1 micron to about 750 microns high, including any value between and any portion thereof. The flake structure 100 may have a third dimension 130 that may be in the range of about 1 micron to about 750 microns, including any value between and any portion thereof. Two or all of the dimensions 110, 120, and 130 may be the same or different.
[0075] For example, in some embodiments, the second dimension 120 and the third dimension 130 may independently be approximately 1 micron to approximately 10 microns, or approximately 10 microns to approximately 100 microns, or approximately 100 microns to approximately 250 microns, approximately 250 to approximately 500 microns, or approximately 500 microns to approximately 750 microns.
[0076] The CNTs within the CNS can vary in length, for example, from about 10 nanometers to about 750 micrometers. In illustrative implementations, the CNTs are about 10 nanometers to about 100 nanometers, about 100 nanometers to about 500 nanometers, about 500 nanometers to about 1 micrometer, about 1 micrometer to about 10 micrometers, about 10 micrometers to about 100 micrometers, about 100 micrometers to about 250 micrometers, about 250 to about 500 micrometers, or about 500 micrometers to about 750 micrometers.
[0077] Figure 1B Shown in is a SEM image of an illustrative carbon nanostructure obtained as a thin-plate material. Figure 1B The carbon nanostructure shown in exists as three-dimensional microstructure due to the entanglement and crosslinking of its highly oriented carbon nanotube.This orientation morphology reflects that on growth substrate, under fast carbon nanotube growth conditions (for example, several micrometers / seconds, for example about 2 micrometers / second-about 10 micrometers / seconds), carbon nanotubes are formed, thereby causes vertical carbon nanotube growth basically from growth substrate.Not subject to any theory or mechanism restriction, it is believed that on growth substrate, fast carbon nanotube growth rate can at least partially contribute to the complex structure morphology of carbon nanostructure.In addition, by regulating carbon nanostructure growth conditions, comprise for example by changing the concentration of the transition metal nanoparticle catalyst particle that is arranged on growth substrate to cause carbon nanotube growth, the packing density of carbon nanostructure can be regulated to a certain extent.
[0078] The lamella structure may include a reticulated network of carbon nanotubes in the form of a carbon nanotube polymer (i.e., a "carbon nanopolymer") having a molecular weight in the following range: about 15,000 g / mol to about 150,000 g / mol, including all values therebetween and in any portion thereof. In some cases, the upper limit of the molecular weight range may be even higher, including about 200,000 g / mol, about 500,000 g / mol, or about 1,000,000 g / mol. This higher molecular weight may be associated with a carbon nanostructure that is long in scale. The molecular weight may also be a function of the dominant carbon nanotube diameter and the number of carbon nanotube walls present in the carbon nanostructure. The crosslinking density of the carbon nanostructure may range from about 2 mol / cm 3 -About 80mol / cm 3Typically, the cross-link density is a function of the carbon nanostructure growth density, carbon nanostructure growth conditions, etc. on the growth substrate surface. It should be noted that the typical CNS structure (which contains many, many CNTs maintained in an open network arrangement) has removed the van der Waals forces or reduced their influence. The structure can be more easily peeled off, which makes them separate or destroy them into many other steps of branched structures unique and different from ordinary CNT.
[0079] In the case of a network-like morphology, the carbon nanostructure may have a relatively low packing density. The produced carbon nanostructure may have a density in the range of about 0.003 g / cm 3 -About 0.015g / cm 3 Further consolidation and / or coating to produce carbon nanostructure sheet materials or similar morphologies can increase the packing density to about 0.1 g / cm 3 -About 0.15g / cm 3 In some embodiments, the optional further modification of the carbon nanostructure can be carried out to further change the packing density and / or other properties of the carbon nanostructure. In some embodiments, the packing density of the carbon nanostructure can be further changed by forming a coating on the carbon nanotubes of the carbon nanostructure and / or infiltrating the inside of the carbon nanostructure with various materials. The inside of the carbon nanotube coating and / or infiltrating the carbon nanostructure can be further designed for the properties of the carbon nanostructure in various applications. In addition, forming a coating on the carbon nanotube can desirably promote the operation (processing) of the carbon nanostructure. Further compaction can increase the packing density to about 1 g / cm 3 The upper limit of the carbon nanostructure is increased by chemical modification to increase the bulk density to about 1.2 g / cm 3 upper limit.
[0080] In addition to the above-mentioned flakes, the CNS material can be provided as granules, pellets, or other forms of loose particulate materials having a typical particle size in the range of about 1 mm to about 1 cm, for example, about 0.5 mm to about 1 mm, about 1 mm to about 2 mm, about 2 mm to about 3 mm, about 3 mm to about 4 mm, about 4 mm to about 5 mm, about 5 mm to about 6 mm, about 6 mm to about 7 mm, about 7 mm to about 8 mm, about 8 mm to about 9 mm, or about 9 mm to about 10 mm.
[0081] The bulk density of the CNS material that can be used can be about 0.005 g / cm 3 -About 0.1g / cm 3 , for example, about 0.01 g / cm 3 -About 0.05g / cm 3 within the range.
[0082] Examples of commercially available CNS materials are those developed by Applied Nanostructured Solutions, LLC (ANS) (Massachusetts, United States).
[0083] The CNS used herein can be confirmed and / or characterized by a variety of techniques. For example, electron microscopy, including techniques such as transmission electron microscopy (TEM) and scanning electron microscopy (SEM) can provide information about, the CNS used herein can be confirmed and / or characterized by a variety of techniques. For example, electron microscopy, including techniques such as transmission electron microscopy (TEM) and scanning electron microscopy (SEM) can provide information about features such as the frequency of the specific number of walls present, branching, the absence of catalyst particles, etc. See, e.g. Figures 2A-2D .
[0084] Raman spectroscopy can reveal bands associated with impurities. For example, the D-band (about 1350 cm -1 ) is associated with amorphous carbon; the G band (about 1580 cm -1 ) is associated with crystalline graphite or CNTs). The G′ band (about 2700 cm -1 ) appears at about 2 times the frequency of the D band. In some cases, it may be possible to distinguish CNS and CNT structures by thermogravimetric analysis (TGA).
[0085] In some embodiments, the CNS is used with additional CCAs such as CBs and / or individualized, pristine CNTs, ie, CNTs that are not generated or derived from the CNS, such as during processing.
[0086] In many cases, the CB particles employed have a particle size of no greater than about 200, 180, 160, 140, 120, 100, 80, 60, or 50 m 2 In some embodiments, the CB particles have a BET surface area in the range of about 200 to about 180 m 2 / g; about 200-about 160m 2 / g; 200-about 140m 2 / g; about 200-120m 2 / g; about 200-about 100m 2 / g, about 200-about 80m 2 / g; about 200-about 60m 2 / g; about 200-about 50m 2 / g; or about 180-about 160m 2 / g; about 180-about 140m 2 / g; about 180-about 120m 2 / g; about 180-about 100m 2 / g, 180-about 80m 2 / g; about 180-about 60m 2 / g; 180-about 50m 2 / g; or about 160-about 140m 2 / g; about 160-about 120m 2 / g; about 160-100m 2 / g, 160-about 80m 2 / g; about 160-about 60m 2 / g; 160-about 50m 2 / g; or about 140-about 120m 2 / g; or about 140-about 100m 2 / g, 140-about 80m 2 / g; about 140-about 60m 2 / g; 140-about 50m 2 / g; or about 120-about 100m 2 / g, 120-about 80m 2 / g; about 120-about 60m 2 / g; 120-about 50m 2 / g; or about 100-about 80m 2 / g; about 100-about 60m 2 / g; 100-about 50m 2 / g; or about 80-about 60m 2 / g; 80-about 50m 2 / g; or about 60-about 50m 2 All BET surface area values disclosed herein refer to "BET nitrogen surface area" and are determined by ASTM D6556-10 (which is incorporated herein by reference in its entirety).
[0087] Suitable CBs may have an oil absorption number (OAN) of at least 130 mL / 100 g, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, or 250 mL / 100 g. Exemplary CBs have an OAN in the following ranges: about 130 to about 150 mL / 100 g; about 130 to about 170 mL / 100 g; about 130 to about 190 mL / 100 g; about 130 to about 210 mL / 100 g; about 130 to about 230 mL / 100 g; 130 to about 250 mL / 100 g or more; or about 150 to about 170, about 150 to about 190; about 150 to about 210; about 150 to about 230 mL / 100 g; about 150 to about 250 mL / 100 g or more. 100g or more; or 170 to about 190mL / 100g; about 170 to about 210; about 170 to about 230mL / 100g; about 170 to about 250mL / 100g or more; or about 190 to about 210mL / 100g; about 190 to about 230mL / 100g; about 190 to about 250mL / 100g or more; or about 210 to about 230mL / 100g; about 210 to about 250mL / 100g or more; or about 230 to about 250mL / 100g or more. All OAN values listed herein are determined by the method described in ASTM D 2414-16 (which is incorporated herein by reference).
