Electrochromic device including a transparent conductive oxide layer and a bus bar and a method of forming the same
By using bus bars made of silver material in electrochromic devices and firing at high temperatures, the problem of difficult to improve the resistivity and adhesion of bus bars is solved, and a crowd with low resistivity and good adhesion is achieved improves the performance of electrochromic devices.
Patent Information
- Application Number
- CN202111597737.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2016-04-19
- Filing Date
- 2017-04-13
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2037-04-13
AI Technical Summary
The resistivity and adhesion of bus bars in existing electrochromic devices are difficult to improve simultaneously, limiting material selection and processing conditions.
Bus bars made of silver material are used in electrochromic devices, by forming a transparent conductive oxide layer and an oxidation layer on the substrate and firing the bus bar precursor at high temperatures to form a bus bar with low resistivity and good viscosity Combined bus bar.
The low resistivity of the bus bar and good adhesion to the underlying material are achieved, and the performance of the electrochromic device is improved, especially under high temperature conditions, without damaging the conductivity of transparent conductive oxides.
Smart Images

Figure CN114265251B_ABST
Abstract
Description
[0001] This application is a divisional application of an application with an application date of April 13, 2017, application number 201780023491.3, and invention name “Electrochromic device including a transparent conductive oxide layer and a bus bar and a method for forming the same”. Technical Field
[0002] The present disclosure relates to electrochromic devices, and more particularly, to electrochromic devices including a transparent conductive layer and bus bars and methods of forming the same. Background Art
[0003] Electrochromic devices help keep rooms in buildings or passenger compartments of vehicles from becoming too hot. Electrochromic devices include bus bars that can be biased and allow the electrochromic device to change from a higher transmission state to a lower transmission state to reduce the transmission of near infrared radiation. Desirable bus bars have low resistivity and good adhesion to underlying materials. One or more layers in an electrochromic device may limit the material selection and processing conditions of the bus bars. Therefore, it is desirable to improve the resistivity and adhesion of the bus bars. Summary of the invention
[0004] In one aspect, the present application provides an electrochromic device comprising:
[0005] substrate;
[0006] a first transparent conductive oxide layer on the substrate; and
[0007] a first bus bar on the substrate, wherein the first bus bar comprises silver and has:
[0008] Up to 8.0×10 -6 Resistivity in Ω*cm;
[0009] Adhesion strength to SiO2 of at least 3N based on 20 measurements as determined by ASTM B905-00, Method A (reapproved in 2010);
[0010] An average bond strength to SiO2 of at least 3 based on 20 measurements as determined by ASTM B905-00, Method B (reapproved 2010); or
[0011] Its combination. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] The embodiments are illustrated by way of example and not limitation to the accompanying drawings.
[0013] Figure 1 Included is a flow chart of a method of forming an electrochromic device according to an embodiment as described herein.
[0014] Figure 2 Included are illustrations of cross-sectional views of a workpiece including a substrate and an electrochromic stack.
[0015] Figure 3 Including after the formation of the anti-oxidation layer, Figure 2 Illustration of a cross-sectional view of a workpiece.
[0016] Figure 4 comprising, after forming a layer having a refractive index between the refractive index of the anti-oxidation layer and the environment, Figure 3 Illustration of a cross-sectional view of a workpiece.
[0017] Figure 5 After patterning the electrochromic stack, Figure 4 Illustration of a cross-sectional view of a workpiece.
[0018] Figure 6 Including after forming the busbar, Figure 5 Illustration of a cross-sectional view of a workpiece.
[0019] Figure 7 comprising, after forming a substantially completed electrochromic device, Figure 6 Illustration of a cross-sectional view of a workpiece.
[0020] Figure 8 An illustration of a cross-sectional view of an insulating glass unit comprising Figure 7 electrochromic device.
[0021] The skilled person will appreciate that the elements in the drawings are illustrated for simplicity and clarity, but are not necessarily drawn to scale. For example, the size of some elements in the drawings may be magnified relative to other elements to help improve the understanding of the embodiments of the present invention. DETAILED DESCRIPTION
[0022] The following description in conjunction with the figures is provided to assist in understanding the teachings disclosed herein. The following discussion will focus on specific implementations and examples of the teachings. This focus is provided to help describe the teachings and should not be interpreted as limiting the scope or applicability of the teachings.
