Electrochemical materials including solid and liquid phases
By using alkali metal alloy electrodes with solid and liquid phases at room temperature in lithium-ion batteries, the limitations of battery energy density and charging rate are solved, and battery performance with high area capacity and current density is achieved.
Patent Information
- Application Number
- CN202080057125.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-06-18
- Filing Date
- 2020-04-17
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-04-17
AI Technical Summary
The energy density and charge/discharge rates of lithium-ion batteries are limited by mechanically unstable interfaces and dendrites between electrodes and electrolytes, resulting in limited energy density and poor charging times.
Using an electrochemical device containing an alkali metal alloy, which has a solid and liquid phase at room temperature, the electrode is improved by alloying alkali metals such as lithium, sodium, and potassium to reduce hardness and yield stress and increase softness and ductility. Critical current density and energy density.
It achieves the reduction of dendrite-induced short circuits under the condition of high area capacity and current density, improves the cycle stability and energy density of the battery, and is suitable for applications such as electric vehicles.
Smart Images

Figure CN114223082B_ABST
Abstract
Description
[0001] Related Applications
[0002] This application claims the benefit of U.S. Provisional Application No. 62 / 863,144, filed on June 18, 2019, under 35 U.S.C. 119(e), the disclosure of which is incorporated herein by reference in its entirety. Technical Field
[0003] Generally, electrochemical devices related to the use of electrochemical materials including solid and liquid phases, as well as associated materials and methods are described. Background Art
[0004] Increasing the energy density and charge / discharge rate of lithium-ion (Li-ion) batteries is important to accelerate the adoption of such batteries for a wide range of applications, including transportation (e.g., electric vehicles) and grid storage (e.g., power grids). Lithium metal-based anodes offer a path to improved energy density, but are limited in electroplating (e.g., charging) current density, e.g., to less than about 1 mA / cm 2 Such limitations prevent the use of high-areal capacity cathodes, thus resulting in batteries with limited energy density and poor charging time. Summary of the invention
[0005] Generally, electrochemical devices and associated materials and methods are described.In some cases, the subject matter of the present disclosure relates to interrelated products, alternative solutions to a particular problem, and / or multiple different uses of one or more devices, materials, and / or methods.
[0006] In certain embodiments, an electrochemical device is described. According to some embodiments, the electrochemical device includes an electrode comprising an alloy, wherein the alloy includes at least one alkali metal and the alloy has a solid phase and a liquid phase at a temperature between or equal to 15°C and 30°C.
[0007] In some embodiments, an electroactive material is described. According to certain embodiments, the electroactive material comprises an alloy comprising at least two alkali metals, wherein the alloy has a solid phase and a liquid phase at a temperature between or equal to 15°C and 30°C.
[0008] In certain embodiments, a method of operating an electrochemical device is described. According to some embodiments, the method includes charging and / or discharging the electrochemical device at a first temperature, wherein at least one electrode of the electrochemical device includes an alloy having a solid phase and a liquid phase at the first temperature.
[0009] Other advantages and novel features of the present invention will become apparent from the following detailed description of various non-limiting embodiments of the invention when considered in conjunction with the accompanying drawings.In the event that this specification and documents incorporated by reference include conflicting and / or inconsistent disclosures, this specification shall prevail. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Non-limiting embodiments of the present invention will be described by way of example with reference to the accompanying drawings, which are schematic and are not intended to be drawn to scale. In the drawings, each identical or nearly identical component shown is generally represented by a single numeral. For clarity, not every component is labeled in every drawing, nor is every component of every embodiment of the invention shown, where the illustrations would not necessarily enable one of ordinary skill in the art to understand the invention. In the drawings:
[0011] Figure 1 shows a schematic cross-sectional view of an electrochemical device according to certain embodiments;
[0012] Figure 2 shows a schematic cross-sectional view of an electrode including a solid phase dispersed in a liquid phase according to certain embodiments;
[0013] Figure 3 shows a schematic cross-sectional view of an electrode including separate solid and liquid phases in contact with each other along an interface according to certain embodiments;
[0014] Figure 4 Methods of operating an electrochemical device according to certain embodiments are shown;
[0015] Figure 5A shows a synthesis temperature phase diagram of a Li-Na alloy at 1 atm according to certain embodiments;
[0016] Figure 5B shows a synthesis temperature phase diagram of a K-Li alloy at 1 atm according to certain embodiments;
[0017] Figure 5C shows a synthesis temperature phase diagram of a K—Na alloy at 1 atm according to certain embodiments;
[0018] Figure 6 shows a pressure-temperature phase diagram of Li according to certain embodiments;
[0019] Fig. 7A shows a phase field simulation of electrode morphology after electrodeposition at large applied current density according to certain embodiments;
[0020] Figure 7B shows a phase field simulation of the interface velocity distribution at a dendrite tip according to certain embodiments;
[0021] Figure 7C shows a phase field simulation of the distribution of the Li ion mole fraction around the dendrite tip according to certain embodiments;
[0022] Fig.7D shows a two-dimensional electric field vector distribution around a dendrite according to certain embodiments;
[0023] Fig. 8A A phase change diagram showing electrode morphology of a metal electrode having dendrites according to certain embodiments;
[0024] Figure 8B shows a distribution diagram of normal stress according to certain embodiments;
[0025] Figure 8C shows a distribution graph of inhibitory factors according to certain embodiments;
[0026] Fig.9A shows critical current density versus area capacity for a symmetric battery cell according to certain embodiments;
[0027] Fig. 9B shows the average critical current density of a symmetric battery cell ignoring area capacity according to certain embodiments;
[0028] Fig. 9C According to some embodiments, Fig.9A Comparative critical current density versus area capacity for a symmetric cell on an enlarged y-axis scale;
[0029] Fig.9D According to some embodiments, Fig. 9B Compared to the average critical current density of a symmetric battery cell ignoring the area capacity on the enlarged y-axis scale;
[0030] Fig. 10A 60 hours of voltage time trace and current density time trace of a NaK(e)-Li / LLZTO / NaK(e)-Li battery cell according to certain embodiments are shown;
[0031] Fig. 10B shows that according to some embodiments, the -2 Up to 1.75 mA cm -2 Electrochemical impedance spectroscopy (EIS) spectrum of the NaK(e)-Li / LLZTO / NaK(e)-Li battery cell;
[0032] Fig. 10C The NaK(e)-Li / LLZTO / NaK(e)-Li battery cell according to certain embodiments is shown in FIG. Fig. 10AVoltage time trace and current density time trace for 20 hours after the data in;
[0033] Fig. 10D shows that according to some embodiments, the -2 Up to 3mA·cm -2 EIS spectrum of NaK(e)-Li / LLZTO / NaK(e)-Li battery cell below;
[0034] Fig.11A shows a 50-hour voltage-time trace and a current-density-time trace of a 95K5Na / KBA / 95K5Na battery cell according to certain embodiments;
[0035] Fig. 11B shows that according to some embodiments, the -2 Up to 10mA·cm -2 The EIS spectrum of the 95K5Na / KBA / 95K5Na battery cell is shown below;
[0036] Fig. 11C The 95K5Na / KBA / 95K5Na battery cell according to certain embodiments is shown in FIG. Fig.11A Voltage time trace and current density time trace for 10 hours after the data in;
[0037] Fig.11D shows that according to some embodiments, the -2 Up to 20mA·cm -2 EIS spectrum of the 95K5Na / KBA / 95K5Na battery cell. DETAILED DESCRIPTION
[0038] The inventors have realized and understood that mechanically soft metal electrodes provide a way to improve the critical current density of the electrode. In some embodiments, an electrochemical device (such as a rechargeable battery) is described, which includes an electrode comprising an alloy, which is used as an electrochemical material of the electrode. In some embodiments, the alloy can have both a solid phase and a liquid phase of a metal alloy within the temperature range of storage and / or utilization of the electrochemical device. Such a temperature can be, for example, at room temperature or close to room temperature (for example, between about 15°C and 30°C or equal to about 15°C and 30°C, but other temperatures above and below the range can be used). In some embodiments, the solid phase includes a first synthesis of one or more alkali metals, and the liquid phase includes a different second synthesis of one or more alkali metals. For example, in some non-limiting embodiments, the solid phase can have a synthesis with a larger percentage of a first alkali metal (such as lithium), and the liquid phase can have a synthesis with a larger percentage of a second alkali metal (such as sodium or potassium). In other non-limiting embodiments, the solid phase and the liquid phase can include different proportions of the same alkali metal. Since alkali metals such as sodium and potassium have significantly lower yield stresses than lithium, alloys containing lithium, for example, in combination with sodium and / or potassium, can be mechanically soft, yet capable of achieving high critical current densities. Thus, such composite electrodes can, in some cases, have a mechanical softness that allows both a desired energy density and an improved current density, compared to, for example, a substantially pure alkali metal (e.g., pure lithium) electrode.
[0039] Without wishing to be bound by theory, one obstacle to achieving batteries with high energy density in continuous cycling is the mechanically unstable interface between the electrode and the electrolyte at standard electrodeposition rates. In some cases, for example, some conventional electrochemical devices with solid electrodes have a maximum sustainable current density (e.g., ~1 mA / cm 2 ), which does not allow devices containing electrodes with high areal capacity to cycle at rates required for applications such as electric vehicles. In addition, conventional electrochemical devices that employ Li-containing electrodes (e.g., anodes) typically generate metal dendrites at current densities used during charging and / or discharging of the device. Such dendrites can propagate at surface cracks in the electrochemical device, thereby inducing undesirable side reactions that can reduce the energy density of the device and / or cause the electrode to short-circuit.
[0040] In view of the above, the inventors have recognized the benefits associated with the use of electroactive materials that include alloys comprising at least one alkali metal. According to some embodiments, alloying the alkali metal with one or more elements can change the chemical and / or mechanical properties of the alkali metal. In certain embodiments, for example, at least one alkali metal can be alloyed with an element, which reduces the hardness, yield stress, creep stress and / or melting point of at least a portion of the alkali metal. In some embodiments, at least one alkali metal can be alloyed with an element, which increases the softness, ductility and / or creep rate of at least a portion of the alkali metal. It should be understood that metal softness / hardness, yield stress, creep stress, melting point, ductility and / or creep rate are chemical and / or mechanical properties that will be understood by a person of ordinary skill in the art. According to certain embodiments, at least one alkali metal can be alloyed with a mass isotope of at least one alkali metal to obtain an alloy including at least one alkali metal enriched beyond the natural distribution of the isotope. In some embodiments, the mass isotope of at least one alkali metal is 6 Li.