[0088] Carbon black particles can also be characterized by their statistical thickness surface area (STSA), which is a property that can be measured by ASTM D 6556-10. For a given carbon black, it may also be meaningful in some cases to specify the ratio of its STSA to its BET surface area (STSA:BET ratio). For the present application, the STSA:BET ratio of the carbon black particles can be in the range of about 0.3 to about 1.
[0089] The crystal domains can be determined by L as determined by Raman spectroscopy. a Crystallite size characterization. a It is defined as 43.5×(G band area / D band area). Crystallite size can give an indication of the degree of graphitization, where the higher the L a The value is associated with a higher degree of graphitization. a The Raman measurements are based on Gruber et al., "Raman studies of heat-treated carbon blacks", Carbon 32(7), pp. 1377-1382, 1994, which is incorporated herein by reference. The Raman spectrum of carbon includes a wavelength of about 1340 cm -1 and 1580cm -1There are two main "resonance" bands at , which are denoted as "D" and "G" bands. It is generally believed that the D band is attributed to the disordered sp 2 carbon, and the G band is attributed to graphitic or "ordered" sp 2 Carbon. Using empirical methods, the ratio of the G / D bands and the L measured by X-ray diffraction (XRD) a are highly correlated, and regression analysis gives the following empirical relationship:
[0090] L a =43.5×(G band area / D band area),
[0091] Where L a is measured in angstroms. Therefore, the higher the L a The higher the value, the more ordered the crystalline structure.
[0092] In some embodiments, the carbon black has a value less than or equal to For example L a Crystallite size. L a The crystallite size may have or include, for example, one of the following ranges: or or or or or or or or or or or or or In certain embodiments, L a The crystallite size can be less than or equal to or less than or equal to or less than or equal to or less than or equal to
[0093] The crystal domain can be c Crystallite size characterization. cCrystallite size is measured by X-ray diffraction using a copper tube, a tube voltage of 45kV, and a tube current of 40mA using an X-ray diffraction instrument (PANalyticalX'Pert Pro, PANalytical BV). The sample of carbon black particles is loaded in a sample holder (accessory of the diffractometer) and measured at a speed of 0.14° / min within an angle (2θ) range of 10°-80°. Peak position and half-peak full width are calculated by the software of the diffractometer. For measurement angle calibration, lanthanum hexaboride (LaB6) is used as an X-ray standard. From the obtained measurement results, L is determined using the Scherrer equation c Crystallite size: where K is the shape factor constant (0.9); λ is Cu K a1 The wavelength of the characteristic X-ray line β is the peak width at half-peak, in radians; and θ is determined by taking half the measured angular peak position (2θ).
[0094] In some embodiments, the carbon black has a value less than or equal to For example L c Crystallite size. L c The crystallite size may have or include, for example, one of the following ranges: or or or or or or or or or or or or or or or or or or or In certain embodiments, L c The crystallite size can be less than or equal to or less than or equal to or less than or equal to or less than or equal to or less than or equal to
[0095] The carbon black particles may have a high degree of graphitization as indicated by a high % crystallinity, which is measured by Raman as the ratio of the G band area to the G and D band areas (I G / IG+D ). In certain embodiments, the carbon black particles have a % crystallinity (I) in the range of about 25% to about 45% as determined by Raman spectroscopy. G / I G+D ). % crystallinity (I G / I G+D ) may have or include, for example, one of the following ranges: 25%-43%, 25%-41%, 25%-37%, 25%-39%, 25%-35%, 25%-30%, 25%-28%; or 30%-45%, 30%-43%, 30%-39%, 30%-35%; or 35%-45%, 35%-41%, 35%-39%; or 37%-45%, 37%-43%, 37%-41%; or 39%-45%, 39%-43%; or 41%-45%, or 41%-43%.
[0096] Some CB specifications characterized by these and / or other properties known and recognized by those skilled in the art are shown in Table 1 as Specifications AF.
[0097] Table 1
[0098]
[0099] Suitable CB particles that can be utilized are commercially available particles. Examples include those available from Cabot Corporation. 50. 66. 200, 300, HP and 500 Carbon black pellets; C-NERGY from Imerys TM C45, C-NERGY TM C65 and products; Li-400, Li-250, Li-100 and Li-435 products from Denka; and EC300 products from Ketjen.
[0100] Other materials that can be used with CNS are exemplified by the specification LN (Table 2 below) describing an exemplary CNT:
[0101] Table 2
[0102]
[0103] The values presented in Table 2 were typically determined using the techniques described above for CB.
[0104] In many cases, the CNS material (in the form of, for example, flakes, pellets, granules) is provided in combination with a liquid medium or in the presence of a liquid medium. Typically, the liquid medium may be any liquid, such as a solvent, suitable for use with the constituents of the composition described herein and capable of being used to manufacture the intended electrode. The solvent may be anhydrous, polar and / or aprotic. In some embodiments, the solvent has high volatility so that during manufacture, it can be easily removed (e.g., evaporated), thereby reducing drying time and manufacturing costs. Suitable examples include, but are not limited to, N-methylpyrrolidone (NMP), acetone, a suitable alcohol, water, or any combination thereof.
[0105] In some cases, the composition further includes one or more dispersants (eg, cellulosic dispersants), and / or one or more additives, typically non-conductive additives, such as maleic anhydride polymers.
[0106] Dispersants generally include materials that are capable of facilitating the dispersion of CNS in a solvent (e.g., via steric hindrance mechanisms and / or electrostatic charge mechanisms) while maintaining the viscosity of the composition low enough to enable practical processing of the composition, such as for use in making electrodes for batteries. In some embodiments, for compositions including CNS, the dispersant, polymer, and solvent have a viscosity at 450 s as measured by a rheometer. -1 The shear rate is equal to or less than 200 centipoise (cP), for example, at 450s -1 At least 30 cP at a shear rate of 450 s -1 The composition may be referred to as a slurry, such as a paste, that can be easily applied or coated to a conductive substrate to form an electrode, in contrast to a slurry that is too thick or too viscous to be effectively applied during manufacture. In addition to its ability to disperse CNS materials, the dispersant is preferably thermally stable, electrochemically inert, and / or rarely hinders the conductivity of the CNS material. Thermally stable or non-volatile dispersants allow solvents (e.g., N-methylpyrrolidone, water, etc.) to be removed and recycled without removing and / or decomposing the dispersant during electrode manufacture. "Electrochemically inert" means that the dispersant is stable during normal use of the battery (e.g., not decomposed or oxidized at or below the operating voltage of the battery) because such decomposition can negatively affect the performance of the battery. In addition, since the dispersant coats at least a portion of the CNS flakes, granules, pellets, etc. to disperse the particles, the dispersant can hinder or reduce the conductive contact surface available for the particles. Therefore, it is preferred to select a dispersant that does little to interfere with the conductivity of the CNS particles.In embodiments where the composition further comprises one or more electroactive materials, the dispersant (eg, polyvinyl pyrrolidone) can reduce the deposition and / or phase separation of the electroactive materials.
[0107] Examples of suitable dispersants include poly(vinyl pyrrolidone), poly(vinyl pyrrolidone-co-vinyl acetate), poly(vinyl butyral) (or PVB), poly(vinyl alcohol), poly(ethylene oxide), poly(propylene oxide), poly(propylene carbonate), cellulosic dispersants such as methyl cellulose, carboxymethyl cellulose, ethyl cellulose, hydroxymethyl cellulose and hydroxypropyl cellulose; poly(carboxylic acids) such as poly(acrylic acid), polyacrylates, poly(methyl acrylate), poly(acrylamide), amide waxes, styrene maleic anhydride resins, octylphenol ethoxylates, multifunctional co-dispersants such as AMP TM Dispersants, including 2-amino-2-methyl-1-propanol, various derivatives and others known in the art. The composition may include one or more than one dispersant or one or more than one dispersant formulation.
[0108] In one example, the dispersant belongs to a class that includes styrene maleic anhydride resins and / or its derivatives, which are polymers made via chemical reactions of styrene maleic anhydride resins or pre-hydrolyzed styrene maleic anhydride resins with small or large organic molecules having at least one reactive terminal group, such as an amine or epoxy group. Typically, this class of polymeric dispersants (also referred to herein as styrene maleic anhydride-based) has a styrene maleic anhydride copolymer backbone modified with various polymeric brushes and / or small molecules.
[0109] In another example, the dispersant includes PVP (of various molecular weights) or its derivatives, the latter generally referring to dispersants having a PVP backbone modified with small or large molecules, such as by chemical reactions. Examples of PVP-based dispersants include Ashland PVP K-12, K-15, K-30, K-60, K-90 and K-120 products, polyvinyl pyrrolidone copolymers such as polyvinyl pyrrolidone-co-vinyl acetate, butylated polyvinyl pyrrolidone such as Ganex TM P-904LC polymer.
