A test method for peeling strength of lithium-ion battery pole piece
By using a tensile machine for mechanical testing in the peel strength test of lithium-ion battery pole pieces, the problem of insufficient test accuracy and repeatability in the existing technology is solved, a more scientific and reliable testing method is provided, and the adhesion of pole pieces is improved. Accuracy of knot strength related data.
Patent Information
- Application Number
- CN202111575401.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-21
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-12-21
AI Technical Summary
Existing lithium-ion battery pole piece peeling strength testing methods have accuracy and repeatability problems, and the sample preparation and fixation processes are not standardized, which affects the stability and efficiency of the test results.
A tensile machine was used for mechanical testing. Long strip samples of pole pieces were prepared, fixed with double-sided tape and hard plates, and tested for natural bending and tensile force. The peeling strength was calculated, and the surface morphology after peeling was recorded to optimize pre-peeling. Starting point and steps.
It improves the accuracy and repeatability of pole piece peeling strength testing, provides basic data for material selection, formula optimization and process improvement, and enhances the scientificity and reliability of the testing.
Smart Images

Figure CN114199760B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion batteries, and in particular to a method for testing the peeling strength of a lithium ion battery pole piece. Background Art
[0002] Lithium-ion batteries have outstanding advantages such as high operating voltage, high specific energy, low self-discharge, long cycle life, no memory effect, and fast charging and discharging. They are one of the most widely used batteries in the world today, and their development in the field of new energy has also attracted much attention.
[0003] Lithium-ion batteries are usually composed of positive and negative electrodes, separators, electrolytes, shells, etc. The positive and negative electrodes are usually composed of a dressing layer and a current collector. The dressing layer contains active substances, conductive substances, and binders. Among them, the active substances mainly play a capacity role, the conductive agent mainly plays a conductive role, and the role of the binder is to bond the active substances and conductive agents to each other and to the current collector at the same time. In order to ensure that the dressing layer will not over-expand or detach from the current collector during the processing and circulation process, causing battery failure, it is very necessary to characterize the bonding force of the dressing layer.
[0004] At present, the industry has a preliminary characterization method for the test characterization of adhesion and peeling force. It basically uses tape to perform adhesion and peeling tests on the surface of the dressing layer or a single point. The result of the peeling test is the peeling strength value, and the morphology is not recorded and compared. In addition, the standardization of the peeling sample preparation and the stability of the peeling have an impact on the accuracy of the test results. The main details are that when the electrode is flipped 180° and peeled, the bending of the electrode needs to be symmetrical on both sides and the importance of pre-peeling. Without pre-peeling, the edge of the steel plate will damage the adhesive layer or the electrode, and the damaged part will break due to the excessive peak value at the beginning of peeling, affecting the test results and efficiency; after pre-peeling, at the starting point of the tape bonding, if it is not smooth enough, the edge of the electrode will be bonded to the tape, which increases the difficulty of operation and pre-peeling failure will also occur. The starting point of pre-peeling needs to be optimized.
[0005] In summary, the test sample preparation and fixation of the electrode peel strength are important for characterizing the accuracy, repeatability and reproducibility of the peel strength results. Based on this, it is necessary to further develop the test method of peel strength. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a test method for the peel strength of a lithium-ion battery electrode. This method can effectively evaluate the peel strength of the electrode, improve the accuracy of the test data, and provide basic data for material selection, formula optimization, process improvement, etc. related to the electrode bonding strength.
[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0008] The present invention provides a method for testing the peel strength of a lithium-ion battery electrode, comprising the following steps:
[0009] S1. Take the rolled positive electrode sheet and make it into a long strip of electrode, wherein the length of the long strip of electrode is greater than 100 mm and the width is 20 to 35 mm;
[0010] S2. Take a hard plate as the base plate, paste double-sided tape in the middle of the front of the base plate, and the two ends of the double-sided tape go around the two side edges of the base plate and paste to the back of the base plate; then, peel off the double-sided tape on the front of the base plate, leaving the bottom surface unpeeled, paste the electrode strip to be tested on the double-sided tape, keep the unpasted margins on both sides of the electrode strip equal, and the pasted part of the electrode strip is not less than half of the total length of the electrode strip; use a pressure roller to roll the electrode strip to make the bonding surface of the electrode strip and the double-sided tape uniform;
[0011] S3. Tear off the unpasted end of the electrode strip to expose the adhesive surface of the electrode strip; fix the torn end of the bottom plate to the fixed end below the tensile machine; bend the natural end of the torn electrode strip upward and clamp it to the upward traction end of the tensile machine;
[0012] S4. Set the parameters of the tensile testing machine and perform tensile force test;
[0013] S5. After the tensile force test is completed, check the tensile force change trend over time in the tensile curve, take the stable stage of tensile force, that is, when the tensile force changes by no more than 10% during this time period, as the stable peeling section, take the average tensile force of the stable peeling section divided by the electrode width, and calculate it as the peeling strength of the battery electrode.
