- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-13
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-12-13
AI Technical Summary
Perovskite nanocrystals are unstable to environmental stimuli and are prone to phase change or decomposition in solution. Existing stabilization methods affect their charge transfer properties, especially the stability of CsPbI3 nanocrystals, which is difficult to improve.
The bis-amino ligand N'-(2-aminoethyl)-N'-hexadecylethane-1,2-diamine (AHDA) is used as a new ligand, synthesized through melting reaction and reflux method, and anchored The surface of perovskite nanocrystals enhances its binding force with nanocrystals and protects them from environmentally induced decomposition and phase changes.
The long-term stability of nanocrystals such as CsPbI3, CsPbBr3, CsPbCl3 and FAPbI3 has been achieved, maintaining optical properties and morphology for more than 110 days, surpassing the stability effects previously reported, and is suitable for industrial production and applications in the field of optoelectronics.
Smart Images

Figure CN114058366B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of perovskite nanocrystals, and specifically relates to a method for stabilizing perovskite nanocrystals by using diamino ligands and perovskite nanocrystals stabilized by the diamino ligands. Background Art
[0002] Inorganic cesium metal halide nanocrystals (perovskite nanocrystals) have attracted great attention due to their narrow-band emission, easy tunability across the entire visible spectrum, and high photoluminescence quantum yield (PL QY) (NanoLett. 2015, 15, 3692-3696). In addition, perovskite nanocrystals (PNCs) also have low crystal formation energy, inherent defect tolerance, and good PL efficiency, and are easy to prepare. Even without inert gas protection, PNCs with excellent optical properties that do not require passivation can be prepared at room temperature (Science. 2017, 358, 745-750; Adv. Funct. Mater. 2016, 26, 2435-2445). This easy preparation advantage has brought a lot of technical advantages to the field of colloidal CNCs. However, PNCs are generally less stable to environmental stimuli (light, heat, moisture), which causes PNCs to easily phase change or decompose during solution-based purification and storage. To improve the environmental stability of PNCs, the commonly used method is to embed PNCs into an inert polymer or silica matrix, but this method will adversely affect the charge transfer properties of PNCs (Angew. Chem. 2021, 60, 7488-7501). Therefore, stabilizing PNCs by appropriate surface modification in solution without affecting their semiconductor properties has become one of the most important and challenging tasks to date.
[0003] The instability of PNCs is largely due to the instability of the binding between the inorganic core and the surface organic ligands. The ligands are easily detached, resulting in defects on the nanocrystal boundaries. Water, oxygen or polar solvents can be absorbed by the exposed defect sites, resulting in phase transition or decomposition of PNCs. Currently, various commercially available surfactants, such as oleylamine (OLA), oleic acid (OA), dodecylbenzenesulfonic acid (DBSA), zwitterionic ligands, alkanethiolates, 2,2'-imidodibenzoic acid (IDA), trioctylphosphine oxide (TOPO), secondary fatty amines and alkylphosphonic acids have been used as ligands or modifiers to stabilize PNCs. In particular, dodecylbenzenesulfonic acid (DBSA) and zwitterionic ligands have been shown to be effective ligands for stabilizing CsPbBr3PNCs during purification and storage. However, for CsPbI3 PNCs, the most unstable among PNCs, improving their stability has become a more challenging issue due to their inherent metastable perovskite structure, and there are few reports on ligands that can improve the stability of CsPbI3 PNCs. In order to give full play to the excellent optoelectronic properties of a series of environmentally unstable PNCs including CsPbI3, CsPbBr3, CsPbCl3 and FAPbI3, such as narrow band gap, wide absorption range and long carrier lifetime, and realize their application in the fields of red photon source, solar cell and photocatalysis, the method of modifying PNCs to improve their stability is of great research significance. Summary of the invention
[0004] The purpose of the present invention is to provide a method for stabilizing perovskite nanocrystals using a diamino ligand and perovskite nanocrystals stabilized by the diamino ligand. Different from the previous method for stabilizing PNCs, the present invention adopts a new diamino ligand for stabilizing perovskite nanocrystals, which can stabilize a series of PNCs that are unstable to environmental stimuli, such as CsPbI3, CsPbBr3, CsPbCl3 and FAPbI3 (formamidine). In addition, a class of perovskite nanocrystals AHDA-CsPbI3 PNCs, AHDA-CsPbBr3 PNCs, AHDA-CsPbCl3 PNCs and AHDA-FAPbI3PNCs that can exist stably in the environment are obtained by the stabilization method.