[0110] In a further example, the dispersant is a cellulose-based dispersant, including, for example, cellulose or a cellulose derivative having a cellulose backbone optionally modified by a small or large organic molecule having at least one reactive end group. In a specific example, the cellulose-based dispersant is CMC (e.g., of various viscosities), a compound typically prepared by the reaction of cellulose with chloroacetic acid. In another example, the dispersant is hydroxyethyl cellulose.
[0111] Other possible candidates include sodium dodecyl sulfate (SDS), sodium dodecylbenzene sulfonate, derivatives of polyacrylic acid, and the like.
[0112] In some cases, the dispersant used may be the one available from BYK under the trademark or The obtained dispersion.
[0113] Dispersants such as PVP-based dispersants can be combined with additional dispersants such as AMP TM and / or PVB combination.
[0114] The concentration of the dispersant in the composition may vary depending on the specific type and concentration of dispersant or dispersant formulation, CNS, polymer, and solvent used. In some embodiments, the concentration of the dispersant is best expressed as a weight ratio of dispersant to CNS material. The weight ratio may range from 3:100-50:100 and may have or include, for example, one of the following ranges: 3:100-40:100, or 3:100-30:100, or 3:100-20:100, or 3:100-10:100, or 10:100-50:100, or 10:100-40:100, or 10:100-30:100, or 10:100-20:100, or 20:100-50:100, or 20:100-40:100, or 20:100-30:100, or 30:100-50:100, or 30:100-40:100, or 40:100-50:100.
[0115] In some cases, the concentration of the polymer derived from maleic anhydride in the composition depends on the composition of the polymer used, as well as the specific type and concentration of CNS materials, dispersants and solvents. In some embodiments, the composition includes 0.1wt%-1.0wt% of the polymer. The concentration of the polymer in the composition can be, for example, in one of the following ranges: 0.1wt%-0.8wt%, or 0.1wt%-0.6wt%, or 0.1wt%-0.4wt%, or 0.3wt%-1.0wt%, or 0.3wt%-0.8wt%, or 0.3wt%-0.6wt%, or 0.5wt%-1.0wt%, or 0.5wt%-0.8wt%, or 0.7wt%-1.0wt%. In various embodiments, the concentration of the polymer is expressed as the ratio of the dispersant to the CNS material by weight. The weight ratio of polymer to CNS may range from 0.1:100-2:100 and may have or include, for example, one of the following ranges: 0.1:100-1.5:100, or 0.1:100-1:100, or 0.1:100-0.5:100, or 0.5:100-2:100, or 0.5:100-1.5:100, or 0.5:100-1:100, or 1:100-2:100, or 1:100-1.5:100, or 1.5:100-2:100.
[0116] One example uses 1.6 wt% CNS / 0.32 wt% PVP-based dispersant; another example uses 1.5 wt% CNS / 0.5 wt% / 2155; A further example using 1.5wt% CNS / 0.32wt% AMP / PVB / 2155; Another example contains 1wt% CNS / 0.2wt% AMP / PVB / 2155,
[0117] Dispersions containing CNS may be pre-made and, in some cases, commercially available, for example, from Cabot Corporation.
[0118] The CNS material can be combined with a liquid, optionally in the presence of a dispersant, by suitable mixing techniques, using, for example, conventional mixing equipment. In various embodiments, the constituent components are blended to form a composition, such as a solution or dispersion. The composition can be, for example, characterized in that the concentration of the CNS in the solvent is about 0.25-about 2.5 weight %. In an illustrative example, the concentration in wt % is in the following range: about 0.25-about 0.5, about 0.5-about 0.75, about 0.75-about 1.0, about 1.0-about 1.25, about 1.25-about 1.50, about 1.50-about 1.75, about 1.75-about 2.0, about 2.0-about 2.25 or about 2.25-about 2.5. Other concentrations of CNS in the solvent can be used.
[0119] Unlike common solutions or dispersions using common, individualized CNTs (e.g., in raw form), CNS, particularly when provided as coated CNS in the form of granules or pellets, can produce stable dispersions. In some embodiments, stable dispersions can be achieved even using water as a solvent in the absence of a stabilizing surfactant. Other embodiments use a solvent in combination with water during wet processing. Examples of usable solvents include, but are not limited to, isopropyl alcohol (IPA), ethanol, methanol, and water.
[0120] In some cases, the technology used to prepare the dispersion produces CNS-derived species such as "CNS fragments" and / or "broken CNTs" that become distributed in individualized form throughout the dispersion (e.g., uniformly). In addition to their reduced size, CNS fragments (also including the term partially fragmented CNS) generally share the properties of intact CNS and can be confirmed by electron microscopy and other techniques, as described above. Broken CNTs can be formed when the crosslinks between CNTs within the CNS are broken, for example, under applied stress. Derived (produced or prepared) from CNS, the broken CNTs are branched and share common walls with each other.
[0121] Compositions consisting of or consisting essentially of CNS materials or compositions prepared from CNS, such as dispersions (such as described above), are combined with other ingredients. They can be used, for example, to make many energy storage devices such as lithium ion batteries. As an example, the composition is used to make an electrode (e.g., cathode) composition for a lithium ion battery. In many embodiments, the composition is combined with an electroactive material (component) for a specific type of electrode.
[0122] Many cathode materials commonly used in lithium-ion batteries are based on intercalation chemistry and typically involve chemical reactions that transfer a single electron. Other types of cathode materials (intercalation of lithium ions into, for example, FeF3) can transfer multiple electrons through more complex reaction mechanisms known as conversion reactions.
[0123] Examples of suitable electroactive materials include, but are not limited to, LCO, LMO, NCM, NCA, LCP, LFP, LFSF, LTS, and others as known in the art or as developed in the future. In some embodiments, the compositions containing CNS described above are used with NCM or NCA electrode compositions. Often, for example, a binder such as poly(vinyl difluoride) (PVDF) is included.
[0124] NCM (also referred to as "NMC") and NCA are well known to those skilled in the battery art.
[0125] In more detail, NCM can be obtained by the formula Li 1+x (Ni y Co 1-y-z Mn z ) 1-x O2 represents, wherein x ranges from 0 to 1, y ranges from 0 to 1 (e.g., 0.3 to 0.8), and z ranges from 0 to 1 (e.g., 0.1 to 0.3). Examples of NCMs include Li 1+x (Ni 0.33 Co 0.33 Mn 0.33 ) 1-x O2、Li 1+x (Ni 0.4 Co 0.3 Mn 0.3 ) 1-x O2、Li 1+x (Ni 0.4 Co 0.2 Mn 0.4 ) 1-x O2、Li 1+x (Ni 0.4 Co 0.1 Mn 0.5 ) 1-x O2、Li 1+x (Ni 0.5 Co 0.1 Mn 0.4 ) 1-x O2、Li 1+x (Ni 0.5 Co 0.3 Mn 0.2 ) 1-x O2、Li 1+x (Ni 0.5 Co 0.2 Mn 0.3 ) 1-x O2、Li 1+x (Ni 0.6 Co 0.2 Mn 0.2) 1-x O2, and Li 1+x (Ni 0.8 Co 0.1 Mn 0.1 ) 1-x O2.
[0126] NCA can be obtained by Li 1+x (Ni y Co 1-y-z Al z ) 1-x O2 represents, where x ranges from 0-1, y ranges from 0-1, and z ranges from 0-1. An example of NCA is Li 1+x (Ni 0.8 Co 0.15 Al 0.05 ) 1-x O2.
[0127] The concentration of NCM or NCA in the electrode composition may vary depending on the specific type of energy storage device. In some cases, NCM or NCA is present in the electrode composition in an amount of at least 90 wt %, such as greater than 95 wt %, relative to the total weight of the electrode composition, such as in an amount ranging from 90 wt % to 99 wt % relative to the total weight of the electrode composition.
[0128] In some embodiments, the electrode composition contains one or more binders, which are used, for example, to enhance the mechanical properties of the formed electrode. Exemplary binder materials include, but are not limited to, fluorinated polymers such as poly (vinyl difluoride) (PVDF), poly (vinyl difluoride-co-hexafluoropropylene) (PVDF-HFP), poly (tetrafluoroethylene) (PTFE), polyimides, and water-soluble binders such as polyoxy (ethylene), polyvinyl alcohol (PVA), cellulose, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone (PVP), and copolymers and mixtures thereof. Other possible binders include polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), and fluororubber and copolymers and mixtures thereof.
[0129] The binder can be present in the cathode composition in an amount of 1-10 wt %, eg, 1-2, 2-3, 3-4, 4-5, 5-6, 6-7, 7-8, 8-9, or 9-10 wt %.
