Adhesive sheet and its use

The adhesive sheet with a specific elastic modulus and impact resistance, combined with a photoreactive monomer, addresses the challenge of balancing deformation and impact resistance, ensuring strong and durable bonds.

CN114051521BActive Publication Date: 2024-12-06NITTO DENKO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202080047095.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-06-22
Filing Date
2020-06-23
Publication Date
2024-12-06
Estimated Expiration
2040-06-23

AI Technical Summary

Technical Problem

Existing adhesive sheets face challenges in balancing high deformation resistance and impact resistance, making it difficult to form bonds that can withstand stress and maintain integrity under impact.

Method used

A pressure-sensitive adhesive sheet with an elastic modulus of 3.0 MPa or more and impact resistance of 2.0 J/(10 mm)^2, comprising a polymer and a photoreactive monomer with a ring structure and two or more ethylenically unsaturated groups, which is photocured to enhance bonding properties.

Benefits of technology

The adhesive sheet achieves high deformation resistance and impact resistance, suitable for joining and fixing components, maintaining bond integrity under stress and impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114051521B_ABST
    Figure CN114051521B_ABST
Patent Text Reader

Abstract

Provided is an adhesive sheet having an adhesive layer. The adhesive sheet has the following properties (a) and (b). (a) The elastic modulus measured by a tensile test is 3.0 MPa or more. (b) The impact resistance measured by a shear impact test is 2.0 J / (10 mm). 2 above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive sheet, a film member with an adhesive sheet, and a method for producing a laminate.

[0002] This application claims priority based on Japanese Patent Application No. 2019-122284 filed on June 28, 2019 and Japanese Patent Application No. 2020-107125 filed on June 22, 2020, the entire contents of which are incorporated herein by reference. Background Art

[0003] Generally, adhesives (also called pressure-sensitive adhesives. The same applies below) have the following properties: they are in a soft solid (viscoelastic) state in a temperature range near room temperature and are easily bonded to an adherend under pressure. Taking full advantage of such properties, adhesives are typically used in various fields in the form of adhesive sheets including an adhesive layer. As technical documents related to adhesive sheets, Patent Document 1 can be cited.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2016-017113 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] Depending on the application, various properties are required of adhesives. Among these properties, it is sometimes difficult to take into account both at a high level, for example, there is a tendency for another property to decrease when one property is improved. As an example of properties that are in such a relationship that is difficult to take into account, the property of not being easily deformed against stress (hereinafter also referred to as "deformation resistance") and the property of withstanding impact and maintaining bonding with the adherend (hereinafter also referred to as "impact resistance") can be listed.

[0009] Therefore, an object of the present invention is to provide an adhesive sheet capable of forming a bond having high deformation resistance and high impact resistance. Another object of the present invention is to provide a film member with an adhesive sheet comprising the above adhesive sheet. Another object of the present invention is to provide a method for producing a laminate using the above adhesive sheet.

[0010] According to this specification, a pressure-sensitive adhesive sheet is provided, which includes a pressure-sensitive adhesive layer and has the following properties (a) and (b).

[0011] (a) The elastic modulus measured by the following tensile test is 3.0 MPa or more.

[0012] (b) The impact resistance measured by the following shear impact test is 2.0 J / (10 mm) 2 above.

[0013] [Tensile test]

[0014] At an illumination of 300mW / cm 2 、Accumulated light intensity 3000mJ / cm 2 The adhesive layer was irradiated with ultraviolet rays under the conditions of , and after aging at 50°C for 48 hours, the adhesive layer was cut into a size of 10 mm in width and 150 mm in length to prepare a test piece. Under the conditions of 23°C and 50% RH, a tensile tester was used to perform a tensile test on the test piece under the conditions of a chuck spacing of 120 mm and a tensile speed of 50 mm / min, and a stress-displacement curve (hereinafter also referred to as "SS curve") was obtained, and the elastic modulus [MPa] (hereinafter also referred to as tensile modulus) was calculated from its initial slope.

[0015] [Shear impact test]

[0016] The shear impact test was conducted using a pendulum-type adhesive shear impact tester based on JIS K6855. As the test sample, the following sample was used: the first surface of the above-mentioned adhesive layer of 10 mm square was attached to the central part of a chemically tempered glass plate of 25 mm square and 1.7 mm thick, and the second surface of the above-mentioned adhesive layer was attached to the central part of a stainless steel plate (SUS304BA plate) of 40 mm square and pressed at a load of 5 N for 10 seconds, and then autoclaved (50°C, 0.5 MPa, 15 minutes) at an illumination of 300 mW / cm 2 、Accumulated light intensity 3000mJ / cm 2 After irradiating the glass plate with ultraviolet rays from the glass plate side under the conditions of , aging was performed at 50° C. for 48 hours to obtain a sample.

[0017] The above-mentioned measurement sample was fixed in a manner such that the above-mentioned stainless steel plate was at the lower side, and the absorbed energy [J] when the outer peripheral side surface of the above-mentioned glass plate was hit by a hammer under the conditions of a hammer energy of 2.75 J and a hammer speed (impact speed) of 3.5 m / sec was measured, thereby determining the impact resistance [J / (10 mm) 2 ].

[0018] By satisfying the above-mentioned characteristic (a), the above-mentioned adhesive layer can exhibit high deformation resistance when the above-mentioned adhesive sheet is used, for example. The adhesive sheet satisfying the above-mentioned characteristics (a) and (b) can form a joint with high deformation resistance and high impact resistance, and can therefore be suitably used for purposes such as joining and fixing components.

[0019] In addition, according to the specification, there is provided an adhesive sheet comprising an adhesive layer, the adhesive layer comprising a polymer (A) and a photoreactive monomer (B). In some embodiments of the above-mentioned adhesive sheet, the above-mentioned photoreactive monomer (B) comprises a compound B1 having a ring structure and two or more ethylenically unsaturated groups in the molecule. The average molecular weight of each of the above-mentioned ethylenically unsaturated groups of the above-mentioned compound B1 is preferably 100 g / mol or more. According to the above-mentioned adhesive sheet with an adhesive layer, a joint with high deformation resistance and high impact resistance can be suitably formed.

[0020] The PSA sheet of any embodiment disclosed herein may satisfy the following property (c). A PSA sheet satisfying property (c) may be suitably used for purposes such as joining and fixing of components.

[0021] (c) The peel strength measured by the following peel test is 1.0 N / 10 mm or more.

[0022] [Peel test]

[0023] The first surface of the adhesive layer was pressed against the glass plate by reciprocating a 2 kg rubber roller once, and then autoclaved (50° C., 0.5 MPa, 15 minutes) and then heated under an illumination of 300 mW / cm 2 、Accumulated light intensity 3000mJ / cm 2 After aging at 50°C for 48 hours, the test piece was subjected to peeling at a peeling angle of 180 degrees and a tensile speed of 60 mm / min using a tensile tester to measure the peel strength when peeling the test piece from the glass plate.

[0024] According to the specification, a film member with an adhesive sheet is provided, comprising: any adhesive sheet disclosed herein, and a film member bonded to the adhesive layer of the adhesive sheet. According to the film member with an adhesive sheet, a bond with high deformation resistance and high impact resistance can be suitably formed.

[0025] According to the specification, a method for producing a laminate is provided, which comprises: laminating any adhesive sheet disclosed herein to an adherend, and irradiating the adhesive sheet with ultraviolet light to photocuring the adhesive layer. According to the method, a laminate having both impact resistance and high deformation resistance can be produced.

[0026] It should be noted that solutions obtained by appropriately combining the above-mentioned elements may also be included in the scope of the invention sought for patent protection through this patent application. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a cross-sectional view schematically showing the structure of a pressure-sensitive adhesive sheet according to one embodiment.

[0028] Figure 2 This is a cross-sectional view schematically showing the structure of a pressure-sensitive adhesive sheet according to another embodiment.

[0029] Figure 3 This is a cross-sectional view schematically showing a film member with a pressure-sensitive adhesive sheet in which a pressure-sensitive adhesive sheet according to one embodiment is attached to a film member. DETAILED DESCRIPTION

[0030] The preferred embodiments of the present invention are described below. It should be noted that matters necessary for implementing the present invention, except for those specifically mentioned in this specification, can be understood by those skilled in the art based on the teachings on the implementation of the invention recorded in this specification and the technical common sense at the time of application. The present invention can be implemented based on the contents disclosed in this specification and the technical common sense in this field. In addition, in the following drawings, components / parts that play the same role are sometimes marked with the same symbols for description, and repeated descriptions are sometimes omitted or simplified. In addition, the embodiments described in the drawings are illustrated for the purpose of clearly explaining the present invention, and do not necessarily accurately represent the size or reduction ratio of the product actually provided.

[0031] In this specification, "acrylic polymer" refers to a polymer derived from a monomer component containing an acrylic monomer in an amount greater than 50% by weight, and also refers to an acrylic polymer. The above-mentioned acrylic monomer refers to a monomer having at least one (meth)acryloyl group in one molecule. In addition, in this specification, "(meth)acryloyl" refers generally to acryloyl and methacryloyl. Similarly, "(meth)acrylate" refers generally to acrylate and methacrylate, and "(meth)acrylic acid" refers generally to acrylic acid and methacrylic acid, respectively.

[0032] It should be noted that in this specification, “mass” and “weight” have the same meaning.

[0033] In this specification, "photoreactive monomer" refers to a compound having at least one functional group (photoreactive functional group) in the molecule that can react by light irradiation, and typically a compound having at least one ethylenically unsaturated group as the photoreactive functional group in the molecule. The photoreactive monomer referred to here can be any monomer that can react, for example, it itself can be a polymer such as an oligomer or a polymer (for example, a polymer having at least one ethylenically unsaturated group in the molecule).

[0034] <Configuration Example of Pressure-Sensitive Adhesive Sheet>

[0035] One structural example of the PSA sheet disclosed herein is shown in Figure 1The adhesive sheet 1 is constituted as a single-sided adhesive sheet (single-sided adhesive sheet with a support), and the single-sided adhesive sheet (single-sided adhesive sheet with a support) comprises: an adhesive layer 10 having one surface 10A as an adhesive surface (adhesive surface) on an adherend, and a support 20 laminated on the other surface 10B of the adhesive layer 10. The adhesive layer 10 is bonded to one surface 20A of the support 20. As the support 20, a resin film such as a polyester film can be used. The support 20 can be, for example, an optical film such as a polarizing plate. Figure 1 In the example shown, the adhesive layer 10 is a single-layer structure. The adhesive sheet 1 before use (before being attached to an adherend) may be, for example, Figure 1 The adhesive surface 10A shown is protected by a release liner 30 whose at least the adhesive layer side is a releasable surface (release surface), and the adhesive sheet 50 with a release liner is in the form. Alternatively, it can also be in the form of: the second surface 20B (the surface on the opposite side to the first surface 20A, also referred to as the back side) of the support 20 is the release surface, and the adhesive surface 10A is abutted against the second surface 20B of the support 20, thereby protecting the adhesive surface 10A.

[0036] The release liner is not particularly limited, and for example, a release liner having a release treatment on the surface of a liner substrate such as a resin film or paper, or a release liner formed of a low-adhesive material such as a fluorine-based polymer (polytetrafluoroethylene, etc.) or a polyolefin-based resin (polyethylene, polypropylene, etc.) can be used. In the above release treatment, for example, a release treatment agent such as a silicone-based or long-chain alkyl-based release agent can be used. In some embodiments, a release-treated resin film can be preferably used as the release liner.

[0037] The adhesive sheet disclosed herein may be a double-sided adhesive sheet without a support including an adhesive layer. Figure 2 As shown, for the two-sided adhesive sheet 2 without a support, before use, each surface 10A, 10B of the adhesive layer 10 can be protected by a release liner 31, 32 whose at least the adhesive layer side is a releasable surface (release surface). Alternatively, it can also be in the following form: the back side (the surface on the opposite side to the adhesive side) of the release liner 31 is the release surface, and the adhesive surface 10B is abutted against the back side of the release liner 31. The adhesive surface 10A, 10B is protected. Such a two-sided adhesive sheet without a support can be used, for example, by bonding a support to any surface of the adhesive layer.

[0038] In addition, the adhesive sheet disclosed herein may be in the form of a double-sided adhesive sheet with a support in which adhesive layers are laminated on one surface and the other surface of a sheet-like support. The support in the adhesive sheet of the above embodiment may be a resin film such as a polyester film, or an optical film such as a polarizing plate.

[0039] The adhesive sheet disclosed herein may be a constituent element of a film member with an adhesive sheet in which a film member is bonded to one surface of an adhesive layer. Figure 3 As shown, Figure 1 The adhesive sheet 1 shown may be a constituent element of a film member 100 with an adhesive sheet in which a film member 70 is bonded to one surface 10A of an adhesive layer 10. The film member may be, for example, an electromagnetic wave transparent metallic luster member, a polarizing plate, or other optical film as described in Japanese Patent Application Publication No. 2018-69462.

[0040] <Characteristics of Adhesive Sheet>

[0041] (tensile modulus)

[0042] For the adhesive sheet disclosed herein, the tensile modulus of the adhesive layer (which may be an adhesive layer formed using any adhesive composition disclosed herein) is preferably 3.0MPa or more. The above-mentioned tensile modulus is measured by the above-mentioned tensile test, and more specifically, it can be measured by the method described in the embodiments described later. The adhesive layer with a higher tensile modulus tends to show better deformation resistance. The adhesive sheet with a high tensile modulus can be suitably used for purposes such as the joining and fixing of components. For example, in a laminated body in which a component and an adherend are joined by an adhesive layer, when the deformation resistance of the adhesive layer is high, it can help to maintain the relative position of the component relative to the adherend with good precision. In addition, in a laminated body in which a film component and an adherend are joined by an adhesive layer, when the deformation resistance of the adhesive layer is high, it can help to suppress the phenomenon that the appearance of the laminated body changes due to local extrusion of the above-mentioned film component side. In the case where the above-mentioned adherend is a laminated body of a rigid component (such as a glass component) with transparency, it is particularly meaningful to suppress the appearance change recognized from the above-mentioned adherend side.

[0043] In some preferred adhesive sheets, the above-mentioned tensile modulus can be, for example, more than 5.0MPa, more than 7.0MPa, more than 10.0MPa, more than 15.0MPa, or more than 20.0MPa. By increasing the above-mentioned tensile modulus, there is a tendency to improve deformation resistance. The upper limit of the above-mentioned tensile modulus is not particularly limited. From the viewpoint of being easily obtained with other characteristics (for example, one or more characteristics selected from impact resistance, peel strength, haze value, etc.), it is advantageous that the above-mentioned tensile modulus is usually less than 150MPa, preferably less than 120MPa, less than 100MPa, less than 80MPa, or less than 60MPa. The tensile modulus can be adjusted by selecting the composition of the adhesive layer, etc.

[0044] It should be noted that the treatment of irradiating the adhesive layer with ultraviolet light in the above-mentioned tensile test is preferably carried out in a state where the above-mentioned adhesive layer is sandwiched between transparent release liners. As the above-mentioned release liner, from the viewpoint of transparency, a polyester resin film (for example, a polyethylene terephthalate resin (PET) film) with at least one side subjected to release treatment can be preferably used. Although not particularly limited, the thickness of the above-mentioned release liner can be, for example, about 10 μm or more and about 125 μm or less, can be 10 μm or more and 75 μm or less, can be 20 μm or more and 50 μm or less.

[0045] The thickness of the test piece used in the above-mentioned tensile test may be the same as the thickness of the adhesive layer constituting the adhesive sheet disclosed herein, or it may be different. For example, when the thickness of the adhesive layer constituting the adhesive sheet is relatively small, for the purpose of improving operability, the result obtained by performing the above-mentioned tensile test using a test piece prepared in a manner of 5 μm or more (for example, about 5 μm to 200 μm) can be used as the tensile modulus of the above-mentioned adhesive layer. The thickness of the test piece can be adjusted, for example, by appropriately overlapping the adhesive layer before ultraviolet irradiation. In addition, the following result can be used as the tensile modulus of the above-mentioned adhesive layer, the result of which is obtained by using the same adhesive composition as the adhesive layer used to form the object of measurement, making a test piece of a thickness that is easy to perform a tensile test, and performing the above-mentioned tensile test on the test piece. The above-mentioned tensile test can be carried out, for example, using a test piece with a thickness of about 10 μm to 50 μm (preferably a thickness of about 15 μm to 25 μm).