[0005] The diamino ligand of the present invention is named N'-(2-aminoethyl)-N'-hexadecylethane-1,2-diamine (AHDA for short, with a structural formula as shown below and a synthesis method as shown in the literature Front. Mater. Sci. 2012, 6, 268). In the literature, white solid AHDA was synthesized by melt reaction and reflux method, and its structure is novel. Compared with the ligand with a single amino group, the diamino structure of AHDA has more action sites that can bind to the surface of PNCs, so that AHDA chelates on the surface of PNCs with super strong binding force. This anchoring edge can effectively protect PNCs from decomposition and phase change induced by various environments. This method of stabilizing PNCs with diamino ligands can effectively solve the problem of instability of PNCs, realize the preparation of stable PNCs, and make the industrial production and application of PNCs in the field of optoelectronics possible.
[0006]
[0007] The method of stabilizing perovskite nanocrystals using diamino ligands of the present invention comprises the following steps:
[0008] AHDA was used to stabilize CsPbI3 NCs to synthesize AHDA-CsPbI3 NCs. First, 1-octadecene (ODE), AHDA and lead iodide (PbI2) were mixed in a mass ratio of 1: (50-100): (10-50), and vacuum degassed and dried at 110-130°C for 1-2h; then, dry bis(2,4,4-trimethylpentyl)-phosphinic acid (BTMPA, the mass ratio of BTMPA to AHDA was 1:150-200) was added at the same temperature, and after the mixed solution became clear, Then, a cesium oleate precursor (the volume ratio of the cesium oleate precursor to BTMPA is 8:2-30) is quickly injected at 70-180°C and in an Ar atmosphere for reaction for 10-300s; the reaction product is cooled to room temperature in an ice-water bath, and then methyl acetate (MeOAc) is added for reverse precipitation, and the volume of MeOAc is 1-5 times the total volume of the mixed solution after the addition of the cesium oleate precursor. When no more precipitate is precipitated, AHDA-CsPbI3 NCs are obtained by centrifugation; in order to verify the stabilizing effect of AHDA on CsPbI3 NCs, toluene and MeOAc are used for dissolution-precipitation purification treatment. After multiple cycles, purified CsPbI3 NCs with good optical properties and morphology are obtained.
[0009] CsPbX3 NCs were stabilized by AHDA. The operation steps were the same as those for stabilizing CsPbI3 NCs by AHDA. The only difference was that different Pb sources were used instead of PbI2, i.e., PbCl2, PbBr2, PbBr2 and PbI2 were used to prepare CsPbCl3 NCs, CsPbBr3 NCs and CsPbI2Br NCs. The purification process was the same as that of AHDA-CsPbI3 NCs. Finally, in order to verify the stabilizing effect of AHDA on CsPbCl3 NCs, CsPbBr3 NCs and CsPbI2Br NCs, toluene and MeOAc were also used for dissolution-precipitation purification. After multiple cycles, purified PNCs with good optical properties and morphology were obtained.
