Anti-glare film
By setting specific anti-glare layer parameters and material combinations, an anti-glare film with high anti-glare properties and transmission image clarity is designed, which solves the problems in the existing technology of reduced light transmittance and difficulty in suppressing glare in displays, and realizes display performance improvement.
Patent Information
- Application Number
- CN202111330165.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2018-06-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2038-06-25
AI Technical Summary
Although the existing anti-glare film can prevent external light from being reflected when installed on the surface of the display, it will reduce the light transmittance of the display, leading to a decrease in display performance, and it is difficult to quantitatively evaluate and suppress the glare problem of the display.
By setting the haze value of the anti-glare layer to be above 50% and below 99%, the standard deviation of the brightness distribution to be above 0 and below 6, and the transmission image clarity of the light comb width to be above 0% and below 60%, a combination of various The phase-separated structure of the resin component and the acrylic UV-curable compound of nanosilica are used to design an anti-glare film with high anti-glare properties and transmission image clarity.
It achieves quantitative evaluation and suppression of display glare, ensures the design freedom of display anti-glare properties and transmission image clarity, and avoids display glare and image blur problems.
Smart Images

Figure CN114167530B_ABST
Abstract
Description
[0001] This application is a divisional application of an application with an application date of June 25, 2018, application number 201880037117.3, and invention name “Anti-glare film”. Technical Field
[0002] The present invention relates to an anti-glare film for preventing external light from being reflected onto a display surface. Background Art
[0003] The anti-glare film is a film having an anti-glare layer with irregularities formed on the surface by, for example, surface roughening, and is attached to the surface of a display to scatter external light and prevent external light from being reflected on the display surface.
[0004] As methods for forming projections and depressions on the surface of the anti-glare layer, for example, there can be cited: a method of dispersing microparticles (fillers) in the anti-glare layer as disclosed in Patent Document 1; a method of utilizing a phase separation structure formed by spinodal decomposition of liquid phases of multiple polymers as disclosed in Patent Document 2; a method of transferring and molding projections and depressions using a mold as disclosed in Patent Document 3, etc.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2009-109702
[0008] Patent Document 2: Japanese Patent No. 3559505
[0009] Patent Document 3: Japanese Patent Application Publication No. 2014-102356 Summary of the invention
[0010] Problem that the invention aims to solve
[0011] When an anti-glare film is installed on the surface of a display, although it can prevent external light from being reflected on the display surface, on the other hand, the light from the display is sometimes affected by the anti-glare film, and the display performance of the display through the anti-glare film is reduced. Therefore, it is desired that the anti-glare film has a high degree of freedom in designing the clarity of the transmitted image.
[0012] In addition, if an anti-glare film is installed on the surface of a display having high-definition pixels, the light from the display that passes through the anti-glare film is refracted due to the surface roughness of the anti-glare layer, or the pixels of the display are magnified due to the lens effect caused by the surface roughness of the anti-glare layer, which may cause the display to be glaring and make it difficult to observe the image.
[0013] As a method for suppressing the glare of the display, for example, reducing the surface unevenness of the anti-glare layer can be considered, but there is a risk of reducing the anti-glare property of the anti-glare film. In addition, there is a problem that the glare of the display is difficult to quantitatively evaluate, and it may be difficult to develop an anti-glare film that can effectively suppress the glare of the display according to objective indicators.
[0014] Therefore, an object of the present invention is to provide an anti-glare film having good anti-glare properties and capable of suppressing display glare while having high design freedom for transmission image clarity by quantitatively evaluating display glare and performing design.
[0015] Solutions to the problem
[0016] In order to solve the above-mentioned problem, one embodiment of the present invention has an anti-glare layer having a haze value in the range of greater than 50% and less than 99%, the standard deviation of the brightness distribution of the display when installed on the surface of the display is in the range of greater than 0 and less than 6, and the clarity of the transmitted image with a light comb width of 0.5 mm is in the range of greater than 0% and less than 60%.
[0017] Here, the value of the standard deviation of the brightness distribution of the display indicates the degree of irregularity of the bright spots on the display, and becomes an objective index that can quantitatively evaluate the glare of the display. Therefore, in the above-mentioned configuration, by setting the standard deviation to a value in the range of 0 or more and 6 or less to form an anti-glare layer, the glare of the display can be quantitatively evaluated to design an anti-glare film. Therefore, compared with, for example, a case where a tester subjectively evaluates glare through naked eye observation, an anti-glare film that can effectively suppress the glare of the display can be stably obtained.
[0018] In addition, by setting the haze value of the anti-glare layer to a value in the range of 50% to 99% while setting the standard deviation to a given value, good anti-glare properties can be obtained while suppressing the glare of the display. In addition, by setting the clarity of the transmitted image of the anti-glare film at a light comb width of 0.5 mm to a value in the range of 0% to 60%, the design freedom of the clarity of the transmitted image of the anti-glare film can be widely ensured.
[0019] The anti-glare layer may contain a plurality of resin components and have a co-continuous phase structure formed by phase separation of the plurality of resin components. By utilizing such a co-continuous phase structure, it is easy to obtain good anti-glare properties while suppressing the glare of the display.
[0020] The anti-glare layer may contain at least one of an acrylic ultraviolet curable compound containing nano-silica and urethane acrylate, an acrylic copolymer, and cellulose acetate propionate. Thus, an anti-glare film having anti-glare properties and capable of suppressing the glare of a display can be easily manufactured.
[0021] The anti-glare layer may include a matrix resin and a plurality of fine particles dispersed in the matrix resin, wherein a difference in refractive index between the fine particles and the matrix resin is a value in a range of 0 to 0.07.
[0022] Thus, the anti-glare layer can be constituted by using the matrix resin and the plurality of fine particles, and an anti-glare film having anti-glare properties and capable of suppressing glare of a display can be easily manufactured.
[0023] The ratio G2 / G1 of the weight G1 of the matrix resin of the anti-glare layer to the total weight G2 of the plurality of microparticles contained in the anti-glare layer may be a value in the range of 0.07 to 0.20. Thus, the anti-glare film having an anti-glare layer having a structure in which a plurality of microparticles are dispersed in a matrix resin can be well manufactured.
[0024] Effects of the Invention
[0025] According to the present invention, by quantitatively evaluating the glare of a display, it is possible to design an anti-glare film having good anti-glare properties and capable of suppressing the glare of a display while having a high degree of design freedom for a transmission image clarity. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] [ Figure 1 ] is a cross-sectional view showing the structure of the anti-glare film of the first embodiment.
[0027] [ Figure 2 ] is a diagram showing a method for manufacturing an anti-glare film according to a second embodiment.
[0028] [ Figure 3 ]Simplified diagram of the glare inspection machine.
[0029] Explanation of symbols
[0030] 1 Anti-glare film
[0031] 3 Anti-glare layer
[0032] 16a Display DETAILED DESCRIPTION
[0033] Hereinafter, embodiments of the present invention will be described with reference to the drawings.
[0034] (First embodiment)
[0035] Figure 1 1 is a cross-sectional view showing the structure of the anti-glare film 1 according to the first embodiment. The anti-glare film 1 is mounted on a display device 16 (see Figure 3 ) on the surface of the display 16a. The anti-glare film 1 includes a base film 2, an anti-glare layer 3, and an adhesive layer 4.
[0036] The base film 2 is disposed between the display 16a and the anti-glare layer 3 to support the anti-glare layer 3. The adhesive layer 4 is disposed between the display 16a and the base film 2 to fix the anti-glare film 1 to the surface of the display 16a. The adhesive layer 4 is, for example, an optical paste and is made of a material that is unlikely to affect the optical properties of the anti-glare film 1.
[0037] The anti-glare layer 3 is formed on at least one side of the base film 2. The anti-glare layer 3 imparts anti-glare properties to the anti-glare film 1, scatters and reflects external light, and prevents external light from being reflected on the surface of the display 16a. The anti-glare layer 3 also functions as a hard coating (HC) layer that protects the surface of the display 16a. As an example, the anti-glare layer 3 includes a plurality of resin components that can undergo phase separation.
[0038] When the anti-glare film 1 is mounted on the surface of the display 16a, the standard deviation of the brightness distribution of the display 16a is set to a value in the range of 0 to 6, and the clarity of the transmitted image with a comb width of 0.5 mm is set to a value in the range of 0% to 60%. The haze value of the anti-glare layer 3 is set to a value in the range of 50% to 99%.
[0039] The haze value shown in this embodiment is a value measured by a method based on JIS K7136.
[0040] The value of the standard deviation can be appropriately set within the above range, preferably a value in the range of 0 to 5.5, and more preferably a value in the range of 0 to 5.0. In addition, the value of the transmission image clarity (imaging) at a comb width of 0.5 mm can also be appropriately set within the above range, preferably a value in the range of 0% to 55%, and more preferably a value in the range of 0% to 50%.
[0041] The haze value of the antiglare layer 3 can be appropriately set within the above range, and is preferably a value within the range of 50% to 90%, and more preferably a value within the range of 50% to 85%.
[0042] Thus, in the present embodiment, the value of the standard deviation of the brightness distribution of the display 16a represents the degree of irregularity of the bright spots on the display 16a, and becomes an objective indicator capable of quantitatively evaluating the glare of the display 16a. Based on this, by constructing the anti-glare film 1 in a manner in which the standard deviation is set to a value in the range of greater than 0 and less than 6, the anti-glare film 1 can be designed by quantitatively evaluating the glare of the display 16a.
[0043] Therefore, compared with, for example, a case where a tester subjectively evaluates the glare of the display 16 a by visual observation, it is possible to stably obtain the anti-glare film 1 that can effectively suppress the glare of the display 16 a .