[0014] Furthermore, in step S1, the pole piece strips are divided into two types, namely pole piece strips whose width direction is perpendicular to the rolling direction and pole piece strips whose width direction is parallel to the rolling direction.
[0015] Furthermore, in step S2, the material of the bottom plate includes stainless steel, glass, and plastic plate.
[0016] Furthermore, in step S2, the width of the double-sided adhesive is narrower than the width of the electrode strip, and the difference between the two is 5 to 6 mm.
[0017] Furthermore, in step S2, when rolling the pole piece strip, a 2 kg roller is used to roll the pole piece strip 3-6 times along the axial direction.
[0018] Furthermore, in step S2, the pressing roller rolls naturally during rolling without using artificial external pressure.
[0019] Furthermore, in step S3, the natural end of the electrode strip is bent in the opposite direction by nearly 180°. Especially for the positive electrode test, the bending strip is symmetrical on both sides and the bending arc is smooth to avoid asymmetric peeling during stretching, which may cause the test value to be small or wrong.
[0020] Furthermore, in step S4, the parameters of the tensile testing machine include stretching speed, sample size parameters, stretching cutoff conditions and peeling interval, wherein the stretching speed is set to 50-300 mm / min.
[0021] Furthermore, in step S4, a stable section of the tensile force is selected according to the “time-force” curve.
[0022] Furthermore, in step S4, when the tensile force does not change by more than 5% during this time period, it is regarded as a stable peeling section.
[0023] Furthermore, step S5 also includes a step of recording the morphology of the surface of the electrode strip and the surface of the tape after peeling.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] Aiming at the need of evaluating the bonding performance of the pole piece coating, the present invention adopts the mechanical testing method of a tensile machine, and formulates detailed steps and various operation modes and related indicators for the pole piece peeling test process, which mainly include: selecting samples, making samples, fixing samples, peeling testing, data selection, sample characterization and other steps; this testing method can effectively evaluate the pole piece peeling strength, improve the accuracy of the test data, and provide basic data for material selection, formula optimization, process improvement and the like related to the pole piece bonding strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is a schematic diagram of a test sample prepared in the present invention;
[0027] Figure 2 Schematic diagram of the fixed tension of the test sample;
[0028] Figure 3 This is a schematic diagram of the value of the tension stable section;
[0029] Figure 4 This is the surface morphology of the electrode after the peeling test. DETAILED DESCRIPTION
[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0031] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0032] Example 1
[0033] This embodiment provides a method for testing the peel strength of a lithium-ion battery electrode, comprising the following steps:
[0034] (1) The positive electrode sheet of a certain type of battery after rolling is made into a long strip of electrode sheet; the width of the long strip of electrode sheet is 25 mm, and the width direction is perpendicular to the rolling direction and parallel to the rolling direction; the length of the long strip of electrode sheet is 170 mm; the double-sided adhesive tape model selected is 3M stcoch 18 mm wide tape;
[0035] (2) The two samples were prepared and tested in the same way: double-sided tape was pasted on the front of the stainless steel base plate, the double-sided tape was pasted in the middle of the base plate, and the double-sided tape was pasted around the edge to the back side, and pasted smoothly on the edge of the base plate; the double-sided tape on the front of the base plate was peeled off, leaving the bottom side unpeeled; one side of the electrode strip was pasted on the double-sided tape on the front of the base plate, and in the left-right direction, the unadhered margin on both sides of the electrode was kept at 3.5 mm each; in the up-down direction, the adhered part of the electrode strip was greater than or equal to half of the electrode strip, and the unadhered part was on the side where the double-sided tape was bent, so as to ensure the integrity of the electrode when the electrode was torn off after rolling; a 2kg roller was used to roll the electrode axially for 6 times to make the electrode and the tape bonding surface uniform;
[0036] (3) Gently tear off the unbonded section of the electrode strip to expose the bonding surface of the electrode; fix the bottom plate of the torn end to the fixed end below the tensile machine; bend the natural end of the slightly torn electrode upward and clamp it to the upward traction end of the tensile machine;
[0037] (4) Set the tensile testing machine tensile speed to 100 mm / min, input the sample size parameters; set the peeling interval to 30%-70% of the deformation; click Test to start the tensile test;
[0038] (5) The tensile force fluctuation of less than 5% was selected as the stable section. The average tensile force of the stable section was divided by the electrode width, and the peel strengths of the two samples were obtained to be 28 N / m and 21 N / m respectively.
