Polarizing plates for foldable displays

By using a polarizing plate with characteristic polyester film and phase difference layer in a foldable display, the problem of image distortion caused by repeated bending of the polarizing plate is solved, and the image is clear and stable.

CN113874766BActive Publication Date: 2024-11-12TOYOBO CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080038863.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-05-30
Filing Date
2020-05-15
Publication Date
2024-11-12
Estimated Expiration
2040-05-15

AI Technical Summary

Technical Problem

In foldable displays, polarizers are prone to deform after repeated bending, resulting in distortion of display images, and the prior art is difficult to effectively solve this problem.

Method used

The polyester film is used as the protective layer of the polarizer. The characteristics are that the refractive index in the bending direction is 1.590 to 1.620, the refractive index in the folding portion is 1.670 to 1.700, the refractive index in the thickness direction is 1.520 or less, and the density is 1.380 g/cm3 or more. , and a phase difference layer is provided on the polarizer to ensure that the polarizer is not prone to folding when it is repeatedly folded.

Benefits of technology

Effectively prevent the polarizer from deforming when folded repeatedly, ensure the clarity and stability of the image in the display, and avoid image distortion problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113874766B_ABST
    Figure CN113874766B_ABST
Patent Text Reader

Abstract

[Subject] The present invention provides: a polarizing plate for a foldable display without worrying about distortion of the image displayed at the folded portion after repeated bending. [Solution] A polarizing plate for a foldable display, wherein a polarizing plate protective film comprising a polyester film is laminated on at least one side of the polarizer, and the aforementioned polyester film satisfies the following conditions. (1) The refractive index in the bending direction is 1.590 to 1.620; (2) The refractive index in the direction of the folded portion is 1.670 to 1.700; (3) The refractive index in the thickness direction is less than 1.520; (4) The density is 1.380 g / cm 3 (Here, the bending direction refers to the direction perpendicular to the folded portion when the polyester film is folded.)
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to: a polarizing plate for a foldable display, a circularly polarizing plate for a foldable display, a method for manufacturing a circularly polarizing plate for a foldable display, and a foldable display. Background Art

[0002] As the lightweight of mobile terminal devices is promoted, mobile terminal devices represented by smartphones have become widely popular. Mobile terminal devices are required to have various functions, but also convenience. Therefore, in popular mobile terminal devices, it is assumed that they can be easily operated with one hand and can be stored in a pocket of clothes, so a small screen size of about 6 inches is sometimes required.

[0003] On the other hand, tablet terminals with a screen size of 7 to 10 inches are expected to be used not only for video content and music but also for business purposes, drawing purposes, reading, etc., and have high functionality. However, they cannot be operated with one hand and have poor mobility, which poses a problem in terms of convenience.

[0004] In order to achieve these problems, a method of connecting a plurality of displays to make them compact has been proposed (see Patent Document 1). However, since the frame portion remains, the image is interrupted, which causes a problem of reduced visibility and has not yet been widely used.

[0005] Therefore, in recent years, mobile terminals equipped with flexible displays or foldable displays have been proposed. In this way, the image is not interrupted, and the convenience of carrying the mobile terminal device equipped with a large-screen display is good.

[0006] In liquid crystal displays, linear polarizers are provided on both sides of the liquid crystal unit, and in EL displays, circular polarizers are provided on the visible side of the unit to prevent reflection. However, in the case of a display that is formed on one side by a folded portion, a flexible polarizer with sufficient polarization degree must be used. However, in a foldable display, the portion that contacts the fixed folded portion is repeatedly bent, so there is a problem that the polarizer at this portion deforms over time, causing the image displayed on the display to be distorted.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2010-228391 Summary of the invention

[0010] Problem that the invention aims to solve

[0011] The present invention intends to provide: a polarizing plate and a circularly polarizing plate for a foldable display, which do not require a concern that an image displayed at a folded portion will be distorted after repeated bending, a method for manufacturing a circularly polarizing plate, and a foldable display.

[0012] Solutions for solving problems

[0013] That is, the present invention includes the following configurations.

[0014] 1. A polarizing plate for a foldable display, wherein a polarizing plate protective film composed of a polyester film is laminated on at least one surface of a polarizing plate, wherein the polyester film satisfies the following conditions.

[0015] (1) The refractive index in the bending direction is 1.590 to 1.620

[0016] (2) The refractive index in the direction of the folded portion is 1.670 to 1.700

[0017] (3) The refractive index in the thickness direction is 1.520 or less

[0018] (4) Density: 1.380 g / cm 3 above

[0019] (Here, the bending direction refers to the direction perpendicular to the folded portion when the polyester film is folded.)

[0020] 2. A circularly polarizing plate for a foldable display, comprising: a retardation layer on at least one surface of the polarizing plate for a foldable display described in the first aspect.

[0021] 3. The circularly polarizing plate for a foldable display according to item 2 above, wherein no self-supporting film other than the polyester film exists, or only one self-supporting film exists.

[0022] 4. The polarizing plate for a foldable display according to item 1 above, wherein the polarizer has a thickness of 12 μm or less.

[0023] 5. The circularly polarizing plate for a foldable display according to item 2 or 3, wherein the thickness of the polarizer is 12 μm or less.

[0024] 6. The polarizing plate for a foldable display according to item 1 or 4, wherein the polarizer contains a polymerizable liquid crystal compound and a dichroic dye.

[0025] 7. The circularly polarizing plate for a foldable display according to item 2, 3 or 5, wherein the polarizer contains a polymerizable liquid crystal compound and a dichroic dye.

[0026] 8. A foldable display comprising the polarizing plate for a foldable display as described in item 1, 4 or 6 above.

[0027] 9. A foldable display comprising the circularly polarizing plate for a foldable display as described in item 2, 3, 5 or 7 above, wherein the phase difference layer comprises a liquid crystal compound.

[0028] 10. A method for manufacturing a circular polarizing plate for a foldable display, comprising the following steps:

[0029] (A) a process for preparing a polyester film having the following properties,

[0030] (1) The refractive index in the bending direction is 1.590 to 1.620,

[0031] (2) The refractive index in the direction of the folded portion is 1.670 to 1.700,

[0032] (3) The refractive index in the thickness direction is less than 1.520,

[0033] (4) Density: 1.380 g / cm 3 above,

[0034] (Here, the bending direction refers to the direction perpendicular to the folded portion when the polyester film is folded.)

[0035] (B) a step of providing a polarizing plate on the polyester film by any of the methods (a) and (b),

[0036] (a) a method of transferring a polarizing plate provided on a releasable supporting substrate to a substrate film,

[0037] (b) a method of forming a polarizing plate by coating a composition for a polarizing film comprising a polymerizable liquid crystal compound and a dichroic dye on a substrate film and aligning the composition; and,

[0038] (C) A step of laminating a retardation layer on the polarizing plate.

[0039] 11. A method for manufacturing a circular polarizing plate for a foldable display, comprising the following steps:

[0040] (A) a process for preparing a polyester film having the following properties,

[0041] (1) The refractive index in the bending direction is 1.590 to 1.620,

[0042] (2) The refractive index in the direction of the folded portion is 1.670 to 1.700,

[0043] (3) The refractive index in the thickness direction is less than 1.520,

[0044] (4) Density: 1.380 g / cm 3 above,

[0045] (Here, the bending direction refers to the direction perpendicular to the folded portion when the polyester film is folded.)

[0046] (B) a step of laminating a polarizing plate on the polyester film; and,

[0047] (C) a step of providing a phase difference layer on the polarizing plate by any of the methods (c) and (d),

[0048] (c) a method of transferring a phase difference layer provided on a releasable supporting substrate onto a polarizing plate,

[0049] (d) A method of forming a retardation layer by coating a composition for a retardation layer containing a liquid crystal compound on a polarizing plate and aligning the composition.

[0050] 12. The method for producing a circularly polarizing plate for a foldable display according to item 10, wherein (C) the step of laminating a phase difference layer on the polarizing plate is any of the following methods:

[0051] (c) a method of transferring a phase difference layer provided on a releasable supporting substrate onto a polarizing plate; or

[0052] (d) A method of forming a retardation layer by coating a composition for a retardation layer containing a liquid crystal compound on a polarizing plate and aligning the composition.

[0053] Effects of the Invention

[0054] The polarizing plate and circular polarizing plate of the present invention are not prone to creases when repeatedly folded, and there is no need to worry about image distortion at the folded portion, so they can be suitable for foldable displays. In addition, the foldable display of the present invention can display an image without distortion at the folded portion. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 It is a schematic diagram for illustrating the bending radius when the foldable display of the present invention is folded.

[0056] Figure 2 This is a schematic diagram for illustrating the bending direction of the polyester film used in the polarizing plate for a foldable display of the present invention. DETAILED DESCRIPTION

[0057] (monitor)

[0058] The display referred to in the present invention refers to all display devices. The types of displays include LCD, organic EL display, inorganic EL display, LED, FED, etc., but LCD, organic EL, and inorganic EL having a bendable structure are preferred. In particular, organic EL and inorganic EL that can reduce the layer structure are particularly preferred, and organic EL with a wide color gamut is further preferred.

[0059] (Foldable Display)

[0060] For a foldable display, a continuous single display can be folded in half or the like when moving. By folding, the size is reduced by half, and mobility can be improved. The bending radius of the foldable display is preferably 5 mm or less, and more preferably 3 mm or less. When the bending radius is 5 mm or less, thinning in the folded state becomes possible. It can be said that the smaller the bending radius, the better, but the smaller the bending radius, the easier it is to produce creases. The bending radius is preferably 0.1 mm or more, can be 0.5 mm or more, and can be 1 mm or more. Even if the bending radius is 1 mm, it is possible to achieve a thinness that is practical enough when moving. The bending radius when folded refers to the measurement of Figure 1 The radius of the inner side of the folded portion when folded is obtained from the position of the symbol 11 in the schematic diagram. It should be noted that the surface protection film described later may be located on the outer side or the inner side of the folded foldable display.

[0061] In addition, the foldable display may be folded in three or four, or may be a so-called rollable type, all of which are included in the scope of the foldable display of the present invention.

[0062] A.Polarizing plate

[0063] Polarizing plates are used in foldable displays. In liquid crystal displays, polarizing plates are provided on both sides of the liquid crystal cell, and in EL displays, circular polarizing plates are often used to prevent reflection of the internal structure.

[0064] The polarizing plate preferably has a laminated structure of a polarizing plate and a polarizing plate protective film for protecting the polarizing plate as a representative structure.

[0065] 1. Polarizer protective film

[0066] First, the polarizer protective film of the polarizing plate is described. In the present invention, the polarizer protective film is preferably a film made of polyester. Hereinafter, when the polarizer protective film is described alone, the polarizer protective film is sometimes referred to as a polyester film.

[0067] The polyester film may be a single-layer film composed of one or more polyester resins, or, when two or more polyesters are used, may be a multilayer film or a super-multilayer laminated film having a repeated structure.

[0068] Examples of the polyester resin used in the polyester film include polyethylene terephthalate, polybutylene terephthalate, polyethylene 2,6-naphthalate, or a polyester film formed of a copolymer having the constituent components of these resins as the main component. Among them, a stretched polyethylene terephthalate film is particularly preferred from the perspectives of mechanical properties, heat resistance, transparency, price, etc.

[0069] When a polyester copolymer is used in a polyester film, as the dicarboxylic acid component of the polyester, for example, aliphatic dicarboxylic acids such as adipic acid and sebacic acid; aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, and 2,6-naphthalene dicarboxylic acid; polyfunctional carboxylic acids such as trimellitic acid and pyromellitic acid. In addition, as the diol component, for example, aliphatic diols such as ethylene glycol, diethylene glycol, 1,4-butanediol, propylene glycol, and neopentyl glycol, aromatic diols such as terephthalic alcohol, alicyclic diols such as 1,4-cyclohexanedimethanol, and polyethylene glycol with an average molecular weight of 150 to 20,000 can be mentioned. The mass ratio of the copolymer components of the preferred copolymer is less than 20 mass%. When it is less than 20 mass%, it is preferred to maintain the film strength, transparency, and heat resistance.

[0070] In addition, in the manufacture of polyester film, the intrinsic viscosity of at least one or more resin pellets is preferably in the range of 0.50 to 1.0 dl / g. When the intrinsic viscosity is 0.50 dl / g or more, the impact resistance of the obtained film is improved, and it is not easy to cause the internal circuit of the display to break due to external impact, which is preferred. On the other hand, when the intrinsic viscosity is 1.00 dl / g or less, the filter pressure of the molten fluid will not increase excessively, and it is easy to operate the film production stably, which is preferred.

[0071] The thickness of the polyester film is preferably 10 to 80 μm, more preferably 25 to 75 μm. When the thickness is 10 μm or more, the workability is excellent and the impact resistance is improved. When the thickness is 80 μm or less, it is advantageous for weight reduction and has excellent flexibility, processability, and workability.

[0072] The haze of the polyester film is preferably 3% or less, more preferably 2% or less, and most preferably 1% or less. When the haze is 3% or less, the visibility of the image can be improved. The lower limit of the haze is as small as possible, but from the perspective of stable production, it is preferably 0.1% or more, and can be 0.3% or more.

