A columnar semiconductor field effect positive feedback transistor based on bulk silicon
By adopting a vertical columnar gate oxide structure in Z2-FET, the problem of reduced capacitance of the planar gate oxide layer is solved, the charge retention time and memory performance are improved, and it is suitable for high-performance dynamic memory.
Patent Information
- Application Number
- CN202111540190.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-16
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-12-16
AI Technical Summary
The capacitance of the planar gate oxide layer of traditional bulk silicon-based Z2-FET decreases as the size of the device decreases, resulting in a reduction in stored charge and easy loss of charge, affecting the performance of high-performance dynamic memory.
A columnar semiconductor field-effect positive feedback transistor based on bulk silicon is used to epitaxially grow weak p-type doped silicon and heavily doped p-type silicon on a doped n-type bulk silicon substrate, and vertically formed by etching and ALD epitaxy. Pillar gate oxide structure increases capacitance and extends data storage time.
It increases the capacitance of the gate oxide layer, extends the charge retention time, improves the reliability and performance of the memory, is compatible with traditional CMOS processes, and is suitable for high-performance memory fields.
Smart Images

Figure CN114242792B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor devices, and in particular relates to a columnar semiconductor field effect positive feedback transistor based on bulk silicon. Background Art
[0002] Compared with the common dynamic memory devices currently available, such as capacitor-based IT-IC dynamic random access memory (DRAM) [1], traditional 6-T static random access memory [2], and thyristor-based RAM (T-RAM) [3-7], and field effect diode (FED) [3-4]. IT-IC DRAM has high integration density and excellent reliability, but slow access speed. In contrast, traditional 6-T static random access memory can provide high access speed but low density. Therefore, memories with high integration and high-speed performance have attracted the attention of more and more researchers. For example, RAM (T-RAM) derived from thyristors is small and compact in size and can perform high-speed reading and writing, but its stable performance is highly dependent on precise doping control on bipolar transistors. In 2011, the applicant proposed a new semiconductor device Z with a working mechanism that is completely different from that of ordinary MOSFET. 2 -FET[5,6]. 2 -FET is built on a silicon-on-insulator (SOI) substrate. Due to its asymmetric device structure and the double gate induction of SOI, a new band structure is formed in the substrate. 2 -FET generates positive carrier feedback inside. Compared with traditional MOSFET, Z 2 -FET has completely different electrical characteristics. Its subthreshold swing is extremely low, which makes it have great application potential in low-voltage and low-power integrated circuits[7]. 2 The output characteristics of -FETs show a huge gate-controlled hysteresis effect. This characteristic has been developed and applied to volatile memory, which is more compact and has greatly improved read and write speeds [8]. In addition, Z based on bulk silicon substrates 2 -FET, due to its symmetrical physical structure and highly compatible self-aligned process with MOSFET, reduces the lithography registration error and reduces the process difficulty. The masking effect of the gate and gate sidewall provides a basis for forming LDD doping and cathode / anode doping regions through a self-aligned ion implantation process similar to MOSFET. 2 -FET can be widely used in low subthreshold swing switches, memories, electrostatic protection and sensors. It uses a feedback mechanism similar to that of Z2-FET and feedback FET (FB-FET). 2-FET DRAM combines a lightly doped drain (LDD) and a front gate to form a potential barrier. It shows similar gate control hysteresis in output characteristics and is used as a single transistor DRAM (1T-DRAM) with excellent performance.
[0003] However, the above Z 2 -FET's cubic gate oxide capacitance is affected by the current requirement for shrinking device size. As the device size shrinks, the capacitance decreases, and the amount of stored charge decreases, resulting in easy loss of charge. In addition, the reduced capacitance leads to a decrease in storage time, which is a disadvantage that cannot be ignored for applications in high-performance dynamic memory. Summary of the invention
[0004] The object of the present invention is to provide a bulk silicon-based columnar semiconductor field effect positive feedback transistor with large gate oxide layer capacitance and excellent electrical performance.