[0044] Furthermore, by setting the standard deviation of the anti-glare film 1 to a given value and setting the haze value of the anti-glare layer 3 to a value in the range of 50% to 99%, it is possible to obtain good anti-glare properties while suppressing the glare of the display 16a. Furthermore, by setting the clarity of the transmitted image of the anti-glare film 1 at a light comb width of 0.5 mm to a value in the range of 0% to 60%, it is possible to widely ensure the design freedom of the clarity of the transmitted image of the anti-glare film 1.
[0045] In addition, the anti-glare layer 3 of the present embodiment includes multiple resin components and has a co-continuous phase structure formed by phase separation of the multiple resin components. By utilizing such a co-continuous phase structure, in the anti-glare film 1, it is easy to obtain good anti-glare properties while suppressing the glare of the display 16a.
[0046] In addition, the anti-glare layer 3 of the present embodiment comprises at least one (here both) of acrylic copolymer, cellulose acetate propionate, and acrylic ultraviolet curable compound containing nano-silica and urethane acrylate. Thus, it is possible to easily manufacture an anti-glare film 1 that can suppress the glare of the display 16a and has anti-glare properties. Below, the specific examples of the substrate film 2 and the anti-glare layer 3 are described.
[0047] Examples of the material of the base film 2 include glass, ceramics, and resins. As the resin, the same resin as the material of the antiglare layer 3 can be used. Preferred materials for the substrate film 2 include transparent polymers, such as cellulose derivatives (cellulose acetate such as triacetate (TAC) and cellulose diacetate), polyester resins (polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), polyarylate resins, etc.), polysulfone resins (polysulfone, polyethersulfone (PES), etc.), polyetherketone resins (polyetherketone (PEK), polyetheretherketone (PEEK), etc.), polycarbonate resins (PC), polyolefin resins (polyethylene, polypropylene, etc.), cyclic polyolefin resins (films manufactured by JSR Corporation [ARTON] (registered trademark), films manufactured by Zeon Corporation [ZEONEX] (registered trademark)), halogen-containing resins (polyvinylidene chloride, etc.), (meth) acrylic resins, styrene resins (polystyrene, etc.), vinyl acetate or vinyl alcohol resins (polyvinyl alcohol, etc.).
[0048] The base film 2 may be uniaxially or biaxially stretched, and is preferably an optically isotropic film with a low refractive index. Examples of the optically isotropic base film 2 include unstretched films.
[0049] The thickness of the base film 2 can be appropriately set, and is, for example, preferably 5 μm to 2000 μm, more preferably 15 μm to 1000 μm, and still more preferably 20 μm to 500 μm.
[0050] [Structure of anti-glare layer]
[0051] The anti-glare layer 3 of the first embodiment has a phase separation structure of multiple resin components. As an example, the anti-glare layer 3 has a plurality of elongated (rope-like or line-like) convex portions formed on the surface through the phase separation structure of multiple resin components. The elongated convex portions are branched to form a co-continuous phase structure in a dense state.
[0052] The anti-glare layer 3 exhibits anti-glare properties by means of a plurality of elongated convex portions and concave portions located between adjacent elongated convex portions. The anti-glare film 1 is provided with such an anti-glare layer 3, so that it is a film having an excellent balance between haze value and transmission image clarity (imaging properties). The surface of the anti-glare layer 3 has a reticular structure, i.e., a plurality of continuous or partially missing irregular ring structures, because the elongated convex portions are formed into a roughly reticular shape.
[0053] As for the surface of the anti-glare layer 3, the formation of lens-shaped (island-shaped) convex parts can be prevented by forming the above-mentioned structure. As a result, it is possible to prevent the light from the display 16a passing through the anti-glare layer 3 from being refracted due to the surface unevenness of the anti-glare layer 3, or to prevent the pixels of the display 16a from being magnified and observed due to the lens effect caused by the surface unevenness of the anti-glare layer 3, thereby suppressing the glare of the display 16a. As a result, even if the anti-glare film 1 is installed on the display 16a with high-definition pixels, the glare of the display 16a can be highly suppressed while ensuring the anti-glare property, and the blurring of text and images and the change of color tone can also be suppressed.
[0054] It should be noted that the plurality of elongated convex portions may be independent of each other or connected together. The phase separation of the anti-glare layer 3 is as follows, and can be formed by spinodal decomposition (wet spinodal decomposition) from a liquid phase using a solution that is a raw material of the anti-glare layer 3. For details of the anti-glare layer 3, for example, reference may be made to the record of Japanese Patent Application No. 2012-231496.
[0055] [Material of anti-glare layer]
[0056] The plurality of resin components contained in the antiglare layer 3 may be phase-separable, and preferably contain a polymer and a curable resin from the viewpoint of obtaining an antiglare layer 3 having elongated protrusions and high scratch resistance.
[0057] As the polymer contained in the anti-glare layer 3, thermoplastic resins can be cited. As thermoplastic resins, styrene resins, (meth) acrylic resins, organic acid vinyl ester resins, vinyl ether resins, halogen-containing resins, olefin resins (including alicyclic olefin resins), polycarbonate resins, polyester resins, polyamide resins, thermoplastic polyurethane resins, polysulfone resins (polyethersulfone, polysulfone, etc.), polyphenylene ether resins (polymers of 2,6-xylenol, etc.), cellulose derivatives (cellulose esters, cellulose carbamates, cellulose ethers, etc.), silicone resins (polydimethylsiloxane, polymethylphenylsiloxane, etc.), rubbers or elastomers (polybutadiene, polyisoprene and other diene rubbers, styrene-butadiene copolymers, acrylonitrile-butadiene copolymers, acrylic rubbers, urethane rubbers, silicone rubbers, etc.), etc. These thermoplastic resins can be used alone or in combination of two or more.
[0058] In addition, the polymer may include a material having a functional group that participates in a curing reaction or a functional group that reacts with a curable compound. The polymer may have a functional group in a main chain or a side chain.
[0059] Examples of the functional group include condensable groups, reactive groups (e.g., hydroxyl groups, acid anhydride groups, carboxyl groups, amino groups or imino groups, epoxy groups, glycidyl groups, isocyanate groups, etc.), polymerizable groups (e.g., vinyl groups, propenyl groups, isopropenyl groups, butenyl groups, allyl groups, etc.), 2-6 Alkenyl, ethynyl, propynyl, butynyl, etc. 2-6 Alkynyl, vinylidene, etc. 2-6 Alkenylene, or a group having these polymerizable groups (such as (meth)acryloyl group), etc. Among these functional groups, the polymerizable group is preferred.
[0060] In addition, the anti-glare layer 3 may also include a plurality of types of polymers. Each of the above-mentioned polymers may be phase-separated by spinodal decomposition from the liquid phase, or may be mutually incompatible. The combination of the first polymer and the second polymer included in the plurality of types of polymers is not particularly limited, and materials that are mutually incompatible near the processing temperature may be used.
[0061] For example, when the first polymer is a styrene resin (polystyrene, styrene-acrylonitrile copolymer, etc.), examples of the second polymer include cellulose derivatives (e.g., cellulose esters such as cellulose acetate propionate), (meth) acrylic resins (polymethyl methacrylate, etc.), alicyclic olefin resins (polymers with norbornene as a monomer, etc.), polycarbonate resins, polyester resins (polyC 2-4 Alkylene aromatic ester copolyesters, etc.
[0062] For example, when the first polymer is a cellulose derivative (e.g., cellulose esters such as cellulose acetate propionate), examples of the second polymer include styrene resins (polystyrene, styrene-acrylonitrile copolymers, etc.), (meth) acrylic resins, alicyclic olefin resins (polymers containing norbornene as a monomer, etc.), polycarbonate resins, polyester resins (polyC 2-4 Alkylene aromatic ester copolyesters, etc.
[0063] The plurality of types of polymers may include at least cellulose esters (e.g., cellulose diacetate, cellulose triacetate, cellulose acetate propionate, cellulose acetate butyrate, etc.) 2-4 alkyl carboxylates).
[0064] Here, the phase separation structure of the anti-glare layer 3 can be fixed by curing the precursor of the curable resin contained in the various resin components by active energy rays (ultraviolet rays or electron beams, etc.), heat, etc. when manufacturing the anti-glare layer 3. In addition, the anti-glare layer 3 can be given scratch resistance and durability by such a curable resin.
[0065] From the viewpoint of the scratch resistance of the anti-glare layer 3, at least one polymer included in the plurality of types of polymers is preferably a polymer having a functional group that can react with a curable resin precursor in a side chain. As the polymer forming the phase separation structure, in addition to the two mutually incompatible polymers, thermoplastic resins and other polymers can also be included. The weight ratio M1 / M2 of the weight M1 of the first polymer and the weight M2 of the second polymer and the glass transition temperature of the polymer can be appropriately set.
[0066] Examples of curable resin precursors include curable compounds having functional groups that react with active energy rays (ultraviolet rays or electron beams), heat, etc., and that can be cured or crosslinked by the functional groups to form resins (particularly cured resins or crosslinked resins).
[0067] Examples of such compounds include thermosetting compounds or thermosetting resins (low molecular weight compounds having epoxy groups, polymerizable groups, isocyanate groups, alkoxysilyl groups, silanol groups, etc. (e.g., epoxy resins, unsaturated polyester resins, urethane resins, silicone resins, etc.)), photocurable (ionizing radiation curable) compounds that are cured by ultraviolet rays, electron beams, etc. (ultraviolet curable compounds such as photocurable monomers and oligomers, etc.), and the like.
[0068] As a preferred curable resin precursor, photocurable compounds that cure in a short time due to ultraviolet rays, electron beams, etc. can be cited. Among them, ultraviolet curable compounds are particularly practical. In order to improve resistance such as scratch resistance, the photocurable compound preferably has more than 2 (preferably 2 to 15, and more preferably about 4 to 10) polymerizable unsaturated bonds in the molecule. Specifically, the photocurable compound is preferably epoxy (meth) acrylate, urethane (meth) acrylate, polyester (meth) acrylate, siloxane (meth) acrylate, and a multifunctional monomer having at least 2 polymerizable unsaturated bonds.
