Method for producing hydrocarbon resin hydride

By using hindered phenolic antioxidants and 2,2,6,6-tetraalkyl-4-piperidinyl antioxidants in combination with hydrogenation catalysts during the hydrogenation process of hydrocarbon resins, the hydrogenation reaction conditions are controlled and the problem of hydrogenation of hydrocarbon resins is solved. The problem of changes in molecular weight and softening point caused by the reaction enables optimization of color tone and odor properties.

CN113993908BActive Publication Date: 2024-10-01ZEON CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202080044066.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-04
Filing Date
2020-06-22
Publication Date
2024-10-01
Estimated Expiration
2040-06-22

AI Technical Summary

Technical Problem

It is difficult to optimize the color tone and reduce odor at the same time while suppressing changes in molecular weight and softening point caused by the hydrogenation reaction of hydrocarbon resins.

Method used

In the presence of a hindered phenolic antioxidant and an antioxidant with a 2,2,6,6-tetraalkyl-4-piperidinyl group, a hydrogenation catalyst is used to contact the hydrocarbon resin with hydrogen for hydrogenation reaction, and the hydrogenation conditions are controlled as follows Temperature, pressure and catalyst selection to suppress changes in molecular weight and softening point.

Benefits of technology

It is possible to significantly optimize the color tone and reduce odor while suppressing the changes in molecular weight and softening point caused by the hydrogenation reaction of the hydrocarbon resin. The obtained hydrocarbon resin hydrogenated product has excellent color tone and low odor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003412655850000041
    Figure BDA0003412655850000041
  • Figure BDA0003412655850000211
    Figure BDA0003412655850000211
  • Figure BDA0003412655850000251
    Figure BDA0003412655850000251
Patent Text Reader

Abstract

The present invention provides a method for producing a hydrocarbon resin hydrogenate, wherein a hydrocarbon resin is brought into contact with hydrogen in the presence of at least one antioxidant compound selected from a hindered phenol antioxidant and an antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group, and a hydrogenation catalyst, thereby conducting a hydrogenation reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a hydrogenated hydrocarbon resin, which can produce a hydrogenated hydrocarbon resin having excellent color tone and low odor properties while suppressing changes in molecular weight and softening point due to a hydrogenation reaction of the hydrocarbon resin. Background Art

[0002] Hydrocarbon resins having carbon-carbon double bonds, such as hydrocarbon resins obtained by copolymerizing monoethylenically unsaturated hydrocarbons and chain-like conjugated dienes, are known. Such hydrocarbon resins are useful, for example, as tackifier resins for forming hot melt adhesives.

[0003] On the other hand, in recent years, in hot melt adhesives, attempts have been made to use hydrogenated hydrocarbon resins as tackifier resins from the viewpoint of improving color tone, etc. For example, Patent Documents 1 and 2 disclose the following technology: by hydrogenating the color body of the hydrocarbon resin, the color of the hydrocarbon resin can be lightened while suppressing changes in physical properties such as molecular weight and softening point.

[0004] In the techniques of Patent Documents 1 and 2, only the color body that is easily hydrogenated is selectively hydrogenated, and the carbon-carbon double bonds present in the skeleton of the hydrocarbon resin are not hydrogenated. There are a large number of carbon-carbon double bonds in the hydrocarbon resin, and although the color tone can be improved to a certain extent according to the techniques of Patent Documents 1 and 2, a technique that can further suppress changes in physical properties such as molecular weight and softening point is required.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent No. 3971468;

[0008] Patent document 2: Japanese Patent No. 3987587. Summary of the invention

[0009] Problem that the invention aims to solve

[0010] The present invention has been made in view of such actual circumstances, and an object of the present invention is to provide a method for producing a hydrogenated hydrocarbon resin which can produce a hydrogenated hydrocarbon resin having excellent color tone and low odor properties while suppressing changes in molecular weight and softening point due to hydrogenation reaction of the hydrocarbon resin.

[0011] Solutions for solving problems

[0012] The present inventors have conducted studies to achieve the above-mentioned object and have found that by contacting a hydrocarbon resin with hydrogen in the presence of at least one antioxidant compound selected from hindered phenol antioxidants and antioxidants having a 2,2,6,6-tetraalkyl-4-piperidinyl group and a hydrogenation catalyst, a hydrocarbon resin hydrogenated product having excellent color tone and low odor properties can be produced while suppressing changes in molecular weight and softening point due to the hydrogenation reaction of the hydrocarbon resin. The present invention has been completed.

[0013] That is, according to the present invention, there is provided a method for producing a hydrocarbon resin hydrogenate, the method comprising contacting a hydrocarbon resin with hydrogen in the presence of at least one antioxidant compound selected from hindered phenol antioxidants and antioxidants having a 2,2,6,6-tetraalkyl-4-piperidinyl group, and a hydrogenation catalyst, thereby conducting a hydrogenation reaction.

[0014] In the production method of the present invention, the antioxidant compound is preferably present in an amount of 0.01 to 10 parts by mass based on 100 parts by mass of the hydrocarbon resin.

[0015] In the production method of the present invention, it is preferred that the hydrocarbon resin is obtained by stripping a polymer solution containing a hydrocarbon resin obtained by cation polymerization using a Lewis acid catalyst.

[0016] In the production method of the present invention, it is preferred that the hydrocarbon resin is heated to 150 to 350° C. and has a melt viscosity in the range of 50 to 1500 mPa·s, and then brought into contact with hydrogen to carry out a hydrogenation reaction.

[0017] In the production method of the present invention, the hydrogen pressure during the hydrogenation reaction is preferably in the range of 0.5 to 3.0 MPa.

[0018] In the production method of the present invention, it is preferred to use a fixed bed reactor to bring the hydrocarbon resin into contact with hydrogen to carry out the hydrogenation reaction.

[0019] In the production method of the present invention, it is preferred to use a granular hydrogenation catalyst having an average diameter of 1 to 5 mmφ and an average length of 1 to 10 mm as the hydrogenation catalyst.

[0020] In the production method of the present invention, the hydrogenation catalyst is preferably a nickel catalyst.

[0021] In the production method of the present invention, it is preferred that the nickel catalyst is a catalyst containing, as a main component, a compound in which nickel is supported on magnesium oxide-silicon dioxide.

[0022] Effects of the Invention

[0023] According to the present invention, there can be provided a method for producing a hydrogenated hydrocarbon resin which can produce a hydrogenated hydrocarbon resin having excellent color tone and low odor properties while suppressing changes in molecular weight and softening point due to hydrogenation reaction of the hydrocarbon resin. DETAILED DESCRIPTION

[0024] In the method for producing a hydrocarbon resin hydrogenate of the present invention, a hydrocarbon resin is contacted with hydrogen in the presence of at least one antioxidant compound selected from hindered phenol antioxidants and antioxidants having a 2,2,6,6-tetraalkyl-4-piperidinyl group and a hydrogenation catalyst to carry out a hydrogenation reaction.

[0025] <Antioxidant Compounds>

[0026] The antioxidant compound used in the present invention can be selected from at least one of a hindered phenol antioxidant and an antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group. Only one of the hindered phenol antioxidant and the antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group can be used, or they can be used in combination. The amount of the antioxidant compound is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, further preferably 0.05 to 2 parts by mass, and most preferably 0.05 to 0.5 parts by mass relative to 100 parts by mass of the hydrocarbon resin. By making the amount of the antioxidant compound present in the above range, the changes in molecular weight and softening point caused by the hydrogenation reaction can be further suppressed. When a hindered phenol antioxidant and an antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group are used in combination, the ratio of these antioxidant compounds to each other is preferably 10:90 to 90:10 in terms of the weight ratio of "hindered phenol antioxidant: antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group".

[0027] <Hindered phenol antioxidants>

[0028] The hindered phenol antioxidant is preferably an antioxidant having at least one hindered group at the 2nd or 6th position of the hydroxyl group. Here, the hindered group refers to a sterically hindered substituent, which is a substituent having 3 or more carbon atoms. Preferred examples include tertiary hydrocarbon groups such as tert-butyl groups. On the other hand, as non-hindered groups, in addition to hydrogen atoms, examples include straight-chain hydrocarbon groups having 2 or less carbon atoms such as methyl and ethyl groups.