[0005] The columnar semiconductor field effect positive feedback transistor based on bulk silicon provided by the present invention has a structure as follows Figure 1 As shown, its structure is as follows: the bottom of the device is a heavily doped cathode 1, on top of which are epitaxially vertically grown p-type channel region 3, intrinsic / weakly doped channel region 6 and heavily doped anode 7; due to over-etching, both sides of the bottom heavily doped cathode 1 are recessed, and the recessed cathode part and both sides of the p-type channel region 3 are filled with insulating layer substrates 2 and 10 respectively; both sides of the intrinsic / weakly doped channel region 6 are gate oxide layers 5 and gate oxide layers 8 respectively, and the outer sides are gate electrodes 4 and gate electrodes 9 respectively; in this way, the gate oxide layers 5 and 8 wrap the channel region 6 and isolate the channel region 6 from the gate electrodes 4 and gate electrodes 9; the heavily doped anode 7 is exposed at the top.
[0006] The columnar semiconductor field effect positive feedback transistor is based on a bulk silicon substrate or is built on other semiconductors, such as germanium, germanium silicon and gallium nitride.
[0007] The columnar semiconductor field effect positive feedback transistor has a channel, a substrate and an LDD region whose doping is weaker than that of a cathode and an anode and are inverse to each other.
[0008] The anode and cathode of the columnar semiconductor field effect positive feedback transistor are heavily inversely doped, that is, one is n-type and the other is p-type doped.
[0009] The present invention also provides a method for preparing the columnar semiconductor field effect positive feedback transistor, the specific steps of which are:
[0010] (1) The starting bulk silicon is the substrate; the substrate is strongly n-doped as the channel and serves as the cathode; on top of the original silicon wafer, a p-type doped channel layer is grown epitaxially; then an intrinsic / low-doped silicon channel layer is grown epitaxially; then a p-type heavily doped layer is grown epitaxially and in-situ doped during the epitaxial growth to finally form a heavily p-doped anode;
[0011] (2) Forming a nanowire structure, first patterning the photoresist mask by electron beam lithography, and using RIE for dry etching to obtain the initial trapezoidal nanowires; anisotropic wet etching is performed in a 5% TMAH solution to reduce the diameter of the nanowires; TMAH wet etching can only etch the nanowires under the photoresist mask layer in the lateral direction, but not in the vertical direction, which results in very steep nanowires; TMAH wet etching can not only eliminate plasma damage, but also smooth the etched Si surface; photolithography opens a window and etches away the periphery to leave a columnar structure;
[0012] (3) Use PECVD to deposit an insulating layer. PECVD deposition has a vertical directionality and no deposition will occur on the outer sidewalls of silicon.
[0013] (4) Depositing a layer of gate oxide material using ALD, the deposition method is atomic layer deposition;
[0014] (5) Deposit a positive gate layer by sputtering. Because sputtering is vertical, there is also a layer of gate metal / polysilicon above the anode, but not on the side walls;
[0015] (6) Applying photoresist (PR) clearly shows the difference in PR thickness. Using dry etching, the PR / gate / gate oxide layer can be removed only on the top of the nanowire during the blank etch process, and the bottom insulation is covered with photoresist;
[0016] (7) Wet etching, generally using SiO2 etching solution to etch away the insulating layer above the p+ layer; immerse the sample in SC-1 to etch only the gate oxide layer to obtain the desired structure;
[0017] (8) Remove the residual PR glue on the surface of the sample and anneal to form electrodes on the source, drain and gate; the annealing temperature is between 300 and 900 degrees.
[0018] In step (1) of the present invention, the doping concentration of the substrate is 10 19 cm -2 Up to 10 21 cm -2 A p-type doped channel layer is grown epitaxially, with a doping concentration of 10 15 cm -2 Up to 10 19 cm -2Between; epitaxial layer of intrinsic / low-doped silicon channel layer, the doping concentration of which is 10 10 cm -2 Up to 10 16 cm -2 between; heavily p-doped anode, doping concentration is 10 19 cm -3 Up to 10 21 cm -3 The thickness of the anode region formed is between 10nm and 100nm.