[0073] As mentioned above, in order to reduce the haze, it is preferred that the surface roughness of the film is not too large. However, from the perspective of operability, as a method of forming roughness in order to impart a certain degree of slippage, particles can be blended into the polyester resin layer of the surface layer, or a coating layer containing particles can be applied in the middle of film formation to form roughness.

[0074] As a method for blending particles in the polyester resin layer, a known method can be used. For example, it can be added at any stage of the polyester production, preferably in the stage of esterification or after the end of the transesterification reaction and before the start of the polycondensation reaction, in the form of a slurry dispersed in ethylene glycol, etc., and the polycondensation reaction is promoted. In addition, it can be carried out by the following methods, etc.: a method of blending a slurry of particles dispersed in ethylene glycol or water, etc. with a polyester raw material using a kneading extruder with a vent; or a method of blending dried particles with a polyester raw material using a kneading extruder.

[0075] Among them, the following method is preferred: adding the inorganic particles in the form of aggregates uniformly dispersed in a monomer solution that is a part of the polyester raw material and then filtered to the remaining portion of the polyester raw material before, during or after the esterification reaction. According to this method, since the monomer solution has a low viscosity, it is easy to uniformly disperse the particles and filter the slurry with high precision, and when adding to the remaining portion of the raw material, the particles have good dispersibility and are less likely to form new aggregates. From the above viewpoints, it is particularly preferred to add to the remaining portion of the raw material in a low temperature state before the esterification reaction.

[0076] Alternatively, the number of protrusions on the film surface can be further reduced by obtaining a polyester containing particles in advance and then kneading and extruding the pellets with pellets containing no particles (masterbatch method).

[0077] The polyester film may contain various additives within a range in which the total light transmittance is maintained within a preferred range. Examples of the additives include antistatic agents, UV absorbers, and stabilizers.

[0078] The total light transmittance of the polyester film is preferably 85% or more, more preferably 87% or more. If the transmittance is 85% or more, visibility can be fully ensured. It can be said that the higher the total light transmittance of the polyester film, the better, but from the perspective of stable production, it is preferably 99% or less, and can be 97% or less.

[0079] The maximum heat shrinkage of the polyester film after heat treatment at 150°C for 30 minutes is preferably 6% or less, and more preferably 5% or less. If the heat shrinkage is 6% or less, plane defects such as curling and ripples during lamination can be suppressed. It can be said that the lower the heat shrinkage, the better, but it is preferably -1% or more, and preferably 0% or more. The negative sign here means that expansion occurs after heating, and if it is -1% or more, there is no need to worry about plane defects and it is preferred.

[0080] Next, regarding the method for producing a biaxially stretched polyester film, an example of using polyethylene terephthalate (hereinafter, sometimes referred to as PET) pellets as a raw material for the polyester film is described in detail, but the invention is not limited thereto. In addition, the number of layers such as a single-layer structure and a multi-layer structure is not limited.

[0081] After the pellets of PET are mixed and dried in a prescribed ratio, they are supplied to a known melt lamination extruder, extruded from a slit-shaped die into a sheet, cooled and solidified on a casting roll to form an unstretched film. In the case of a single layer, one extruder may be used, and in the case of a multi-layer film, two or more extruders, a multi-manifold or a confluence block (e.g., a confluence block with a square confluence portion) may be used to laminate a plurality of film layers constituting each outermost layer, extrude a sheet of two or more layers from a nozzle, and cool it on a casting roll to form an unstretched film.

[0082] In the above case, during melt extrusion, it is preferred to perform high-precision filtration to remove foreign matter contained in the resin while the molten resin is maintained at an arbitrary position of about 280° C. The filter material used in the high-precision filtration of the molten resin is not particularly limited, and a filter material made of sintered stainless steel is preferred because it excels in removing aggregates having Si, Ti, Sb, Ge, and Cu as main components and high-melting-point organic matter.

[0083] Furthermore, the filter particle size (initial filtration efficiency 95%) of the filter material is preferably less than 20 μm, particularly preferably less than 15 μm. When the filter particle size (initial filtration efficiency 95%) of the filter material exceeds 20 μm, foreign matter larger than 20 μm cannot be fully removed. Although the high-precision filtration of the molten resin by using a filter material having a filter particle size (initial filtration efficiency 95%) of less than 20 μm may sometimes reduce productivity, it is preferred in terms of obtaining a film with fewer protrusions generated by coarse particles.

[0084] (Refractive index with respect to bending direction)

[0085] In the present invention, the refractive index of at least one of the longitudinal direction (mechanical flow direction) and the width direction of the polyester film is preferably 1.590 to 1.620, and more preferably 1.591 to 1.600. In addition, the refractive index of the polyester film as a polarizer protective film when a polarizing plate is prepared is preferably 1.590 to 1.620, and more preferably 1.591 to 1.600. Here, the bending direction refers to, for example Figure 2As shown by symbol 22 on the polyester film (symbol 2), it is a direction orthogonal to the folding portion (symbol 21) envisioned in the use of the foldable display. When the refractive index in at least one of the length direction and the width direction is 1.590 to 1.620, there is less deformation during repeated folding, and there is no worry about the image quality of the foldable display being reduced, which is preferred. The refractive index is more preferably 1.591 to 1.600. Of course, this direction is preferably the aforementioned bending direction. If it is above 1.590, there is no worry about cracks in the direction of the folding portion after the bending test described later, and of course no breakage occurs, so the visibility of the display can be maintained well. The refractive index of the polyester film can be effectively adjusted by adjusting the stretching ratio and the stretching temperature. In addition, in order to adjust the refractive index, a relaxation process in the stretching direction and multi-stage stretching can be used. In the case of multi-stage stretching, it is preferred to make the stretching ratio of the second stage and thereafter higher than the stretching ratio of the first stage.

[0086] By controlling the refractive index of at least one of the length direction (mechanical flow direction) and the width direction of the polyester film within the above range, and more preferably controlling the refractive index of the bending direction within the above range, fatigue caused by the compressive stress applied to the inner side of the fold when folding can be reduced. It is believed that fatigue caused by compressive stress mainly occurs in the crystal part, and the less crystallization in the bending direction, the less fatigue. Therefore, it can be considered that by reducing the refractive index, the amount of oriented crystallization in the bending direction is reduced, and compression fatigue is suppressed.

[0087] In addition, by reducing the refractive index, the creep phenomenon caused by the tensile stress applied to the outside of the fold during folding can be suppressed. It is believed that fatigue caused by tensile stress mainly occurs in the amorphous part, and the alignment of the molecular chains occurs due to the repeated stress, resulting in deformation. It can be inferred that when there are fewer molecular chains arranged in the bending direction, the deformation caused by alignment is less. In addition, when there are fewer amorphous parts, fatigue caused by stretching can be suppressed, so it is preferred that the crystallinity, that is, the density is high.

[0088] In the present invention, for the unstretched polyester sheet, the stretching ratio in at least one of the longitudinal direction (mechanical flow direction) and the width direction is preferably set to 1.2 to 2.0 times, and more preferably 1.7 to 2.0 times. In addition, the stretching direction is preferably the aforementioned bending direction. When the stretching ratio is 1.2 times or more, there is no deformation in post-processing such as hard coating, so it is preferred. When the stretching ratio is 2.0 times or less, no uneven thickness of the film occurs, so it is preferred. As the stretching temperature, 75 to 120°C is preferred, and 75 to 105°C is more preferred. It should be noted that the heating method during stretching can adopt the previously known means such as hot air heating, roller heating, infrared heating, etc. By setting the stretching temperature to 75 to 120°C, the large uneven thickness caused by stretching at the above-mentioned stretching ratio can be prevented. In addition, by stretching at a low temperature as low as possible within the range that does not produce the aforementioned large uneven thickness, the refractive index in the thickness direction can be reduced.

[0089] (Refractive index with respect to the direction of the folded portion)

[0090] The refractive index of the polyester film in the direction orthogonal to the direction in which the refractive index is 1.590 to 1.620 is preferably 1.670 to 1.700. That is, the refractive index in the direction orthogonal to the bending direction (the direction of the folded portion) is preferably 1.670 to 1.700. By setting it to 1.670 to 1.700, the deformation during folding along the bending direction can be reduced. By setting it to less than 1.700, cracks or breaks in the direction of the folded portion can be suppressed. By setting it to more than 1.670, the bendability in the bending direction can be improved. More preferably 1.680 to 1.695. As a method for adjusting the refractive index in the direction orthogonal to the bending direction, stretching ratio, stretching preheating temperature, stretching temperature, multi-stage stretching, and film relaxation can be listed. The stretching ratio is preferably 4.0 to 6.0 times, and more preferably 4.4 to 6.0 times. In addition, the stretching preheating temperature in the direction orthogonal to the bending direction is preferably 70 to 110°C. When multiple stretching is performed in a direction perpendicular to the bending direction, the stretching ratios in the second and subsequent stages are preferably higher than those in the first stage. The film may be relaxed by 1 to 10% in both the machine flow direction (length direction) and the perpendicular direction (width direction).

[0091] (Refractive index in the thickness direction)

[0092] The refractive index in the thickness direction is preferably 1.520 or less. This is because, by setting it to 1.520 or less, the orientation in the plane can be made firm and the deformation during folding can be reduced. It is more preferably 1.515 or less, further preferably 1.510 or less, particularly preferably 1.505 or less, and most preferably 1.500 or less. A low refractive index in the thickness direction is preferred, but from the perspective of stable production, it is preferably 1.3 or more, and further can be 1.4 or more. It is particularly preferably 1.410 or more. It can be said that the above range can be achieved by increasing the stretching ratio in both the bending direction and the folding direction, but in order to control the refractive index in the bending direction and the width direction within the preferred range and control the refractive index in the thickness direction, it is preferred to set the conditions while confirming the balance of the conditions of each process of the film-making process.

[0093] The methods for controlling the refractive index in the thickness direction within the above range include: the stretching preheating temperature in the bending direction, the stretching temperature, the stretching ratio, the stretching preheating temperature in the direction of the folded portion, the stretching temperature, the multi-stage stretching, the high-ratio stretching, or the temperature setting of the heat setting. The stretching preheating temperature in the bending direction is preferably 70°C to 110°C. The stretching temperature in the bending direction is preferably 75 to 120°C. The stretching ratio in the bending direction is preferably 1.2 to 2.0 times, and more preferably 1.7 to 2.0 times. By lowering the stretching temperature and stretching at a low stretching ratio, the refractive index in the thickness direction can be effectively reduced while maintaining the bendability in the bending direction. The stretching preheating temperature in the folded portion direction is also preferably 75°C to 110°C. The stretching temperature is preferably 75 to 120°C. The stretching ratio of the folded portion is preferably 4.0 to 6.0 times, and more preferably 4.4 to 6.0 times. The refractive index in the bending direction can be maintained or reduced while effectively reducing the refractive index in the thickness direction. As a method of high-ratio stretching, multi-stage stretching can be used. At this time, it is preferred to make the stretching ratio of the second section higher than the stretching ratio of the first section so as to effectively control the refractive index. In addition, a method of stretching again after the crystallization step can also be used. It is also possible to use accelerated stretching in which the stretching speed is increased from the initial stage of stretching to the second half.

[0094] The heat setting temperature is preferably 180 to 240° C. By heat setting, oriented crystallization in the stretching direction proceeds, and the refractive index in the thickness direction can be reduced.

[0095] The reason why the hardness of the film surface is improved by reducing the refractive index in the thickness direction is not necessarily clear, but it is considered that aromatic groups such as benzene rings in the molecular chain are oriented in the plane direction, which has the effect of suppressing deformation caused by stress applied in the thickness direction.

[0096] (About the density of polyester film)

[0097] The density of the polyester film is preferably 1.380 g / cm3 More preferably 1.383 g / cm 3 By setting it to 1.380g / cm 3 The higher the density, the better. It also depends on the presence or absence of particles in the film, but 1.40 g / cm is preferred. 3 By setting the heat setting temperature during film formation to 180 to 240° C., crystallization can be promoted and the density can be effectively increased.

[0098] The bending direction of the polyester film preferably corresponds to the longitudinal direction (mechanical flow direction). As a result, it is easy to reduce the refractive index in the bending direction during biaxial stretching, and it is easy to improve the bendability. That is, a polyester film can be obtained by preferably stretching the unstretched polyester sheet along the longitudinal direction at a stretching ratio of 1.2 to 2.0 times, more preferably 1.7 to 2.0 times. In addition, stretching along the width direction at a stretching ratio of 4.0 to 6.0 times, more preferably 4.4 to 6.0 times can be said to be a preferred method.