[0046] (Impact resistance)

[0047] The impact resistance of the PSA sheet disclosed herein is preferably 2.0 J / (10 mm) 2 The above-mentioned impact resistance is measured by the above-mentioned shear impact test, and more specifically, can be measured by the method described in the embodiments described later. According to the above-mentioned adhesive sheet with high impact resistance, a highly reliable joint can be formed. This can be an advantageous feature of an adhesive sheet used, for example, for joining and fixing components. Even if the above-mentioned adhesive sheet is subjected to an impact caused by, for example, falling, impact, etc., it can withstand the impact and maintain good bonding between the component and the adherend.

[0048] In some preferred embodiments of the adhesive sheet, the impact resistance may be, for example, 2.1 J / (10 mm). 2 Above, it can be 2.3J / (10mm) 2 Above, it can be 2.5J / (10mm) 2 Above, it can be 2.7J / (10mm) 2 Above, it can be 3.0J / (10mm) 2The adhesive sheet disclosed herein may preferably have the above-mentioned impact resistance of 3.3 J / (10 mm) 2 Above or 3.5J / (10mm) 2 The above method is implemented. There is no particular upper limit on the impact resistance. From the perspective of easily obtaining a balance with other properties, the impact resistance can be, for example, 20 J / (10 mm). 2 Below, it can be 15J / (10mm) 2 Below, it can be 10J / (10mm) 2 Below, it can be 8.0J / (10mm) 2 , can be 6.0J / (10mm) 2 The impact resistance can be adjusted by selecting the composition, thickness, etc. of the adhesive layer.

[0049] It should be noted that the adhesive sheet disclosed in this specification includes a mode in which the tensile modulus is not limited, and in such a mode, the adhesive sheet is not limited to those satisfying the above tensile modulus. Similarly, the adhesive sheet disclosed in this specification includes a mode in which the impact resistance is not limited, and in such a mode, the adhesive sheet is not limited to those satisfying the above impact resistance.

[0050] (Peel Strength)

[0051] The peel strength of the adhesive sheet disclosed herein is not particularly limited and can be set according to the purpose. The above-mentioned peel strength can be measured by the above-mentioned peel test, and more specifically, it can be measured by the method described in the embodiment described later. In some ways, the above-mentioned peel strength can be, for example, 0.5N / 10mm or more, and from the viewpoint of bonding reliability, it is preferably 1.0N / 10mm or more, more preferably 1.5N / 10mm or more, can be 2.0N / 10mm or more, can be 2.2N / 10mm or more, can be 2.3N / 10mm or more. In addition, from the viewpoint of easy acquisition of balance with other characteristics, the above-mentioned peel strength can be, for example, 10N / 10mm or less, can be 8.0N / 10mm or less, can be 6.0N / 10mm or less, can be 5.0N / 10mm or less, can be 4.0N / 10mm or less. The peel strength can be adjusted by selecting the composition, thickness, etc. of the adhesive layer.

[0052] (Haze value)

[0053] In the adhesive sheet disclosed herein, the haze value of the adhesive layer is not particularly limited. When transparency is required for the adhesive layer, the haze value of the adhesive layer may be, for example, less than 10%, less than 5.0%, less than 3.0%, or less than 1.0%. As non-limiting examples of usage requiring transparency for the adhesive layer, there can be cited a usage in which a component is joined to an adherend having transparency through an adhesive layer, and the component is identified from the adherend side through the adhesive layer; an adhesive sheet having a support is joined to an adherend having transparency, and the support is identified from the adherend side through the adhesive layer, etc. In some embodiments, the haze value of the adhesive layer may be lower than 1.0%, lower than 0.7%, or lower than 0.5% (for example, 0 to 0.5%).

[0054] The "haze value" here refers to the ratio of diffuse transmitted light to total transmitted light when the object to be measured is irradiated with visible light. It is also called haze value. The haze value can be expressed by the following formula.

[0055] Th[%]=Td / Tt×100

[0056] In the above formula, Th is the haze value [%], Td is the scattered light transmittance, and Tt is the total light transmittance.

[0057] The haze value can be measured as follows: at an illumination of 300 mW / cm 2 、Accumulated light intensity 3000mJ / cm 2 The adhesive layer is irradiated with ultraviolet rays under the conditions of , and the adhesive layer after aging at 50°C for 48 hours is used as a measurement sample, and measured using a haze meter (for example, "MR-100" manufactured by Murakami Color Technology Research Institute). The haze value can be adjusted, for example, by selecting the composition and thickness of the adhesive layer. It should be noted that the treatment of irradiating the adhesive layer with ultraviolet rays is similar to the tensile test in the above-mentioned tensile modulus measurement, and is preferably carried out in a state where the above-mentioned adhesive layer is clamped between transparent release liners (for example, PET films that have been subjected to release treatment).

[0058] <Adhesive Layer>

[0059] The adhesive sheet in the technology disclosed herein (including an adhesive sheet, a film member with an adhesive sheet, and a method for producing a laminate, the same shall apply hereinafter) comprises an adhesive layer. The composition of the adhesive layer can be selected so as to form a bond with high deformation resistance and high impact resistance.

[0060] (Polymer (A))

[0061] In some embodiments, the adhesive layer contains a polymer (A). Examples of materials that can be used as the polymer (A) include acrylic polymers, rubber polymers, polyester polymers, urethane polymers, polyether polymers, silicone polymers, polyamide polymers, fluorine polymers, and other polymers that exhibit rubber elasticity in the room temperature region and are well known in the field of adhesives. These can be used alone or in combination of two or more.

[0062] For the weight ratio of the polymer (A) shared in the overall weight of the adhesive layer, from the viewpoint of impact resistance, it is usually suitable to be more than 40 weight %, preferably more than 50 weight %, can be more than 60 weight %, can be more than 70 weight %. In addition, the weight ratio of the polymer (A) shared in the overall weight of the adhesive layer is typically lower than 100 weight %, from the viewpoint of easy adjustment of the balance of characteristics, it is usually advantageous to be less than 95 weight %, preferably less than 92 weight %, can be less than 90 weight %, can be less than 87 weight %.

[0063] As a preferred example of the polymer (A), an acrylic polymer can be cited. The adhesive layer in the technology disclosed herein can be an acrylic adhesive layer containing an acrylic polymer as a base polymer (the main component in the polymer component, that is, a component that occupies more than 50% by weight). The acrylic polymer as polymer (A) (hereinafter sometimes referred to as "acrylic polymer (A)") is preferably an acrylic polymer composed of a monomer component containing a (meth)acrylic acid alkyl ester at a ratio of more than 40% by weight, wherein the (meth)acrylic acid alkyl ester has a linear or branched alkyl group with a carbon number of 1 to 20 at the ester end. In the following, the (meth)acrylic acid alkyl ester having an alkyl group with a carbon number of more than X and less than Y at the ester end is sometimes referred to as "(meth)acrylic acid C X-Y Alkyl esters".

[0064] In some embodiments, the (meth)acrylic acid C in the total monomer components of the acrylic polymer (A) is 1-20 The proportion of the alkyl ester is preferably greater than 40% by weight, for example, 45% by weight or more, 50% by weight or more, 55% by weight or more, or 60% by weight or more, from the perspective of easily obtaining a balance of properties. 1-20 The proportion of the alkyl ester may be 100 wt %, but from the perspective of easily obtaining a balance of properties, it is usually preferably 98 wt % or less, for example, 95 wt % or less, or 90 wt % or less. In some embodiments, the proportion of (meth)acrylic acid C in the total monomer components of the acrylic polymer (A) is preferably 98 wt % or less, for example, 95 wt % or less, or 90 wt % or less. 1-20From the viewpoint of improving the aggregation of the adhesive layer, the proportion of the alkyl ester may be, for example, less than 85 wt %, less than 80 wt %, less than 75 wt %, less than 70 wt %, less than 65 wt %, or less than 60 wt %.

[0065] As (meth)acrylic acid C 1-20 Specific non-limiting examples of the alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, amyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, and the like.

[0066] Among them, it is preferred to use at least (meth)acrylic acid C 4-20 Alkyl esters, more preferably at least (meth) acrylic acid C 4-18 As particularly preferred (meth)acrylic acid C 4-18 As the alkyl ester, n-butyl acrylate (BA) and 2-ethylhexyl acrylate (2EHA) can be mentioned. 4-20 Other specific examples of alkyl esters include isononyl acrylate, n-butyl methacrylate (BMA), 2-ethylhexyl methacrylate (2EHMA), isostearyl acrylate (iSTA), and the like. 4-20 The alkyl esters may be used alone or in combination of two or more.

[0067] The above-mentioned monomer component preferably includes, for example, any one or both of n-butyl acrylate (BA) and 2-ethylhexyl acrylate (2EHA). In some embodiments, the above-mentioned monomer component preferably includes at least BA. Here, examples of monomer components containing at least BA include: monomer components containing BA but not 2EHA; monomer components containing BA and 2EHA, and a content of 2EHA less than the content of BA (for example, the content of 2EHA is less than 0.5 times or less than 0.3 times the content of BA).

[0068] In some embodiments, the monomer components constituting the acrylic polymer (A) may contain (meth)acrylic acid C in a ratio of 40% by weight or more. 4-18 Alkyl ester. (Meth) acrylic acid C in the monomer component 4-18 The ratio of the alkyl ester may be, for example, 50% by weight or more, 60% by weight or more, or 65% by weight or more.

[0069] In addition, from the viewpoint of improving the cohesiveness of the pressure-sensitive adhesive layer, (meth)acrylic acid C 4-18 The proportion of the alkyl ester in the monomer components is usually appropriately 99.5% by weight or less, and may be 95% by weight or less, 85% by weight or less, or 75% by weight or less.

[0070] The monomer components constituting the acrylic polymer (A) may include alkyl (meth)acrylates and, if necessary, other monomers (copolymerizable monomers) copolymerizable with the alkyl (meth)acrylates. As copolymerizable monomers, monomers having polar groups (e.g., carboxyl groups, hydroxyl groups, rings containing nitrogen atoms, etc.) and monomers having a relatively high glass transition temperature of the homopolymer (e.g., above 10° C.) may be preferably used. Monomers having polar groups may contribute to the introduction of crosslinking points in the acrylic polymer (A) or to the improvement of the cohesive force of the adhesive. Copolymerizable monomers may be used alone or in combination of two or more.

[0071] Specific non-limiting examples of the copolymerizable monomer include the following monomers.

[0072] Carboxyl group-containing monomers: for example, acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, isocrotonic acid, and the like.

[0073] Anhydride group-containing monomers: for example, maleic anhydride, itaconic anhydride.

[0074] Hydroxyl-containing monomers: for example, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, hydroxyalkyl (meth)acrylates such as (4-hydroxymethylcyclohexyl)methyl (meth)acrylate, and the like.

[0075] Monomers containing sulfonic acid groups or phosphoric acid groups: for example, styrene sulfonic acid, allyl sulfonic acid, sodium vinyl sulfonate, 2-(meth)acrylamide-2-methylpropanesulfonic acid, (meth)acrylamidepropanesulfonic acid, sulfopropyl (meth)acrylate, (meth)acryloyloxynaphthalenesulfonic acid, 2-hydroxyethylacryloyl phosphate, etc.

[0076] Epoxy group-containing monomers: For example, epoxy group-containing acrylates such as glycidyl (meth)acrylate and 2-ethyl glycidyl (meth)acrylate, allyl glycidyl ether, and glycidyl (meth)acrylate.

[0077] Cyano group-containing monomers: for example, acrylonitrile, methacrylonitrile, etc.

[0078] Isocyanate group-containing monomer: for example, 2-isocyanateethyl (meth)acrylate, etc.

[0079] Amide group-containing monomers: for example, (meth)acrylamide; N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N,N-dipropyl (meth)acrylamide, N,N-diisopropyl (meth)acrylamide, N,N-di(n-butyl) (meth)acrylamide, N,N-di(tert-butyl) (meth)acrylamide and the like N,N-dialkyl (meth)acrylamide; N-ethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-butyl (meth)acrylamide, N-n-butyl (meth)acrylamide and the like N-alkyl (meth)acrylamide; N-vinyl carboxylic acid amides such as N-vinyl acetamide; monomers having hydroxyl and amide groups, for example, N-(2-hydroxyethyl) (meth)acrylamide, N-(2-hydroxypropyl)(meth)acrylamide, N-(1-hydroxypropyl)(meth)acrylamide, N-(3-hydroxypropyl)(meth)acrylamide, N-(2-hydroxybutyl)(meth)acrylamide, N-(3-hydroxybutyl)(meth)acrylamide, N-(4-hydroxybutyl)(meth)acrylamide; monomers having an alkoxy group and an amide group, for example, N-alkoxyalkyl(meth)acrylamide such as N-methoxymethyl(meth)acrylamide, N-methoxyethyl(meth)acrylamide, and N-butoxymethyl(meth)acrylamide; and N,N-dimethylaminopropyl(meth)acrylamide, N-(meth)acryloylmorpholine, and the like.

[0080] Amino group-containing monomers: for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, tert-butylaminoethyl (meth)acrylate.

[0081] Monomers having an epoxy group: for example, glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, allyl glycidyl ether.

[0082] Monomers having a ring containing a nitrogen atom: for example, N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-(meth)acryloyl-2-pyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-(meth)acryloylmorpholine, N-vinylmorpholine, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, N-vinylpyrazole, N-vinylisoxazole, N-vinylthiazole, N-vinylisothiazole, N-vinylpyridazine, etc. (for example, lactams such as N-vinyl-2-caprolactam).

[0083] Monomers having a succinimide skeleton include, for example, N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, and N-(meth)acryloyl-8-oxyhexamethylenesuccinimide.

[0084] Maleimides: for example, N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, N-phenylmaleimide, etc.

[0085] Itaconimides: for example, N-methyl itaconimide, N-ethyl itaconimide, N-butyl itaconimide, N-octyl itaconimide, N-2-ethylhexyl itaconimide, N-cyclohexyl itaconimide, N-lauryl itaconimide and the like.

[0086] Aminoalkyl (meth)acrylates: for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, tert-butylaminoethyl (meth)acrylate.

[0087] Alkoxy-containing monomers: for example, alkoxyalkyl (meth)acrylates (alkoxyalkyl (meth)acrylates) such as 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, propoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, and ethoxypropyl (meth)acrylate; and alkoxyalkylene glycol (meth)acrylates (for example, alkoxypolyalkylene glycol (meth)acrylate) such as ethylene glycol methoxy (meth)acrylate, polyethylene glycol methoxy (meth)acrylate, and polypropylene glycol methoxy (meth)acrylate.

[0088] Alkoxysilyl group-containing monomers: for example, alkoxysilyl group-containing (meth)acrylates such as 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, and alkoxysilyl group-containing vinyl compounds such as vinyltrimethoxysilane and vinyltriethoxysilane.

[0089] Vinyl esters: for example, vinyl acetate, vinyl propionate, etc.

[0090] Vinyl ethers: For example, vinyl alkyl ethers such as methyl vinyl ether and ethyl vinyl ether.

[0091] Aromatic vinyl compounds: for example, styrene, α-methylphenylene, vinyltoluene, etc.

[0092] Olefins: for example, ethylene, butadiene, isoprene, isobutylene, etc.

[0093] (Meth)acrylates having an alicyclic hydrocarbon group: for example, alicyclic hydrocarbon group-containing (meth)acrylates such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentyl (meth)acrylate, and adamantyl (meth)acrylate.

[0094] (Meth)acrylates having an aromatic hydrocarbon group: for example, (meth)acrylates having an aromatic hydrocarbon group, such as phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, and benzyl (meth)acrylate.

[0095] In addition, (meth)acrylates containing heterocycles such as tetrahydrofurfuryl (meth)acrylate, (meth)acrylates containing halogen atoms such as (meth)acrylates containing vinyl chloride and fluorine atoms, (meth)acrylates containing silicon atoms such as silicone (meth)acrylate, and (meth)acrylates obtained from terpene compound derivative alcohols, etc.

[0096] When using such a copolymerizable monomer, its consumption is not particularly limited, and is usually suitable for more than 0.01% by weight of the overall monomer component. From the viewpoint of better exerting the use effect of the copolymerizable monomer, the consumption of the copolymerizable monomer can be more than 0.1% by weight of the overall monomer component, or more than 0.5% by weight. In addition, from the viewpoint of easily obtaining the balanced property of adhesive properties, the consumption of the copolymerizable monomer is usually suitable for less than 50% by weight of the overall monomer component, preferably less than 40% by weight.

