A test method for the cycle endurance of valve-controlled lead-acid batteries for parking air conditioners
Through the test of lead-acid batteries for parking air conditioners, the cyclic durability test method based on operating conditions, including weighing, reserve capacity measurement and cycle charge and discharge testing, solves the problem that the existing technology cannot accurately evaluate lead batteries for parking air conditioners. The problem of life span enables accurate screening and performance evaluation of batteries under different working conditions, significantly improving the accuracy of test results and battery cycle durability.
Patent Information
- Application Number
- CN202111417627.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-26
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-11-26
AI Technical Summary
Existing battery cycle testing methods cannot accurately evaluate the life of lead-acid batteries used in parking air conditioners, especially the performance under different vehicle operating conditions.
Using a testing method based on operating conditions, through weighing, reserve capacity measurement, cycle charge and discharge testing and low-temperature starting capability evaluation, batteries that meet the standards are screened out, including 30 times of undercharging, 50 times of overcharging and 100 times of deep discharge cycles Test to evaluate the capacity fading rate and mass loss rate of the battery respectively to ensure the durability of the battery under different working conditions.
By accurately evaluating the cycle durability of the battery under different working conditions, batteries suitable for different driving conditions are screened out, which significantly improves the accuracy of the test results and the cycle durability performance of the battery.
Smart Images

Figure CN114236411B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for testing the cycle durability of a battery, and in particular to a method for testing the cycle durability of a valve-controlled lead-acid battery for a parking air conditioner based on an operating condition. Background Art
[0002] Lead-acid batteries for parking air conditioners are suitable for heavy trucks, buses, RVs, etc. These vehicles operate all over the country, with both hot and humid climates in the south and cold and dry climates in the north. Compared with ordinary starting batteries for heavy trucks, buses, RVs, etc., lead-acid batteries for parking air conditioners also bear the electricity consumption of car air conditioners, refrigerators, televisions, water heaters, induction cookers, electric blankets, and audio-visual systems. These low-voltage DC power-consuming equipment have large power demand and high power consumption frequency during use, requiring the battery to not only have good cycle charge and discharge capabilities, but also require the battery to still have normal starting capabilities in a low charge state after multiple deep discharges. Since parking air conditioners have only been used in recent years, the existing test standards do not have specific test methods for lead-acid batteries for parking air conditioners, especially battery cycle test methods.
[0003] Usually, the battery cycle test is carried out under constant ambient temperature (e.g. 25°C), and the battery is charged to the upper limit of the battery's SOC (state of charge) at a constant current or voltage, and then discharged to the lower limit of the SOC at a constant current / power. In this way, the battery is repeatedly charged and discharged until the battery's available capacity / power reaches the set life end condition. Due to different vehicle driving conditions, the operating conditions of parking air conditioner batteries are different. The unified use of this existing method cannot accurately evaluate the life of lead-acid batteries for parking air conditioners. Summary of the invention
[0004] In order to overcome the drawbacks of the prior art, the present invention provides a test method for the cycle endurance of a valve-controlled lead-acid battery for a parking air conditioner based on operating conditions. The test method determines the cycle endurance of the battery according to the operating conditions of the lead-acid battery for the parking air conditioner, and the test method is more accurate.
[0005] The technical solution adopted by the present invention to solve its technical problem is:
[0006] A method for testing the cycle endurance of a lead-acid battery for a parking air conditioner, a method for testing the life of a lead-acid battery for a parking air conditioner according to a battery operating condition, the method comprising the following steps:
[0007] a. Battery weighing: The weight of the battery before the test begins is W0;
[0008] b. Reserve capacity: discharge to 10.5V at a constant current of 25A and record the discharge time RC0;
[0009] c. Capacity decay rate after 30 undercharges: The lead-acid battery is discharged at 25A constant current to 11.4V at 25℃, and then the current is limited to 0.3C at a constant voltage of 14.0V. 20 Charge A for 6 hours, repeat the cycle 30 times, and after the 30th charge, test the reserve capacity RC1 according to step b;
[0010] d. Result determination: RC1 / RC0≥80%, the screened batteries are qualified batteries.
