Ultraviolet absorber, ultraviolet absorbing composition, ultraviolet absorbing film, laminate and novel compound

By introducing sulfonic acid groups or carboxylic acid groups into the ultraviolet absorber and optimizing the molecular structure, the stability problem of water-soluble ultraviolet absorber in aqueous media is solved, and efficient ultraviolet absorption and long-term long-term in the wavelength range of 380nm to 400nm is achieved. stability.

CN113993856BActive Publication Date: 2024-11-26FUJIFILM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080042155.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-06-28
Filing Date
2020-06-01
Publication Date
2024-11-26
Estimated Expiration
2040-06-01

AI Technical Summary

Technical Problem

The existing water-soluble ultraviolet absorbers have stability problems in aqueous media, especially in the long-wavelength ultraviolet band, which are insufficient in the absorption capacity and solubility of the long-wavelength ultraviolet band, and are prone to precipitation or condensation due to crystallization, affecting their application in water.

Method used

An ultraviolet absorber with benzodithiocyclopentane skeleton as the core is designed. By introducing sulfonic acid groups or carboxylic acid groups as substituents in the molecule, it forms an acid group, thereby improving its solubility and stability in water. and inhibit crystallization by specific molecular structure, so as to have good ultraviolet absorption capacity in the wavelength range of 380 nm to 400 nm.

Benefits of technology

High solubility in water and long-term stability in aqueous media are achieved, precipitation and aggregation of ultraviolet absorbers are inhibited, and the transparency and blocking properties of the ultraviolet absorbers are maintained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113993856B_ABST
    Figure CN113993856B_ABST
Patent Text Reader

Abstract

The present invention provides an ultraviolet absorber represented by the general formula (1) and its application. In the general formula (1), R 11 represents a monovalent substituent. n is 1 or 2. 1 and W 2 W each independently represents a hydrogen atom, a cyano group, a carbamoyl group, a sulfamoyl group, a nitro group, an acyl group, an alkylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an arylsulfinyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an alkyl group, an aryl group or a heterocyclic group, and W 1 and W 2 At least one of W represents a substituent with a Hammett substituent constant σp value of 0.2 or more. 1 and W 2 Can bond to each other to form a ring. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an ultraviolet absorber, an ultraviolet absorbing composition, an ultraviolet absorbing film, a laminate and a novel compound. Background Art

[0002] In order to reduce the influence of ultraviolet rays, various inorganic ultraviolet absorbers, organic ultraviolet absorbers, etc. are used together with liquid media, resins, etc. Among them, organic ultraviolet absorbers are more widely used than inorganic ultraviolet absorbers because they have a higher degree of freedom in formulation.

[0003] Organic ultraviolet absorbers are mostly oil-soluble compounds and are usually used in combination with organic solvents, oils, etc. When an organic ultraviolet absorber is used together with an aqueous medium, the ultraviolet absorber may be dissolved in an oil component to prepare an oil-in-water emulsion composition.

[0004] From the viewpoint of environmental load, a water-soluble ultraviolet absorber is required as the ultraviolet absorber, and a water-soluble ultraviolet absorber that absorbs short-wavelength ultraviolet rays is known.

[0005] However, water-soluble ultraviolet absorbers, which are ultraviolet absorbers capable of absorbing long-wavelength ultraviolet rays having a maximum absorption wavelength of 380 nm to 400 nm, have not been widely used.

[0006] Regarding water-soluble ultraviolet absorbers, for example, a two-layer cosmetic containing a phenylbenzimidazole compound having a sulfonic acid group as an ultraviolet absorber is disclosed, and the solubility of the water-soluble ultraviolet absorber in water is 0.01% or more (see Japanese Patent Application Laid-Open No. 2016-124817).

[0007] Furthermore, there is disclosed an ultraviolet absorber having two benzodithiocyclopentane skeletons in the molecule and having a maximum absorption in a wavelength range of 360 nm or longer, wherein the ultraviolet absorber may contain a water-soluble group as a substituent (see Japanese Patent No. 5364611).

[0008] Furthermore, a UV absorber is disclosed which can absorb UV rays with a wavelength of 320 nm to 400 nm and has a benzodithiocyclopentane skeleton whose UV absorption capacity is suppressed from decreasing over time. The UV absorber may have a carboxyl group or a sulfone group as a water-soluble group (see Japanese Patent Application Laid-Open No. 2009-263617). Summary of the invention

[0009] Technical issues to be solved by the invention

[0010] According to the research of the present inventors, the solubility in water of the ultraviolet absorber described in Japanese Patent Application Laid-Open No. 2016-124817 is not yet at a level that allows the ultraviolet absorber to stably exist alone in an aqueous medium.

[0011] Regarding the ultraviolet absorber described in Japanese Patent Gazette No. 5364611, although the ultraviolet absorption capacity is well maintained, if it is allowed to pass for a period of time in a medium such as an aqueous medium or a water-soluble polymer, precipitation may occur due to crystallization or haze (turbidity) or haze may increase due to aggregation, and there is room for improvement in stability in the medium.

[0012] Regarding the ultraviolet absorber described in Japanese Patent Publication No. 2009-263617, although specific examples of compounds having a carboxyl group as an acid group are disclosed, only compounds in which a carboxyl group is directly bonded to a benzene ring in a benzodithiocyclopentane skeleton are disclosed. The disclosed compounds have the same problem of poor stability in a medium as the ultraviolet absorber described in Japanese Patent Publication No. 5364611.

[0013] An object of one embodiment of the present invention is to provide a water-soluble ultraviolet absorbing composition having excellent temporal stability, comprising an ultraviolet absorber having ultraviolet absorbing ability at least in the wavelength range of 380 nm to 400 nm and having excellent solubility in water and temporal stability in an aqueous medium, and an aqueous medium.

[0014] Another embodiment of the present invention aims to provide an ultraviolet absorbing film having ultraviolet absorbing ability at least in the wavelength range of 380 nm to 400 nm, containing a water-soluble polymer and suppressing the time-dependent increase in haze, and a laminate having the ultraviolet absorbing film.

[0015] Another embodiment of the present invention aims to provide a novel compound having ultraviolet absorption capability at least in the wavelength range of 380 nm to 400 nm.

[0016] Means for solving technical problems

[0017] Means for solving the above-mentioned problems include the following aspects.

[0018] <1> A UV absorber represented by the following general formula (1).

[0019] [Chemical formula 1]

[0020]

[0021] In the general formula (1), R 11 represents a monovalent substituent. n is 1 or 2. When n is 2, the two R11 They can be the same or different.

[0022] W 1 and W 2 W each independently represents a hydrogen atom, a cyano group, a carbamoyl group, a sulfamoyl group, a nitro group, an acyl group, an alkylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an arylsulfinyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an alkyl group, an aryl group or a heterocyclic group, and W 1 and W 2 At least one of W represents a substituent with a Hammett's substituent constant σp value of 0.2 or more. 1 and W 2 They may be bonded to each other to form a ring.

[0023] R 11 , W 1 and W 2 At least one of the groups has an acid group selected from the group consisting of a sulfonic acid group, a carboxylic acid group, and a phosphoric acid group.

[0024] <2> according to <1> The ultraviolet absorber is represented by the following general formula (2).

[0025] [Chemical formula 2]

[0026]

[0027] In the general formula (2), R 1 and R 2 Each independently represents a monovalent substituent.

[0028] W 1 and W 2 W each independently represents a hydrogen atom, a cyano group, a carbamoyl group, a sulfamoyl group, a nitro group, an acyl group, an alkylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an arylsulfinyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an alkyl group, an aryl group or a heterocyclic group, and W 1 and W 2 At least one of W represents a substituent with a Hammett's substituent constant σp value of 0.2 or more. 1 and W 2 They may be bonded to each other to form a ring.

[0029] R 1 , R 2 , W 1 and W 2 At least one of the groups has an acid group selected from the group consisting of a sulfonic acid group, a carboxylic acid group, and a phosphoric acid group.

[0030] <3> according to <1> The ultraviolet absorber is represented by the following general formula (3).

[0031] [Chemical formula 3]

[0032]

[0033] In the general formula (3), R 1 and R 2 Each independently represents a monovalent substituent.

[0034] R 3 represents an alkyl group, an aryl group or a heterocyclic group,

[0035] R 1 , R 2 and R 3 At least one of the groups has an acid group selected from the group consisting of a sulfonic acid group, a carboxylic acid group, and a phosphoric acid group.

[0036] <4> according to <1> to <3> The ultraviolet absorber according to any one of the preceding claims, wherein

[0037] The acid group is a sulfonic acid group.

[0038] <5> according to <1> to <4> The ultraviolet absorber described in any one of the above aspects has a solubility in water at 25° C. of 1% by mass or more.

[0039] <6> A UV absorbing composition comprising <1> to <5> The ultraviolet absorber described above and an aqueous medium.

[0040] <7> according to <6> The ultraviolet absorbing composition further comprises a water-soluble polymer.

[0041] <8> A UV absorbing film, which is <6> or <7> The cured product of the ultraviolet absorbing composition.

[0042] <9> A laminated body comprising a substrate and a <8> The ultraviolet absorbing film.

[0043] <10> A compound represented by the following general formula (4).

[0044] [Chemical formula 4]

[0045]

[0046] In the general formula (4), L 1 and L 2 Each independently represents an alkylene group.

[0047] X each independently represents a hydrogen atom or -SO3 - of the counter cation.

[0048] W 1 and W 2W each independently represents a hydrogen atom, a cyano group, a carbamoyl group, a sulfamoyl group, a nitro group, an acyl group, an alkylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an arylsulfinyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an alkyl group, an aryl group or a heterocyclic group, and W 1 and W 2 At least one of W represents a substituent with a Hammett's substituent constant σp value of 0.2 or more. 1 and W 2 They may be bonded to each other to form a ring.

[0049] Effects of the Invention

[0050] According to one embodiment of the present invention, there is provided a water-soluble ultraviolet absorbing composition having excellent temporal stability, comprising an ultraviolet absorber having ultraviolet absorbing ability at least in the wavelength range of 380 nm to 400 nm and having excellent solubility in water and temporal stability in an aqueous medium, and an aqueous medium.

[0051] According to another embodiment of the present invention, there can be provided an ultraviolet absorbing film having ultraviolet absorbing ability at least in the wavelength range of 380 nm to 400 nm, containing a water-soluble polymer, and suppressing the time-dependent increase in haze, and a laminate having the ultraviolet absorbing film.

[0052] According to another embodiment of the present invention, there is provided a novel compound having ultraviolet absorption capability at least in the wavelength range of 380 nm to 400 nm. DETAILED DESCRIPTION

[0053] Hereinafter, the ultraviolet absorber, ultraviolet absorbing composition, ultraviolet absorbing film, laminated body and compound of the present invention will be described.