[0097] In some embodiments, the monomer components constituting the acrylic polymer (A) may include a monomer having a nitrogen atom. By using a monomer having a nitrogen atom, the cohesive force of the adhesive can be increased and the peel strength after photocuring can be suitably improved. As a preferred example of a monomer having a nitrogen atom, a monomer having a ring containing a nitrogen atom can be listed. As a monomer having a ring containing a nitrogen atom, the monomers exemplified above can be used, for example, the general formula (1) can be used:

[0098]

[0099] Here, in the general formula (1), R 1 is a divalent organic group, and specific examples thereof include -(CH2) n -. Here, n is an integer of 2 to 7 (preferably 2, 3 or 4). Among them, N-vinyl-2-pyrrolidone can be preferably used. Other preferred examples of the monomer having a nitrogen atom include amide group-containing monomers such as (meth)acrylamide.

[0100] The amount of the monomer with nitrogen atoms (preferably a monomer with a ring containing nitrogen atoms) is not particularly limited, for example, it can be more than 1% by weight of the overall monomer component, it can be more than 3% by weight, and further can be more than 5% by weight or more than 7% by weight. In one embodiment, the amount of the monomer with nitrogen atoms can be more than 10% by weight of the overall monomer component, it can be more than 15% by weight, or it can be more than 20% by weight. In addition, the amount of the monomer with nitrogen atoms is suitable for, for example, less than 40% by weight of the overall monomer component, it can be less than 35% by weight, it can be less than 30% by weight, or it can be less than 25% by weight. In another embodiment, the amount of the monomer with nitrogen atoms can be, for example, less than 20% by weight of the overall monomer component, or it can be less than 15% by weight.

[0101] In some ways, the monomer components constituting the acrylic polymer (A) may include hydroxyl-containing monomers. By using hydroxyl-containing monomers, the cohesion of the adhesive and the degree of crosslinking (for example, crosslinking based on isocyanate crosslinking agent) can be appropriately adjusted. The amount used when using hydroxyl-containing monomers is not particularly limited, for example, it can be more than 0.01% by weight of the overall monomer component, it can be more than 0.1% by weight, it can be more than 0.5% by weight, it can be more than 1% by weight, it can be more than 5% by weight or more than 10% by weight. In addition, from the viewpoint of suppressing the water absorption of the adhesive layer, in some ways, the amount of hydroxyl-containing monomers is suitable for, for example, less than 40% by weight of the overall monomer component, it can be less than 30% by weight, it can be less than 25% by weight, it can be less than 20% by weight. In another way, the amount of hydroxyl-containing monomers can be less than 15% by weight of the overall monomer component, it can be less than 10% by weight, it can be less than 5% by weight.

[0102] In some embodiments, the proportion of carboxyl-containing monomers in the monomer components of acrylic polymer (A) can be, for example, less than 2% by weight, less than 1% by weight, or less than 0.5% by weight (for example, less than 0.1% by weight). As the monomer components of acrylic polymer (A), carboxyl-containing monomers can also be substantially not used. Here, substantially not using carboxyl-containing monomers means at least not intentionally using carboxyl-containing monomers. For the adhesive layer of acrylic polymer (A) containing a limited amount of carboxyl-containing monomers as described above, it is preferred from the viewpoint of preventing metal corrosion. The above-mentioned adhesive sheet with an adhesive layer can be preferably used in a manner such as that the adhesive layer is in contact with an adherend and / or a support having a metal material (which can be a support film containing a metal foil or a metal material).

[0103] In some embodiments, the monomer components constituting the acrylic polymer (A) may include (meth)acrylates containing alicyclic hydrocarbon groups. Thus, the cohesive force of the adhesive can be increased and the peel strength after photocuring can be improved. As (meth)acrylates containing alicyclic hydrocarbon groups, the above-mentioned examples can be used, for example, cyclohexyl acrylate and isobornyl acrylate can be preferably used. There is no particular restriction on the amount of (meth)acrylates containing alicyclic hydrocarbon groups, for example, it can be more than 1% by weight, more than 3% by weight or more than 5% by weight of the entire monomer component. In one embodiment, the amount of (meth)acrylates containing alicyclic hydrocarbon groups can be more than 10% by weight of the entire monomer component, and can be more than 15% by weight. It is suitable that the upper limit of the amount of (meth)acrylates containing alicyclic hydrocarbon groups is about 40% by weight or less, for example, it can be less than 30% by weight, and can be less than 25% by weight (for example, less than 15% by weight, and further less than 10% by weight).

[0104] The polymerization method for forming (synthesizing) the polymer (A) from the monomer components is not particularly limited, and various polymerization methods known in the art can be suitably used. For example, thermal polymerization such as solution polymerization, emulsion polymerization, and bulk polymerization (typically carried out in the presence of a thermal polymerization initiator); photopolymerization by irradiation with light such as ultraviolet rays (typically carried out in the presence of a photopolymerization initiator); radiation polymerization by irradiation with radiation such as β rays and γ rays; and other polymerization methods can be suitably used. It is also possible to combine two or more polymerization methods (for example, in stages) for implementation.

[0105] As the solvent (polymerization solvent) for solution polymerization, for example, any one solvent selected from aromatic compounds such as toluene (typically aromatic hydrocarbons); esters such as ethyl acetate and butyl acetate; aliphatic or alicyclic hydrocarbons such as hexane and cyclohexane; halogenated alkanes such as 1,2-dichloroethane; lower alcohols such as isopropyl alcohol (for example, monohydric alcohols having 1 to 4 carbon atoms); ethers such as tert-butyl methyl ether; ketones such as methyl ethyl ketone; etc., or a mixed solvent of two or more thereof can be used.

[0106] When the polymerization is carried out, a known or customary thermal polymerization initiator or photopolymerization initiator may be used according to the polymerization method, polymerization mode, etc. Such polymerization initiators may be used alone or in appropriate combination of two or more.

[0107] The thermal polymerization initiator is not particularly limited, and for example, an azo polymerization initiator, a peroxide initiator, a redox initiator based on a combination of a peroxide and a reducing agent, a substituted ethane initiator, and the like can be used. More specifically, for example, azo initiators such as 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis(2-methylpropionamidine) disulfate, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis(N,N'-dimethyleneisobutyramidine), and 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] hydrate; persulfates such as potassium persulfate and ammonium persulfate; peroxide initiators such as benzoyl peroxide, tert-butyl hydroperoxide, and hydrogen peroxide; substituted ethane initiators such as phenyl-substituted ethane; redox initiators such as a combination of a persulfate and sodium bisulfite and a combination of a peroxide and sodium ascorbate; etc., but the present invention is not limited to these. Thermal polymerization can be suitably performed at a temperature of, for example, about 20 to 100° C. (typically, 40 to 80° C.), but the present invention is not limited thereto.

[0108] The photopolymerization initiator is not particularly limited, and for example, ketal-based photopolymerization initiators, acetophenone-based photopolymerization initiators, benzoin ether-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, α-ketol-based photopolymerization initiators, aromatic sulfonyl chloride-based photopolymerization initiators, photoactive oxime-based photopolymerization initiators, benzoin-based photopolymerization initiators, benzil-based photopolymerization initiators, benzophenone-based photopolymerization initiators, thioxanthone-based photopolymerization initiators, etc. can be used.

[0109] The amount of the polymerization initiator used may be a normal amount corresponding to the polymerization method, polymerization mode, etc., and is not particularly limited. For example, about 0.001 to 5 parts by weight (typically about 0.01 to 2 parts by weight, for example about 0.01 to 1 part by weight) of the polymerization initiator may be used relative to 100 parts by weight of the monomer to be polymerized.

[0110] In the above polymerization, various chain transfer agents known in the past (also understood as molecular weight regulators or polymerization degree regulators) can be used as needed. As chain transfer agents, thiols such as n-dodecyl mercaptan, tert-dodecyl mercaptan, thioglycolic acid, and α-thioglycerol can be used. Alternatively, a chain transfer agent that does not contain a sulfur atom (non-sulfur chain transfer agent) can be used. Specific examples of non-sulfur chain transfer agents include: anilines such as N,N-dimethylaniline and N,N-diethylaniline; terpenes such as α-pinene and terpinolene; styrenes such as α-methylstyrene and α-methylstyrene dimer; compounds having benzylidene acetone, cinnamyl alcohol, cinnamaldehyde, etc.; hydroquinones such as hydroquinone and dihydroxynaphthalene; quinones such as benzoquinone and naphthoquinone; olefins such as 2,3-dimethyl-2-butene and 1,5-cyclooctadiene; alcohols such as phenol, benzyl alcohol, and allyl alcohol; benzyl hydrogens such as diphenylbenzene and triphenylbenzene; etc. The chain transfer agent may be used alone or in combination of two or more. The technology disclosed herein can be preferably implemented without using a chain transfer agent.

[0111] When a chain transfer agent is used, the amount used may be, for example, about 0.005 to 1 part by weight relative to 100 parts by weight of the monomer component. In some embodiments, from the viewpoint of impact resistance, the amount of the chain transfer agent used may be, for example, 0.01 parts by weight or more, 0.03 parts by weight or more, 0.05 parts by weight or more, or 0.07 parts by weight or more relative to 100 parts by weight of the monomer component. In addition, in some embodiments, from the viewpoint of deformation resistance, the amount of the chain transfer agent used may be, for example, less than 0.5 parts by weight, less than 0.2 parts by weight, less than 0.1 parts by weight, or less than 0.1 parts by weight (for example, less than 0.09 parts by weight).

[0112] In the technology disclosed herein, the glass transition temperature (Tg) of the polymer (A) is not particularly limited, and it is usually suitable to be lower than 0°C, preferably lower than -10°C, and preferably lower than -20°C. By lowering the Tg of the polymer (A), there is a tendency to improve the above-mentioned impact resistance. In some embodiments, the Tg of the polymer (A) may be lower than -25°C, and may be lower than -30°C. In addition, the Tg of the polymer (A) is typically above -80°C, for example, it may be above -70°C, it may be above -60°C, and it may be above -55°C. From the viewpoint of improving the above-mentioned tensile modulus, in some embodiments, the Tg of the polymer (A) is preferably above -50°C, more preferably above -45°C, it may be above -40°C, it may be above -38°C, and it may be above -35°C.

[0113] Here, in this specification, the Tg of a polymer refers to the Tg obtained by the Fox equation based on the composition of the monomer components used in the preparation of the polymer. As shown below, the Fox equation is a relationship between the Tg of a copolymer and the glass transition temperature Tgi of a homopolymer obtained by homopolymerizing the monomers constituting the copolymer.

[0114] 1 / Tg=Σ(Wi / Tgi)

[0115] In the above Fox formula, Tg represents the glass transition temperature of the copolymer (unit: K), Wi represents the weight fraction of monomer i in the copolymer (copolymerization ratio based on weight), and Tgi represents the glass transition temperature of the homopolymer of monomer i (unit: K). When the polymer of the specific object of Tg is a homopolymer, the Tg of the homopolymer is consistent with the Tg of the target polymer.

[0116] As the glass transition temperature of the homopolymer used for calculation of Tg, the value described in the known document is used. For example, regarding the monomers listed below, as the glass transition temperature of the homopolymer of the monomer, the following value is used.

[0117]

[0118] Regarding the glass transition temperature of homopolymers of monomers other than those exemplified above, the values ​​described in "Polymer Handbook" (3rd edition, John Wiley & Sons, Inc., 1989) were used. When a plurality of values ​​were described in the document, the highest value was adopted.

[0119] The weight average molecular weight (Mw) of the polymer (A) is not particularly limited. From the viewpoint of achieving good balance between deformation resistance and impact resistance, in some embodiments, the Mw of the polymer (A) is, for example, about 10×10 4 The above are suitable, preferably more than 20×10 4, can exceed 30×10 4 , can exceed 40×10 4 , can exceed 50×10 4 In addition, the upper limit of the Mw of polymer (A) can usually be about 500×10 4 From the viewpoint of adhesion to the adherend and peel strength, in some embodiments, the Mw of the polymer (A) may be, for example, 150×10 4 Below, it can be 100×10 4 Below, it can be 90×10 4 Below, it can be 75×10 4 Herein, Mw refers to the value converted to standard polystyrene obtained by gel permeation chromatography (GPC). As a GPC device, for example, the model name "HLC-8320GPC" (column: TSKgel GMH-H (S), manufactured by Tosoh Corporation) can be used. The same is true in the embodiments described later. The examples of the above Mw can be used for the Mw of the polymer (A) in the adhesive layer of the adhesive sheet disclosed herein, and can also be used for the Mw of the polymer (A) in the adhesive composition used to form the adhesive layer.

[0120] (Photoreactive monomer (B))

[0121] The adhesive layer in the technology disclosed herein may contain a photoreactive monomer (B) in addition to the polymer (A) as described above (for example, an acrylic polymer (A)). As the photoreactive monomer (B), a compound having a number of ethylenically unsaturated groups contained in the molecule (hereinafter also referred to as "functional group number") of 2 or more can be used. The upper limit of the number of functional groups of the compound used as the photoreactive monomer (B) is not particularly limited. The above-mentioned number of functional groups may be, for example, 50 or less, 40 or less, 30 or less, 20 or less, or 15 or less. In some embodiments, a compound having an ethylenically unsaturated group having a functional group number of, for example, 2 to 10 can be used, preferably a compound having a functional group number of 2 to 8, and more preferably a compound having a functional group number of 2 to 6. The photoreactive monomer (B) may be used alone or in combination of two or more.

[0122] The photoreactive monomer (B) contained in the adhesive layer is attached to the adherend and then irradiated with light (e.g., ultraviolet rays) to react the above-mentioned ethylenically unsaturated groups, thereby forming a cross-linked structure. The adhesive sheet containing the photoreactive monomer (B) in the adhesive layer is attached to the adherend and then irradiated with ultraviolet rays to cure the adhesive layer, thereby improving the deformation resistance of the adhesive layer. Thus, it is possible to appropriately take into account the good followability to the surface shape of the adherend when attached to the adherend and the high deformation resistance after attachment.

[0123] Examples of the above-mentioned ethylenically unsaturated groups include, but are not limited to, acryloyl, methacryloyl, vinyl and allyl groups. The two or more ethylenically unsaturated groups in the photoreactive monomer (B) may be the same groups as each other or may be two or more different groups. From the viewpoint of photoreactivity, preferred ethylenically unsaturated groups include acryloyl and methacryloyl. Among them, acryloyl is preferred.

[0124] The functional group equivalent of the compound used as the photoreactive monomer (B) is not particularly limited. The functional group equivalent can be, for example, about 50 to 10,000 g / mol, about 50 to 8,000 g / mol, about 50 to 5,000 g / mol, about 50 to 3,000 g / mol, or about 50 to 2,000 g / mol. In some embodiments, as the photoreactive monomer (B), from the viewpoint of photocurability, a compound having a functional group equivalent of about 60 to 800 g / mol (more preferably about 80 to 600 g / mol) can be preferably used.

[0125] It should be noted that the functional group equivalent of the photoreactive monomer (B) can be calculated by dividing the molecular weight [g / mol] of the photoreactive monomer (B) by the number of ethylenically unsaturated functional groups possessed by the photoreactive monomer (B). The molecular weight of the photoreactive monomer (B) can be obtained, for example, in the form of a weight average molecular weight converted to standard polystyrene by gel permeation chromatography (GPC). In addition, as the molecular weight [g / mol] of the photoreactive monomer (B), the manufacturer's nominal value or the molecular weight calculated from the molecular structure can also be used.

[0126] The molecular weight of the photoreactive monomer (B) is not particularly limited and can be selected in a manner that suitably exerts the desired effect. For example, as the photoreactive monomer (B), a monomer having a molecular weight of about 20,000 or less can be used. From the viewpoint of the ease of preparation and coating of the adhesive composition, in some embodiments, the molecular weight of the photoreactive monomer (B) can be, for example, less than 16,000, less than 10,000, less than 4,000, less than 1,500, or less than 1,000. The molecular weight of the photoreactive monomer (B) is, for example, more than 100, typically more than 120. From the viewpoint of the processability and handling of the adhesive sheet, in some embodiments, the molecular weight of the photoreactive monomer (B) can be, for example, more than 150, more than 200, more than 280, more than 350, more than 420, more than 480, or more than 550.