[0023] Polymers include homopolymers and copolymers. Homopolymers are formed from a single polymer precursor, and copolymers are formed from different polymer precursors.
[0024] In this specification, the refractive index is measured at 550 nm.
[0025] As used herein, the terms "comprises / comprising," "includes / including," "has / having," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a process, method, article, or apparatus that includes a list of features is not necessarily limited to only those features, but may include other features not expressly listed or inherent to such process, method, article, or apparatus. In addition, unless expressly stated to the contrary, "or" refers to an inclusive, or non-exclusive, or. For example, a condition A or B is satisfied by any one of the following: A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), and both A and B are true (or exist).
[0026] The use of "a" or "an" is used to describe elements and components described herein. This is done only for convenience and to give a general sense of the scope of the invention. Unless it is obvious that other situations are intended, this specification should be understood to include one or at least one, and the singular also includes the plural, or vice versa.
[0027] The use of the words "about," "approximately," or "substantially" is intended to indicate that the value of a parameter is close to the stated value or position. However, slight differences may prevent the value or position from being exactly as previously stated. Therefore, differences of up to ten percent (10%) of the stated values are reasonable variations from the ideal goal of being exactly as described.
[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the invention belongs. The materials, methods, and examples are illustrative only and are not intended to be limiting. To the extent not described herein, many details about specific materials and processing behaviors are conventional and can be found in textbooks and other sources within glass, vapor deposition, and electrochromic technology.
[0029] The electrochromic device may include a bus bar having low resistivity and good adhesion to underlying materials such as a transparent conductive oxide and a substrate, each of which may be in physical contact with the bus bar. The electrochromic device may include a substrate, a transparent conductive oxide layer on the substrate, and a bus bar on the substrate. The bus bar may include silver and have a maximum of 8.0×10 -6 Resistivity of Ω*cm; an average adhesion strength to SiO2 of at least 3N based on 20 measurements as measured by Method A of ASTM B905-00 (reapproved in 2010); at least 3 categories as measured by Method B according to ASTM B905-00 (reapproved in 2010); or any combination thereof.
[0030] In another aspect, a method of forming an electrochromic device may include forming a transparent conductive oxide layer on a substrate; forming a bus bar precursor on the substrate, wherein the bus bar precursor includes silver; and firing the bus bar precursor to form a bus bar, wherein the firing is performed such that the bus bar is at a temperature of at least 390°C.
[0031] The anti-oxidation layer can be used to reduce the likelihood that the transparent conductive oxide will be significantly adversely affected during the formation of the busbars. The anti-oxidation layer can allow the use of silver-based glass frits with relatively higher sintering temperatures compared to electrochromic devices formed with the anti-oxidation layer. In a specific embodiment, the anti-oxidation layer contributes to the transparent conductive oxide becoming over-oxidized, which is undesirable because the transparent conductive oxide needs to have an acceptable resistivity.
[0032] Anti-oxidation layers may also be used between the substrate and the electrochromic stack. Such embodiments may help reduce the amount of mobile ions (such as Li + 、Na + The anti-oxidation layer may be located on the opposite major surface of the electrochromic stack.
[0033] When the anti-oxidation layer is adjacent to air or other gas, a cover layer may be provided between the anti-oxidation layer and the air or other gas. The cover layer may have a refractive index between the refractive index of the anti-oxidation layer and the air or other gas. The cover layer may help reduce total reflection.
[0034] The embodiments as shown in the drawings and described below help to understand specific applications for implementing the concepts as described herein. The embodiments are exemplary and are not intended to limit the scope of the appended claims.
[0035] Figure 1 A method flow for forming an electrochromic device according to one embodiment is included. The method may include forming an electrochromic stack on a substrate at block 102 . Figure 2An illustration of a cross-sectional view of a partially fabricated electrochromic device after forming an electrochromic stack is included. The electrochromic device may include a transparent substrate 200, which includes a glass substrate, a sapphire substrate, an aluminum oxynitride (AlON) substrate, a spinel substrate, or a transparent polymer. In a specific embodiment, the transparent substrate 200 may include ultrathin glass, which is a mineral glass having a thickness in the range of 50 microns to 300 microns. The transparent polymer may include polyacrylates, polyesters, polycarbonates, polysiloxanes, polyethers, polyvinyl compounds, another suitable transparent polymer, or a mixture thereof. In another embodiment, the transparent substrate 200 may be a laminate comprising a layer of materials constituting the aforementioned transparent substrate. In another embodiment, the laminate may include a sunlight control layer or a low-emissivity material that reflects ultraviolet radiation. The substrate 200 may or may not be flexible.