[0010] AHDA was used to stabilize FAPbI3 NCs to synthesize AHDA-FAPbI3 NCs. First, 1-octadecene (ODE), AHDA, and lead iodide (PbI2) were vacuum degassed and dried at 110-130°C for 1-2h in a mass ratio of 1:(50-100):(10-50); then, dry BTMPA (the mass ratio of BTMPA to AHDA was 1:150-200) was added at the same temperature, and after the mixed solution became clear, FA-oleate precursor (the volume of FA-oleate precursor was about the same as that of BTMP) was quickly added at 70-150°C in an Ar atmosphere. The volume ratio of A to A was 1:2-10 and 1-10:1 to prepare FA-less and FA-rich FAPbI3NCs respectively); the reaction mixture was cooled to room temperature by ice-water bath, and then methyl acetate (MeOAc) was added for reverse precipitation. The volume of MeOAc was 1-5 times the total volume of the mixed solution after adding the cesium oleate precursor. When no more precipitation was precipitated, AHDA-FAPbI3(FA-less)NCs and AHDA-FAPbI3(FA-rich)NCs were obtained by centrifugation. Finally, in order to verify the stabilizing effect of AHDA on FAPbI3(FA-less)NCs and FAPbI3(FA-rich)NCs, toluene and MeOAc were also used for dissolution-precipitation purification. After multiple cycles, purified FAPbI3NCs with good optical properties and morphology were obtained.
[0011] The method of the present invention has the following advantages: first, it is the first time that the diamino ligand (AHDA) is proposed to be used as a ligand for stabilizing perovskite nanocrystals. The method is innovative and easy to operate. The diamino-stabilized perovskite nanocrystals have a novel structure and stable properties. Second, the method of AHDA stabilizing PNCs has an effective stabilizing effect on a series of PNCs that are unstable to the environment, including CsPbI3, CsPbBr3, CsPbCl3 and FAPbI3, and the stabilizing effect is outstanding. The obtained series of AHDA-PNCs can maintain optical properties and morphology for more than 110 days, and can even maintain for more than 15 purification cycles. This stability has surpassed the stabilizing effect of all reported ligands for stabilizing perovskite nanocrystals on nanocrystals. In addition, its mechanism of stabilizing PNCs is also applicable to inorganic Cs3Bi2X9 NCs, Cs2AgInX6 NCs, Cs3Cu2X5 NCs, Rb3Cu2X5 NCs and organic-inorganic hybrid FA3Bi2X9 NCs, FA2AgInX6 NCs, FA3Cu2X5 NCs and MA3Bi2X9NCs, MA2AgInX6 NCs, MA3Cu2X5NCs, Rb a Cs 1-a PbX3(0≤a≤1),FA a GA 1-a PbX3 (0≤a≤1, FA=formamidine, GA=guanidine) or DMAPbX3 (DMA=dimethylamine) (X=Cl, Br, I); thirdly, the synthesis method of AHDA-stabilized perovskite nanocrystals is simple and easy to industrialize, which can greatly promote the application of PNCs in optoelectronic fields such as red photon sources, solar cells and photocatalysis. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 The NMR spectra of AHDA-CsPbI3 NCs, BTMPA and AHDA prepared in Example 1;
[0013] Figure 2 UV absorption (left) and fluorescence (right) spectra of CsPbI3 NCs during 15 purification cycles of AHDA-CsPbI3 NCs prepared in Example 1;
[0014] Figure 3 The fluorescence quantum efficiency spectrum of CsPbI3 NCs during 15 purification cycles of AHDA-CsPbI3 NCs prepared in Example 1;
[0015] Figure 4 The fluorescence lifetime spectrum of CsPbI3 NCs during 15 purification cycles of AHDA-CsPbI3 NCs prepared in Example 1;
[0016] Figure 5 TEM image of CsPbI3 NCs during 15 purification cycles of AHDA-CsPbI3 NCs prepared in Example 1;
[0017] Figure 6 X-ray diffraction (XRD) spectrum of CsPbI3 NCs during 15 purification cycles of AHDA-CsPbI3 NCs prepared in Example 1;
[0018] Figure 7 Fluorescence spectra of (a) CsPbCl3 NCs, (b) CsPbBr3 NCs, and (c) CsPbI2Br NCs during 6 purification cycles of AHDA-CsPbX3 NCs prepared in Example 2;
[0019] Figure 8 TEM images of (a) CsPbCl3 NCs, (b) CsPbBr3 NCs, and (c) CsPbI2Br NCs after 6 purification cycles of AHDA-CsPbX3 NCs prepared in Example 2;