[0019] In step (3) of the present invention, an insulating layer is deposited by PECVD and filled with silicon nitride, silicon dioxide, or a low dielectric constant medium such as SiOCN and SiBCN.
[0020] In step (4) of the present invention, the gate oxide layer is made of materials such as silicon dioxide (SiO2), silicon nitride, aluminum oxide or hafnium oxide, and has a thickness between 1 nm and 30 nm.
[0021] In step (5) of the present invention, a positive gate is deposited by sputtering. The positive gate is polysilicon or metal, or a composite layer of polysilicon and metal, and its thickness is 10nm to 500nm.
[0022] Traditional field effect positive feedback devices, such as Z 2 -FET, built on a silicon-on-insulator (SOI) substrate. It is expensive and asymmetrical in structure, incompatible with the common bulk silicon CMOS process and device structure. The ever-shrinking device size leads to a decrease in the capacitance of the planar gate oxide layer, a decrease in the amount of charge that can be stored in the gate oxide layer, and the charge carried by the device has been lost, resulting in a decrease in storage time and performance.
[0023] The present invention is based on the Z of bulk silicon substrate 2 -FET, a novel vertical columnar gate oxide structure is proposed to improve the planar gate oxide Z 2 -FET defects. By epitaxially growing weakly p-type doped silicon, n-type silicon and heavily doped p-type silicon on a doped n-type bulk silicon substrate, and then etching and ald epitaxially growing a gate oxide layer on the sidewall and depositing metal by PECVD, a special energy band structure required for the positive feedback mechanism is formed, which is equivalent to the ordinary Z 2 -FET structure is vertical, using the feedback between electron and hole currents and the corresponding injection barrier formed by the front gate and the back gate. While retaining its original electrical performance and function, the gate oxide capacitance is greatly increased due to the vertical structure. In addition, the new columnar Z 2-FET positive feedback device has a symmetrical physical structure similar to MOSFET. Combining the device structure of bulk silicon substrate, symmetrical and vertical columnar gate oxide layer and epitaxial doping, the new device proposed by the present invention not only has excellent electrical performance and special application functions, but also has a process that is fully compatible with traditional CMOS and greatly increases the capacitance and charge retention time, and can be applied to the field of high-performance memory.
[0024] In the present invention, the special energy band structure (electron and hole injection barrier) required for the field effect positive feedback device is formed by the positive gate and the low drain doping region adjacent to the channel. Figure 1 As shown in the figure, it is a forward biased pin diode, with an intrinsic / lightly doped channel covered by the gate and the remaining part not covered by the gate. By changing the vertical columnar n-channel doping and the positive voltage strength applied to the positive gate, the injection barrier height of the holes formed together in the vertical columnar channel is adjusted, thereby regulating the injection of anode holes on the right side of the gate. The p-type low-drain doped area below the vertical columnar channel will form an electron barrier to control the injection of cathode electrons. By changing the gate oxide layer to a vertical cylindrical shape, the device capacitance increases and the retention power consumption time increases.
[0025] The present invention increases the capacitance of the gate oxide layer by changing the planar gate oxide layer into a vertical columnar structure, prolongs the data storage time and improves reliability. The key vertical gate oxide layer structure is introduced, and its ring-gate-like metal gate can control the middle channel from all directions, suppressing the short channel effect, and can be applied to high-performance dynamic memory DRAM. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic diagram of the structure of a columnar semiconductor field effect positive feedback transistor according to the present invention.
[0027] Figure 2 It is a schematic diagram of the preparation process of the columnar semiconductor field effect positive feedback transistor of the present invention.