[0011] The method for testing the cycle endurance of the lead-acid battery for parking air conditioner mentioned above, in step c, the method for testing the cycle endurance of multiple groups of batteries at the same time also includes: the capacity retention rate and mass loss rate after 50 overcharges: the battery is charged at 0.1C at 40°C. 20 A discharges for 5h, then limits the current to 0.3C at a constant voltage of 14.7V 20 A is charged for 8 hours and repeated 50 times. After the 50th charge, test the reserve capacity RC2 according to step b and weigh W1, and it meets RC2 / RC0≥90%, (W0-W1) / C 20 Batteries that meet the condition of ≤0.4g / Ah are qualified.
[0012] The test method for the cycle endurance of the lead-acid battery for parking air conditioner mentioned above, in step c, the method for testing the cycle endurance of multiple groups of batteries at the same time also includes: the capacity retention rate and low temperature starting ability after 100 deep discharge cycles: the battery is discharged at a constant current of 25A to 10.5V at 25°C, and then the current is limited to 0.3C at a constant voltage of 14.4V 20 A is charged for 6 hours. When the discharge time RC3≤0.5RC0, the cycle stops. When the discharge time RC3>0.5RC0, the cycle is repeated 100 times. After the 100th charge, low temperature start is performed with a starting current of 3C. 20 A, start time 30s, record 30s voltage, 30s voltage ≥ 9.0V, and RC3 / RC0 ≥ 50% is a qualified battery.
[0013] The test method for the cycle endurance of the lead-acid battery for the above-mentioned parking air conditioner, the battery operating conditions include: operating condition 1: the vehicle's cumulative driving time is less than 8h / day, the parking air conditioner is used for more than 10h / day, the battery discharge depth is large, the charging time is short, and the battery failure mode is insufficient charging; operating condition 2: the vehicle has been continuously driven for more than 14h / day, the parking air conditioner is used for less than 6h / day, the battery is in a continuous charging state, and the battery failure mode is overcharging resulting in a reduction in electrolyte; operating condition 3: the vehicle has been driven for a cumulative period of 8-14h / day, the parking air conditioner is used for 6-10h / day, the battery is in a relatively high charge state, and the battery failure mode is starting failure caused by softening of the positive active material.
[0014] In the above-mentioned method for testing the cycle endurance of the lead-acid battery for parking air conditioning, in the step c, the low-temperature starting temperature is -18±1°C.
[0015] The beneficial effects of the present invention are as follows: the present invention determines the battery operating conditions according to the vehicle driving conditions, and then determines the test method for the cycle endurance of the lead-acid battery for the parking air conditioner based on the battery operating conditions, and uses three different methods to test the endurance of multiple groups of batteries of the same model and specification at the same time, and sets standards that the test results need to meet, so that the cycle endurance test results screened out are more accurate, and the screened batteries are suitable for vehicles with different driving conditions and can exhibit excellent cycle endurance. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a graph showing the relationship between the cyclic discharge voltage and the number of discharges in the GB / T5008.1-2013 cyclic test method in comparative example 1;
[0017] Figure 2 A graph showing the relationship between discharge time and discharge times when the qualified batteries selected from Comparative Example 1 are subjected to undercharge and deep discharge cycle tests respectively;
[0018] Figure 3 This is a comparison chart of the changing relationship between the discharge time and the number of discharges when the qualified batteries are undercharged 30 times selected in Example 4 of the present invention and the changing relationship between the discharge time and the number of discharges under the same conditions in Comparative Example 1. DETAILED DESCRIPTION
[0019] The present invention will be further described below in conjunction with the embodiments.
[0020] The driving conditions of parked air-conditioned vehicles affect the operating conditions of the batteries, and the operating conditions of the batteries directly affect the cycle durability of the batteries. The failure mode of lead-acid batteries during vehicle driving is often related to the driving conditions of the vehicles.
[0021] During actual operation, the failure modes of the battery include: (1) Whether the battery voltage displayed on the dashboard when the vehicle is at rest is often lower than 12.5V: The voltage of a normal battery when the vehicle is at rest is above 12.9V. If the voltage is often lower than 12.5V, it means that the battery is undercharged. The corresponding vehicle driving conditions are that the vehicle has a cumulative driving time of less than 8h / day and the parking air conditioner is used for more than 10h / day.