[0069] The curable resin precursor may also contain a curing agent corresponding to its type. For example, a thermosetting resin precursor may contain a curing agent such as an amine or a polycarboxylic acid, and a photopolymerization initiator may be contained in a photocurable resin precursor. As the photopolymerization initiator, conventional components such as acetophenones or propiophenones, benzyls, benzoins, benzophenones, thioxanthones, acylphosphine oxides, etc. may be cited.
[0070] Furthermore, the curable resin precursor may contain a curing accelerator. For example, the photocurable resin precursor may contain a photocuring accelerator such as a tertiary amine (dialkylaminobenzoic acid ester, etc.), a phosphine-based photopolymerization accelerator, and the like.
[0071] In the manufacturing process of the anti-glare layer 3, at least two components of the polymer and curable resin precursor contained in the solution that will become the raw material of the anti-glare layer 3 are used in a combination that phase separates from each other near the processing temperature. As a combination that causes phase separation, for example, there can be mentioned: (a) a combination in which multiple types of polymers are incompatible with each other and phase separation occurs; (b) a combination in which a polymer and a curable resin precursor are incompatible and phase separation occurs; or (c) a combination in which multiple types of curable resin precursors are incompatible with each other and phase separation occurs. Among these combinations, (a) a combination of multiple types of polymers, (b) a combination of a polymer and a curable resin precursor, and (a) a combination of multiple types of polymers is particularly preferred.
[0072] Here, usually, the polymer and the cured resin or cross-linked resin generated by the curable resin precursor through curing have different refractive indices. In addition, usually, the refractive indices of multiple types of polymers (the first polymer and the second polymer) are also different from each other. The difference in refractive index between the polymer and the cured resin or cross-linked resin, and the difference in refractive index between multiple types of polymers (the first polymer and the second polymer) are preferably values in the range of 0 or more and 0.04 or less, and more preferably values in the range of 0 or more and 0.02 or less.
[0073] The anti-glare layer 3 may include a plurality of fine particles (fillers) dispersed in a matrix resin. The fine particles may be any of organic fine particles and inorganic fine particles, and the plurality of fine particles may include fine particles of a plurality of types.
[0074] As organic particles, cross-linked acrylic particles and cross-linked styrene particles can be cited. In addition, as inorganic particles, silicon dioxide particles and aluminum oxide particles can be cited. In addition, as an example, the difference in refractive index between the particles contained in the anti-glare layer 3 and the matrix resin can be set to a value in the range of 0 or more and 0.20 or less. The difference in refractive index is preferably a value in the range of 0 or more and 0.15 or less, and more preferably a value in the range of 0 or more and 0.07 or less.
[0075] The average particle size of the fine particles is not particularly limited, and can be, for example, 0.5 μm to 5.0 μm. The average particle size is preferably 0.5 μm to 3.0 μm, and more preferably 0.5 μm to 2.0 μm.
[0076] It should be noted that the so-called average particle size here is the 50% volume average particle size in the Coulter counter method (the same applies to the average particle size described below). The particles can be solid or hollow. If the average particle size of the particles is too small, it is difficult to obtain anti-glare properties. If it is too large, there is a hidden danger of increased glare on the display, so it is necessary to pay attention.
[0077] The thickness of the anti-glare layer 3 can be appropriately set, for example, preferably a value in the range of 0.3 μm or more and 20 μm or less, more preferably a value in the range of 1 μm or more and 15 μm or less, and further preferably a value in the range of 1 μm or more and 10 μm or less. Usually, it can be set to a value in the range of 2 μm or more and 10 μm or less (particularly a value in the range of 3 μm or more and 7 μm or less).
[0078] The antiglare film may be formed without the base film 2 . In this case, the thickness of the antiglare layer 3 is preferably, for example, 1 μm to 100 μm, more preferably 3 μm to 50 μm.
[0079] The anti-glare layer 3 may contain conventional additives within the range that does not impair the optical properties, such as organic or inorganic particles, stabilizers (antioxidants, ultraviolet absorbers, etc.), surfactants, water-soluble polymers, fillers, crosslinking agents, coupling agents, colorants, flame retardants, lubricants, waxes, preservatives, viscosity modifiers, tackifiers, leveling agents, defoaming agents, etc.
[0080] As for the manufacturing method of the anti-glare film 1 in the first embodiment, as an example, it includes the following steps: a preparation step of preparing a solution (hereinafter, also referred to as the solution) which is a raw material of the anti-glare layer 3; a formation step of applying the solution prepared in the preparation step to the surface of a given support (the substrate film 2 in this embodiment), evaporating the solvent in the solution, and forming a phase separation structure by spinodal decomposition from the liquid phase; and a curing step of curing the curable resin precursor after the formation step.
[0081] [Preparation process]
[0082] In the preparation process, a solution containing a solvent, a resin composition for constituting the anti-glare layer 3, and predetermined particles is prepared. The solvent can be selected according to the type and solubility of the polymer and curable resin precursor contained in the anti-glare layer 3. The solvent is a solvent that can at least uniformly dissolve the solid components (multiple types of polymers and curable resin precursors, reaction initiators, and other additives).
[0083] Examples of the solvent include ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc.), ethers (dimethyl The solvent may be selected from the group consisting of alkylene, tetrahydrofuran, etc., aliphatic hydrocarbons (hexane, etc.), alicyclic hydrocarbons (cyclohexane, etc.), aromatic hydrocarbons (toluene, xylene, etc.), halogenated carbons (methylene chloride, ethylene dichloride, etc.), esters (methyl acetate, ethyl acetate, butyl acetate, etc.), water, alcohols (ethanol, isopropanol, butanol, cyclohexanol, etc.), cellosolves (methyl cellosolve, ethyl cellosolve, etc.), cellosolve acetates, sulfoxides (dimethyl sulfoxide, etc.), amides (dimethylformamide, dimethylacetamide, etc.), etc. The solvent may also be a mixed solvent.
[0084] The resin composition preferably includes the thermoplastic resin, the photocurable compound, the photopolymerization initiator, the thermoplastic resin, and the photocurable compound. Alternatively, the resin composition preferably includes a plurality of mutually incompatible polymers, the photocurable compound, and the photopolymerization initiator.
[0085] The concentration of the solute (polymer and curable resin precursor, reaction initiator, other additives) in the solution can be adjusted within a range where phase separation of the various resin components occurs and within a range where the castability and coating properties of the solution are not impaired.
[0086] Here, the haze value of the anti-glare layer 3, the clarity of the transmitted image of the anti-glare film 1, and the standard deviation value (glare value) of the brightness distribution of the display 16a on which the anti-glare film 1 is mounted on the surface may vary depending on the combination of the resin composition in the solution, the weight ratio, or the construction conditions of the preparation process, the formation process, and the curing process. Therefore, the anti-glare layer can be formed by changing the various conditions, and the physical properties of the obtained anti-glare layer can be measured / understood in advance to obtain an anti-glare film with target physical properties.
[0087] [Formation process]
[0088] In the forming process, the solution prepared in the preparation process is cast or coated on the surface of the support (here as an example, the substrate film 2). As the casting method or coating method of the solution, conventional methods can be cited, for example: a spray coater, a spin coater, a roll coater, an air knife coater, a blade coater, a rod coater, a reverse coater, a wire rod coater, a notch wheel coater, a dip coater, an immersion extrusion coater, a die coater, a gravure coater, a micro gravure coater, a screen coater, etc.
[0089] The solvent is evaporated and removed from the solution cast or coated on the surface of the support by drying. As the solution is concentrated during the evaporation process, phase separation occurs due to spinodal decomposition of various resin components from the liquid phase, forming a phase separation structure with a relatively regular interphase distance (pitch or mesh diameter). The co-continuous phase structure of the elongated convex portions can be formed by setting drying conditions and ratios that can improve the melt fluidity of the resin components after the solvent is evaporated to a certain extent.
[0090] As for the evaporation of the solvent, it is preferably carried out by heat drying from the viewpoint that the elongated convex portions are easily formed on the surface of the anti-glare layer 3. If the drying temperature is too low or the drying time is too short, there is a hidden danger that insufficient heat is imparted to the resin component, the melt fluidity of the resin component is reduced, and the formation of the elongated convex portions becomes difficult, so it is necessary to pay attention.
[0091] On the other hand, if the drying temperature is too high or the drying time is too long, the temporarily formed elongated protrusions may flow and reduce their height, but the structure of the elongated protrusions is maintained. Therefore, the drying temperature and the drying time can be used as a means to adjust the anti-glare property and the slipperiness of the anti-glare layer 3 by changing the height of the elongated protrusions. In addition, in the formation process, a co-continuous phase structure in which phase separation structures are connected can be formed by increasing the evaporation temperature of the solvent or using a low-viscosity component in the resin component.
[0092] When a co-continuous phase structure is formed and coarsened as a result of phase separation caused by spinodal decomposition of multiple resin components from the liquid phase, the continuous phase becomes discontinuous and forms a droplet phase structure (an island structure of independent phases such as spheres, true spheres, disks, and ellipsoids). Here, depending on the degree of phase separation, an intermediate structure between the co-continuous phase structure and the droplet phase structure (a phase structure in the process of transition from the co-continuous phase to the droplet phase) may also be formed. After the solvent is removed, a layer with fine concavoconvexities on the surface is formed.
[0093] [Curing process]
[0094] In the curing step, the curable resin precursor in the solution is cured, thereby fixing the phase separation structure formed in the forming step to form the anti-glare layer 3. The curing of the curable resin precursor is carried out by heating or irradiation with active energy rays, or a combination of these methods, depending on the type of the curable resin precursor. The active energy rays to be irradiated are selected according to the type of photocurable components, etc.