[0029] The hindered phenol antioxidant is not particularly limited, and examples thereof include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2,6-di-tert-butyl-p-cresol, di-tert-butyl-4-methylphenol, and the like. Among these, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and 2,6-di-tert-butyl-p-cresol are preferred, and pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate is particularly preferred. The hindered phenol antioxidant may be used alone or in combination of two or more.

[0030] <Antioxidant having 2,2,6,6-tetraalkyl-4-piperidinyl group>

[0031] The 2,2,6,6-tetraalkyl-4-piperidinyl group of the antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group is a group represented by the following general formula.

[0032] [Chemical formula 1]

[0033]

[0034] In the formula, R1 to R4 are any alkyl groups, preferably alkyl groups having 1 to 4 carbon atoms. R5 is hydrogen or an alkyl group or alkoxy group having 1 to 8 carbon atoms which may have a substituent. * represents a binding site. R1 to R4 may be the same or different from each other, and specific examples thereof include methyl, ethyl, propyl, butyl, hexyl, octyl, etc., preferably methyl, ethyl, propyl, butyl. Specific examples of R5 include hydrogen, methyl, octyl, etc., preferably hydrogen.

[0035] The antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group may be a commercially available product. Specific examples of commercially available antioxidants having a 2,2,6,6-tetraalkyl-4-piperidinyl group include poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidinyl)imino}] (trade name "Chimassorb (registered trademark) 944"), N,N'-bis(3-aminopropyl)ethylenediamine-2,4- Bis[N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidinyl)amino]-6-chloro-1,3,5-triazine condensate (trade name "Chimassorb (registered trademark) 119"), and poly[{(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidinyl)imino}] (trade name "Chimassorb (registered trademark) 2020"), etc. (all manufactured by BASF JAPAN). Among the above, poly[{(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidinyl)imino}] (trade name "Chimassorb (registered trademark) 2020") is particularly preferred. The antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group may be used alone or in combination of two or more.

[0036] <Hydrogenation Catalyst>

[0037] As the hydrogenation catalyst used in the present invention, it is not particularly limited, and a nickel catalyst is preferably used. In particular, from the viewpoint of high reactivity, it is preferably used as a catalyst containing a compound in which nickel as a metal is supported on a supported inorganic compound as a carrier as a main component. As a specific example of the supported inorganic compound of the carrier, it is possible to enumerate: silicon dioxide, aluminum oxide, boron oxide, silicon dioxide-alumina, diatomaceous earth, clay, magnesium oxide, magnesium oxide-silicon dioxide (silicon dioxide-magnesium oxide), titanium dioxide, zirconium oxide, etc. Among these, from the viewpoint of reactivity, magnesium oxide-silicon dioxide is preferably used.

[0038] The shape of the hydrogenation catalyst is not particularly limited. From the viewpoint of reactivity, a granular shape is preferred. Hydrogenation catalysts in various shapes such as granular, spherical, and cylindrical shapes can be used. From the viewpoint of further improving reactivity, the average diameter is preferably 1 to 5 mmφ, more preferably 1 to 4 mmφ, and further preferably 1 to 3 mmφ. In addition, the average length is preferably 1 to 10 mm, more preferably 1 to 8 mm, and further preferably 1 to 4 mm.

[0039] <Hydrogenation reaction>

[0040] In the present invention, a hydrocarbon resin is brought into contact with hydrogen in the presence of at least one antioxidant compound selected from hindered phenol antioxidants and antioxidants having a 2,2,6,6-tetraalkyl-4-piperidinyl group, and a hydrogenation catalyst, thereby conducting a hydrogenation reaction. In the production method of the present invention, a hydrocarbon resin hydrogenate having excellent color tone and low odor can be produced by hydrogenating the hydrocarbon resin, and by conducting the hydrogenation reaction in the presence of the above-mentioned antioxidant compound, changes in molecular weight and softening point caused by the hydrogenation reaction of the hydrocarbon resin can be suppressed. Furthermore, according to the production method of the present invention, a hydrocarbon resin hydrogenate having a small Gardner color scale value and excellent heat resistance can be produced even when heated at 200°C for 3 hours.

[0041] The state of the hydrocarbon resin during the hydrogenation reaction is not particularly limited, and may be in a state of being dissolved in an organic solvent, in a solid state, or in a molten state.

[0042] The organic solvent for dissolving the hydrocarbon resin is not particularly limited as long as it is an organic solvent inactive to the hydrogenation catalyst. From the viewpoint of solubility, a hydrocarbon solvent can be preferably used. Examples of the hydrocarbon solvent include aromatic hydrocarbons such as benzene and toluene; aliphatic hydrocarbons such as n-pentane and hexane; alicyclic hydrocarbons such as cyclohexane and decalin. Among these, cyclic aromatic hydrocarbons and alicyclic hydrocarbons are preferred. These organic solvents can be used alone or in combination of two or more.

[0043] The method for contacting the hydrocarbon resin with hydrogen in the presence of the above-mentioned antioxidant compound and the hydrogenation catalyst is not particularly limited, and examples thereof include: a batch treatment method in which the hydrocarbon resin, the above-mentioned antioxidant compound and the hydrogenation catalyst are coexisted in an appropriately selected container and stirred as needed to contact the hydrocarbon resin with hydrogen; and a continuous treatment method in which the hydrocarbon resin is contacted with hydrogen while the hydrocarbon resin and the above-mentioned antioxidant compound are circulated in a fixed bed reactor in which the hydrogenation catalyst is fixed.

[0044] In the production method of the present invention, from the viewpoint of being able to obtain a hydrocarbon resin hydrogenate having a target hydrogenation rate more stably and more efficiently, it is preferred to adopt a method in which the hydrocarbon resin is directly contacted with hydrogen in a solid or molten state. In particular, it is more preferred to adopt the above-mentioned continuous treatment method, that is, the hydrocarbon resin is contacted with hydrogen while circulating the hydrocarbon resin in a solid or molten state in a fixed bed reactor in which a hydrogenation catalyst is fixed. In addition, the hydrocarbon resin in a solid or molten state is preferably in a state that does not substantially contain a volatile solvent.

[0045] As a fixed bed reactor, there is no particular limitation, and from the viewpoint of reaction efficiency, a multi-tubular heat exchange type hydrogenation reaction device can be preferably used. A multi-tubular heat exchange type hydrogenation reaction device is a device that has a plurality of reaction tubes filled with a hydrogenation catalyst, heats the outside of the reaction tube by a heating medium, and circulates hydrogen and a polymer as a hydrogenation object in the reaction tube, thereby being able to continuously carry out a hydrogenation reaction. For example, devices disclosed in Japanese Patent Laid-Open No. 5-276269, Japanese Patent Laid-Open No. 63-141638, Japanese Patent Laid-Open No. 2-56238, etc. can be used. In addition, the inner diameter of the reaction tube of the multi-tubular heat exchange type hydrogenation reaction device is preferably 6 to 100 mm, more preferably 10 to 70 mm, and the length of the reaction tube is preferably 0.1 to 10 m, more preferably 0.3 to 7 m.

[0046] In the production method of the present invention, it is particularly preferred to carry out the hydrogenation reaction under the following conditions: the hydrocarbon resin is heated to preferably 150 to 350°C, more preferably 150 to 300°C, further preferably 160 to 275°C, and particularly preferably 170 to 250°C, and the melt viscosity is controlled in the range of preferably 50 to 1500 mPa·s, more preferably 50 to 1000 mPa·s, further preferably 75 to 800 mPa·s, and particularly preferably 100 to 600 mPa·s.