[0022] (2) Does the battery need frequent water replenishment, especially in hot summer weather? Frequent water replenishment in hot summer weather is caused by the loss of battery electrolyte, especially when the temperature is high, the electrolyte loss is greater, indicating that the battery is in a state of frequent overcharging. The corresponding vehicle driving conditions are that the vehicle is continuously driven for more than 14 hours per day, and the parking air conditioner is used for less than 6 hours per day. The battery here is a flooded battery, which can be restored by water replenishment. However, after the electrolyte of the valve-regulated battery is lost, it cannot be replenished due to its special structure. Water loss is an irreversible damage to it. This type of vehicle driving condition causes the failure mode of the flooded battery, which will also cause the valve-regulated battery to produce the same failure mode.
[0023] (3) The battery has been used for more than 6 months, the air conditioning cooling time gradually becomes shorter, the car is difficult to start, and there is no improvement after repair and charging: The battery has been used for more than 6 months, and the air conditioning cooling time gradually becomes shorter, which means that the battery capacity has decreased. The factors that lead to the capacity reduction may be a. insufficient charging. In this case, the capacity can be partially or fully restored after repair and charging, and the air conditioning cooling time will become longer. This is repairable; b. The battery capacity has decayed. This is caused by frequent deep discharge leading to the softening of the positive electrode active material. This situation causes irreversible damage to the positive electrode active material. The battery capacity will not improve after repair and charging, and the car starting is getting worse and worse. The corresponding vehicle driving conditions are that the vehicle has traveled a total of 8-14 hours / day and the air conditioning is used 6-10 hours / day.
[0024] The battery operating conditions are confirmed according to the above vehicle driving conditions and battery failure forms. Operating condition 1: the vehicle's cumulative driving is less than 8h / day, the parking air conditioner is used for more than 10h / day, the battery discharge depth is large, the charging time is short, and the battery failure mode is insufficient charging; Operating condition 2: the vehicle has been running continuously for more than 14h / day, the parking air conditioner is used for less than 6h / day, the battery is in a continuous charging state, and the battery failure mode is overcharging resulting in a reduction in electrolyte; Operating condition 3: the vehicle has been running for 8-14h / day, the parking air conditioner is used for 6-10h / day, the battery is in a higher state of charge, and the battery failure mode is softening of the positive active material.
[0025] A test method for determining the cycle endurance of a valve-controlled lead-acid battery for a parking air conditioner according to the above battery operating conditions comprises the following steps:
[0026] a. Battery weighing: The weight of the battery before the test begins is W0;
[0027] b. Reserve capacity: discharge to 10.5V at a constant current of 25A and record the discharge time RC0;
[0028] c. Simultaneously test the cycle endurance of multiple groups of batteries of the same model using the following methods:
[0029] ① Capacity decay rate after 30 undercharge cycles: Lead-acid battery is discharged at 25A constant current to 11.4V at 25℃, and then current limited to 0.3C at 14.0V constant voltage 20 Charge A for 6 hours, repeat the cycle 30 times, and after the 30th charge, test the reserve capacity RC1 according to step b;
[0030] ② Capacity retention rate and quality loss rate after 50 overcharge cycles: The battery is charged at 40℃ and 0.1C 20 A discharges for 5h, then limits the current to 0.3C at a constant voltage of 14.7V 20 A is charged for 8 hours and repeated 50 times. After the 50th charge, the reserve capacity RC2 is tested according to step b and W1 is weighed;
[0031] ③Capacity retention rate and low temperature starting capability after 100 deep discharge cycles: The battery is discharged at 25A constant current to 10.5V at 25℃, and then the current is limited to 0.3C at a constant voltage of 14.4V 20 A is charged for 6 hours. When the discharge time RC3≤0.5RC0, the cycle stops. When the discharge time RC3>0.5RC0, the cycle is repeated 100 times. After the 100th charge, a low-temperature start is performed. The starting temperature is -18±1℃ and the starting current is 3C. 20 A, start time 30s, record 30s voltage;
[0032] d. Result judgment: The battery is qualified if the following three conditions are met:
[0033] (1) RC1 / RC0 ≥ 80%;
[0034] (2) RC2 / RC0 ≥ 90% and (W0-W1) / C 20 ≤0.4g / Ah;
[0035] (3) 30s voltage ≥ 9.0V, and RC3 / RC0 ≥ 50%.