[0039] (6) Record the peeling surface morphology and determine that it is peeling between the slurry coating, without dots, particles, etc.
[0040] Example 2
[0041] This embodiment provides a method for testing the peel strength of a lithium-ion battery electrode, comprising the following steps:
[0042] (1) The positive electrode sheet of a certain type of battery after rolling is made into a long strip of electrode sheet; the width of the long strip of electrode sheet is 30 mm, and the width direction is perpendicular to the rolling direction and parallel to the rolling direction; the length of the long strip of electrode sheet is 180 mm; the double-sided adhesive tape model is 3Mstcoch 24 mm wide tape;
[0043] (2) The two samples were prepared and tested in the same way: double-sided tape was pasted on the front of the plastic base plate, the double-sided tape was pasted in the middle of the base plate, and the double-sided tape was pasted around the edge to the back side, and pasted smoothly on the edge of the base plate; the double-sided tape on the front of the base plate was peeled off, leaving the bottom side unpeeled; one side of the electrode strip was pasted on the double-sided tape on the front of the base plate, and in the left-right direction, the unadhered margin on both sides of the electrode was kept at 3mm each; in the up-down direction, the adhered part of the electrode strip was greater than or equal to half of the electrode strip, and the unadhered part was on the side where the double-sided tape was bent, so as to ensure the integrity of the electrode when the electrode was torn off after rolling; a 2kg roller was used to roll the electrode axially for 6 times to make the electrode and the tape bonding surface uniform;
[0044] (3) Gently tear off the unbonded section of the electrode strip to expose the bonding surface of the electrode; fix the bottom plate of the torn end to the fixed end below the tensile machine; bend the natural end of the slightly torn electrode upward and clamp it to the upward traction end of the tensile machine;
[0045] (4) Set the tensile testing machine’s tensile speed to 60 mm / min, input the sample size parameters, set the peeling interval to 30%-70% of the deformation, and click Test to start the tensile test.
[0046] (5) The tensile force fluctuation is less than 5% as the stable section. The test shows that the peel strengths of the two samples are 48N / m and 44N / m respectively;
[0047] (6) Record the peeling surface morphology and determine that it is peeling between the slurry coating, without dots, particles, etc.
[0048] Example 3
[0049] This embodiment provides a method for testing the peel strength of a lithium-ion battery electrode, comprising the following steps:
[0050] (1) Take the positive electrode sheet of a certain type of battery after rolling to make a long strip of electrode sheet; the width of the long strip of electrode sheet is 30 mm, and the width direction is perpendicular to the rolling direction and parallel to the rolling direction; the length of the long strip of electrode sheet is 180 mm; the double-sided adhesive model is 3M 9080 24 mm wide tape;
[0051] (2) The two samples were prepared and tested in the same way: double-sided tape was pasted on the front of the plastic base plate, the double-sided tape was pasted in the middle of the base plate, and the double-sided tape was pasted around the edge to the back side, and pasted smoothly on the edge of the base plate; the double-sided tape on the front of the base plate was peeled off, leaving the bottom side unpeeled; one side of the electrode strip was pasted on the double-sided tape on the front of the base plate, and in the left-right direction, the unadhered margin on both sides of the electrode was kept at 3mm each; in the up-down direction, the adhered part of the electrode strip was greater than or equal to half of the electrode strip, and the unadhered part was on the side where the double-sided tape was bent, so as to ensure the integrity of the electrode when the electrode was torn off after rolling; a 2kg roller was used to roll the electrode axially for 6 times to make the electrode and the tape bonding surface uniform;
[0052] (3) Gently tear off the unbonded section of the electrode strip to expose the bonding surface of the electrode; fix the bottom plate of the torn end to the fixed end below the tensile machine; bend the natural end of the slightly torn electrode upward and clamp it to the upward traction end of the tensile machine;
[0053] (4) Set the tensile testing machine's tensile speed to 150 mm / min, input the sample size parameters, set the peeling interval to 30%-70% of the deformation, and click Test to start the tensile test.