[0047] By adjusting the temperature and melt viscosity of the hydrocarbon resin during the hydrogenation reaction within the above range, when the hydrogenation reaction is performed using a fixed bed reactor, for example, even when the number of times of passing through the fixed bed reactor is set to one (for example, when the residence time in the fixed bed reactor is preferably set to 0.15 to 1.8 hours, more preferably 0.2 to 1.5 hours), a hydrocarbon resin hydrogenated product having a target hydrogenation rate can be appropriately obtained. Furthermore, by appropriately adjusting the temperature and melt viscosity of the hydrocarbon resin within the above range, the wetting of the catalyst by the hydrocarbon resin required for the hydrogenation reaction and the controllability of the solubility of the added hydrogen in the hydrocarbon resin can be improved, and the target hydrogenation rate can be adjusted. Therefore, even when the number of times of passing through the fixed bed reactor is set to one, a hydrocarbon resin hydrogenated product having a target hydrogenation rate can be stably and more efficiently obtained. Moreover, as a result, a hydrocarbon resin hydrogenated product having an excellent color tone and low odor can be appropriately obtained. In addition, in the present invention, from the perspective of productivity, it is preferred to set the number of circulations to 1. If the total residence time in the fixed bed reactor can be almost equal to the case where the number of circulations is 1, then under such conditions, it is also preferred to set the number of circulations to multiple times (that is, it is also preferred that the number of circulations is multiple times and the total residence time is 0.3 to 1.8 hours). In this case, the same effect as above can be obtained.

[0048] Furthermore, in the production method of the present invention, since the hydrocarbon resin is hydrogenated in the presence of the above-mentioned antioxidant compound, as described above, even when the hydrocarbon resin is heated to a high temperature and molten to carry out the hydrogenation reaction of the hydrocarbon resin, the changes in the molecular weight and softening point due to the hydrogenation reaction of the hydrocarbon resin can be suppressed, and a hydrocarbon resin hydrogenate having excellent color tone and low odor can be produced.

[0049] As a method for adjusting the temperature of the hydrocarbon resin during the hydrogenation reaction, there are a method of preheating the hydrocarbon resin introduced into the fixed bed reactor and a method of heating in the fixed bed reactor. From the viewpoint of appropriately obtaining a hydrocarbon resin hydrogenate having a target hydrogenation rate, it is desirable to adopt these two heating methods. In addition, the melt viscosity of the hydrocarbon resin is measured using, for example, a thermocouple type (ThermoCell) Brookfield viscometer using a rotor No. 31.

[0050] In addition, the range of the hydrogen pressure during the hydrogenation reaction is preferably 0.5 to 3.0 MPa, more preferably 0.8 to 2.5 MPa, and further preferably 1.0 to 2.0 MPa in absolute pressure. When the hydrogen pressure during the hydrogenation reaction is too low, the hydrogenation rate becomes too low, and the color tone of the obtained hydrocarbon resin hydrogenate may deteriorate. On the other hand, when the hydrogen pressure is too high, hydrogenation and decomposition will occur simultaneously, the odor of the obtained hydrocarbon resin hydrogenate will deteriorate, the selectivity of the hydrogenation reaction will deteriorate, and the target quality may not be obtained.

[0051] Furthermore, the hydrocarbon resin hydrogenate may be subjected to a treatment to remove low molecular weight oligomer components by steam distillation, etc. The heating conditions at this time are preferably 160 to 350°C, more preferably 180 to 320°C.

[0052] Furthermore, an antioxidant different from the antioxidant compound added before hydrogenation may be additionally blended into the hydrogenated hydrocarbon resin obtained by the production method of the present invention as required.

[0053] <Hydrocarbon resin>

[0054] Next, the hydrocarbon resin before hydrogenation used in the present invention will be described. The hydrocarbon resin used in the present invention is not particularly limited as long as it is obtained by polymerizing a monomer mixture containing an unsaturated hydrocarbon.

[0055] The monomer mixture for obtaining the hydrocarbon resin is not particularly limited as long as it contains at least an unsaturated hydrocarbon, but preferably contains at least an aliphatic monoolefin and a conjugated diene.

[0056] Examples of the aliphatic monoolefin include alicyclic monoolefins having 4 to 6 carbon atoms and acyclic monoolefins having 4 to 8 carbon atoms.

[0057] Alicyclic monoolefins having 4 to 6 carbon atoms are hydrocarbon compounds having 4 to 6 carbon atoms and having a non-aromatic ring structure and one ethylenically unsaturated bond in their molecular structure. Specific examples of alicyclic monoolefins having 4 to 6 carbon atoms include cyclobutene, cyclopentene, cyclohexene, methylcyclobutene, and methylcyclopentene.

[0058] The content of the alicyclic monoolefin monomer units having 4 to 6 carbon atoms in the hydrocarbon resin used in the present invention is preferably 5 to 35% by mass, more preferably 10 to 33% by mass, and still more preferably 15 to 32% by mass. By setting the content of the alicyclic monoolefin monomer units having 4 to 6 carbon atoms to the above range, the low odor and heat resistance of the hydrogenated hydrocarbon resin after hydrogenation can be further improved.

[0059] The alicyclic monoolefin having 4 to 6 carbon atoms may be used alone or in combination of two or more. It preferably contains at least cyclopentene, and more preferably the proportion of cyclopentene in the alicyclic monoolefin having 4 to 6 carbon atoms is 50 mass % or more.

[0060] The non-cyclic monoolefin having 4 to 8 carbon atoms is a chain hydrocarbon compound having 4 to 8 carbon atoms which has one ethylenically unsaturated bond in its molecular structure and has no ring structure. Specific examples of the non-cyclic monoolefin having 4 to 8 carbon atoms include butenes such as 1-butene, 2-butene, and isobutylene (2-methylpropylene); pentenes such as 1-pentene, 2-pentene, 2-methyl-1-butene, 3-methyl-1-butene, and 2-methyl-2-butene; hexenes such as 1-hexene, 2-hexene, and 2-methyl-1-pentene; heptenes such as 1-heptene, 2-heptene, and 2-methyl-1-hexene; octenes such as 1-octene, 2-octene, 2-methyl-1-heptene, and diisobutylene (2,4,4-trimethyl-1-pentene and 2,4,4-trimethyl-1-pentene); and the like.

[0061] The content of the non-cyclic monoolefin monomer units having 4 to 8 carbon atoms in the hydrocarbon resin used in the present invention is preferably 5 to 30% by mass, more preferably 6 to 28% by mass, further preferably 7 to 26% by mass, and particularly preferably 8 to 24% by mass. By setting the content of the non-cyclic monoolefin monomer units having 4 to 8 carbon atoms to the above range, the low odor property and heat resistance of the hydrogenated hydrocarbon resin after hydrogenation can be further improved.

[0062] The non-cyclic monoolefin having 4 to 8 carbon atoms may be used alone or in combination of two or more. It is preferred that the non-cyclic monoolefin contains at least one selected from 2-methyl-2-butene, isobutylene and diisobutylene. More preferably, the total amount of 2-methyl-2-butene, isobutylene and diisobutylene in the non-cyclic monoolefin having 4 to 8 carbon atoms accounts for 50% by mass or more.

[0063] The conjugated diene is preferably a chain-shaped conjugated diene having 4 to 6 carbon atoms, and specific examples thereof include 1,3-butadiene, isoprene, 1,3-pentadiene, and 1,3-hexadiene.

[0064] The content of the conjugated diene monomer unit in the hydrocarbon resin used in the present invention is preferably 20 to 80% by mass, more preferably 25 to 75% by mass, further preferably 30 to 70% by mass, and particularly preferably 35 to 65% by mass. By making the content of the conjugated diene monomer unit within the above range, the low odor and heat resistance of the hydrogenated hydrocarbon resin after hydrogenation can be further improved.

[0065] The conjugated diene may be used alone or in combination of two or more, preferably at least 1,3-pentadiene, and more preferably the proportion of 1,3-pentadiene in the conjugated diene is 50% by mass or more. In addition, the cis / trans isomer ratio in 1,3-pentadiene may be any ratio and is not particularly limited.

[0066] Furthermore, the monomer mixture for obtaining the hydrocarbon resin may further contain an alicyclic diene and / or an aromatic monoolefin.