[0036] When rapid screening of battery cycle endurance is required, only test method ① is performed, and batteries that meet the test results RC1 / RC0 ≥ 80% are qualified batteries; when more precise screening of batteries is required, different batteries from the same batch are tested using methods ① to ③ respectively, and batteries that meet the requirements of step d are screened as qualified batteries.
[0037] For the operating conditions where the battery is undercharged, when RC1 / RC0 ≥ 80%, the battery can recover its capacity and maintain its performance by reducing the depth of discharge and extending the charging time. When the capacity decay rate is lower than 80%, the large particles of lead sulfate accumulated during long-term undercharging of the battery are difficult to be reduced to metallic lead by reducing the depth of discharge and extending the charging time, making it difficult to recover the battery capacity or even causing rapid failure.
[0038] For the operating condition of battery overcharge, after testing, the charging amount is greater than 110%, which is overcharge, while the normal charging amount is about 105%. In addition to being used to convert active substances, the excess charging electricity is used for the decomposition and precipitation of the electrolyte, which reduces the volume of the electrolyte and loses the battery quality. When the mass loss rate after 50 overcharge cycles is ≤0.4g / Ah, it has little effect on the battery capacity, and the capacity retention rate of the battery after 50 overcharges is ≥90%, and the battery can still be used normally; when the mass loss rate after 50 overcharge cycles is greater than 0.4g / Ah, the reduction in the amount of electrolyte leads to a significant decrease in the pole group saturation and a decrease in the capacity retention rate. Long-term accumulation will cause irreversible damage to the battery.
[0039] In view of the operating condition of the softening of the positive active material of the battery, after the battery is repeatedly cycled 100 times, the battery is 20 When starting at -18℃ with A current, if the active material is in normal state, the voltage is ≥9.0V in 30s, and the vehicle can be started normally. When the positive active material softens, the RC3 of the battery is ≤0.5RC0, or the starting voltage is low in 30s, the battery is difficult to ignite, and there is a risk of vehicle breakdown.
[0040] Example 1
[0041] A test method for the cycle endurance of a valve-controlled lead-acid battery for a parking air conditioner. The test method for a 200Ah (rated reserve capacity 428min) battery is:
[0042] a. Battery weighing: The weight of the battery before the test is W0 = 64.13 kg;
[0043] b. Reserve capacity: Discharge to 10.5V at a constant current of 25A, and record the discharge time RC0 as 440min;
[0044] c. The lead-acid battery is discharged at a constant current of 25A to 11.4V at 25°C, and then charged at a constant voltage of 14.0V with a current limit of 60A for 6 hours, and the cycle is repeated 30 times. After the 30th charge, the reserve capacity RC1 is tested according to step b and is 374min;
[0045] d. Result determination: RC1 / RC0=374 / 440=85%≥80%. The test battery meets this condition and is a qualified battery.
[0046] Example 2
[0047] A test method for the cycle endurance of valve-controlled lead-acid batteries for parking air conditioners, two 200Ah (rated reserve capacity 428min) batteries are randomly selected, and the test method is:
[0048] a. Battery weighing: Before the test, the weight of the battery is W0 = 64.13 kg for battery 1# and W0 = 64.25 kg for battery 2#;
[0049] b. Reserve capacity: Discharge to 10.5V at a constant current of 25A, record the discharge time 1# battery RC0 = 440min, 2# battery RC0 = 438min;
[0050] c. Perform the following steps to test the cycle endurance of multiple battery groups at the same time:
[0051] At 25°C, the 1# lead-acid battery was discharged at a constant current of 25A to 11.4V, and then charged at a constant voltage of 14.0V with a current limit of 60A for 6h, and the cycle was repeated 30 times. After the 30th charge, the reserve capacity was tested according to step b. The RC1 of the 1# battery was 374min.
[0052] Battery 2# was discharged at 20A for 5h at 40℃, and then charged at a constant voltage of 14.7V with a current limit of 60A for 8h. This cycle was repeated 50 times. After the 50th charge, the reserve capacity was tested according to step b. The RC2 of battery 2# was 418min, and the weight W1 was 64.18kg.