[0099] In addition, in the present invention, it is particularly preferred that the polyester film has the following four properties at the same time:

[0100] (1) The refractive index in the bending direction is 1.590 to 1.620

[0101] (2) The refractive index in the direction of the folded portion is 1.670 to 1.700

[0102] (3) The refractive index in the thickness direction is 1.520 or less

[0103] (4) Density: 1.380 g / cm 3 above

[0104] However, even in the case of a combination within the range of the above-mentioned preferred manufacturing conditions, such as a combination in which the stretch ratio in the bending direction is 1.4 times or less, the stretch ratio in the folding direction is less than 4.4 times, and the heat setting temperature is 220°C or less, which is not the best combination within the range of each preferred manufacturing condition, a polyester film that satisfies the above-mentioned four characteristics may not necessarily be obtained at the same time. In this case, by fine-tuning any of the conditions such as increasing the stretch ratio in the bending direction to 1.7 times or more, increasing the stretch ratio in the folding direction to 4.4 times or more, increasing the heat setting temperature to about 230°C, or lowering the stretching temperature in the bending direction and / or the folding direction, or by a combination thereof, the above-mentioned four characteristics can be satisfied at the same time.

[0105] In order to adjust film forming properties, film strength, thermal dimensional stability, appearance defects, etc., any film forming method such as stretching, relaxation, heat setting, surface treatment, etc. can be adopted, but controlling the refractive index and density of the film within the above preferred ranges can be said to be a particularly preferred method in the present invention. By controlling the refractive index and density within the preferred ranges, a polyester film suitable for foldable displays can be provided.

[0106] Specifically, for example, after the PET pellets are fully vacuum dried, they are supplied to an extruder, melt-extruded into a sheet at about 280°C and cooled to solidify to form an unstretched PET sheet. The obtained unstretched sheet is stretched to 1.2 to 2.0 times, more preferably 1.7 to 2.0 times, in the length direction with a roller heated to 75 to 120°C to obtain a uniaxially oriented PET film. Furthermore, the end of the film is gripped with a clamp, introduced into a hot air zone heated to 75 to 120°C for drying, and then stretched to 4.0 to 6.0 times, more preferably 4.4 to 6.0 times in the width direction. Next, it can be introduced into a heat treatment zone at 180 to 240°C for 1 to 60 seconds of heat treatment. In this heat treatment process, a relaxation treatment of 0 to 10% can be performed in the width direction or the length direction as needed.

[0107] The intrinsic viscosity of the polyester film is preferably in the range of 0.50 to 1.0 dl / g. If the intrinsic viscosity is 0.50 dl / g or more, not only the film-forming property of the film is stable, but also the impact resistance is improved, and cracks caused by external impact are not easily generated, which is preferred. On the other hand, if the intrinsic viscosity is 1.00 dl / g or less, the filter pressure of the molten fluid will not increase excessively, and the film production is stable, which is preferred.

[0108] (Easy Adhesion Layer)

[0109] In order to improve adhesion with a polarizing film or an alignment layer described later, an easy-adhesion layer (easy-adhesion layer P1) may be provided on the polyester film.

[0110] As the resin used in the easy bonding layer, polyester resin, polyurethane resin, polyester polyurethane resin, polycarbonate resin, polycarbonate polyurethane resin, acrylic resin etc. can be cited, wherein, preferably polyester resin, polyester polyurethane resin, polycarbonate polyurethane resin and acrylic resin. The easy bonding layer is preferably cross-linked. As a cross-linking agent, isocyanate compounds, melamine compounds, epoxy resins, oxazoline compounds etc. can be cited. In addition, adding polyvinyl alcohol, polyamide, polyimide, polyamide-imide etc. and resins similar to the resins used in the orientation layer or polarizing film is also a useful means for improving adhesion.

[0111] The easy-adhesion layer can be formed by applying a water-based coating material to which these resins and, if necessary, a crosslinking agent, particles, etc. are added to a polyester film and drying the coating material. Examples of the particles include those used in the above-mentioned base materials.

[0112] The easy-adhesion layer can be provided offline on the stretched substrate film, or it can be provided online in the film-forming process. The easy-adhesion layer is preferably provided online in the film-forming process. When the easy-adhesion layer is provided online, it can be provided before the longitudinal stretching or before the transverse stretching. It is particularly preferred to apply the aforementioned water-based coating immediately before the transverse stretching, preheat and heat it using a tenter, and dry and cross-link it in the heat treatment process, so as to provide the easy-adhesion layer online. It should be noted that when the online coating is performed immediately before the longitudinal stretching using a roller, it is preferred that after the aforementioned water-based coating is applied, it is dried using a vertical dryer and then introduced into the stretching roller. The coating amount of the aforementioned water-based coating is preferably 0.01 to 1.0 g / m 2 , more preferably 0.03 to 0.5 g / m 2 .

[0113] (Functional layer)

[0114] It is also a preferred embodiment to provide a functional layer such as a hard coat layer, an antireflection layer, a low reflection layer, an antiglare layer, an antistatic layer, etc. on the side of the polyester film opposite to the side on which the polarizing film is laminated.

[0115] The thickness of these functional layers can be appropriately set, and is preferably 0.1 to 50 μm, more preferably 0.5 to 20 μm, and further preferably 1 to 10 μm. In addition, these layers may be provided in a plurality of layers.

[0116] When a functional layer is provided, an easy bonding layer (easy bonding layer P2) may be provided between the functional layer and the substrate film. The resins and cross-linking agents listed in the above-mentioned easy bonding layer P1 are suitable for use in the easy bonding layer P2. In addition, the easy bonding layer P1 and the easy bonding layer P2 may have the same composition or different compositions.

[0117] The easy-adhesive layer P2 is also preferably provided in-line. The easy-adhesive layer P1 and the easy-adhesive layer P2 can be formed by sequentially coating and drying. In addition, it is also a preferred method to simultaneously coat the easy-adhesive layer P1 and the easy-adhesive layer P2 on both sides of the polyester film.

[0118] It should be noted that in the following description, the polarizer protective film and polyester film include not only the case where an easy adhesion layer is not provided but also the case where an easy adhesion layer is provided. Similarly, the case where a functional layer is provided is also included in the polarizer protective film and polyester film.

[0119] 2. Polarizer

[0120] The polarizer (polarizing film) of the polarizing plate used in the present invention can be directly arranged on the polarizer protective film, or an orientation layer can be arranged on the polarizer protective film and arranged on the orientation layer. It should be noted that in the present invention, the orientation film and the polarizing film are sometimes collectively referred to as polarizers. In addition, when a polarizing film is arranged on the polarizer protective film without an orientation film, the polarizing film is sometimes referred to as a polarizer.

[0121] (Polarizing film)

[0122] The polarizing film has the function of passing polarized light only in one direction. The polarizing film can be formed by mixing iodine or dichroic pigments in a stretched film of polyvinyl alcohol (PVA) or the like, a coating film obtained by mixing dichroic pigments in a dichroic pigment film or a polymerizable liquid crystal compound, a stretched film of polyene, a wire grid, etc. without particular limitation.

[0123] Among them, a polarizing film in which iodine is adsorbed in PVA and a polarizing film in which a dichroic dye is blended in a polymerizable liquid crystal compound are preferred examples.

[0124] First, a polarizing film in which iodine is adsorbed into PVA will be described.

[0125] A polarizing film in which iodine is adsorbed in PVA can generally be obtained by immersing an unstretched PVA film in a bath containing iodine and then uniaxially stretching it, or by immersing a uniaxially stretched film in a bath containing iodine and then crosslinking it in a boric acid bath.

[0126] The thickness of the polarizing film is preferably 1 to 30 μm, more preferably 1.5 to 20 μm, and further preferably 2 to 15 μm. If the thickness of the polarizing film is less than 1 μm, sufficient polarization characteristics cannot be obtained, and it is sometimes difficult to handle because it is too thin. If the thickness of the polarizing film exceeds 30 μm, it does not meet the purpose of being thin to ensure flexibility.

[0127] When the polarizing film adsorbed with iodine in PVA is laminated with the polarizer protective film, it is preferred to laminate the polarizing film with the polarizer protective film. As the adhesive for laminating, any adhesive that has been used by users can be used without restriction. Among them, water-based adhesives and ultraviolet curing adhesives of PVA are preferred examples, and ultraviolet curing adhesives are more preferred.

[0128] In this way, the polarizing film adsorbed with iodine in PVA can be used as a separate film of polarizer, and laminated with the polarizer protective film. Alternatively, it is also possible to laminate the polarizing film by transferring the polarizing film to the polarizer protective film by using a release support substrate coated with PVA, stretched in this state, and a polarizer laminated on the release support substrate (release support substrate laminated polarizer). The method of laminating by the transfer is also the same as the above-mentioned laminating method, preferably as a laminating method of polarizer and polarizer protective film. In the case of the transfer method, the thickness of the polarizer is preferably 12 μm or less, more preferably 10 μm or less, further preferably 8 μm or less, and particularly preferably 6 μm or less. Even if it is such a very thin polarizer, there is a release support substrate, therefore, it is also easy to operate, and the polarizer can be easily laminated to the polarizer protective film. By using such a thin polarizer, further repeated flexibility can be ensured. In addition, the technique of laminating a polarizing plate and a polarizing plate protective film is well known, and for example, Japanese Patent Application Laid-Open Nos. 2001-350021 and 2009-93074 can be referred to.

[0129] The method of laminating polarizers and polarizer protective films by transfer is specifically described. First, PVA is coated on a release support substrate of a thermoplastic resin that is not stretched or uniaxially stretched perpendicular to the length direction, and the laminate of the release support substrate of the thermoplastic resin and PVA is stretched to 2 to 20 times, preferably 3 to 15 times, in the length direction. The stretching temperature is preferably 80 to 180°C, more preferably 100 to 160°C. Then, the stretched laminate is immersed in a bath containing a dichroic pigment to adsorb the dichroic pigment. As dichroic pigments, for example, iodine, organic dyes, etc. can be cited. When iodine is used as a dichroic pigment, an aqueous solution containing iodine and potassium iodide is preferably used as a dyeing bath. Then, it is immersed in an aqueous solution of boric acid for treatment, washed with water, and dried. It should be noted that 1.5 to 3 times of stretching can be performed as a pre-stretching before the dichroic pigment is adsorbed. It should be noted that the above method is an example, and the dichroic pigment can be adsorbed before stretching, and boric acid can also be used to treat before the dichroic pigment is adsorbed. It is also possible to stretch in a bath containing a dichroic pigment or a bath of boric acid solution. In addition, these steps can be combined in multiple stages.

[0130] As the release support substrate (release film) of the thermoplastic resin, polyester films such as polyethylene terephthalate, polyolefin films such as polypropylene and polyethylene, polyamide films, polyurethane films, etc. are used. The release support substrate (release film) of the thermoplastic resin can be subjected to corona treatment or provided with a release coating, an easy-adhesion coating, etc., so that the peeling force can be adjusted.

[0131] The polarizer surface of the laminated polarizer of the release support substrate is attached to the polarizer protective film by an adhesive or an adhesive, and then the release support substrate is peeled off to obtain a laminate of the polarizer protective film and the polarizer. The thickness of the adhesive commonly used is 5 to 50 μm, and the thickness of the adhesive is 1 to 10 μm. It is preferred to use an adhesive for thinning, and more preferably, an ultraviolet curing adhesive. It is also preferred to use an adhesive in the process that does not require special equipment.

[0132] Next, a polarizing film in which a dichroic dye is blended with a polymerizable liquid crystal compound will be described.

[0133] A dichroic dye is a dye having a property in which the absorbance in the long axis direction of the molecule is different from the absorbance in the short axis direction.

[0134] The dichroic pigment preferably has a maximum absorption wavelength (λMAX) in the range of 300 to 700 nm. Examples of such dichroic pigments include organic dichroic pigments such as acridine pigments, oxazine pigments, cyanine pigments, naphthalene pigments, azo pigments, and anthraquinone pigments, among which azo pigments are preferred. Azo pigments include monoazo pigments, disazo pigments, triazo pigments, tetrazo pigments, and stilbene azo pigments, among which disazo pigments and triazo pigments are preferred. The dichroic pigments may be used alone or in combination of two or more. In order to adjust the (achromatic) hue, it is preferred to combine two or more. It is particularly preferred to use three or more in combination. It is particularly preferred to use three or more azo compounds in combination.

[0135] Preferred azo compounds include dyes described in JP-A-2007-126628, JP-A-2010-168570, JP-A-2013-101328, JP-A-2013-210624, and the like.

[0136] It is also a preferred embodiment that the dichroic dye is a dichroic dye polymer introduced into the side chain of an acrylic polymer. Examples of these dichroic dye polymers include polymers listed in Japanese Patent Publication No. 2016-4055, polymers obtained by polymerizing compounds of [Chemical Formula 6] to [Chemical Formula 12] in Japanese Patent Publication No. 2014-206682, and the like.

[0137] The content of the dichroic dye in the polarizing film is preferably 0.1 to 30% by mass, more preferably 0.5 to 20% by mass, further preferably 1.0 to 15% by mass, and particularly preferably 2.0 to 10% by mass in the polarizing film from the viewpoint of achieving good orientation of the dichroic dye.

[0138] The polarizing film preferably contains a polymerizable liquid crystal compound in order to improve film strength, polarization degree, film homogeneity, etc. The polymerizable liquid crystal compound includes a polymerized substance as a film.

[0139] The polymerizable liquid crystal compound is a compound having a polymerizable group and showing liquid crystallinity.