[0067] Alicyclic dienes are hydrocarbon compounds having a non-aromatic ring structure and two ethylenically unsaturated bonds in their molecular structure. Specific examples of alicyclic dienes include polymers of cyclopentadiene such as cyclopentadiene and dicyclopentadiene, methylcyclopentadiene, and polymers of methylcyclopentadiene.

[0068] The content of the alicyclic diene monomer unit in the hydrocarbon resin used in the present invention is preferably 1% by mass or less, more preferably 0.8% by mass or less, further preferably 0.6% by mass or less, particularly preferably 0.4% by mass or less.

[0069] The aromatic monoolefin is an aromatic compound having one ethylenically unsaturated bond in its molecular structure. Specific examples of the aromatic monoolefin include styrene, α-methylstyrene, vinyltoluene, indene, benzofuran, and the like.

[0070] The content of the aromatic monoolefin monomer unit in the hydrocarbon resin used in the present invention is preferably 40% by mass or less, more preferably 38% by mass or less, further preferably 36% by mass or less, particularly preferably 34% by mass or less.

[0071] In addition, the monomer mixture for obtaining the hydrocarbon resin may contain other monomers other than the above, and examples of such other monomers include: non-cyclic dienes such as 1,2-butadiene and 1,4-pentadiene; alicyclic monoolefins having 7 or more carbon atoms such as cycloheptene; non-cyclic monoolefins having 3 or less carbon atoms or 9 or more carbon atoms such as ethylene, propylene, and nonene, etc. The content of other monomer units in the hydrocarbon resin used in the present invention is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less.

[0072] The hydrocarbon resin used in the present invention is not particularly limited as long as it is obtained by polymerizing a monomer mixture containing the above unsaturated hydrocarbon. From the viewpoint of efficiently obtaining the hydrocarbon resin, a hydrocarbon resin obtained by cation polymerization of a monomer mixture containing the above unsaturated hydrocarbon using a Lewis acid catalyst is preferred. The Lewis acid catalyst used at this time is not particularly limited, and examples thereof include Friedel-Crafts type cationic polymerization catalysts and the like.

[0073] There are no particular limitations on the Friedel-Crafts type cationic polymerization catalyst, and examples include halides of aluminum, iron, tantalum, zirconium, tin, beryllium, boron, antimony, gallium, bismuth, molybdenum, and the like. Among these, aluminum halides such as aluminum chloride (AlCl3) and aluminum bromide (AlBr3) are preferred. The amount of the Friedel-Crafts type cationic polymerization catalyst added is preferably 0.05 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the monomer mixture used for polymerization.

[0074] When a monomer mixture containing an unsaturated hydrocarbon is polymerized, it is preferred to use a halogenated hydrocarbon in addition to the Friedel-Crafts type cationic polymerization catalyst in order to further improve the catalyst activity.

[0075] Specific examples of halogenated hydrocarbons include halogenated hydrocarbons in which a halogen atom is bonded to a tertiary carbon atom, such as tert-butyl chloride, tert-butyl bromide, 2-chloro-2-methylbutane, and triphenylmethyl chloride; halogenated hydrocarbons in which a halogen atom is bonded to a carbon atom adjacent to a carbon-carbon unsaturated bond, such as benzyl chloride, benzyl bromide, (1-chloroethyl)benzene, allyl chloride, 3-chloro-1-propyne, 3-chloro-1-butene, 3-chloro-1-butyne, and cinnamyl chloride. Among these, tert-butyl chloride and benzyl chloride are preferred from the viewpoint of excellent balance between catalyst activity and handling properties. Halogenated hydrocarbons may be used alone or in combination of two or more. The amount of halogenated hydrocarbon used is preferably in the range of 0.05 to 50, more preferably 0.1 to 10, in terms of molar ratio relative to the Friedel-Crafts type cationic polymerization catalyst.

[0076] When the polymerization reaction is carried out, the order in which the monomer mixture and the components of the polymerization catalyst are added to the polymerization reactor is not particularly limited, and they may be added in any order. From the viewpoint of well controlling the polymerization reaction and thus making the color tone of the hydrogenated hydrocarbon resin after hydrogenation more excellent, it is preferred to add a part of the monomer mixture and the polymerization catalyst components to the polymerization reactor, and after initiating the polymerization reaction, add the remaining part of the polymerization catalyst to the polymerization reactor.

[0077] Furthermore, when an alicyclic monoolefin having 4 to 6 carbon atoms is used as a monomer for obtaining a hydrocarbon resin, it is preferred to first mix a Friedel-Crafts type cationic polymerization catalyst with the alicyclic monoolefin having 4 to 6 carbon atoms during the polymerization reaction from the viewpoint of preventing the generation of gel and thereby making the color tone of the hydrogenated hydrocarbon resin after hydrogenation more excellent.

[0078] From the viewpoint of making the catalyst activity sufficient and preventing the generation of gel more appropriately, the amount of the alicyclic monoolefin having 4 to 6 carbon atoms mixed with the Friedel-Crafts type cationic polymerization catalyst is preferably in the range of 5:1 to 120:1, more preferably 10:1 to 100:1, and even more preferably 15:1 to 80:1, in terms of the mass ratio of "alicyclic monoolefin having 4 to 6 carbon atoms:Friedel-Crafts type cationic polymerization catalyst".

[0079] When the Friedel-Crafts type cationic polymerization catalyst and the alicyclic monoolefin having 4 to 6 carbon atoms are mixed, the order of addition is not particularly limited. The Friedel-Crafts type cationic polymerization catalyst may be added to the alicyclic monoolefin having 4 to 6 carbon atoms, or vice versa. Since mixing is usually accompanied by heat generation, an appropriate diluent may be used. As the diluent, a volatile solvent described later may be used.

[0080] From the viewpoint of better controlling the polymerization reaction, it is preferred to add a volatile solvent to the polymerization reaction system to carry out the polymerization reaction. The type of volatile solvent is not particularly limited as long as it does not hinder the polymerization reaction, and saturated aliphatic hydrocarbons or aromatic hydrocarbons are preferred. As saturated aliphatic hydrocarbons, for example, chain saturated aliphatic hydrocarbons having 5 to 10 carbon atoms such as n-pentane, n-hexane, 2-methylpentane, 3-methylpentane, n-heptane, 2-methylhexane, 3-methylhexane, 3-ethylpentane, 2,2-dimethylpentane, 2,3-dimethylpentane, 2,4-dimethylpentane, 3,3-dimethylpentane, 2,2,3-trimethylbutane, 2,2,4-trimethylpentane, etc.; cyclic saturated aliphatic hydrocarbons having 5 to 10 carbon atoms such as cyclopentane, cyclohexane, cycloheptane, cyclooctane, etc. As aromatic hydrocarbons, for example, aromatic hydrocarbons having 6 to 10 carbon atoms such as benzene, toluene, and xylene, etc., can be mentioned. The volatile solvent may be used alone or in combination of two or more. The amount of the volatile solvent used is not particularly limited, but is preferably 10 to 1000 parts by mass, more preferably 50 to 500 parts by mass, relative to 100 parts by mass of the monomer mixture used for polymerization. In addition, a mixture of addition polymerizable components and non-addition polymerizable components, such as a mixture of cyclopentane and cyclopentene from a C5 fraction, may be added to the polymerization reaction system, the addition polymerizable components being used as components of the monomer mixture, and the non-addition polymerizable components being used as solvents.

[0081] The polymerization temperature during the polymerization reaction is not particularly limited, but is preferably -20°C to 100°C, more preferably 10°C to 70°C. The polymerization reaction time may be appropriately selected, but is usually 10 minutes to 12 hours, preferably 30 minutes to 6 hours.

[0082] When a desired polymerization conversion rate is obtained, a polymerization terminator such as methanol, sodium hydroxide solution, or ammonia solution is added to the polymerization reaction system to terminate the polymerization reaction, thereby obtaining a polymer solution containing a hydrocarbon resin.