[0020] Fig. 9 Fluorescence spectra of (a) AHDA-FAPbI3(FA-less) NCs and (b) AHDA-FAPbI3(FA-rich) NCs prepared in Example 3 during 6 purification cycles;
[0021] Fig.10 TEM images of (a) AHDA-FAPbI3(FA-less) NCs and (b) AHDA-FAPbI3(FA-rich) NCs prepared in Example 3 after 6 purification cycles. DETAILED DESCRIPTION
[0022] Example 1
[0023] 10 mL ODE, 510 mg AHDA and 200 mg PbI2 (the mass ratio of the three is about 1:63.75:25) were placed in a 250 mL three-necked flask, vacuum degassed and dried at 120 ° C for 1 h; then, dried BTMPA (3 mL) was injected into the three-necked flask at this temperature. After the solution became clear, the temperature was set to a suitable temperature (80 ° C), and 1.6 mL of cesium oleate precursor (0.0625 M, preheated to 70 ° C) was quickly injected under Ar atmosphere for 150 s; the reaction mixture was cooled to room temperature by ice water bath, 32 mL MeOAc was added for reverse precipitation, and no more precipitation was precipitated, and then centrifuged at 8800 rpm for 5 minutes to obtain AHDA-CsPbI3 NCs were precipitated with a mass of 70 mg; the precipitate was then redispersed in 4 mL of toluene, 12 mL of MeOAc was added for precipitation, and the mixture was centrifuged again at 8800 rpm for 5 minutes to obtain AHDA-stabilized purified CsPbI3 NCs, namely AHDA-CsPbI3 NCs; finally, in order to verify the stabilizing effect of AHDA on CsPbI3 NCs, the above-mentioned toluene and MeOAc were continued to be used for dissolution-precipitation purification treatment, and after 15 purification cycles of the AHDA-stabilized CsPbI3 NCs, CsPbI3 NCs that still maintained good optical properties and morphology were obtained.
[0024] Figure 1 The NMR spectrum of the prepared AHDA-CsPbI3 NCs is given in the article. There is an obvious chemical shift peak of AHDA in the NMR spectrum of PNCs, which proves that AHDA-CsPbI3 NCs are successfully prepared. At the same time, the NMR spectra of BTMPA and AHDA are compared, and it is found that there are almost no BTMPA molecules on the surface of CsPbI3 PNCs, indicating that it is passivated by only one type of ligand, namely AHDA.
[0025] Figure 2 The ultraviolet absorption and fluorescence spectra of AHDA-CsPbI3 NCs during 15 purification cycles are given in the figure. It can be seen from the spectra that CsPbI3 NCs can always maintain good absorption and fluorescence properties during the 15 purification processes, indicating that the new diamino ligand (AHDA) of titanite nanocrystals has an effective stabilizing effect on the crystal structure of CsPbI3 NCs.
[0026] Figure 3The spectrum of the change in fluorescence quantum yield of AHDA-CsPbI3 NCs during 15 purification cycles is given in the figure. It can be seen that the fluorescence quantum yield of CsPbI3 NCs remains basically unchanged at around 60% during the 15 purification processes, which also proves that the new diamino ligand (AHDA) of titanite nanocrystals has an effective stabilizing effect on the crystal structure of CsPbI3 NCs.
[0027] Figure 4 The fluorescence lifetime change spectrum of AHDA-CsPbI3 NCs during 15 purification cycles is given in the figure. It can be seen that the fluorescence quantum lifetime of CsPbI3 NCs remains basically unchanged during the 15 purifications, which once again proves that the new diamino ligand (AHDA) of titanite nanocrystals has an effective stabilizing effect on the crystal structure of CsPbI3 NCs.
[0028] Figure 5 The TEM images of AHDA-CsPbI3 NCs during 15 purification cycles are given in the figure. It is observed that the morphology of CsPbI3 NCs did not change significantly after different numbers of purification cycles until the 15th purification cycle, and the average particle size remained at around 9 nm without growth or degradation. This proves that the new diamino ligand (AHDA) of titanite nanocrystals has an effective stabilizing effect on the crystal morphology and structure of CsPbI3 NCs.