[0041] In some embodiments, the alloy includes more than one alkali metal (e.g., two alkali metals, three alkali metals, etc.). For example, in certain embodiments, the alloy includes lithium (Li), sodium (Na), potassium (K), rubidium (Rb), and / or cesium (Cs). In some embodiments, lithium can be 6 Li and / or 7 Li. Other isotopes of other alkali metals are also contemplated.
[0042] In certain embodiments, the alloy includes an alkali metal alloyed with a non-alkali metal. For example, in certain embodiments, the alloy may include gallium (Ga), indium (In), tin (Sn), lead (Pb), bismuth (Bi) and / or mercury (Hg). Examples of eutectic mixtures that may be included in the alloy are Ga-In-Sn (e.g., potassium indium tin alloy) and / or Cs-Na-K. The inventors further recognize the benefits associated with using an electroactive material for an electrode of an electrochemical device, which has both a solid phase and a liquid phase of a metal alloy system within a desired operating temperature range. In certain embodiments, the solid phase of the alloy includes one or more alkali metals. For example, in some embodiments, the solid phase of the alloy may include Li, Na and / or K. In certain embodiments, the liquid phase of the alloy includes one or more alkali metals. For example, in some embodiments, the liquid phase of the alloy includes Li, Na and / or K. According to certain embodiments, the synthesis of at least one elemental component of the alloy varies between the solid phase and the liquid phase. For example, in a specific embodiment, the solid phase of the alloy may have a higher molar percentage of the electroactive component of the electroactive material compared to the liquid phase. For example, Li-ion based devices may use materials with a higher mole percentage of Li in the solid phase compared to a liquid phase that may include a higher concentration of Na and / or K. Likewise, a larger percentage of Na, K, or any other suitable electroactive component may be present in the solid phase of an electroactive material where these materials serve as the electroactive component of an alloy.
[0043] In some embodiments, the composition of the liquid phase may have a reduced solubility in the solid phase of the alloy forming the electrode of the electrochemical device. For example, in such an embodiment, at least one alkali metal of the solid phase may be different from at least one alkali metal of the liquid phase, or at least exhibit a lower concentration in the liquid phase. For example, the solid phase of the alloy may include Li and / or Na, and the liquid phase of the alloy includes K. In another non-limiting embodiment, the solid phase of the alloy includes Li and / or K, and the liquid phase of the alloy includes Na. In another non-limiting embodiment, the solid phase of the alloy includes Na and / or K, and the liquid phase of the alloy includes Li. In another non-limiting embodiment, the solid phase of the alloy includes Li, and the liquid phase of the alloy includes Na and / or K. In another non-limiting embodiment, the solid phase of the alloy includes Na, and the liquid phase of the alloy includes Li and / or K. In another non-limiting embodiment, the solid phase of the alloy includes K, and the liquid phase of the alloy includes Li and / or Na.
[0044] When the device is operated at a set temperature, the relative amounts of the solid and liquid phases of the alloy can change depending on the synthesis of the alloy. Therefore, since the concentration of the electroactive component within the entire electrode changes throughout the charge and discharge cycle of the electroactive material due to ion transfer between the anode and cathode of the device, the overall ratio of the solid and liquid phases can change depending on the charge state of the electroactive material, which is explained in more detail below.
[0045] Depending on the desired operating parameters, the synthesis of the electrode alloy can be selected to provide any desired solid-to-liquid operating range during the charge-discharge cycle of the electrochemical device. For example, during nominal operation of the electrochemical device, the electrode can have an atomic ratio of solid and liquid phases that is at least 1%, at least 10%, at least 20%, at least 30%, at least 40%, at least 50%, at least 60%, at least 70%, at least 80%, or at least 90%. In some embodiments, the atomic ratio of the solid phase to the liquid phase in the alloy can be maintained within a range of less than 100%, less than or equal to 90%, less than or equal to 80%, less than or equal to 70%, less than or equal to 60%, less than or equal to 50%, less than or equal to 40%, less than or equal to 30%, less than or equal to 20%, or less than or equal to 10%. Combinations of the above ranges are also possible (e.g., the atomic ratio of the solid phase to the liquid phase in the alloy can be maintained in a range of at least 1% and less than 100%, and the atomic ratio of the solid phase to the liquid phase in the alloy can be maintained in a range of at least 70% and less than or equal to 80%). Other ranges are also possible.
[0046] As described above, in certain embodiments, when the electrochemical device is operating, at least a portion of the solid phase and / or at least a portion of the liquid phase of the alloy may change its material state. For example, in certain embodiments, when the electrochemical device is being charged and / or discharged, the atomic ratio of the solid phase to the liquid phase may change according to the temperature, pressure and / or charge state of the device. For example, in certain embodiments, when the device is being charged and / or discharged, the atomic ratio of the solid phase to the liquid phase may change to less than or equal to 30%, less than or equal to 20%, less than or equal to 10%, less than or equal to 8%, less than or equal to 6%, less than or equal to 4%, or less than or equal to 2%. In some embodiments, when the device is being charged and / or discharged, the atomic ratio of the solid phase to the liquid phase may change to greater than or equal to 1%, greater than or equal to 2%, greater than or equal to 4%, greater than or equal to 6%, or greater than or equal to 8%. Combinations of the above-referenced ranges are also possible (e.g., when the device is being charged and / or discharged, the atomic ratio of the solid phase to the liquid phase changes by less than or equal to 30% and greater than or equal to 1%, when the device is being charged and / or discharged, the atomic ratio of the solid phase to the liquid phase changes by less than or equal to 6% and greater than or equal to 2%). Other ranges greater and less than those recited above are also possible.
[0047] In certain embodiments, the solid phase of the alloy (eg, electroactive material) includes Li, Na, and / or K. In some embodiments, the solid phase includes at least one alkali metal, at least two alkali metals, or at least three alkali metals.
[0048] In some embodiments, the solid phase includes Li. In some such embodiments, the solid phase may include any suitable amount of Li in various suitable amounts. In some embodiments, for example, the solid phase includes Li in an amount greater than or equal to 1 mol%, greater than or equal to 10 mol%, greater than or equal to 20 mol%, greater than or equal to 30 mol%, greater than or equal to 40 mol%, greater than or equal to 50 mol%, greater than or equal to 60 mol%, greater than or equal to 70 mol%, greater than or equal to 80 mol%, or greater than or equal to 90 mol% based on the total moles in the solid phase. In certain embodiments, the solid phase includes Li in an amount less than or equal to 99.9 mol%, less than or equal to 90 mol%, less than or equal to 80 mol%, less than or equal to 70 mol%, less than or equal to 60 mol%, less than or equal to 50 mol%, less than or equal to 40 mol%, less than or equal to 30 mol%, less than or equal to 20 mol%, or less than or equal to 10 mol% based on the total moles in the solid phase. Combinations of the above-referenced ranges are also possible (e.g., the solid phase includes Li in an amount greater than or equal to 1 mol % and less than or equal to 99.9 mol %, based on the total moles in the solid phase, and the solid phase includes Li in an amount greater than or equal to 90 mol % and less than or equal to 99.9 mol %, based on the total moles in the solid phase). Other ranges of Li in the solid phase of the alloy greater than and less than those ranges recited above are also possible.
[0049] In certain embodiments, the solid phase includes Na. In some such embodiments, the solid phase may include any suitable amount of Na in various suitable amounts. In some embodiments, for example, the solid phase includes Na in an amount greater than or equal to 1 mol%, greater than or equal to 10 mol%, greater than or equal to 20 mol%, greater than or equal to 30 mol%, greater than or equal to 40 mol%, greater than or equal to 50 mol%, greater than or equal to 60 mol%, greater than or equal to 70 mol%, greater than or equal to 80 mol% or greater than or equal to 90 mol% based on the total moles in the solid phase. In certain embodiments, the solid phase includes Na in an amount less than or equal to 99.9 mol%, less than or equal to 90 mol%, less than or equal to 80 mol%, less than or equal to 70 mol%, less than or equal to 60 mol%, less than or equal to 50 mol%, less than or equal to 40 mol%, less than or equal to 30 mol%, less than or equal to 20 mol% or less than or equal to 10 mol% based on the total moles in the solid phase. Combinations of the above-referenced ranges are also possible (e.g., the solid phase includes Na in an amount greater than or equal to 1 mol % and less than or equal to 99.9 mol % based on the total moles in the solid phase, the solid phase includes Na in an amount greater than or equal to 1 mol % and less than or equal to 10 mol % based on the total moles in the solid phase). Other ranges of Na in the solid phase of the alloy greater than and less than those ranges recited above are also possible.
[0050] In some embodiments, the solid phase includes K. In some such embodiments, the solid phase can include K in any of a variety of suitable amounts. In some embodiments, for example, the solid phase includes K in an amount greater than or equal to 1 mol%, greater than or equal to 10 mol%, greater than or equal to 20 mol%, greater than or equal to 30 mol%, greater than or equal to 40 mol%, greater than or equal to 50 mol%, greater than or equal to 60 mol%, greater than or equal to 70 mol%, greater than or equal to 80 mol%, or greater than or equal to 90 mol%, based on the total moles in the solid phase. In certain embodiments, the solid phase includes K in an amount less than or equal to 99.9 mol%, less than or equal to 90 mol%, less than or equal to 80 mol%, less than or equal to 70 mol%, less than or equal to 60 mol%, less than or equal to 50 mol%, less than or equal to 40 mol%, less than or equal to 30 mol%, less than or equal to 20 mol%, or less than or equal to 10 mol%, based on the total moles in the solid phase. Combinations of the above-referenced ranges are also possible (e.g., the solid phase includes K in an amount greater than or equal to 1 mol % and less than or equal to 99.9 mol %, based on the total moles in the solid phase, and the solid phase includes K in an amount greater than or equal to 1 mol % and less than or equal to 10 mol %, based on the total moles in the solid phase). Other ranges of K in the solid phase of the alloy greater than and less than those ranges recited above are also possible.