[0053] d. Result determination:
[0054] (1) 1# battery RC1 / RC0=374 / 440=85%≥80%;
[0055] (2) 2# battery RC2 / RC0=418 / 438=95%≥90%;
[0056] (W0-W1) / C 20 =(64.25-64.18) / 200=0.35≤0.4g / Ah;
[0057] The tested batteries meet the requirements of both standards and are qualified batteries.
[0058] Example 3
[0059] A test method for the cycle endurance of valve-controlled lead-acid batteries for parking air conditioners, three 200Ah (rated reserve capacity 428min) batteries are randomly selected, and the test method is:
[0060] a. Battery weighing: Before the test, the weight of the battery is 1# battery W0=64.13kg, 2# battery W0=64.25kg, 3# battery W0=64.31kg;
[0061] b. Reserve capacity: Discharge to 10.5V at a constant current of 25A, RC0 = 440min for battery 1#, RC0 = 438min for battery 2#, and RC0 = 441min for battery 3#;
[0062] c. Simultaneously test the cycle endurance of multiple battery groups using the following methods:
[0063] ①1# lead-acid battery is discharged at 25A constant current to 11.4V at 25℃, then charged at 14.0V constant voltage with current limit of 60A for 6h, and the cycle is repeated 30 times. After the 30th charge, the reserve capacity is tested according to step b. The RC1 of 1# battery is 374min;
[0064] ②2# battery was discharged at 20A for 5h at 40℃, then charged at constant voltage 14.7V with current limit 60A for 8h, and repeated 50 times. After the 50th charge, the reserve capacity was tested according to step b. The RC2 of 2# battery was 418min, and the weight W1 was 64.18kg.
[0065] ③Under 25℃, the 3# battery is discharged at a constant current of 25A to 10.5V, and then charged at a constant voltage of 14.4V with a current limit of 60A for 6h, and the cycle is repeated 100 times. When the discharge time RC3≤0.5RC0, the cycle stops; at the 100th discharge time, the 3# battery discharge time RC3 is 321min. After the 100th charge, low-temperature starting is performed, the starting temperature is -18±1℃, the starting current is 600A, the starting time is 30s, and the voltage after 30s is 9.36V;
[0066] d. Result judgment: The battery is qualified if the following three conditions are met:
[0067] (1) 1# battery RC1 / RC0=374 / 440=85%≥80%;
[0068] (2) 2# battery RC2 / RC0=418 / 438=95%≥90%;
[0069] (W0-W1) / C 20 =(64.25-64.18) / 200=0.35≤0.4g / Ah;
[0070] (3) Battery #3 RC3 / RC0=321 / 440=73%>50%, 30s voltage is 9.36V>9.0V.
[0071] From this we can see that the cycle endurance of this batch of batteries meets the requirements and are qualified batteries.
[0072] Example 4
[0073] A test method for the cycle endurance of a valve-controlled lead-acid battery for a parking air conditioner. The test method for a 220Ah (rated reserve capacity 476min) battery is as follows:
[0074] a. Battery weighing: Before the test, the weight of the battery is 1# battery W0 = 66.51kg, 2# battery W0 = 66.37kg, 3# battery W0 = 66.50kg;
[0075] b. Reserve capacity: Discharge to 10.5V at a constant current of 25A, record the discharge time, 1# battery RC0 = 484min, 2# battery RC0 = 489min, 3# battery RC0 = 480min;
[0076] c. Test the cycle endurance of multiple battery groups using different methods at the same time:
[0077] ①1# lead-acid battery is discharged at 25A constant current for 5h at 25℃, then charged at 14.0V constant voltage with current limit of 66A for 6h, and the cycle is repeated 30 times. After the 30th charge, the reserve capacity RC1 of 1# battery is tested according to step b, which is 426min;
[0078] ②2# battery was discharged at 22A for 5h at 40℃, then charged at constant voltage 14.7V with current limit 66A for 8h, and the cycle was repeated 50 times. After the 50th charge, the reserve capacity RC2 of 2# battery was tested according to step b, which was 455min, and the weight W1 was 66.29kg;
[0079] ③Under 25℃, the 3# battery is discharged at a constant current of 25A to 10.5V, and then charged at a constant voltage of 14.4V with a current limit of 66A for 6h, and the cycle is repeated 100 times. When the discharge time RC3≤0.5RC0, the cycle stops; the 100th discharge time RC3 of the 3# battery is 334min. After the 100th charge, low-temperature starting is performed, the starting temperature is -18±1℃, the starting current is 660A, the starting time is 30s, and the voltage after 30s is 9.47V;
[0080] d. Result judgment: The battery is qualified if the following three conditions are met:
[0081] (1) 1# battery RC1 / RC0=426 / 484=88%≥80%;
[0082] (2) 2# battery RC2 / RC0=455 / 489=93%≥90%;
[0083] (W0-W1) / C 20 =(66.37-66.29) / 220=0.36≤0.4g / Ah;
[0084] (3) Battery #3 RC3 / RC0=334 / 480=70%>50%, 30s voltage is 9.47V>9.0V.