[0036] In one embodiment, the transparent substrate 200 may be a glass substrate, which may be a mineral glass including SiO2 and one or more other oxides. These other oxides may include Al2O3, oxides of alkali metals, oxides of alkaline earth metals, B2O3, ZrO2, P2O5, ZnO, SnO2, SO3, As2O2, or Sb2O3. The transparent substrate 200 may include a colorant, such as an oxide of iron, vanadium, titanium, chromium, manganese, cobalt, nickel, copper, cerium, neodymium, praseodymium, or erbium; or a metal colloid, such as copper, silver, or gold; or elemental or ionic forms of these substances, such as selenium or sulfur.
[0037] In an embodiment where the transparent substrate 200 is a glass substrate, the glass substrate is at least 50% by weight of SiO2. In one embodiment, the SiO2 content is in the range of 50% by weight to 85% by weight. For example, when the main surface is along the exposed surface of the formed laminate, Al2O3 can contribute to scratch resistance. When present, the Al2O3 content can be in the range of 1% by weight to 20% by weight. B2O3 can be effectively used to reduce the viscosity of the glass and its thermal expansion coefficient. The B2O3 content can be no more than 20% by weight, and in a specific embodiment, less than 15% by weight. Alkaline earth metals include magnesium, calcium, strontium and barium. The oxides of alkaline earth metals are suitable for reducing the viscosity of the glass and promoting fusion without being detrimental to the expansion coefficient to a large extent. Compared with some other oxides, calcium and magnesium have a relatively low effect on the density of the glass. The total content of alkali metal oxides can be no more than 25%, 20% by weight or 15% by weight. The oxides of alkali metals can reduce the viscosity of the glass substrate and its tendency to lose its glass luster. The total content of alkali metal oxides can be up to 8%, 5% by weight or 1% by weight. In some applications, it is desired that the glass substrate is transparent and therefore the content of colorants is not high. In a specific embodiment, the iron content is less than 200 ppm.
[0038] The glass substrate may include heat strengthened glass, tempered glass, partially heat strengthened or tempered glass, or annealed glass. "Heat strengthened glass" and "tempered glass", as those terms are known in the art, are two types of glass that have been heat treated to cause surface compression and otherwise strengthen the glass. Heat treated glass is classified as fully tempered or heat strengthened. In one embodiment, the glass substrate is tempered glass and has a surface compression of about 69 MPa or more and an edge compression of about 67 MPa or more. In another embodiment, the transparent substrate is heat strengthened and has a surface compression in the range of 24 MPa to 69 MPa and an edge compression between 38 MPa and 67 MPa. The term "annealed glass" refers to glass produced without internal strain imparted by heat treatment and subsequent rapid cooling. Therefore, annealed glass only excludes heat strengthened glass or tempered glass. The glass substrate can be laser cut.
[0039] Transparent conductive oxide layer 202 covers transparent substrate 200. Transparent conductive oxide layer 202 may include a doped metal oxide. The doped metal oxide may include zinc oxide or tin oxide, either of which may be doped with a Group 13 element, such as Al, Ga, or In. Indium tin oxide (ITO) and aluminum zinc oxide (AZO) are exemplary non-limiting materials that may be used. Figure 2 As shown, transparent conductive oxide layer 202 has a cutout to allow a subsequently formed bus bar to contact the right portion of transparent conductive oxide layer 202 without electrically shorting the bus bar to the left portion of transparent conductive oxide layer 202. Transparent conductive oxide layer 202 has a thickness in the range of 150 nm to 600 nm.
[0040] Electrode layer 204, electrolyte layer 206, and another electrode layer 208 cover transparent conductive oxide layer 202 and transparent substrate 200. Electrode layer 204 may be one of an electrochromic (EC) layer or a counter electrode (CE) layer, and electrode layer 208 is the other of the CE layer or the EC layer.