[0127] In the adhesive sheet disclosed herein, the amount of the photoreactive monomer (B) contained in the adhesive layer is not particularly limited and can be appropriately set according to the target performance (e.g., the tensile modulus of the adhesive layer after photocuring). In some embodiments in which the adhesive layer comprises a polymer (A) and a photoreactive monomer (B), the amount of the photoreactive monomer (B) can be, for example, 1 part by weight or more, and usually 3 parts by weight or more is suitable relative to 100 parts by weight of the polymer (A) contained in the adhesive layer. From the viewpoint of easily improving the tensile modulus of the adhesive layer after photocuring, the amount of the photoreactive monomer (B) can be 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, or 20 parts by weight or more relative to 100 parts by weight of the polymer (A). In addition, from the viewpoint of the agglomeration of the adhesive layer before photocuring and the handleability (e.g., processability) of the adhesive sheet, the amount of the photoreactive monomer (B) is generally suitable to be 80 parts by weight or less, preferably 60 parts by weight or less, and can be 50 parts by weight or less, 40 parts by weight or less, or 35 parts by weight or less, relative to 100 parts by weight of the polymer (A).

[0128] In some embodiments, the adhesive layer preferably contains at least a compound B1 having a ring structure and two or more ethylenically unsaturated groups in the molecule as the photoreactive monomer (B). According to the adhesive layer of the compound B1 containing such a structure, the deformation resistance of the adhesive layer can be effectively improved by light irradiation. The ring in the ring structure can be an aliphatic ring or an aromatic ring. In addition, the ring can be a carbocyclic ring or a heterocyclic ring. The number of rings contained in a molecule of compound B1 can be 1 or more than 2. The upper limit of the number of rings contained in compound B1 is not particularly limited, for example, it can be less than 100, less than 70, less than 50, less than 30, less than 15, less than 8, less than 6, less than 5, or less than 4. When compound B1 contains more than 2 rings, these rings optionally form or do not form a condensed ring (typically, a dicyclic or tricyclic condensed ring) formed by 1 or more rings. The above ring is preferably contained in the main chain of compound B1. That is, it is preferred that one ethylenically unsaturated group of compound B1 is linked to at least one other ethylenically unsaturated group via the ring structure. Compound B1 may be used alone or in combination of two or more.

[0129] As compound B1, it is preferred to use a compound having a ring structure and two or more ethylenically unsaturated groups in the molecule and a functional group equivalent of 100 g / mol or more. According to the adhesive sheet containing the compound B1 satisfying the above functional group equivalent in the adhesive layer, it is possible to suitably form a joint with high deformation resistance and high impact resistance. As the reason for obtaining such an effect, there is no special limiting explanation, but it can be considered that: according to compound B1, due to the rigidity of the ring structure, the tensile modulus of the adhesive layer after light irradiation is effectively improved and deformation resistance can be given, on the other hand, by making the functional group equivalent of the compound B1 more than the specified, and maintaining the distance between the crosslinking points, a crosslinked structure with high impact resistance can be formed. In some ways, the functional group equivalent of compound B1 can be, for example, more than 120 g / mol, more than 150 g / mol, more than 180 g / mol, more than 230 g / mol, more than 280 g / mol, more than 320 g / mol, and more than 350 g / mol. As the functional group equivalent of compound B1 increases, there is a tendency for impact resistance to be improved. In addition, the functional group equivalent of compound B1 can be, for example, less than 10000g / mol, less than 8000g / mol, less than 5000g / mol, less than 3000g / mol, less than 2000g / mol. In some ways, from the viewpoint of photocurability, the functional group equivalent of compound B1 is preferably less than 800g / mol, more preferably less than 600g / mol. In some ways, the functional group equivalent of compound B1 can be less than 500g / mol, less than 400g / mol, less than 300g / mol.

[0130] In some embodiments, the number of functional groups of compound B1 (i.e., the number of ethylenically unsaturated groups contained in the molecule) can be, for example, 2 to 50, 2 to 40, 2 to 30, or 2 to 10, for example, preferably 2 to 6, 2 to 4, or 2 to 3. In some embodiments, compound B1 having a functional group number of 2 can be preferably used.

[0131] Compound B1 may have a functional group other than an ethylenically unsaturated group. Examples of the functional group other than an ethylenically unsaturated group include a hydroxyl group, a carboxyl group, an amino group, etc. Preferred examples of the functional group other than an ethylenically unsaturated group include a hydroxyl group and an amino group.

[0132] Examples of compound B1 include bisphenol A glycidyl ether (meth) acrylic acid adducts, bisphenol A glycidyl amine (meth) acrylic acid adducts, bisphenol A glycidyl ester (meth) acrylic acid adducts, and the like, bisphenol A type epoxy (meth) acrylates; ethylene oxide (EO)-modified bisphenol A di(meth) acrylates, propylene oxide (PO)-modified bisphenol A di(meth) acrylates, and the like, alkylene oxide-modified bisphenol A (meth) acrylates; bisphenol F glycidyl ether (meth) acrylic acid adducts, bisphenol F glycidyl amine (meth) acrylic acid adducts, bisphenol F glycidyl ester (meth) acrylic acid adducts, and the like, bisphenol F type epoxy (meth) acrylates; E O-modified bisphenol F di(meth)acrylate, PO-modified bisphenol F di(meth)acrylate, etc., alkylene oxide-modified bisphenol F (meth)acrylate; bisphenol E glycidyl ether (meth)acrylate adduct, bisphenol E glycidyl amine (meth)acrylate adduct, bisphenol E glycidyl ester (meth)acrylate adduct, etc., bisphenol E type epoxy (meth)acrylate; EO-modified bisphenol E di(meth)acrylate, PO-modified bisphenol E di(meth)acrylate, etc., alkylene oxide-modified bisphenol E (meth)acrylate; 9,9-bis(4-hydroxyphenyl)fluorene di(meth)acrylate, 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene di(meth)acrylate Acrylates, (meth)acrylates containing a fluorene skeleton; (meth)acrylates having an aliphatic ring (which may be an alicyclic condensed ring) such as tricyclodecane dimethanol di(meth)acrylate, hydrogenated bisphenol A epoxy (meth)acrylate, hydrogenated bisphenol F epoxy (meth)acrylate, hydrogenated bisphenol E epoxy (meth)acrylate, hydrogenated phthalic acid epoxy (meth)acrylate, hydrogenated terpene phenol (meth)acrylate, 1,4-cyclohexanedimethanol diglycidyl ether (meth)acrylate, etc.; (meth)acrylate adducts of novolac epoxy resins; (meth)acrylate adducts of thioether epoxy resins; (meth)acrylate adducts of naphthalene epoxy resins. Acrylic acid adduct; (meth) acrylic acid adduct of dicyclopentadiene type epoxy resin; (meth) acrylic acid adduct of alkyl diphenol type epoxy resin; (meth) acrylic acid adduct of biphenyl type epoxy resin; (meth) acrylic acid adduct of terpene phenol resin; tris (2-hydroxyethyl) isocyanurate di (meth) acrylate, tris (2-hydroxyethyl) isocyanurate tri (meth) acrylate, etc., isocyanurate type (meth) acrylate; divinylbenzene; hydroquinone di (meth) acrylate; resorcinol di (meth) acrylate; modified products of any of the above materials (such as amine modified products, acid modified products, halogen modified products); etc., but not limited to these. In some embodiments, compound B1 having an aromatic carbocyclic ring can be preferably used.Preferred examples of compound B1 include compounds containing a bisphenol A structure, such as bisphenol A epoxy (meth)acrylate, alkylene oxide-modified bisphenol A (meth)acrylate, and modified products thereof (eg, amine-modified products).

[0133] Commercially available products that can be used as compound B1 include, but are not limited to, "A-DCP" and "A-BPE-4" manufactured by Shin-Nakamura Chemical Industry, "Viscoa#540" and "Viscoa#700HV" manufactured by Osaka Organic Chemical Industry, "R-114F" manufactured by Nippon Kayaku, "Epoxy Ester 3000A" and "Epoxy Ester 80MFA" manufactured by Kyoeisha Chemical, and "EBECRYL 3700", "EBECRYL 3703" and "EBECRYL 3603" manufactured by DaicelOrnex Co., Ltd.

[0134] Relative to 100 parts by weight of the polymer (A) contained in the adhesive layer, the amount of compound B1 is not particularly limited, for example, it can be 0.5 parts by weight or more. From the viewpoint of easily obtaining an adhesive layer that is well balanced and takes into account both deformation resistance and impact resistance, in some ways, relative to 100 parts by weight of polymer (A), the amount of compound B1 can be, for example, more than 1 part by weight, more than 3 parts by weight, more than 5 parts by weight, more than 7 parts by weight, more than 10 parts by weight, or more than 15 parts by weight. In addition, from the viewpoint of the agglomeration of the adhesive layer before photocuring and the handling of the adhesive sheet, relative to 100 parts by weight of polymer (A), the amount of compound B1 is usually suitable for less than 80 parts by weight, preferably less than 60 parts by weight, less than 50 parts by weight, less than 40 parts by weight, or less than 35 parts by weight.

[0135] In some embodiments, the adhesive layer may also include a compound B2 having a functional group number of 2 or more and having no ring structure in the molecule as the photoreactive monomer (B). Compound B2 is preferably used in combination with compound B1. Thus, the cross-linked structure of the adhesive layer can be adjusted, and a more suitable bonding that takes into account both deformation resistance and impact resistance can be formed. Compound B2 can be used alone or in combination of two or more.

[0136] The number of functional groups of compound B2 may be, for example, 50 or less, 40 or less, 30 or less, 20 or less, or 15 or less. The number of functional groups of compound B2 used in some embodiments may be, for example, 2 to 10, preferably 3 to 10, 3 to 8, or 4 to 6. For example, in an embodiment in which a compound having a functional group number of 2 is used as compound B1, it may be advantageous to use compound B2 having a functional group number of 3 or more (preferably 4 or more, more preferably 5 or more, and further preferably 6 or more).

[0137] The functional group equivalent of compound B2 is not particularly limited, for example, it can be less than 5000g / mol, less than 2000g / mol, or less than 1000g / mol. In some ways, the functional group equivalent of compound B2 can be, for example, less than 600g / mol, from the viewpoint of improving photocurability, hardness of cured product, etc., it can be less than 400g / mol, less than 300g / mol, less than 200g / mol, less than 150g / mol, or less than 100g / mol. The functional group equivalent of compound B2 is typically more than 50g / mol, preferably more than 60g / mol, more than 70g / mol, more than 80g / mol, or more than 90g / mol.

[0138] Examples of compounds that can be used as compound B2 include: pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, trimethylolethane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, neopentyl glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, allyl (meth)acrylate, vinyl (meth)acrylate, EO modified products of any of the above materials, PO modified products, etc., but are not limited to these.

[0139] In the method of using compound B2, the amount of compound B2 is not particularly limited relative to 100 parts by weight of the polymer (A) contained in the adhesive layer, and for example, it can be more than 0.1 parts by weight. From the viewpoint of easily obtaining an adhesive layer that is well balanced and takes into account both deformation resistance and impact resistance, in some ways, relative to 100 parts by weight of polymer (A), the amount of compound B2 can be, for example, more than 1 part by weight, more than 2 parts by weight, more than 4 parts by weight, more than 6 parts by weight, more than 10 parts by weight, or more than 12 parts by weight. In addition, from the viewpoint of suppressing the adhesion to the adherend caused by excessive cross-linking, in some ways, relative to 100 parts by weight of polymer (A), the amount of compound B2 is, for example, suitable for less than 25 parts by weight, preferably less than 17 parts by weight, less than 15 parts by weight, less than 13 parts by weight, or less than 9 parts by weight.

[0140] In the method of using compound B1 and compound B2 in combination, as compound B2, a compound having a functional group equivalent less than the functional group equivalent of compound B1 having a functional group number of 3 or more and used in combination therewith can be preferably used. In some methods, the ratio (FE2 / FE1) of the functional group equivalent FE2 of compound B2 relative to the functional group equivalent FE1 of compound B1 can be, for example, less than 0.9, less than 0.7, less than 0.5, or less than 0.4. According to the above method, the tensile modulus improvement effect brought by the photoreactive monomer (B) can be effectively exerted. The lower limit of the above ratio (FE2 / FE1) is not particularly limited, for example, it can be more than 0.01, more than 0.1, or more than 0.2.

[0141] In the method of using compound B1 and compound B2 in combination, the weight ratio (W2 / W1) of the amount W2 of compound B2 to the amount W1 of compound B1 is not particularly limited. In some embodiments, the weight ratio (W2 / W1) can be, for example, 0.05 to 10, 0.1 to 5, 0.2 to 3, or 0.3 to 2. By making the weight ratio (W2 / W1) any range among the above, there is a tendency to appropriately exert the effect of using compound B1 and compound B2 in combination.

[0142] In some embodiments of the adhesive sheet disclosed herein, the photoreactive monomer (B) may be contained in the adhesive layer in a free form. The above-mentioned adhesive layer can be suitably formed by using an adhesive composition containing the photoreactive monomer (B) in a free form. Here, "free form" means that the photoreactive monomer (B) is not chemically bonded to other components (e.g., polymer (A)) contained in the adhesive layer or adhesive composition. From the viewpoint of ease of preparation and suppression of gelation, an adhesive composition containing a photoreactive monomer (B) in a free form can become advantageous.

[0143] In some other aspects of the adhesive sheet disclosed herein, from the viewpoint of improving the processability of the adhesive sheet, at least a portion of the photoreactive monomer (B) may be contained in the adhesive layer in a chemically bonded manner with other components (e.g., polymer (A), a crosslinking agent described below, etc.) contained in the adhesive layer or adhesive composition. The chemical bonding may be, for example, a bonding formed by the reaction of a functional group F1 other than an ethylenically unsaturated group in the molecule of the photoreactive monomer (B) with a functional group F2 in the molecule of the other component, i.e., a functional group that can react with the functional group F1. The other component may be a crosslinking agent, and the photoreactive monomer (B) may be bonded to the polymer (A) through the crosslinking agent.

[0144] (Acrylic oligomer)

[0145] In the adhesive layer of the adhesive sheet disclosed herein, from the viewpoint of improving cohesion, improving adhesion to the surface adjacent to the adhesive layer (for example, the surface of the support in the adhesive sheet, the surface of the adherend to which the adhesive sheet is attached, etc.), an acrylic acid oligomer may be contained. The adhesive layer containing the acrylic acid oligomer may be suitably formed using an adhesive composition containing the acrylic acid oligomer. As the acrylic acid oligomer, a person having a Tg higher than the Tg of the above-mentioned polymer (A) may be preferably used.

[0146] The Tg of the acrylic oligomer is not particularly limited, and can be, for example, about 20°C or more and 300°C or less. The Tg can be, for example, about 30°C or more, about 40°C or more, about 60°C or more, about 80°C or more, or about 100°C or more. When the Tg of the acrylic oligomer becomes higher, there is a tendency that the effect of improving the cohesive force is generally increased. In addition, from the viewpoint of anchoring with the support, impact absorption, etc., the Tg of the acrylic oligomer can be, for example, about 250°C or less, about 200°C or less, about 180°C or less, or about 150°C or less. It should be noted that the Tg of the acrylic oligomer is the same as the Tg of the polymer (A), and is a value calculated based on the Fox formula.

[0147] The Mw of acrylic acid oligomer is not particularly limited, for example, can be about more than 1000, usually about more than 1500 is suitable, can be about more than 2000, can be about more than 3000. In addition, the Mw of acrylic acid oligomer can be, for example, less than about 30000, usually less than about 10000 is suitable, can be less than about 7000, can be less than about 5000. When Mw is within the above range, it is easy to suitably play the effect of improving the aggregation of adhesive layer and the adhesion of adjacent faces. The Mw of acrylic acid oligomer can be measured by gel permeation chromatography (GPC) and calculated as the value of standard polystyrene. Specifically, for example, in the HPLC8020 made by Tosoh Corporation, TSKgel GMH-H (20) × 2 roots can be used as columns, and tetrahydrofuran solvent is utilized to measure under the condition of flow velocity of about 0.5mL / minute.

[0148] Examples of the monomer components constituting the acrylic oligomer include the following (meth)acrylate monomers: the various (meth)acrylate monomers described above; 1-20 Alkyl esters; the above-mentioned various alicyclic hydrocarbon group-containing (meth)acrylates; the above-mentioned various aromatic hydrocarbon group-containing (meth)acrylates; (meth)acrylates obtained from terpene compound derivative alcohols, etc. These can be used alone or in combination of two or more.