[0054] However, the ultraviolet absorber, ultraviolet absorbing composition, laminate, and novel compound of the present invention are not limited to any of the embodiments described below, and can be implemented with appropriate changes within the intended range.

[0055] In the present invention, a numerical range expressed by "to" indicates a range including the numerical values ​​described before and after "to" as the minimum value and the maximum value, respectively.

[0056] In the numerical ranges recorded in stages in the present invention, the upper limit or lower limit recorded in a certain numerical range can be replaced by the upper limit or lower limit of the numerical range recorded in other stages. In addition, in the numerical ranges recorded in the present invention, the upper limit or lower limit recorded in a certain numerical range can be replaced by the value shown in the embodiments.

[0057] Furthermore, in the present invention, a combination of two or more preferred aspects is a more preferred aspect.

[0058] When there are plural substances corresponding to each component in the present invention, the content of each component means the total content of the plural substances unless otherwise specified.

[0059] In the present invention, “(meth)acrylic acid” means at least one of acrylic acid and methacrylic acid, and “(meth)acrylate” means at least one of acrylate and methacrylate.

[0060] Unless otherwise specified, the term "substituent" is used to mean an unsubstituted substituent or a substituent further having a substituent. For example, when "alkyl" is used, it is used to mean both an unsubstituted alkyl group and an alkyl group further having a substituent. The same applies to other substituents.

[0061] In the present invention, the term "process" includes not only independent processes but also processes that cannot be clearly distinguished from other processes as long as the intended purpose of the process can be achieved.

[0062] In the present invention, "the compound is water-soluble" means that the compound dissolves in water at 25°C at a rate of 1% by mass or more.

[0063] Furthermore, the "ultraviolet absorption ability" in the present invention refers to the absorption of at least ultraviolet rays in the wavelength range of 380nm to 400nm, and includes not only completely blocking ultraviolet rays in the wavelength range of 380nm to 400nm by absorption, but also absorbing at least a portion of the above ultraviolet rays and reducing the transmittance of ultraviolet rays.

[0064] [Ultraviolet absorber represented by general formula (1)]

[0065] The ultraviolet absorber of the present invention is represented by the following general formula (1).

[0066] In addition, hereinafter, the ultraviolet absorber represented by the following general formula (1) may be referred to as a "specific ultraviolet absorber".

[0067] 〔Specific UV absorbers〕

[0068] The specific ultraviolet absorber of the present invention is represented by the following general formula (1).

[0069] The specific ultraviolet absorber is a compound having only one benzodithiocyclopentane skeleton in the molecule, and preferably has a maximum absorption wavelength in the wavelength range of 380 nm to 400 nm.

[0070] [Chemical formula 5]

[0071]

[0072] In the general formula (1), R 11represents a monovalent substituent. n is 1 or 2. When n is 2, there are two R 11 They can be the same or different.

[0073] W 1 and W 2 W each independently represents a hydrogen atom, a cyano group, a carbamoyl group, a sulfamoyl group, a nitro group, an acyl group, an alkylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an arylsulfinyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an alkyl group, an aryl group or a heterocyclic group, and W 1 and W 2 At least one of them represents a substituent with a Hammett substituent constant σp value of 0.2 or more, W 1 and W 2 They may be bonded to each other to form a ring.

[0074] R 11 , W 1 and W 2 At least one of the groups has an acid group selected from the group consisting of a sulfonic acid group, a carboxylic acid group, and a phosphoric acid group.

[0075] The mechanism of action of the present invention is not yet clear, but is presumed to be as follows.

[0076] It is speculated that the specific ultraviolet absorber of the present invention has only one benzodithiocyclopentane skeleton in the molecule, so the crystallization rate becomes slow. In addition, the acid group in the specific ultraviolet absorber is a structure bonded to the benzene ring or to the dithiocyclopentane skeleton via an oxygen atom, and it is therefore believed that even if the specific ultraviolet absorber is allowed to pass in an aqueous medium for a period of time, precipitation caused by long-term crystallization can be suppressed, and the stability in the aqueous medium becomes good.

[0077] It is presumed that the slow crystallization rate of the specific ultraviolet absorber suppresses precipitation and aggregation of the specific ultraviolet absorber due to crystallization in the ultraviolet absorbing film which is a cured product of the ultraviolet absorbing composition containing the specific ultraviolet absorber, thereby suppressing an increase in haze of the ultraviolet absorbing film for a long period of time.

[0078] Furthermore, the specific ultraviolet absorber has a good ultraviolet absorption capability at least in the wavelength range of 380 nm to 400 nm due to the benzodithiocyclopentane skeleton contained in the molecule.

[0079] When the maximum absorption wavelength of the specific ultraviolet absorber is greater than 380 nm, better ultraviolet blocking properties on the long wavelength side can be obtained, and when it is less than 400 nm, coloration of a cured product of the ultraviolet absorbing composition containing the specific ultraviolet absorber, such as an ultraviolet absorbing film, can be suppressed.

[0080] In addition, the above-mentioned mechanism of action is only speculation and does not impose any limitation on the present invention.

[0081] For example, the maximum absorption wavelength of the ultraviolet absorber can be measured using a spectrophotometer. Examples of the device include SHIMADZU CORPORATION's spectrophotometer UV3600 and ultraviolet-visible-near-infrared spectrophotometer UV3150. In the present invention, the maximum absorption wavelength of the ultraviolet absorber is measured using the spectrophotometer UV3600.

[0082] The measurement was performed at room temperature (25° C.) under the conditions that air was used as a reference, and the absorbance was measured using a spectrophotometer to obtain an absorption spectrum.

[0083] By measuring the absorbance at wavelengths in a predetermined wavelength range, the maximum absorption wavelength, transmittance, etc. can be calculated.

[0084] Each substituent in the above general formula (1) is described below.

[0085] In the general formula (1), R 11 Represents a monovalent substituent. Examples of the monovalent substituent include an alkyl group, an aryl group, a heterocyclic group, an acyl group, a carbamoyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an alkylsulfonyl group, an arylsulfonyl group, and a sulfamoyl group. From the viewpoint of suppressing the crystallization rate of the specific ultraviolet absorber to a lower level, the monovalent substituent is preferably an alkyl group, an aryl group, an alkoxycarbonyl group, and the like.

[0086] The monovalent substituent may be unsubstituted or may further have a substituent.

[0087] As R 11 When the monovalent substituent further has a substituent, examples of the substituent that can be introduced include an acid group selected from the group including (selected from the group including the substituents listed as examples of the monovalent substituent) a sulfonic acid group, a carboxylic acid group and a phosphoric acid group.

[0088] The alkyl group as a monovalent substituent may be linear or branched, or may form a ring. The alkyl group preferably has 1 to 20 carbon atoms, more preferably 1 to 18 carbon atoms.

[0089] Examples of the alkyl group include methyl, ethyl, n-propyl, isopropyl, tert-butyl, n-octyl, eicosyl, 2-chloroethyl, 2-cyanoethyl, 2-ethylhexyl, cyclohexyl, cyclopentyl, and 4-n-dodecylcyclohexyl.

[0090] The aryl group is preferably an aryl group having 6 to 30 carbon atoms, and examples thereof include phenyl, p-tolyl, naphthyl, m-chlorophenyl, and o-hexadecanoylaminophenyl, and phenyl is preferred.

[0091] A heterocyclic group is a monovalent group obtained by removing a hydrogen atom from an aromatic or non-aromatic heterocyclic compound, and these may be further fused.

[0092] The heterocyclic group is preferably a 5- or 6-membered heterocyclic group, and the heteroatom constituting the ring is preferably an oxygen atom, a sulfur atom, or a nitrogen atom, and more preferably a 5- or 6-membered aromatic heterocyclic group having 3 to 30 carbon atoms.

[0093] Examples of the heterocyclic ring in the heterocyclic group include a pyridine ring, a pyrazine ring, a pyridazine ring, a pyrimidine ring, a triazine ring, a quinoline ring, an isoquinoline ring, a quinazoline ring, a cinnoline ring, a phthalazine ring, a quinoxaline ring, a pyrrole ring, an indole ring, a furan ring, a benzofuran ring, a thiophene ring, a benzothiophene ring, a pyrazole ring, an imidazole ring, a benzimidazole ring, a triazole ring, an oxazole ring, a benzoxazole ring, a thiazole ring, a benzothiazole ring, an isothiazole ring, a benzisothiazole ring, a thiadiazole ring, an isoxazole ring, a benzisoxazole ring, a pyrrolidine ring, a piperidine ring, a piperazine ring, an imidazoline ring, and a thiazoline ring.

[0094] The acyl group is preferably a formyl group, an aliphatic carbonyl group having 2 to 30 carbon atoms (e.g., an alkylcarbonyl group), an arylcarbonyl group having 7 to 30 carbon atoms (preferably a phenylcarbonyl group), or a heterocyclic carbonyl group having 4 to 30 carbon atoms bonded to a carbonyl group via a carbon atom.

[0095] Examples of the acyl group include acetyl, pivaloyl, 2-chloroacetyl, stearoyl, benzoyl, p-n-octyloxyphenylcarbonyl, 2-pyridylcarbonyl, and 2-furylcarbonyl.

[0096] The carbamoyl group is preferably a carbamoyl group having 1 to 30 carbon atoms. Examples of the carbamoyl group include a carbamoyl group, an N-methylcarbamoyl group, an N,N-dimethylcarbamoyl group, an N,N-di-n-octylcarbamoyl group, and an N-(methylsulfonyl)carbamoyl group.

[0097] The alkoxycarbonyl group is preferably an alkoxycarbonyl group having 2 to 20 carbon atoms, and more preferably an alkoxycarbonyl group having 2 to 9 carbon atoms.

[0098] Examples of the alkoxycarbonyl group include a methoxycarbonyl group, an ethoxycarbonyl group, a tert-butoxycarbonyl group, and a benzyloxycarbonyl group.

[0099] The aryloxycarbonyl group is preferably an aryloxycarbonyl group having 7 to 30 carbon atoms. Examples of the aryloxycarbonyl group include a phenoxycarbonyl group, an o-chlorophenoxycarbonyl group, a m-nitrophenoxycarbonyl group, and a p-tert-butylphenoxycarbonyl group. A phenoxycarbonyl group is preferred.

[0100] Examples of the alkylsulfonyl group or arylsulfonyl group include aliphatic sulfonyl groups having 1 to 30 carbon atoms (e.g., alkylsulfonyl groups) and arylsulfonyl groups having 6 to 30 carbon atoms (preferably, phenylsulfonyl groups). Specific examples include methylsulfonyl, ethylsulfonyl, phenylsulfonyl, and p-toluenesulfonyl groups.