[0029] Figure 6 The X-ray diffraction (XRD) spectra of AHDA-CsPbI3 NCs during 15 purification cycles are given in the figure. It is observed that the full width half maximum value and diffraction intensity of PNCs remain basically unchanged, further proving that AHDA-PNCs have a stable perovskite phase and particle size during the 15 purification processes, once again proving that the new diamino ligand (AHDA) of titanite nanocrystals has an effective stabilizing effect on the crystal morphology and structure of CsPbI3 NCs.
[0030] Example 2
[0031] Inorganic CsPbX3 PNCs of other components were synthesized according to the synthetic route of AHDA-CsPbI3 NCs. Different Pb sources were used to replace PbI2, i.e., 120 mg PbCl2, 160 mg PbBr2, 53 mg PbBr2, and 133 mg PbI2 were used to prepare CsPbCl3, CsPbBr3, and CsPbI2Br NCs, respectively. The purification process of CsPbI2Br NCs was the same as that of AHDA-CsPbI3 NCs prepared in Example 1. Finally, in order to verify the stabilizing effect of AHDA on CsPbX3 PNC, the purification cycle method in Example 1 was continued to be used, and toluene and MeOAc were used for dissolution-precipitation purification treatment. The AHDA-stabilized CsPbCl3NCs, CsPbBr3NCs and CsPbI2BrNCs were purified for 6 cycles, and CsPbX3NCs with good optical properties and morphology were obtained.
[0032] Figure 7 The fluorescence change spectra of AHDA-CsPbX3 NCs during the six purification cycles are given in the figure. It can be observed from the spectra that during the six purification cycles, (a) CsPbCl3 NCs, (b) CsPbBr3 NCs and (c) CsPbI2Br NCs all maintained good fluorescence properties, indicating that the new diamino ligand (AHDA) of titanite nanocrystals has a universal and effective stabilizing effect on the crystal structure of CsPbX3 NCs.
[0033] Figure 8 The TEM images of AHDA-CsPbX3 NCs after 6 purification cycles are given in the figure. It can be seen from the images that (a) CsPbCl3 NCs, (b) CsPbBr3 NCs and (c) CsPbI2Br NCs all maintain good morphology after 6 purification cycles, which once again proves that the new diamino ligand (AHDA) of titanite nanocrystals has a universal and effective stabilizing effect on the crystal morphology and structure of CsPbX3 NCs.
[0034] Example 3
[0035] AHDA was used to stabilize FAPbI3 NCs, thereby synthesizing AHDA-FAPbI3 NCs. First, 10 mL of ODE, 510 mg of AHDA, and 200 mg of PbI2 were added to a 250 mL three-necked flask, and vacuum degassed and dried at 120 ° C for 1 h; then dry BTMPA (3 mL) was added to the three-necked flask, and after the solution became clear, the temperature was set to a suitable temperature (130 ° C), and 0.4 mL and 9 mL of FA-oleate precursor were quickly injected under Ar atmosphere to prepare FA-poor and FA-rich FAPbI3 NCs; the reaction mixture was cooled to room temperature by an ice-water bath, and then 32 mL of methyl acetate (MeOAc) was added for reverse precipitation. When no more precipitate was precipitated, AHDA-FAPbI3(FA-less)NCs and AHDA-FAPbI3(FA-rich)NCs were obtained by centrifugation, and the product mass was 80 mg; finally, in order to verify the stabilizing effect of AHDA on FAPbI3(FA-less)NCs and FAPbI3(FA-rich)NCs, the purification cycle method in Example 1 was continued to be used, and toluene and MeOAc were used for dissolution-precipitation purification treatment. The AHDA-stabilized FAPbI3(FA-less)NCs and FAPbI3(FA-rich)NCs were purified for 6 cycles, and FAPbI3 NCs with good optical properties and morphology were obtained.