[0140] The polymerizable group refers to a group that participates in the polymerization reaction, preferably a photopolymerizable group. Here, the photopolymerizable group refers to a group that can produce a polymerization reaction through active free radicals, acids, etc. generated by the photopolymerization initiator described later. As the polymerizable group, vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, acryloyloxy, methacryloyloxy, oxirane, oxetane, etc. can be cited. Among them, acryloyloxy, methacryloyloxy, vinyloxy, oxirane and oxetane are preferred, and acryloyloxy is more preferred. The compound showing liquid crystal properties can be a thermotropic liquid crystal or a lyotropic liquid crystal. In addition, it can be a nematic liquid crystal in a thermotropic liquid crystal or a smectic liquid crystal.

[0141] In terms of obtaining higher polarization characteristics, the polymerizable liquid crystal compound is preferably a smectic liquid crystal compound, and more preferably a high-order smectic liquid crystal compound. If the liquid crystal phase formed by the polymerizable liquid crystal compound is a high-order smectic phase, a polarizing film with a higher degree of alignment order can be produced.

[0142] Specific examples of preferred polymerizable liquid crystal compounds include compounds described in JP-A-2002-308832, JP-A-2007-16207, JP-A-2015-163596, JP-A-2007-510946, JP-A-2013-114131, WO2005 / 045485, Lub et al. Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996), etc.

[0143] The content ratio of the polymerizable liquid crystal compound in the polarizing film is preferably 70 to 99.5% by mass, more preferably 75 to 99% by mass, further preferably 80 to 97% by mass, and particularly preferably 83 to 95% by mass in the polarizing film from the viewpoint of improving the orientation of the polymerizable liquid crystal compound.

[0144] The polarizing film including the polymerizable liquid crystal compound and the dichroic dye can be provided by coating the polarizing film composition.

[0145] The polarizing film composition may contain a solvent, a polymerization initiator, a sensitizer, a polymerization inhibitor, a leveling agent, a polymerizable non-liquid crystal compound, a crosslinking agent, and the like in addition to the polymerizable liquid crystal compound and the dichroic dye.

[0146] As a solvent, any solvent can be used without limitation as long as it dissolves the polymerizable liquid crystal compound. Specific examples of the solvent include water; alcohol solvents such as methanol, ethanol, isopropanol, ethylene glycol, propylene glycol, and cellosolve; ester solvents such as ethyl acetate, butyl acetate, and γ-butyrolactone; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, and cyclohexanone; aromatic hydrocarbon solvents such as toluene and xylene; ether solvents such as tetrahydrofuran and dimethoxyethane, etc. These solvents can be used alone or in combination.

[0147] The polymerization initiator can be used without limitation as long as it polymerizes the polymerizable liquid crystal compound. As the polymerization initiator, a photopolymerization initiator that generates active free radicals by light is preferred. As the polymerization initiator, for example, benzoin compounds, benzophenone compounds, alkylphenone compounds, acylphosphine oxide compounds, triazine compounds, iodonium salts, and sulfonium salts can be cited.

[0148] As the sensitizer, a photosensitizer is preferred. Examples of the photosensitizer include xanthone compounds, anthracene compounds, phenothiazine, and rubrene.

[0149] Examples of the polymerization inhibitor include hydroquinones, catechols, and thiophenols.

[0150] Examples of the leveling agent include various known surfactants.

[0151] As a polymerizable non-liquid crystal compound, it is preferably copolymerized with a polymerizable liquid crystal compound. For example, when the polymerizable liquid crystal compound has a (meth)acryloyloxy group, as a polymerizable non-liquid crystal compound, (meth)acrylates can be cited. (Meth)acrylates can be monofunctional or multifunctional. By using multifunctional (meth)acrylates, the strength of the polarizing film can be improved. When a polymerizable non-liquid crystal compound is used, it is preferably set to 1 to 15% by mass in the polarizing film, more preferably set to 2 to 10% by mass, and further preferably set to 3 to 7% by mass. If the content of the polymerizable non-liquid crystal compound exceeds 15% by mass, the degree of polarization is sometimes reduced.

[0152] Examples of the crosslinking agent include compounds that can react with functional groups of polymerizable liquid crystal compounds and polymerizable non-liquid crystal compounds, etc. Specific examples of the crosslinking agent include isocyanate compounds, melamine, epoxy resins, and oxazoline compounds.

[0153] The polarizing film composition may be directly applied onto a polarizer protective film or an alignment layer, and then dried, heated, and cured as necessary to form a polarizing film.

[0154] As the coating method, a coating method such as a gravure coating method, a die coating method, a bar coating method, and an applicator method; a printing method such as a flexographic method, and the like, and other known methods can be used.

[0155] Drying is performed by introducing the coated polarizer protective film into a hot air dryer, infrared dryer, etc., preferably at 30 to 170° C., more preferably 50 to 150° C., and further preferably 70 to 130° C. The drying time is preferably 0.5 to 30 minutes, more preferably 1 to 20 minutes, and further preferably 2 to 10 minutes.

[0156] The polarizing film may be heated in order to more firmly align the dichroic dye and the polymerizable liquid crystal compound in the polarizing film. The heating temperature is preferably set to a temperature range at which the polymerizable liquid crystal compound forms a liquid crystal phase.

[0157] The polarizing film composition contains a polymerizable liquid crystal compound, and therefore, is preferably cured. As a curing method, heating and light irradiation can be cited, preferably light irradiation. It can be fixed in a state where the dichroic pigment is oriented by curing. Curing is preferably performed in a state where a liquid crystal phase is formed in the polymerizable liquid crystal compound, and it can also be cured by light irradiation at a temperature showing a liquid crystal phase.

[0158] Examples of the light used in the light irradiation include visible light, ultraviolet light, and laser light, etc. Ultraviolet light is preferred because of its ease of handling.

[0159] The irradiation intensity varies depending on the type or amount of the polymerization initiator or the resin (monomer), but is preferably 100 to 10,000 mJ / cm2 based on 365 nm. 2 , more preferably 200 to 5000 mJ / cm 2 .

[0160] For polarizing film, the composition for polarizing film is applied to an orientation layer provided as required, so that the pigment is oriented along the orientation direction of the orientation layer, and as a result, the polarized light transmission axis becomes having a specified direction. When the composition for polarizing film is directly applied to a substrate without providing an orientation layer, polarized light is irradiated to cure the composition for polarizing film, thereby also being able to orient the polarizing film. At this time, polarized light in an oblique direction relative to the long dimension direction of the polarizer protective film is irradiated. It is preferably further heat treated thereafter, so that the dichroic pigment is firmly oriented along the orientation direction of the polymer liquid crystal.

[0161] The thickness of the polarizing film is usually 0.1 to 5 μm, preferably 0.3 to 3 μm, and more preferably 0.5 to 2 μm.

[0162] When a polarizing film comprising a polymerizable liquid crystal compound and a dichroic pigment is laminated with a polarizer protective film, it is preferred not only to directly arrange the polarizing film on the substrate film and laminate it, but also to arrange the polarizing film on another release film according to the above method, and to transfer it to the polarizer protective film. As a release film, a release support substrate laminated with the aforementioned release support substrate and a release support substrate used in a laminated polarizer can be cited as a preferred example, and polyester film, polypropylene film, etc. can be cited as particularly preferred release films. The release film is subjected to corona treatment, or a release coating, an easy-adhesion coating, etc. are provided, so that the peeling force can be adjusted.

[0163] The method of transferring the polarizing film to the polarizer protective film is also the same as the method in the case of the releasable supporting substrate-laminated polarizing plate laminated with the releasable supporting substrate described above.

[0164] (Orientation Layer)

[0165] The polarizing plate used in the present invention may be not only a polarizing film alone as described above, but may also be a combination of a polarizing film and an alignment layer.

[0166] The orientation layer controls the orientation direction of the polarizing film. By providing the orientation layer, a polarizing plate with a higher degree of polarization can be provided.

[0167] As the orientation layer, any orientation layer can be used as long as the polarizing film can be in a desired orientation state. As a method for providing the orientation layer with an orientation state, for example, a surface brushing treatment, an oblique evaporation of an inorganic compound, and a layer having microgrooves can be cited. Furthermore, a method of forming a photo-orientation layer that generates an orientation function by orienting molecules through light irradiation with polarized light is also preferred.

[0168] Hereinafter, two examples of a rubbing-treated alignment layer and a photo-alignment layer will be described.

[0169] (Brushing treatment of the alignment layer)

[0170] As the polymer material used for the alignment layer formed by the rubbing treatment, polyvinyl alcohol and its derivatives, polyimide and its derivatives, acrylic resins, polysiloxane derivatives, etc. are preferably used.

[0171] First, a coating solution for a brush-brushed alignment layer containing the above-mentioned polymer material is applied to a polarizer protective film, and then heated and dried to obtain an alignment layer before brush-brushing. The coating solution for the alignment layer may contain a crosslinking agent. Examples of the crosslinking agent include: compounds containing multiple isocyanate groups, epoxy groups, oxazoline groups, vinyl groups, acryl groups, carbodiimide groups, alkoxysilyl groups, etc.; amide resins such as melamine compounds; phenolic resins, etc.

[0172] As the solvent of the coating liquid for the brushing treatment orientation layer, any solvent can be used without limitation as long as it can dissolve the polymer material. Specific examples of the solvent include water; alcohol solvents such as methanol, ethanol, isopropanol, ethylene glycol, propylene glycol, and cellosolve; ester solvents such as ethyl acetate, butyl acetate, and γ-butyrolactone; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, and cyclohexanone; aromatic hydrocarbon solvents such as toluene and xylene; ether solvents such as tetrahydrofuran and dimethoxyethane, etc. These solvents can be used alone or in combination.

[0173] The concentration of the rubbing treatment alignment layer coating solution can be appropriately adjusted depending on the type of polymer, the thickness of the alignment layer to be produced, etc., and is preferably in the range of 0.2 to 20% by mass, more preferably 0.3 to 10% by mass, expressed as solid content concentration.

[0174] As the coating method, a coating method such as a gravure coating method, a die coating method, a bar coating method, and an applicator method; a printing method such as a flexographic method, and the like, and a known method are used.

[0175] The temperature of heating and drying also depends on the polarizer protective film. In the case of PET, it is preferably in the range of 30 to 170°C, more preferably in the range of 50 to 150°C, and further preferably in the range of 70 to 130°C. If the drying temperature is too low, a longer drying time is required, and productivity is sometimes poor. If the drying temperature is too high, the orientation state of the polarizer protective film is affected, the optical function that meets the design cannot be achieved, and the planarity deteriorates. The heating and drying time is usually 0.5 to 30 minutes, preferably 1 to 20 minutes, and more preferably 2 to 10 minutes.

[0176] The thickness of the rubbing-treated alignment layer is preferably 0.01 to 10 μm, more preferably 0.05 to 5 μm, and further preferably 0.1 to 1 μm.

[0177] The brushing treatment can be generally performed by rubbing the surface of the polymer layer with paper or cloth in a constant direction. The surface of the oriented film is generally brushed using a brushing roller made of napped cloth made of nylon, polyester, acrylic or the like.

[0178] In order to arrange the polarizing film having a light transmission axis in a predetermined direction inclined relative to the length direction of the long polarizer protective film, the brushing direction of the orientation layer must also be set to an angle that matches the predetermined direction. The angle can be adjusted by adjusting the angle between the brushing roller and the polarizer protective film, the conveying speed of the polarizer protective film, and the rotation speed of the roller.

[0179] It should be noted that the polarizer protective film may be directly subjected to a brushing treatment to allow the surface of the polarizer protective film to have an alignment layer function, which is also included in the protection scope of the present invention.

[0180] (Photo-Alignment Layer)

[0181] The photo-orientation layer is preferably an orientation film formed as follows: a coating liquid containing a polymer or monomer having a photoreactive group and a solvent is applied to a substrate film, and an orientation film is given an orientation restriction force by irradiating polarized light, preferably polarized ultraviolet light. A photoreactive group refers to a group that produces liquid crystal orientation ability by light irradiation. Specifically, it is a group that produces a photoreaction that is the origin of the liquid crystal orientation ability, such as an orientation-inducing or isomerization reaction, dimerization reaction, photocrosslinking reaction, or photodecomposition reaction of molecules generated by irradiation with light. Among the photoreactive groups, those that cause dimerization reaction or photocrosslinking reaction are preferred in terms of excellent orientation and maintaining the smectic liquid crystal state of the polarizing film. As a photoreactive group that can produce the above reaction, an unsaturated bond is preferred, a double bond is particularly preferred, and a group having at least one selected from the group consisting of a C=C bond, a C=N bond, an N=N bond, and a C=O bond is particularly preferred.

[0182] As photoreactive groups having C=C bonds, for example, vinyl, polyene, stilbene, amidozolyl, azostilbenium, chalcone and cinnamoyl groups can be cited. As photoreactive groups having C=N bonds, groups having structures such as aromatic Schiff bases and aromatic hydrazones can be cited. As photoreactive groups having N=N bonds, azophenyl, azonaphthyl, aromatic heterocyclic azo, disazo, and formazan, and those with azooxybenzene as the basic structure can be cited. As photoreactive groups having C=O bonds, benzophenone, coumarin, anthraquinone and maleimide groups can be cited. These groups optionally have substituents such as alkyl, alkoxy, aryl, allyloxy, cyano, alkoxycarbonyl, hydroxyl, sulfonic acid and halogenated alkyl groups.