[0051] Any of the above ranges for the amount of Li, Na and / or K in the solid phase can be combined. In certain non-limiting embodiments, the solid phase includes Li and Na. For example, in some embodiments, the solid phase may include Li in an amount greater than or equal to 90 mol% based on the total moles in the solid phase and Na in an amount less than or equal to 10 mol%. In another non-limiting embodiment, the solid phase includes Li and K. For example, in certain embodiments, the solid phase may include Li in an amount greater than or equal to 90 mol% based on the total moles in the solid phase and K in an amount less than or equal to 10 mol%. In yet another non-limiting embodiment, the solid phase may include Na and K. In some embodiments, for example, the solid phase may include Na in an amount of 50 mol% based on the total moles in the solid phase and K in an amount of 50 mol%. In yet another non-limiting embodiment, the solid phase may include Li, Na and K. In some embodiments, for example, the solid phase may include Li in an amount greater than or equal to 80 mol%, Na in an amount less than or equal to 10 mol%, and K in an amount less than or equal to 10 mol% based on the total moles in the solid phase. Based on the ranges described herein, other combinations are also possible.
[0052] In certain embodiments, the liquid phase of the alloy (eg, electroactive material) includes Li, Na, and / or K. In some embodiments, the liquid phase includes at least one alkali metal, at least two alkali metals, or at least three alkali metals.
[0053] In some embodiments, the liquid phase includes Li. In some such embodiments, the liquid phase may include any suitable amount of Li in various suitable amounts. In some embodiments, for example, the liquid phase includes Li in an amount greater than or equal to 1 mol%, greater than or equal to 10 mol%, greater than or equal to 20 mol%, greater than or equal to 30 mol%, greater than or equal to 40 mol%, greater than or equal to 50 mol%, greater than or equal to 60 mol%, greater than or equal to 70 mol%, greater than or equal to 80 mol%, or greater than or equal to 90 mol% based on the total moles in the liquid phase. In certain embodiments, the liquid phase includes Li in an amount less than or equal to 99.9 mol%, less than or equal to 90 mol%, less than or equal to 80 mol%, less than or equal to 70 mol%, less than or equal to 60 mol%, less than or equal to 50 mol%, less than or equal to 40 mol%, less than or equal to 30 mol%, less than or equal to 20 mol%, or less than or equal to 10 mol% based on the total moles in the liquid phase. Combinations of the above-referenced ranges are also possible (e.g., the liquid phase includes Li in an amount greater than or equal to 1 mol % and less than or equal to 99.9 mol %, the liquid phase includes Li in an amount greater than or equal to 1 mol % and less than or equal to 10 mol %). Other ranges of Li in the liquid phase of the alloy greater than and less than those ranges recited above are also possible.
[0054] In certain embodiments, the liquid phase includes Na. In some such embodiments, the liquid phase may include any suitable amount of Na in various suitable amounts. In some embodiments, for example, the liquid phase includes Na in an amount greater than or equal to 1 mol%, greater than or equal to 10 mol%, greater than or equal to 20 mol%, greater than or equal to 30 mol%, greater than or equal to 40 mol%, greater than or equal to 50 mol%, greater than or equal to 60 mol%, greater than or equal to 70 mol%, greater than or equal to 80 mol% or greater than or equal to 90 mol% based on the total moles in the liquid phase. In certain embodiments, the liquid phase includes Na in an amount less than or equal to 99.9 mol%, less than or equal to 90 mol%, less than or equal to 80 mol%, less than or equal to 70 mol%, less than or equal to 60 mol%, less than or equal to 50 mol%, less than or equal to 40 mol%, less than or equal to 30 mol%, less than or equal to 20 mol% or less than or equal to 10 mol% based on the total moles in the liquid phase. Combinations of the above-referenced ranges are also possible (e.g., the liquid phase includes Na in an amount greater than or equal to 1 mol % and less than or equal to 99.9 mol %, the liquid phase includes Na in an amount greater than or equal to 90 mol % and less than or equal to 99.9 mol %). Other ranges of Na in the liquid phase of the alloy greater than and less than those ranges recited above are also possible.
[0055] In some embodiments, the liquid phase includes K. In some such embodiments, the liquid phase can include K in any of a variety of suitable amounts. In some embodiments, for example, the liquid phase includes K in an amount greater than or equal to 1 mol%, greater than or equal to 10 mol%, greater than or equal to 20 mol%, greater than or equal to 30 mol%, greater than or equal to 40 mol%, greater than or equal to 50 mol%, greater than or equal to 60 mol%, greater than or equal to 70 mol%, greater than or equal to 80 mol%, or greater than or equal to 90 mol%, based on the total moles in the liquid phase. In certain embodiments, the liquid phase includes K in an amount less than or equal to 99.9 mol%, less than or equal to 90 mol%, less than or equal to 80 mol%, less than or equal to 70 mol%, less than or equal to 60 mol%, less than or equal to 50 mol%, less than or equal to 40 mol%, less than or equal to 30 mol%, less than or equal to 20 mol%, or less than or equal to 10 mol%, based on the total moles in the liquid phase. Combinations of the above-referenced ranges are also possible (e.g., the liquid phase includes K in an amount greater than or equal to 1 mol % and less than or equal to 99.9 mol %, the liquid phase includes K in an amount greater than or equal to 90 mol % and less than or equal to 99.9 mol %). Other ranges of K in the liquid phase of the alloy greater than and less than those ranges recited above are also possible.
[0056] Any of the above ranges for the amount of Li, Na and / or K in the liquid phase can be combined. In certain non-limiting embodiments, the liquid phase includes Na and Li. In some embodiments, for example, the liquid phase may include Na in an amount greater than or equal to 90 mol% based on the total moles in the liquid phase and Li in an amount less than or equal to 10 mol%. In another non-limiting embodiment, the liquid phase includes K and Li. For example, in certain embodiments, the liquid phase may include K in an amount greater than or equal to 90 mol% based on the total moles in the liquid phase and Li in an amount less than or equal to 10 mol%. In yet another non-limiting embodiment, the liquid phase includes Na and K. For example, in certain embodiments, the liquid phase may include Na in an amount of 50 mol% based on the total moles in the liquid phase and K in an amount of 50 mol%. As another example, in some embodiments, the liquid phase may include Na in an amount greater than or equal to 10 mol% and less than or equal to 60% (e.g., 23 mol%) based on the total moles in the liquid phase and K in an amount greater than or equal to 40 mol% and less than or equal to 90 mol% (e.g., 77 mol%). In yet another non-limiting embodiment, the liquid phase includes Na, K, and Li. For example, in certain embodiments, the liquid phase may include Na in an amount greater than or equal to 40 mol %, K in an amount less than or equal to 40 mol %, and Li in an amount less than or equal to 10 mol % based on the total moles in the liquid phase. Other combinations are possible based on the ranges described herein.
[0057] The above ranges of compositions of the solid phase and liquid phase may be combined. In one such embodiment, the solid phase may include Li, and the liquid phase may include at least one of Na and K. For example, the solid phase may include Li in an amount greater than or equal to 90 mol % or any other suitable percentage based on the total moles in the solid phase. Accordingly, the liquid phase may include Na and / or K in an amount greater than or equal to 40 mol %, 60 mol %, 80 mol %, 90 mol % and / or any other suitable percentage based on the total moles in the liquid phase.
[0058] In some embodiments, both the solid phase and the liquid phase of the alloy include Li. In some embodiments, based on the total moles in the alloy, the solid phase may include a greater mole % of Li than the liquid phase. For example, in some embodiments, based on the total moles in the alloy, the solid phase includes more than 50 mole % of Li (e.g., 60 mole % of Li, 70 mole % of Li, 80 mole % of Li, 90 mole % of Li), and the liquid phase includes less than 50 mole % of Li (e.g., 40 mole % of Li, 30 mole % of Li, 20 mole % of Li, 10 mole % of Li). In some such embodiments in which both the solid phase and the liquid phase of the alloy include Li, the solid phase or the liquid phase may also include Na and / or K.
[0059] In some embodiments, both the solid phase and the liquid phase of the alloy include Na. In some embodiments, based on the total moles in the alloy, the solid phase includes a greater mole % of Na than the liquid phase. For example, in some embodiments, based on the total moles in the alloy, the solid phase includes more than 50 mole % of Na (e.g., 60 mole % of Na, 70 mole % of Na, 80 mole % of Na, 90 mole % of Na), and the liquid phase includes less than 50 mole % of Na (e.g., 40 mole % of Na, 30 mole % of Na, 20 mole % of Na, 10 mole % of Na). In some such embodiments in which both the solid phase and the liquid phase of the alloy include Na, the solid phase or the liquid phase may also include Li and / or K.
[0060] In some embodiments, both the solid phase and the liquid phase of the alloy include K. In some embodiments, the solid phase includes a greater mol % of K than the liquid phase based on the total moles in the alloy. For example, in some embodiments, the solid phase includes greater than 50 mol % K (e.g., 60 mol % K, 70 mol % K, 80 mol % K, 90 mol % K) and the liquid phase includes less than 50 mol % K (e.g., 40 mol % K, 30 mol % K, 20 mol % K, 10 mol % K) based on the total moles in the alloy. In some such embodiments in which both the solid phase and the liquid phase of the alloy include K, the solid phase or the liquid phase may also include Li and / or Na.
[0061] In certain non-limiting embodiments, the solid phase includes 80 mol % Li based on the total moles in the alloy, and the liquid phase includes 15.4 mol % K and 4.6 mol % Na based on the total moles in the alloy.
[0062] For the sake of clarity, alloys that include only a single solid phase and a single liquid phase are discussed. However, due to the complex interactions of multi-component alloys, it should be understood that some electrochemical materials, including the alloys described herein, can include multiple solid phases and / or liquid phases that coexist with each other during operation. Therefore, the present disclosure should not be interpreted as limited to systems that include a single solid phase and a single liquid phase.