[0028] Figure 3 This is an embodiment structure of the columnar semiconductor field effect positive feedback transistor of the present invention. Among them, the doping types of the anode and cathode of variant 1 are opposite to those of the main structure, and the bottom types of the anode and cathode of variants 2 and 3 are opposite, respectively. DETAILED DESCRIPTION
[0029] Based on the same working principle, the structure of the device can be different, and the specific implementation methods can be divided into the following according to different embodiments:
[0030] Example 1 (corresponding to Figure 1 The device structure and Figure 2 Process flow):
[0031] (1) If Figure 2 (a) shows the starting bulk silicon substrate. This substrate is generally strongly n-type doped as a channel doping, and as a cathode, the doping concentration is 10 19 cm -2 Up to 10 21 cm -2 On the original silicon wafer, a p-type doped channel layer is grown epitaxially, with a doping concentration of 10 15 cm -2 Up to 10 19 cm -2 Then an intrinsic / low-doped silicon channel layer is grown epitaxially, with a doping concentration of 10 10 cm -2 Up to 10 16 cm -2 During the epitaxial growth of a p-type heavily doped layer, in-situ doping is performed to finally form a heavily p-doped anode. The thickness of the anode region formed is between 10nm and 100nm, and the doping concentration is between 10 19 cm -3 Up to 10 21 cm -3 between.
[0032] (2) To form the nanowire structure, the photoresist mask is first patterned by electron beam lithography with a width of 300 nm and a pitch of 300 nm. Dry etching is performed using RIE to obtain the initial trapezoidal nanowires; generally fluorine-based gases such as SF6, CHF3 or CH3F are used. The height is 300 nm. Anisotropic wet etching is performed in a 5% TMAH solution to reduce the diameter of the nanowires. The TMAH solution etches the nanowires below the photoresist mask layer only in the lateral direction, not in the vertical direction, which results in very steep nanowires with an average diameter of 100 nm, as shown in Figure 2. Figure 2 (b) and (c) are shown. TMAH wet etching can not only eliminate plasma damage, but also smooth the etched Si surface. In this way, nanowires with a diameter of about 30nm can be achieved. The photolithography window is opened and the periphery is etched away to leave a columnar structure, such as Figure 2 (c) shown.
[0033] (3) Deposit an insulating layer using PECVD, such as Figure 2 As shown in (d), if commonly used silicon nitride, silicon dioxide, or low dielectric constant dielectrics such as SiOCN and SiBCN are used as filling materials, PECVD deposition has a vertical directionality and will not deposit on the outer sidewalls of silicon.
[0034] (4) Use ALD to deposit a layer of gate oxide material. The gate oxide layer is generally made of silicon dioxide (SiO2), but can also be made of silicon nitride, aluminum oxide or hafnium oxide. The thickness is generally between 1nm and 30nm. The deposition method is atomic layer deposition. Figure 2 (e) shown.
[0035] (5) Sputtering is used to deposit a positive gate layer, which is generally polysilicon or metal, or a composite layer of polysilicon and metal, with a thickness of 10nm to 500nm. Because sputtering is vertical, there is also a layer of gate metal / polysilicon above the anode, but not on the sidewalls. Figure 2 (f) shown.
[0036] (6) Coating (PR) clearly shows the difference in PR thickness, e.g. Figure 2 As shown in (g), dry etching generally uses fluorine-based or halogen-based gases, and generally uses reactive ion etching with vertical directionality, such as CF4, O2, N2, SF6, CHF3, NF3, He, C2F6, etc. Select the condition with large etching selectivity, so that during the blank etching process, only the PR / gate / gate oxide layer can be removed on the top of the nanowire, and the bottom insulation can be covered with photoresist, while wet etching generally uses SiO2 etching liquid. Etch away the insulating layer above the p+, see Figure 2 (h) shown.
[0037] The sample was immersed in SC-1 (70°C, NH4OH:H2O2:H2O=1:1:5) to etch only the gate oxide layer. Figure 2 (i) The structure shown.
[0038] (7) Remove the residual PR glue on the surface of the sample and anneal to form electrodes on the source, drain and gate; the annealing temperature is between 300 and 900 degrees.