[0083] Then, the obtained polymer solution containing the hydrocarbon resin may be subjected to a treatment of removing catalyst residues insoluble in the volatile solvent by filtration or the like, or an adsorbent contact treatment of contacting the catalyst residues with an adsorbent, as required.

[0084] There are no particular limitations on the adsorbent used in the adsorbent contact treatment, and it may be a chemical adsorbent or a physical adsorbent. Specific examples of chemical adsorbents include zinc-based adsorbents such as basic zinc carbonate, zinc oxide, zinc sulfate, zinc laurate, zinc stearate, and zinc myristate; zirconium-based adsorbents such as zirconium oxide, zirconium hydroxide, and zirconium phosphate; manganese-based adsorbents such as manganese dioxide; cobalt-based adsorbents such as cobalt chloride; copper-based adsorbents such as copper chloride and copper oxide; amine-based adsorbents such as polyamine compounds, etc. Specific examples of physical adsorbents include zeolite-based adsorbents such as sodium aluminum silicate, which are collectively referred to as a group of hydrous aluminum silicate minerals; silicon dioxide, magnesium oxide, silica gel, silicon dioxide / alumina, aluminum silicate, activated alumina, acid clay, activated clay, dawsonite compounds, and hydrotalcite compounds. The adsorbent may be used alone or in combination of two or more. In particular, from the viewpoint of achieving a greater odor reduction effect, it is preferred to use a chemical adsorbent, more preferably a zinc-based adsorbent, and particularly preferably basic zinc carbonate.

[0085] In the adsorbent contact treatment, there is no particular limitation on the method for bringing the obtained polymer solution containing the hydrocarbon resin into contact with the adsorbent, and examples thereof include: a batch treatment method in which the polymer solution and the adsorbent are allowed to coexist in a container and stirred as needed to bring them into contact; a continuous treatment method in which the adsorbent is pre-filled in a packed tower and the polymer solution is circulated therein to bring them into contact, etc.

[0086] The amount of adsorbent used when the polymer solution containing hydrocarbon resin obtained by the batch method is contacted with the adsorbent is not particularly limited, and is generally 0.01 to 5.0 parts by mass, preferably 0.03 to 3.0 parts by mass, and more preferably 0.05 to 2.0 parts by mass relative to 100 parts by mass of the hydrocarbon resin contained in the polymer solution. In addition, the temperature when the polymer solution is contacted with the adsorbent is not particularly limited, and is generally selected within the range of 10°C to 70°C. In addition, the treatment time is not particularly limited, and is generally selected within the range of 0.1 to 2 hours. In addition, when the polymer solution is contacted with the adsorbent by the batch method, the adsorbent can be removed as needed.

[0087] The obtained polymer solution containing hydrocarbon resin is preferably subjected to stripping treatment in order to further remove volatile components such as volatile solvents and unreacted monomers. In the production method of the present invention, when hydrogenating the hydrocarbon resin before hydrogenation, the hydrogenation reaction is carried out in a state where the volatile solvent and unreacted monomers are removed by pre-stripping treatment, which can effectively suppress the reduction in controllability of the hydrogenation rate caused by the hydrogenation of unreacted monomers in the hydrogenation reaction. In particular, in hydrocarbon resins obtained by cationic polymerization using a Lewis acid catalyst, although hydrocarbon resins with excellent properties can be obtained efficiently, about 10% to 20% of unreacted monomers are inevitably contained. Such unreacted monomers are hydrogenated, and the hydrogenation rate will be biased, etc., and the controllability is reduced, which may make it difficult to obtain the desired hydrogenation rate. By performing stripping treatment to carry out the hydrogenation reaction in a state where the volatile solvent and unreacted monomers are removed, the controllability of the hydrogenation rate can be improved, thereby stably and efficiently obtaining a hydrocarbon resin hydrogenate having a target hydrogenation rate. Moreover, as a result, a hydrocarbon resin hydrogenate with a better color tone and lower odor can be appropriately obtained.

[0088] In addition, as a stripping treatment, the following method is preferred: if necessary, the polymer solution containing the hydrocarbon resin is heated to preferably 80 to 240° C., more preferably 100 to 200° C., in an inert gas environment such as argon or nitrogen, thereby removing volatile components such as volatile solvents and unreacted monomers. At this time, when an inert gas is used, its flow rate is preferably 0.2 to 1.0 m 2 / (hr·kg). In addition, the steam stripping treatment time is preferably 0.5 to 24 hours. When the steam stripping is performed by continuous circulation, the residence time is 0.01 to 1 hour. In addition, after the volatile components are removed by heating, the hydrocarbon resin from which the volatile components have been removed may be further treated by steam distillation or the like to remove low molecular weight oligomer components. The heating conditions at this time are preferably 160 to 350°C, more preferably 180 to 320°C.

[0089] The amount of impurities such as unreacted monomers and low molecular weight oligomers remaining in the hydrocarbon resin without being removed by the stripping treatment is preferably 1000 ppm by mass or less. By setting the amount of impurities within the above range, the controllability of the hydrogenation rate during the hydrogenation reaction can be suitably improved.

[0090] <Hydrocarbon resin hydrogenated product>

[0091] From the viewpoint of making the color tone and low odor of the obtained hydrocarbon resin hydrogenate more excellent, the hydrogenation rate of the hydrocarbon resin hydrogenate obtained by the production method of the present invention (the proportion of hydrogenated carbon-carbon double bonds in all non-aromatic carbon-carbon double bonds of the hydrocarbon resin before hydrogenation) is preferably 3 to 95%, more preferably 10 to 95%, further preferably 20 to 90%, and particularly preferably 30 to 80%. The hydrogenation rate can be calculated based on the difference in the amount of non-aromatic carbon-carbon double bonds contained in the hydrocarbon resin before hydrogenation and the hydrocarbon resin hydrogenate after hydrogenation. Here, the amount of non-aromatic carbon-carbon double bonds can be calculated, for example 1 H-NMR spectrum measurement. According to the present invention, by carrying out the hydrogenation reaction in the presence of the above-mentioned antioxidant compound, the changes in the molecular weight and softening point of the hydrocarbon resin caused by the hydrogenation reaction can be more effectively suppressed compared to the case where the hydrogenation reaction is carried out in the absence of the above-mentioned antioxidant compound to the same hydrogenation rate. For example, even when the hydrogenation reaction is carried out to make the hydrogenation rate of the hydrocarbon resin reach 30% or more, preferably 40% or more, the decrease in the weight average molecular weight can be suppressed to within 12% relative to the weight average molecular weight of the hydrocarbon resin before hydrogenation, preferably within 10%, and the decrease in the softening point caused by the hydrogenation reaction of the hydrocarbon resin can be suppressed to within 5% relative to the softening point of the hydrocarbon resin before hydrogenation.

[0092] In addition, the weight average molecular weight (Mw) of the hydrogenated hydrocarbon resin hydrogenate is preferably in the range of 1000 to 5000, more preferably in the range of 1500 to 4500, and further preferably in the range of 1800 to 4000. In addition, the Z average molecular weight (Mz) of the hydrogenated hydrocarbon resin hydrogenate is preferably in the range of 2500 to 10000, more preferably in the range of 2500 to 9000, and further preferably in the range of 3000 to 8000. By making the weight average molecular weight (Mw) and the Z average molecular weight (Mz) in the above range, when the hydrocarbon resin hydrogenate is used for a hot melt adhesive composition, for example, the compatibility with the base polymer can be further improved, thereby further improving the adhesive performance.

[0093] The weight average molecular weight (Mw) and the Z average molecular weight (Mz) of the hydrogenated hydrocarbon resin can be determined as polystyrene-equivalent values ​​measured by high performance liquid chromatography.

[0094] The ratio of the Z average molecular weight to the weight average molecular weight (Mz / Mw) of the hydrogenated hydrocarbon resin is preferably in the range of 1.5 to 2.5, more preferably 1.6 to 2.4, and even more preferably 1.65 to 2.35.