[0041] Depending on the bias conditions, the EC layer can have variable transmission of visible light and near-infrared radiation (e.g., electromagnetic radiation having a wavelength in the range of 700 nm to 2500 nm). For example, in the absence of an electric field, the electrochromic device is in a highly transmissive ("bleached") state, and an electric field can cause mobile ions (such as Li + 、Na + or H +)From the CE layer, they migrate through the electrolyte layer to the EC layer and reduce the transmission of visible light and near-infrared radiation through the electrochromic device. The lower transmission state can also be referred to as the colored or tinted state. The EC layer can include oxides of transition metals such as iridium, rhodium, ruthenium, tungsten, manganese, cobalt, etc. In a specific embodiment, the CE layer includes WO3. When initially formed, the EC layer may not include any substantial amount of mobile ions that cause the EC layer to have reduced transmission. In another embodiment, the EC layer may include at least some mobile ions. However, the electrochromic device can be reverse-biased to move the mobile ions from the EC layer through the electrolyte layer 206 to the CE layer. In one embodiment, the thickness of the EC layer as deposited is in the range of 80 nm to 600 nm.
[0042] The CE layer can provide the primary source of mobile ions. Additionally, the CE layer remains substantially transparent to visible light when the electrochromic device is in its high transmission state or its low transmission state. The CE layer can include oxides of transition metal elements. In an embodiment, the CE layer can include an oxide of nickel. Nickel can be in its divalent state (Ni 2+ ), its trivalent state (Ni 3+ ) or a combination thereof. The CE layer can include oxides of transition metal elements such as iridium, rhodium, ruthenium, tungsten, manganese, cobalt, etc. The CE layer can also provide a source of mobile ions that can pass through the electrolyte layer 206. The source of mobile ions can be incorporated into the CE layer during formation. In the finished device, the CE layer can be represented by the following chemical formula:
[0043] A x Ni 2+ (1-y) Ni 3+ y M z O a ,
[0044] where:
[0045] A is an element that generates mobile ions, such as Li, Na, or H;
[0046] M is a metal; and
[0047] 0 < x ≤ 10, 0 ≤ y ≤ 1, 0 ≤ z ≤ 10, and (0.5x + 1 + 0.5y + z) ≤ a ≤ (0.5x + 1 + 0.5y + 3.5z).
[0048] In a specific non-limiting embodiment, A is Li, M is W, and in the finished device, the CE layer can be represented by the following chemical formula:
[0049] Li x Ni 2+ (1-y) Ni 3+y W z O (1+0.5x+0.5y+3z) ,
[0050] Where 1.5≤x≤3, 0.4≤y≤0.95, and 0.15≤z≤1.
[0051] In one embodiment, the thickness of the CE layer is in the range of 80 nm to 500 nm.
[0052] The electrolyte layer 206 includes a solid electrolyte that allows ions to migrate through the electrolyte layer 206 when the electric field across the electrolyte layer changes from a high transmission state to a low transmission state, or vice versa. In one embodiment, the electrolyte layer 206 may be a ceramic electrolyte. In another embodiment, the electrolyte layer 206 may include a silicate-based or borate-based material. The electrolyte layer 206 may include a silicate, an aluminum silicate, an aluminum borate, a borate, a zirconium silicate, a niobate, a borosilicate, a phosphosilicate, a nitride, an aluminum fluoride, or another suitable ceramic material. Other suitable ion-conducting materials may be used, such as tantalum pentoxide or garnet or perovskite materials based on lanthanide-transition metal oxides. In another embodiment, as formed, the electrolyte layer 206 may include mobile ions. Therefore, any of the aforementioned lithium-doped or lithium-containing compounds may be used. The electrolyte layer 206 may include multiple layers having alternating or different materials, including reaction products between at least one pair of adjacent layers. In another embodiment, the refractive index and thickness of the electrolyte layer 206 are selected to have an acceptable visible light transmittance while maintaining an extremely low electronic current. In another embodiment, the electrolyte layer 206 has low or insignificant electronic conductivity (eg, low leakage current). The thickness of the electrolyte layer 206 may be in the range of 10 nm to 70 nm.
[0053] Transparent conductive oxide layer 210 covers transparent substrate 200, transparent conductive oxide layer 202, electrode layer 204, electrolyte layer 206, and electrode layer 208. Transparent conductive oxide layer 210 may include any material as previously described with respect to transparent conductive oxide layer 202. Transparent conductive oxide layer 210 may include the same material or a different material compared to transparent conductive oxide layer 202. Transparent conductive oxide layer 210 has a thickness in a range of 150 nm to 600 nm.