[0039] The columnar positive feedback transistor not only has excellent electrical properties and special application functions, but its preparation process is fully compatible with traditional CMOS, which greatly increases the gate oxide layer capacitance, increases the charge retention time, prolongs the data storage time, and improves the performance of the device as a high-performance memory.
[0040] Example 2 (corresponding to Figure 3 Device structure diagram)
[0041] Variant 1 in Example 2 is similar to Example 1, except that Example 2 is an n-type device, while Example 1 is a p-type device. The anode and cathode are swapped, and the channel is n-type doped. To achieve this structure, it is only necessary to change the first layer of epitaxial growth to n-type, the subsequent second layer of epitaxial doping to weak type, and the third layer of heavy doping to n-type. Variant 2 in Example 2 is similar to Variant 3, except that the anode and cathode are swapped at the bottom.
[0042] References
[0043] 1. C. J. Radens, S. Kudelka, L. Nesbit, R. Malik, T. Dyer, C. Dubuc, T. Joseph, M. Seitz, L. Clevenger, N. Arnold, J. Mandelman, R. Divakaruni, D. Casarotto, D. Lea, V. C. Jaiprakash, J. Sim, J. Faltermeier, K. Low, J. Strane, S. Halle, Q. Ye, S. Bukofsky, U. Gruening, T. Schloesser, and G. Bronner, “An orthogonal 6F trench sidewall vertical device cell for 4 Gb / 16 Gb DRAM,” in IEDM Tech. Dig., 2000, pp. 349–352.
[0044] 2. L. Chang, D. M. Fried, J. Hergenrother, J. W. Sleight, R. H. Dennard, R. K. Montoye, L. Sekaric, S. J. McNab, A. W. Topol, C. D. Adams, K. W. Guarini, and W. Haensch, “Stable SRAM cell design for the 32 nm node and beyond,” in VLSI Symp. Tech. Dig., 2005, pp. 128–129.
[0045] 3. M. Bawedin, S. Cristoloveanu, A. Hubert, K.-H. Park, and F. Martinez, “Floating body SOI memory: The scaling tournament,” in Semiconductor on-Insulator Materials for Nanoelectronics Applications, A. Nazarov, J.-P. Colinge, F. Balestra, J.-P. Raskin, F. Gamiz, and V. Lysenko, Eds. Heidelberg, Germany: Springer-Verlag, 2011, pp. 393–421.
[0046] 4. H.-J. Cho, F. Nemati, R. Roy, R. Gupta, K. Yang, M. Ershov, S. Banna, M. Tarabbia, C. Sailing, D. Hayes, A. Mittal, and S. Robins, “A novel capacitor-less DRAM cell using thin capacitively-coupled thyristor (TCCT),” in IEDM Tech. Dig., 2005, pp. 311–314.
[0047] 5. J. Wan, C. Le Royer, A. Zaslavsky and S. Cristoloveanu, Z2-FET field-effect transistor with a vertical subthreshold slope and with no impact ionization, 2013, U.S. Patent: US8,581,310.
[0048] 6.J. Wan, S. Cristoloveanu, C. Le Royer and A. Zaslavsky, Dynamicmemory cell provided with a field-effect transistor having zero swing, 2013,Publication: 20,130,100,729.
[0049] 7.J. Wan, S. Cristoloveanu, C. Le Royer, and A. Zaslavsky, A feedback silicon-on-insulator steep switching device with gate-controlled carrier injection. Solid-State Electronics, 2012. 76: p. 109-111.
[0050] 8. J. Wan, C. Le Royer, A. Zaslavsky, and S. Cristoloveanu, 1999 . A Compact Capacitor-Less High-Speed DRAM Using Field Effect-Controlled Charge Regeneration. IEEE Electron Device Letters, 2012. 33(2): p. 179-181.