[0130] In some implementations, the CNS loading relative to the dry electrode composition (e.g., used in an NCM electrode, for example, for a lithium battery) is less than 2 wt%, such as less than 1.9, 1.8, 1.7, or 1.6 wt%. In other embodiments, the CNS loading in the dry electrode composition (e.g., used in an NCM electrode, for example, for a lithium battery) is 1.5 wt% or less, such as at least 1.4, 1.3, 1.2, 1.2, 1.0, 0.95, 0.90, 0.85, 0.80, 0.75, 0.70, 0.65, 0.60, 0.55, 0.50, 0.45, 0.40, 0.35, 0.30, 0.25, 0.20, 0.15, or 0.10 wt%. In one example, the amount of CNS used to prepare the cathode composition is comparable to the minimum concentration at which the resulting dry cathode composition becomes conductive (i.e., the percolation threshold).
[0131] The electrode composition can be prepared by combining (eg, by intimately mixing) the above-mentioned constituent components, which can be added in any order to obtain a mixture, and in particular a homogeneous mixture. Suitable mixing techniques include mechanical agitation, shaking, stirring, and the like.
[0132] In one example, the electrode (e.g., cathode) composition is made by uniformly distributing (e.g., by uniformly mixing) a composition consisting of, consisting essentially of, or comprising CNS or a composition prepared using CNS starting materials with NCM or NCA components. In another example, a binder is uniformly dispersed, e.g., with a composition containing CNS and with NCM or NCA.
[0133] When provided in some form, such as in the form of granules, pellets or flakes, the CNS can be directly introduced into a slurry containing an active electrode material (eg, NCM or NCA).
[0134] In other embodiments, pellets, granules, flakes or other forms of CNS are first dispersed in a liquid medium such as NMP to produce CNS fragments (including partially fragmented CNS) and / or ruptured CNTs. The dispersion can be prepared from starting materials such as uncoated, PU or PEG coated CNS, or CNS with any other polymeric binder coating.
[0135] Various embodiments feature dispersions prepared, for example, from CNS and PVP-based dispersants. Another example uses a dispersion prepared from 2155. Optionally in AMP TMIn some examples, the cathode composition is prepared as follows: 98.25wt% NCM622+0.25wt% CNS+1.5wt% PVDF (eg, KF7200 manufactured by Kureha Corp.); or 98wt% NCM622+0.5wt% CNS+1.5wt% PVDF.
[0136] In one implementation, an electroactive material such as NCM is added to a CNS granule, pellet, flake, etc., in the presence of a solvent such as NMP, a mixture of a liquid medium such as NMP and a binder such as PVDF. Illustrative CNS fragment sizes present in the dispersion may be in the range of about 0.5 to about 20 μm, for example, in the following ranges: about 0.5 to about 1 μm; about 1 to about 5 μm; about 5 to about 10 μm; about 10 to about 15 μm; or about 15 to about 20 μm. In some cases, reducing the fragment size too much, for example to less than 0.5 μm, may impair the electrical properties associated with utilizing CNS.
[0137] The resulting electrode composition may be in the form of a slurry (e.g., paste) combining particulate NCM or NCA, CNS-based conductive additives, dispersant (one or more) (if present), non-conductive additive (one or more) (if present), solvent, and binder (if present). In other embodiments, the electrode composition is a solid formed by removing the solvent from the slurry. Adoptable drying techniques include air drying, heating (e.g., in a suitable oven), etc.
[0138] The battery electrode can be formed by applying an electrode composition (such as described above) (such as in the form of a paste) to a conductive substrate (such as an aluminum current collector) followed by removal of the solvent. The paste can be applied by techniques such as doctor blade coating, reverse comma bar coating, or extrusion.
[0139] In some implementations, the paste has a solid loading (i.e., a high solids concentration) high enough to enable deposition onto a substrate while minimizing the formation of intrinsic defects (e.g., cracking) that can occur with less viscous pastes (e.g., with lower solid loadings). In addition, higher solid loadings reduce the amount of solvent required and its removal.
[0140] The solvent is removed by heating the paste at ambient temperature or under low heat conditions, for example, at a temperature in the range of 20° C. to 100° C. The deposited electrode / current collector may be cut to the desired dimensions, optionally followed by calendering.
[0141] The process leading to the formation of the electrode can maintain the integrity of at least some of the initial CNS used, which will remain intact. However, some process operations and / or conditions can change at least some of the initial CNS used. As described above, one example involving such operations and / or conditions is the application of shear forces, such as encountered when preparing an emulsion from a CNS starting material.
[0142] In some cases, the initial CNS is disrupted into smaller CNS units or fragments. In addition to their reduced size, these fragments generally share the properties of the intact CNS and can be confirmed by electron microscopy and other techniques, as described above.
[0143] It is also possible that the initial nanostructure morphology of CNS changes. For example, the applied shear can destroy the crosslinking between the CNTs in the CNS to form CNTs that are typically dispersed in the electrode composition as separate CNTs. It is found that for many of these CNTs, even after crosslinking is removed, the structural features of branching and shared walls are also retained. CNTs derived (prepared) by CNS and retaining the structural features of CNT branching and shared walls are referred to as "broken ()" CNTs in this article. These species can impart improved interconnectivity (between CNT units), resulting in better conductivity at lower concentrations.
[0144] Thus, compared to electrodes or electrode compositions employing ordinary, individualized CNTs (e.g., in pristine form), the electrodes and electrode compositions described herein will often include broken CNTs. These broken CNTs can be easily distinguished from ordinary carbon nanotubes by standard carbon nanotube analysis techniques such as SEM. It is further noted that not every CNT encountered needs to be branched and share a common wall; rather, a plurality of broken CNTs as a whole will have these features.
[0145] The formed electrode can be introduced into a lithium ion battery according to methods known in the art, such as described in "Lithium Ion Batteries Fundamentals and Applications", Yuping Wu, CRC press, (2015). In some embodiments, the battery is a coin type, such as a 2032 coin cell, a 18650 cylindrical cell, a pouch cell, and others. In addition to a cathode containing CNS (e.g., as described above), the battery also includes other components such as an anode, and a suitable electrolyte such as ethylene carbonate-dimethyl carbonate-ethyl methyl carbonate (EC-DMC-EMC), vinylene carbonate (VC), LiPF6; ethylene carbonate-diethyl carbonate (EC-DEC, LiPF6; or (EC-DMC), LiPF6. A suitable glass fiber microfilter (e.g., Whatman GF / A) or a polypropylene / polyethylene membrane (e.g., Celgard 2300) is used as a separator that absorbs the electrolyte and prevents electrical contact between the electrodes while allowing diffusion of Li ions.
[0146] In some of the Li cells described herein, the anode contains an active anode material and a binder (eg, PVDF, CMC with SBR, etc.) and in some cases a conductive additive.
[0147] In many implementations, the active anode material is graphite such as natural graphite, artificial graphite, or a blend of the two. Commercially available types of graphite that can be used include mesophase carbon microbeads (MCMB), carbon fibers (MCF) based on mesophase pitch, vapor-grown carbon fibers (VGCF), large-scale artificial graphite (MAG), natural graphite, and others. In other implementations, the active anode compound used comprises silicon, consists essentially of silicon, or consists of silicon. In one example, the active anode material is a silicon-graphite composite, a nano-silicon (Si) or SiO x Particles of graphite.
[0148] Examples of other active anode materials include, but are not limited to: (a) intercalation / deintercalation materials (e.g., carbon-based materials, porous carbon, carbon nanotubes, graphene, TiO2, Li4Ti5O 12 (b) alloy / de-alloy materials (e.g., Si, SiO x , doped Si, Ge, Sn, Al, Bi, SnO2, etc.); and (c) conversion materials (e.g., transition metal oxides (Mn x O y 、NiO、Fe x O y , CuO, Cu2O, MoO2, etc.), by formula M x X yMetal sulfides, metal phosphides and metal nitrides represented by X=S, P, N)).
[0149] Active anode materials such as graphite, silicon, lithium titanate (Li4Ti5O 12 ) etc. may vary depending on the specific type of energy storage device. In an illustrative example, the active component is present in the electrode composition in an amount of at least 80 wt %, such as at least 85, 90 or 95 wt %, relative to the total weight of the (dry) electrode composition, such as in an amount ranging from 80 wt % to 99 wt %, such as about 80 to about 85 wt %, about 85 to about 88 wt %, about 88 to about 90 wt %, about 90 to about 92 wt %, about 92 to about 95 wt %, about 95 to about 97 wt %, or about 97 to about 99 wt %, relative to the total weight of the electrode composition.