[0101] The sulfamoyl group is preferably a sulfamoyl group having 0 to 30 carbon atoms. Examples of the sulfamoyl group include a sulfamoyl group, an N,N-dimethylaminosulfonyl group, and an N-n-octylaminosulfonyl group.

[0102] In the general formula (1), n ​​is 1 or 2. From the viewpoint of improving the solubility of the specific ultraviolet absorber in water and the stability in an aqueous medium, n is preferably 2. When n is 2, there are two R 11 They may be the same or different from each other, but are preferably the same in terms of synthetic suitability.

[0103] W 1 and W 2 W each independently represents a hydrogen atom, a cyano group, an alkylcarbonyl group, an arylcarbonyl group, a carbamoyl group, a sulfamoyl group, a nitro group, an acyl group, an alkylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an arylsulfinyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an alkyl group, an aryl group or a heterocyclic group, and W 1 and W 2 At least one of them represents a substituent having a Hammett's substituent constant σp value of 0.2 or more.

[0104] If it can be imported, then W 1 and W 2 It may further have a substituent.

[0105] The Hammett's substituent constant σp value will be described.

[0106] The Hammett equation is an empirical equation advocated by LP Hammett in 1935 to quantitatively demonstrate the effect of substituents on the reaction or equilibrium of benzene derivatives. Its effectiveness has been widely recognized. The substituent constants obtained by the Hammett equation include σp value and σm value, which can be found in many general books. For example, J.A. Dean, "Lange's Handbook of Chemistry", 12th edition, 1979 (McGraw-Hill), "Chemical Field", Supplement, No. 122, pp. 96-103, 1979 (Nankodo), Chem. Rev., 1991, Vol. 91, pp. 165-195, etc. have detailed records.

[0107] In the present invention, a substituent having a Hammett substituent constant σp of 0.2 or more refers to an electron withdrawing group. The σp value is preferably 0.25 or more, more preferably 0.3 or more, and particularly preferably 0.35 or more. The upper limit of the σp value is not particularly limited, but is preferably 1.20 or less, and more preferably 1.00 or less.

[0108] Examples of substituents having a Hammett substituent constant σp value of 0.2 or more include cyano (0.66), alkoxycarbonyl (-COOMe: 0.45), aryloxycarbonyl (-COOPh: 0.44), carbamoyl (-CONH2: 0.36), alkylcarbonyl (-COMe: 0.50), arylcarbonyl (-COPh: 0.43), and alkylsulfonyl (-SO2Me: 0.72). 1 or W 2 The σp value of the carboxylic acid group (—COOH) which may be present as the acid group is 0.45, and is included in the substituents having a σp value of 0.2 or more.

[0109] In the present invention, a methyl group may be abbreviated as Me, and a phenyl group may be abbreviated as Ph.

[0110] The values ​​in parentheses are σp values ​​of representative substituents extracted from Chem. Rev., 1991, Vol. 91, pp. 165-195.

[0111] W 1 and W 2 Examples of the carbamoyl, sulfamoyl, nitro, acyl, alkylsulfonyl, arylsulfonyl, alkylsulfinyl, arylsulfinyl, alkoxycarbonyl, aryloxycarbonyl, alkyl and aryl groups in R are the same as those shown in R 11 The groups are the same.

[0112] As W 1 and W 2 When the heterocyclic group is represented, the heterocyclic group is preferably a heterocyclic group obtained by removing one hydrogen atom from a 5-membered or 6-membered saturated or unsaturated heterocyclic ring. The heterocyclic ring may be further condensed with an aliphatic ring, an aromatic ring or another heterocyclic ring.

[0113] Examples of the hetero atom contained in the heterocyclic ring include B, N, O, S, Se, and Te. As the hetero atom, N, O, and S are preferred.

[0114] The heterocyclic ring has a free carbon atom (monovalent), and the heterocyclic group is bonded to an adjacent carbon atom, an oxygen atom, or a nitrogen atom on the carbon atom.

[0115] The heterocyclic group may further have a substituent, and examples of the substituent that can be introduced include the substituents described in paragraphs

[0020] to

[0039] of JP-A-2008-81445.

[0116] The number of carbon atoms in the heterocyclic group is preferably 3 to 40, more preferably 3 to 30, and further preferably 3 to 20. Examples of saturated heterocyclic rings include pyrrolidine rings, morpholine rings, 2-borane-1,3-dioxolane rings, and 1,3-thiazolidine rings. Examples of unsaturated heterocyclic rings include imidazole rings, thiazole rings, benzothiazole rings, benzoxazole rings, benzotriazole rings, benzoselenazole rings, pyridine rings, pyrimidine rings, and quinoline rings. Preferably, the heterocyclic group is a group in which one hydrogen atom is removed from these saturated heterocyclic rings.

[0117] W 1 and W 2 Can be bonded to each other to form a ring, as W 1 and W 2 The ring that can be formed includes an aliphatic ring, an aromatic ring, a heterocyclic ring, etc., and may be a condensed ring formed by condensing two or more rings. 1 and W 2 Examples of the ring that can be formed include cyclohexane-1,3-dione, cyclopentane-1,3-dione, and pyrazolidine-1,3-dione.

[0118] In the general formula (1), R 11 , W 1 and W 2 At least one of the groups has an acid group selected from the group consisting of a sulfonic acid group, a carboxylic acid group, and a phosphoric acid group. The position of the acid group is arbitrary and can be 11 , W 1 and W 2 An acid group is bonded to the substituent exemplified as the substituent.

[0119] R 11 , W 1 and W 2 When at least one of the groups has an acid group, the number of acid groups possessed by each group is arbitrary, but from the viewpoint of synthetic suitability, an embodiment in which each group has one acid group is preferred.

[0120] As the acid group, from the viewpoint of better solubility of the specific ultraviolet absorber in water, a sulfonic acid group and a phosphoric acid group are preferred, and a sulfonic acid group is more preferred.

[0121] The acid group may be in the form of a salt. Examples of the salt of the acid group that can dissociate into a counter cation in an aqueous medium include alkali metal salts such as sodium salts, potassium salts, and lithium salts, and quaternary ammonium salts.

[0122] The number of acid groups in the compound represented by the general formula (1) may be 1 or more, and may have 2 or more acid groups. The upper limit of the number of acid groups is not particularly limited, but is preferably 5 or less. From the viewpoint of better solubility of the specific ultraviolet absorber in water and better stability in an aqueous medium, the number of acid groups possessed by the specific ultraviolet absorber is preferably 1 to 4, and more preferably 2 to 3.

[0123] When the specific ultraviolet absorber has two or more acid groups, the plurality of acid groups may be the same as or different from each other. In terms of synthetic suitability, the plurality of acid groups are preferably the same as each other.

[0124] From the viewpoint of stability in an aqueous medium, the solubility of the specific ultraviolet absorber in water at 25° C. is preferably 1% by mass. The solubility in water at 25° C. is more preferably 1.5% by mass or more, further preferably 2% by mass or more, and further preferably 3% by mass or more.

[0125] The solubility of the specific ultraviolet absorber in the present invention in water can be measured by the following method based on the amount of the specific ultraviolet absorber dissolved in 10 g of distilled water at 25°C.

[0126] After 10 g of distilled water was mixed with 1 g of the specific ultraviolet absorber, ultrasonic waves were irradiated at a liquid temperature of 25° C. for 15 minutes, and the liquid temperature was maintained at 25° C. and allowed to stand for 24 hours. The ultrasonic waves were irradiated using Bransonic tabletop ultrasonic cleaner 1510 manufactured by Emerson Japan, Ltd.'s Branson Business Headquarters.

[0127] After standing for 24 hours, the mixture was filtered using a membrane filter (0.1 μm mesh, manufactured by Advantec Co., Ltd.). The specific ultraviolet absorber that was not filtered was separated and the mass was measured after drying. The amount of the specific ultraviolet absorber that was not filtered was removed from 1 g of the specific ultraviolet absorber to obtain the amount of the specific ultraviolet absorber dissolved in water, and the solubility of the specific ultraviolet absorber in water was calculated based on this value.

[0128] As an example of a preferred embodiment of the compound represented by the general formula (1), a compound represented by the following general formula (2) can be cited. From the viewpoint of more effectively absorbing long-wavelength ultraviolet rays and having higher solubility in water, the ultraviolet absorber represented by the general formula (1) is preferably an ultraviolet absorber represented by the following general formula (2).

[0129] [Chemical formula 6]

[0130]

[0131] In the general formula (2), R 1 and R 2Each independently represents a monovalent substituent.

[0132] W 1 and W 2 W each independently represents a hydrogen atom, a cyano group, a carbamoyl group, a sulfamoyl group, a nitro group, an acyl group, an alkylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an arylsulfinyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an alkyl group, an aryl group or a heterocyclic group, and W 1 and W 2 At least one of them represents a substituent with a Hammett substituent constant σp value of 0.2 or more, W 1 and W 2 They may be bonded to each other to form a ring.

[0133] R 1 , R 2 , W 1 and W 2 At least one of the groups has an acid group selected from the group consisting of a sulfonic acid group, a carboxylic acid group, and a phosphoric acid group.

[0134] In the general formula (2), R 1 and R 2 The meanings are the same as those of R in the above general formula (1). 11 The same applies to the preferred examples.

[0135] In the general formula (2), W 1 and W 2 The meanings of are independently the same as those of W in the above general formula (1). 1 and W 2 same.

[0136] In the general formula (2), from the viewpoint of improving the solubility of the specific ultraviolet absorber in water and the stability in the aqueous medium, W 1 and W 2 Preferred are cyano, alkylcarbonyl, arylcarbonyl, alkylsulfonyl, arylsulfonyl, alkylsulfinyl, arylsulfinyl, alkoxycarbonyl, aryloxycarbonyl and the like, and more preferred are cyano, alkylcarbonyl, arylcarbonyl, alkoxycarbonyl and the like.

[0137] In the general formula (2), R 1 , R 2 , W 1 and W 2 The acid group of at least one of the groups is selected from the group consisting of a sulfonic acid group, a carboxylic acid group and a phosphoric acid group, preferably a sulfonic acid group and a phosphoric acid group, and more preferably a sulfonic acid group. As described above, the acid group may be in a salt state.

[0138] The number of acid groups in the compound represented by the general formula (2) may be 1 or more, and may have 2 or more acid groups. The upper limit of the number of acid groups is the same as that of the general formula (1).

[0139] The number of acid groups in the general formula (2) is preferably 1 to 3, more preferably 2, from the viewpoint of improving the solubility of the specific ultraviolet absorber in water and the stability in an aqueous medium.