[0149] From the viewpoint of improving adhesiveness, the acrylic oligomer preferably contains, as monomer units, acrylic monomers having a relatively bulky structure, such as (meth) alkyl esters having a branched alkyl group, such as isobutyl (meth) acrylate and tert-butyl (meth) acrylate; (meth) acrylates containing alicyclic hydrocarbon groups; (meth) acrylates containing aromatic hydrocarbon groups. In addition, when ultraviolet rays are used when synthesizing acrylic oligomers or when forming adhesive layers, monomers having a saturated hydrocarbon group at the ester terminal are preferred from the viewpoint of not easily causing polymerization inhibition, such as (meth) alkyl esters having a branched alkyl group and (meth) acrylates containing saturated alicyclic hydrocarbon groups.

[0150] The proportion of the (meth)acrylate monomer in all monomer components constituting the acrylic oligomer is typically more than 50% by weight, preferably 60% by weight or more, more preferably 70% by weight or more (e.g. 80% by weight or more, and further 90% by weight or more). In a preferred embodiment, the acrylic oligomer has a monomer composition consisting essentially of only one or more (meth)acrylate monomers. For example, the monomer components constituting the acrylic oligomer include a (meth)acrylate containing an alicyclic hydrocarbon group and (meth)acrylic acid C 1-20In some embodiments, the weight ratio of alicyclic hydrocarbon group-containing (meth)acrylate / (meth)acrylate C 1-20 The weight ratio of the alkyl ester may be, for example, 10 / 90 or more, 20 / 80 or more, or 30 / 70 or more, and may be 90 / 10 or less, 80 / 20 or less, or 70 / 30 or less.

[0151] As the monomer components constituting the acrylic oligomer, in addition to the above-mentioned (meth) acrylate monomers, monomers containing functional groups can also be used as needed. As monomers containing functional groups, monomers having heterocyclic rings containing nitrogen atoms such as N-vinyl-2-pyrrolidone and N-acryloylmorpholine; monomers containing amino groups such as (meth) acrylic acid N,N-dimethylaminoethyl ester; monomers containing amide groups such as N,N-diethyl (meth)acrylamide; monomers containing carboxyl groups such as acrylic acid (AA) and methacrylic acid (MAA); hydroxyl-containing monomers such as (meth) 2-hydroxyethyl acrylate. These monomers containing functional groups can be used alone or in combination of two or more. When using monomers containing functional groups, the proportion of monomers containing functional groups in all monomer components constituting the acrylic oligomer can be, for example, 1% by weight or more, 2% by weight or more, or 3% by weight or more, and can be, for example, 15% by weight or less, 10% by weight or less, or 7% by weight or less. The acrylic oligomer can be one that does not use monomers containing functional groups.

[0152] Preferred acrylic oligomers include, for example, homopolymers of dicyclopentanyl methacrylate (DCPMA), cyclohexyl methacrylate (CHMA), isobornyl methacrylate (IBXMA), isobornyl acrylate (IBXA), dicyclopentanyl acrylate (DCPA), 1-adamantyl methacrylate (ADMA), and 1-adamantyl acrylate (ADA); copolymers of DCPMA and MMA, copolymers of DCPMA and IBXMA, copolymers of ADA and methyl methacrylate (MMA), copolymers of CHMA and isobutyl methacrylate (IBMA), copolymers of CHMA and IBXMA, copolymers of CHMA and acryloylmorpholine (ACMO), copolymers of CHMA and diethylacrylamide (DEAA), and copolymers of CHMA and AA.

[0153] The acrylic oligomer can be formed by polymerizing its constituent monomer components. The polymerization method and polymerization mode are not particularly limited, and various conventionally known polymerization methods (e.g., solution polymerization, emulsion polymerization, bulk polymerization, photopolymerization, radiation polymerization, etc.) can be used in an appropriate manner. The type of polymerization initiator (e.g., azo polymerization initiator) that can be used as required is as exemplified in the synthesis of acrylic polymer (A), and the amount of polymerization initiator and the amount of chain transfer agent (e.g., thiol) that can be used are appropriately set based on technical common sense in order to obtain the desired molecular weight, and therefore detailed description is omitted.

[0154] When an acrylic acid oligomer is contained in an adhesive layer or an adhesive composition, its content is relative to 100 parts by weight of polymer (A), for example, it can be more than 0.01 parts by weight, from the viewpoint of obtaining a higher effect, it can be more than 0.05 parts by weight, it can be more than 0.1 parts by weight or more than 0.2 parts by weight. In addition, from the viewpoint of compatibility with polymer (A), relative to 100 parts by weight of polymer (A), it is suitable that the content of acrylic acid oligomer is usually less than 50 parts by weight, preferably less than 30 parts by weight, more preferably less than 25 parts by weight, for example, less than 10 parts by weight, less than 5 parts by weight or less than 1 part by weight. It can also be an adhesive layer or adhesive composition that does not contain an acrylic acid oligomer.

[0155] The adhesive layer or adhesive composition of the adhesive sheet disclosed herein may contain various additives commonly used in the field of adhesives such as tackifier resins (e.g., rosin-based, petroleum-based, terpene-based, phenol-based, ketone-based tackifier resins), viscosity modifiers (e.g., thickeners), leveling agents, plasticizers, fillers, pigments, dyes and other colorants, stabilizers, preservatives, anti-aging agents as other optional components as needed. For such various additives, conventionally known substances can be used, and since no special features are given to the present invention, detailed description is omitted.

[0156] It should be noted that the technology disclosed herein can exert good bonding force without using the above-mentioned tackifying resin. Therefore, in some ways, the content of the above-mentioned tackifying resin in the above-mentioned adhesive layer or adhesive composition is relative to 100 parts by weight of polymer (A), for example, can be less than 10 parts by weight, and then can be less than 5 parts by weight. The content of the above-mentioned tackifying resin can be less than 1 part by weight (for example, less than 0.5 parts by weight), and can be less than 0.1 parts by weight (more than 0 parts by weight and less than 0.1 parts by weight). The above-mentioned adhesive layer or adhesive composition may not include tackifying resin.

[0157] When the adhesive sheet disclosed herein is used for optical purposes, the adhesive layer of the adhesive sheet can have a specified optical property (such as transparency). From the viewpoint of such optical properties, it is preferred that the amount of the polymer (A) and the components other than the above-mentioned photoreactive monomer (B) used as needed in the adhesive layer (or even the adhesive composition for forming the adhesive layer) is limited. In the technology disclosed herein, the amount of the components other than the polymer (A) and the photoreactive monomer (B) in the adhesive layer is usually about 30% by weight or less, about 15% by weight or less is suitable, and preferably about 12% by weight or less (for example, about 10% by weight or less). In a method of adhesive sheet, the amount of the components other than the polymer (A) and the photoreactive monomer (B) in the adhesive layer can be about 5% by weight or less, can be about 3% by weight or less, and can be about 1.5% by weight or less (for example, about 1% by weight or less).

[0158] (Crosslinking agent)

[0159] A cross-linking agent can be used as needed in the adhesive layer. In the adhesive sheet disclosed herein, the cross-linking agent is typically contained in the adhesive layer in the form after the cross-linking reaction. By using a cross-linking agent, the cohesion of the adhesive layer can be appropriately adjusted. In addition, in the adhesive sheet containing a photoreactive monomer (B) in the adhesive layer, a cross-linking agent and a photoreactive monomer (B) are used in combination, so that the flexibility of the adhesive layer before the photocuring of the above-mentioned photoreactive monomer and the deformation resistance of the adhesive layer after the photocuring can be appropriately taken into account.

[0160] The type of crosslinking agent is not particularly limited, and can be selected from conventionally known crosslinking agents, for example, in a manner that the crosslinking agent exerts an appropriate crosslinking function in the adhesive layer according to the composition of the adhesive composition. As usable crosslinking agents, isocyanate crosslinking agents, epoxy crosslinking agents, oxazoline crosslinking agents, aziridine crosslinking agents, carbodiimide crosslinking agents, melamine crosslinking agents, urea crosslinking agents, metal alkoxide crosslinking agents, metal chelate crosslinking agents, metal salt crosslinking agents, hydrazine crosslinking agents, amine crosslinking agents, etc. can be exemplified. These can be used alone or in combination of two or more.

[0161] As the isocyanate crosslinking agent, a polyfunctional isocyanate compound having two or more functions can be used. For example, aromatic isocyanates such as toluene diisocyanate, xylene diisocyanate, polymethylene polyphenyl diisocyanate, tris(p-isocyanatephenyl)thiophosphate, and diphenylmethane diisocyanate; alicyclic isocyanates such as isophorone diisocyanate; aliphatic isocyanates such as hexamethylene diisocyanate; and the like can be cited. Examples of commercially available products include isocyanate adducts such as trimethylolpropane / toluene diisocyanate trimer adduct (manufactured by Tosoh Corporation, trade name “Coronate L”), trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Tosoh Corporation, trade name “Coronate HL”), isocyanurate of hexamethylene diisocyanate (manufactured by Tosoh Corporation, trade name “Coronate HX”), and trimethylolpropane / xylylene diisocyanate adduct (manufactured by Mitsui Chemicals, Inc., trade name “TAKENATE D-110N”).

[0162] As the epoxy crosslinking agent, a substance having two or more epoxy groups in one molecule can be used without particular limitation. An epoxy crosslinking agent having 3 to 5 epoxy groups in one molecule is preferred. Specific examples of epoxy crosslinking agents include N,N,N',N'-tetraglycidyl meta-xylylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, polyethylene glycol diglycidyl ether, polyglycerol polyglycidyl ether, and the like. Commercially available products of epoxy crosslinking agents include trade names "TETRAD-X" and "TETRAD-C" manufactured by Mitsubishi Gas Chemical Co., Ltd., trade name "EPICLON CR-5L" manufactured by DIC Corporation, trade name "Denacol EX-512" manufactured by Nagase Chemtex Corporation, and trade name "TEPIC-G" manufactured by Nissan Chemical Industries, Ltd.

[0163] As the oxazoline-based crosslinking agent, any crosslinking agent having one or more oxazoline groups in one molecule can be used without particular limitation.

[0164] Examples of the aziridine crosslinking agent include trimethylolpropane tris[3-(1-aziridinyl)propionate] and trimethylolpropane tris[3-(1-(2-methyl)aziridinyl propionate)].

[0165] As the carbodiimide-based crosslinking agent, a low molecular weight compound or a high molecular weight compound having two or more carbodiimide groups can be used.

[0166] In some ways, peroxide can be used as a crosslinking agent. As peroxide, di(2-ethylhexyl) peroxydicarbonate, di(4-tert-butylcyclohexyl) peroxydicarbonate, di-sec-butyl peroxydicarbonate, tert-butyl peroxyneodecanoate, tert-hexyl peroxypivalate, tert-butyl peroxypivalate, dilauroyl peroxide, di-n-octanoyl peroxide, 1,1,3,3-tetramethylbutyl peroxide, dibenzoyl peroxide, etc. can be listed. Among these, as the particularly excellent peroxide of crosslinking reaction efficiency, di(4-tert-butylcyclohexyl) peroxydicarbonate, dilauroyl peroxide, dibenzoyl peroxide, etc. can be listed. It should be noted that, when peroxide is used as the above-mentioned polymerization initiator, the peroxide that is not used and remains in the polymerization reaction can also be used in the crosslinking reaction. In this case, the residual amount of peroxide is quantitatively measured, and when the ratio of peroxide does not meet the prescribed amount, peroxide can be added as required in the mode of becoming the prescribed amount. The quantitative determination of peroxide can be performed by the method described in Japanese Patent No. 4971517. The quantitative determination of peroxide can be performed by the method described in Japanese Patent No. 4971517.

[0167] The amount of crosslinking agent used (the total amount of crosslinking agents when using more than two crosslinking agents) is not particularly limited. From the perspective of realizing an adhesive that exerts adhesive properties such as adhesion and cohesion in a well-balanced manner, the amount of crosslinking agent used is generally about 5 parts by weight or less relative to 100 parts by weight of polymer (A), which is suitable, can be 3 parts by weight or less, can be 2 parts by weight or less, can be 1 part by weight or less, and can be less than 1 part by weight. In the method of using a crosslinking agent and a photoreactive monomer (B) in combination, from the perspective of easily and appropriately exerting the effect brought about by the above-mentioned combination, the amount of crosslinking agent used can be, for example, 0.80 parts by weight or less, can be 0.60 parts by weight or less, can be 0.30 parts by weight or less, and can be 0.10 parts by weight or less relative to 100 parts by weight of polymer (A). The lower limit of the amount of crosslinking agent used is not particularly limited, and can be used in an amount greater than 0 parts by weight relative to 100 parts by weight of polymer (A). In some embodiments, the amount of the crosslinking agent used may be, for example, 0.001 parts by weight or more, 0.01 parts by weight or more, or 0.03 parts by weight or more, relative to 100 parts by weight of the polymer (A).

[0168] The technology disclosed herein can preferably be implemented in such a manner that at least an isocyanate-based crosslinking agent is used as the crosslinking agent. An isocyanate-based crosslinking agent and other crosslinking agents can also be used in combination. In the manner of using an isocyanate-based crosslinking agent, the amount of the isocyanate-based crosslinking agent can be, for example, 0.005 parts by weight or more, 0.01 parts by weight or more, 0.03 parts by weight or more, relative to 100 parts by weight of the polymer (A). In addition, the amount of the isocyanate-based crosslinking agent can be, for example, 10 parts by weight or less, 5 parts by weight or less, 3 parts by weight or less, less than 2 parts by weight, less than 1 part by weight, less than 0.80 parts by weight, less than 0.60 parts by weight, less than 0.30 parts by weight, less than 0.10 parts by weight, less than 0.08 parts by weight, relative to 100 parts by weight of the polymer (A).

[0169] In order to make the crosslinking reaction proceed more effectively, a crosslinking catalyst can be used. As the crosslinking catalyst, metal-based crosslinking catalysts such as tetra-n-butyl titanate, tetra-isopropyl titanate, iron(III) acetylacetonate (Japanese original: ナーセム第ニ鉄), butyltin oxide, dioctyltin dilaurate, etc. can be exemplified. Among them, tin-based crosslinking catalysts such as dioctyltin dilaurate are preferred. The amount of the crosslinking catalyst is not particularly limited. The amount of the crosslinking catalyst can be, for example, about 0.0001 parts by weight or more, about 0.001 parts by weight or more, about 0.005 parts by weight or more, etc., relative to 100 parts by weight of the polymer (A). In addition, it can be about 1 part by weight or less, about 0.1 part by weight or less, about 0.05 part by weight or less, etc.

[0170] In the adhesive composition for forming the adhesive layer, a compound that generates keto-enol tautomerism can be contained as a crosslinking retarder according to the expectation. For example, in an adhesive composition containing an isocyanate-based crosslinking agent or an adhesive composition that can be compounded with an isocyanate-based crosslinking agent and used, a compound that generates keto-enol tautomerism can be preferably used. Thereby, the effect of extending the pot life of the adhesive composition can be exerted.

[0171] As the compound that generates keto-enol tautomerism, various β-dicarbonyl compounds can be used. As specific examples, β-diketones such as acetylacetone and 2,4-hexanedione can be cited; acetoacetates such as methyl acetoacetate and ethyl acetoacetate; propionylacetates such as ethyl propionylacetate; isobutyrylacetates such as ethyl isobutyrylacetate; malonates such as methyl malonate and ethyl malonate; etc. Among them, as suitable compounds, acetylacetone and acetoacetates can be cited. The compound that generates keto-enol tautomerism can be used alone or in combination of two or more kinds.

[0172] The amount of the compound producing keto-enol tautomerism used, relative to 100 parts by weight of the polymer (A), can be, for example, more than 0.1 parts by weight and less than 20 parts by weight, and is generally more than 0.5 parts by weight and less than 15 parts by weight. It can be, for example, more than 1 part by weight and less than 10 parts by weight, or more than 1 part by weight and less than 5 parts by weight.

[0173] (Silane coupling agent)

[0174] The adhesive layer of the adhesive sheet disclosed herein can contain a silane coupling agent as desired. By using a silane coupling agent, the peel strength of the adhesive sheet peeled off from an adherend (e.g., a glass plate) can be improved. The adhesive layer containing a silane coupling agent can be suitably formed using an adhesive composition containing a silane coupling agent. In the above-mentioned adhesive composition, from the viewpoint of suppressing gelation, the silane coupling agent is preferably included in the above-mentioned adhesive composition in a free form. In addition, in some ways, the silane coupling agent is preferably included in the adhesive layer of the adhesive sheet disclosed herein in a free form. The silane coupling agent contained in the adhesive layer in this way can efficiently contribute to improving the peeling force. It should be noted that "free form" here refers to: the silane coupling agent is not chemically bonded to other components contained in the adhesive composition or the adhesive layer.