[0150] In some embodiments, the anode composition also contains a conductive additive such as a conductive carbon additive (CCA). Examples include CB, CNT, etc. In a variety of specific implementations, the anode composition includes CNS, CNS fragments and / or broken CNTs. Such anode compositions and their preparation and use are described as follows: U.S. Provisional Patent Application No. 62 / 822,101, entitled Anode Electrode Compositions for Battery Applications, filed on March 22, 2019, and a non-provisional U.S. patent application entitled Anode Electrode Compositions for Battery Applications, filed simultaneously therewith, with agent case number 2018613, both of which are fully incorporated herein by reference. In many cases, the CNS used to prepare the anode composition is coated, such as PU or PEG coated. When dried, the illustrative anode composition contains an amount of not more than about 1wt% and in many cases not more than 0.5wt% of carbon nanostructures, fragments of carbon nanostructures and / or broken nanotubes.
[0151] Thus, in various embodiments of the invention, both the cathode and the anode contain CNS, fragments of CNS, and / or disrupted CNTs.
[0152] In some implementations, the CNS loading relative to the dry electrode composition (e.g., for use in a graphite negative electrode, for example, for LIB) is no greater than about 5 wt% and often no greater than about 2 wt%, such as less than 1.9, 1.8, 1.7, or 1.6 wt%. In other embodiments, the CNS loading relative to the dry electrode composition (e.g., for use in a graphite anode, for example, for LIB) is 1.5 wt% or less, such as at least 1.4, 1.3, 1.2, 1.2, 1.0, 0.95, 0.90, 0.85, 0.80, 0.75, 0.70, 0.65, 0.60, 0.55, 0.50, 0.45, 0.40, 0.35, 0.30, 0.25, 0.20, 0.15, or 0.10 wt%. In many implementations, the CNS loading relative to the dry electrode composition (e.g., used in a graphite anode for a lithium battery) is no greater than 0.5 wt%, for example, in the range of about 0.5 wt%-0.1 wt%, such as in the range of about 0.1-about 0.2, about 02-about 0.3, about 0.3-about 0.4, or about 0.4-about 0.5 wt%. Other embodiments employ a loading in the range of about 2-about 5 wt%, such as at least about 2.25, 2.5, 2.75, 3.0, 3.25, 3.5, 3.75, 4.0, 4.25, 4.5 or 4.75.
[0153] The compositions described herein can be used in (e.g., incorporated into) electrodes of other energy storage devices such as primary alkaline batteries, primary lithium batteries, nickel metal hydride batteries, sodium batteries, lithium sulfur batteries, lithium air batteries, and supercapacitors. Methods for making such devices are known in the art and are described, for example, in the following: "Battery Reference Book", TR Crompton, Newness (2000).
[0154] A variety of techniques can be used to characterize the electrodes, batteries or electrode compositions described herein, and / or to confirm the presence of CNS. Examples include, but are not limited to, electron microscopy such as TEM, SEM, Raman spectroscopy, or other suitable qualitative or quantitative analysis methods.
[0155] Electrode performance and / or properties can be evaluated by procedures known in the art, or by adapting or developing techniques. Suitable techniques include, for example, in-plane and homeotropic electrode conductivity, electrochemical impedance spectroscopy (EIS), constant current charge-discharge, hybrid pulse power characterization (HPPC). Some examples are described below.
[0156] In applications such as those described herein, CNS-based conductive additives perform as well as and often better than CBs, individualized CNTs, or graphene (materials that have high electrical and thermal conductivity and are mechanically strong and exist as thin sheets of carbon atoms). For many LIBs, CNS loadings are lower than those required with other CCAs such as CBs. In one implementation, CNS loadings as low as 0.25 wt% impart good cathode performance, and such low loadings were found to be above the percolation threshold (i.e., the lowest concentration at which an insulating material converts to a conductive material).
[0157] In some embodiments, electrodes containing CNS perform as well as comparative electrodes (made with the same active electrode material, e.g., NCM, solvent, and, if used, other ingredients, e.g., dispersant) containing CB at a higher loading. For example, a loading of CNS up to 1.5 wt% imparts at least as good performance (e.g., expressed as cathode resistance or capacity of a battery made with the electrode) as an electrode containing 2 or more wt% CB. In other embodiments, electrodes containing a certain CNS loading, e.g., 1.5 wt% or less, exhibit better performance (e.g., expressed as cathode resistance or capacity of a battery made with the electrode) relative to comparative electrodes containing the same amount of CB.
[0158] CB particles, which are typically used as CCA in electrodes and can be used to prepare comparative cathode formulations, often have a diameter greater than 50 μm. 2 / g, and an oil absorption number (OAN) greater than 150 mL / 100 g. CNTs and particularly MWCNTs may also be used. Shown below in Table 3 are several illustrative CB and CNT specifications, some of which are referenced in the following non-limiting Examples, and are presented to further describe aspects of the invention.
[0159] Table 3
[0160]
[0161] Example 1: CNS dispersion in NMP
[0162] Use 3wt.% of the CNS material (PU-coated CNS) coated with a water-soluble polyurethane sizing agent to prepare 0.375% CNS dispersion in N-methylpyrrolidone (NMP). Weigh an appropriate amount of NMP (99.625% of the formulation) and place it in a jacketed beaker and bring it to Nanoenclosure (protective cover) under secondary containment. An appropriate amount of PU-coated CNS pellets (0.375%) are added to the NMP and introduced into the solvent. The PU polymer coating on the pellets is ignored when calculating because it is a very small percentage of the total formulation, i.e. 0.02 weight %. The mixture is covered and brought back to the laboratory under secondary containment. The jacketed container is connected to cold water to prevent excessive heat accumulation during processing. The mixture is stirred with a standard overhead mixer while using an ultrasonic probe to provide 0.5kJ / g of energy to the mixture. For a 200g batch size, the ultrasonic duration is 10min. The container is then transferred to a hood where the dispersion is bottled.
[0163] Example 2: Electrode Preparation
[0164] Formulations were made at 0.25%, 0.5%, 1.0% and 1.5% CNS using 1.5% PVDF binder (Arkema Kynar HSV900). The active material was NCM 111, i.e., Li 1+x (Ni 0.33 Co 0.33 Mn 0.33 ) 1-x O2(7 micron D 50 ), which was supplied by BASF TODA Battery Materials LLC and had a mass median diameter (D 50 ). The slurry was prepared by weighing appropriate amounts of CNS dispersion, PVDF binder solution (pre-dissolved in NMP at 10 wt.%), NCM111 powder and NMP. The final solid loadings achieved to produce sufficient slurry viscosity for coating are listed in Table 4. The electrode slurry was mixed in one step using a SPEX800 mill with two zirconia media for 30 minutes.
[0165] Table 4
[0166] CNS loading Total solids of paste 0.25% 56% 0.5% 41% 1.0% 26% 1.5% 20%
[0167] The electrode slurry was coated onto aluminum foil using an automated knife coater (Model MSK-AFA-III from MTI Corp.). NMP was evaporated in a convection oven set at 80° C. for 20 minutes. The electrode paste was coated at 10 mg / cm 2The dry electrode loading was coated and calendered to a density of 2.8 g / cc using a hand roller compactor.
[0168] Example 3: Electrode Resistance
[0169] The sheet resistance of the coated electrodes was measured with a Lucas Lab 302 four-probe workstation and an SP4 probe head (connected to the back of a Keithley 2410C source meter). The measurements were performed in a two-wire configuration mode because it was found that four-wire measurements resulted in a strong contribution from the substrate conductivity. The reported values are direct ohmic readings from the instrument at a current of 0.1 milliamperes (mA) and a cathode calendering density of 2.8 g / cc. All cathodes tested here were of the same thickness.
[0170] Figure 4 Depict a plastic sheet such as Mylar made of CNS with a loading of 0.25 wt% to 1.5 wt%. TM The resistances obtained for cathode sheets (active material: lithiated nickel cobalt manganese CM111; binder: Arkema Kynar HSV-900) on Al foil or Mylar. The resistances of cathode sheets made with 2 wt% and 4 wt% of carbon black particles having the properties of specification III in Table 3 are also shown. It was found that the resistances of cathode sheets made with 2 wt% and 4 wt% of carbon black particles having the properties of specification III in Table 3 were significantly higher than those of cathode sheets made with 2 wt% and 4 wt% of carbon black particles having the properties of specification III in Table 3 were significantly lower than those of cathode sheets made with 2 wt% and 4 wt% of carbon black particles having the properties of specification III in Table 3. TM 0.5 wt% CNS on both sheets showed much lower resistance than 2% CB additive. The resistance measured for the electrode with 1.5% CNS was as good as that observed with 4% carbon additive.