[0140] When the specific ultraviolet absorber represented by the general formula (2) has two or more acid groups, the acid groups may be the same as or different from each other. In terms of synthetic suitability, the acid groups are preferably the same as each other.

[0141] Preferred combinations of substituents in the general formula (2) include: 1 and R 2 is an alkyl group having a sulfonic acid group, a phosphoric acid group or a carboxylic acid group and W 1 and W 2 One of them is cyano and the other is arylcarbonyl or alkylcarbonyl, R 1 and R 2 is an alkyl group having a sulfonic acid group and W 1 and W 2 Both are cyano groups, R 1 and R 2 is an alkyl group having a sulfonic acid group and W 1 and W 2 A combination of one of which is a cyano group and the other is an alkoxyimino group, R 1 and R 2 is an alkyl group having a sulfonic acid group and W 1 and W 2 One of them is a cyano group and the other is a sulfonyl group, and the like.

[0142] As another preferred embodiment of the compound represented by the general formula (1), a compound represented by the following general formula (3) can be cited. From the viewpoint of higher light stability and higher solubility in water, the ultraviolet absorber represented by the general formula (1) is preferably an ultraviolet absorber represented by the following general formula (3).

[0143] [Chemical formula 7]

[0144]

[0145] In the general formula (3), R 1 and R 2 Each independently represents a monovalent substituent.

[0146] R 3 represents an alkyl group, an aryl group or a heterocyclic group,

[0147] R 1 , R 2 and R 3At least one of the groups has an acid group selected from the group consisting of a sulfonic acid group, a carboxylic acid group, and a phosphoric acid group.

[0148] In the general formula (3), R 1 and R 2 The meanings are the same as those of R in the above general formula (1). 11 The same applies to the preferred examples.

[0149] In the general formula (3), R 3 represents an alkyl group, an aryl group or a heterocyclic group, and an alkyl group, an aryl group or the like is preferred from the viewpoint of better stability of the specific ultraviolet absorber in an aqueous medium.

[0150] The two R in the general formula (3) 3 Same as each other.

[0151] In the general formula (3), R 1 , R 2 and R 3 The acid group of at least one of the groups is selected from the group consisting of a sulfonic acid group, a carboxylic acid group and a phosphoric acid group, preferably a sulfonic acid group and a phosphoric acid group, and more preferably a sulfonic acid group. As described above, the acid group may be in a salt state.

[0152] The number of acid groups in the compound represented by the general formula (3) may be 1 or more, and may have 2 or more acid groups. The upper limit of the number of acid groups is the same as that of the general formula (1).

[0153] The number of acid groups in the general formula (3) is preferably 1 to 3, more preferably 2 to 3, from the viewpoint of improving the solubility of the specific ultraviolet absorber in water and the stability in an aqueous medium.

[0154] When the specific ultraviolet absorber represented by the general formula (3) has two or more acid groups, the plurality of acid groups may be the same as or different from each other. In terms of synthetic suitability, the plurality of acid groups are preferably the same as each other.

[0155] Preferred combinations of substituents in the general formula (3) include: 1 and R 2 is an alkyl group having a sulfonic acid group or an alkyl group having a phosphoric acid group and R 3 is a combination of alkyl or aryl, R 1 and R 2 One of them is an alkyl group, the other is an alkyl group having a sulfonic acid group, and R 3 is a combination of an alkyl group having a sulfonic acid group, R 1 and R 2 is an alkyl group and R 3 It is a combination of an alkyl group having a sulfonic acid group or a phosphoric acid group, and the like.

[0156] [Compound represented by general formula (4)]

[0157] In the present invention, the compound represented by the following general formula (4) is a novel compound.

[0158] [Chemical formula 8]

[0159]

[0160] In the general formula (4), L 1 and L 2 Each independently represents an alkylene group.

[0161] X each independently represents a hydrogen atom or -SO3 - of the counter cation.

[0162] W 1 and W 2 W each independently represents a hydrogen atom, a cyano group, a carbamoyl group, a sulfamoyl group, a nitro group, an acyl group, an alkylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an arylsulfinyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an alkyl group, an aryl group or a heterocyclic group, and W 1 and W 2 At least one of them represents a substituent with a Hammett substituent constant σp value of 0.2 or more, W 1 and W 2 They may be bonded to each other to form a ring.

[0163] L 1 and L 2 Each independently represents an alkylene group, and is preferably an alkylene group having 1 to 10 carbon atoms, and more preferably an alkylene group having 2 to 5 carbon atoms.

[0164] X each independently represents a hydrogen atom or -SO3 - As the counter cation, an alkali metal ion such as sodium ion, potassium ion, lithium ion, etc. is preferred.

[0165] W 1 and W 2 W each independently represents a hydrogen atom, a cyano group, a carbamoyl group, a sulfamoyl group, a nitro group, an acyl group, an alkylsulfonyl group, an arylsulfonyl group, an alkylsulfinyl group, an arylsulfinyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an alkyl group, an aryl group or a heterocyclic group, and W 1 and W 2 At least one of them represents a substituent with a Hammett substituent constant σp value of 0.2 or more, W 1 and W 2 They may be bonded to each other to form a ring.

[0166] W 1 and W 2 The meaning of is the same as W in the general formula (1) 1 and W2 The same applies to the preferred examples.

[0167] The compound represented by the general formula (4) has a maximum absorption in the wavelength range of 380 nm to 400 nm and can be used as an ultraviolet absorber.

[0168] The following are illustrated compounds (M-1) to (M-10) as preferred examples of the compound represented by the general formula (1), i.e., specific examples of the compound represented by the general formula (2), and (M-11) to (M-20) as specific examples of the compound represented by the general formula (3) by clearly indicating the general formula and the substituents in the general formula. In addition, the specific ultraviolet absorber in the present invention is not limited to the following illustrated compounds.

[0169] The solubility of each compound in water at 25° C. is also described (described as “solubility (25° C.)” in the table). The method for measuring the solubility in water (distilled water) is as described above.

[0170] In the following exemplary compounds, "Me" represents a methyl group, "Et" represents an ethyl group, "Ph" represents a phenyl group, "n-Bu" represents an n-butyl group, and "t-Bu" represents a tert-butyl group.

[0171] [Chemical formula 9]

[0172]

[0173] [Chemical formula 10]

[0174]

[0175] [Chemical formula 11]

[0176]

[0177] [Chemical formula 12]

[0178]

[0179] Among the above-mentioned exemplified compounds, from the viewpoint of better solubility in water and stability in aqueous media, preferred are compounds (M-1) to (M-3), (M-11) to (M-13), (M-14) and (M-16), and more preferred are compounds (M-3), (M-11) and (M-12).

[0180] In addition, among the above-mentioned exemplary compounds, compounds (M-1), (M-2), (M-3), (M-5), (M-6), (M-11), (M-12), (M-13) and (M-16) are novel compounds included in the general formula (4).

[0181] The specific ultraviolet absorber has good ultraviolet absorbency at a wavelength of 380nm to 400nm, and has good solubility in water and stability in aqueous media, so it is not easy to aggregate or precipitate even if it is left in an aqueous medium for a period of time. In addition, when the ultraviolet absorbing composition containing the specific ultraviolet absorber, the water-soluble polymer and the aqueous medium is cured to form an ultraviolet absorbing film, the transparency of the ultraviolet absorbing film is good and the increase in haze caused by aggregation or precipitation of the specific ultraviolet absorber in the ultraviolet absorbing film is suppressed.

[0182] The "haze" in the present invention can be measured with a haze meter.

[0183] As the haze meter, for example, a haze meter (manufactured by NIPPON DENSHOKU INDUSTRIES Co., Ltd., NDH4000: device name), a haze meter (manufactured by Suga Test Instruments Co., Ltd., HGM-2DP: device name), etc. can be used.

[0184] The specific ultraviolet absorber of the present invention having a sulfonic acid group in the molecule can be synthesized by reacting a cyclic sulfone with a corresponding hydroxyl body or amino body having a benzothiocyclopentane skeleton under basic conditions.

[0185] Furthermore, the specific ultraviolet absorber of the present invention having a carboxylic acid group in the molecule can be synthesized by reacting an acid anhydride with a corresponding hydroxyl body or amino body having a benzothiocyclopentane skeleton under basic conditions.

[0186] The detailed synthesis method will be described in the examples given below.

[0187] [Ultraviolet absorbing composition]

[0188] The ultraviolet absorbing composition of the present invention contains the above-mentioned specific ultraviolet absorber of the present invention and an aqueous medium.

[0189] The ultraviolet absorbing composition of the present invention may contain only one type of the above-mentioned specific ultraviolet absorber, or may contain two or more types.

[0190] The content of the specific ultraviolet absorber based on the total amount of the ultraviolet absorbing composition can be appropriately selected depending on the purpose.

[0191] Among them, the content of the specific ultraviolet absorber relative to the total amount of the ultraviolet absorbing composition is preferably 0.05% by mass to 5.0% by mass, and more preferably 0.10% by mass to 3.0% by mass.

[0192] When the content of the specific ultraviolet absorber is 0.05% by mass or more, the ultraviolet absorbing composition can obtain sufficient ultraviolet absorbency, and when the content of the specific ultraviolet absorber is 5.0% by mass or less, the occurrence of turbidity, increase in haze, etc. caused by precipitation or aggregation of the specific ultraviolet absorber in the ultraviolet absorbing composition and the cured product of the ultraviolet absorbing composition can be more effectively suppressed.

[0193] The specific ultraviolet absorber of the present invention has good solubility in water and stability in an aqueous medium, so the ultraviolet absorbing composition of the present invention is also excellent in stability over time. More specifically, even if the ultraviolet absorbing composition of the present invention (hereinafter, sometimes referred to as "the composition of the present invention" or "composition") is left in an aqueous medium for a period of time, the decrease in ultraviolet absorbency and changes in appearance of the ultraviolet absorbing composition caused by precipitation or aggregation of the specific ultraviolet absorber of the present invention can be suppressed.

[0194] (Aqueous medium)

[0195] The "aqueous medium" in the present invention refers to water and a mixture of water and a water-soluble organic solvent.

[0196] The aqueous medium functions as a solvent for the specific ultraviolet absorber.

[0197] Examples of the water-soluble organic solvent that the aqueous medium may contain include monohydric alcohols having 1 to 3 carbon atoms (such as methanol, ethanol, and propanol), polyhydric alcohols having 1 to 4 carbon atoms (such as diethylene glycol and glycerol), tetrahydrofuran, acetonitrile, and dimethyl sulfoxide.

[0198] The water-soluble organic solvent to be mixed with water may be used alone or in combination of two or more, as necessary.