[0095] The irradiation of active energy rays can be carried out in an inert gas atmosphere. When the active energy rays are ultraviolet rays, as the light source, there can be used: a far ultraviolet lamp, a low-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a halogen lamp, a laser light source (a light source such as a helium-cadmium laser or an excimer laser), etc.
[0096] It should be noted that when forming the adhesive layer 4, after preparing a solution containing an adhesive component, the solution can be applied / dried on the other side of the base film 2 by a conventional method, such as the casting method or coating method described in the formation step, so that the adhesive layer 4 can be formed.
[0097] By going through the above steps, the anti-glare film 1 of the first embodiment can be manufactured. It should be noted that, when a peelable support is used as the support, by peeling the anti-glare layer 3 from the support, an anti-glare film consisting only of the anti-glare layer 3 can be obtained. In addition, when a non-peelable support (preferably a transparent support such as a substrate film 2) is used as the support, an anti-glare film 1 having a laminated structure of a support (substrate film 2) and an anti-glare layer 3 can be obtained.
[0098] Here, as a method for suppressing the glare of the display 16a, for example, reducing the surface unevenness of the anti-glare layer can be considered, but there is a risk of reducing the anti-glare property of the anti-glare film. However, by not only reducing the unevenness of the anti-glare layer, but also increasing the number of unevenness while increasing the inclination of the unevenness of the anti-glare layer to make the unevenness steeper, the anti-glare property can be improved while suppressing the glare of the display.
[0099] In the first embodiment, such concavities and convexities can be formed in the anti-glare layer by the above-mentioned spinodal decomposition, and such concavities and convexities can also be formed in the anti-glare layer by other methods. For example, in the case where a plurality of particles are used to form the surface concavities and convexities of the anti-glare layer as described in the second embodiment, by selecting materials in a manner that the repulsive interaction between the particles and the resin and solvent other than the particles is enhanced when the anti-glare layer is formed, it is possible to cause appropriate aggregation of the particles and form a steep and high-density concavity and convexity distribution structure in the anti-glare layer. Therefore, the anti-glare layer of other embodiments is described below with the difference from the first embodiment as the center.
[0100] (Second embodiment)
[0101] The anti-glare layer of the anti-glare film of the second embodiment comprises a matrix resin and a plurality of microparticles dispersed in the matrix resin. The microparticles can be formed into a true sphere, but are not limited thereto, and can also be formed into a substantial sphere or ellipsoid. In addition, the microparticles can be formed into a solid shape or into a hollow shape. When the microparticles are formed into a hollow shape, the hollow part of the microparticles can be filled with air or other gases. In the anti-glare layer, each microparticle can be dispersed in the form of a primary particle, or can be dispersed with a plurality of secondary particles formed by the agglomeration of a plurality of microparticles.
[0102] The difference in refractive index between the matrix resin and the fine particles is set to a value in the range of 0 to 0.20. The difference in refractive index is more preferably a value in the range of 0 to 0.15, and more preferably a value in the range of 0 to 0.07.
[0103] The average particle size of the fine particles is set to a value in the range of 0.5 μm to 5.0 μm. The average particle size of the fine particles is more preferably a value in the range of 0.5 μm to 3.0 μm, and more preferably a value in the range of 0.5 μm to 2.0 μm.
[0104] Furthermore, the particle size dispersion of the fine particles is preferably small. For example, in the particle size distribution of the fine particles contained in the antiglare layer, the average particle size of 50% by weight or more of the fine particles contained in the antiglare layer is preferably controlled to be within a dispersion of 1.0 μm.
[0105] Thus, by using fine particles having a relatively uniform particle size and an average particle size set within the above range, uniform and appropriate irregularities can be formed on the surface of the anti-glare layer, thereby ensuring anti-glare properties while suppressing glare of the display 16a.
[0106] The ratio of the weight of the matrix resin in the anti-glare layer to the total weight of the plurality of microparticles can be appropriately set. In the present embodiment, the ratio G2 / G1 of the weight G1 of the matrix resin of the anti-glare layer to the total weight G2 of the plurality of microparticles contained in the anti-glare layer is set to a value in the range of 0.07 to 0.20. The ratio G2 / G1 is preferably a value in the range of 0.10 to 0.20, and more preferably a value in the range of 0.12 to 0.20.
[0107] The microparticles dispersed in the matrix resin may be any inorganic or organic microparticles, preferably having good transparency. As organic microparticles, plastic beads may be mentioned. As plastic beads, styrene beads (refractive index 1.59), melamine beads (refractive index 1.57), acrylic beads (refractive index 1.49), acrylic-styrene beads (refractive index 1.54), polycarbonate beads, polyethylene beads, etc. may be mentioned. Styrene beads may be cross-linked styrene beads, and acrylic beads may be cross-linked acrylic beads. Plastic beads preferably have a hydrophobic group on the surface. As such plastic beads, styrene beads may be mentioned.
[0108] Examples of the matrix resin include at least one of a photocurable resin that is cured by active energy rays, a solvent-drying resin that is cured by drying a solvent added during coating, and a thermosetting resin.
[0109] Examples of the photocurable resin include resins having acrylate functional groups, such as relatively low molecular weight polyester resins, polyether resins, acrylic resins, epoxy resins, urethane resins, alkyd resins, spiroacetal resins, polybutadiene resins, polythiol polyene resins, oligomers, prepolymers, and reactive diluents of (meth)acrylates of multifunctional compounds such as polyols.
[0110] Specific examples of these include monofunctional monomers such as ethyl (meth)acrylate, ethylhexyl (meth)acrylate, styrene, methylstyrene, and N-vinyl pyrrolidone, and polyfunctional monomers such as polymethylolpropane tri(meth)acrylate, hexanediol (meth)acrylate, tripropylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and neopentyl glycol di(meth)acrylate.
[0111] When the photocurable resin is an ultraviolet curable resin, it is preferred to use a photopolymerization initiator. Examples of the photopolymerization initiator include acetophenones, benzophenones, Michlerbenzoylbenzoate, α-amyl oxime esters, tetramethylthiuram monosulfide, and thioxanthones. In addition, it is also preferred to mix a photosensitizer with the photocurable resin. Examples of the photosensitizer include n-butylamine, triethylamine, and poly-n-butylphosphine.
[0112] As the solvent drying type resin, known thermoplastic resins can be cited. As the thermoplastic resin, styrene resins, (meth) acrylic resins, vinyl acetate resins, vinyl ether resins, halogen-containing resins, alicyclic olefin resins, polycarbonate resins, polyester resins, polyamide resins, cellulose derivatives, silicone resins, and rubber or elastomers can be cited. As the solvent drying type resin, a resin soluble in an organic solvent is preferred, and a resin soluble in an organic solvent and having excellent formability, film forming properties, transparency and weather resistance is particularly preferred. As such a solvent drying type resin, styrene resins, (meth) acrylic resins, alicyclic olefin resins, polyester resins, cellulose derivatives (cellulose esters, etc.) can be cited.
[0113] Here, when the material of the substrate film 2 is a cellulose resin such as triacetyl cellulose (TAC), a cellulose resin can be cited as a thermoplastic resin used in the solvent-drying resin. The cellulose resin can include cellulose derivatives such as nitrocellulose, cellulose acetate, butyl cellulose acetate, ethyl cellulose, methyl cellulose, cellulose acetate propionate, and ethyl hydroxyethyl cellulose. By using a cellulose resin as a solvent-drying resin, the substrate film 2 and the anti-glare layer 3 can be well adhered, and an anti-glare film 1 with excellent transparency can be obtained.
[0114] Examples of the solvent drying type resin include vinyl resins, acetal resins, acrylic resins, polystyrene resins, polyamide resins, and polycarbonate resins.
[0115] Examples of the thermosetting resin include phenolic resins, urea-formaldehyde resins, diallyl phthalate resins, melamine resins, guanamine resins, unsaturated polyester resins, polyurethane resins, epoxy resins, aminoalkyd resins, melamine-urea co-condensation resins, silicone resins, polysiloxane resins, etc. When a thermosetting resin is used as the base resin, at least any one of a crosslinking agent, a curing agent such as a polymerization initiator, a polymerization accelerator, a solvent, and a viscosity modifier may be used in combination.
[0116] As an example, the method for manufacturing the anti-glare film in the second embodiment includes the following steps: a preparation step of preparing a solution that serves as a raw material for the anti-glare layer 3; a coating step of applying the solution prepared in the preparation step onto the surface of a given support (the substrate film 2 in this embodiment); and a curing step of curing the resin in the applied solution.
[0117] [Preparation process]
[0118] In the preparation process, a solution containing a solvent, a resin composition for constituting an anti-glare layer, and microparticles is prepared. As the solvent, at least one of alcohols (isopropanol, methanol, ethanol, etc.), ketones (methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), cyclohexanone, etc.), esters (methyl acetate, ethyl acetate, butyl acetate, etc.), halogenated hydrocarbons, and aromatic hydrocarbons (toluene, xylene, etc.) can be mentioned. A known leveling agent can be further added to the solution. For example, by using a fluorine-based or silicone-based leveling agent, the anti-glare layer can be given good scratch resistance.
[0119] [Coating / curing process]
[0120] In the coating step, the solution prepared in the preparation step is cast or coated on the surface of a support (here, as an example, the base film 2) by the same method as in the first embodiment. The solvent is evaporated and removed from the solution cast or coated on the surface of the support by drying.
[0121] When the matrix resin is a photocurable resin, after the coating process, as an example, a curing process based on ultraviolet rays or electron beams is performed. As the ultraviolet light source, various mercury lamps, ultraviolet carbon arc lamps, black light lamps, and metal halide lamps can be cited. In addition, as the wavelength range of ultraviolet rays, for example, a wavelength range of 190 nm or more and 380 nm or less can be cited.