[0085] From this we can see that the cycle endurance of this batch of batteries meets the requirements and are qualified batteries.
[0086] Comparative Example 1
[0087] The existing method in the industry is to test in accordance with the GB / T5008.1-2013 standard for starting lead-acid batteries. Specifically, the test method for 220Ah (rated reserve capacity 476min) batteries is to perform the following cycles at 25°C:
[0088] 1) At 0.25C 20 A constant current discharge for 2h;
[0089] 2) Then limit the current to 0.25C at a constant voltage of 14.4V 20 A charging 4h45min;
[0090] 3) Then use a constant current of 0.025C 20 A charging for 15 minutes;
[0091] 4) Steps 1) to 3) are repeated 18 times as one unit;
[0092] 5) Current limit 0.25C at constant voltage 14.4V 20 A charging 6h;
[0093] 6) Open circuit and let stand for 5 hours;
[0094] 7) At 0.25C 20 A constant current discharge to 10.0V, the capacity is not less than 0.5C 20 Ah;
[0095] 8) Current limit 0.25C at constant voltage 14.4V 20 A is charged for 20h, then charged at a constant current of 0.025C 20 A charging 4h;
[0096] 9) Steps 1) to 8) constitute a complete test cycle, and then the battery is placed in a low temperature box at -18±1℃ for more than 24 hours;
[0097] 10) Discharge at 660A for 30s, and the voltage should be ≥7.2V for 30s;
[0098] 11) Then proceed to the next unit test.
[0099] According to the test method of comparative example 1, the battery was subjected to 5 unit cycle tests. The relationship between the cycle discharge voltage and the number of discharges during the test is shown in Figure 1 .Depend on Figure 1 It can be seen that: with the increase of the number of cycles, the discharge voltage gradually increases. This is because the cyclic overcharge causes the decomposition and precipitation of the electrolyte, which reduces the volume of the electrolyte and increases the acid concentration, resulting in a continuous increase in the battery voltage. It can be seen that the cycle test in the standard in Comparative Example 1 is actually an overcharge cycle process. After calculation, the charging amount exceeds 110%. Although the test results are qualified, this cycle test cannot accurately evaluate the operating conditions and failure modes of the battery for the parking air conditioner.
[0100] The qualified batteries selected by comparative example 1 were subjected to cyclic discharge tests corresponding to operating conditions 1 (undercharge) and 3 (deep discharge), and the relationship curve between the discharge time (ordinate / h) and the number of discharges (abscissa) is shown in FIG. Figure 2 .Depend on Figure 2 It can be seen that the first discharge time RC0 of the undercharged battery is 476min, the 30th discharge time RC1 is 252min, RC1 / RC0=252 / 476=53%≤80%, and the capacity decay rate after 30 undercharge cycles is high. The accumulated large particles of lead sulfate are difficult to be reduced to metallic lead by reducing the depth of discharge or extending the charging time, and the battery capacity is difficult to recover. The first discharge time RC0 of the deep discharge battery is 486min, and the 36th discharge time RC3 is 238min. RC3 / RC0=238 / 486=49%≤0.5RC0. After restorative charging, the battery capacity is difficult to recover. After the battery is dissected, the positive active material has been softened visually. The 30s starting voltage of the battery is low, and the battery is difficult to ignite.