[0183] Among them, photoreactive groups that can cause photodimerization reaction are preferred, and cinnamoyl and chalcone groups are preferred because they can easily obtain a photo-alignment control layer with less polarized light irradiation required for photo-alignment and excellent thermal stability or stability over time. Furthermore, as a polymer having a photoreactive group, a cinnamoyl group having a cinnamic acid structure at the end of the polymer side chain is particularly preferred. As the structure of the main chain, polyimide, polyamide, (meth) acrylic acid, polyester, etc. can be cited.

[0184] Specific examples of the alignment layer include Japanese Patent Application Laid-Open Nos. 2006-285197, 2007-76839, 2007-138138, 2007-94071, 2007-121721, 2007-140465, 2007-156439, 2007-133184, and 2007-140465. Orientation layers described in Japanese Unexamined Patent Application Publication No. 009-109831, Japanese Unexamined Patent Application Publication No. 2002-229039, Japanese Unexamined Patent Application Publication No. 2002-265541, Japanese Unexamined Patent Application Publication No. 2002-317013, Japanese Unexamined Patent Application Publication No. 2003-520878, Japanese Unexamined Patent Application Publication No. 2004-529220, Japanese Unexamined Patent Application Publication No. 2013-33248, Japanese Unexamined Patent Application Publication No. 2015-7702, Japanese Unexamined Patent Application Publication No. 2015-129210, etc.

[0185] As the solvent of the coating liquid for forming the photo-alignment layer, any solvent can be used without limitation as long as it can dissolve the polymer and monomer having the photoreactive group. As specific examples of solvents, those listed in the alignment layer for brushing treatment can be exemplified. Photopolymerization initiators, polymerization inhibitors, various stabilizers, etc. can also be added to the coating liquid for forming the photo-alignment layer as needed. In addition, polymers other than polymers and monomers having photoreactive groups, monomers without photoreactive groups that can copolymerize with monomers having photoreactive groups, etc. can also be added to the coating liquid for forming the photo-alignment layer.

[0186] The concentration, coating method, drying conditions, etc. of the coating liquid for forming the photo-alignment layer can be exemplified by those exemplified in the rubbing-treated alignment layer. The thickness of the photo-alignment layer is also the same as the preferred thickness of the rubbing-treated alignment layer.

[0187] By irradiating the thus obtained pre-aligned photo-alignment layer with polarized light in a predetermined oblique direction relative to the longitudinal direction of the polarizer protective film, a photo-alignment layer having an alignment regulating force in an oblique direction relative to the longitudinal direction of the long polarizer protective film can be obtained.

[0188] The polarized light may be directly irradiated to the photo-alignment layer before alignment, or may be irradiated through a polarizing plate protective film.

[0189] The wavelength of polarized light is preferably in a wavelength region where the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, ultraviolet light in the wavelength range of 250 to 400 nm is preferred.

[0190] Examples of the polarized light source include xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, ultraviolet lasers such as KrF and ArF, and the like. Preferred are high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps.

[0191] Polarized light can be obtained, for example, by passing light from the light source through a polarizing plate. The direction of polarized light can be adjusted by adjusting the polarization angle of the polarizing plate. Examples of the polarizing plate include polarizing filters; polarizing prisms such as GranThomson and GLAN TAYLOR; and wire grid type polarizing plates. The polarized light is preferably substantially parallel light.

[0192] By adjusting the angle of the irradiated polarized light, the direction of the alignment regulating force of the photo-alignment layer can be arbitrarily adjusted.

[0193] The irradiation intensity varies depending on the type or amount of the polymerization initiator or the resin (monomer), but is preferably 10 to 10,000 mJ / cm2 based on 365 nm. 2 , more preferably 20 to 5000 mJ / cm 2 .

[0194] (Angle between the transmission axis of the polarizer and the slow axis of the polarizer protective film)

[0195] The angle between the light transmission axis of the polarizer and the slow axis of the polarizer protective film is not particularly limited. For the purpose of preventing black vision or coloring when wearing polarized sunglasses to observe the image, the range of 30 to 60 degrees is preferred, and the range of 35 to 55 degrees is more preferred. In order to reduce the weak rainbow spots when observing with the naked eye from a shallow angle, it is preferably set to less than 10 degrees, further set to less than 7 degrees, or set to 80 to 100 degrees, and further set to 83 to 97 degrees. These angles can be adjusted by the lamination angle of the polarizer protective film and the polarizer, the stretching direction of the oblique stretching of the polarizer protective film, or the angle of the orientation control of the orientation layer.

[0196] 3. Phase difference layer

[0197] In the present invention, laminating a retardation layer on a polarizing plate is also a preferred embodiment.

[0198] The phase difference layer is also preferably laminated on one side of the polarizing plate having polarizer protective films on both sides of the polarizer, but it is preferred that the polarizer protective film is laminated on one side of the polarizer and the phase difference layer is provided on the other side of the polarizer. By forming such a form, the thickness is reduced, thereby satisfying high flexibility and being less likely to have creases when folded.

[0199] When the foldable display is a liquid crystal display, the phase difference layer may be a phase difference layer commonly used in liquid crystal displays, such as a positive or negative A plate, a positive or negative C plate, or a tilted alignment of a discotic liquid crystal compound, depending on the type of liquid crystal unit.

[0200] When the foldable display is an organic EL display or the like, the retardation layer is preferably a quarter wavelength layer in order to form a circularly polarizing plate for antireflection.

[0201] Hereinafter, the retardation layer will be described by taking a circularly polarizing plate in which the retardation layer is a 1 / 4 wavelength layer as a representative example.

[0202] In the circular polarizing plate, there is a phase difference layer on the opposite side of the polarizer to the polarizer protective film surface. It is preferred that there is no self-supporting film between the polarizer and the phase difference layer, or there is only one self-supporting film (here, the phase difference layer itself is also included between the polarizer and the phase difference layer). It should be noted that the self-supporting film here refers to a form that exists independently as a film in the process.

[0203] The “retardation layer” referred to herein is a layer that functions as a circular polarizing plate, and specifically refers to a 1 / 4 wavelength layer, a 1 / 2 wavelength layer, a C plate, or the like.

[0204] The absence of a self-supporting film between the polarizer and the phase difference layer means that the phase difference layer that is not a self-supporting film is directly laminated on the polarizer. Here, the so-called "directly" means that there are no other layers between the polarizer and the phase difference layer, and between the phase difference layers, or even if there are, they are only adhesive layers or bonding layers.

[0205] The existence of one self-supporting film between the polarizing plate and the retardation layer means that only one of the polarizing plate protective film and the retardation layer is a self-supporting film.

[0206] The 1 / 4 wavelength layer can be obtained by laminating a separately prepared phase difference film (self-supporting film) provided with a coated 1 / 4 wavelength layer described later on an oriented film (self-supporting film) of polycarbonate, cycloolefin, etc. or these films or a triacetyl cellulose (TAC) film. However, in terms of thinning, it is preferred to directly provide a coated 1 / 4 wavelength layer on the polarizer.

[0207] The coated 1 / 4 wavelength layer refers to a 1 / 4 wavelength layer formed by coating itself, and does not become a separate independent state. As a method for setting a 1 / 4 wavelength layer, the following methods can be cited: a method of coating a phase difference compound on a polarizer; a method of separately setting a 1 / 4 wavelength layer on a substrate with mold release properties and transferring it to a polarizer, etc. As a 1 / 4 wavelength layer, a layer formed by a liquid crystal compound is preferred. As liquid crystal compounds, for example, rod-shaped liquid crystal compounds, polymer-like liquid crystal compounds, liquid crystal compounds with reactive functional groups, etc. can be cited. As a method for coating a phase difference compound on a polarizer, it is preferred to brush the polarizer, or to coat the liquid crystal compound on the basis of setting an orientation layer as described above on the polarizer so that it has an orientation control force.

[0208] In the method of separately providing a coated 1 / 4 wavelength layer on a releasable substrate and transferring it to a polarizer, it is preferred to perform a brushing treatment on the releasable substrate, or to provide an orientation layer as described above on the releasable substrate so that it has an orientation control force, and then coat the liquid crystal compound (1 / 4 wavelength layer).

[0209] As a transfer method, a method of coating a birefringent resin on a releasable substrate and stretching the substrate together with the substrate to form a quarter wavelength layer is also preferred.

[0210] After the transfer type 1 / 4 wavelength layer thus obtained is bonded to the polarizer with an adhesive or a bonding agent, the release substrate is peeled off. For thinning, it is preferably bonded with an adhesive, especially an ultraviolet curing adhesive. In terms of the process that does not require special equipment, it is also preferably used.

[0211] In order to make the polarizing plate less susceptible to the coating solvent of the quarter wavelength layer, a method of separately providing a coating type quarter wavelength layer on a releasable substrate and transferring it onto the polarizing plate is preferred.

[0212] The front retardation of the quarter wavelength layer is preferably 100 to 180 nm, more preferably 120 to 150 nm.

[0213] For these methods and phase difference layers, for example, Japanese Patent Application Laid-Open No. 2008-149577, Japanese Patent Application Laid-Open No. 2002-303722, WO2006 / 100830, Japanese Patent Application Laid-Open No. 2015-64418, etc. can be referred to.

[0214] In addition, when the 1 / 4 wavelength layer is independent, in the wide wavelength region of visible light, it sometimes does not become 1 / 4 wavelength but is colored. In this case, a 1 / 2 wavelength layer can be further provided. In this case, the 1 / 2 wavelength layer is preferably provided between the polarizer and the 1 / 4 wavelength layer.

[0215] Preferred raw materials, forms, production methods, lamination methods, etc. of the half wavelength layer are the same as those of the above-mentioned quarter wavelength layer.

[0216] The front retardation of the half-wave layer is preferably 200 to 360 nm, more preferably 240 to 300 nm.

[0217] When only the quarter wavelength layer is used as the retardation layer, the angle between the orientation axis (slow axis) of the quarter wavelength layer and the transmission axis of the polarizer is preferably 35 to 55 degrees, more preferably 40 to 50 degrees, and further preferably 42 to 48 degrees.

[0218] When a 1 / 4 wavelength layer and a 1 / 2 wavelength layer are used in combination as a phase difference layer, the angle (θ) between the orientation axis (slow axis) of the 1 / 2 wavelength layer and the light transmission axis of the polarizer is preferably 5 to 20 degrees, more preferably 7 to 17 degrees. The angle between the orientation axis (slow axis) of the 1 / 2 wavelength layer and the orientation axis (slow axis) of the 1 / 4 wavelength layer is preferably in the range of 2θ+45 degrees ± 10 degrees, more preferably in the range of 2θ+45 degrees ± 5 degrees, and further preferably in the range of 2θ+45 degrees ± 3 degrees.

[0219] When an oriented film is laminated, these angles can be adjusted by the lamination angle, the stretching direction of the oriented film, and the like.

[0220] In the case of a coating type 1 / 4 wavelength layer and a 1 / 2 wavelength layer, it can be controlled by the brushing angle, the irradiation angle of the polarizing plate external light, and the like.

[0221] In the method of providing a coating type 1 / 4 wavelength layer on a substrate and transferring it to a polarizer, in the case of roll-to-roll lamination, it is preferably controlled in advance by a brushing angle or an irradiation angle of the polarizer external light so as to be a predetermined angle.

[0222] When an oriented film is used or a birefringent resin is applied to a polarizer protective film and stretched together with a substrate, when roll-to-roll bonding is performed, it is preferred to stretch in an oblique direction at a predetermined angle.

[0223] Furthermore, in order to reduce the change in coloration when observed from an oblique direction, it is also a preferred embodiment to provide a C plate layer on the 1 / 4 wavelength layer. The C plate layer may be a positive or negative C plate layer depending on the characteristics of the 1 / 4 wavelength layer or the 1 / 2 wavelength layer. The C plate layer is preferably a liquid crystal compound layer. The C plate layer may be provided by directly coating a coating liquid to be a C plate layer on the 1 / 4 wavelength layer, or a separately prepared C plate layer may be transferred.

[0224] Various methods can be adopted as these lamination methods, and for example, the following methods can be mentioned.

[0225] A method in which a 1 / 2 wavelength layer is provided on a polarizing plate by transfer, and a 1 / 4 wavelength layer is further provided thereon by transfer.

[0226] A method in which a quarter wavelength layer and a half wavelength layer are sequentially provided on a release film and then transferred to a polarizing plate.

[0227] A method in which a 1 / 2 wavelength layer is provided on a polarizing plate by coating, and a 1 / 4 wavelength layer is provided by transfer.

[0228] A method in which a film-like 1 / 2 wavelength layer is prepared, a 1 / 4 wavelength layer is provided thereon by coating or transfer, and the layer is then bonded to a polarizing plate.