[0063] As will be understood by those of ordinary skill in the art, the material state of the material depends on the environment of the material, such as the temperature and / or pressure of the material. Therefore, the alloys described herein may include solid and liquid phases at any desired combination of operating temperature and / or pressure. In some embodiments, it may be desirable for the electrochemical device to include a liquid phase under ambient conditions. For example, it may be beneficial that the alloy includes a solid phase and a liquid phase at room temperature or near room temperature so as to store and / or utilize the electrode in various applications without controlling the temperature of the electrochemical device. In certain embodiments, the alloy may include a solid phase and a liquid phase at a temperature of at least 15°C, at least 20°C, or at least 25°C. In some embodiments, the alloy may also include a solid phase and a liquid phase at a temperature of less than or equal to 30°C, less than or equal to 25°C, or less than or equal to 20°C. Combinations of the above ranges are also possible (e.g., the alloy includes a solid phase and a liquid phase at a temperature between 15°C and 30°C, and the alloy includes a solid phase and a liquid phase at a temperature between 20°C and 25°C). However, depending on the desired application and the specific composition used, operating temperatures of both the solid phase and the liquid phase of the alloy greater than and less than those temperatures described above are also envisioned.
[0064] In certain embodiments, the solid phase of the electrode described herein may have any of a variety of yield stresses. As explained herein, in some embodiments, it may be advantageous to use an electrode with a relatively low yield stress, which may be able to provide both high energy density and current density. According to some embodiments, when alloyed with other elements (such as Na and / or K), the yield stress of alkali metals (such as Li) can be reduced. In certain embodiments, the yield stress of the solid phase of the electrode is less than or equal to 0.5MPa, less than or equal to 0.4MPa, less than or equal to 0.3MPa, less than or equal to 0.2MPa, less than or equal to 0.1MPa, less than or equal to 0.05MPa, less than or equal to 0.01MPa or less than or equal to 0.005MPa. In certain embodiments, the yield stress of the solid phase is greater than or equal to 0.001 MPa, greater than or equal to 0.005 MPa, greater than or equal to 0.01 MPa, greater than or equal to 0.05 MPa, greater than or equal to 0.1 MPa, greater than or equal to 0.2 MPa, greater than or equal to 0.3 MPa, or greater than or equal to 0.4 MPa. Combinations of the above ranges are also possible (e.g., the electrode solid phase has a yield stress of less than or equal to 0.5 MPa and greater than or equal to 0.001 MPa, and the electrode solid phase has a yield stress of less than or equal to 0.2 MPa and greater than or equal to 0.1 MPa). Other ranges are also possible. The yield stress of the solid phase material can be measured in any appropriate manner, including using a typical tensile specimen test with a determined yield point and / or a 0.2% offset yield point.
[0065] The electroactive materials described herein can be used as electrode materials in electrochemical devices (e.g., batteries) that can be charged / discharged with high areal capacity. For example, in certain embodiments, the electroactive materials can be used in electrochemical devices that can charge / discharge at a capacity greater than or equal to 2 mAh / cm 2 , greater than or equal to 3mAh / cm 2 , greater than or equal to 4mAh / cm 2 , greater than or equal to 5mAh / cm 2 , greater than or equal to 6mAh / cm 2 , greater than or equal to 7mAh / cm 2 Or greater than or equal to 8 mAh / cm 2 Area capacity charge / discharge.
[0066] The electroactive materials described herein can be used as electrode materials in electrochemical devices (e.g., batteries) that can be charged / discharged at high current densities. For example, in certain embodiments, the electroactive materials can be used in electrochemical devices that can be charged / discharged at a current density greater than or equal to 1 mA / cm 2 , greater than or equal to 2mA / cm 2 , greater than or equal to 3 mA / cm 2 , greater than or equal to 4 mA / cm 2 , greater than or equal to 5mA / cm 2 , greater than or equal to 6 mA / cm 2 , greater than or equal to 7 mA / cm 2 , greater than or equal to 8mA / cm 2 , greater than or equal to 9mA / cm 2 Or greater than or equal to 10mA / cm 2 The current density is charged / discharged.
[0067] In certain embodiments, the above-mentioned areal capacities and / or current densities can be achieved without dendrite-induced short circuits. Such devices can advantageously provide high areal capacities and / or energy densities over a large number of cycles (e.g., greater than 500 cycles, greater than 1000 cycles, greater than 1500 cycles, etc.).
[0068] The alloy-based electroactive materials described herein and the corresponding electrodes that they can form can be manufactured using techniques known to those of ordinary skill in the art, such as melting, casting, expanding, doctor blade coating, spray deposition, evaporation, sputtering, chemical vapor deposition (CVD), mechanical mixing of components as solids and / or liquids, ball milling, mechanical compression molding, sintering of mixed particles, and / or any other suitable method.
[0069] In some embodiments, the electroactive alloys described herein can be used as an electrode (e.g., cathode or anode) in an electrochemical device such as a battery, a capacitor, a supercapacitor, or other suitable electrochemical device. According to some such embodiments, the electrochemical device can be a battery, such as a rechargeable battery (e.g., a secondary battery) or a non-rechargeable battery (e.g., a primary battery). In some embodiments, the battery (e.g., a rechargeable battery) can be used in transportation (e.g., electric vehicles, electric aircraft, electric ships, spacecraft), consumer products, grid storage applications (e.g., a grid for storing renewable energy), and / or any other suitable application.
[0070] In some embodiments, the anode of the device includes an electroactive material as described herein (e.g., an alloy having a solid phase and a liquid phase). The cathode may include any of a variety of electroactive materials (e.g., a cathode active material). In certain embodiments, the cathode is or includes a cathode active material of a lithium ion battery, a sodium ion battery, or a potassium ion battery. In some embodiments, the cathode active material includes one or more metal oxides. In some embodiments, an embedded cathode (e.g., a lithium embedded cathode) can be used. Non-limiting examples of suitable materials that can embed ions of electroactive materials (e.g., alkali metal ions) include metal oxides, metal sulfides, metal halides, and / or redox active organic compounds. In some embodiments, the cathode is an embedded cathode including a lithium transition metal oxide or a lithium transition metal phosphate. In some embodiments, the cathode includes lithium nickel manganese cobalt oxide or lithium iron phosphate. In such embodiments, the cathode or other electrodes of the electrochemical device may include one or more additives, electrolytes, salts, and / or binder materials (e.g., polymers).
[0071] According to certain embodiments, the electrochemical devices described herein may include a solid electrolyte disposed between a first electrode including a solid phase and a liquid phase as described herein and a second electrode located on an opposite side of the solid electrolyte. In some embodiments, the solid electrolyte may include an inorganic compound, such as a ceramic and / or a crystalline material. For example, in certain embodiments, the solid electrolyte includes a lithium garnet, such as lithium lanthanum titanium oxide (LLTO). In certain embodiments, the solid electrolyte includes Li-β"-Al 2 O 3 (LBA), Na-β”-Al 2 O 3 (NBA) or K-β”-Al 2 O 3(KBA). In certain embodiments, the solid electrolyte includes a superionic conductor (SICON), such as LiSICON and / or NaSICON. In certain embodiments, the solid electrolyte may include a lithium solid electrolyte such as lithium phosphide, or a potassium solid electrolyte. In some embodiments, one or more solid polymers may be used to form a solid electrolyte. Examples of useful solid polymer electrolytes include, but are not limited to, those comprising one or more polymers selected from the group consisting of: polyethers, polyethylene oxides, polypropylene oxides, polyimides, polyphosphazenes, polyacrylonitrile, polysiloxanes, the aforementioned derivatives, the aforementioned copolymers, the aforementioned crosslinked and network structures, and the aforementioned blends. In certain embodiments, a combination of the above-mentioned inorganic compounds and / or polymers may be used as a solid electrolyte, such as a mixed or synthetic solid electrolyte comprising an inorganic compound and a polymer. In certain embodiments, the inorganic compound and / or polymer is a conductor of the working ion (e.g., Li) of an electrochemical device. Turning to the accompanying drawings, specific non-limiting embodiments are described in more detail. It should be understood that the various systems, components, features, and methods described with respect to these embodiments may be used alone and / or in any desired combination, because the present disclosure is not limited to the specific embodiments described herein.
[0072] According to some embodiments, an electrochemical device (e.g., a battery) is described, wherein the electrochemical device includes at least one electrode. In some embodiments, the electrochemical device includes two electrodes, such as a cathode and an anode. One of ordinary skill in the art will be familiar with the term "cathode" referring to the positive electrode as a power source during normal use of the device (e.g., during discharge) and the term "anode" referring to the negative electrode. Figure 1 Schematic cross-sectional view of an electrochemical device according to certain embodiments is shown. Figure 1 As shown in , the electrochemical device 100 includes: a first electrode 102; a solid electrolyte 104 disposed on the first electrode; and a second electrode 106 disposed on the solid electrolyte on a side opposite to the first electrode. The first electrode and the second electrode of the electrochemical device may include corresponding first and second electroactive materials. For example, as described herein, the first and / or second electroactive materials may include an alloy having a solid phase and a liquid phase during nominal operation.
[0073] Although a single plane geometry of the electrode is depicted in the drawings, where the electrode is located on opposite sides of the solid electrolyte, other configurations are possible. For example, a jelly roll of the electrode, a planar stack, and any other suitable electrode configuration may also be used. In addition, other suitable components not depicted in the drawings, such as current collectors (wires, foils, grids, etc.) that are in electrical contact with the electrode may also be included in the electrochemical device, because the depicted embodiments are schematic in nature. In addition, although a solid electrolyte has been depicted, any suitable components that can separate the two electrodes from each other may also be used, including a separator of a suitable structure, because the present disclosure is not limited in such a manner.
[0074] One or more electrodes of the electrochemical devices described herein can have any of a variety of suitable thicknesses. Figure 1 , for example, electrode 102 may have a thickness 108. In some embodiments, one or more electrodes of the electrochemical device have a thickness of less than or equal to 1 mm, less than or equal to 500 microns, less than or equal to 400 microns, less than or equal to 300 microns, less than or equal to 200 microns, less than or equal to 100 microns, less than or equal to 50 microns, less than or equal to 25 microns, or less than or equal to 10 microns. In certain embodiments, the electrode has a thickness of at least 1 micron, at least 10 microns, at least 25 microns, at least 50 microns, at least 100 microns, at least 200 microns, at least 300 microns, or at least 400 microns. Combinations of the above-mentioned ranges are also possible (for example, one or more electrodes may have a thickness of at least 1 micron and less than or equal to 1 mm, and one or more electrodes may have a thickness of at least 10 microns and less than or equal to 50 microns). Other ranges are also possible.