[0036] Fig. 9 The fluorescence spectra of (a) AHDA-FAPbI3(FA-less) NCs and (b) AHDA-FAPbI3(FA-rich) NCs during 6 purification cycles are given in the figure. It can be observed from the spectra that both FAPbI3(FA-less) NCs and FAPbI3(FA-rich) NCs have maintained good fluorescence properties during the 6 purification cycles, indicating that the new diamino ligand (AHDA) of titanite nanocrystals also has an effective stabilizing effect on the crystal structure of FAPbI3 NCs.
[0037] Fig.10 The TEM images of (a) AHDA-FAPbI3(FA-less) and (b) AHDA-FAPbI3(FA-rich) NCs after 6 purification cycles are given. It can be seen from the photos that after 6 purification cycles, both FAPbI3(FA-less) NCs and FAPbI3(FA-rich) NCs maintained good particle morphology, which once again proves that the new diamino ligand (AHDA) of titanite nanocrystals also has a universal and effective stabilizing effect on the crystal morphology and structure of FAPbI3 NCs.
Claims
1. A method for stabilizing perovskite nanocrystals using diamino ligands, characterized in that: First, 1-octadecene, AHDA and a lead source are mixed in a mass ratio of 1: (50-100): (10-50), and vacuum degassed and dried at 110-130° C. for 1-2 hours; then, dry bis(2,4,4-trimethylpentyl)-phosphinic acid BTMPA is added at the same temperature, and the mass ratio of BTMPA to AHDA is 1: 150-200. After the mixed solution becomes clear, it is heated at 70-180° C. and Ar Rapidly inject cesium oleate precursor under atmosphere to react for 10 to 300 seconds, the volume ratio of cesium oleate precursor to BTMPA is 8:2 to 30; cool the reaction product to room temperature in an ice-water bath, then add methyl acetate MeOAc for reverse precipitation, the volume of MeOAc is 1 to 5 times the total volume of the mixed solution after adding the cesium oleate precursor, and centrifuge until no more precipitation is precipitated to obtain double amino ligand stabilized perovskite nanocrystals AHDA-CsPbI3 NCs, AHDA-CsPbCl3 NCs, AHDA-CsPbBr3 NCs or AHDA-CsPbI2Br NCs precipitation; wherein the lead source is PbI2, PbCl2, PbBr2 or a mixture of PbBr2 and PbI2, and the structural formula of AHDA is as follows, 2. A diamino ligand-stabilized perovskite nanocrystal AHDA-CsPbI3 NCs, AHDA-CsPbCl3 NCs, AHDA-CsPbBr3 NCs or AHDA-CsPbI2Br NCs, characterized in that: The method is prepared by the method of claim 1.
3. A method for stabilizing perovskite nanocrystals using diamino ligands, characterized in that: First, 1-octadecene, AHDA and PbI2 are mixed in a mass ratio of 1: (50-100): (10-50), and vacuum degassed and dried at 110-130° C. for 1-2 hours; then, dry bis(2,4,4-trimethylpentyl)-phosphinic acid BTMPA is added at the same temperature, and the mass ratio of BTMPA to AHDA is 1: 150-200. After the mixed solution becomes clear, FA-oleic acid precursor is quickly added at 70-150° C. and in an Ar atmosphere, and the volume ratio of the FA-oleic acid precursor to the volume of BTMPA is 1: 2-10 or 1-10: 1; the reaction mixture is cooled to room temperature by an ice-water bath, and then methyl acetate MeOAc is added for reverse precipitation, and the volume of MeOAc is 1-5 times the total volume of the mixed solution after the cesium oleate precursor is added. When no more precipitation is precipitated, AHDA-FAPbI3FA-less is obtained by centrifugation. NCs or AHDA-FAPbI3FA-rich NCs precipitation.
4. A diamino ligand-stabilized perovskite nanocrystal AHDA-FAPbI3 FA-less NCs or AHDA-FAPbI3 FA-rich NCs, characterized in that: The method is prepared by the method described in claim 3.