[0175] Examples of the silane coupling agent include silicon compounds having an epoxy structure such as 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropylmethyldimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; silicon compounds containing amino groups such as 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)3-aminopropyltrimethoxysilane, and N-(2-aminoethyl)3-aminopropylmethyldimethoxysilane; 3-chloropropyltrimethoxysilane; trimethoxysilane containing acetoacetyl groups; silane coupling agents containing (meth)acryloyl groups such as 3-acryloxypropyltrimethoxysilane and 3-methacryloxypropyltriethoxysilane; silane coupling agents containing isocyanate groups such as 3-isocyanatepropyltriethoxysilane; etc. In some embodiments, the above-mentioned effects can be more preferably exerted by using a silane coupling agent having a trialkoxysilyl group. Among them, as preferred silane coupling agents, 3-glycidyloxypropyltrimethoxysilane and acetoacetyl group-containing trimethoxysilane can be exemplified.

[0176] The amount of the silane coupling agent used can be set in a manner that can obtain the desired effect of use, and is not particularly limited. In some embodiments, the amount of the silane coupling agent used can be, for example, 0.001 parts by weight or more relative to 100 parts by weight of the polymer (A). From the viewpoint of obtaining a higher effect, it can be 0.01 parts by weight or more, 0.05 parts by weight or more, or 0.1 parts by weight or more. In addition, from the viewpoint of inhibiting the gelation of the adhesive composition, the amount of the silane coupling agent used is usually suitable for less than 3 parts by weight relative to 100 parts by weight of the polymer (A), can be less than 1 part by weight, or can be less than 0.5 parts by weight.

[0177] (Photopolymerization Initiator)

[0178] The adhesive layer of the adhesive sheet disclosed herein may contain a photopolymerization initiator as needed for the purpose of improving or imparting photocurability. As the photopolymerization initiator, ketal-based photopolymerization initiators, acetophenone-based photopolymerization initiators, benzoin ether-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, α-ketol-based photopolymerization initiators, aromatic sulfonyl chloride-based photopolymerization initiators, photoactive oxime-based photopolymerization initiators, benzoin-based photopolymerization initiators, benzyl-based photopolymerization initiators, benzophenone-based photopolymerization initiators, thioxanthone-based photopolymerization initiators, etc. can be used, as exemplified by the photopolymerization initiators that can be used for synthesizing polymer (A). One type of photopolymerization initiator can be used alone, or two or more types can be used in combination.

[0179] Specific examples of the ketal-based photopolymerization initiator include 2,2-dimethoxy-1,2-diphenylethane-1-one and the like.

[0180] Specific examples of acetophenone-based photopolymerization initiators include: 1-hydroxycyclohexyl-phenyl-ketone, 4-phenoxydichloroacetophenone, 4-tert-butyl-dichloroacetophenone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propane-1-one, 2-hydroxy-2-methyl-1-phenyl-propane-1-one, methoxyacetophenone, etc.

[0181] Specific examples of the benzoin ether-based photopolymerization initiator include benzoin ethers such as benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, and benzoin isobutyl ether, and substituted benzoin ethers such as anisole methyl ether.

[0182] Specific examples of the acylphosphine oxide-based photopolymerization initiator include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,4-di-n-butoxyphenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide.

[0183] Specific examples of α-ketol-based photopolymerization initiators include 2-methyl-2-hydroxypropiophenone, 1-[4-(2-hydroxyethyl)phenyl]-2-methylpropane-1-one, and the like. Specific examples of aromatic sulfonyl chloride-based photopolymerization initiators include 2-naphthalenesulfonyl chloride, and the like. Specific examples of photoactive oxime-based photopolymerization initiators include 1-phenyl-1,1-propanedione-2-(o-ethoxycarbonyl)-oxime, and the like. Specific examples of benzoin-based photopolymerization initiators include benzoin, and the like. Specific examples of benzyl-based photopolymerization initiators include benzyl, and the like.

[0184] Specific examples of the benzophenone-based photopolymerization initiator include benzophenone, benzoylbenzoic acid, 3,3′-dimethyl-4-methoxybenzophenone, polyvinylbenzophenone, and α-hydroxycyclohexylphenylketone.

[0185] Specific examples of the thioxanthone-based photopolymerization initiator include thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone.

[0186] The content of the photopolymerization initiator in the adhesive layer is not particularly limited and can be set in a manner that suitably exerts the desired effect. In some ways, the content of the photopolymerization initiator can be, for example, about 0.005 parts by weight or more relative to 100 parts by weight of the polymer (A) contained in the adhesive layer, and is usually suitable for being 0.01 parts by weight or more, preferably 0.05 parts by weight or more, 0.10 parts by weight or more, 0.15 parts by weight or more, or 0.20 parts by weight or more. By increasing the content of the photopolymerization initiator, there is a tendency to improve the photocurability of the adhesive layer. In addition, relative to 100 parts by weight of the polymer (A), the content of the photopolymerization initiator is usually suitable for being 10 parts by weight or less, preferably 7 parts by weight or less, 5 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, or 1 part by weight or less. When the content of the photopolymerization initiator is not too much, it can be advantageous from the viewpoint of improving the storage stability of the adhesive sheet (for example, stability against light degradation).

[0187] The adhesive layer containing a photopolymerization initiator can typically be formed by using an adhesive composition containing the photopolymerization initiator (for example, a solvent-based adhesive composition). The adhesive composition containing a photopolymerization initiator can be prepared, for example, by mixing other components used in the composition with a photopolymerization initiator. In addition, when the adhesive composition is prepared using a polymer (A) (for example, an acrylic polymer (A)) synthesized (photopolymerized) in the presence of a photopolymerization initiator, the residue (unreacted product) of the photopolymerization initiator used when synthesizing the polymer (A) can be used as part or all of the photopolymerization initiator contained in the adhesive layer. The same is true for the case of using an acrylic oligomer synthesized in the presence of a photopolymerization initiator as used as needed. From the viewpoint of ease of manufacturing management, the adhesive layer disclosed herein can be preferably formed using an adhesive composition prepared by newly adding the above-mentioned amount of photopolymerization initiator to other components.

[0188] In addition, the adhesive layer in the technology disclosed herein may contain a leveling agent, a plasticizer, a softener, a colorant (dyes, pigments, etc.), a filler, an antistatic agent, an antioxidant, an ultraviolet absorber, an antioxidant, a light stabilizer, a preservative, etc., and known additives that can be used in the adhesive as required within the range that does not significantly damage the effect of the present invention. It should be noted that in an adhesive sheet for applications that do not wish to contain siloxane (e.g., applications for manufacturing electronic devices, etc.), it is desirable to avoid the use of silicone-based additives (e.g., silicone-based leveling agents, defoaming agents).

[0189] <Formation of Adhesive Layer>

[0190] The adhesive layer constituting the adhesive sheet disclosed herein may be a cured layer of an adhesive composition comprising the corresponding component. That is, the adhesive layer may be formed in the following manner, after the adhesive composition is imparted (e.g., applied) to an appropriate surface, and then appropriately dried (e.g., heated and dried), cross-linked (e.g., cross-linked based on the reaction of the cross-linking agent), cooled, and other curing treatments are performed to form. When two or more curing treatments are performed, they may be performed simultaneously or in stages.

[0191] In some embodiments, the adhesive composition contains at least any of the above-mentioned polymers (A). A preferred adhesive composition comprises an acrylic polymer (A) as the above-mentioned polymer (A). The above-mentioned adhesive composition may comprise the above-mentioned polymer (A) in the form of its precursor. The above-mentioned adhesive composition preferably comprises any of the above-mentioned polymers (A) and any of the above-mentioned photoreactive monomers (B). The above-mentioned photoreactive monomer (B) preferably comprises a compound B1 having a ring structure and two or more ethylenically unsaturated groups in the molecule. The average molecular weight of each of the above-mentioned ethylenically unsaturated groups of the above-mentioned compound B1 is preferably 100 g / mol or more.

[0192] The form of the above-mentioned adhesive composition is not particularly limited, and may be, for example, a water-dispersible adhesive composition in which the adhesive (adhesive component) is dispersed in water; a solvent-type adhesive composition in which the adhesive is contained in an organic solvent; a hot-melt adhesive composition that forms an adhesive when applied in a heated molten state and cooled to near room temperature; or various forms known in the art. From the viewpoint of the ease of preparation of the adhesive composition, the ease of forming the adhesive layer, etc., a solvent-type adhesive composition may be preferably used in some forms. The solvent-type adhesive composition can be preferably prepared by using a polymer (A) that is a polymer obtained by solution polymerization based on a monomer component.

[0193] The coating of the adhesive composition can be carried out using a conventional coating machine such as a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a rod coater, a knife coater, a spray coater, etc. For an adhesive sheet having a support body, as a method for providing an adhesive layer on the support body, a direct method of directly applying the adhesive composition to the support body to form the adhesive layer can be used, and a transfer method of transferring the adhesive layer formed on the release surface to the support body can also be used.

[0194] The thickness of the adhesive layer is not particularly limited, and for example, it can be about 3 μm to 500 μm. From the viewpoint of impact resistance, in some embodiments, it is suitable that the thickness of the adhesive layer is 5 μm or more, preferably 10 μm or more, and more preferably 15 μm or more. In addition, in some embodiments, the thickness of the adhesive layer can be, for example, 200 μm or less, and from the viewpoint of suppressing deformation of the adhesive layer, it is preferably 120 μm or less, 100 μm or less, 70 μm or less, 50 μm or less, or 35 μm or less. According to the adhesive sheet disclosed herein, in a method having an adhesive layer with a thickness of, for example, 70 μm or less, a joint with high deformation resistance and high impact resistance can be formed.

[0195] <Support>

[0196] Some forms of adhesive sheets can be in the form of adhesive sheets with a support body including a support body bonded to an adhesive layer. The material of the support body is not particularly limited and can be appropriately selected according to the purpose of use, the mode of use, etc. of the adhesive sheet. As non-limiting examples of usable supports, there can be listed: polyolefin films with polyolefins such as polypropylene and ethylene-propylene copolymer as the main component, polyester films with polyesters such as polyethylene terephthalate and polybutylene terephthalate as the main component, and resin films such as polyvinyl chloride films with polyvinyl chloride as the main component; foam sheets formed by foams such as polyurethane foam, polyethylene foam, and polychloroprene foam; fabrics and non-woven fabrics formed by various fibrous materials (which can be natural fibers such as hemp and cotton, synthetic fibers such as polyester and vinylon, and semi-synthetic fibers such as acetate, etc.) alone or in a blend; paper such as Japanese paper, high-quality paper, kraft paper, and crepe paper; metal foils such as aluminum foil and copper foil; etc. It can be a support body composed of them. Examples of such a composite structure support include a metal layer (e.g., metal foil, continuous or discontinuous metal sputtering layer, metal vapor deposition layer, metal plating layer, etc.), a support having a structure in which a metal oxide layer and the above-mentioned resin film are laminated, a resin sheet reinforced with inorganic fibers such as glass cloth, etc. The above-mentioned support may be an optical member (e.g., an optical film) described later, or a transparent member formed of a transparent material (e.g., a transparent resin material, glass, etc.).

[0197] As the support of the adhesive sheet disclosed herein, various films (hereinafter, also referred to as support films) can be preferably used. The above-mentioned support film can be a porous film such as a foam film, a non-woven fabric sheet, etc., or a non-porous film, or a film having a structure in which a porous layer and a non-porous layer are stacked. In some embodiments, as the above-mentioned support film, a film containing a (self-supporting or non-dependent) resin film that can independently maintain a shape as a base film can be preferably used. The so-called "resin film" here is a non-porous structure, typically referring to a resin film that is substantially free of bubbles (non-porous). Therefore, the above-mentioned resin film is a concept distinguished from a foam film and a non-woven fabric. The above-mentioned resin film can be a single-layer structure, or a multilayer structure (such as a three-layer structure) of more than two layers.

[0198] As the resin material constituting the resin film, for example, polyester, polyolefin, polycycloolefin derived from a monomer having an aliphatic ring structure such as a norbornene structure, nylon 6, nylon 66, polyamide (PA) such as partially aromatic polyamide, polyimide (PI), polyamideimide (PAI), polyetheretherketone (PEEK), polyethersulfone (PES), polyphenylene sulfide (PPS), polycarbonate (PC), polyurethane (PU), ethylene-vinyl acetate copolymer (EVA), polystyrene, polyvinyl chloride, polyvinylidene chloride, polytetrafluoroethylene (PTFE) and other fluororesins, acrylic resins such as polymethyl methacrylate, cellulose polymers such as diacetyl cellulose and triacetyl cellulose, vinyl butyral polymers, acrylate polymers, polyoxymethylene polymers, epoxy polymers and other resins can be used. The above-mentioned resin film can be a resin film formed using a resin material containing only one such resin, or a resin film formed using a resin material obtained by blending two or more. The above-mentioned resin film can be unstretched or stretched (for example, uniaxially stretched or biaxially stretched).

[0199] Preferred examples of resin materials constituting the resin film include polyester resins, PPS resins, and polyolefin resins. Here, the so-called polyester resin refers to a resin containing polyester in a ratio exceeding 50% by weight. Similarly, PPS resin refers to a resin containing PPS in a ratio exceeding 50% by weight, and polyolefin resin refers to a resin containing polyolefin in a ratio exceeding 50% by weight.

[0200] As the polyester resin, a polyester resin containing a polyester obtained by polycondensation of a dicarboxylic acid and a diol as a main component can be used. Specific examples of the polyester resin include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polybutylene naphthalate, etc.

[0201] As the polyolefin resin, one polyolefin may be used alone or in combination of two or more polyolefins. The polyolefin may be, for example, a homopolymer of an α-olefin, a copolymer of two or more α-olefins, a copolymer of one or more α-olefins and other vinyl monomers, etc. As specific examples, polyethylene (PE), polypropylene (PP), poly-1-butene, poly-4-methyl-1-pentene, ethylene-propylene rubber (EPR) and other ethylene-propylene copolymers, ethylene-propylene-butene copolymers, ethylene-butene copolymers, ethylene-vinyl alcohol copolymers, ethylene-ethyl acrylate copolymers, etc. may be cited. Both low-density (LD) polyolefins and high-density (HD) polyolefins may be used. Examples of polyolefin resin films include unstretched polypropylene (CPP) films, biaxially stretched polypropylene (OPP) films, low-density polyethylene (LDPE) films, linear low-density polyethylene (LLDPE) films, medium-density polyethylene (MDPE) films, high-density polyethylene (HDPE) films, polyethylene (PE) films obtained by blending two or more polyethylene (PE), and PP / PE blended films obtained by blending polypropylene (PP) and polyethylene (PE).

[0202] Specific examples of resin films that can be preferably used as a support include PET films, PEN films, PPS films, PEEK films, CPP films, and OPP films. From the perspective of strength, preferred examples include PET films, PEN films, PPS films, and PEEK films. From the perspective of ease of acquisition, dimensional stability, optical properties, etc., preferred examples include PET films.

[0203] The resin film may be mixed with known additives such as light stabilizers, antioxidants, antistatic agents, colorants (dyes, pigments, etc.), fillers, slip agents, anti-blocking agents, etc. as needed. The amount of the additives is not particularly limited and can be appropriately set according to the use of the adhesive sheet.

[0204] The method for producing the resin film is not particularly limited, and for example, conventionally known general resin film forming methods such as extrusion molding, inflation molding, T-die casting, and calender roll molding can be appropriately adopted.

[0205] The support may be a support film substantially composed of such a resin film. In addition, the support may be a support film including an auxiliary layer in addition to the resin film. The auxiliary layer may be arranged on the adhesive layer side of the resin film, may be arranged on the opposite side of the adhesive layer, and may be arranged on both sides of the resin film. Examples of the auxiliary layer include an optical property adjustment layer (e.g., a coloring layer, an anti-reflection layer), a decorative layer (e.g., a printed layer, a laminated layer, a continuous or discontinuous metal layer, a continuous or discontinuous metal oxide layer, etc.) that gives the support or adhesive sheet a desired appearance, a conductive layer, an antistatic layer, a primer layer, a peeling layer, etc.