[0075] The liquid phase and the solid phase in the alloy can coexist with each other in any of a variety of configurations. In some embodiments, the electrode 102 may include a plurality of particles of the solid phase 120 disposed in or otherwise dispersed (e.g., randomly dispersed) within the liquid phase 130, see Figure 2 In certain embodiments, the solid phase 120 and / or the liquid phase 130 may form an interconnected network, depending on the specific atomic ratio of the solid phase to the liquid phase. In some embodiments, the alloy may form a solid-liquid mixture, slurry, or amalgam having any suitable combination of resulting physical and electrochemical properties. In certain embodiments, the liquid phase and / or the solid phase may form an interconnected network.
[0076] In another embodiment, Figure 3As depicted in , electrode 102 includes a solid phase 120 separated from a liquid phase 130, wherein an interface extends between the two phases. In such embodiments, the solid phase or the liquid phase may be first deposited onto a current collector or other substrate not depicted. While these configurations are shown in the accompanying drawings, it should be understood that in some embodiments, other configurations of other electrodes having solid and liquid phases may exist.
[0077] According to some embodiments, a method of operating an electrochemical device is described. Figure 4 A method of operating an electrochemical device according to certain embodiments is shown. In certain embodiments, method 200 includes discharging the electrochemical device at a first temperature at step 202. In some such embodiments, at least one electrode of the electrochemical device includes an alloy having a solid phase and a liquid phase at the first temperature, as described herein.
[0078] The temperature at which the electrochemical device is discharged (e.g., the first temperature) can be any of a variety of temperatures. As described above, in certain embodiments, it may be desirable to discharge the electrochemical device at room temperature or near room temperature depending on the application of the device. In some embodiments, for example, the temperature at which the electrochemical device is discharged is at least 15°C, at least 20°C, or at least 25°C. In some embodiments, the temperature at which the electrochemical device is discharged is less than or equal to 30°C, less than or equal to 25°C, or less than or equal to 20°C. Combinations of the above ranges are also possible (e.g., the temperature at which the electrochemical device is discharged is between 15°C and 30°C, and the temperature at which the electrochemical device is discharged is between 20°C and 25°C). Other temperature ranges greater than and less than those ranges described above are also possible for the alloy to include both solid and liquid phases during operation.
[0079] In some embodiments, as a result of discharging the electrochemical cell, ions (e.g., Li ions) can flow from the electroactive material of the first electrode (e.g., anode) to the second electrode (e.g., cathode) through the electrolyte (e.g., solid electrolyte), as will be understood by one of ordinary skill in the art. For example, with reference to Figure 4 , method 200 may further include causing ions to flow from the first electrode to the second electrode at step 204. In certain embodiments, for example, an electrode of an electrochemical device comprising an alloy having a solid phase and a liquid phase may be discharged such that ions flow through at least a portion of the solid phase and / or the liquid phase of the alloy. Advantageously, as a result of the combination of the solid phase and the liquid phase in the alloy, ions (e.g., Li ions) may have a higher flux and / or mobility in the alloy, resulting in a higher critical current density of the electrochemical device, as described. Without wishing to be bound by theory, depending on the configuration of the electrodes (e.g., see Figure 2 and Figure 3), embodiments are contemplated in which ions of the electroactive material flow through both the solid and liquid phases of the alloy, only the solid phase of the alloy, only the liquid phase of the alloy, or a combination thereof.
[0080] In addition, as described herein, as a result of operating (e.g., discharging) an electrochemical device and causing ions to flow from a first electrode (e.g., an anode) to a second electrode (e.g., a cathode), the relative amounts of the solid and liquid phases of the alloy can change depending on the synthesis of the alloy. For example, removing electroactive ions from an alloy electrode can change the overall synthesis of the alloy, which will result in a corresponding change in the ratio of the solid and liquid phases of the alloy.
[0081] According to some embodiments, method 200 may include charging the electrochemical device at step 206. For example, referring to Figure 4 , method 200 may include charging the electrochemical device at a first temperature at step 206. As described above, the temperature at which the electrochemical device is charged may be at or near room temperature (e.g., between 15° C. and 30° C.), but other temperatures are contemplated. In some embodiments, as a result of charging the electrochemical cell, ions may flow from the second electrode to the first electrode through the electrolyte. Reference Figure 4 , for example, method 200 may include causing ions to flow from the second electrode to the first electrode at step 208. As the ions flow back into the first electrode, the composition of the alloy including the solid phase and the liquid phase that forms the electrode may change again due to the addition of other electroactive ions back into the alloy. This may result in a change in the relative proportions of the solid and liquid phases to recover towards the initial atomic ratio at the fully charged state of the electrochemical device. Thus, the charging and discharging of the electrochemical device may correspond to a change in the relative proportions of the solid and liquid phases present within the alloy that forms the electrode of the device.
[0082] In some embodiments, discharging the electrochemical device (e.g., as in step 202) and charging the electrochemical device (e.g., as in step 208) can constitute cycling the electrochemical device. In certain embodiments, method 200 can be repeated (e.g., the electrochemical device can be cycled) 500 times, 1,000 times, 5,000 times, 10,000 times, etc.
[0083] Although as explained in this article, Figure 4 Discharging the electrochemical device and then charging the device is described, but one of ordinary skill in the art will appreciate that embodiments are contemplated in which the electrochemical device may be charged first and then discharged. Alternatively, in some embodiments, an electrochemical device such as a primary battery is also described, and the method of operating such a device may include only discharging the device.
[0084] Example 1
[0085] The following examples describe electroactive materials having solid and liquid phases for use in electrochemical devices.
[0086] In a first embodiment, a semisolid electrode is described that includes a liquid metal phase in equilibrium with a solid phase. For example, a mixture of Na and K is described that readily alloys at room temperature to produce a two-phase (liquid-solid) system (see, for example, Figure 5C ), allowing the mechanical properties of metal electrodes to be further tuned by adjusting the amount of liquid in equilibrium at room temperature. Thus, increasing the amount of liquid present can reduce the deformation resistance of electroactive metals and increase the critical current density.
[0087] In a second embodiment, an energy-dense solid electrode with a small amount of interfacial metallic liquid is described. For example, based on the binary Li-Na and Li-K phase diagrams (see, for example, Figure 5A and Figure 5B ) is expected to show a small amount of solubility for Li. A Li-rich anode with a small amount of liquid Na-K alloy is placed at the interface between Li and the electrolyte. Both the high energy density of lithium and the softness of sodium and potassium can be exploited, because such a battery cell can be energy-dense and exhibit a reduced likelihood of short circuiting as the liquid Na-K layer alleviates the significant stress accumulation at the Li electrolyte interface by transporting Li away from the electrolyte surface. The introduction of Na and K to the Li-rich alloy should not excessively hinder the diffusion of lithium working ions. That is, lithium can be significantly dissolved in the Na-K synthesis used. In addition, the introduction of Na-K should promote the formation of a mechanically soft and deformable interface between Li metal and the solid electrolyte, which can use sodium or potassium to preferentially wet the electrolyte instead of lithium.
[0088] Several symmetrical cell systems were investigated under galvanostatic conditions. See Table 1 for examples. Three unique solid electrolytes with similar microstructure, surface finish, hardness, fracture toughness, and ionic conductivity were used as ionic conductors for Li, Na, and K (Li 6.6 La 3 Zr 1.6 Ta 0.4 O 12 (LLZTO), Na-β”-Al 2 O 3 (NBA), K-β”-Al 2 O 3 (KBA)) to isolate the effect of the mechanical properties of electroactive metals on the critical current density. 6.6 La 3 Zr 1.6 Ta 0.4 O 12 (LLZTO), Na-β”-Al 2 O 3(NBA), K-β”-Al 2 O 3 The ionic conductivities of (KBA) were measured via EIS to be 1.03±0.2 mS / cm, 1.72±0.56 mS / cm, and 1.07±0.3 mS / cm, respectively. 6.6 La 3 Zr 1.6 Ta 0.4 O 12 、Na-β”-Al 2 O 3 and K-β”-Al 2 O 3 The fracture toughness was measured by Vickers microindentation test to be 2.51±0.64MPa.m 0.5 、2.93±0.70MPa.m 0.5 and 3.06±0.90MPa.m 0.5 .
[0089] Table 1
[0090]
[0091] Table 1 summarizes the evaluation and comparison of the symmetric cell tests detailed below. 95K5Na and 90K10Na represent binary alloy electrodes of 95 mol% and 90 mol% K, respectively, while NaK(e)-Li represents a Li electrode with a thin coating (~5 μm) of Na-K alloy under eutectic synthesis (68 mol% K, 32 mol% Na). CCD represents critical current density. "Average area correction factor" represents the ratio between the initially assumed electrode area and the true contact area between the electrode and the solid electrolyte as determined by post hoc image analysis.
[0092] Through highly polished (1 micron grain size) polycrystalline solid electrolyte (Li 6.6 La 3 Zr 1.6 Ta 0.4 O 12 (LLZTO), Na-β”-Al 2 O 3 (NBA), K-β”-Al 2 O 3 (KBA) creates an alkali metal flux (Li, Na, and K) from a metal counter electrode (CE) to a metal working electrode for alkali metal electrodeposition. Galvanostatic experiments were performed to obtain a 3 mAh cm -2 、1.5mAh·cm -2 and 0.25mAh·cm -2The critical current density is measured at a fixed area capacity of 3 mAh / cm 2 The upper limit of the area capacity is assumed to be that of the actual metal anode battery using similar electrode area capacities. 1.5 mAh / cm 2 and 0.25mAh / cm 2 The minimum current density applied was 0.25 mA.cm -2 , which corresponds to 3 mAh / cm 2 ~1C / 12C charge rate of the cell. In contrast, real batteries will be chargeable at rates of at least 1C to 2C. These tests produced cell voltages of <1000mV, which are sufficient to propagate uniform nm-scale surface defects (the applied 1V driving force is balanced by a compressive stress of 7.5GPa at the electrodeposition site).