[0171] Example 4: Electrode Capacity
[0172] The cathode of Example 2 was tested in a 2032 coin cell half cell. 15 mm diameter discs were punched out for the preparation of coin cells and dried at 110° C. under vacuum for a minimum of 4 hours. The discs were rolled to a density of 2.8 g / cc with a hand roller press and assembled into 2032 coin cells in an argon-filled glove box (M-Braun) for testing against lithium foil. A glass fiber microfilter (Whatman GF / A) was used as a separator. The electrolyte was 100 microliters of ethylene carbonate-dimethyl carbonate-ethyl methyl carbonate (EC-DMC-EMC), vinylene carbonate (VC) 1%, LiPF61M (BASF). Four coin cells were assembled for each formulation tested. The capacity reported is the average of four coin cells, which is standardized in milliampere hours / gram (mAh / g) active cathode mass.
[0173] The capacities of half coin cell cells using the above cathode electrodes comparing 0.25% CNS, 2% CB and 4% CB additives are shown in Figure 5Overall, 0.25% CNS showed the best discharge capacity up to 10C c-rate. This can be attributed to the benefit of reducing the conductive additive in the electrode (higher loading). Figure 6 The direct current internal resistance (DCIR) obtained at different states of charge (SOC) for coin cells made with cathodes containing 0.25 wt% CNS, 2 wt% CB and 4 wt% CB additives, respectively, is shown. It was found that 0.25% CNS resulted in the lowest coin cell resistance compared to 2% and 4 wt% CB additives at 20, 50 and 80% SOC.
[0174] Example 5: Preparation of electrodes using CNS powder
[0175] Active cathode powder (Sanshan NCM622), NMP, 10% solid binder NMP solution (Kureha KF7200) were mixed together at 70% solid loading using a Thinky ARE310 planetary mixer for 12 minutes (3*4 minutes active period, 3*3 minutes intermittent cooling period). PU coated CNS granules (CNS_PU 3%) were added at 0.5 wt.% solids and mixed for another 12 minutes (3*4 minutes active period, 3*3 minutes intermittent cooling period).
[0176] After the CNS addition, NMP was gradually added to achieve 60% final solids in the slurry and maintain a coatable slurry viscosity.
[0177] The electrode slurry was coated onto aluminum foil using an automated knife coater (Model MSK-AFA-III from MTI Corp.). NMP was evaporated in a convection oven set at 80° C. for 20 minutes. The electrode paste was coated at 25 mg / cm 2 The dry electrode loading was coated and rolled to 3.5 g / cm using a manual roller press. 3 The electrode solid content is 98% NCM622, 0.5% CNS and 1.5% KF7200 PVDF binder.
[0178] Example 6: Electrode resistance using CNS dry powder additive
[0179] The in-plane electrode resistance was measured as described in Example 3, and the electrodes prepared using the CNS powder additive were compared with other control electrodes containing 1% carbon black (having the properties of specification III in Table 3) or 0.5% carbon nanotubes (CNT) (having the properties of specification V in Table 3). All electrodes tested here were of the same thickness. A manual drop gauge (drop gauge) in which a flat measuring contact head of 7.14 mm diameter was connected to the front of a Keithley 2410C source meter was used to measure the vertical electrode resistance. The measurement was carried out in a two-wire configuration mode, with a direct ohmic reading from the instrument at a current of 0.1 milliamperes (mA) and a cathode calendering density of 3.5 g / cc, and further converted to the vertical electrode conductivity (in S / m) as reported herein. The characteristics of the electrode are listed in Table 5. Figure 7 The results shown in show that the 0.5% CNS electrode has an in-plane resistance similar to that of 0.5% CNT and half that of the electrode using 1% CB. The homeotropic conductivity is statistically higher than that observed with 0.5% CNT and 1% CB.
[0180] Table 5
[0181]
[0182] Example 7: Preparation of CNS dispersion in NMP - Method 2
[0183] CNS dispersions were made by first loading the medium into the Netzsch Minicer Agitator Bead Mill. For these samples, 100 ml of 0.4-0.6 mm yttria-stabilized zirconium oxide beads were added to the chamber. This amount was equivalent to 70% filling of the grinding chamber. Then, a known amount of NMP was supplied to the system. Based on the amount added, the amount of PEG-coated CNS (Cabot Corporation) required to achieve the target loading was calculated. The amount was then broken down into multiple doses of about 0.2% wt. The system was set to the preferred operating conditions of 4200 rpm and a pumping rate of about 80 ml / min, and the first dose of carbon nanostructures was added. The system was run and monitored until the pressure in the system stabilized and the dispersion appeared smooth. A second dose was added, and the process was repeated until the desired loading was achieved. The deeper the process progressed, the longer the energy required to reach the ideal state after each dose. Finally, after the material was loaded and fully ground, a dispersant was added to the dispersion and another half an hour of circulation was allowed to be fully introduced into the system. The sample was then pumped out into a container and the Minicer mill was flushed to remove remaining material.
[0184] Two CNS dispersions have been prepared following this protocol. The composition and PSD (measured by Microtrac instrument) details are summarized in Table 6.
[0185] Table 6
[0186]
[0187] Example 8: Preparation of electrodes using CNS dispersions – Method 2
[0188] Conductive carbon materials used for electrode preparation included: pre-dispersed CNS particles from Cabot Corporation as listed in Table 6, and commercially available MWCNTs with properties of specifications VI-IX as listed in Table 3. All CCAs were used in the form of NMP-based dispersions. The cathode was prepared with NCM622 active material from ShanShan (China) and KF7200 PVDF binder from Kureha.
[0189] The NCM electrode slurry was made using a Thinky planetary centrifugal mixer (model ARE-310) following a two-step mixing protocol. The first step included actively mixing the CNS dispersion with the PVDF binder at 2000 rpm for twelve minutes; the second step included adding the active NCM622 material and NMP required to adjust the viscosity, and actively mixing at 2000 rpm for another 12 minutes. The slurry was mixed during the first step using two 1 / 4 inch diameter tungsten carbide media; the slurry was mixed without media during the second step.
[0190] The resulting electrode slurry was manually coated onto 16 micron thick aluminum foil using an automated knife coater (Model MSK-AFA-III from MTI Corp.). The target loading was 25 mg / cm on one side. 2 The NMP was evaporated in a convection oven set at 110°C for 1 hour and finally dried in a vacuum oven at -100°C. The electrode was calendered with a hand roller press to a density of 3.5 g / cc.
[0191] Fourteen electrode formulations (see Table 7 for details) were prepared for electrode resistance measurements and initial unit cell performance testing. Two more electrodes were prepared as comparative examples for electrode resistance testing: {0.5% CCA: 98% NCM622: 1.5% PVDF} formulation, where CCA is CNT with properties of specifications VIII and IX in Table 3.
[0192] Table 7
[0193]
[0194] Example 9: Electrode Resistivity
[0195] Figure 8 The electrode vertical resistivity obtained from cathode sheets on aluminum foil made with different CCA types (see details in Table 7) as a function of the percent weight of CCA content in the electrode ranging from 0.1 wt% to 1.0 wt% is depicted. The reported values are derived from direct ohmic readings (electrode resistance) measured using a manual drop meter in which a 7.14 mm diameter flat measuring contact head is connected to the front of a Keithley 2410-C source meter. The measurements were performed in a two-wire configuration mode, at a current of 0.1 milliamperes (mA), and a cathode calendering density of 3.5 g / cc.
[0196] It was found that the electrode resistivity varies up to several orders of magnitude depending on the CCA type and improves with higher CCA content. Electrodes using 0.25% and 0.5% loadings of pre-dispersed CNS-A and CNS-B show the lowest resistivity compared to the two multi-walled CNT materials tested at the same loadings. Only at loadings of 0.75% and 1% when the percolation threshold is reached do electrodes containing CNTs match the resistivity of the 0.25% CNS sample. The data show that CNSs require ~1 / 3 the weight of material to create enough connection points within the electrode and form a conductive percolation network compared to multi-walled CNTs.
[0197] Fig. 9 Electrode resistivity for selected electrode formulations with 0.5% CCA is depicted. It is demonstrated that while electrodes using CNS-B are slightly more resistive than electrodes using CNS-A when tested at 0.5%, CNS materials overall show the lowest electrode resistivity compared to all multi-walled CNTs tested at the same loading, suggesting that higher amounts of CNT material are needed to match CNS performance.
[0198] Example 10: Initial Cell Performance
[0199] The cathode formulations listed in Table 7 were tested in 2032 half coin cells. 15 mm diameter discs were punched out for the preparation of coin cells and dried at 100° C. under vacuum for a minimum of 4 hours. The discs were rolled to a density of 3.5 g / cc using a hand roller press and assembled into 2032 coin cells in an argon-filled glove box (M-Braun) for testing against lithium foil. A glass fiber microfilter (Whatman GF / A) was used as a separator. The electrolyte was 175 microliters of ethylene carbonate-dimethyl carbonate-ethyl methyl carbonate (EC-DMC-EMC), vinylene carbonate (VC) 1%, LiPF61M (BASF). The reported capacity is standardized in milliampere hours / gram (mAh / g) of active cathode mass.