[0206] The thickness of the support is not particularly limited and can be selected according to the purpose of use, the method of use, etc. of the adhesive sheet. The thickness of the support can be, for example, less than 1000 μm, less than 500 μm, less than 100 μm, less than 70 μm, less than 50 μm, less than 25 μm, less than 10 μm, or less than 5 μm. When the thickness of the support becomes smaller, there is a tendency to improve the softness of the adhesive sheet and the followability of the surface shape of the adherend. In addition, from the viewpoint of operability, processability, etc., the thickness of the support can be, for example, more than 2 μm, more than 5 μm or more than 10 μm. In some ways, the thickness of the support can be, for example, more than 20 μm, more than 35 μm, or more than 55 μm.

[0207] The surface of one side bonded with the adhesive layer in the support may be subjected to corona discharge treatment, plasma treatment, ultraviolet irradiation treatment, acid treatment, alkali treatment, coating of primer (primer), antistatic treatment and other previously known surface treatments as needed. Such surface treatments may be used to improve the adhesion between the support and the adhesive layer, in other words, the anchoring of the adhesive layer to the support. The composition of the primer is not particularly limited and may be appropriately selected from known substances. The thickness of the primer layer is not particularly limited, and is usually about 0.01 μm to 1 μm, preferably about 0.1 μm to 1 μm.

[0208] In the single-sided adhesive sheet with a support, the surface of the support that is on the opposite side to the side bonded to the adhesive layer (hereinafter, also referred to as the back side) can be subjected to peeling treatment, treatment to improve adhesion or adhesiveness, antistatic treatment and other previously known surface treatments as needed. For example, by surface treating the back side of the support with a peeling agent, the unwinding force of the adhesive sheet wound into a roll can be reduced. As the peeling agent, a silicone-based peeling agent, a long-chain alkyl-based peeling agent, an olefin-based peeling agent, a fluorine-based peeling agent, a fatty acid amide-based peeling agent, molybdenum sulfide, silica powder, etc. can be used.

[0209] <Laminate Manufacturing Method>

[0210] The adhesive sheet disclosed herein can be preferably used in a manner of pasting to the above-mentioned adherend by a method including photocuring the adhesive layer after being pasted to the adherend. By pasting the adhesive sheet to the adherend, an adherend laminated with the adhesive sheet can be formed. By photocuring the adhesive layer of the adhesive sheet, a laminated body including the adhesive sheet with the cured adhesive layer and the above-mentioned adherend can be obtained. Therefore, according to the specification, a laminated body manufacturing method is provided, which sequentially includes: pasting any adhesive sheet disclosed herein to the adherend, and irradiating the above-mentioned adhesive sheet with ultraviolet rays to photocure the above-mentioned adhesive layer.

[0211] <Purpose>

[0212] The adhesive sheet disclosed herein can be used for fixing, joining, molding, decorating, protecting, supporting and other purposes of components constituting various products. The material constituting at least the surface of the above-mentioned component can be, for example, glass such as alkali glass and alkali-free glass; metal materials such as stainless steel (SUS) and aluminum; resin materials such as acrylic resin, ABS resin, polycarbonate resin, polystyrene resin; etc. The above-mentioned component can be, for example, a component constituting various portable equipment, automobiles, home appliances, etc. In addition, in the above-mentioned component, the surface to which the adhesive sheet is pasted can be a coating surface based on a coating such as acrylic, polyester, alkyd, melamine, urethane, acid-epoxy crosslinking, or a composite thereof (such as acrylic melamine, alkyd melamine), such as a plated surface such as a galvanized steel sheet. In addition, the above-mentioned component can be any supporting film exemplified as a material that can be used for a support body (for example, a resin film, a supporting film having a continuous or discontinuous inorganic layer (which can be a metal layer, a metal oxide layer, etc.) on a resin film). The PSA sheet disclosed herein may be a constituent element of a member with a PSA sheet in which the above-mentioned member is bonded to at least one surface of a PSA layer constituting the above-mentioned PSA layer, for example.

[0213] As an example of preferred use, optical use can be cited. More specifically, for example, as an optical adhesive sheet used in the use of bonding optical components (optical component bonding), the manufacturing use of products (optical products) using the above optical components, etc., the adhesive sheet disclosed herein can be preferably used.

[0214] The above-mentioned optical component refers to a component with optical properties (for example, polarization, light refraction, light scattering, light reflectivity, light transmittance, light absorption, light diffraction, optical rotation, visual recognition, etc.). As the above-mentioned optical component, as long as it is a component with optical properties, it is not particularly limited. For example, components constituting devices (optical devices) such as display devices (image display devices) and input devices or components used by these devices can be listed. For example, polarizing plates, wavelength plates, phase difference plates, optical compensation films, brightness improvement films, light guide plates, reflective films, anti-reflection films, hard coating (HC) films, impact absorption films, antifouling films, photochromic films, dimming films, transparent conductive films (ITO films), design films, decorative films, surface protection plates, prisms, lenses, color filters, transparent substrates, and components stacked with them (sometimes collectively referred to as "functional films"). ) etc. It should be noted that the above-mentioned "plate" and "film" each include forms such as plate, film, and sheet. For example, "polarizing film" includes "polarizing plate", "polarizing film", and the like.

[0215] Examples of the display device include a liquid crystal display device, an organic EL (electroluminescence) display device, a PDP (plasma display panel), and electronic paper. Examples of the input device include a touch panel and the like.

[0216] The optical component is not particularly limited, and examples thereof include components formed of glass, acrylic resin, polycarbonate, polyethylene terephthalate, metal film, etc. (e.g., sheet-shaped, film-shaped, plate-shaped components), etc. It should be noted that the "optical component" in this specification also includes components that play a decorative and protective role while maintaining the visual recognizability of the display device and input device (design film, decorative film, surface protection film, etc.).

[0217] There is no particular limitation on the method of bonding optical components using the adhesive sheet disclosed herein, and for example, it may be (1) a method of bonding optical components to each other via the adhesive sheet disclosed herein, (2) a method of bonding optical components to components other than optical components via the adhesive sheet disclosed herein, or (3) a method in which the adhesive sheet disclosed herein contains an optical component and the adhesive sheet is bonded to an optical component or a component other than an optical component. It should be noted that in the above-mentioned method (3), the adhesive sheet containing an optical component may be, for example, an adhesive sheet whose support is an optical component (for example, an optical film). Such an adhesive sheet containing an optical component as a support may also be considered as an adhesive-type optical component (for example, an adhesive-type optical film). In addition, in the case where the adhesive sheet disclosed herein is an adhesive sheet of a type having a support, and the above-mentioned functional film is used as the above-mentioned support, the adhesive sheet disclosed herein may also be considered as an "adhesive functional film" having an adhesive layer disclosed herein on at least one side of the functional film.

[0218] It should be noted that the matters disclosed by this specification include the following aspects.

[0219] (1) A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer,

[0220] The adhesive layer contains a polymer (A) and a photoreactive monomer (B).

[0221] The photoreactive monomer (B) includes a compound B1 having two or more ethylenically unsaturated groups,

[0222] The average molecular weight (functional group equivalent) of each ethylenically unsaturated group in the compound B1 is greater than 100 g / mol.

[0223] (2) The pressure-sensitive adhesive sheet according to (1) above, wherein the compound B1 contains a ring structure in the molecule.

[0224] (3) The pressure-sensitive adhesive sheet according to (2) above, wherein the compound B1 contains at least one structure selected from the group consisting of a bisphenol A structure, a bisphenol F structure, and a bisphenol E structure in the molecule.

[0225] (4) The PSA sheet according to (2) or (3) above, wherein the compound B1 contains an aliphatic ring structure as the ring structure.

[0226] (5) The pressure-sensitive adhesive sheet according to any one of (1) to (4) above, wherein the compound B1 contains at least one structure selected from the group consisting of a hydroxyl group and an amino group in the molecule.

[0227] (6) The pressure-sensitive adhesive sheet according to any one of (1) to (5), wherein the content of the compound B1 in the pressure-sensitive adhesive layer is 0.5 parts by weight or more and 60 parts by weight or less per 100 parts by weight of the polymer (A).

[0228] (7) The pressure-sensitive adhesive sheet according to any one of (2) to (5), wherein the pressure-sensitive adhesive layer comprises the compound B1 and a compound B2 having a functional group number of 2 or more and having no ring structure in the molecule as the photoreactive monomer (B).

[0229] (8) The pressure-sensitive adhesive sheet according to (7) above, wherein the functional group equivalent weight of the compound B2 is smaller than the functional group equivalent weight of the compound B1.

[0230] (9) The pressure-sensitive adhesive sheet according to (7) or (8) above, wherein the functional group equivalent of the compound B2 is 400 g / mol or less.

[0231] (10) The pressure-sensitive adhesive sheet according to any one of (7) to (9) above, wherein the content of the compound B2 in the pressure-sensitive adhesive layer is 25 parts by weight or less based on 100 parts by weight of the polymer (A).

[0232] (11) The pressure-sensitive adhesive sheet according to any one of (1) to (10), wherein the content of the photoreactive monomer (B) in the pressure-sensitive adhesive layer is 1 part by weight or more and 80 parts by weight or less based on 100 parts by weight of the polymer (A).

[0233] (12) The pressure-sensitive adhesive sheet according to any one of (1) to (11) above, wherein the polymer (A) is an acrylic polymer.

[0234] (13) The pressure-sensitive adhesive sheet according to (12) above, wherein the monomer component constituting the acrylic polymer includes a monomer having a ring containing a nitrogen atom.

[0235] (14) The pressure-sensitive adhesive sheet according to any one of (1) to (13) above, wherein the polymer (A) has a glass transition temperature of -45°C or higher and lower than 0°C.

[0236] (15) The pressure-sensitive adhesive sheet according to any one of (1) to (14) above, wherein the pressure-sensitive adhesive layer is crosslinked with a crosslinking agent.

[0237] (16) The pressure-sensitive adhesive sheet according to any one of (1) to (15), wherein the pressure-sensitive adhesive layer contains a photopolymerization initiator.

[0238] (17) The pressure-sensitive adhesive sheet according to any one of (1) to (14) above, wherein the pressure-sensitive adhesive layer contains a silane coupling agent.

[0239] (18) The pressure-sensitive adhesive sheet according to any one of (1) to (17) above, wherein the tensile modulus measured by the tensile test is 3.0 MPa or more.

[0240] (19) The pressure-sensitive adhesive sheet according to any one of (1) to (18) above, wherein the impact resistance measured by the shear impact test is 2.0 J / (10 mm). 2 above.

[0241] (20) The pressure-sensitive adhesive sheet according to any one of (1) to (19) above, wherein the peel strength measured by the peel test is 1.0 N / 10 mm or more.

[0242] (21) An adhesive composition comprising a polymer (A) and a photoreactive monomer (B),

[0243] The photoreactive monomer (B) includes a compound B1 having two or more ethylenically unsaturated groups,

[0244] The average molecular weight (functional group equivalent) of each ethylenically unsaturated group in the compound B1 is greater than 100 g / mol.

[0245] (22) The pressure-sensitive adhesive sheet according to (21) above, wherein the compound B1 contains a ring structure in the molecule.

[0246] (23) The adhesive composition according to (22) above, wherein the compound B1 contains at least one structure selected from the group consisting of a bisphenol A structure, a bisphenol F structure, and a bisphenol E structure in the molecule.

[0247] (24) The adhesive composition according to (2) or (23) above, wherein the compound B1 contains an aliphatic ring structure as the ring structure.

[0248] (25) The adhesive composition according to any one of (21) to (24) above, wherein the compound B1 contains at least one structure selected from the group consisting of a hydroxyl group and an amino group in the molecule.

[0249] (26) The adhesive composition according to any one of (21) to (25) above, wherein the content of the compound B1 in the adhesive layer is 0.5 parts by weight or more and 60 parts by weight or less relative to 100 parts by weight of the polymer (A).

[0250] (27) The adhesive composition according to any one of (22) to (25) above, wherein the adhesive layer contains the compound B1 and a compound B2 having a functional group number of 2 or more and no ring structure in the molecule as the photoreactive monomer (B).

[0251] (28) The adhesive composition according to (27) above, wherein the functional group equivalent weight of the compound B2 is smaller than the functional group equivalent weight of the compound B1.

[0252] (29) The adhesive composition according to (27) or (28) above, wherein the functional group equivalent of the compound B2 is 400 g / mol or less.

[0253] (30) The adhesive composition according to any one of (27) to (29) above, wherein the content of the compound B2 in the adhesive layer is 25 parts by weight or less based on 100 parts by weight of the polymer (A).

[0254] (31) The adhesive composition according to any one of (21) to (30) above, wherein the content of the photoreactive monomer (B) in the adhesive layer is 1 part by weight or more and 80 parts by weight or less relative to 100 parts by weight of the polymer (A).

[0255] (32) The pressure-sensitive adhesive composition according to any one of (21) to (31) above, wherein the polymer (A) is an acrylic polymer.

[0256] (33) The pressure-sensitive adhesive composition according to (32) above, wherein the monomer component constituting the acrylic polymer includes a monomer having a ring containing a nitrogen atom.

[0257] (34) The adhesive composition according to any one of (21) to (33) above, wherein the glass transition temperature of the polymer (A) is -45°C or higher and lower than 0°C.

[0258] (35) The adhesive composition according to any one of (21) to (34) above, wherein the adhesive composition contains a cross-linking agent.

[0259] (36) The adhesive composition according to any one of (21) to (35) above, wherein the adhesive composition contains a photopolymerization initiator.

[0260] (37) The adhesive composition according to any one of (21) to (36) above, wherein the adhesive composition contains a silane coupling agent.

[0261] (38) The PSA composition according to any one of (21) to (37) above, which is used to form a PSA layer of the PSA sheet according to any one of (1) to (20).

[0262] (39) A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer comprising the pressure-sensitive adhesive composition according to any one of (21) to (37) above.

[0263] (40) A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer,

[0264] The tensile modulus measured by the tensile test is 3.0 MPa or more, and the impact resistance measured by the shear impact test is 2.0 J / (10 mm). 2 above.

[0265] (41) The pressure-sensitive adhesive sheet according to (40) above, wherein the peel strength measured by the peel test is 1.0 N / 10 mm or more.

[0266] (42) The pressure-sensitive adhesive sheet according to any one of (40) to (41) above, wherein the pressure-sensitive adhesive layer is the pressure-sensitive adhesive layer according to any one of (1) to (17) above.

[0267] (43) The pressure-sensitive adhesive sheet according to any one of (40) to (42) above, wherein the pressure-sensitive adhesive layer is a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition according to any one of (21) to (37) above.

[0268] (44) An adhesive composition according to any one of (21) to (37) above, wherein, in the above-mentioned adhesive composition, an adhesive layer (for example, an adhesive layer with a thickness of 20 μm) formed by the adhesive composition and having a thickness selected from the range of 5 μm to 200 μm (preferably the range of 15 μm to 25 μm) has a tensile modulus of 3.0 MPa or more measured by the above-mentioned tensile test.

[0269] (45) The adhesive composition according to (44) above, wherein the impact resistance of the adhesive layer of the thickness formed by the adhesive composition measured by the shear impact test is 2.0 J / (10 mm). 2 above.

[0270] (46) The adhesive composition described in (44) or (45) above, wherein the peel strength of the adhesive layer of the above thickness formed by the adhesive composition measured by the above peel test is greater than 1.0 N / 10 mm.

[0271] (47) A film member with an adhesive sheet, comprising: the adhesive sheet according to any one of (1) to (20) and (40) to (43) above, and a film member bonded to the adhesive layer.

[0272] (48) A method for manufacturing a laminate, comprising:

[0273] The pressure-sensitive adhesive sheet according to any one of (1) to (20) and (40) to (43) is bonded to an adherend, and

[0274] The pressure-sensitive adhesive sheet is irradiated with ultraviolet rays to photo-cure the pressure-sensitive adhesive layer.

[0275] Hereinafter, some embodiments of the present invention will be described, but the present invention is not intended to be limited to the contents shown in these embodiments. It should be noted that, unless otherwise specified, in the following description, "parts" and "%" are based on weight.