[0093] Two distinct cell failure modes were identified in the assembled cells. The first mode, short circuiting at a critical current density, was identified in the majority (39 / 42) of cells tested. The second mode, delamination of the working electrode (resulting in excessive cell impedance, prematurely ending the experiment) was uncommon and occurred primarily at low voltages or high areal capacities (<1.5 mAh / cm 2 ) in a pure Li / LLZTO / Li symmetric battery cell (classification 1). The critical current density corresponding to the first failure mode is measured at 9A to 9D and are summarized in Table 1. Each classified electrochemical cell exhibits a unique critical current density range. The main parameter that varies between each cell is the deformation resistance of the electrodeposited metal, quantified by the yield stress in the case of the all-solid approach, or by the liquid fraction in the case of the semi-solid electrode approach.
[0094] When comparing the performance of cells containing all-solid electrodes, it can be observed that the average critical current density increases from 0.50 mA / cm2 to 0.60 mA / cm3 as the yield stress decreases (Li-Na-K). 2 (Li) increased to 2.52 mA / cm 2 (K) (see, for example, Table 1). Such an increase in critical current density can be attributed to the relative ease of squeezing of the lower yield stress metal, thereby relieving the pressure that builds up inside surface defects.
[0095] With respect to the semi-solid electrode approach (Classification 4 and Classification 5), it was observed that as the K electrode was alloyed with increasing amounts of Na metal from 5 mol% to 10 mol%, increasing the amount of binary Na-K liquid in equilibrium with the solid alloy at room temperature from about 25% to 75%, the critical current was observed to be again around 1.5 mAh / cm 2 The true area capacity (taking into account the increase in electrode electrolyte contact area after cycling) is from 5.2 mA / cm 2 (95K-5Na) increased to 14.2 mA / cm on average 2 (90K-10Na). To put these numbers into context, the current state-of-the-art solid-state lithium symmetric battery cell has a capacity of 0.25 mAh / cm 2 The area capacity shows ~1mA / cm 2 , corresponding to a >10x improvement in critical current density and a >5x improvement in areal capacity for this particular embodiment of the invention.
[0096] In another approach, a small amount (<50 μm thick) of eutectic Na-K alloy introduced to the interface between Li metal and LLZTO electrolyte was shown to increase the critical current from 0.50 mA / cm 2 (Li) increased to an average of 1.21 mA / cm 2 (Li-NaK). It is interesting to observe that such a “self-healing” approach (class 6) exhibits higher critical current density (based on real electrode area from 0.25 mAh / cm2) independent of the applied pressure over all the area capacities considered, compared to conventional all solid Li (class 1). 2 To 3.5mAh / cm 2 ). At 3mAh / cm 2 The lack of data points for Class 1 cells around the areal capacity region is due to premature termination of the experiment due to prolonged stripping and plating (>1.5 mAh / cm 2 ) during the period of excessive cell impedance, preventing access to higher areal capacities of the cell as constructed. Such observations are consistent with a delamination mechanism occurring simultaneously with the formation of "voids" at the electrode electrolyte interface, which is the second failure mode identified above. The results suggest a "self-healing" approach to circumvent such limitations, likely due to the liquid Na-K phase naturally "filling" any voids that may form, while providing solubility for the working Li ions, thus allowing the interface to "self-heal".
[0097] When considering the results for the all-solid electrodes, the increase in critical current density for the Na cell and K cell relative to the Li cell may be due to different reaction products at the electrode electrolyte interface, which promotes interface stability. However, when considering the results of the semi-solid electrode method using a K-rich Na-K alloy with small synthetic changes on the KBA electrolyte, any chemical reaction products at the electrode electrolyte interface between these cells (classes 4 and 5) should not show significant changes. However, an increase in critical current density was observed when the amount of liquid phase present was increased by increasing the degree of Na alloying. Without being bound by any particular scientific explanation, this result supports the hypothesis that interface stability, i.e., mitigation of dendrites, is improved when the interfacial electrode material is better able to yield mechanically.
[0098] Typical galvanostatic experiments on a NaK(e)-Li / LLZTO / NaK(e)-Li cell (class 6) FIG. 10A to FIG. 10D As assembled, the battery cell exhibits an EIS spectrum with both resistive and capacitive components. The high frequency resistive impedance (~100Ω) corresponds to a capacitance as measured (1 mS / cm 2 -2mS / cm 2 ), while the presence of capacitive impedance indicates the presence of an interfacial transport barrier. These observations indicate that the cell has not experienced a short circuit, which should be indicated by a purely resistive impedance with a low magnitude.
[0099] In the NaK(e)-Li / LLZTO / NaK(e)-Li typical cell, the time elapsed until short circuit was observed at approximately 60 hours corresponds to the beginning of the 7th cycle and a cumulative lithium plating thickness of ∼360 μm. Fig. 10A and Fig. 10C Both show voltage time traces and current density time traces. The sudden drop to zero voltage at ~0 h corresponds to the growth of the crack completely filled by the electrolyte disk. EIS spectrum measurement results ( Fig. 10B and Fig. 10D ) corresponds to a decrease in high frequency resistive impedance and the disappearance of the capacitive component in the EIS spectrum, consistent with the formation of a metal short through the electrolyte. Similar features were observed during electrochemical cycling tests on a typical symmetric 95K5Na / KBA / 95K5Na battery cell, such as FIG. 11A to FIG. 11D As described in .
[0100] After the electronic short circuit occurred, the cell was subsequently disassembled and imaged under an optical microscope to examine the electrolyte electrode interface on both sides of the solid electrolyte. In the typical NaK(e)-Li / LLZTO / NaK(e)-Li cell, the metallic Li electrode is confined within the boundaries of the solid electrolyte disk, ruling out the possibility of electronic short circuiting via Li metal on either side of the electrolyte through contact on both sides. This supports the following statement inferred from the EIS measurements that the sudden drop in the cell impedance is due to electronic short circuiting caused by metal penetration into the solid electrolyte.
[0101] During cell assembly, pre-cycle heat treatment, and cycling, the contact area between the Li metal electrode and the LLZTO electrolyte evolves over time due to squeezing or non-uniform Li stripping and plating. This will reduce the true current density relative to the apparent current density based on the initial area. Therefore, a “post hoc area correction” is performed to determine a more accurate value for the critical current density at which shorting is observed. For cell classes 1 and 6, this area was observed to remain relatively constant, corresponding to no increase from 3 mAh cm -2 For cell categories 2 to 5, it was observed that the area increased by a factor of 2 to 3 between cells, corresponding to an increase in the area capacity from the initial 3 mAh cm -2 Reduced to 1 to 1.5 mAh cm -2 .
[0102] Higher areal capacities (~3 mAh cm) were observed during stripping and plating in a “self-healing” electrode approach using an interfacial Na-K alloy with Li metal. -2 ), rather than pure Li itself (~1.5 mAh cm -2 ). The areal capacity limitation of pure Li metal cells (category 1) is attributed to the large impedance rise in the late stages of prolonged unidirectional stripping / plating, where galvanostatic deposition at the required current density becomes unsustainable. 2 Down to 1.5mAh / cm 2 Such an impedance rise was observed at the 45 hour mark of cycle 4 (~100 micron cumulative Li thickness passed). The impedance rise was indicated by a sharp increase in polarization from <200 mV to >750 mV under galvanostatic conditions, indicating a large increase in cell impedance.
[0103] In contrast, when cycling cells that include a “self-healing” electrode approach (Class 6, FIG. 10A to FIG. 10D ), no increase in cell impedance was observed, with polarization remaining below 300 mV for ~60 hours, corresponding to a cell current of 1.5 mA / cm 23.0mAh / cm 2 The increase can be attributed to the “self-healing” behavior of any Li voids formed during stripping by thermodynamic preferential wetting of the Na-K alloy to the LLZTO electrolyte wafer relative to solid Li. In the cell studied, the amount of Na-K alloy applied (5 μL) corresponds to 1.5% Na-K per electrode area (~360 μm). 2 ) of the liquid thickness of ~60 microns. However, due to the applied stacking pressure (1.5 MPa in most cases), the actual liquid layer thickness inside the battery cell is expected to be much lower than this amount, and the excess liquid accumulates at the edges of the electrodes. Overall, it was found that the performance of the "self-healing" electrode battery cell does not depend on the applied stacking pressure, nor on the volume of the applied eutectic Na-K alloy.
[0104] Overall, these observations suggest that when considering the mechanisms of solid-state battery cell shorting, the risk of electroactive metal penetration (i.e., during charging of lithium metal batteries) can be reduced by utilizing metal anodes with mechanical properties that promote yielding at the electrode electrolyte interface. This can be accomplished by the methods outlined below: by using semi-solid electrodes composed of solid and liquid or by utilizing a low yield stress interface between the electroactive metal and the electrolyte. These strategies may be attractive in the search for high energy density all-solid-state batteries.
[0105] Example 2
[0106] The following examples describe materials and methods for making and evaluating electroactive materials and electrochemical devices.
[0107] Electrolyte collection: Polycrystalline LLZTO, NBA and KBA samples were obtained from commercial suppliers (LLZTO: Toshima Manufacturing Co., Japan, NBA / KBA: Ionotec, UK).
[0108] X-ray diffraction: The crystal structure, single crystallinity and phase purity of the electrolyte were determined via X-ray diffraction (XRD).
[0109] Conductivity measurements: EIS was performed on symmetric cells including Au blocking electrodes on either side of the solid electrolyte disk using a BioLogic VMP-3 cell test system. Au thin films (~100 nm) were deposited onto the electrolyte via magnetron sputtering. Values of ionic conductivity (and dielectric capacitance) were extrapolated from circuit fits of the resulting EIS spectra.
[0110] Sample surface preparation and characterization: The electrolyte samples were polished using an EcoMetTM250Pro grinder-polisher (Buehler, Lake Bluff, IL, USA). The samples were first polished using 600 grit SiC grinding paper to reveal two faces. The two largest parallel surfaces were polished to a final grit size of 1 μm using successively finer grit sizes of diamond paste to obtain a mirror finish. To obtain finely polished faces, the samples were then polished sequentially for 25 minutes and 10 minutes using an aqueous diamond suspension of 9 μm and 1 μm particle sizes, respectively. The samples were then ultrasonicated in deionized water for 5 minutes to remove polishing debris.