[0199] Examples of the aqueous medium that can be used in the ultraviolet absorbing composition of the present invention include water, a mixture of water and a monohydric alcohol having 1 to 3 carbon atoms, and acetonitrile.

[0200] From the viewpoint of the stability of the specific ultraviolet absorber in the ultraviolet absorbing composition, water or a mixture of water and a monohydric alcohol having 1 to 3 carbon atoms (hereinafter sometimes referred to as a lower alcohol) is preferred, and water is more preferred.

[0201] The water used as the aqueous medium is not particularly limited, and tap water can be used. Among them, distilled water, ion-exchanged water, pure water, etc. can be preferably used as the water from the viewpoint of less impurities.

[0202] As a mixture of water and a lower alcohol, the mixing ratio of water / lower alcohol can be 20 / 80 to 99 / 1 in terms of mass ratio.

[0203] The ultraviolet absorbing composition of the present invention may further include various components according to the purpose of use of the composition in addition to the specific ultraviolet absorber and the aqueous medium. Other components that may be included in the ultraviolet absorbing composition of the present invention include water-soluble polymers, colorants, viscosity modifiers other than water-soluble polymers, crosslinking agents, leveling agents, etc.

[0204] (Water-soluble polymer)

[0205] The ultraviolet absorbing composition of the present invention may contain a water-soluble polymer. By containing a water-soluble polymer, the viscosity of the composition can be adjusted according to the purpose. In addition, by selecting the water-soluble polymer used, film-forming properties can be imparted to the composition.

[0206] As the water-soluble polymer that can be used in the composition of the present invention, a polymer that is soluble in the above-mentioned aqueous medium is used.

[0207] The "water-soluble polymer" in the present invention refers to a polymer that dissolves 0.1% by mass or more in distilled water at 25° C. The water-soluble polymer dissolves preferably 1% by mass or more, more preferably 3.0% by mass or more, in distilled water at 25° C.

[0208] The water-soluble polymer is not particularly limited as long as it is water-soluble, and can be appropriately selected from known polymers depending on the purpose.

[0209] As the water-soluble polymer, for example, there can be mentioned acrylic polymers having an acidic group; polyvinyl ether / maleic anhydride polymers described in Japanese Patent Publication No. 46-2121, Japanese Patent Publication No. 56-40824, etc.; water-soluble salts of carboxyalkyl cellulose; water-soluble cellulose ethers; water-soluble salts of carboxyalkyl starch; polyvinyl alcohol; polyvinyl alcohol derivatives such as water-soluble polyvinyl butyral and water-soluble polyvinyl acetal; polyvinyl pyrrolidone; various polyacrylic amines; various water-soluble polyamides such as poly-2-acrylamide-2-methylpropane sulfonic acid; water-soluble salts of polyacrylic acid; gelatin; ethylene oxide polymers such as polyethylene oxide and polypropylene oxide; water-soluble salts of a group consisting of various starches and their analogs; polystyrene-4-sulfonate; copolymers of styrene / maleic acid; maleate resins, etc.

[0210] Among them, the water-soluble polymer is preferably an acrylic polymer having an acid group, polyvinyl alcohol and its derivatives, and more specifically, an acrylic polymer having an acid group, polyvinyl butyral, polyvinyl acetal, completely saponified polyvinyl alcohol or polyvinyl alcohol obtained by saponifying part of polyvinyl acetate.

[0211] The weight average molecular weight of the water-soluble polymer is preferably 1,000,000 or less, more preferably 1,000 to 1,000,000, and most preferably 2,000 to 100,000.

[0212] The weight average molecular weight of the water-soluble polymer can be measured by the following method, for example, by gel permeation chromatography (GPC) using an aqueous eluent (for example, tetrahydrofuran).

[0213] The weight average molecular weight of the water-soluble polymer in the present invention is measured as a polystyrene conversion value by gel permeation chromatography (GPC) under the following conditions. The calibration curve is prepared by 8 samples of "Standard Sample TSK Standard, Polystyrene" manufactured by Tosoh Corporation: "F-40", "F-20", "F-4", "F-1", "A-5000", "A-2500", "A-1000", and "n-propylbenzene".

[0214] <Conditions>

[0215] ·GPC: HLC (registered trademark)-8020GPC (manufactured by Tosoh Corporation)

[0216] Column: G3000HXL and G2000HXL

[0217] · Eluent: can be selected from THF (tetrahydrofuran), chloroform, NMP (N-methyl-2-pyrrolidone), m-cresol / chloroform (Shonan Wako Pure Chemical Industries Co., Ltd.). When the water-soluble polymer is dissolved in THF, THF is used as the eluent.

[0218] Sample concentration: 0.45 mass%

[0219] Flow rate: 1mL / min (ml / min)

[0220] Sample injection volume: 10 μL (microliter)

[0221] ·Measurement temperature: 23℃

[0222] Use a refractive index (RI) detector

[0223] When the composition of the present invention contains a water-soluble polymer, the content of the water-soluble polymer can be appropriately selected depending on the intended use of the composition.

[0224] When the composition of the present invention contains a water-soluble polymer, it may contain only one type of water-soluble polymer or may contain two or more types of water-soluble polymer.

[0225] For example, when adjusting the viscosity of the composition, it is sufficient to adjust at least one of the type and the addition amount of the aqueous medium and the water-soluble polymer in order to achieve the target viscosity.

[0226] Furthermore, for example, when an ultraviolet absorbing film is formed from the composition of the present invention, the water-soluble polymer is preferably contained in an amount of 0.1 to 50% by mass, more preferably 1 to 20% by mass, based on the total amount of the composition.

[0227] (Colorant)

[0228] The ultraviolet absorbing composition of the present invention can contain a colorant.

[0229] In the composition of the present invention, examples of the colorant that can be used together with the specific ultraviolet absorber include pigments and dyes.

[0230] As the pigment, preferably there can be mentioned inorganic pigments such as titanium oxide, zinc oxide, carbon black, aluminum powder, iron oxide (iron red), lead chromate, molybdenum orange, chrome yellow, yellow iron oxide, ochre, ultramarine blue, cobalt green, and the like, and organic pigments such as azo pigments, naphthol pigments, pyrazolone pigments, anthraquinone pigments, perylene pigments, quinacridone pigments, disazo pigments, isoindolinone pigments, benzimidazole pigments, phthalocyanine pigments, and quinophthalone pigments.

[0231] Preferred examples of the dye include anthraquinone-based, quinophthalone-based, methine-based, phthalocyanine-based, and perylene-based organic dyes.

[0232] When the composition of the present invention contains a colorant, it may contain only one type of colorant or may contain two or more types of colorants.

[0233] In addition, preferred coloring agents when the composition of the present invention is applied to a water-based coating material will be described in detail below.

[0234] The composition of the present invention contains a specific ultraviolet absorber having absorption at a wavelength of 380 nm to 400 nm and has excellent stability, and therefore can be used in various applications.

[0235] The composition of the present invention contains an aqueous medium and does not necessarily contain a volatile organic solvent, and therefore can be used as an ultraviolet-absorbing film-forming composition with little environmental load, an aqueous coating, a cosmetic for skin or hair, and the like.

[0236] Furthermore, by curing the composition of the present invention, an ultraviolet absorbing film described below can be obtained.

[0237] The composition of the present invention can also appropriately select and include known components according to the purpose in addition to comprising a specific ultraviolet light absorber, an aqueous medium and a preferred optional component, i.e., a water-soluble polymer and a colorant. As the optional component that the composition of the present invention can include except the water-soluble polymer and the colorant, the optional component that the water-based coating described later can include can also be cited.

[0238] (Water-based paint)

[0239] Hereinafter, a preferred embodiment when the composition of the present invention is applied to a water-based coating material will be described.

[0240] The composition of the present invention can be applied to water-based coatings.

[0241] The water-based paint preferably contains a specific ultraviolet absorber, an aqueous medium, a water-soluble polymer, and a colorant.

[0242] Colorants can be either dyes or pigments.

[0243] As the water-soluble polymer, it is preferable to use the water-soluble polymers described in the above-mentioned section of the composition of the present invention.

[0244] When the composition of the present invention is used as a water-based paint, it is preferred that a crosslinking agent is contained from the viewpoint of further improving the stability of the formed paint film.

[0245] As a crosslinking agent that can be used in water-based coatings, a metal alkoxide compound selected from Si, Ti, Zr and Al is preferred. The metal alkoxide used in water-based coatings is a hydrolyzable polymerizable compound having a functional group capable of hydrolysis and polycondensation in its structure and functioning as a crosslinking agent, and a strong crosslinked film having a crosslinked structure is formed by mutual polycondensation of the metal alkoxides, and is further chemically bonded to the above-mentioned hydrophilic polymer.

[0246] Examples of the metal alkoxide include compounds represented by the following general formula (VI-1) and general formula (VI-2).

[0247] (R 8 ) m -Z-(OR 9 ) 4-m (VI-1)

[0248] Al--(OR 9 )3 (VI-2)

[0249] In formula (VI-1) or (VI-2), R 8 represents a hydrogen atom, an alkyl group or an aryl group, R 9 represents an alkyl group or an aryl group, Z represents Si, Ti or Zr, and m represents an integer of 0 to 2.

[0250] R 8 and R 9 When each independently represents an alkyl group, the alkyl group preferably has 1 to 4 carbon atoms.

[0251] The alkyl group or aryl group may have a substituent, and examples of the substituent that can be introduced include a halogen atom, an amino group, a mercapto group, etc. The metal alkoxide compound that can be used as a crosslinking agent is preferably a low molecular weight compound having a molecular weight of 2,000 or less.

[0252] Specific examples of the hydrolyzable metal alkoxide compound represented by the general formula (VI-1) or (VI-2) are given below, but the present invention is not limited thereto.

[0253] In the general formula (VI-1), when Z is Si, that is, examples of the metal alkoxide compound as a crosslinking agent containing a silicon compound include trimethoxysilane, tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, γ-chloropropyltriethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane, etc. Among these, trimethoxysilane, tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, etc. are particularly preferred compounds.

[0254] When Z is Ti, that is, regarding the compound containing titanium as the metal alkoxide compound serving as the crosslinking agent, for example, trimethoxy titanate, tetramethoxy titanate, triethoxy titanate, tetraethoxy titanate, tetrapropoxy titanate, chlorotrimethoxy titanate, chlorotriethoxy titanate, ethyl trimethoxy titanate, methyl triethoxy titanate, ethyl triethoxy titanate, diethyl diethoxy titanate, phenyl trimethoxy titanate, phenyl triethoxy titanate, and the like can be cited.