[0276] <Synthesis of Polymer (A)>

[0277] (Polymer P1)

[0278] In a reaction vessel equipped with a condenser, a nitrogen inlet pipe, a thermometer and a stirring device, 60 parts of n-butyl acrylate (BA), 6 parts of cyclohexyl acrylate (CHA), 18 parts of N-vinyl-2-pyrrolidone (NVP), 1 part of isostearyl acrylate (iSTA) and 15 parts of 4-hydroxybutyl acrylate (4HBA) as monomer components, 0.085 parts of α-thioglycerol as a chain transfer agent, 122 parts of ethyl acetate as a polymerization solvent, 0.2 parts of 2,2'-azobisisobutyronitrile (AIBN) as a thermal polymerization initiator were added and solution polymerization was carried out under a nitrogen atmosphere to obtain a solution of polymer P1. The weight average molecular weight (Mw) of polymer P1 is 300,000. The Tg of polymer P1 calculated from the composition of the above monomer components is -33°C.

[0279] (Polymer P2)

[0280] In a reaction vessel equipped with a condenser, a nitrogen inlet pipe, a thermometer and a stirring device, 64.5 parts of BA, 6 parts of CHA, 9.6 parts of NVP, 5 parts of iSTA and 14.9 parts of 4HBA as monomer components, 0.07 parts of α-thioglycerol as a chain transfer agent, 122 parts of ethyl acetate as a polymerization solvent, 0.2 parts of AIBN as a thermal polymerization initiator were added and solution polymerization was carried out under a nitrogen atmosphere to obtain a solution of polymer P2. The Mw of polymer P2 is 600,000. The Tg of polymer P2 calculated from the composition of the above monomer components is -39°C.

[0281] <Preparation of Adhesive Composition>

[0282] (Example 1)

[0283] To the solution of the polymer P1 obtained above, 0.05 parts of an isocyanate crosslinking agent X1 (trimethylolpropane / xylylene diisocyanate adduct (manufactured by Mitsui Chemicals, trade name: TAKENATE D-110N, solid content concentration 75%)) was added based on the solid content, and dioctyltin dilaurate (manufactured by Tokyo Fine Chemical Co., Ltd., trade name: EMBILIZER XT) as a crosslinking accelerator was added. In addition, 0.01 parts of 1-hydroxycyclohexyl-phenyl-ketone (manufactured by IGM Regins, trade name: Omnirad 184) and 0.72 parts of 1-hydroxycyclohexyl-phenyl-ketone (manufactured by IGM Regins, trade name: Omnirad 184) as a photopolymerization initiator were uniformly mixed to prepare a solvent-based adhesive composition of Example 1.

[0284] (Examples 2 to 3, 5 to 12)

[0285] The solvent-based PSA composition of each example was prepared in the same manner as in Example 1 except that the type and amount of the photoreactive monomer, the amount of the crosslinking agent, and the amount of the photopolymerization initiator were changed as shown in Tables 1 and 2.

[0286] (Example 4)

[0287] The solvent-based PSA composition of this example was prepared in the same manner as in Example 3 except that the isocyanate crosslinking agent X2 (trimethylolpropane / toluene diisocyanate trimer adduct (manufactured by Tosoh Corporation, trade name: Coronate L)) was used instead of the isocyanate crosslinking agent X1.

[0288] (Example 13)

[0289] A solvent-based PSA composition of this example was prepared in the same manner as in the preparation of the solvent-based PSA composition of Example 10, except that a solution of the polymer P2 was used instead of the solution of the polymer P1.

[0290] <Preparation of Adhesive Sheet>

[0291] The solvent-based adhesive composition of each example prepared above was applied to the release surface of a release film R1 (MRF#38, manufactured by Mitsubishi Resins Co., Ltd.) with a thickness of 38 μm on one side of a polyester film, and dried at 130°C for 3 minutes to form a photocurable adhesive layer (double-sided adhesive sheet without a support) with a thickness of 20 μm. The release surface of a release film R2 (MRE#38, manufactured by Mitsubishi Resins Co., Ltd.) with a thickness of 38 μm on one side of a polyester film was attached to the surface of the adhesive layer for protection. In this way, a laminated sheet consisting of a release film R1, a double-sided adhesive sheet without a support, and a release film R2 was obtained.

[0292] <Measurement and Evaluation>

[0293] The following measurements and evaluations were performed on the obtained pressure-sensitive adhesive sheets.

[0294] (1) Determination of tensile modulus

[0295] Use high pressure mercury lamp at an illumination of 300mW / cm 2 、Accumulated light intensity 3000mJ / cm 2 Under the conditions of , the laminated sheets of each example (laminated sheets with an adhesive layer without a support body sandwiched between two transparent release films) were irradiated with ultraviolet rays, and after aging at 50°C for 48 hours, the laminated sheets were cut into a size of 10 mm in width and 150 mm in length. Under an environment of 23°C and 50% RH, the release films R1 and R2 were peeled off to expose the adhesive layer, and a tensile tester (Minebea, universal tensile compression tester, device name "tensile compression tester, TCM-1kNB") was used to perform a tensile test on the above test pieces under the conditions of a chuck spacing of 120 mm and a tensile speed of 50 mm / min, and the SS curve was obtained. The tensile modulus [MPa] was calculated from its initial slope (the elastic deformation region of the above SS curve, specifically the slope within the range where the displacement is less than about 5%). The measurement was performed 3 times (i.e., n=3), and their arithmetic mean values ​​are shown in Tables 1 and 2.

[0296] (2) Measurement of impact resistance

[0297] The shear impact test was conducted using a pendulum-type adhesive shear impact tester based on JIS K6855. As the test sample, the following sample was used: the laminated sheet of each example was cut into 10 mm squares, the release film R1 was peeled off and the first side of the adhesive layer was exposed, and the first side was bonded to the center of a 25 mm square, 1.7 mm thick chemically tempered glass plate (produced by Corning), the release film R2 was peeled off and the second side of the above adhesive layer was bonded to the center of a 40 mm square stainless steel plate (SUS304BA plate) and pressed with a load of 5 N for 10 seconds, followed by autoclave treatment (50°C, 0.5 MPa, 15 minutes), and a high-pressure mercury lamp was used at an illumination of 300 mW / cm 2 、Accumulated light intensity 3000mJ / cm 2 After irradiating the glass plate with ultraviolet rays from the glass plate side under the conditions of , aging was performed at 50° C. for 48 hours to obtain a sample.

[0298] The above-mentioned measurement sample was fixed in a manner such that the above-mentioned stainless steel plate was at the lower side, and the absorbed energy [J] when the outer peripheral side surface of the above-mentioned glass plate was hit by a hammer under the conditions of a hammer energy of 2.75 J and a hammer speed (impact speed) of 3.5 m / sec was measured, thereby determining the impact resistance [J / (10 mm) 2 The measurement was performed three times, and Tables 1 and 2 show their arithmetic mean values.

[0299] (3) Peel strength

[0300] The laminated sheet of each example was cut into a size of 10 mm in width and 150 mm in length to prepare a test piece, and a 2 kg rubber roller was reciprocated once to press the first surface of the adhesive layer in the test piece onto a glass plate (alkali glass plate manufactured by Matsunami Glass Industries, produced by float process, 1.35 mm in thickness, blue plate edge polished product), and then autoclaved (50° C., 0.5 MPa, 15 minutes) using a high pressure mercury lamp at an illumination of 300 mW / cm 2 、Accumulated light intensity 3000mJ / cm 2 After aging at 50°C for 48 hours, the test piece was peeled off from the glass plate at a peeling angle of 180 degrees and a tensile speed of 60 mm / min using a tensile tester (Minebea, a universal tensile compression tester, device name "tensile compression tester, TCM-1kNB") under an environment of 23°C and 50% RH. The test piece was irradiated with ultraviolet light from the glass plate side. The test piece was ripened at 50°C for 48 hours, and the peeling strength when peeling off the test piece from the glass plate was measured under the conditions of a peeling angle of 180 degrees and a tensile speed of 60 mm / min. Tables 1 and 2 show the arithmetic mean values ​​thereof.

[0301] The haze values ​​of the PSA layers of the PSA sheets of Examples 1, 6, 8, and 11 were measured by the above method and were found to be approximately 0.5% or less. The PSA layers of the PSA sheets of Examples 6 and 8 exhibited particularly good transparency.

[0302] [Table 1]

[0303] Table 1

[0304]

[0305] [Table 2]

[0306] Table 2

[0307]

[0308] In addition, the photoreactive monomers used in Examples 1 to 13 are as follows. In Tables 1 and 2, each photoreactive monomer is represented by an abbreviation.

[0309] DPHA: dipentaerythritol hexaacrylate (Shin-Nakamura Chemical Industry, trade name "A-DPH", functional group equivalent 96)

[0310] A-DCP: tricyclodecane dimethanol diacrylate (Shin-Nakamura Chemical Industry, trade name "A-DCP", functional group equivalent 152)

[0311] #540: Bisphenol A diglycidyl ether acrylic acid adduct (Osaka Organic Chemical Industry, trade name "Viscoa #540", functional group equivalent 250)

[0312] R115F: Bisphenol A diglycidyl ether acrylic acid adduct (Nippon Kayaku, trade name "KAYARAD R-115F", functional group equivalent 450)

[0313] #700HV: Bisphenol A ethylene oxide 3.8 mol adduct diacrylate (Osaka Organic Chemical Industry, trade name "Viscoa #700HV", functional group equivalent 350)

[0314] E3703: Amine-modified bisphenol A epoxy diacrylate (Daicel Ornex Co., Ltd., trade name "EBECRYL 3703", functional group equivalent 425)

[0315] APG400: Polypropylene glycol #400 diacrylate (Shin-Nakamura Chemical Industry, trade name "APG-400", functional group equivalent 268)

[0316] The PSA sheets of Examples 1 to 9 shown in Table 1 have excellent deformation resistance due to their high tensile modulus and exhibit high impact resistance. On the other hand, the PSA sheets of Examples 10, 12, and 13 shown in Table 2 have low deformation resistance, and the PSA sheet of Example 11 has low peel strength.

[0317] Although the specific examples of the present invention have been described in detail above, these are only examples and do not limit the scope of the claims. The technology described in the scope of the claims includes various modifications and substitutions of the specific examples described above.

[0318] Description of Reference Numerals

[0319] 1, 2 Adhesive sheet

[0320] 10 Adhesive layer

[0321] 10A One surface (bonding surface)

[0322] 10B Another Surface

[0323] 20 Support

[0324] 20A Side 1

[0325] 20B Second side (back side)

[0326] 30, 31, 32 Release liner

[0327] 50 Adhesive sheet with release liner

[0328] 70 Thin film components

[0329] 100 Components with adhesive sheet

Claims

1. A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer, The adhesive layer contains a polymer (A) and a photoreactive monomer (B), The photoreactive monomer (B) includes a compound B1 having a ring structure and two or more ethylenically unsaturated groups in the molecule, and a compound B2 having two or more functional groups and no ring structure in the molecule, The adhesive sheet has an elastic modulus of 3.0 MPa or more as measured by the following tensile test, and an impact resistance of 2.0 J / (10 mm) as measured by the following shear impact test. 2 above, [Tensile test] At an illumination of 300mW / cm 2 、Accumulated light intensity 3000mJ / cm 2 The adhesive layer was irradiated with ultraviolet rays under the conditions of , and after aging at 50°C for 48 hours, the adhesive layer was cut into a size of 10 mm in width and 150 mm in length to prepare a test piece. A tensile test was performed on the test piece under the conditions of 23°C and 50% RH with a tensile testing machine at a chuck spacing of 120 mm and a tensile speed of 50 mm / min, and a stress-displacement curve was obtained. The elastic modulus [MPa] was calculated from its initial slope. [Shear impact test] The shear impact test was conducted using a pendulum-type adhesive shear impact tester based on JIS K6855. As the test sample, the following sample was used: the first surface of the adhesive layer of 10 mm square was attached to the central part of a chemically tempered glass plate of 25 mm square and 1.7 mm thick, and the second surface of the adhesive layer was attached to the central part of a stainless steel plate of 40 mm square, i.e., a SUS304BA plate, and pressed at a load of 5 N for 10 seconds, and then subjected to an autoclave treatment at 50° C., 0.5 MPa, and 15 minutes, and an illumination of 300 mW / cm 2 、Accumulated light intensity 3000mJ / cm 2 After irradiating the glass plate with ultraviolet rays from the side under the conditions of , aging was performed at 50° C. for 48 hours, thereby obtaining a sample, The sample was fixed with the stainless steel plate at the bottom, and the absorbed energy [J] when the outer peripheral side of the glass plate was struck by a hammer at an energy of 2.75 J and a speed of 3.5 m / s was measured under the conditions of 23°C and 50% RH, thereby determining the impact resistance [J / (10 mm) 2 ].

2. The adhesive sheet according to claim 1, wherein The peel strength measured by the following peel test is 1.0N / 10mm or more. [Peel test] The adhesive sheet was cut into a test piece with a width of 10 mm and a length of 150 mm, and the test piece was pressed against a glass plate by reciprocating a 2 kg rubber roller once. After autoclaving at 50°C and 0.5 MPa for 15 minutes, the test piece was heated under an illumination of 300 mW / cm 2 、Accumulated light intensity 3000mJ / cm 2 The glass plate was irradiated with ultraviolet rays from the side under the conditions of , and aged at 50°C for 48 hours. Then, the peel strength of the test piece when it was peeled off from the glass plate at a peeling angle of 180 degrees and a tensile speed of 60 mm / min was measured using a tensile testing machine in an environment of 23°C and 50% RH.

3. The adhesive sheet according to claim 1 or 2, wherein The average molecular weight of each ethylenically unsaturated group in the compound B1 is greater than 100 g / mol.

4. A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer, The adhesive layer contains a polymer (A) and a photoreactive monomer (B), The photoreactive monomer (B) includes a compound B1 having a ring structure and two or more ethylenically unsaturated groups in the molecule, and a compound B2 having two or more functional groups and no ring structure in the molecule, The average molecular weight of each ethylenically unsaturated group in the compound B1 is greater than 100 g / mol.

5. The adhesive sheet according to claim 4, wherein The elastic modulus measured by the following tensile test is 3.0 MPa or more, [Tensile test] At an illumination of 300mW / cm 2 、Accumulated light intensity 3000mJ / cm 2 The adhesive layer was irradiated with ultraviolet rays under the conditions of and aged at 50°C for 48 hours, then cut into test pieces with a width of 10 mm and a length of 150 mm to prepare test pieces. The test pieces were subjected to a tensile test using a tensile testing machine at a chuck spacing of 120 mm and a tensile speed of 50 mm / min under the conditions of stress-displacement curve, and the elastic modulus was calculated from its initial slope.

6. The adhesive sheet according to claim 4 or 5, wherein The impact resistance measured by the following shear impact test is 2.0 J / (10 mm) 2 above, [Shear impact test] The shear impact test was conducted using a pendulum-type adhesive shear impact tester based on JIS K6855. As the test sample, the following sample was used: the first surface of the adhesive layer of 10 mm square was attached to the central part of a chemically tempered glass plate of 25 mm square and 1.7 mm thick, and the second surface of the adhesive layer was attached to the central part of a stainless steel plate of 40 mm square, i.e., a SUS304BA plate, and pressed at a load of 5 N for 10 seconds, and then subjected to an autoclave treatment at 50° C., 0.5 MPa, and 15 minutes, and an illumination of 300 mW / cm 2 、Accumulated light intensity 3000mJ / cm 2 After irradiating the glass plate with ultraviolet rays from the side under the conditions of , aging was performed at 50° C. for 48 hours, thereby obtaining a sample, The sample was fixed with the stainless steel plate at the bottom, and the absorbed energy [J] when the outer peripheral side of the glass plate was struck by a hammer at an energy of 2.75 J and a speed of 3.5 m / s was measured under the conditions of 23°C and 50% RH, thereby determining the impact resistance [J / (10 mm) 2 ]. 7 . A film member with an adhesive sheet, comprising: the adhesive sheet according to claim 1 , and a film member bonded to the adhesive layer.

8. A method for manufacturing a laminate, comprising: The pressure-sensitive adhesive sheet according to any one of claims 1 to 6 is bonded to an adherend, and The pressure-sensitive adhesive sheet is irradiated with ultraviolet rays to photo-cure the pressure-sensitive adhesive layer.

Citation Information

Patent Citations

  • An electric motor having a drive valve

    JP1974071517A

  • Adhesive sheet

    JP2016017113A

  • Electromagnetic wave transmissive metallic sheen member, article using the same and thin metallic film

    JP2018069462A

  • Release method and release device of marine animal and plant

    JP2019122284A

  • Information processing system, server device, information processing method, and program

    JP2020107125A