[0200] The room temperature (25°C) performance of the half coin cells was measured by first forming them using two C / 5-D / 5 charge-discharge cycles, then charging them at a C / 2 rate and discharging them at C / 5, C / 2, 1C, 2C, 3C, 4C, and 5C discharge rates. Then, their hybrid pulse power characteristics (HPPC) were tested using 10 s of 1.5C charge and 2C discharge pulses from full charge to full discharge every 10% state of charge.
[0201] Fig.10 Depict the C-rate performance and DC-IR internal resistance at 50% SOC of the formulations with CCA contents ranging from 0.1wt% to 1.0wt% as listed in Table 7. The results show that 0.5% CNS-A provides better initial cell performance than multi-walled CNTs in terms of both 2C capacity (full discharge in 30 minutes) and DC-IR at 50% SOC. No difference was observed for 0.5C capacity because the rate was too slow to reveal the effect of CCA type (full discharge in 2 hours). Since CNS reaches the percolation threshold at a lower loading than multi-walled CNTs, the difference becomes apparent at 0.25%. Both CNS samples (CNS-A and CNS-B) show performance superior to CNTs (here, CNT-VI and CNT-VII) tested at the same 0.25% loading, and are comparable to those at 0.75% and 1.0%.
[0202] Example 11: Low temperature performance
[0203] Another benefit of CNS over multi-walled CNT in NCM electrode formulations is the improvement in low temperature performance as demonstrated below. The cathode formulations were tested in half coin cell cells with NCM622 cathodes having 25 mg / cm 2 The examples include CNS-A and CNS-B samples pre-dispersed as described in Example 7, CNS pellets, and CNTs (having the properties of Specification IX in Table 3), which were tested at 0.25, 0.5, and 1% CCA loading, respectively, as detailed in Table 8. The low temperature capacity of the half coin cells was measured by fully charging them at 1 h rate, 25°C (CC-CV 1C, 4.3V-0.05C), and then fully discharging them at 25, 0, -10, -20°C, 1D to 2.8V (1 h rate).
[0204] Table 8
[0205]
[0206] Fig.11 The -10°C capacity retention of the electrode (as % of 25°C capacity) is shown for cells using the cathode formulations in Table 8. It was found that cathodes prepared with 0.25% and 0.5% pre-dispersed CNS-A showed an improvement of -48% in -10°C capacity retention compared to 1% MWCNT. The cathodes using 0.5% CNS-B were ~13% better than those using 1% MWCNT. Unlike the pre-dispersed CNS samples, the CNS pellets maintained the same capacity retention as with 1% CNT, but at a lower loading of one-half (capacity retention of 0.5% CNS pellets ≈ 1% CNT). These results suggest that at low temperatures, CNS materials provide better cell performance than even higher loadings of individual CNTs. Advantages in low temperature performance may also be associated with providing CNS via a dispersion.
[0207] As used herein, the term "and / or" includes any and all combinations of one or more of the related enumerated items. In addition, the singular form and the articles "a, an" and "the" are also intended to include plural forms, unless otherwise expressly stated. It will be further understood that the terms: including, comprising, containing and / or containing, when used in this specification, indicate the presence of stated features, wholes, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more additional features, wholes, steps, operations, elements, components, and / or their collections. In addition, it will be understood that when an element, including its parts or subsystems, is referred to and / or shown as being connected or coupled to another element, it may be directly connected or coupled to the other element or there may be an intermediate element.
[0208] It will be understood that although terms such as "first" and "second" are used herein to describe various elements, these elements should not be limited by these terms. These terms are only used to distinguish one element from another element. Therefore, without departing from the teachings of the present invention, the element discussed below may be referred to as a second element, and similarly, the second element may be referred to as a first element.
[0209] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the present invention pertains. It will be further understood that terms, such as those defined in commonly used dictionaries, should be interpreted as having a meaning consistent with their meaning in the context of the relevant art and will not be interpreted in an idealized or overly formal sense unless clearly so defined herein.
[0210] While the present invention has been particularly shown and described with reference to preferred embodiments thereof, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the scope of the invention as encompassed by the appended claims.
Claims
1. An electrode composition comprising: electroactive materials; and at least one material selected from the group consisting of a carbon nanostructure, a fragment of a carbon nanostructure, and a broken multi-walled carbon nanotube, wherein the electroactive material is a lithium transition metal compound, wherein the carbon nanostructure or the fragment of the carbon nanostructure comprises a plurality of multi-walled carbon nanotubes cross-linked into a polymeric structure by branching, interlacing, entanglement and / or sharing a common wall, in, The fragments of the carbon nanostructure are derived from the carbon nanostructure, have a reduced size, share the properties of the intact carbon nanostructure and can be identified by electron microscopy and other techniques, and wherein the broken multi-walled carbon nanotubes are derived from a carbon nanostructure and are branched and share a common wall with each other, in: At least one of the multi-walled carbon nanotubes has a length equal to or greater than 2 micrometers, as determined by SEM, at least one of the multi-walled carbon nanotubes has an aspect ratio of length to diameter in the range of 200-1000, Along a 2 micron length of at least one of the multi-walled carbon nanotubes, there are at least two branches, as determined by SEM, At least one multi-walled carbon nanotube exhibits asymmetry with respect to the number of walls observed in the region after the branch point relative to the region before the branch point, and / or, there are no catalyst particles at or near the branch point, as determined by TEM.
2. The electrode composition of claim 1, wherein the multi-walled carbon nanotubes comprise 2 to 30 coaxial carbon nanotubes as determined by TEM at a magnification sufficient to count the number of walls.
3. The electrode composition of claim 1, wherein at least 1% of the multi-walled carbon nanotubes have a length equal to or greater than 2 microns as determined by SEM, An aspect ratio of length to diameter in the range of 200-1000, and / or an asymmetry in the number of walls observed in the region after the branch point relative to the region before the branch point.
4. The electrode composition of claim 1, further comprising a binder.
5. The composition of claim 4, wherein the binder is polyvinylidene fluoride.
6. The composition of claim 1, wherein the at least one material comprises carbon nanostructures provided as a dispersion or as a loose particulate material.
7. The composition of claim 1, further comprising a dispersant selected from the group consisting of a PVP-based dispersant, a styrene maleic anhydride-based dispersant, a cellulose-based dispersant, a co-dispersant, and any combination thereof.
8. The electrode composition of claim 1, wherein the composition is a slurry or a solid.
9. The electrode composition of claim 1, wherein the composition further comprises a solvent.
10. The electrode composition of claim 9, wherein the solvent is N-methylpyrrolidone.
11. The electrode composition of claim 1, wherein the electrode composition contains carbon nanostructures, fragments of carbon nanostructures, and / or broken multi-walled carbon nanotubes in an amount of no greater than 1 wt% when dried.
12. The electrode composition of claim 1, wherein the carbon nanostructure is a coated carbon nanostructure. 13 . The electrode composition of claim 12 , wherein the coated carbon nanostructure is a polyurethane-coated nanostructure or a polyethylene glycol-coated carbon nanostructure.
14. The electrode composition of claim 12, wherein the weight of the coating is in the range of 0.1% to 10% relative to the weight of the coated carbon nanostructure.
15. The electrode composition of claim 12, wherein the electrode composition contains the capped carbon nanostructures in an amount of no greater than 1 wt. % when dried.
16. The electrode composition of claim 1, further comprising a carbon conductive additive selected from the group consisting of carbon black, individualized carbon nanotubes in pristine form, and any combination thereof.
17. The electrode composition of claim 1, further comprising carbon black, wherein the carbon black has a carbon black content of 200 m 2 / g or less and an OAN of at least 130 mL / 100 g.
18. The electrode composition of claim 1, wherein the electroactive material is a lithium transition metal oxide selected from the group consisting of lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide.
19. The electrode composition of claim 1 comprising 90-99 wt% of said electroactive material.
20. An electrode comprising the electrode composition according to any one of claims 1 to 19 and a current collector contacting the electrode composition.
21. A battery comprising an electrode composition according to any one of claims 1 to 19 or an electrode according to claim 20.
22. A rechargeable lithium ion battery comprising the electrode composition of any one of claims 1 to 19 or the electrode of claim 20.