[0229] In addition, various methods can be used to laminate the C plate, such as a method of disposing a C plate layer on a quarter wavelength layer disposed on a polarizing plate by coating or transfer, or a method of pre-laminating a C plate layer on a transferred or laminated quarter wavelength layer.

[0230] In the present invention, when there is a C plate layer between the polarizer and the 1 / 4 wavelength layer (including the 1 / 4 wavelength layer), all layers from the polarizer to the C plate layer (including the C plate layer) are preferably a coating layer. This indicates that there is no self-supporting film on the opposite side of the polarizer to the polarizer protective film. Specifically, it means that on the opposite side of the polarizer to the polarizer protective film, there is only an adhesive layer, an adhesive layer, a protective coating layer, an orientation layer, and any combination of a coating-type phase difference layer. By setting it to this configuration, the circular polarizer can be thinned.

[0231] Specific preferred lamination examples between the polarizing plate and the quarter wavelength layer include:

[0232] Polarizer / adhesive layer / 1 / 4 wavelength layer,

[0233] Polarizer / Protective coating layer / Adhesive layer / 1 / 4 wavelength layer,

[0234] Polarizer / 1 / 2 wavelength layer / adhesive layer / 1 / 4 wavelength layer,

[0235] Polarizer / adhesive layer / 1 / 2 wavelength layer / adhesive layer / 1 / 4 wavelength layer,

[0236] Polarizer / Protective coating layer / 1 / 2 wavelength layer / Adhesive layer / 1 / 4 wavelength layer,

[0237] Polarizer / protective coating layer / adhesive layer / 1 / 2 wavelength layer / adhesive layer / 1 / 4 wavelength layer, etc.

[0238] It should be noted that the above-mentioned intermediate binder layer may be an adhesive layer. In addition, the 1 / 4 wavelength layer and the 1 / 2 wavelength layer may include an orientation layer on any side thereof.

[0239] As the adhesive layer, adhesives such as rubber, acrylic, urethane, olefin, and silicone can be used without limitation. Among them, acrylic adhesives are preferred. The adhesive can be applied to an object, such as the polarizer surface of a polarizing plate. The following method is preferred: after peeling off the single-sided release film of a substrate-free optical transparent adhesive (release film / adhesive layer / release film), it is attached to the polarizer surface to set the adhesive layer. As the adhesive, ultraviolet curing type, urethane, and epoxy are preferably used.

[0240] The adhesive layer or pressure-sensitive adhesive layer is used for lamination of polarizing plates, protective coating layers, coating-type phase difference layers, or image display units.

[0241] It should be noted that, in the above, the phase difference layer (1 / 4 wavelength layer or 1 / 2 wavelength layer) can be provided on the laminate of the polarizer protective film and the polarizer and then attached to the object, but the phase difference layer (1 / 4 wavelength layer or 1 / 2 wavelength layer) can also be provided on the object in advance, so that the laminate of the polarizer protective film and the polarizer is attached thereto. The same is true for the case of providing a C plate layer.

[0242] When the phase difference layer is a layer formed of a liquid crystal compound, a protective coating layer may be provided on the opposite side of the phase difference layer to the polarizer. In addition, a protective film (self-supporting film) may also be provided, but for thinning, it is preferably not used.

[0243] The thickness of the circularly polarizing plate obtained in this manner is preferably 130 μm or less, more preferably 100 μm or less, further preferably 90 μm or less, and particularly preferably 85 μm or less.

[0244] The circularly polarizing plate is preferably attached to a touch panel, an organic EL unit, or the like using an adhesive or a pressure-sensitive adhesive.

[0245] B. Display unit

[0246] The foldable display of the present invention has the aforementioned polarizing plate on the visible side closer to the display unit. As the image display unit, a unit of a foldable display such as a liquid crystal unit, an organic electroluminescent (EL) unit, an inorganic EL unit, etc. can be used without particular limitation. Among them, the organic EL unit is thin and excellent in flexibility, and is preferred. It is preferred that the image display unit and the polarizing plate are bonded with an adhesive.

[0247] As a foldable display, it is preferred to use an image display device that can be folded into a V shape, Z shape, W shape, double door shape, etc. when moved (foldable image display device), or a display that can be rolled up (roll-up display).

[0248] In the case where a foldable display has a display unit on the inner side of the fold, the bending radius of the circular polarizer in the folded state becomes smaller. In the case of such an image display device, the main orientation direction of the substrate film is arranged in a direction perpendicular to the folding direction (the direction of the folding action), thereby effectively reducing the occurrence of fold marks caused by repeated folding operations. It should be noted that in the vertical direction, the angle between the main orientation direction of the polarizer protective film and the folding direction is preferably 75 to 105 degrees, more preferably 80 to 100 degrees, and further preferably 83 to 97 degrees.

[0249] The foldable display of the present invention can be manufactured to have a bending radius of 5 mm or less, further 4 mm or less, and particularly 3 mm or less.

[0250] C. Other components

[0251] The foldable display of the present invention may have other components in addition to the image display unit and the polarizing plate (circular polarizing plate). As other components, a touch panel, a surface protection film, a back protection film, etc. can be cited. Furthermore, in the case of a liquid crystal display device, it is preferably provided with a backlight unit. These components are preferably bonded with an adhesive or a bonding agent.

[0252] In addition, it is also a preferred method to use the polyester film used as the polarizer protective film of the present invention as the substrate film of these components. In particular, in a foldable display, it is a preferred method to use the polarizing plate of the present invention as a polarizing plate, and to use the polyester film used as the polarizer protective film of the present invention for at least one side of the surface protective film and the back protective film, or both sides. The surface protective film at this time can be a surface protective film for a foldable display called a window, or a surface protective film that can be replaced by a user called a rear window (after), or both.

[0253] When the polyester film is used as a base film of the above-mentioned member, it is also preferable that the longitudinal direction of the polyester film is the bending direction.

[0254] It should be noted that, in the case of a component such as a touch panel disposed between an image display unit and a polarizing plate, a substrate film is preferably a film having a small birefringence that does not change the circular polarization characteristics. Specifically, a film having an in-plane retardation of 100 nm or less, further 50 nm or less, and particularly 30 nm or less, such as a polyimide film, a polyamide film, a polyamideimide film, a polycarbonate film, an acrylic film, a triacetyl cellulose film, a cycloolefin polymer film, a polyphenylene sulfide film, and a polymethylpentene film is preferably used.

[0255] Example

[0256] Next, the present invention will be described using Examples and Comparative Examples. First, the evaluation method of the characteristic values ​​implemented in the present invention is shown below.

[0257] (1) Intrinsic viscosity

[0258] The film or polyester resin was crushed and dried, and then dissolved in a mixed solvent of phenol / tetrachloroethane = 60 / 40 (mass ratio). The solution was centrifuged to remove inorganic particles, and then the flow time of the solution with a concentration of 0.4 (g / dl) and the flow time of the solvent alone were measured at 30°C using an Ubbelohde viscometer. From the ratio of these time, the intrinsic viscosity was calculated using the Huggins formula, assuming that the Huggins constant was 0.38.

[0259] (2) Bending resistance of polyester film samples (bending radius 1.5 mm)

[0260] Prepare a polyester film sample with a size of 20mm in width direction and 110mm in flow direction. Use a no-load U-shaped stretch tester (made by Yuasa System Equipment Co., Ltd., DLDMLH-FS) and set the bending radius to 1.5mm. Bend it 200,000 times at a speed of 1 time / second. At this time, for the sample, fix the position of 10mm at both ends of the long side, and set the bending part to 20mm×90mm. Here, Figure 1 This is a schematic diagram for illustrating the bending radius when a foldable display is folded. Consider the case where a polyester film is arranged on the inner surface of the folded state so as to Figure 1 The bending test was performed as a model so that the position of the symbol 11 was set to 1.5 mm. After the bending process was completed, the sample was placed on a flat surface with the inner side of the bend facing downward, and visually observed.

[0261] ○: No cracks or deformation were observed in the sample.

[0262] ×: There are cracks or creases in the sample, and the maximum height of the floating when placed horizontally is 5 mm or more.

[0263] (3) Bending resistance of polyester film samples (bending radius 0.5 mm)

[0264] The bending test was performed in the same manner as above, with the bending radius set to 0.5 mm and the bending was performed 200,000 times at a rate of 1 time / second. Figure 1 This is a schematic diagram showing the bending radius when a foldable display is folded. Consider the case where a polyester film is arranged on the inner surface of the folded state so as to Figure 1 The bending test was carried out in a manner that the position of the symbol 11 was set to 0.5mm as a model. The film surface on the outside of the bending portion was observed with a digital microscope (RH8800 manufactured by HIROX Corporation) at 700 times magnification to observe the presence or absence of wrinkles (cracks). Independently from the above-mentioned visual test of bending resistance with a bending radius of 1.5mm, this test with the bending radius reduced to 0.5mm is carried out for the purpose of evaluating the folding display in a state close to the actual use state of the laminated or pasted hard coating or other components. It is independent of the visual observation based on the above-mentioned bending radius of 1.5mm, and is a test for detecting fine defects that are difficult to detect visually, i.e. defects that are easy to break or crack.

[0265] ○: The film surface on the outer side of the bend has no defects.

[0266] ×: Broken, or wrinkles (cracks) were observed on the film surface outside the bend.

[0267] (4) Bending resistance of circular polarizing plate (bending radius 3 mm)

[0268] Prepare a circular polarizer sample of size 50mm×100mm, use a no-load U-shaped telescopic tester (made by Yuasa System Equipment Co., Ltd., DLDMLH-FS), set the bending radius to 3mm, and bend 100,000 times at a speed of 1 time / second. At this time, the sample is fixed at a position of 10mm at both ends of the long side, and the bent part is set to 50mm×80mm, so that the inner side of the bend becomes the substrate film side, and the slow axis of the substrate film is orthogonal to the bending direction. After the bending process is completed, the inner side of the bend of the sample is placed as the lower plane for visual inspection. Then, observe under a digital microscope. The evaluation criteria are as follows.

[0269] ○: No deformation or breakage of the sample was observed, and no wrinkles (cracks) were observed.

[0270] ×: The sample is deformed or has wrinkles (cracks).

[0271] (5) Refractive index

[0272] The refractive index in the longitudinal direction, the refractive index in the width direction, and the refractive index in the thickness direction were determined using an Abbe refractometer (NAR-4T manufactured by ATAGO CO., LTD., measuring wavelength 589 nm) in accordance with JIS K 7142:2008 “Method for determination of refractive index of plastics (Method A)”.

[0273] (6) Total light transmittance, haze

[0274] The measurement was performed using a haze meter (NDH5000, manufactured by Nippon Denshoku Industries, Ltd.).

[0275] (7) Density

[0276] The density was measured by the method in accordance with JIS K 7112:1999 (density gradient tube method). (Unit: g / cm 3 ).

[0277] (8) Maximum thermal shrinkage

[0278] The sample film was cut into 10 mm in length and 250 mm in width, and marked at intervals of 200 mm along the direction of the long side to be measured. The marked interval A was measured under a constant tension of 5 g. Next, the sample film was placed in an oven at 150°C for 30 minutes without load, then taken out of the oven and cooled to room temperature. Then, the marked interval B was calculated under a constant tension of 5 g, and the heat shrinkage rate (%) was calculated using the following formula. It should be noted that the above heat shrinkage rate was measured at three equal positions along the width direction of the sample film, and the average value of the three points was taken as the heat shrinkage rate (%).

[0279] Thermal shrinkage (%) = [(AB) × 100] / A

[0280] The sample film was cut and measured independently in both the bending direction and the folding direction so that the longitudinal and transverse directions were different, and the data in the direction with the larger measured value was taken as the maximum heat shrinkage (%).

[0281] <Manufacturing of the adhesive layer component>

[0282] (Polymerization of polyester resin)

[0283] In a stainless steel autoclave equipped with a stirrer, a thermometer and a partial reflux condenser, 194.2 parts by mass of dimethyl terephthalate, 184.5 parts by mass of dimethyl isophthalate, 14.8 parts by mass of dimethyl isophthalate-5-sodium sulfonate, 233.5 parts by mass of diethylene glycol, 136.6 parts by mass of ethylene glycol, and 0.2 parts by mass of tetra-n-butyl titanate were added, and an ester exchange reaction was carried out at a temperature of 160°C to 220°C for 4 hours. Then, the mixture was heated to 255°C, the reaction system was slowly depressurized, and then reacted under a reduced pressure of 30 Pa for 1 hour and 30 minutes to obtain a copolyester resin. The obtained copolyester resin was light yellow and transparent. The reduced viscosity of the copolyester resin was measured and the result was 0.70 dl / g. The reduced viscosity is a value obtained by measuring 0.1 g of the resin using 25 mL of a mixed solvent of phenol (60% by mass) and 1,1,2,2-tetrachloroethane (40% by mass) at 30° C. The glass transition temperature determined by DSC is 40° C.

[0284] (Preparation of Polyester Aqueous Dispersion)

[0285] In a reactor equipped with a stirrer, a thermometer, and a reflux device, 30 parts by mass of a polyester resin and 15 parts by mass of ethylene glycol n-butyl ether were placed, and the mixture was stirred while heating at 110° C. to dissolve the resin. After the resin was completely dissolved, the polyester solution was stirred and 55 parts by mass of water was slowly added. After the addition was completed, the mixed solution was stirred and cooled to room temperature to obtain a milky white polyester aqueous dispersion having a solid content of 30% by mass.