[0255] When Z is Zr, that is, as for the compound containing zirconium in the metal alkoxide compound as the cross-linking agent, for example, zirconate esters corresponding to the compounds exemplified as the compound containing titanium can be cited.

[0256] Furthermore, when the metal alkoxide compound serving as a crosslinking agent is a compound represented by the general formula (VI-2) in which the central metal is Al, that is, the metal alkoxide compound serving as a crosslinking agent is a compound containing aluminum, for example, trimethoxyaluminate, triethoxyaluminate, tripropoxyaluminate, triisopropoxyaluminate, etc. can be cited.

[0257] When a metal alkoxide compound selected from Si, Ti, Zr, and Al is used as a crosslinking agent in a water-based coating, the content of the metal alkoxide compound is preferably 1% to 80% by mass, more preferably 5% to 70% by mass, relative to the total solid content of the water-based coating. In addition, "total solid content" refers to the total amount of components contained in the water-based coating except the solvent, and the case where a water-soluble polymer or the like is dissolved in the aqueous medium is also included in the solid content.

[0258] When the water-based coating material contains a cross-linking agent, it may contain only one type of cross-linking agent, or may contain two or more types.

[0259] The water-based paint may further contain particles.

[0260] The particles that can be contained in water-based paints are inorganic, organic, or particles composed of inorganic and organic substances, and are solid components having shapes such as spheres, plates, or rods.

[0261] The size of particles that can be used for the water-based paint is not particularly limited, but from the viewpoint of maintaining the film quality of the coating film formed using the water-based paint, the particle size is preferably in the range of 10 nm to 10 μm.

[0262] Regardless of the shape of the particle, such as a spherical particle, a flat particle, or a rod-shaped particle, the particle size of the particle in the present invention refers to the longest diameter in the projection diagram of the particle.

[0263] The average particle size of particles can be measured by observing the coating film of the water-based coating material at 50 to 100 times using an optical microscope, measuring the particle sizes of 20 particles in the viewing angle, and calculating the arithmetic average.

[0264] When the water-based paint contains particles, effects such as improving hydrophilicity, preventing cracks in the film formed by the water-based paint, and improving film strength can be expected.

[0265] Specifically, for example, particles include inorganic particles composed of inorganic pigments, silica, alumina, magnesium, titanium, calcium and other inorganic substances; organic particles composed of organic substances such as acrylic acid, styrene, vinyl acetate, butadiene, chloroprene, ethylene, vinyl chloride, alkylene oxide and the like; and composite particles having a coating layer composed of an organic substance on the surface of the inorganic particles.

[0266] When the aqueous coating material contains particles, it may contain only one type of particles or two or more types of particles.

[0267] Waterborne coatings may have a surfactant.

[0268] Examples of surfactants that can be used for water-based coatings include surfactants described in Japanese Patent Application Laid-Open Nos. 62-173463 and 62-183457.

[0269] Examples of the surfactant include anionic surfactants such as dialkyl sulfosuccinates, alkylnaphthalene sulfonates, and fatty acid salts; nonionic surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene alkyl allyl ethers, acetylene glycols, and polyoxyethylene / polypropylene chloride block copolymers; and cationic surfactants such as alkylamine salts and quaternary ammonium salts.

[0270] Furthermore, a fluorine compound such as an organic fluorine compound may be used as a surfactant or in place of the surfactant. The organic fluorine compound preferably has hydrophobicity.

[0271] As the organic fluorine compound in the present invention, for example, fluorine-based surfactants, oily fluorine-based compounds (e.g., fluorine oils) and solid fluorine compound resins (e.g., tetrafluoroethylene resins) are included. As the organic fluorine compound, more specifically, compounds described in the respective gazettes of Japanese Patent Publication No. 57-9053 (columns 8 to 17) and Japanese Patent Publication No. 62-135826 can be cited.

[0272] When the water-based coating material contains a surfactant, it may contain only one type of surfactant or may contain two or more types of surfactant.

[0273] Water-based paints may contain antioxidants.

[0274] When the water-based coating material contains an antioxidant, the stability of the composition as the water-based coating material is further improved.

[0275] Examples of the antioxidant include European Patent Application Publication No. 223739, European Patent Application Publication No. 309401, European Patent Application Publication No. 309402, European Patent Application Publication No. 310551, European Patent Application Publication No. 310552, European Patent Application Publication No. 459416, German Patent Application Publication No. 3435443, Japanese Patent Application Publication No. 54-262047, Antioxidants described in Japanese Patent Application No. 1994-1999, Japanese Patent Application No. 63-113536, Japanese Patent Application No. 63-163351, Japanese Patent Application No. 2-262654, Japanese Patent Application No. 2-71262, Japanese Patent Application No. 3-121449, Japanese Patent Application No. 5-61166, Japanese Patent Application No. 5-119449, U.S. Patent No. 4814262, U.S. Patent No. 4980275, etc.

[0276] When the water-based coating material contains an antioxidant, it may contain only one type of antioxidant or may contain two or more types.

[0277] The water-based paint may contain an organic solvent other than the water-based medium within a range that does not impair the effect.

[0278] By containing an organic solvent, when a coating film is formed from the composition, it can be expected that the uniformity of forming the coating film on the substrate will be further improved.

[0279] Examples of organic solvents other than aqueous media include ketone solvents such as acetone, methyl ethyl ketone, and diethyl ketone, chlorine solvents such as chloroform and dichloromethane, aromatic solvents such as benzene and toluene, ester solvents such as ethyl acetate, butyl acetate, and isopropyl acetate, ether solvents such as diethyl ether, and glycol ether solvents such as ethylene glycol monomethyl ether and ethylene glycol dimethyl ether.

[0280] The water-based coating material may contain other polymer compounds in addition to the above-mentioned water-soluble polymers in order to adjust the physical properties of the coating film within a range that does not impair the hydrophilicity.

[0281] As other polymer compounds, acrylic polymers that do not contain an acid group, polyurethane resins, polyamide resins, polyester resins, epoxy resins, phenolic resins, polycarbonate resins, polyvinyl formal resins, shellac, vinyl resins that do not contain an acid group, rubber resins, paraffins, other natural resins, etc. can be used.

[0282] When the water-based coating material contains other polymer compounds, it is preferred that the other polymer compounds contain an ethylene-based copolymer obtained by copolymerization of an acrylic monomer.

[0283] When the water-based coating material contains other polymer compounds, it may contain only one type of other polymer compounds, or may contain two or more types.

[0284] The water-based paint may contain a known colorant generally used in water-based paints in order to adjust the hue of the coating film of the water-based paint.

[0285] The colorant is not particularly limited and may be a dye or a pigment. Among them, pigments are preferred from the viewpoint of light resistance and durability.

[0286] Examples of pigments that can be used in water-based paints include inorganic pigments such as titanium oxide, zinc oxide, carbon black, aluminum powder, iron oxide (iron red), lead chromate, molybdenum orange, chrome yellow, yellow iron oxide, ochre, ultramarine blue, and cobalt green; and organic pigments such as azo pigments, naphthol pigments, pyrazolone pigments, anthraquinone pigments, perylene pigments, quinacridone pigments, disazo pigments, isoindolinone pigments, benzimidazole pigments, phthalocyanine pigments, and quinophthalone pigments.

[0287] The water-based paint may contain extender pigments such as heavy calcium carbonate, clay, kaolin, talc, precipitated barium sulfate, barium carbonate, white carbon, diatomaceous earth, etc. In particular, when a matte coating is formed on the surface of a substrate using a water-based paint, white carbon and diatomaceous earth are preferably used as extender pigments because they have the least detrimental effect on the non-fouling effect on the coating surface.

[0288] When the water-based paint contains inorganic particles such as extender pigments and inorganic pigments, the surface of the pigment can be treated with a coupling agent or a coupling agent can be added to the water-based paint in order to further improve the uniform dispersibility in the aqueous medium.

[0289] When the water-based paint contains a colorant, it may contain only one kind of colorant, or may contain two or more kinds of colorants depending on the purpose.

[0290] The content of pigment in water-based paint can be appropriately adjusted according to the purpose. From the viewpoints of the coloring of the formed coating (such as the concealment of the substrate) and the uniformity of the coating, the content of the pigment is preferably 0.1% by mass to 20% by mass relative to the total solid content of the water-based paint. From the viewpoint that the effect, hydrophilicity, and film strength of the pigment are better at the same time, the content of the pigment relative to the total solid content of the water-based paint is more preferably 1% by mass to 10% by mass.

[0291] The particle size of the pigment is not particularly limited, but is preferably 0.01 μm to 100 μm, more preferably 0.1 μm to 10 μm, from the viewpoint of film strength. The particle size of the pigment can be measured in the same manner as the particle size of the particles that can be contained in the above-mentioned water-based paint.

[0292] The water-based paint may contain other ultraviolet absorbers other than the specific ultraviolet absorber within a range that does not impair the effect. Hereinafter, ultraviolet absorbers other than the specific ultraviolet absorber may be referred to as other ultraviolet absorbers.

[0293] As other ultraviolet absorbers that can be contained in the water-based paint, for example, benzotriazole compounds described in Japanese Patent Laid-Open No. 58-185677, Japanese Patent Laid-Open No. 61-190537, Japanese Patent Laid-Open No. 2-782, Japanese Patent Laid-Open No. 5-197075, Japanese Patent Laid-Open No. 9-34057, etc., and diisocyanates described in Japanese Patent Laid-Open No. 46-2784, Japanese Patent Laid-Open No. 5-194483, U.S. Patent No. 3214463, etc. can be mentioned. Benzophenone compounds, cinnamic acid compounds described in Japanese Patent Publication No. 48-30492, Japanese Patent Publication No. 56-21141, Japanese Patent Application Publication No. 10-88106, etc., triazine compounds described in Japanese Patent Publication No. 4-298503, Japanese Patent Publication No. 8-53427, Japanese Patent Publication No. 8-239368, Japanese Patent Publication No. 10-182621, Japanese Patent Publication No. 8-501291, etc., compounds described in Research Disclosure No. 24239, compounds that absorb ultraviolet light and emit fluorescence, represented by stilbene and benzoxazole compounds, i.e., so-called fluorescent whitening agents, etc.

[0294] As the type of other ultraviolet absorbers that can be contained in the water-based coating material, benzotriazole compounds, benzophenone compounds, and benzoxazole compounds are preferred.

[0295] The content of other ultraviolet absorbers in the water-based coating of the present invention is not particularly limited. The content of other ultraviolet absorbers is preferably in the range of 10% to 100% by mass, more preferably in the range of 50% to 80% by mass, relative to the specific ultraviolet absorber.

[0296] When the water-based paint contains other ultraviolet absorbers other than the specific ultraviolet absorber, it may contain only one type of other ultraviolet absorbers, or may contain two or more types.