[0095] The hydrogenated hydrocarbon resin obtained by the production method of the present invention is excellent in color tone and low odor, and can be preferably used in various applications such as hot melt adhesives by making effective use of such characteristics. However, the application is not limited to these.

[0096] Example

[0097] The present invention will be further described below based on detailed examples, but the present invention is not limited to these examples. In addition, unless otherwise specified, "parts" and "%" are based on mass. In addition, the tests and evaluations are as follows.

[0098] Various measurements were performed according to the following methods.

[0099] [Weight average molecular weight]

[0100] The hydrocarbon resin before hydrogenation and the hydrocarbon resin hydrogenate were subjected to gel permeation chromatography analysis to determine the weight average molecular weight (Mw) of the standard polystyrene conversion value. In addition, in the gel permeation chromatography analysis, as a measuring device, "HLC-8320GPC" manufactured by Tosoh was used, and three "TSKgel SuperMultiporeHZ" manufactured by Tosoh were connected as columns, and tetrahydrofuran was used as a solvent, and the measurement was performed at 40°C and a flow rate of 1.0 mL / min.

[0101] [Softening point (℃)]

[0102] The softening point (°C) of the hydrocarbon resin before hydrogenation and the hydrocarbon resin hydrogenate was measured in accordance with JIS K 2207.

[0103] [Hydrogenation rate (%)]

[0104] Hydrocarbon resins before hydrogenation and hydrocarbon resin hydrides are subjected to 1 The amount of non-aromatic carbon-carbon double bonds was determined by H-NMR spectrum measurement, and the hydrogenation rate (%) was determined based on the difference in the amount of non-aromatic carbon-carbon double bonds before and after hydrogenation. 1 In the H-NMR spectrum measurement, deuterated chloroform was used as a solvent, and JMN-AL series AL400 (manufactured by JEOL) was used as an NMR measurement apparatus for measurement.

[0105] [Gardner Color Scale]

[0106] A 50 mass % toluene solution of the hydrocarbon resin hydrogenate was prepared using the hydrocarbon resin hydrogenate, and the Gardner color scale of the solution was measured in accordance with JIS K 0071-2. The smaller the value of the Gardner color scale, the better the color tone.

[0107] [Odor evaluation test]

[0108] The sensory test of the hydrocarbon resin hydrogenate was conducted in accordance with the olfaction method of odor-5 revision of the olfaction method of odor issued by the Japan Odor / Fragrance Environment Association.

[0109] Specifically, first, 10 g of a hydrocarbon resin hydride pellet of about 10 mm × 5 mm × 5 mm in size was placed in a 120 mL heat-resistant container and covered with aluminum foil. Then, the heat-resistant container containing the hydrocarbon resin hydride was placed in an oven and heated at 150° C. for 30 minutes to confirm the odor after heating.

[0110] The odor was confirmed by a group of 6 people who were not familiar with the odor of petroleum resin (i.e., they were not exposed to the odor of petroleum resin in their daily lives). In this test, in order to prevent olfactory fatigue, the 6-person group was divided into 2 groups, 3 people in each group, and one group smelled the odor at a time. In addition, the order of smelling the samples was random.

[0111] 0: No odor

[0112] 1: Barely identifiable odor (detection threshold concentration)

[0113] 2: A faint odor that is judged to be a certain odor (identification threshold concentration)

[0114] 3: Smells that can be easily detected

[0115] 4: Strong odor

[0116] 5. Strong odor

[0117] The results of the sensory test were obtained by removing the maximum and minimum values ​​from the judgment values ​​of the six-person group and averaging the judgment values ​​of the remaining four people. The smaller the value of the sensory test, the better.

[0118] [Example 1]

[0119] A mixture of 49.5 parts of cyclopentane and 12.4 parts of cyclopentene was added to a polymerization reactor, and after the temperature was raised to 60°C, 0.7 parts of aluminum chloride was added to obtain a mixture A1. Next, a mixture B1 composed of 54.1 parts of 1,3-pentadiene, 15.3 parts of isobutylene, 1.8 parts of styrene, 15.2 parts of cyclopentene, 1.2 parts of C4-C6 unsaturated hydrocarbons, and 9.8 parts of C4-C6 saturated hydrocarbons, and 0.4 parts of tert-butyl chloride were kept at 60°C for 60 minutes through another pipeline, and then continuously added to the polymerization reactor containing the mixture A1 obtained above, while polymerization was carried out. Then, an aqueous sodium hydroxide solution was added to the polymerization reactor to terminate the polymerization reaction. The precipitate generated by the termination of the polymerization was removed by filtration to obtain a polymer solution containing hydrocarbon resins before hydrogenation and unreacted monomers. Next, the polymer solution was transferred to a distillation kettle and heated at 150° C. for 1 hour under a nitrogen atmosphere to perform a stripping operation, thereby removing the polymerization solvent and unreacted monomers to obtain a hydrocarbon resin before hydrogenation. Then, the obtained hydrocarbon resin before hydrogenation was subjected to various tests and evaluations of weight average molecular weight and softening point according to the above methods. The results are shown in Table 1.

[0120] The amount of volatile solvent and the amount of unreacted monomers in the obtained hydrocarbon resin before hydrogenation were measured by headspace gas chromatography after heating at 150° C. for 0.5 hour under reduced pressure. The results showed that both were less than 1000 mass ppm, which was the detection limit.

[0121] Then, a hindered phenolic antioxidant (pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], trade name "Irganox (registered trademark) 1010") was added as an antioxidant compound to the hydrocarbon resin before hydrogenation so that the amount of the hindered phenolic antioxidant added was 0.1 parts per 100 parts of the hydrocarbon resin before hydrogenation, and then, in a state where the temperature of the hydrocarbon resin was kept at 220°C, the mixture was continuously introduced into a multi-tube heat exchange type hydrogenation reaction apparatus together with hydrogen gas, thereby carrying out a hydrogenation reaction to obtain a hydrocarbon resin hydrogenate. In addition, the melt viscosity of the hydrocarbon resin before hydrogenation in the state where the temperature was heated to 220°C (measured by a thermocouple type Brookfield viscometer, using a rotor No. 31) was 200 mPa·s, and the hydrogen pressure during the hydrogenation reaction was 2 MPa in absolute pressure. In addition, as a multi-tubular heat exchange type hydrogenation reaction apparatus, a multi-tubular heat exchange type hydrogenation reaction apparatus (inner diameter of reaction tube: 25 mm, length of reaction tube: 3 m, number of reaction tubes: 1700) in which a nickel / silica-magnesia supported catalyst (trade name "N102F", manufactured by JGC Catalysts and Chemicals Ltd., cylindrical with average diameter: 2.8 mmφ, average length: 2.8 mm) was filled in the reaction tube was used, the residence time in the reaction tube was 1.5 hours, and the number of circulations was 1 time.

[0122] Next, the obtained hydrocarbon resin hydrogenate was heated to 250°C to be molten, saturated steam was blown in, and low molecular weight oligomer components were distilled off, thereby obtaining the hydrocarbon resin hydrogenate of Example 1. Then, the obtained hydrocarbon resin hydrogenate was subjected to various tests and evaluations of hydrogenation rate, weight average molecular weight, softening point, Gardner color scale, and odor evaluation test according to the above method. The results are shown in Table 1.