Claims
1. A columnar semiconductor field effect positive feedback transistor based on bulk silicon, It is characterized in that The structure is as follows: the substrate is a heavily doped cathode (1), and a p-type channel region (3), an intrinsic / weakly doped channel region (6) and a heavily doped anode (7) are epitaxially grown vertically on the cathode (1); due to over-etching, both sides of the bottom heavily doped cathode (1) are recessed, and the recessed cathode part and both sides of the p-type channel region (3) are filled with insulating layer substrate (2, 10); both sides of the intrinsic / weakly doped channel region (6) are gate oxide layers (5, 8), and the outer sides are gate electrodes (4, 9); in this way, the gate oxide layers (5, 8) wrap the channel region (6) and isolate the channel region (6) from the gate electrodes (4, 9); the heavily doped anode (7) is exposed at the top.
2. The columnar semiconductor field effect positive feedback transistor according to claim 1, It is characterized in that The substrate is silicon, germanium, silicon germanium or gallium nitride.
3. The columnar semiconductor field effect positive feedback transistor according to claim 1, It is characterized in that Its anode and cathode are heavily inversely doped, that is, one is n-type and the other is p-type.
4. A method for preparing a columnar semiconductor field effect positive feedback transistor based on bulk silicon, It is characterized in that The specific steps are: (1) The starting bulk silicon is the substrate; the substrate is strongly n-doped as the channel and serves as the cathode; on top of the original silicon wafer, a p-type doped channel layer is grown epitaxially; then an intrinsic / low-doped silicon channel layer is grown epitaxially; then a p-type heavily doped layer is grown epitaxially and in-situ doped during the epitaxial growth to finally form a heavily p-doped anode; (2) Forming the nanowire structure, first patterning the photoresist mask by electron beam lithography, and dry etching using RIE to obtain the initial trapezoidal nanowires; Anisotropic wet etching was performed in a 5% TMAH solution to reduce the diameter of the nanowires; TMAH wet etching etches the nanowires under the photoresist mask layer only in the lateral direction, making the nanowires steep; photolithography opens a window and etches away the periphery to leave a columnar structure; (3) Depositing an insulating layer using PECVD; (4) Depositing a layer of gate oxide material using ALD; (5) Deposit a positive gate layer by sputtering. Since sputtering is vertical, there is also a layer of gate metal / polysilicon above the anode; (6) Apply photoresist, showing the difference in photoresist thickness, and use dry etching. During the blank etching process, the photoresist / gate / gate oxide layer is removed only on the top of the nanowire, and the bottom insulation is covered with photoresist; (7) Wet etching to etch away the insulating layer above the p+; Immerse the sample in SC-1 to etch only the gate oxide layer to obtain the desired structure; (8) Removing the residual photoresist on the surface of the sample and annealing to form electrodes on the source, drain and gate; the annealing temperature is between 300°C and 900°C.
5. The preparation method according to claim 4, It is characterized in that In step (1), the doping concentration of the substrate is 10 19 cm -2 Up to 10 21 cm -2 Between; epitaxially grow a p-type doped channel layer with a doping concentration of 10 15 cm -2 Up to 10 19 cm -2 Between; epitaxial layer of intrinsic / low-doped silicon channel layer, the doping concentration of which is 10 10 cm -2 Up to 10 16 cm -2 between; heavily p-doped anode, doping concentration is 10 19 cm -3 Up to 10 21 cm -3 The thickness of the anode region formed is between 10nm and 100nm.
6. The preparation method according to claim 4, It is characterized in that In step (3), the insulating layer is deposited by PECVD and is filled with silicon nitride, silicon dioxide, SiOCN or SiBCN.
7. The preparation method according to claim 4, It is characterized in that In step (4), the gate oxide layer is made of silicon dioxide, silicon nitride, aluminum oxide or hafnium oxide; and has a thickness between 1 nm and 30 nm.
8. The preparation method according to claim 4, It is characterized in that In step (5), a positive gate is deposited by sputtering. The positive gate is polysilicon or metal, or a composite layer of polysilicon and metal, and has a thickness of 10 nm to 500 nm.