[0297] The water-based paint may further contain components that can be used for general paints in addition to the essential components and preferred optional components described above.

[0298] Examples of other components include aggregates, thickeners, film-forming aids, leveling agents, wetting agents, plasticizers, antifreeze agents, pH adjusters, preservatives, mildew inhibitors, algaecides, dispersants, defoamers, and rust inhibitors.

[0299] The composition of the present invention can be suitably used in various applications such as a composition for forming an ultraviolet-absorbing film, a water-based coating material, and a cosmetic for skin or hair.

[0300] [Ultraviolet absorption film]

[0301] The ultraviolet absorbing film of the present invention is a cured product of the above-mentioned ultraviolet absorbing composition.

[0302] The method for producing the ultraviolet absorbing film of the present invention is not particularly limited, and a known film-forming method can be applied.

[0303] Examples of the film-forming method include a method of molding the ultraviolet absorbing composition having an adjusted viscosity into a film by an extrusion method or the like and curing the molded film, a method of coating the ultraviolet absorbing composition on a substrate to form a film of the ultraviolet absorbing composition and curing the film, and a method of immersing a substrate in the ultraviolet absorbing composition to form a film of the ultraviolet absorbing composition and curing the film.

[0304] The curing of the film composed of the ultraviolet absorbing composition can be carried out by any of the following methods: reducing the solvent contained in the film of the ultraviolet absorbing composition by drying, applying energy such as light and heat to the film of the ultraviolet absorbing composition containing a crosslinking agent and forming a crosslinked structure in the film using the crosslinking agent, cooling the film of the ultraviolet absorbing composition containing gelatin as a water-soluble polymer and curing it by low temperature based on a sol-gel reaction, etc.

[0305] The thickness of the ultraviolet absorbing film can be appropriately selected depending on the purpose.

[0306] When the ultraviolet absorbing film is transparent, the thickness of the ultraviolet absorbing film can be 0.01 μm to 1000 μm, preferably 0.1 μm to 100 μm, from the viewpoint of being able to sufficiently absorb ultraviolet rays having a wavelength of 380 nm to 400 nm and having good transparency.

[0307] The thickness of the ultraviolet absorbing film is not limited to the above range. For example, when the ultraviolet absorbing film is formed from an ultraviolet absorbing composition containing a colorant such as an aqueous paint, the thickness may be appropriately adjusted in consideration of the concealing property of the substrate.

[0308] The ultraviolet absorbing film of the present invention can absorb ultraviolet rays with a wavelength of 380 nm to 400 nm, has low haze and good transparency, and can suppress the increase of haze caused by precipitation or aggregation of a specific ultraviolet absorber even after a period of time, and has good durability.

[0309] In the present invention, the haze is evaluated by observing the degree of turbidity of the ultraviolet absorbing film of the present invention, which is a cured product of the ultraviolet absorbing composition. Regarding the time-dependent increase in haze, the measured value of the initial haze of the ultraviolet absorbing film is compared with the measured value of the haze after time. When turbidity occurs or the degree of turbidity increases after time, and the measured value of the haze after time increases compared to the measured value of the initial haze, it is evaluated that the haze has increased over time.

[0310] The method for measuring the haze is as described above.

[0311] The haze of the ultraviolet absorbing film of the present invention is preferably 2% or less, and more preferably 1% or less, in a film thickness of 0.01 μm to 1000 μm.

[0312] The ultraviolet absorbing film of the present invention is a hydrophilic film and can therefore be used in various applications requiring hydrophilicity.

[0313] [Laminated body]

[0314] The laminated body of the present invention comprises a substrate and the above-mentioned ultraviolet absorbing film of the present invention formed on the substrate.

[0315] The substrate is not particularly limited, and any substrate that can form the ultraviolet absorbing film of the present invention can be used. Examples of the substrate include inorganic substrates such as glass plates, metal plates, and gypsum boards, and organic substrates such as resin plates.

[0316] The ultraviolet absorbing film of the present invention has good absorption at a wavelength of 380 nm to 400 nm and low haze, so it is also preferable to use a transparent substrate. In addition, in order to reduce the influence of ultraviolet rays on the substrate, it is also preferable to use an ultraviolet absorbing film. When an ultraviolet absorbing film is used to reduce the influence of ultraviolet rays, the substrate does not necessarily need to be a transparent substrate, and for example, any molded body can be used as the substrate.

[0317] When the ultraviolet absorbing film of the present invention is a coating film (cured product) of a water-based paint, the substrate (molded body) coated with the water-based paint becomes the substrate of the laminate of the present invention.

[0318] As the laminate, there can be mentioned a laminate having an ultraviolet absorbing film on the surface of a glass substrate. The laminate of the present invention having a glass substrate can be used for window glass of a house, window glass of a vehicle such as an automobile, front window glass, etc. In addition, it can also be set as a laminate having an ultraviolet absorbing film between two glass plates. For example, by having an ultraviolet absorbing film between two sheets of laminated glass, the durability of the ultraviolet absorbing film is further improved.

[0319] Furthermore, by providing an ultraviolet absorbing film which is a cured product of a coating film of a water-based paint on the surface of various molded bodies, the laminate of the present invention has an arbitrary hue based on the water-based paint, has a coating film with excellent ultraviolet shielding properties, and becomes a laminate that takes into account both surface decoration and shielding of ultraviolet rays on the long wavelength side of 380nm to 400nm.

[0320] Example

[0321] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to the following Examples unless it exceeds the gist of the present invention.

[0322] In addition, unless otherwise specified, "%" and "part" in the following examples are based on mass.

[0323] The structure of the specific ultraviolet absorber obtained by synthesis was confirmed by NMR.

[0324] The maximum absorption wavelength and the solubility in distilled water (25° C.) were measured by the above method.

[0325] The molar absorption coefficient was determined by the following method.

[0326] After dissolving 1.0 mg of the sample in 100 mL of pure water, the absorbance of the aqueous solution was measured using a 1 cm colorimetric cell using a SHIMADZUCORPORATION spectrophotometer (model: UV 3150). From the measurement results, the molar absorptivity was calculated using the Beer-Lambert law based on the absorbance value at the maximum absorption wavelength.

[0327] [Synthesis of Compound M-3]

[0328] Compound M-3 as a specific ultraviolet absorber was synthesized according to the following scheme. In addition, raw material M-3A was synthesized by a method described in the literature (Chem. Crystallography, 1997, Vol. 27, pp. 515-526). Compound M-3 is the above-mentioned exemplary compound M-3.

[0329] [Chemical formula 13]

[0330]

[0331] Specifically, 2.5 g of raw material M-3A, 0.81 g of sodium hydroxide (manufactured by Tokyo Chemical Industry Co., Ltd.), and 3.0 g of 1,4-butane sultone (manufactured by Tokyo Chemical Industry Co., Ltd.) were dissolved in 50 mL of ethanol, and then refluxed with stirring for 2 hours. The reaction solution was cooled to 25° C., and the precipitated crystals were filtered out.

[0332] The filtered crystals were washed with methanol cooled to 0°C and dried at room temperature to obtain 2.6 g of the target compound M-3 as a white powder.

[0333] [Chemical formula 14]

[0334]

[0335] The analysis results of the obtained compound M-3 are as follows.

[0336] 1 H-NMR (DMSO-d6) δ1.6-1.9 (m, 8H), 2.3-2.5 (m, 4H), 4.0-4.2 (m, 4H), 7.2 (s, 2H)

[0337] Maximum absorption wavelength: 372nm (H2O)

[0338] Molar Absorption Coefficient: 28,100

[0339] Solubility in distilled water (25°C): 3.1% by mass

[0340] [Synthesis of Compound M-11]

[0341] Compound M-11 as a specific ultraviolet absorber was synthesized according to the following scheme. In addition, raw material M-11A was synthesized by the method described in Example 1 of International Publication No. 2019 / 065043. Compound M-11 is an exemplary compound M-11.

[0342] [Chemical formula 15]

[0343]

[0344] Specifically, 3.9 g of the raw material M-11A, 0.81 g of sodium hydroxide (manufactured by Tokyo Chemical Industry Co., Ltd.), and 3.0 g of 1,4-butane sultone (manufactured by Tokyo Chemical Industry Co., Ltd.) were dissolved in 50 mL of ethanol, and then stirred under reflux for 2 hours. The reaction solution was cooled to 25° C., and the precipitated crystals were filtered out. The filtered crystals were washed with methanol cooled to 0° C. and dried at room temperature, thereby obtaining 5.6 g of the target compound M-11 as a white powder.

[0345] [Chemical formula 16]

[0346]

[0347] The analysis results of the obtained compound M-11 are as follows.

[0348] 1 H-NMR (DMSO-d6) δ0.86 (t, 6H), 1.2-1.4 (m, 8H), 1.5-1.6 (m, 4H), 1.8-1.9 (m, 4H), 2.3-2.5 (m, 4H), 3.6-3.8 (m, 4H), 4.0-4.2 (m, 4H), 7.2 (s, 2H)

[0349] Maximum absorption wavelength: 387nm (H2O)

[0350] Molar Absorption Coefficient: 35,900

[0351] Solubility in distilled water (25°C): 3.4% by mass

[0352] [Synthesis of Compound M-5]

[0353] Compound M-5 as a specific ultraviolet absorber was synthesized according to the following scheme.

[0354] 3.0 g of raw material M-3A, 1.0 g of sodium hydroxide (Tokyo Chemical Industry Co., Ltd.) and 3.5 g of 1,4-butane sultone (Tokyo Chemical Industry Co., Ltd.) were dissolved in 50 mL of methanol, and then stirred under reflux for 2 hours. The reaction solution was cooled to 25°C and the precipitated crystals were filtered out. The filtered crystals were washed with methanol cooled to 0°C and dried at room temperature to obtain 3.6 g of the target compound M-5 as a white powder. Compound M-5 is an exemplary compound M-5.

[0355] [Chemical formula 17]

[0356]

[0357] The analysis results of the obtained compound M-5 are as follows.

[0358] 1 H-NMR (DMSO-d6) δ1.6-1.9 (m, 8H), 2.3-2.5 (m, 4H), 3.7 (s, 3H), 4.0-4.3 (m, 4H), 7.15 (s, 2H), 8.0 (s, 1H)

[0359] Maximum absorption wavelength: 390nm (H2O)

[0360] Molar Absorption Coefficient: 27,400

[0361] Solubility in distilled water (25°C): 3.1% by mass

[0362] [Synthesis of Compound M-18]

[0363] 3.0 g of raw material M-3A, 1.0 g of triethylamine (Tokyo Chemical Industry Co., Ltd.), and 2.5 g of succinic anhydride (Tokyo Chemical Industry Co., Ltd.) were dissolved in 50 mL of acetonitrile, and then refluxed and stirred for 2 hours. The reaction solution was cooled to 25°C, and 1 mL of acetic acid was added. The precipitated crystals were filtered out. The filtered crystals were washed with methanol cooled to 0°C and dried at room temperature to obtain 3.2 g of the target compound M-18 as a white powder. Compound M-18 is an exemplary compound M-18.