[0054] (5) The tensile force fluctuation is less than 5% as the stable section. The test shows that the peel strengths of the two samples are 9N / m and 7N / m respectively;
[0055] (6) Record the morphology of the peeling surface and determine whether it is the peeling between the dressing coating and the current collector, without dots, particles, etc.
[0056] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. A method for testing the peel strength of a lithium-ion battery electrode, characterized in that: The following steps are involved: S1. Take the rolled positive electrode sheet and make it into a long strip of electrode, wherein the length of the long strip of electrode is greater than 100 mm and the width is 20 to 35 mm; S2. Take a hard plate as the base plate, paste double-sided tape in the middle of the front of the base plate, and the two ends of the double-sided tape go around the two side edges of the base plate and paste to the back of the base plate; then, peel off the double-sided tape on the front of the base plate, leaving the bottom surface unpeeled, paste the electrode strip to be tested on the double-sided tape, keep the unpasted margins on both sides of the electrode strip equal, and the pasted part of the electrode strip is greater than half of the total length of the electrode strip; use a pressure roller to roll the electrode strip to make the bonding surface of the electrode strip and the double-sided tape uniform; S3. Tear off the unpasted end of the electrode strip to expose the adhesive surface of the electrode strip; fix the torn end of the bottom plate to the fixed end below the tensile machine; bend the natural end of the torn electrode strip upward and clamp it to the upward traction end of the tensile machine; S4. Set the parameters of the tensile testing machine and perform tensile force test; S5. After the tensile force test is completed, the stage in the tensile force curve where the tensile force changes by no more than 10% is taken as the stable peeling section, and then the average tensile force of the stable peeling section is divided by the width of the electrode sheet to calculate the peeling strength of the battery electrode sheet; In step S1, the pole piece strips are divided into two types, namely pole piece strips whose width direction is perpendicular to the rolling direction and pole piece strips whose width direction is parallel to the rolling direction; In step S2, when rolling the pole piece strip, a 2 kg roller is used to roll the pole piece strip 3-6 times along the axial direction.
2. A method for testing the peel strength of a lithium-ion battery electrode according to claim 1, characterized in that: In step S2, the base plate is made of stainless steel, glass or plastic.
3. The method for testing the peel strength of a lithium-ion battery electrode according to claim 1, characterized in that: In step S2, the width of the double-sided adhesive tape is narrower than the width of the electrode strip, and the difference between the two is 5 to 6 mm.
4. The method for testing the peel strength of a lithium-ion battery electrode according to claim 1, characterized in that: In step S2, the pressing roller rolls naturally during rolling without using artificial external pressure.
5. The method for testing the peel strength of a lithium-ion battery electrode according to claim 1, characterized in that: In step S3, the natural end of the pole piece strip is bent into a reverse 180° bend.
6. The method for testing the peel strength of a lithium-ion battery electrode according to claim 1, characterized in that: In step S4, the parameters of the tensile testing machine include stretching speed, sample size parameters and peeling interval, wherein the stretching speed is set to 50-300 mm / min.
7. The method for testing the peel strength of a lithium-ion battery electrode according to claim 1, characterized in that: In step S5, the tensile force stable section is selected according to the "time-force" curve.
8. The method for testing the peel strength of a lithium-ion battery electrode according to claim 1, characterized in that: Step S5 also includes the step of recording the morphology of the surface of the electrode strip and the surface of the tape after peeling.