[0111] Scanning electron microscopy (SEM) images are almost featureless for polished LLZTO, whereas for NBA and KBA micrographs, zirconium oxide (ZrO) added by the supplier to increase fracture toughness is observed. 2 ) distribution of particles. Thermal etching of the polished solid electrolyte (at 500°C, 1000°C, 1000°C for 1 hour for LLZTO, NBA and KBA, respectively) shows grain sizes ranging from 5 microns to 10 microns for all three solid electrolytes. SEM imaging of the samples was performed using a Merlin GEMINI II SEM (Carl Zeiss microscope, Jena, Germany) operating at 15 kV accelerating potential and 215 pA current. All samples were prepared in an argon-filled glove box (oxygen and water levels below 0.1 ppm).
[0112] Stylus profilometry was performed to quantify the roughness of the polished samples. Over a scan length of 5 mm, the polished surface was observed to have sub-micrometer surface defects consistently for all solid electrolyte samples (by independent measurements performed on three samples per electrolyte classification).
[0113] Fracture toughness measurements were performed via the Vickers microindentation method: Several indentations were placed under a load sufficient to produce cracks radiating from the corners using a Vickers microindenter (LECO LM248 AT microindentation hardness testing system). These cracks have a semicircular crack front extending perpendicular to the surface into the crystal. A range of crack lengths were generated and evaluated by SEM by varying the applied load. Indentation loads of 20N, 10N, and 5N were used to determine the fracture toughness in this study. Crack lengths were measured by optical microscopy.
[0114] Two independent methods (Anstis and Evans) for evaluating fracture toughness from indentation data are included. The Anstis method uses the value of the Young's modulus of the indented material, while the Evans method is modulus independent. 2 O 3Previous measurements of Naβ”-Al 2 O 3 and Kβ”-Al 2 O 3 The lower and upper limits of the Young's modulus of 210 GPa and 300 GPa are given in Table 1. These values do significantly affect the fracture toughness calculated within the Anstis method. Overall, the data suggest that the fracture toughness of the solid electrolytes considered in this study is between 2 MPa·m 1 / 2 To 3MPa·m 1 / 2 range, and have a similar magnitude of variance between samples (3 indentations on three independent samples for each electrolyte classification).
[0115] Electrochemical cell assembly and X-ray photoelectron spectroscopy (XPS) analysis: Prior to assembly, each polished solid electrolyte disk was wet polished and immediately heat treated in an inert atmosphere to remove any surface layer on the electrolyte that could cause high interfacial impedance. The LLZTO pellets were heat treated at 500 °C for 3 h to remove LiCO 3 NBA and KBA pellets were heat treated at 1000°C for 1 hour to remove any chemically adsorbed moisture.
[0116] Independent XPS elemental measurements indicate that a negligible amount of contamination layer is present on the surface of the solid electrolyte after heat treatment. XPS analysis was performed using an electron spectrometer (PHI Versaprobe) II XPS (Ultek-PHI, Japan). A monochromatic Al K-α X-ray source was operated at 50 W with a spot size of 200 μm. The base pressure during the analysis exceeded 2.0 × 10 -8 The main reactive contaminant found with alkali metals is trace amounts of oxygen, which reacts with the metal over time (even in an inert Ar atmosphere) to form its corresponding oxide, producing a visible film.
[0117] By placing a flat lithium foil disk (0.375 inch diameter, 0.1 mm thickness, 50 mAh cm -2 , ~10 μL Li) was placed between the LLZTO solid electrolyte and the stainless steel current collectors on either side to complete the battery cell assembly. Therefore, the initial area of the lithium electrode is equal to 0.80 cm 2 (1.27cm with half-inch diameter electrolyte surface 2Prior to electrochemical cycling, the cells were heated to 170 °C for 3 hours under an applied stacking pressure of 1.5 MPa in a custom spring-loaded fixture. Subsequently, the cells were slowly cooled to room temperature. The study showed that this process significantly reduced the interfacial impedance of the cells, allowing the application of high current densities (up to 6 mA cm -2 ), while keeping the cell potential well below 1.0 V. When assembling the "low voltage" cell, the spring is minimally tightened using an assumed upper strain limit of 2% based on visual inspection. This upper strain limit corresponds to a 75 kPa load, assuming the spring has linear elasticity.
[0118] The molten Na, K or premixed Na-K alloy was pipetted into its respective β"-Al 2 O 3 The cells of classes 2 to 4 were assembled by flattening the droplets on the solid electrolyte by means of a steel current collector under an applied stacking pressure of 1.5 MPa, which was maintained during electrochemical cycling. Thus, the initial area of the lithium electrode was equal to the surface area of the exposed current collector face, which was 0.40 cm 2 (1.27cm with half-inch diameter electrolyte surface 2 area). It is not necessary to pre-cycle heat treatment to produce a low impedance battery cell for testing.
[0119] The eutectic Na-K alloy (~5 or 10 μL of 77 mol% K, corresponding to ~50 μm thick NaK alloy) was added to a perforated Li disk (0.375 in. diameter, 0.1 mm thickness, 50 mAh cm -2 , ~10 μL Li) on one side, and the battery cells of category 6 were assembled in a manner similar to those of category 1. Then, one side of the Li disk with the added Na-K alloy was placed in contact with the LLZTO solid electrolyte wafer.
[0120] Electrochemical Cycling: Galvanostatic experiments were performed on the samples using a BioLogic VMP-3 cell test system. A total of ~40 cells prepared in the above manner were studied at room temperature (22 °C) under two different current density profiles. Li / LLZTO / Li and NaK(e)-Li / LLZTO / NaK(e)-Li were subjected to constant current cycling at 0 to 3 mA cm -2 0.125 mA·cm -2 The increments were 0.25, 1.5 or 3 mAh cm per cycle. -2The areal capacities of the Na / NBA / Na, K / KBA / K, 95K5Na / KBA / 95K5Na, and 90K10Na / KBA / 90K10Na cells were subjected to galvanostatic cycling at 0 to 40 mA cm -2 At 0.5 mA cm -2 The increment is 3 mAh cm per cycle. -2 The areal capacity of the solid electrolyte was galvanostatically cycled with 30 μm and 45 μm thickness for Na and K, respectively. The current density and areal capacity are defined relative to the initial contact area between the alkali metal and the solid electrolyte.
[0121] Between the galvanostatic cycles, EIS spectra were also collected at set intervals (between each cycle of cells i) and vi), and between every 5 cycles of cells ii) to iv) to monitor the state of the electrode electrolyte interface by examining the evolution of the resistance and capacitance components of the cell over time. Throughout the entire process, the device was contained in an argon-filled glove box with oxygen and water contents below 0.1 ppm and 1 ppm, respectively.
[0122] Post-mortem characterization: Symmetrical cells disassembled after cycling were examined using optical microscopy. After completion of electrochemical cycling, in situ microscopy was performed using a Leica DMS300 (Leica, Germany) digital microscope.
[0123]
[00136] Sessile Droplet Test: The surface energies of lithium, sodium, and potassium in contact with various solid electrolytes were evaluated via the sessile droplet test. A substrate disk of interest (prepared by polishing as described above) was placed on a hot plate. The temperature was adjusted to be approximately 20°C above the melting point of the metal alloy to be tested. 10 microliters of the alloy sample was taken from a pipette and deposited onto the center of the substrate disk. The system was equilibrated at temperature for 5 minutes while the camera was positioned horizontally facing the droplet and vertically aligned to the top surface of the substrate disk. The substrate and droplet were covered with a small dome of magnesium oxide ceramic to isolate the test area. For each measurement, the hot plate was increased by an increment of 20°C, the temperature of the droplet was stabilized for 4 minutes after the hot plate indicated that it had reached the desired temperature, and the image was captured. This process was repeated for a total of eight data points for each sample.
[0124] Example 3
[0125] The following examples describe three binary Li alloy systems Li-Na ( Figure 5A )、K-Li( Figure 5B ) and K-Na( Figure 5C ) Calculated synthesis temperature phase diagram at 1 atm.
[0126] The phase separation tendency between Li and K is stronger than that between Li and Na, probably due to the large atomic size mismatch between Li and K. At ambient pressure and below about 450 K, Li metal coexists with nearly pure solid Na below ∼360 K, as shown in Figure 5A or coexist with almost pure solid K below ~340 K, as shown in Figure 5B Below these temperatures, which represent practical use temperatures for many battery applications, the Li-Na or Li-K anode consists of a harder Li and a softer Na or K phase. The anode composition traverses a Figure 5A and Figure 5B phase region in; for example, if the working ion is Li + , then in the discharged state, the anode will be depleted of Li and therefore softer. Such a composite material could have mechanical behavior that allows higher current densities in battery cells using lithium-conducting solid electrolytes.
[0127] As discussed previously, softer composite materials exist if a solid Li phase coexists with a small amount of liquid. Such a type of anode is similar to dental amalgam. Figure 5A and Figure 5B In , such coexistence occurs between the solidus temperatures of 450 K and ~360 K, and between the solidus temperatures of 450 K and ~340 K, respectively. Figure 5C It is shown that compared with the cases of Li-Na and Li-K, there is no liquid miscibility gap between Na and K, but a deep eutectic extending to ∼260 K. In the ternary system, Li coexists with a liquid rich in Na and K, and such two-phase coexistence can be designed to fall within the operating temperature range of interest for electric vehicle applications.
[0128] Example 4
[0129] The following example describes the calculated pressure-temperature phase diagram of Li ( Figure 6 ).
[0130] An important variable to consider in the state of matter is pressure, because during electrodeposition, the pressure generated, especially at small-scale features such as cracks, holes and grain boundaries, can be very high. The pressure-temperature phase diagrams of pure metals Li, Na and K are known. "Simple" alkali metals show complex behavior under pressure. All three elements crystallize in a bcc structure at ambient pressure and transform into a fcc structure when pressure increases. They also show unusual behavior at certain pressures, i.e., transform from a solid to a liquid as pressure increases within a certain range. A possible explanation is that quantum effects begin to play a leading role under high compression. Another interesting phenomenon is that, although Na has a lower melting point than Li at ambient pressure, it has a much higher melting point (~1000K under ~30GPa) under high pressure.
[0131] Density functional theory (DFT) calculations were used to calculate the pressure-temperature phase diagram of Li along with a simple Debye model for estimating the free energy, as Figure 6 The low-pressure region of the phase diagram agrees well with known values, but in the high-pressure region, the phase boundary between fcc and cI16 (space group I-43d) phases is correctly predicted only near 0 K. The Debye model, which is usually used successfully for metals at ambient pressure, fails to describe solids at high pressures. The unusual thermodynamic behavior of Li at high pressures is also exemplified by its phonon instability that occurs under pressure.