[0123] [Example 2]

[0124] The hydrocarbon resin before hydrogenation obtained in the same manner as in Example 1 was used, and the temperature when it was introduced into the multi-tube heat exchange type hydrogenation reaction device together with hydrogen was changed from 220°C to 320°C, and the temperature of the hydrocarbon resin was continuously introduced while being maintained at 320°C, thereby carrying out the hydrogenation reaction. In addition, in Example 2, the residence time in the reaction tube was 0.2 hours, and the number of circulations was 1 time. In addition, the melt viscosity of the hydrocarbon resin before hydrogenation when heated to a temperature of 320°C (measured by a thermocouple type Brookfield viscometer using rotor No. 31) was 120 mPa·s. Then, the obtained hydrocarbon resin hydrogenate was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0125] [Example 3]

[0126] Hydrocarbon resin hydrogenated product was obtained in the same manner as in Example 1 except that the amount of the hindered phenol antioxidant added was 0.3 parts per 100 parts of the hydrocarbon resin before hydrogenation. In Example 3, the residence time in the reaction tube was 1.5 hours and the number of circulations was 1. The obtained hydrocarbon resin hydrogenated product was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0127] [Example 4]

[0128] Hydrocarbon resin hydrogenated product was obtained in the same manner as in Example 2 except that the amount of the hindered phenol antioxidant added was 0.3 parts per 100 parts of the hydrocarbon resin before hydrogenation. In Example 4, the residence time in the reaction tube was 0.2 hours and the number of circulations was 1. The obtained hydrocarbon resin hydrogenated product was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0129] [Example 5]

[0130] In Example 1, as an antioxidant compound, the hindered phenol antioxidant was changed to an antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group (poly[{(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidinyl)imino}] trade name "Chimassorb (registered trademark) 2020"), and the addition amount of the antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group was 0.3 parts relative to 100 parts of the hydrocarbon resin before hydrogenation. Hydrocarbon resin hydrogenated products were obtained in the same manner as in Example 1. In addition, in Example 5, the residence time in the reaction tube was 1.5 hours, and the number of circulations was 1 time. Then, the obtained hydrocarbon resin hydrogenated products were evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0131] [Example 6]

[0132] In Example 2, as an antioxidant compound, the hindered phenol antioxidant was changed to an antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group (poly[{(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidinyl)imino}] trade name "Chimassorb (registered trademark) 2020"), and the addition amount of the antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group was 0.3 parts relative to 100 parts of the hydrocarbon resin before hydrogenation. Hydrocarbon resin hydrogenated products were obtained in the same manner as in Example 2. In addition, in Example 6, the residence time in the reaction tube was 0.2 hours, and the number of circulations was 1 time. Then, the obtained hydrocarbon resin hydrogenated products were evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0133] [Example 7]

[0134] In Example 1, as an antioxidant compound, an antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group (poly[{(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidinyl)imino}] trade name "Chimassorb (registered trademark) 2020") was used together with a hindered phenol antioxidant, and the amount of the hindered phenol antioxidant added was 0.2 parts relative to 100 parts of the hydrocarbon resin before hydrogenation, and the amount of the antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group added was 0.1 parts relative to 100 parts of the hydrocarbon resin before hydrogenation. The same procedure as in Example 1 was used to obtain a hydrocarbon resin hydrogenated product. In Example 7, the residence time in the reaction tube was 1.5 hours, and the number of circulations was 1. Then, the obtained hydrocarbon resin hydrogenated product was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0135] [Example 8]

[0136] In Example 2, an antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group (poly[{(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidinyl)imino}] trade name "Chimassorb (registered trademark) 2020") was used as an antioxidant compound together with a hindered phenol antioxidant, and the amount of the hindered phenol antioxidant added was 0.2 parts relative to 100 parts of the hydrocarbon resin before hydrogenation, and the amount of the antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group added was 0.1 parts relative to 100 parts of the hydrocarbon resin before hydrogenation. The same procedure as in Example 2 was used to obtain a hydrocarbon resin hydrogenated product. In Example 8, the residence time in the reaction tube was 0.2 hours, and the number of circulations was 1. Then, the obtained hydrocarbon resin hydrogenated product was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0137] [Comparative Example 1]

[0138] The hydrocarbon resin before hydrogenation obtained in the same manner as in Example 1 was heated to 220° C. without adding a hindered phenol antioxidant, and was continuously introduced into a multi-tube heat exchange type hydrogenation reaction apparatus with hydrogen gas while the temperature of the hydrocarbon resin was maintained at 220° C., thereby conducting a hydrogenation reaction to obtain a hydrocarbon resin hydrogenate. The melt viscosity of the hydrocarbon resin before hydrogenation when heated to 220° C. (measured by a thermocouple type Brookfield viscometer using a rotor No. 31) was 200 mPa·s, and the hydrogen pressure during the hydrogenation reaction was 2 MPa in absolute pressure. In addition, as a multi-tubular heat exchange type hydrogenation reaction apparatus, a multi-tubular heat exchange type hydrogenation reaction apparatus (inner diameter of reaction tube: 25 mm, length of reaction tube: 3 m, number of reaction tubes: 1700) in which a nickel / silica-magnesia supported catalyst (trade name "N102F", manufactured by JGC Catalysts and Chemicals Ltd., cylindrical with average diameter: 2.8 mmφ, average length: 2.8 mm) was filled in the reaction tube was used, the residence time in the reaction tube was 1.5 hours, and the number of circulations was 1 time.

[0139] Then, a hindered phenol antioxidant (pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], trade name "Irganox (registered trademark) 1010") was added to the obtained hydrocarbon resin hydrogenate so that the added amount of the hindered phenol antioxidant was 0.3 parts relative to 100 parts of the hydrocarbon resin before hydrogenation, and the mixture was heated to 250°C to be molten, saturated steam was blown in, and low molecular weight oligomer components were distilled off to obtain a hydrocarbon resin hydrogenate of Comparative Example 1. Then, the obtained hydrocarbon resin hydrogenate was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0140] [Comparative Example 2]

[0141] The hydrocarbon resin before hydrogenation obtained in the same manner as in Example 1 was used, and the temperature when the hydrocarbon resin was introduced into the multi-tube heat exchange type hydrogenation reaction device together with hydrogen was changed from 220°C to 320°C, and the hydrocarbon resin was continuously introduced while the temperature was maintained at 320°C to carry out the hydrogenation reaction. In Comparative Example 2, the residence time in the reaction tube was 0.2 hours, and the number of circulations was 1. Then, the obtained hydrocarbon resin hydrogenated product was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0142] [Comparative Example 3]

[0143] In Comparative Example 1, an antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group (poly[{(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidinyl)imino}] trade name "Chimassorb (registered trademark) 2020") was used as an antioxidant compound together with a hindered phenol antioxidant, and the amount of the hindered phenol antioxidant added was 0.2 parts relative to 100 parts of the hydrocarbon resin before hydrogenation, and the amount of the antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group added was 0.1 parts relative to 100 parts of the hydrocarbon resin before hydrogenation. The same procedure as in Comparative Example 1 was performed to obtain a hydrocarbon resin hydrogenated product. In Comparative Example 3, the residence time in the reaction tube was 1.5 hours, and the number of circulations was 1. Then, the obtained hydrocarbon resin hydrogenated product was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0144] [Comparative Example 4]

[0145] In Comparative Example 2, an antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group (poly[{(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidinyl)imino}] trade name "Chimassorb (registered trademark) 2020") was used as an antioxidant compound together with a hindered phenol antioxidant, and the amount of the hindered phenol antioxidant added was 0.2 parts relative to 100 parts of the hydrocarbon resin before hydrogenation, and the amount of the antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group added was 0.1 parts relative to 100 parts of the hydrocarbon resin before hydrogenation. The same procedure as in Comparative Example 2 was performed to obtain a hydrocarbon resin hydrogenated product. In Comparative Example 4, the residence time in the reaction tube was 0.2 hours, and the number of circulations was 1. Then, the obtained hydrocarbon resin hydrogenated product was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0146] [Table 1]

[0147]

[0148] As shown in Table 1, by contacting a hydrocarbon resin with hydrogen in the presence of at least one antioxidant compound selected from a hindered phenol antioxidant and an antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group and a hydrogenation catalyst, a hydrogenation reaction is carried out, thereby suppressing changes in molecular weight and softening point caused by the hydrogenation reaction of the hydrocarbon resin. Furthermore, the obtained hydrocarbon resin hydrogenate has excellent color tone (Gardner color scale) and low odor (Examples 1 to 8).