[0122] In addition, the electron beam source may be a known electron beam accelerator, specifically, various electron beam accelerators such as the Van de Graaff type, Cocklof-Walton type, resonance transformer type, insulating core transformer type, linear type, high frequency high voltage (Dynamitron) type, and high frequency type.
[0123] By curing the matrix resin contained in the solution, the positions of the microparticles in the matrix resin can be fixed, thereby forming an anti-glare layer having a plurality of microparticles dispersed in the matrix resin and having a concavo-convex structure formed on the surface due to the microparticles.
[0124] According to the antiglare film of the second embodiment, by setting the difference in refractive index between the matrix resin and the fine particles within a predetermined range and dispersing a plurality of fine particles in the matrix resin, it is possible to prevent the antiglare film from being colored while ensuring good antiglare properties and suppressing the glare of the display 16 a .
[0125] Furthermore, since the ratio G2 / G1 of the antiglare layer is set to a value in the range of 0.07 to 0.20, an antiglare film having an antiglare layer having a structure in which a plurality of fine particles are dispersed in a matrix resin can be produced favorably.
[0126] (Third embodiment)
[0127] The anti-glare layer 33 of the anti-glare film of the third embodiment has a structure in which a concavo-convex shape is formed on the surface opposite to the substrate film side. The anti-glare layer 33 is composed of a resin layer. As an example, the resin layer is formed of the same material as the base resin of the second embodiment.
[0128] Specifically, the antiglare film of the third embodiment can be produced by forming a coating layer containing a curable resin on a base film, giving a concavo-convex shape to the surface of the coating layer, and then curing the coating layer. Figure 2 It is a figure which shows the manufacturing method of the anti-glare film of 3rd Embodiment. Figure 2 In the example, an ultraviolet curing resin is used as the curable resin.
[0129] like Figure 2 As shown, in this manufacturing method, the base film 20a is unwound from a unwinding roll (not shown) and conveyed in a predetermined direction. The downstream end of the base film 20a in the conveying direction is inserted into and passes through the nip point N1 of the pair of rollers 21 and 22.
[0130] The ultraviolet curable resin precursor is attached to the peripheral surface of the roller 22 by the peripheral surface of the roller 23 axially supported adjacent to the roller 22. When the base film 20a passes through the nip point N1, the ultraviolet curable resin precursor is applied to one surface of the base film 20a.
[0131] The layer of the ultraviolet curable resin precursor applied to the base film 20a (hereinafter referred to as the coating layer) is pressed together with the base film 20a at the nip point between the rollers 21 and 24. The roller 24 is a roller-shaped mold (embossing roller) with fine concavoconvex shapes formed on the circumferential surface, and when passing through the nip point N2 between the rollers 21 and 24, the concavoconvex shapes are transferred to the surface of the coating layer.
[0132] The coating layer having the concavo-convex shape transferred to the surface by the roller 24 can be cured by ultraviolet rays irradiated by the ultraviolet lamp 26 provided below the rollers 21 and 24. Thus, the anti-glare layer 33 can be formed. The anti-glare film 33 thus manufactured is released from the roller 24 by the roller 25 axially supported adjacent to the roller 24 and conveyed in a given direction.
[0133] Here, the concavo-convex portions on the surface of the roller 24 are formed by blasting particles of a predetermined particle size by a blasting method. By adjusting the blasting particle size, the concavo-convex shape formed on the coating layer of the anti-glare film 33 can be adjusted.
[0134] As the base film 20 a , PET (polyethylene terephthalate) film, TAC (cellulose triacetate) film, COP (cycloolefin polymer) film, acrylic resin film, or polycarbonate resin film can be preferably used.
[0135] Thus, the preparation method of the anti-glare film of the third embodiment includes the following steps: a step (a) of coating a curable resin precursor on a substrate film; a step (b) of preparing a roller-shaped mold having a concave-convex shape on a surface by hitting the sprayed particles; a step (c) of transferring the concave-convex shape to the surface of the curable resin precursor coated on the substrate film using the roller-shaped mold; and a step (d) of curing the curable resin precursor to which the concave-convex shape was transferred to form an anti-glare layer having a concave-convex shape on a surface.
[0136] The average particle size of the sprayed particles used in step (b) can be appropriately set, but as an example, it can be set to a value in the range of 10 μm or more and 50 μm or less. The average particle size of the sprayed particles is further preferably a value in the range of 20 μm or more and 45 μm or less, and more preferably a value in the range of 30 μm or more and 40 μm or less. Thus, an anti-glare layer 33 having a concavo-convex shape on the surface can be obtained.
[0137] It should be noted that the mold used in the third embodiment can be a roll-shaped mold or a plate-shaped mold (embossed plate). In addition, after forming a coating (resin layer) on one side of the substrate film, the surface of the coating can be shaped by the mold to cure the coating, thereby forming the anti-glare layer 33. In addition, in the above example, the coating is cured after the surface of the coating is shaped, but the coating can also be shaped and cured at the same time.
[0138] As for the material of the mold, as an example, metal, plastic, and wood can be cited. On the contact surface of the mold with the coating, in order to improve the durability (wear resistance) of the mold, a film can be provided. As an example, the material of the sprayed particles can be cited as metal, silicon dioxide, aluminum oxide, and glass. The sprayed particles can, for example, hit the surface of the mold by the pressure of gas or liquid. In addition, if the curing resin precursor is an electron beam curing type, an electron beam source such as an electron beam accelerator can be used instead of the ultraviolet lamp 26, and if it is thermosetting, a heating source such as a heater can be used instead of the ultraviolet lamp 26.
[0139] In the antiglare film of the third embodiment, fine particles can be dispersed in the antiglare layer 33 , so that light incident into the antiglare film is scattered at a wide angle due to the difference in refractive index between the matrix resin in the antiglare layer and the fine particles, thereby effectively preventing the antiglare film from being colored.
[0140] It should be noted that the anti-glare layer of the anti-glare film of each embodiment described above may further include an upper layer disposed on the surface opposite to the substrate film 2. By providing the upper layer, the haze value of the anti-glare layer can be easily adjusted, and the anti-glare film can be easily protected from the outside.
[0141] The thickness of the upper layer can be appropriately set, for example, it can be set to a value in the range of 0.5 μm to 20 μm. The thickness of the upper layer is preferably a value in the range of 2.0 μm to 12 μm, and more preferably a value in the range of 3.0 μm to 8.0 μm. Hereinafter, the glare inspection machine and the glare evaluation method for inspecting / evaluating the anti-glare film of each embodiment described above will be described in turn.
[0142] (Glare inspection machine)
[0143] Figure 3 1 is a schematic diagram of a glare inspection machine 10. The glare inspection machine 10 is a device for evaluating the glare of a display 16a in a display device 16 having a film such as an anti-glare film mounted on the surface, and comprises: a housing 11, a camera 12, a holding portion 13, a camera stand 14, a display stand 15, and an image processing device 17. Examples of commercially available glare inspection machines 10 include "Film Glare Inspection Machine" manufactured by KOMATSU NTC Co., Ltd.
[0144] The housing 11 has a dark room for photographing the display 16a by the photographing device 12. The housing 11 accommodates the photographing device 12, the holding unit 13, the photographing device stand 14, the display device stand 15, and the display device 16 to be evaluated.
[0145] As an example, the camera 12 is an area camera having a lens 18 and a camera element, and it captures an image displayed on the display 16a. The camera 12 is connected to the image processing device 17 and is held by the holding unit 13 in such a manner that the lens 18 faces the display 16a. Image data captured by the camera 12 is sent to the image processing device 17.
[0146] The holding portion 13 extends in the vertical direction, and the lower end is fixed to the camera bracket 14, while holding the camera 12. The holding portion 13 holds the camera 12 in a manner that the relative distance between the display 16a and the lens 18 can be changed by relatively moving the camera 12 in the vertical direction relative to the display device 16.
[0147] The display device 16 is placed on the display device support 15 in a state where the display 16a with the film mounted thereon is opposite to the camera 12. The display device support 15 supports the display device 16 in a manner that the surface of the display 16a with the film mounted thereon is opposite to the camera 12 and becomes a horizontal plane, and at the same time, the display device 16 is relatively moved in a direction perpendicular to the camera 12.
[0148] In the glare inspection machine 10, by adjusting the relative distance between the imaging device 12 and the display 16a, the pixel size of the image captured per unit pixel (for example, 1 pixel) of the imaging element of the imaging device 12 and displayed on the display 16a can be adjusted.
[0149] The image processing device 17 performs data processing on the image data captured by the image capturing device 12. Specifically, the image processing device 17 obtains the standard deviation of the brightness of the display 16a based on the image data captured by the image capturing device 12.
[0150] The image processing device 17 of this embodiment includes: an input unit that inputs image data captured by the imaging device 12, an image processing unit that performs image processing on the input image data, and an output unit that outputs the results processed by the image processing unit to a display device, a printing device, etc.
[0151] As a method for adjusting the pixel size of an image captured by each unit pixel (for example, 1 pixel) of the imaging element when the imaging device 12 captures an image displayed on the display 16a, in addition to the method of changing the relative distance between the imaging device 12 and the display 16a, when the lens 18 provided in the imaging device 12 is a zoom lens, a method of changing the focal length of the imaging device 12 can be adopted.
[0152] (Evaluation method for glare)
[0153] Next, a description will be given of a method for evaluating glare of the display 16a using the glare inspection device 10. In this method, the display 16a having a film mounted on its surface is uniformly illuminated in a single color (green, for example) for easy evaluation.
[0154] Next, an adjustment step is performed to adjust the pixel size of the display 16a with a film mounted thereon captured per unit pixel of the imaging element of the imaging device 12. In the adjustment step, the relative distance between the imaging device 12 and the display 16a with a film mounted thereon is adjusted to the following extent based on the number of effective pixels of the imaging element of the imaging device 12: there are no bright lines based on pixels in the image captured by the imaging device 12, or even if there are bright lines based on pixels, the evaluation of the glare of the display 16a is not affected.