[0132] Although the understanding of the thermodynamics in alloy systems containing Li, Na, and K at non-ambient pressures is still lacking, if the atomic size mismatch is indeed the main factor determining alloying, it is hypothesized that pressure will improve the alloying ability between Li and Na / K. Since Na and K have much lower bulk moduli than Li, their compression under pressure will reduce the atomic size mismatch between them and Li.
[0133] Example 5
[0134] The following examples describe the lithium deposition process and the effect of external stress on dendrite growth.
[0135] In order to understand the lithium deposition process and the effect of external stress on dendrite growth, phase field simulation of the electrodeposition process coupled with mechanics is used to understand the mechanical response at the solid electrode electrolyte interface. The morphological evolution of the metal electrode during electrodeposition is studied using phase field simulation. The simulation requires real-time metal electrodeposition with time scales and length scales comparable to experimental observations. Incorporating electrochemical mechanical driving forces into the framework enables precise determination of the effects of intrinsic material parameters and externally applied forces (such as stacking pressure) on the inhibition of dendrite growth. In addition, phase field simulations provide a treatment of the basic physics of dendrite growth.
[0136] Phase-field simulation of lithium metal deposition with liquid electrolytes FIG. 7A to FIG. 7D Long needle-like dendrites are formed at relatively large current densities. The formation of dendrites leads to the accumulation of lithium ions around the dendrite tip, which further promotes the growth of the dendrite tip region. In contrast, in the recessed regions, lithium ions are expelled by the growth of the dendrite tip, resulting in much smaller interface velocities in these regions. The spatially resolved electric field distribution is also shown in Fig.7D , which shows that the electric field vector points toward the dendrite tip, causing further convection of lithium ions to the tip.
[0137] Mechanical stress at the interface is an effective way to suppress dendrites with solid electrolytes. The mechanical properties of the electrode and electrolyte as well as the effect of the applied stacking pressure were evaluated by employing a mechanical force balance equation within a phase-field model. The kinetic reaction rate is directly related to the change in chemical potential due to the presence of local stress. Compressive stress on dendrites leads to lower kinetic rates, which is expected to suppress the growth of dendrites.
[0138] As a result of the internal stress caused by the formation of dendrites with solid electrolytes FIG. 8A to FIG. 8C In the absence of external stress, large compressive stresses are generated in the dendrite region, while tensile stresses are generated in the solid electrolyte. This suggests that the large capacity expansion during electrodeposition tends to be offset by the deformation of the solid electrolyte. In particular, it is interesting to note that the roots or junctions of the dendrites have higher stresses, suggesting that these regions are more susceptible to "flaking" during cycling, leading to a decrease in Coulombic efficiency. In addition, due to the generated internal stress, the growth of dendrites is inhibited (positive inhibition factor), while the growth of recesses is favored (negative inhibition factor), resulting in the phenomenon of "intrinsic inhibition" of dendrite growth.
[0139] Although several embodiments of the present invention have been described and illustrated herein, a person of ordinary skill in the art will readily conceive of various other methods and / or structures for performing the functions and / or obtaining the results and / or one or more of the advantages described herein, and each of such changes and / or modifications is considered to be within the scope of the present invention. More generally, it will be readily understood by those skilled in the art that all parameters, dimensions, materials, and configurations described herein are intended to be exemplary, and that the actual parameters, dimensions, materials, and / or configurations will depend on the specific application or applications in which the teachings of the present invention are used. Those skilled in the art will recognize, or will be able to determine many equivalents of the specific embodiments of the present invention described herein using only routine experiments. Therefore, it should be understood that the foregoing embodiments are presented only as examples, and within the scope of the appended claims and their equivalents, the present invention may be practiced in other ways, rather than as specifically described and claimed. The present invention relates to each individual feature, system, article, material, and / or method described herein. In addition, if such features, systems, articles, materials, and / or methods are consistent with each other, any combination of two or more such features, systems, articles, materials, and / or methods is included within the scope of the present invention.
[0140] Unless expressly indicated to the contrary, the indefinite articles "a" and "an" as used herein in the specification and claims should be understood to mean "at least one".
[0141] As used herein, in the specification and claims, the phrase "and / or" should be understood to refer to "either or both" of the elements so combined, i.e., elements present in combination in some cases and separately in other cases. Unless expressly indicated to the contrary, other elements may optionally be present in addition to the elements specifically identified by the "and / or" clause, whether or not related to those specifically identified. Thus, as a non-limiting example, when used in conjunction with open language such as "comprising," a reference to "A and / or B" may: refer to A without B (optionally including elements in addition to B) in one embodiment; refer to B without A (optionally including elements in addition to A) in another embodiment; refer to both A and B (optionally including other elements) in yet another embodiment; and so on.
[0142] As used herein in this specification and claims, "or" should be understood to have the same meaning as "and / or" as defined above. For example, when the items in the list are separated, "or" or "and / or" should be interpreted as being inclusive, i.e., including at least one, but also including more than one of many or a series of elements, and optionally, other unlisted items. Only terms that clearly indicate the opposite, such as "only one of" or "exactly one of" or, when used in the claims, "consisting of..." will refer to including exactly one element in many or a series of elements. Usually, when there is an exclusive term in front, such as "any one", "one of", "only one of" or "exactly one of", the term "or" as used herein should only be interpreted as indicating an exclusive alternative (i.e., "one or the other, not two"). When used in the claims, "substantially including" should have its ordinary meaning as used in the field of patent law.
[0143] As used herein in this specification and claims, the phrase "at least one" with respect to a list of one or more elements should be understood to refer to at least one element selected from any one or more of the elements in the list of elements, but not necessarily including at least one of each and every element specifically listed in the list of elements, and not excluding any combination of elements in the list of elements. This definition also allows that elements other than the elements specifically identified in the list of elements to which the phrase "at least one" refers may optionally exist, whether or not related to those specifically identified elements. Thus, as a non-limiting example, "at least one of A and B" (or equivalently, "at least one of A or B", or equivalently, "at least one of A and / or B") may: in one embodiment, refer to at least one, optionally including more than one A without B (and optionally including elements other than B); in another embodiment, refer to at least one, optionally including more than one B without A (and optionally including elements other than A); in yet another embodiment, refer to at least one, optionally including more than one A, and at least one, optionally including more than one B (and optionally including other elements); and so on.
[0144] In the claims, and throughout the specification above, all transitional phrases such as "comprises," "comprising," "carrying," "having," "containing," "involving," "having," and the like shall be construed as open ended, i.e., meaning including, but not limited to. Only the transitional phrases "consisting of" and "consisting essentially of" shall be closed or semi-closed transitional phrases, respectively, as set forth in Section 2111.03 of the U.S. Patent Office Manual of Patent Examining Procedures.
Claims
1. An electrochemical device comprising: a solid electrode comprising an alloy, wherein the alloy comprises at least one alkali metal; and The alloy comprising a liquid phase at a temperature between or equal to 15°C and 30°C is disposed on the solid electrode at an interface between the solid electrode and an electrolyte.
2. The electrochemical device according to claim 1, wherein: The alloy includes at least two alkali metals.
3. The electrochemical device according to any one of claims 1 to 2, wherein: The alloy includes lithium (Li), sodium (Na) and / or potassium (K).
4. The electrochemical device according to any one of claims 1 to 2, wherein: The atomic ratio of the solid phase to the liquid phase in the alloy is at least 50%.
5. The electrochemical device according to any one of claims 1 to 2, wherein: The atomic ratio of the solid phase to the liquid phase in the alloy is at least 80%.
6. The electrochemical device according to any one of claims 1 to 2, wherein: The liquid phase includes Li, Na and / or K.
7. The electrochemical device according to any one of claims 1 to 2, wherein: The solid phase in the alloy includes Li, Na and / or K.
8. The electrochemical device according to any one of claims 1 to 2, wherein: The solid phase in the alloy includes Li in an amount greater than or equal to 50 mol % based on total moles in the solid phase.
9. The electrochemical device according to any one of claims 1 to 2, wherein: The solid phase in the alloy includes Li in an amount greater than or equal to 90 mol % based on total moles in the solid phase.
10. The electrochemical device according to any one of claims 1 to 2, wherein: The solid phase in the alloy includes Li, and the liquid phase includes Li, and the solid phase includes a greater mol % of Li than the liquid phase based on the total moles in the alloy.
11. The electrochemical device according to any one of claims 1 to 2, wherein: The solid phase in the alloy includes Na, and the liquid phase includes Na, and the solid phase includes a greater mol % of Na than the liquid phase based on the total moles in the alloy.
12. The electrochemical device according to any one of claims 1 to 2, wherein: The solid phase in the alloy includes K, and the liquid phase includes K, and the solid phase includes a greater mol % of K than the liquid phase based on the total moles in the alloy.
13. The electrochemical device according to any one of claims 1 to 2, wherein: The electrochemical device is a battery.
14. An electroactive material comprising: A solid electrode comprising an alloy comprising at least two alkali metals; as well as The alloy includes a liquid phase at a temperature between or equal to 15°C and 30°C, disposed at an interface of the solid electrode.
15. The electroactive material according to claim 14, wherein The at least two alkali metals are selected from the group consisting of Li, Na and K.
16. The electroactive material according to any one of claims 14 to 15, wherein The atomic ratio of the solid phase to the liquid phase in the alloy is at least 50%.
17. A method of operating an electrochemical device, the method comprising: Charging and / or discharging an electrochemical device at a first temperature, wherein the electrochemical device comprises: a solid electrode comprising an alloy, wherein the alloy comprises at least one alkali metal; and The alloy comprising a liquid phase at a temperature between or equal to 15°C and 30°C is disposed on the solid electrode at an interface between the solid electrode and an electrolyte.
18. The method according to claim 17, wherein: The alloy includes at least two alkali metals.
19. The method according to claim 18, wherein: The at least two alkali metals are selected from the group consisting of Li, Na and K.
20. The method according to any one of claims 17 to 18, wherein: The atomic ratio of the solid phase to the liquid phase in the alloy is at least 50%.