[0101] The qualified batteries selected from Example 4 of the present invention were subjected to 30 undercharge cycles. The relationship between the discharge time and the number of discharges during the cycle is shown in FIG. Figure 3 , compared with the variation diagram of discharge time and discharge number during 30 undercharge cycles of qualified batteries screened out in Comparative Example 1, Figure 3 It can be seen that the qualified batteries screened out by the method of the present invention have a discharge time change significantly less than that of comparative example 1 under under-charging operating conditions, indicating that the qualified batteries screened out by the method of the present invention have a low capacity attenuation rate after 30 under-charging cycles and higher durability.
[0102] Two batteries were randomly selected from the qualified batch of batteries screened by the method of Example 4 for vehicle installation test. The battery reserve capacity and -18±1°C low-temperature starting performance were tested before installation. The battery condition was followed up by the driver, and feedback was given that the battery was in good condition. The batteries were recalled 1.5 years later and tested. The results were compared with the test before installation, as shown in Table 1 below. It can be seen that after 1.5 years of installation and use, the reserve capacity of the battery did not decrease by more than 20%, the 30s low-temperature starting voltage was above 9.0V, and the battery performance was normal, which further proved the accuracy of the present test method.
[0103] Table 1 Comparison of performance changes of qualified batteries screened by the method of the present invention before and after installation
[0104]
Claims
1. A test method for the cycle endurance of a lead-acid battery for a parking air conditioner, Features: A test method for determining the life of a lead-acid battery for a parking air conditioner according to the battery operating conditions, the method comprising the following steps: a. Battery weighing: The weight of the battery before the test begins is W 0 ; b. Reserve capacity: Discharge to 10.5V at a constant current of 25A, and record the discharge time RC 0 ; c. Capacity decay rate after 30 undercharges: The lead-acid battery is discharged at 25A constant current to 11.4V at 25℃, and then the current is limited to 0.3C at a constant voltage of 14.0V. 20 Charge A for 6 hours and repeat the cycle 30 times. After the 30th charge, test the reserve capacity RC according to step b. 1 ; d. Result determination: RC 1 / RC 0 ≥80%, the screened batteries are qualified batteries; In the step c, the method for testing the cycle endurance of multiple groups of batteries at the same time also includes: the capacity retention rate and mass loss rate after 50 overcharges: the battery is heated at 0.1C at 40°C. 20 A discharges for 5 h, then limits the current to 0.3C at a constant voltage of 14.7V 20 Charge A for 8 hours and repeat the cycle 50 times. After the 50th charge, test the reserve capacity RC according to step b. 2 , and weigh W 1 , and meets RC 2 / RC 0 ≥90%, (W 0 -W 1 ) / C 20 Batteries with a value of ≤0.4g / Ah are qualified; In the step c, the method of testing the cycle endurance of multiple groups of batteries at the same time also includes: the capacity retention rate and low temperature starting ability after 100 deep discharge cycles: the battery is discharged at 25A constant current to 10.5V at 25°C, and then the constant voltage is 14.4V with a current limit of 0.3C 20 A is charged for 6h, when the discharge time RC 3 ≤0.5RC 0 When the discharge time RC 3 >0.5RC 0 After the 100th charge, the battery is started at low temperature with a starting current of 3C. 20 A, start time 30s, record 30s voltage, 30s voltage ≥ 9.0V, and RC 3 / RC 0 Batteries with a test rate of ≥50% are qualified.
2. The method for testing the cycle durability of a lead-acid battery for a parking air conditioner according to claim 1, Features: The battery operating conditions include: operating condition 1: the vehicle's cumulative mileage is less than 8 hours / day, the parking air conditioner is used for more than 10 hours / day, the battery discharge depth is large, the charging time is short, and the battery failure mode is insufficient charging; operating condition 2: the vehicle has been continuously driven for more than 14 hours / day, the parking air conditioner is used for less than 6 hours / day, the battery is in a continuous charging state, and the battery failure mode is overcharging resulting in a reduction in electrolyte; operating condition 3: the vehicle has been driven for 8-14 hours / day, the parking air conditioner is used for 6-10 hours / day, the battery is in a higher charge state, and the battery failure mode is starting failure caused by softening of the positive active material.
3. The method for testing the cycle durability of a lead-acid battery for a parking air conditioner according to claim 2, Features: In the step c, the temperature of the low temperature start is -18±1°C.