[0155] It should be noted that the relative distance between the camera 12 and the display device 16 is preferably set in consideration of the usage of the display device 16 (for example, the relative distance between the user's eyes and the surface of the display 16 a ).
[0156] After the adjustment step is performed, a setting step is performed to set a measurement area for evaluating the glare of the display 16a on which the film is attached. In the setting step, the measurement area is appropriately set according to, for example, the size of the display 16a.
[0157] After the adjustment step is performed, a photographing step is performed in which the measuring area of the display 16a on which the film is mounted is photographed by the photographing device 12. At this time, as an example, at least one of the exposure time of the photographing device 12 or the brightness of all pixels of the display 16a is adjusted to obtain image data in the form of a grayscale image with an 8-bit grayscale display and an average brightness of 170 grayscales. The image data obtained by the photographing step is input to the image processing device 17.
[0158] After the photographing step, the image processing device 17 performs a calculation step of obtaining the unevenness of brightness in the measurement area of the display 16a on which the film is mounted using the image data. In the calculation step, the unevenness of brightness is digitized as the standard deviation of the brightness distribution.
[0159] Here, the greater the unevenness of the brightness of the display 16a with the film installed, the greater the glare of the display 16a with the film installed. Therefore, the smaller the value of the standard deviation of the brightness distribution, the less glare the display 16a can be quantitatively evaluated. In addition, since the bright line of the display 16a with the film installed is adjusted to a degree that does not affect the evaluation of the glare of the display 16a in the adjustment step, it is possible to suppress the uneven brightness caused by the bright line and perform an accurate evaluation of the glare of the display 16a.
[0160] By going through the above steps, the standard deviation of the luminance distribution of the display 16 a with the film mounted on the surface can be obtained, and the glare of the display 16 a can be evaluated based on the value.
[0161] (Examples and Comparative Examples)
[0162] Hereinafter, the present invention will be described in more detail based on examples, but the present invention is not limited to these examples.
[0163] In Examples 1 to 4, an anti-glare layer 3 having a phase separation structure as a basic structure and containing a given component is formed. In Example 5, an anti-glare layer having an improved haze value is formed by beads (silicon dioxide particles). In Comparative Example 1, an anti-glare layer having an improved haze value is formed by beads (zirconia particles). In Comparative Examples 2 and 3, an anti-glare layer containing a phase separation structure is formed.
[0164] In Comparative Examples 4 and 5, an anti-glare layer with an increased haze value is formed by beads (acrylic particles). In Comparative Example 6, an anti-glare layer with an increased haze value is formed by beads (silicon dioxide particles). In Comparative Examples 7 to 9, an anti-glare layer with an increased haze value is formed by high-refractive index beads (polystyrene particles, etc.). In Comparative Examples 10 and 11, an anti-glare layer is formed by forming depressions and projections on the surface of a transparent resin coated on a substrate film by molding. It should be noted that the refractive index described in the following embodiments and descriptions of comparative examples, for substances cured by crosslinking, represents the refractive index after crosslinking (after curing).
[0165] [raw material]
[0166] The following materials were used as the raw materials used in Examples and Comparative Examples.
[0167] Acrylic polymer A having a polymerizable group: [CYCLOMER P] manufactured by Daicel Allnex Corporation, refractive index: 1.51
[0168] Cellulose acetate propionate: [CAP-482-20] manufactured by Eastman Co., Ltd., degree of acetylation = 2.5%, degree of propionylation = 46%, number average molecular weight in terms of polystyrene: 75,000, refractive index: 1.49
[0169] Silicone acrylate: [EB1360] manufactured by Daicel Allnex Co., Ltd., refractive index 1.52 Urethane acrylate: [UA-53H] manufactured by Shin-Nakamura Chemical Co., Ltd.
[0170] Dipentaerythritol hexaacrylate: [DPHA] manufactured by Daicel Allnex Corporation, refractive index 1.52
[0171] Pentaerythritol tetraacrylate: [PETRA] manufactured by Daicel Allnex Corporation, refractive index 1.52
[0172] Nanosilica-containing acrylic UV curable compound A: manufactured by MOMENTIVE PERFORMANCE MATERIALS JAPAN (Co., Ltd.) [UVHC-7800]
[0173] Acrylic ultraviolet curable compound containing silica (refractive index 1.46): [Z-753-11R] manufactured by AICA INDUSTRY CO., LTD., refractive index 1.52
[0174] Acrylic hard coating mixture A: [FA-3155KURIA] manufactured by Nippon Kagaku Paint Co., Ltd., containing acrylic microparticles (refractive index 1.50) and a matrix resin (refractive index 1.46)
[0175] Acrylic hard coating mixture B: [FA-3155M] manufactured by Nippon Kagaku Paint Co., Ltd., refractive index 1.46
[0176] Fluorine compound A having a polymerizable group: Shin-Etsu Chemical Co., Ltd. [KY-1203]
[0177] Fluorine compound B having a polymerizable group: [FTERGENT 602A] manufactured by NEOS Corporation
[0178] Zirconia fine particles (refractive index about 20 Dispersion liquid: manufactured by TOYOINK Co., Ltd. [LIODURAS TYZ]
[0179] Photoinitiator A: BASF Japan Co., Ltd. [IRGACURE 184]
[0180] Photoinitiator B: BASF Japan Co., Ltd. [IRGACURE 907]
[0181] Polyethylene terephthalate (PET) film: Made by Mitsubishi Plastics Corporation [DIAFOIL]
[0182] Triacetyl cellulose (TAC) film: FUJIFILM Corporation [FUJITACT G60UL]
[0183] [Example 1]
[0184] A solution was prepared by dissolving 12.5 parts by weight of an acrylic polymer A having a polymerizable group, 4 parts by weight of cellulose acetate propionate, 150 parts by weight of an acrylic ultraviolet curable compound A containing nanosilica, 1 part by weight of silicone acrylate, 1 part by weight of a photoinitiator A, and 1 part by weight of a photoinitiator B in a mixed solvent of 81 parts by weight of methyl ethyl ketone, 24 parts by weight of 1-butanol, and 13 parts by weight of 1-methoxy-2-propanol.
[0185] This solution was cast on a PET film (substrate film 2) using a wire bar (#20), and then placed in an oven at 80°C for 1 minute to evaporate the solvent, thereby forming a coating layer with a thickness of about 9 μm.
[0186] Then, the coating layer was irradiated with ultraviolet light for about 5 seconds using a high pressure mercury lamp to perform ultraviolet curing treatment on the coating layer. Thus, an antiglare layer 3 was formed, and an antiglare film of Example 1 was obtained.
[0187] [Example 2]
[0188] A solution was prepared by dissolving 15.0 parts by weight of an acrylic polymer A having a polymerizable group, 3 parts by weight of cellulose acetate propionate, 150 parts by weight of an acrylic ultraviolet curable compound A containing nanosilica, 1 part by weight of silicone acrylate, 1 part by weight of a photoinitiator A, and 1 part by weight of a photoinitiator B in a mixed solvent of 101 parts by weight of methyl ethyl ketone and 24 parts by weight of 1-butanol.
[0189] This solution was cast on a PET film (substrate film 2) using a wire bar (#20), and then placed in an oven at 80°C for 1 minute to evaporate the solvent, thereby forming a coating layer with a thickness of about 9 μm.
[0190] Then, the coating layer was irradiated with ultraviolet light for about 5 seconds using a high pressure mercury lamp to perform ultraviolet curing treatment on the coating layer. Thus, an antiglare layer 3 was formed, and an antiglare film of Example 2 was obtained.
[0191] [Example 3]
[0192] A solution was prepared by dissolving 12.5 parts by weight of an acrylic polymer A having a polymerizable group, 5.5 parts by weight of cellulose acetate propionate, 149.2 parts by weight of an acrylic ultraviolet curable compound A containing nanosilica, 0.1 parts by weight of a fluorine compound B having a polymerizable group, 1 part by weight of a photoinitiator A, and 1 part by weight of a photoinitiator B in a mixed solvent of 129 parts by weight of methyl ethyl ketone, 24 parts by weight of 1-butanol, and 13 parts by weight of 1-methoxy-2-propanol.
[0193] This solution was cast on a PET film (substrate film 2) using a wire bar (#16), and then placed in an oven at 80°C for 1 minute to evaporate the solvent, thereby forming a coating layer with a thickness of about 7 μm.
[0194] Then, the coating layer was irradiated with ultraviolet light for about 5 seconds using a high pressure mercury lamp to perform ultraviolet curing treatment on the coating layer. Thus, an antiglare layer 3 was formed, and an antiglare film of Example 3 was obtained.
[0195] [Example 4]
[0196] A solution was prepared by dissolving 50 parts by weight of an acrylic polymer A having a polymerizable group, 2.5 parts by weight of cellulose acetate propionate, 79.5 parts by weight of urethane acrylate, 1 part by weight of silicone acrylate, 1 part by weight of a photoinitiator A, and 1 part by weight of a photoinitiator B in a mixed solvent of 106 parts by weight of methyl ethyl ketone, 28 parts by weight of 1-butanol, and 70 parts by weight of cyclohexanone.
[0197] This solution was cast on a PET film (substrate film 2) using a wire bar (#12), and then placed in an oven at 80°C for 1 minute to evaporate the solvent, thereby forming a coating layer with a thickness of about 5 μm.
[0198] Then, the coating layer was irradiated with ultraviolet light for about 5 seconds using a high pressure mercury lamp to perform ultraviolet curing treatment on the coating layer. Thus, an antiglare layer 3 was formed, and an antiglare film of Example 4 was obtained.