[0286] (Preparation of polyvinyl alcohol aqueous solution)

[0287] In a container equipped with a stirrer and a thermometer, 90 parts by mass of water were placed, and 10 parts by mass of a polyvinyl alcohol resin (manufactured by Kuraray, with a degree of polymerization of 500 and a degree of saponification of 74%) was slowly added while stirring. After the addition was completed, the mixed solution was heated to 95°C while stirring to dissolve the resin. After the resin was dissolved, the mixed solution was cooled to room temperature while stirring to obtain a polyvinyl alcohol aqueous solution with a solid content of 10% by mass.

[0288] (Polymerization of Blocked Polyisocyanate Crosslinking Agent Used in Easy Adhesion Layer P1)

[0289] In a flask equipped with a stirrer, a thermometer and a reflux condenser, 100 parts by mass of a polyisocyanate compound having an isocyanurate structure (Duranate TPA manufactured by Asahi Kasei Chemicals Corporation) with hexamethylene diisocyanate as a raw material, 55 parts by mass of propylene glycol monomethyl ether acetate, and 30 parts by mass of polyethylene glycol monomethyl ether (average molecular weight 750) were added, and kept at 70° C. for 4 hours under a nitrogen atmosphere. After that, the temperature of the reaction liquid was lowered to 50° C., and 47 parts by mass of methyl ethyl ketone oxime was added dropwise. The infrared spectrum of the reaction liquid was measured to confirm that the absorption of the isocyanate group disappeared, and a blocked polyisocyanate aqueous dispersion having a solid content of 75% by mass was obtained.

[0290] (Preparation of coating liquid for easy-adhesion layer P1)

[0291] The following raw materials were mixed to prepare a coating liquid.

[0292]

[0293] (Polymerization of polyurethane resin used in easy-adhesion layer P2)

[0294] A polyurethane resin with aliphatic polycarbonate polyol as a constituent component was prepared according to the following steps. In a four-necked flask equipped with a stirrer, a serpentine condenser, a nitrogen inlet tube, a silica gel drying tube and a thermometer, 43.75 parts by mass of 4,4-diphenylmethane diisocyanate, 12.85 parts by mass of dimethylolbutyric acid, 153.41 parts by mass of polyhexamethylene carbonate diol with a number average molecular weight of 2000, 0.03 parts by mass of dibutyltin dilaurate, and 84.00 parts by mass of acetone as a solvent were added, and stirred at 75°C for 3 hours under a nitrogen atmosphere, and it was confirmed that the reaction liquid reached the specified amine equivalent. Then, after the temperature of the reaction liquid was lowered to 40°C, 8.77 parts by mass of triethylamine was added to obtain a polyurethane prepolymer solution. Next, in a reaction container equipped with a homogeneous disperser capable of high-speed stirring, 450 g of water was added and adjusted to 25°C while the water was stirred at 2000 min. -1 The polyurethane prepolymer solution was added and dispersed while stirring and mixing. Then, acetone and part of water were removed from the mixed solution under reduced pressure to prepare a water-soluble polyurethane resin with a solid content of 35%. The obtained polyurethane resin having aliphatic polycarbonate polyol as a constituent component had a glass transition temperature of -30°C.

[0295] (Polymerization of Oxazoline Crosslinking Agent Used in Easy Adhesion Layer P2)

[0296] In a flask equipped with a thermometer, a nitrogen inlet tube, a reflux condenser, a dropping funnel, and a stirrer, a mixture of 58 parts by mass of ion exchange water and 58 parts by mass of isopropanol as an aqueous medium and 4 parts by mass of a polymerization initiator (2,2'-azobis(2-amidinopropane)·dihydrochloride) were added. On the other hand, in the dropping funnel, a mixture of 16 parts by mass of 2-isopropenyl-2-oxazoline as a polymerizable unsaturated monomer having an oxazoline group, 32 parts by mass of methoxypolyethylene glycol acrylate (average addition mole number of ethylene glycol: 9 mol, manufactured by Shin-Nakamura Chemical) and 32 parts by mass of methyl methacrylate were added dropwise under a nitrogen atmosphere at 70°C for 1 hour. After the dropwise addition was completed, the reaction solution was stirred for 9 hours and cooled to obtain a water-soluble resin having an oxazoline group having a solid content concentration of 40% by mass.

[0297] (2) Preparation of Coating Solution for Easy-Adhesion Layer P2 The following raw materials were mixed to prepare a coating solution for forming a coating layer having excellent adhesion to the functional layer.

[0298]

[0299] (Preparation of polyethylene terephthalate pellets)

[0300] As the esterification reaction apparatus, a continuous esterification reaction apparatus consisting of a stirring device, a partial condenser, and a three-stage complete mixing tank with a raw material input port and a product output port was used. TPA was set to 2 tons / hour, EG was set to 2 mol relative to 1 mol of TPA, and antimony trioxide was set to an amount in which Sb atoms were 160 ppm relative to the generated PET. These slurries were continuously supplied to the first esterification reactor of the esterification reaction apparatus, and the reaction was carried out at 255° C. under normal pressure with an average residence time of 4 hours.

[0301] Next, the reaction product in the first esterification reactor was continuously taken out of the system and supplied to the second esterification reactor, and EG distilled from the first esterification reactor was supplied to the second esterification reactor in an amount of 8% by mass relative to the produced polymer (produced PET), and further, an EG solution containing magnesium acetate in an amount of 65 ppm of Mg atoms relative to the produced PET and an EG solution containing TMPA in an amount of 20 ppm of P atoms relative to the produced PET were added, and the mixture was reacted at 260° C. at an average residence time of 1.5 hours under normal pressure. Next, the reaction product in the second esterification reactor was continuously taken out of the system and supplied to the third esterification reactor, and an EG solution containing TMPA in an amount of 20 ppm of P atoms relative to the produced PET was further added, and the mixture was reacted at 260° C. at an average residence time of 0.5 hours under normal pressure. The esterification reaction product generated in the third esterification reactor is continuously supplied to a three-stage continuous polycondensation reaction device for polycondensation, and then filtered using a stainless steel sintered filter material (nominal filtration accuracy 5 μm particles 90% cutoff) to obtain polyethylene terephthalate pellets with an intrinsic viscosity of 0.62 dl / g.

[0302] (PET film 1)

[0303] The pellets of polyethylene terephthalate are supplied to the extruder and melted at 285°C. The polymer is filtered with a filter material of a stainless steel sintered body (nominal filtration accuracy 10μm particles 95% cutoff), extruded from a nozzle into a sheet, and then, by an electrostatic application casting method, contacted with a casting drum with a surface temperature of 30°C for cooling and solidification to produce an unstretched film. The unstretched film is uniformly heated to 75°C with a heating roller, heated to 85°C with a non-contact heater, and 1.4 times roller stretching (longitudinal stretching) is performed. The above-mentioned easy-adhesion layer forming coating liquid P1 is applied to one side of the obtained uniaxially stretched film by a roller coating method, and P2 is applied to the opposite side, and then dried at 80°C for 20 seconds. It should be noted that the final (after biaxial stretching) dried coating amount is 0.06g / m 2 Then, the film was introduced into a tenter and preheated at 105°C, stretched to 4.0 times in the transverse direction at 95°C, fixed in width, heat-set at 230°C for 5 seconds, and then relaxed by 4% in the width direction at 180°C to obtain a polyethylene terephthalate film (PET film 1) with a thickness of 50 μm. The evaluation results are shown in Table 1.

[0304] (PET film 2-3)

[0305] PET films 2 and 3 were obtained in the same manner as in PET film 1 except that the stretching ratio in the longitudinal direction was changed to that described in Table 1.

[0306] (PET film 4)

[0307] A PET film 4 was obtained in the same manner as the PET film 1 except that the stretching ratio in the width direction was changed to 4.4 times and the heat setting temperature was changed to 220°C.

[0308] (PET film 5~6)

[0309] PET films 5 and 6 were obtained in the same manner as in PET film 4 except that the stretching ratio in the longitudinal direction was changed as described in Table 1.

[0310] (PET film 7)

[0311] A PET film 7 was obtained in the same manner as the PET film 1 except that the stretching ratio in the width direction was changed to 5.5 times and the heat setting temperature was changed to 190°C.

[0312] (PET film 8~9)

[0313] PET films 8 and 9 were obtained in the same manner as in PET film 7 except that the stretching ratio in the longitudinal direction was changed as described in Table 1.

[0314] (PET film 10)

[0315] In the manufacturing process of the PET film 5 , the PET film 10 was obtained in the same manner as the PET film 5 except that the PET film 5 was stretched in the longitudinal direction and then subjected to a 10% relaxation heat treatment at 100° C.

[0316] (PET film 11)

[0317] In the manufacturing process of PET film 5, the clamps were opened at 200°C after heat setting, and relaxation heat treatment was performed in the longitudinal direction and the width direction. PET film 11 was obtained in the same manner as PET film 5. The tenter speed and the winding roller speed were adjusted so that the relaxation rate in the longitudinal direction was 3%. The relaxation in the width direction was set to a free state.

[0318] (PET film 12)

[0319] A PET film 12 was obtained in the same manner as the PET film 1 except that the temperature during the longitudinal direction stretching was changed to 75°C and the heat setting temperature was changed to 220°C.

[0320] (PET film 13)

[0321] A PET film 13 was obtained in the same manner as the PET film 1 except that the temperature during stretching in the longitudinal direction was changed to 75° C. and the stretching ratio was changed to 1.2 times, and then the stretching ratio in the width direction was changed to 5.0 times.

[0322] (PET film 14)

[0323] The PET film 14 was obtained in the same manner as the PET film 3 except that the longitudinal stretching of the PET film 3 was performed in two stages, the stretching ratio in the first stage was set to 1.2 times, and the stretching ratio in the second stage was set to 1.67 times. The total longitudinal stretching ratio was about 2.0 times.

[0324] (PET film 15)

[0325] A PET film 15 was obtained in the same manner as the PET film 5 except that the preheating temperature during the width direction stretching was changed to 95°C and the heat setting temperature was changed to 190°C.

[0326] (PET film 16)

[0327] The PET film 2 was stretched in the width direction in two stages, the stretching ratio in the first stage was 1.5 times, the stretching ratio in the second stage was 4.0 times, and the heat setting temperature was changed to 190° C., and a PET film 16 was obtained in the same manner as the PET film 2. The total stretching ratio in the width direction was 6.0 times.

[0328] (PET film 17-18)

[0329] PET films 17 to 18 were obtained in the same manner as in PET film 2 except that the thickness was changed as described in Table 1.

[0330] (PET film 19)

[0331] In the production process of the PET film 1, the PET film 19 was obtained in the same manner as the PET film 1 except that the relaxation heat treatment in the width direction was not performed.

[0332] (PET film 20)

[0333] After preparing an unstretched film in the same manner as PET film 1, the unstretched film was preheated at 75°C in a tenter and stretched transversely to 1.4 times at 85°C. The above-mentioned coating solution for forming an easy-adhesion layer was applied to both sides of the obtained uniaxially stretched film by a roller coating method, and then dried at 80°C for 20 seconds. It should be noted that the final (after biaxial stretching) dried coating amount was 0.06 g / m 2 The film was adjusted in the manner of . The film was heated uniformly to 105°C using a heating roller, heated to 95°C using a non-contact heater, and roller stretched (longitudinal stretching) to 4.0 times. The width was fixed, and heat set at 230°C for 5 seconds to obtain a PET film 20 with a thickness of 50 μm.

[0334] (PET film 21)

[0335] The ET film 21 was obtained in the same manner as the PET film 7 except that stretching in the longitudinal direction was not performed and only stretching in the width direction was performed as transverse uniaxial stretching.

[0336] (PET film 22)

[0337] The PET film 22 was obtained in the same manner as the PET film 1 except that the heat setting temperature was changed to 220° C. and the thickness was changed to 75 μm.

[0338] (PET film 23)

[0339] A PET film 23 was obtained in the same manner as the PET film 4 except that the heat setting temperature was changed to 100°C.

[0340] Table 1 shows the properties of each film.

[0341] [Table 1]

[0342]

[0343] (Lamination of polarizing plates)

[0344] As a method of providing a polarizing plate on a polyester film (polarizing plate protective film), the following two methods were performed.

[0345] (A) A method of providing a brushed alignment layer on a polyester film and providing a polarizing film containing a liquid crystal compound and a dichroic dye thereon (polarizing plate lamination method A)

[0346] (B) A method of providing a polarizing film composed of PVA / iodine on a thermoplastic substrate and then transferring the polarizing film to a polyester film (polarizing plate lamination method B)

[0347] The details of each method are described below.

[0348] Polarizer Lamination Method A

[0349] (Formation of Orientation Layer by Brushing)

[0350] The coating for the rubbing orientation layer of the following composition was applied to the easy-adhesion layer P1 of the polyester film using a rod coater and dried at 120°C for 3 minutes to form a film with a thickness of 200 nm. Then, the surface of the obtained film was treated with a rubbing roller wound with a nylon napped cloth to obtain a polyester film laminated with a rubbing orientation layer. The rubbing direction was parallel or orthogonal to the slow axis of the polyester film.