[0149] On the other hand, when a hydrocarbon resin is brought into contact with hydrogen in the presence of a hydrogenation catalyst in the absence of the above-mentioned antioxidant compound to thereby carry out a hydrogenation reaction, the changes in the molecular weight and the softening point before and after the hydrogenation are large compared to the case where the hydrocarbon resin is brought into contact with hydrogen in the presence of the above-mentioned antioxidant compound and a hydrogenation catalyst to thereby carry out a hydrogenation reaction to the same hydrogenation rate, and the changes in the molecular weight and the softening point due to the hydrogenation reaction of the hydrocarbon resin cannot be suppressed (Comparative Examples 1 to 4).

[0150] [Example 9]

[0151] The hydrocarbon resin obtained in the same manner as in Example 1 was used, and the temperature when it was introduced into the multi-tubular heat exchange type hydrogenation reaction device together with hydrogen was changed from 220°C to 160°C, and the temperature of the hydrocarbon resin was continuously introduced while being maintained at 160°C, thereby carrying out the hydrogenation reaction. In addition, in Example 9, the residence time in the reaction tube was 0.8 hours, and the number of circulations was 1 time. In addition, the melt viscosity of the hydrocarbon resin before hydrogenation when heated to a temperature of 160°C (measured by a thermocouple type Brookfield viscometer using rotor No. 31) was 1200 mPa·s. Then, the obtained hydrocarbon resin hydrogenate was evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0152] [Example 10]

[0153] The hydrocarbon resin obtained in the same manner as in Example 1 was used, the amount of the hindered phenol antioxidant added was 0.3 parts per 100 parts of the hydrocarbon resin before hydrogenation obtained, the temperature when the hydrocarbon resin was introduced into the multi-tube heat exchange type hydrogenation reaction device together with hydrogen was changed from 220°C to 160°C, and the hydrocarbon resin was continuously introduced while the temperature was maintained at 160°C to carry out the hydrogenation reaction, and the hydrocarbon resin hydrogenated product was obtained in the same manner as in Example 1. In Example 10, the residence time in the reaction tube was 0.8 hours, and the number of circulations was 1. Then, the obtained hydrocarbon resin hydrogenated product was evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0154] [Example 11]

[0155] In Example 9, as an antioxidant compound, the hindered phenol antioxidant was changed to an antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group (poly[{(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidinyl)imino}] trade name "Chimassorb (registered trademark) 2020"), and the addition amount of the antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group was 0.3 parts relative to 100 parts of the hydrocarbon resin before hydrogenation. Hydrocarbon resin hydrogenated products were obtained in the same manner as in Example 9. In addition, in Example 11, the residence time in the reaction tube was 0.8 hours, and the number of circulations was 1 time. Then, the obtained hydrocarbon resin hydrogenated products were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0156] [Example 12]

[0157] In Example 9, an antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group (poly[{(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidinyl)imino}] trade name "Chimassorb (registered trademark) 2020") was used as an antioxidant compound together with a hindered phenol antioxidant, and the amount of the hindered phenol antioxidant added was 0.2 parts relative to 100 parts of the hydrocarbon resin before hydrogenation, and the amount of the antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group added was 0.1 parts relative to 100 parts of the hydrocarbon resin before hydrogenation. The same procedure as in Example 9 was used to obtain a hydrocarbon resin hydrogenated product. In Example 12, the residence time in the reaction tube was 0.8 hours, and the number of circulations was 1. Then, the obtained hydrocarbon resin hydrogenated product was evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0158] [Comparative Example 5]

[0159] The hydrocarbon resin obtained in the same manner as in Example 1 was used, and the temperature when the hydrocarbon resin was introduced into the multi-tube heat exchange type hydrogenation reaction device together with hydrogen was changed from 220°C to 160°C, and the hydrocarbon resin was continuously introduced while the temperature of the hydrocarbon resin was kept at 160°C to carry out the hydrogenation reaction. In Comparative Example 3, the residence time in the reaction tube was 0.8 hours, and the number of circulations was 1. Then, the obtained hydrocarbon resin hydrogenated product was evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0160] [Comparative Example 6]

[0161] In Comparative Example 5, an antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group (poly[{(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidinyl)imino}] trade name "Chimassorb (registered trademark) 2020") was used as an antioxidant compound together with a hindered phenol antioxidant, and the amount of the hindered phenol antioxidant added was 0.2 parts relative to 100 parts of the hydrocarbon resin before hydrogenation, and the amount of the antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group added was 0.1 parts relative to 100 parts of the hydrocarbon resin before hydrogenation. The same procedure as in Comparative Example 5 was performed to obtain a hydrocarbon resin hydrogenated product. In Comparative Example 6, the residence time in the reaction tube was 0.8 hours, and the number of circulations was 1. Then, the obtained hydrocarbon resin hydrogenated product was evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0162] [Table 2]

[0163]

[0164] As shown in Table 2, even when the hydrogenation rate is low, by bringing a hydrocarbon resin into contact with hydrogen in the presence of at least one antioxidant compound selected from a hindered phenol antioxidant and an antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group, and a hydrogenation catalyst, a hydrogenation reaction is carried out, thereby producing a hydrocarbon resin hydrogenated product having excellent color tone and low odor while suppressing changes in the molecular weight and softening point due to the hydrogenation reaction of the hydrocarbon resin (Examples 9 to 12).

[0165] On the other hand, when the hydrocarbon resin is brought into contact with hydrogen in the presence of a hydrogenation catalyst in the absence of the antioxidant compound to thereby conduct a hydrogenation reaction, changes in the molecular weight and softening point of the hydrocarbon resin due to the hydrogenation reaction cannot be suppressed (Comparative Examples 5 and 6).

Claims

1. A method for producing a hydrocarbon resin hydrogenate, the method comprising contacting a hydrocarbon resin with hydrogen in the presence of at least one antioxidant compound selected from a hindered phenol antioxidant and an antioxidant having a 2,2,6,6-tetraalkyl-4-piperidinyl group, and a hydrogenation catalyst, thereby conducting a hydrogenation reaction, The hydrocarbon resin is obtained by cationically polymerizing a monomer mixture containing unsaturated hydrocarbons using a Lewis acid catalyst.

2. The method for producing a hydrocarbon resin hydrogenate according to claim 1, in, The antioxidant compound is present in an amount of 0.01 to 10 parts by mass relative to 100 parts by mass of the hydrocarbon resin.

3. The method for producing a hydrocarbon resin hydrogenate according to claim 1 or 2, in, The hydrocarbon resin is obtained by stripping a polymer solution containing a hydrocarbon resin obtained by cation polymerization using a Lewis acid catalyst.

4. The method for producing a hydrocarbon resin hydrogenate according to claim 1 or 2, in, The hydrocarbon resin is heated to 150 to 350° C. and has a melt viscosity in the range of 50 to 1500 mPa·s, and is brought into contact with hydrogen to carry out a hydrogenation reaction.

5. The method for producing a hydrocarbon resin hydrogenate according to claim 1 or 2, in, The hydrogen pressure during the hydrogenation reaction is in the range of 0.5 to 3.0 MPa.

6. The method for producing a hydrocarbon resin hydrogenate according to claim 1 or 2, in, The hydrocarbon resin is brought into contact with hydrogen using a fixed bed reactor, thereby conducting a hydrogenation reaction.

7. The method for producing a hydrocarbon resin hydrogenate according to claim 1 or 2, in, As the hydrogenation catalyst, a granular hydrogenation catalyst having an average diameter of 1 to 5 mmφ and an average length of 1 to 10 mm is used.

8. The method for producing a hydrocarbon resin hydrogenate according to claim 1 or 2, in, The hydrogenation catalyst is a nickel catalyst.

9. The method for producing a hydrocarbon resin hydrogenate according to claim 8, in, The nickel catalyst is a catalyst containing a compound in which nickel is supported on magnesium oxide-silicon dioxide as a main component.

Citation Information

Patent Citations

  • Facsimile equipment

    JP1993276269A

  • Production of hydrogenated petroleum resin

    JP1986204210A

  • Hydrogenation of polymer

    JP1991247604A

  • Production of hydrogenated petroleum resin

    JP1992372606A

  • Phenol-modified 9c-based hydrogenated petroleum resin and its production

    JP1997268209A