[0199] [Example 5]
[0200] A solution was prepared by mixing 25 parts by mass of acrylic hard coating mixture A, 25 parts by mass of acrylic ultraviolet curable compound containing silicon dioxide, and 50 parts by mass of 1-butanol. The solution was cast on a PET film (substrate film 2) using a wire rod (#16), and then placed in an oven at 80°C for 1 minute to evaporate the solvent and form a coating with a thickness of about 7 μm. Then, the coating was irradiated with ultraviolet light for about 5 seconds by an ultraviolet lamp to perform ultraviolet curing treatment, thereby forming an anti-glare layer 3, and an anti-glare film of Example 5 was obtained.
[0201] [Comparative Example 1]
[0202] 50 parts by weight of dipentaerythritol hexaacrylate, 50 parts by weight of pentaerythritol tetraacrylate, 100 parts by weight of zirconium oxide fine particle dispersion, 2 parts by weight of photoinitiator A, and 1 part by weight of photoinitiator B were dissolved in a mixed solvent of 116 parts by weight of methyl ethyl ketone, 19 parts by weight of 1-butanol, and 58 parts by weight of 1-methoxy-2-propanol to prepare a solution.
[0203] This solution was cast on a PET film (substrate film 2) using a wire bar (#14), and then placed in an oven at 80°C for 1 minute to evaporate the solvent, thereby forming a coating layer with a thickness of about 6 μm.
[0204] Then, the coating layer was irradiated with ultraviolet light for about 5 seconds by a high pressure mercury lamp to cure the coating layer. Thus, an anti-glare layer was formed to obtain an anti-glare film of Comparative Example 1.
[0205] [Comparative Example 2]
[0206] 5.7 parts by weight of acrylic polymer A having a polymerizable group, 1.2 parts by weight of cellulose acetate propionate, 4 parts by weight of dipentaerythritol hexaacrylate, 2.77 parts by weight of silicone acrylate, and 0.5 parts by weight of photoinitiator A were dissolved in a mixed solvent of 25 parts by weight of methyl ethyl ketone and 12.2 parts by weight of 1-butanol to prepare a solution.
[0207] This solution was cast on a PET film (substrate film) using a wire bar (#24), and then placed in an oven at 80° C. for 1 minute to evaporate the solvent, thereby forming a coating layer with a thickness of about 7 μm.
[0208] Then, the coating layer was irradiated with ultraviolet light for about 5 seconds using a high pressure mercury lamp to perform ultraviolet curing treatment on the coating layer, thereby forming an anti-glare layer and obtaining an anti-glare film of Comparative Example 2.
[0209] [Comparative Example 3]
[0210] 4.1 parts by weight of acrylic polymer A having a polymerizable group, 1.2 parts by weight of cellulose acetate propionate, 4 parts by weight of dipentaerythritol hexaacrylate, 2.77 parts by weight of silicone acrylate, and 0.5 parts by weight of photoinitiator A were dissolved in a mixed solvent of 25 parts by weight of methyl ethyl ketone and 12.2 parts by weight of 1-butanol. The solution was cast on a PET film (base film) using a wire rod (#22), and then placed in an oven at 100°C for 1 minute to evaporate the solvent, thereby forming a coating with a thickness of about 6 μm.
[0211] Then, the coating layer was irradiated with ultraviolet light for about 5 seconds using a high pressure mercury lamp to perform ultraviolet curing treatment on the coating layer. Thus, an antiglare layer was formed, and an antiglare film of Comparative Example 3 was obtained.
[0212] [Comparative Example 4]
[0213] 63 parts by weight of acrylic hard coating mixture A and 37 parts by weight of acrylic hard coating mixture B were mixed, and the solution was cast on a TAC film (substrate film) using a wire bar (#10), and then placed in an oven at 100°C for 1 minute to evaporate the solvent, thereby forming a coating layer with a thickness of about 6 μm.
[0214] Then, the coating layer was irradiated with ultraviolet light for about 5 seconds by a high pressure mercury lamp to cure the coating layer. Thus, an anti-glare layer was formed to obtain an anti-glare film of Comparative Example 4.
[0215] [Comparative Example 5]
[0216] 32 parts by weight of acrylic hard coating mixture A and 68 parts by weight of acrylic hard coating mixture B were mixed, and the solution was cast on a TAC film (substrate film) using a wire bar (#10), and then placed in an oven at 100°C for 1 minute to evaporate the solvent, thereby forming a coating layer with a thickness of about 6 μm.
[0217] Then, the coating layer was irradiated with ultraviolet light for about 5 seconds using a high pressure mercury lamp to perform ultraviolet curing treatment on the coating layer. Thus, an antiglare layer was formed, and an antiglare film of Comparative Example 5 was obtained.
[0218] [Comparative Example 6]
[0219] As a substrate film, a transparent polyester film with a thickness of 125 μm (manufactured by Toyobo Co., Ltd., COSMOSHINEA 4300) was used. As a transparent resin, OPSTAR Z7501 (manufactured by JSR Corporation, solid content 50%), which is an organic-inorganic hybrid ionizing radiation curing resin composition, was used, wherein 8.5 parts of OK-500 (manufactured by DEGUSSA, average particle size 3.0 μm, refractive index 1.46) as translucent silica particles were contained relative to 200 parts by weight of the transparent resin. 1 part by weight of IRGACURE 651 (manufactured by BASF) as a photopolymerization initiator and 200 parts by weight of butyl acetate (boiling point 100°C) as a solvent were mixed therein, and the obtained resin composition was coated on the substrate film, and 85°C dry air was circulated at a flow rate of 1 m / s, and dried for 1 minute.
[0220] Irradiate with ultraviolet light (200 / cm in nitrogen atmosphere) 2 ) and the transparent resin was cured to form an anti-glare layer, thereby obtaining an anti-glare film of Comparative Example 6. The coating thickness was set to 6 μm.
[0221] [Comparative Example 7]
[0222] As a substrate film, cellulose triacetate (manufactured by FUJIFILM Co., Ltd., thickness 80 μm) was prepared. As a transparent resin, pentaerythritol triacrylate (PETA; manufactured by DAICEL ALLNEX Co., Ltd., refractive index 1.51) was used, and styrene-acrylic copolymer particles (refractive index 1.51, average particle size 9.0 μm) and polystyrene particles (refractive index 1.60, average particle size 3.5 μm) as light-transmitting particles were contained in an amount of 10.0 parts by weight and 16.5 parts by weight, respectively, relative to 100 parts by weight of the transparent resin. A mixed solvent (weight ratio 7:3) of toluene (boiling point 110°C) and cyclohexanone (boiling point 156°C) was added as a solvent in an amount of 190 parts by weight relative to 100 parts by weight of the transparent resin, and the resulting resin composition was applied on the substrate film, and dry air at 85°C was circulated at a flow rate of 1 m / s, and dried for 1 minute.
[0223] Irradiate with ultraviolet light (200 / cm in nitrogen atmosphere) 2 ) and the transparent resin was cured to form an anti-glare layer, thereby obtaining an anti-glare film of Comparative Example 7. The coating thickness was set to 5 μm.
[0224] [Comparative Example 8]
[0225] As a substrate film, cellulose triacetate (manufactured by Fujifilm Co., Ltd., thickness 80 μm) was prepared. As a transparent resin, a mixture of pentaerythritol triacrylate (PETA; manufactured by Daicel Allnex Co., Ltd.), dipentaerythritol hexaacrylate (DPHA; manufactured by Daicel Allnex Co., Ltd.), and polymethyl methacrylate (BR85; manufactured by Mitsubishi Rayon Co., Ltd.) (weight ratio; PETA / DPHA / PMMA=86 / 5 / 9) (refractive index 1.51) was used, wherein polystyrene particles (refractive index 1.60, average particle size 3.5 μm) and styrene-acrylic copolymer particles (refractive index 1.56, average particle size 3.5 μm) as light-transmitting particles were contained in an amount of 18.5 and 3.5 parts by weight, respectively, relative to 100 parts by weight of the transparent resin. A mixed solvent of toluene (boiling point 110°C) and cyclohexanone (boiling point 156°C) was added as a solvent (weight ratio 7:3) in an amount of 190 parts by weight relative to 100 parts by weight of the transparent resin, and the resulting resin composition was applied on a substrate film, and dry air at 70°C was passed through at a flow rate of 0.2 m / s, and dried for 1 minute.
[0226] Then, ultraviolet light (200 mJ / cm in nitrogen atmosphere) was irradiated. 2 ) and the transparent resin was cured to form an anti-glare layer, thereby obtaining an anti-glare film of Comparative Example 8. The coating thickness was set to 3.5 μm.
[0227] [Comparative Example 9]
[0228] As a substrate film, cellulose triacetate (manufactured by FUJIFILM Co., Ltd., thickness 80 μm) was prepared. As a transparent resin, pentaerythritol triacrylate (PE-3A; manufactured by Kyoeisha Chemical Co., Ltd., refractive index 1.53) was used, wherein 26 parts by weight and 6.6 parts by weight of silica particles (SS50F; manufactured by TOSOH-SILICA Co., Ltd., refractive index 1.47, average particle size 1.1 μm) and polystyrene particles (refractive index 1.59, average particle size 3.5 μm) as light-transmitting particles were contained, respectively, relative to 100 parts by weight of the transparent resin. 5.3 parts by weight of IRGACURE 184 (manufactured by BASF) as a photopolymerization initiator and 138 parts by weight of toluene (boiling point 110° C.) as a solvent were mixed therewith, and the obtained resin composition was coated on the substrate film, and dry air at 90° C. was circulated at a flow rate of 0.2 m / s, and dried for 1 minute.
[0229] Then, ultraviolet light (200 mJ / cm in nitrogen atmosphere) was irradiated. 2 ) and the transparent resin was cured to form an anti-glare layer, thereby obtaining an anti-glare film of Comparative Example 9. The coating thickness was set to 5 μm.
[0230] [Comparative Examples 10 and 11]
[0231] The anti-glare films of Comparative Examples 10 and 11 are as follows Figure 3 As shown, a coating layer made of ultraviolet curing resin with concavities and convexities transferred to the surface is formed on a base film using a mold.