[0351] Paint for brushing orientation layer

[0352] Completely saponified polyvinyl alcohol molecular weight 800 2 parts by mass

[0353] 100 parts by mass of ion exchange water

[0354] (Synthesis of polymerizable liquid crystal compounds)

[0355] The following compound (I) and the following compound (II) were synthesized with reference to the description in paragraph

[0134] of JP-A-2007-510946 and Lub et al. Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996).

[0356]

[0357]

[0358] The following pigment (ハ) was synthesized with reference to Example 1 of Japanese Patent Application Laid-Open No. 63-301850.

[0359]

[0360] Using Example 2 of Japanese Patent Publication No. 5-49710 as a reference, a pigment (II) represented by the following formula (4) was synthesized.

[0361]

[0362] The following dye (ホ) was synthesized with reference to the method for producing the compound of the general formula (1) in Japanese Patent Publication No. 63-1357.

[0363]

[0364] (Formation of polarizing film)

[0365] A coating for polarizing film containing 75 parts by mass of compound (I), 25 parts by mass of compound (R), 2.5 parts by mass of pigment (H), 2.5 parts by mass of pigment (II), 2.5 parts by mass of pigment (H), 6 parts by mass of IRGACURE (R) 369E (manufactured by BASF Corporation), and 250 parts by mass of o-xylene was applied to a substrate film laminated with a rubbed alignment layer using a bar coater, and dried at 110° C. for 3 minutes to form a film with a thickness of 2 μm. Then, UV light was irradiated to set a polarizer on the substrate film.

[0366] Polarizer stacking method B

[0367] (Manufacture of substrate-laminated polarizing plate)

[0368] As a thermoplastic resin substrate, polyethylene terephthalate pellets (a) were used to prepare an unstretched film with a thickness of 100 μm, and an aqueous solution of polyvinyl alcohol with a polymerization degree of 2400 and a saponification degree of 99.9 mol % was applied to one side of the unstretched film and dried to form a PVA layer.

[0369] The obtained laminate was stretched to 2 times in the length direction between rollers of different circumferential speeds at 120°C and rolled up. Next, the obtained laminate was treated in a 4% boric acid aqueous solution for 30 seconds, then immersed in a mixed aqueous solution of iodine (0.2%) and potassium iodide (1%) for 60 seconds for dyeing, and then treated in a mixed aqueous solution of potassium iodide (3%) and boric acid (3%) for 30 seconds.

[0370] Furthermore, the laminate is uniaxially stretched in a mixed aqueous solution of boric acid (4%) and potassium iodide (5%) at 72°C in the length direction. The stretched laminate is then cleaned with a 4% potassium iodide aqueous solution, and after removing the aqueous solution with an air knife, it is dried in an oven at 80°C, cut at both ends and rolled up to obtain a substrate laminated polarizer with a width of 30cm and a length of 1000m. The total stretching ratio is 6.5 times, and the thickness of the polarizer is 5μm. It should be noted that the thickness is as follows: the substrate laminated polarizer is embedded in epoxy resin, the slice is cut out, and it is observed and read under an optical microscope.

[0371] (Lamination of polarizing layers)

[0372] After coating a UV-curable acrylic adhesive on a polyester film, the polarizer surface of the substrate-laminated polarizer cut to a desired length is laminated, and UV rays are irradiated from the substrate-laminated polarizer side to laminate the substrate-laminated polarizer on the polyester film. Thereafter, the thermoplastic resin substrate is peeled off and the polarizer is placed on the polyester film.

[0373] (Lamination of Phase Difference Layers)

[0374] As a method of providing a retardation layer on a polarizing plate, the following two methods are performed.

[0375] (C) Method of providing a quarter wavelength layer and a half wavelength layer on a release film and transferring the layer to a polarizing plate (retardation layer lamination method C)

[0376] (D) A method of providing a 1 / 2 wavelength layer on a 1 / 4 wavelength layer by coating, and laminating the 1 / 2 wavelength layer to a polarizing plate (retardation layer lamination method D)

[0377] The details of each method are described below.

[0378] Lamination method of phase difference layer C

[0379] A 50 μm thick biaxially stretched polyethylene terephthalate (PET) film was subjected to a brushing treatment, and a phase difference layer forming solution having the following composition was applied to the brushed surface by a rod coating method. The coated film was dried, oriented, and then cured by ultraviolet irradiation to form a 1 / 4 wavelength layer.

[0380] Phase difference layer forming solution

[0381] LC242 (manufactured by BASF Corporation) 75 parts by mass

[0382] 20 parts by mass of the following compounds

[0383]

[0384] 5 parts by mass of trimethylolpropane triacrylate

[0385] IRGACURE 379 3 parts by mass

[0386] Surfactant 0.1 parts by mass

[0387] 250 parts by mass of methyl ethyl ketone

[0388] Furthermore, a 2 mass % aqueous solution of polyvinyl alcohol (polyvinyl alcohol 1000 completely saponified type) (surfactant 0.2%) was applied to the 1 / 4 wavelength layer and dried to obtain a polyvinyl alcohol film with a thickness of about 100 nm. Then, the surface of the polyvinyl alcohol film was subjected to a brushing treatment. A phase difference layer forming solution was applied to the brushed surface of PVA by a rod coating method, dried, and oriented, and then cured by ultraviolet irradiation to set a 1 / 2 wavelength layer.

[0389] The phase difference was adjusted according to the film thickness, and the angle between the brushing direction when setting the 1 / 4 wavelength layer and the brushing direction when setting the 1 / 2 wavelength layer was 60 degrees. The light release liner of the optical transparent adhesive sheet was peeled off, and the adhesive surface was bonded to the 1 / 2 wavelength layer. After that, the heavy release liner of the optical transparent adhesive sheet was peeled off and bonded to the polarizer set on the polarizer protective film. After that, the biaxially stretched PET film was peeled off. The bonding was performed in a manner that the absorption axis of the polarizer was 15 degrees to the brushing direction of the 1 / 2 wavelength layer and 75 degrees to the brushing direction of the 1 / 4 wavelength layer.

[0390] Lamination method of phase difference layer D

[0391] A 1 / 4 wavelength roll is rolled out from a roll of a 1 / 4 wavelength film having a slow axis along the length direction, cut into the required length, and the surface is brushed. A phase difference layer forming solution is applied to the brushed surface by a rod coating method and dried. After orientation treatment, it is irradiated with ultraviolet light to solidify it and set a 1 / 2 wavelength layer. On the other hand, the light release liner of the optical transparent adhesive sheet is peeled off, so that the adhesive surface is bonded to the 1 / 2 wavelength layer. After that, the heavy release liner of the optical transparent adhesive sheet is peeled off and bonded to the polarizer set on the polarizer protective film. It should be noted that the 1 / 4 wavelength film used is a film (thickness 20μm) made by extruding a propylene-ethylene random copolymer (ethylene content 5%) in a sheet shape and stretching it with a roller along the length direction. The bonding is carried out in a manner that the absorption axis of the polarizer and the brushing direction of the 1 / 2 wavelength layer are 15 degrees and the slow axis direction of the 1 / 4 wavelength layer is 75 degrees.

[0392] The thickness of the retardation layer obtained by the above coating was 1.2 μm in the quarter wavelength layer and 2.3 μm in the half wavelength layer. The thickness of the adhesive layer was 3 μm.

[0393] Examples 1 to 26, Comparative Examples 1 to 3

[0394] A polarizing plate and a phase difference layer were provided on the PET film shown in Table 2 by the method shown in Table 2 to prepare a circularly polarizing plate, and the bending resistance was evaluated.

[0395] [Table 2]

[0396]

[0397] Industrial Applicability

[0398] The polarizing plate and circular polarizing plate for foldable display of the present invention are not easy to cause creases when repeatedly folded, and there is no need to worry about image distortion at the folded portion, so they can be suitable for foldable display. In addition, the foldable display of the present invention can display an image without distortion at the folded portion.

[0399] Description of Reference Numerals

[0400] 1: Foldable display

[0401] 11: Bending radius

[0402] 2: Polyester film used as polarizer protective film in polarizing plates of foldable displays

[0403] 21: Folding part

[0404] 22: Bending direction (direction perpendicular to the folded portion)

Claims

1. A polarizing plate for a foldable display, wherein a polarizing plate protective film comprising a polyester film is laminated on at least one surface of a polarizing plate, The polyester film is a biaxially stretched polyethylene terephthalate film. The polyester film meets the following conditions: (1) The refractive index in the bending direction is 1.590 to 1.600, (2) The refractive index in the direction of the folded portion is 1.687 to 1.700, (3) The refractive index in the thickness direction is less than 1.520, (4) Density: 1.383 g / cm 3 above, Here, the bending direction refers to the direction perpendicular to the folded portion when the polyester film is folded. The polarizer has a thickness of 12 μm or less. 2 . A circularly polarizing plate for a foldable display, comprising a phase difference layer on at least one surface of the polarizing plate for a foldable display according to claim 1 .

3. The circularly polarizing plate for a foldable display according to claim 2, wherein: There is no self-supporting film other than the polyester film, or there is only one self-supporting film.

4. The polarizing plate for a foldable display according to claim 1, wherein: The polarizer includes a polymerizable liquid crystal compound and a dichroic pigment.

5. The circularly polarizing plate for a foldable display according to claim 2 or 3, wherein: The polarizer includes a polymerizable liquid crystal compound and a dichroic pigment.

6. The circularly polarizing plate for a foldable display according to claim 2, wherein: The polyester film has an easy-adhesion layer.

7. The circularly polarizing plate for a foldable display according to claim 6, wherein: The easy-adhesion layer contains at least one resin selected from the group consisting of polyester resins, polyurethane resins, polyester polyurethane resins, polycarbonate resins, polycarbonate polyurethane resins, and acrylic resins.

8. The circularly polarizing plate for a foldable display according to claim 6, wherein: The easy-adhesion layer contains at least one water-soluble or water-dispersible resin selected from the group consisting of melamine compounds, isocyanate compounds, oxazoline compounds, and epoxy resins.

9. The circularly polarizing plate for a foldable display according to claim 2, wherein: The angle between the transmission axis of the polarizer and the slow axis of the polarizer protective film is 30 to 60 degrees.

10. The circularly polarizing plate for a foldable display according to claim 2, wherein: The angle between the transmission axis of the polarizer and the slow axis of the polarizer protective film is 0 to 10 degrees or 80 to 100 degrees. 11 . A foldable display comprising the polarizing plate for a foldable display according to claim 1 or 4 . 12 . A foldable display comprising the circularly polarizing plate for a foldable display according to claim 2 , 3 or 5 , wherein the phase difference layer comprises a liquid crystal compound.

13. A method for manufacturing a circular polarizing plate for a foldable display, comprising the following steps: (A) a process for preparing a polyester film having the following properties, (1) The refractive index in the bending direction is 1.590 to 1.600, (2) The refractive index in the direction of the folded portion is 1.687 to 1.700, (3) The refractive index in the thickness direction is less than 1.520, (4) Density: 1.383 g / cm 3 above, Here, the bending direction refers to the direction orthogonal to the folded portion when the polyester film is folded; (B) a step of providing a polarizing plate on the polyester film by any of the methods (a) and (b), (a) a method of transferring a polarizing plate provided on a releasable supporting substrate to a substrate film, (b) a method of forming a polarizing plate by coating a composition for a polarizing film comprising a polymerizable liquid crystal compound and a dichroic dye on a substrate film and aligning the composition; and, (C) a step of laminating a phase difference layer on the polarizing plate, The polyester film is a biaxially stretched polyethylene terephthalate film.

14. A method for manufacturing a circular polarizing plate for a foldable display, comprising the following steps: (A) a process for preparing a polyester film having the following properties, (1) The refractive index in the bending direction is 1.590 to 1.600, (2) The refractive index in the direction of the folded portion is 1.687 to 1.700, (3) The refractive index in the thickness direction is less than 1.520, (4) Density: 1.383 g / cm 3 above, Here, the bending direction refers to the direction orthogonal to the folded portion when the polyester film is folded; (B) a step of laminating a polarizing plate on the polyester film; and, (C) a step of providing a phase difference layer on the polarizing plate by any of the methods (c) and (d), (c) a method of transferring a phase difference layer provided on a releasable supporting substrate onto a polarizing plate, (d) a method of forming a phase difference layer by coating a phase difference layer composition containing a liquid crystal compound on a polarizing plate and orienting the composition, The polyester film is a biaxially stretched polyethylene terephthalate film.

15. The method for manufacturing a circularly polarizing plate for a foldable display according to claim 13, wherein: (C) The step of laminating a phase difference layer on the polarizing plate is any of the following methods: (c) a method of transferring a phase difference layer provided on a releasable supporting substrate onto a polarizing plate; or (d) A method of forming a retardation layer by coating a composition for a retardation layer containing a liquid crystal compound on a polarizing plate and aligning the composition.