23. A method for preparing an electrode composition, the method comprising: combining a dispersion containing at least one material selected from the group consisting of carbon nanostructures, fragments of carbon nanostructures, and broken multi-walled carbon nanotubes with an electroactive material to form a mixture, wherein the carbon nanostructure or the fragment of the carbon nanostructure comprises a plurality of multi-walled carbon nanotubes cross-linked into a polymeric structure by branching, interlacing, entanglement and / or sharing a common wall, wherein the fragments of the carbon nanostructure are derived from the carbon nanostructure, have a reduced size, share the properties of the intact carbon nanostructure and can be identified by electron microscopy and other techniques, wherein the broken multi-walled carbon nanotubes are derived from a carbon nanostructure and are branched and share a common wall with each other, and wherein the electroactive material is a lithium transition metal compound, in: At least one of the multi-walled carbon nanotubes has a length equal to or greater than 2 micrometers, as determined by SEM, at least one of the multi-walled carbon nanotubes has an aspect ratio of length to diameter in the range of 200-1000, Along a 2 micron length of at least one of the multi-walled carbon nanotubes, there are at least two branches, as determined by SEM, At least one multi-walled carbon nanotube exhibits asymmetry with respect to the number of walls observed in the region after the branch point relative to the region before the branch point, and / or, there are no catalyst particles at or near the branch point, as determined by TEM.
24. The method of claim 23, wherein the multi-walled carbon nanotubes comprise 2-30 coaxial carbon nanotubes as determined by TEM at a magnification sufficient to count the number of walls.
25. The method of claim 23, wherein at least 1% of the multi-walled carbon nanotubes have a length equal to or greater than 2 microns as determined by SEM, An aspect ratio of length to diameter in the range of 200-1000, and / or an asymmetry in the number of walls observed in the region after the branch point relative to the region before the branch point.
26. The method of claim 23, wherein the dispersion is prepared by combining the carbon nanostructure with a dispersant selected from the group consisting of a PVP-based dispersant, a styrene maleic anhydride-based dispersant, a cellulose-based dispersant, a co-dispersant, and any combination thereof.
27. The method of claim 26, wherein the carbon nanostructures are provided in the form of loose particulate material.
28. The method of claim 23, wherein the electroactive material is a lithium transition metal oxide selected from the group consisting of lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide.
29. The method of claim 23, wherein the mixture further comprises a binder.
30. The method of claim 29, wherein the binder is polyvinylidene fluoride.
31. The method of claim 23, wherein the mixture further comprises a carbon conductive additive selected from the group consisting of carbon black, individualized carbon nanotubes in pristine form, and any combination thereof.
32. The method of claim 23, further comprising carbon black, wherein the carbon black has a 200 m 2 / g or less and an OAN of at least 130 mL / 100 g.
33. The method of claim 23, further comprising drying the mixture.
34. The method of claim 23, wherein The mixture contains carbon nanostructures, fragments of carbon nanostructures, and / or broken multi-walled carbon nanotubes in an amount of no greater than 1 wt % when dried.
35. The method of claim 23, wherein the electroactive material is provided in an amount of 90-99 weight percent based on the weight of the mixture when dry.
36. The method of claim 23, further comprising applying the mixture to a current collector.
37. The method of claim 23, wherein the carbon nanostructure is a coated carbon nanostructure.
38. The method of claim 37, wherein the carbon nanostructure is a polyurethane-coated nanostructure or a polyethylene glycol-coated carbon nanostructure.
39. The method of claim 37, wherein The weight of the coating is in the range of 0.1-10% relative to the weight of the coated carbon nanostructure.
40. The method of claim 37, wherein The mixture contains the capped carbon nanostructures in an amount of no greater than 1 wt % when dried.
41. A method for preparing an electrode composition, the method comprising introducing a carbon nanostructure into a slurry comprising an electroactive material, wherein the electroactive material is a lithium transition metal compound, and wherein the carbon nanostructure comprises a plurality of multi-walled carbon nanotubes cross-linked into a polymeric structure by branching, interlacing, entanglement and / or sharing a common wall, in: At least one of the multi-walled carbon nanotubes has a length equal to or greater than 2 micrometers, as determined by SEM, at least one of the multi-walled carbon nanotubes has an aspect ratio of length to diameter in the range of 200-1000, Along a 2 micron length of at least one of the multi-walled carbon nanotubes, there are at least two branches, as determined by SEM, At least one multi-walled carbon nanotube exhibits asymmetry with respect to the number of walls observed in the region after the branch point relative to the region before the branch point, and / or, there are no catalyst particles at or near the branch point, as determined by TEM.
42. The method of claim 41, wherein the multi-walled carbon nanotubes comprise 2-30 coaxial carbon nanotubes as determined by TEM at a magnification sufficient to count the number of walls.
43. The method of claim 41, wherein at least 1% of the multi-walled carbon nanotubes have a length equal to or greater than 2 microns as determined by SEM, An aspect ratio of length to diameter in the range of 200-1000, and / or an asymmetry in the number of walls observed in the region after the branch point relative to the region before the branch point.
44. The method of claim 41, wherein the carbon nanostructures are provided as loose particulate material having the form of flakes, pellets, or granules.
45. The method of claim 41, wherein the electroactive material is provided in an amount of 90-99% by weight.
46. The method of claim 41, further comprising applying the slurry to a current collector.
47. The method of claim 41, further comprising drying the slurry.
48. The method of claim 41, wherein the slurry, when dried, comprises carbon nanostructures, fragments of carbon nanostructures, and / or broken multi-walled carbon nanotubes in an amount of no greater than 1 wt. %.
49. The method of claim 41, wherein the slurry further comprises a carbon conductive additive selected from the group consisting of carbon black, individualized carbon nanotubes in pristine form, and any combination thereof.
50. The method of claim 41, wherein the slurry further comprises carbon black, wherein the carbon black has a 200 m 2 / g or less and an OAN of at least 130 mL / 100 g.
51. The method of claim 41, wherein the carbon nanostructure is a coated carbon nanostructure.
52. The method of claim 51, wherein the coated carbon nanostructure is a polyurethane coated nanostructure or a polyethylene glycol coated carbon nanostructure.
53. The method of claim 51, wherein The weight of the coating is in the range of 0.1-10% relative to the weight of the coated carbon nanostructure.
54. The method of claim 51, wherein The capped carbon nanostructure is provided in an amount of no greater than 1 wt % based on the weight of the composition when dry.
55. The method of claim 41, wherein the lithium transition metal compound is selected from the group consisting of lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide.
56. The method of claim 41, wherein the slurry further comprises a binder.
57. The method of claim 56, wherein the binder is polyvinylidene fluoride.
58. The method of claim 41, wherein the slurry further comprises a liquid.
59. The method of claim 58, wherein the liquid is selected from the group consisting of N-methylpyrrolidone, acetone, alcohol, water, and any combination thereof.
60. The method of claim 41, wherein the method produces fragments of carbon nanostructures and / or broken multi-walled carbon nanotubes, wherein the fragments of the carbon nanostructures include a plurality of multi-walled carbon nanotubes cross-linked into a polymeric structure by branching, interlacing, entanglement and / or sharing a common wall, in, The fragments of the carbon nanostructure are derived from the carbon nanostructure, have a reduced size, share the properties of the intact carbon nanostructure and can be identified by electron microscopy and other techniques, and The broken multi-walled carbon nanotubes are derived from a carbon nanostructure and are branched and share a common wall with each other.
61. Lithium batteries, including: a cathode comprising a lithium transition metal compound and a first carbon conductive additive; and an anode comprising an active anode material selected from graphite, silicon or lithium titanate and a second carbon conductive additive, wherein the first and second carbon conductive additives are selected from the group consisting of carbon nanostructures, fragments of carbon nanostructures, and broken multi-walled carbon nanotubes, wherein the carbon nanostructure or the fragment of the carbon nanostructure comprises a plurality of multi-walled carbon nanotubes cross-linked into a polymeric structure by branching, interlacing, entanglement and / or sharing a common wall, in, The fragments of the carbon nanostructure are derived from the carbon nanostructure, have a reduced size, share the properties of the intact carbon nanostructure and can be identified by electron microscopy and other techniques, and wherein the broken multi-walled carbon nanotubes are derived from a carbon nanostructure and are branched and share a common wall with each other, in: At least one of the multi-walled carbon nanotubes has a length equal to or greater than 2 micrometers, as determined by SEM, at least one of the multi-walled carbon nanotubes has an aspect ratio of length to diameter in the range of 200-1000, Along a 2 micron length of at least one of the multi-walled carbon nanotubes, there are at least two branches, as determined by SEM, At least one multi-walled carbon nanotube exhibits asymmetry with respect to the number of walls observed in the region after the branch point relative to the region before the branch point, and / or, there are no catalyst particles at or near the branch point, as determined by TEM.
62. The lithium battery of claim 61, wherein the multi-walled carbon nanotubes comprise 2-30 coaxial carbon nanotubes as determined by TEM at a magnification sufficient to count the number of walls.
63. The lithium battery of any one of claims 61-62, wherein at least 1% of the multi-walled carbon nanotubes have a length equal to or greater than 2 microns as determined by SEM, An aspect ratio of length to diameter in the range of 200-1000, and / or an asymmetry in the number of walls observed in the region after the branch point relative to the region before the branch point.