[0232] That is, in Example 5 and Comparative Examples 2 to 5, Figure 3 As shown, the base film 20a unwound from an unwinding roller (not shown) is inserted into and passed through the roller gap point of a pair of rollers 21 and 22, so that the ultraviolet curing resin precursor adheres to the peripheral surface of the roller 22 from the peripheral surface of the roller 23 axially supported adjacent to the roller 22, and the ultraviolet curing resin precursor is coated on the upper surface of the base film 20a.
[0233] The applied ultraviolet curable resin precursor is squeezed together with the base film 20a at the nip point N1 of the rollers (roller-shaped molds) 21 and 24. Thus, when the applied ultraviolet curable resin precursor passes through the nip point N1 of the rollers 21 and 24 together with the base film 20a, a concavo-convex shape is transferred to the surface of the ultraviolet curable resin precursor.
[0234] The ultraviolet curing resin precursor to which the concavo-convex shape is transferred by the roller 24 is cured by ultraviolet rays irradiated by a UV lamp disposed below the rollers 21 and 24, thereby obtaining a coating layer (anti-glare layer). The anti-glare film thus obtained is released from the roller 24 by the roller 25 axially supported adjacent to the roller 24, and is transported in a given direction. As the base film, a TAC (triacetyl cellulose) film is used.
[0235] In step (b) of making a roll-shaped mold having a concavo-convex shape on the surface by hitting the sprayed particles, the roll-shaped mold was made by changing the value of the sprayed particle size within the range of 30 μm to 40 μm. Two films (Comparative Examples 10 and 11) with different haze (Hz) values were made by the above-mentioned production method.
[0236] Next, the following items were measured and evaluated for each antiglare film of Examples 1 to 5 and Comparative Examples 1 to 11. When the haze, total light transmittance, transmission image clarity, and 60-degree glossiness were measured, the adhesive layer was omitted.
[0237] [Haze and total light transmittance]
[0238] The haze was measured using a haze meter (NDH-5000W manufactured by Nippon Denshoku Co., Ltd.) in accordance with JIS K 7136. The haze was measured by placing the antiglare layer so that the surface having the concavo-convex structure was on the light receiving device side.
[0239] [Transmission image clarity]
[0240] The image clarity meter (ICM-1T manufactured by SUGA TEST INSTRUMENTS Co., Ltd.) was used to measure the anti-glare film in accordance with JIS K 7105, with the film forming direction of the anti-glare film being parallel to the direction of the comb teeth of the optical comb. The optical comb width was 0.5 mm.
[0241] [60 degree glossiness]
[0242] The glossiness was measured at an angle of 60° using a gloss meter (IG-320, manufactured by Horiba, Ltd.) in accordance with JIS K7105.
[0243] [Standard deviation of display brightness distribution (glare value)]
[0244] As the display device 16, a smartphone (Galaxy S4 manufactured by Samsung Electronics Co., Ltd.) was used, and the anti-glare film of each sample was attached to the surface of the display 16a via an adhesive layer (optical paste). The standard deviation (glare σ: glare value) of the brightness distribution of the display 16a was measured through the anti-glare film of each sample using a film glare inspection machine 10 manufactured by KOMATSU NTC Co., Ltd. During the measurement, at least one of the exposure time of the camera 12 or the brightness of all pixels of the display 16a was adjusted to obtain image data in the form of a grayscale image with an 8-bit grayscale display and an average brightness of 170 grayscales.
[0245] The measurement results are shown in Tables 1 and 2.
[0246] [Table 1]
[0247]
[0248] [Table 2]
[0249]
[0250] As shown in Table 1, in the anti-glare films 1 of Examples 1 to 5, the clarity of the transmitted image at a comb width of 0.5 mm is set to a value in the range of 3% to 40%, and the haze value of the anti-glare layer 3 is set to a range of 55.5% to 93.0%. In addition, by using the anti-glare films of Examples 1 to 5, the glare value (glare σ) of the display 16a is suppressed to a value in the range of 4.2 to 6.0. That is, it can be seen that by using the anti-glare films 1 of Examples 1 to 5, good anti-glare properties are obtained while suppressing the glare value of the display.
[0251] The reason for this is that it is considered that, with the anti-glare layer 3 of Examples 1 to 4, phase separation occurs between the acrylic copolymer A and the cellulose acetate propionate, and at the same time, the phase separation structure is enhanced by the acrylic ultraviolet curable compound A containing nano-silica and the urethane acrylate, thereby enabling the surface of the anti-glare layer 3 to be formed into a very steep structure or a structure with a height difference.
[0252] That is, it is considered that the nanosilica-containing acrylic ultraviolet curable compound A and urethane acrylate have high affinity for the acrylic copolymer A and produce repulsive interaction with cellulose acetate propionate, thereby reinforcing the phase separation structure of the antiglare layer 3 of Examples 1 to 4.
[0253] In addition, it can be considered that in the anti-glare layer 3 of Example 5, by adding a large amount of butanol, a solvent with low affinity for silica particles in the acrylic ultraviolet curable compound containing silica, the agglomeration of silica particles occurs rapidly, and the surface of the anti-glare layer 3 can be formed into a very steep or high-low structure. That is, it can be considered that the repulsive interaction between the silica particles and butanol enhances the concavo-convex structure formed on the surface of the anti-glare layer 3 to a degree that does not occur in a solvent with high affinity. In addition, in the anti-glare layer 3 of Example 5, by making the acrylic ultraviolet curable resin and the acrylic hard coating mixture A coexist, the optical properties are adjusted to the range shown in Table 1.
[0254] As shown in Tables 1 and 2, the values of the transmission image clarity and 60-degree glossiness of Comparative Examples 1 to 6 and 11 are higher than those of Examples 1 to 5. The values of the transmission image clarity of Comparative Examples 7 to 9 are lower, but the values of the 60-degree glossiness are higher, and the value of the 60-degree glossiness of Comparative Example 10 is lower, but the value of the transmission image clarity is higher. Thus, it is considered that the balance of the transmission image clarity and the 60-degree glossiness of Comparative Examples 1 to 11 is not excellent compared with Examples 1 to 5, and therefore the anti-glare property is lowered compared with Examples 1 to 5.
[0255] Specifically, in the anti-glare film of Comparative Example 1, beads (zirconia fine particles) are used to increase the haze value of the anti-glare layer, and the difference in refractive index between the beads contained in the anti-glare layer and the matrix resin is set to 0.2. However, as for the anti-glare film of Comparative Example 1, as shown in Table 2, although the glare value of the display is suppressed to a certain extent, the values of the clarity of the transmitted image and the 60-degree glossiness are high, and the anti-glare property is not excellent.
[0256] It is found that the antiglare films of Comparative Examples 2 and 3 have an antiglare layer formed of a phase separation structure, but the phase separation structure of the antiglare layer is not enhanced as in Examples 1 to 4, and therefore the antiglare properties are not as good as in Examples 1 to 4.
[0257] It is found that since the difference in refractive index between the beads contained in the antiglare layer and the matrix resin is small in Comparative Examples 4 to 6, it is difficult to increase the haze value compared to Examples 1 to 5, and it is difficult to obtain good antiglare properties while suppressing the glare value of the display.
[0258] It can be seen that although the internal haze value of the anti-glare layer is adjusted by using high refractive index beads (polystyrene microparticles, etc.) in Comparative Examples 7 to 9, thereby improving the haze value of the anti-glare layer to a certain extent, it is difficult to obtain good anti-glare properties while suppressing the glare value of the display as in Examples 1 to 5.
[0259] It is found that although Comparative Examples 10 and 11 have an anti-glare layer with uneven surfaces formed by embossing, it is difficult to obtain good anti-glare properties while suppressing the glare value of the display as in Examples 1 to 5.
[0260] It should be noted that, based on the trends of the characteristics shown in Examples 1 to 5 and other discussions conducted by the inventors of the present application, it can be considered that the same effects as in Examples 1 to 5 can be achieved when the glare value of the display 16a is set to a value in the range of greater than 0 and less than 4.2, the clarity of the transmitted image with a light comb width of 0.5 mm of the anti-glare film 1 is set to a value in the range of greater than 0% and less than 8.4%, and greater than 55% and less than 60%, and the haze value of the anti-glare layer 3 is set to a value in the range of greater than 50% and less than 55.5, and greater than 93.0 and less than 99.0%.
[0261] The present invention is not limited to the above-described embodiments, and its aspects or methods may be changed, added, or deleted without departing from the technical concept of the present invention.
Claims
1. An anti-glare film comprising an anti-glare layer, wherein the haze value of the anti-glare layer is a value in the range of 55.5% to 93%. When the anti-glare film is attached to the surface of a display, the standard deviation of the brightness distribution of the display is a value in the range of 4.2 to 6.
0. Furthermore, the 60-degree glossiness of the anti-glare film is a value in the range of 0.9% to 30%. The anti-glare layer includes a matrix resin and a plurality of fine particles dispersed in the matrix resin, thereby having a distribution structure of concavities and convexities formed on the surface and excluding a co-continuous phase structure formed by phase separation of a plurality of resin components.
2. The anti-glare film according to claim 1, wherein: The difference in refractive index between the fine particles and the matrix resin is a value in a range of 0 to 0.
07.
3. The anti-glare film according to claim 2, wherein: A ratio G2 / G1 of a weight G1 of the base resin of the anti-glare layer to a total weight G2 of the plurality of fine particles included in the anti-glare layer is a value in a range of 0.07 to 0.20.
Citation Information
Patent Citations
Light diffusion sheet
JP2009109702A
Optical film and production method of the same
JP2014102356A
Surface illumination assembly and surface illumination device
CN103629594A
Frosted protection film with anti-static function and preparation method
CN106111497A
Antiglare hard coat film and method for producing the same
JP2008257041A