[0364] [Chemical formula 18]

[0365]

[0366] The analysis results of the obtained compound M-18 are as follows.

[0367] 1 H-NMR (DMSO-d6) δ2.1-2.4 (m, 8H), 7.20 (s, 2H), 10.5 (b, 2H)

[0368] Maximum absorption wavelength: 385nm (H2O)

[0369] Solubility in distilled water (25°C): 2.8% by mass

[0370] <Example 1>

[0371] 5.0 parts by mass of compound M-3, 45.0 parts by mass of polyvinyl alcohol (PVA) and 500 parts by mass of water were mixed and stirred at 40°C for 1 hour to completely dissolve the mixture, thereby obtaining the ultraviolet absorbing composition of Example 1. After cooling to room temperature, the obtained composition was applied to a glass plate (size: 76 mm × 52 mm × 1 mm, product name; S9111, manufactured by Matsunami Glass Ind., Ltd.) by dip coating to form a coating film, and dried on a hot plate at 100°C for 20 seconds to form an ultraviolet cured film as a cured product of the ultraviolet absorbing composition. The coating amount of one dip coating was 0.3 g / cm 2 (The film thickness after drying is 300 μm).

[0372] Dipping and drying were repeated five times to obtain a laminate having an ultraviolet absorbing film with a thickness of 1.5 mm on a glass plate, i.e., a substrate.

[0373] The thickness of the laminate was 2.5 mm.

[0374] [Performance evaluation]

[0375] The transmittance, haze (initial haze), light resistance, moisture and heat resistance, and haze after the moisture and heat resistance test of the obtained laminate were evaluated by the following methods.

[0376] 1. Transmittance

[0377] The laminate of the obtained glass plate and the ultraviolet absorbing film was used as a measurement object, and the transmittance of the ultraviolet absorbing film containing a specific ultraviolet absorber at 380 nm was measured using a UV / vis spectrometer (UV / vis spectrometer UV3400 manufactured by SHIMADZU CORPORATION).

[0378] The haze of the glass plate as the substrate measured with a haze meter was 0.20%, and the ultraviolet absorption rate of the glass plate at 380 nm was 1% or less. Therefore, the transmittance was evaluated based on the result of measuring the laminate as the transmittance of the ultraviolet absorbing film of the present invention.

[0379] 2. Haze (initial haze)

[0380] The haze of the laminate of the obtained glass plate and the ultraviolet absorbing film was measured using a haze meter (NDH4000 manufactured by NIPPON DENSHOKU INDUSTRIES Co., Ltd.) The haze of the ultraviolet absorbing film listed in Table 1 below is a measured value corrected based on the haze (0.20%) of the glass plate itself.

[0381] 3.Lightfastness

[0382] First, the transmittance of the laminate of the obtained glass plate and the ultraviolet absorbing film at a wavelength of 380 nm was measured using a spectrophotometer (model: UV 3150) manufactured by SHIMADZU CORPORATION.

[0383] Next, the ultra-accelerated weathering tester (product name: EYE SUPER UV TESTER, IWASAKIELECTRIC CO., LTD.) was used to test the 2 (Exposure energy: 90mJ / cm 2 ), temperature 63°C, relative humidity 50%, the obtained laminate of the glass plate and the ultraviolet absorbing film was irradiated with light from a metal halide lamp (cutoff below about 290nm) for 60 hours.

[0384] After the light irradiation, the transmittance of the laminate of the obtained glass plate and the ultraviolet absorbing film at a wavelength of 380 nm was measured by a spectrophotometer (model: UV 3150) manufactured by SHIMADZU CORPORATION in the same manner as described above.

[0385] The change in transmittance at a wavelength of 380 nm before and after light irradiation was calculated, and a change of less than 5% was evaluated as "particularly good" light resistance, a change of 5% or more and less than 10% was evaluated as "good" light resistance, and a change of 10% or more was evaluated as "poor" light resistance.

[0386] 4. Resistance to moisture and heat

[0387] The wet heat test was conducted at 60°C and 90%RH using a constant temperature and humidity device (IG420 manufactured by Yamato Scientific Co., Ltd.). The transmittance at 380nm after 160 hours was measured by the above method. The change in transmittance at a wavelength of 380nm before and after the wet heat durability test was calculated, and the case where the change was less than 5% was evaluated as "particularly good" wet heat resistance, the case where the change was more than 5% and less than 10% was evaluated as "good" wet heat resistance, and the case where the change was more than 10% was evaluated as "poor" wet heat resistance.

[0388] The haze after the moist heat resistance test was measured in the same manner as in the above (2. Initial haze).

[0389] 5. Yellowing

[0390] The laminate of the produced glass plate and the ultraviolet absorbing film was placed on a white paper, and one evaluator visually observed the laminate on the paper and evaluated whether the laminate was yellowed.

[0391] [Example 2 to Example 5]

[0392] In Example 1, except that the type of the specific ultraviolet absorber (Compound M-3) was changed to the type shown in the following Table 1, the same method as in Example 1 was carried out to obtain ultraviolet absorbing compositions of Examples 2 to 5.

[0393] The obtained ultraviolet absorbing composition was used to perform the same evaluation as in Example 1. The results are shown in Table 1 below.

[0394] [Comparative Example 1 to Comparative Example 5]

[0395] In Example 1, except that the type of the specific ultraviolet absorber (Compound M-3) was changed to the comparative ultraviolet absorbers (Comparative Compound H-1) to the comparative ultraviolet absorbers (Comparative Compound H-5) shown in Table 1 below, the ultraviolet absorbing compositions of Comparative Examples 1 to Comparative Examples 5 were obtained in the same manner as in Example 1.

[0396] Using the obtained composition, the same evaluation as in Example 1 was performed. The results are shown in Table 1 below.

[0397] The structures of the comparative ultraviolet absorbers (Comparative Compound H-1) to (Comparative Compound H-5) used in the comparative examples are shown below.

[0398] [Chemical formula 19]

[0399]

[0400] [Chemical formula 20]

[0401]

[0402] [Chemical formula 21]

[0403]

[0404] [Example 6]

[0405] 2.0 parts by mass of compound M-3, 98.0 parts by mass of polyvinyl alcohol and 1000 parts by mass of water were mixed and stirred at 40°C for 1 hour to completely dissolve the mixture and obtain a UV absorbing composition. After the composition was cooled to room temperature (25°C), a coating film was formed on a glass plate by spin coating (1000 rpm (revolutions / minute), 10 seconds), and the film was dried on a hot plate at 100°C for 20 seconds to form a cured product of the UV absorbing composition of Example 6, i.e., a UV absorbing film.

[0406] [Example 7 to Example 9]

[0407] In Example 6, except that the type of the specific ultraviolet absorber (Compound M-3) was changed to the type shown in the following Table 1, the same method as in Example 1 was carried out to obtain ultraviolet absorbing compositions of Examples 7 to 9.

[0408] The obtained ultraviolet absorbing composition was used to perform the same evaluation as in Example 1. The results are shown in Table 1 below.

[0409] [Table 1]

[0410]

[0411] According to the results described in Table 1, the laminated bodies of Examples 1 to 5, which are ultraviolet absorbing films that are cured products of ultraviolet absorbing compositions containing the specific ultraviolet absorbers of the present invention, all have excellent ultraviolet blocking properties at 380 nm, low initial haze, and good light resistance and moisture and heat resistance. In addition, not only is the initial haze good, but no significant increase in haze is observed after the moisture and heat resistance test, and all hazes are at a level that does not cause problems in practical use.

[0412] In addition, in the laminates of Examples 6 to 9, in which the content of the specific ultraviolet absorber is lower, the ultraviolet shielding property is slightly lower than that of Examples 1 to 5, but the ultraviolet blocking property of 380 nm is not problematic in practical applications. In addition, the initial haze is low, and the light resistance and moisture and heat resistance are good. In addition, no significant increase in the haze after the moisture and heat resistance test was found, and all the hazes were at a level that is not problematic in practical applications.

[0413] On the other hand, Comparative Examples 1 to 3 and Comparative Example 5, which used comparative ultraviolet absorbers instead of the specific ultraviolet absorbers, had poor ultraviolet blocking properties at 380 nm. The laminate of Comparative Example 4, which contained a comparative ultraviolet absorber (H-4) having two benzothiocyclopentane skeletons in the molecule, had good initial haze, but after the wet heat resistance test, the haze increased significantly due to crystallization of the ultraviolet absorber.

[0414] The invention of Japanese Patent Application No. 2019-122032 filed on June 28, 2019 is incorporated herein by reference.

[0415] All documents, patent applications, and technical standards described in the present invention are incorporated herein by reference to the same extent as if each individual document, patent application, or technical standard was specifically and individually indicated to be incorporated by reference.

Claims

1. A UV absorber represented by the following general formula (2): In the general formula (2), R 1 and R 2 Each independently represents an alkyl group having a sulfonic acid group, wherein the sulfonic acid group is optionally in the form of a salt, 1 and W 2 Each independently represents a cyano group, a carbamoyl group, a nitro group, an alkoxycarbonyl group, an aryloxycarbonyl group or -CH(=NOCH3).

2. A UV absorber represented by the following general formula (3): In the general formula (3), R 1 and R 2 Each independently represents an alkyl group having a sulfonic acid group, wherein the sulfonic acid group is optionally in the form of a salt, R 3 It represents an alkyl group. 3 . The ultraviolet absorber according to claim 1 , which has a solubility in water at 25° C. of 1% by mass or more.

4. An ultraviolet absorbing composition comprising the ultraviolet absorber according to claim 1 or 2 and an aqueous medium. The ultraviolet absorbing composition according to claim 4 , further comprising a water-soluble polymer. 6 . An ultraviolet absorbing film, which is a cured product of the ultraviolet absorbing composition according to claim 4 or 5 . 7 . A laminate comprising a substrate and the ultraviolet absorbing film according to claim 6 formed on the substrate.

8. A compound represented by the following general formula (4): In the general formula (4), L 1 and L 2 Each independently represents an alkylene group, X each independently represents a hydrogen atom or -SO3 - The counter cation, W 1 and W 2 Each independently represents a cyano group, a carbamoyl group, a nitro group, an alkoxycarbonyl group, an aryloxycarbonyl group or -CH(=NOCH3).