[0054] The layers within the electrochromic stack may be formed by physical vapor deposition, chemical vapor deposition, atomic layer deposition, another suitable technique, or any combination thereof.
[0055] The method may further include Figure 1An anti-oxidation layer is formed on the electrochromic stack at frame 122 in FIG. The anti-oxidation layer helps protect the bottom layer during thermal cycles used for annealing or curing to subsequently form busbars, heating to bend substrate 200 into a desired curvature or shape, or other purposes. The performance of one or more layers in the electrochromic stack may be adversely affected by thermal cycles. In a specific embodiment, transparent conductive oxide layers 202 and 210 may include partially and incompletely oxidized transparent conductive oxides. If the transparent conductive oxide is fully oxidized, the transparent conductive oxide may not have sufficient conductivity and the resistivity may become too high or become an insulator (if fully oxidized). The anti-oxidation layer helps prevent transparent conductive oxide layers 202, 210, or both from becoming over-oxidized.
[0056] Figure 3 An illustration of an electrochromic device after forming an anti-oxidation layer 302 on the transparent conductive oxide layer 210 is included. The anti-oxidation layer 302 may include a nitride, such as silicon nitride, aluminum nitride, titanium nitride, tungsten nitride, tantalum nitride, titanium silicon nitride, tungsten silicon nitride, tantalum silicon nitride, or another metal nitride. In a specific embodiment, the anti-oxidation layer 302 includes silicon nitride. The thickness of the anti-oxidation layer 302 is selected to provide sufficient visible light transmission. In one embodiment, the thickness of the anti-oxidation layer is in the range of at least 10nm to 20nm to provide a continuous layer, and in another embodiment, the thickness is up to 300nm or up to 250nm, because larger thicknesses may cause excessive compressive stress, which may cause delamination. In a specific embodiment, the compressive stress may be up to 1GPa. In a specific embodiment, the thickness is in the range of 50nm to 100nm to allow the formation of a continuous layer with sufficient oxidation resistance without generating too much stress.
[0057] The method may further include Figure 1 A layer with an intermediate refractive index is formed on the anti-oxidation layer at frame 12 in FIG. The anti-oxidation layer 302 may have a relatively high refractive index, and if the major surface of the anti-oxidation layer 302 is exposed to air or another gas, the relative difference in refractive index may make the total reflection too high. Therefore, a layer with an intermediate refractive index between the refractive index of the anti-oxidation layer and air or another gas may help reduce total reflection.
[0058] Figure 4 An illustration of an electrochromic device is included after forming a capping layer 402 having an intermediate refractive index on the anti-oxidation layer 302. The capping layer 402 can be an insulating layer. In one embodiment, the capping layer 402 can include an oxide, such as silicon oxide or another suitable oxide. The oxide may or may not be porous. For example, a mixture of oxide and organic particles can be applied, and the organic particles can be burned off during subsequent firing, leaving a porous oxide.
[0059] The thickness of layer 402 can be thick enough to significantly affect total reflection. In practice, sputtering SiO2 is a relatively slow process, so the upper limit may be limited by equipment throughput. In terms of actual thickness, in one embodiment, the cover layer 402 may have a thickness of at least 30nm, at least 40nm, or at least 50nm, and in another embodiment, the cover layer 402 may have a thickness of at most 200nm, at most 150nm, or at most 150nm. In terms of range, the cover layer 402 may have a thickness in the range of 30nm to 200nm, 40 to 150nm, or 50nm to 120nm.
[0060] Layers 302 and 402 may be formed by physical vapor deposition, chemical vapor deposition, atomic layer deposition, another suitable technique, or any combination thereof.
[0061] The method may include Figure 1 At block 142, portions of the electrochromic stack are removed at areas where bus bars will subsequently be formed. Figure 4 , one of the bus bars will be electrically connected to Figure 4 The transparent conductive oxide layer 202 near the left side, and another bus bar will be electrically connected to Figure 4 Transparent conductive oxide layer 202 near the right. Removal of portions of the electrochromic stack may be performed using ablation techniques such as laser ablation, or may be removed using etching techniques. Figure 5 As shown, layers 204, 206, 208, 210, 302, and 402 are patterned to define openings 502 and 504 at which transparent conductive oxide layer 202 is exposed. In another embodiment, opening 504 may extend to a different depth than opening 502. For example, opening 504 may extend to a variety of different depths as long as transparent conductive oxide layer 210 is exposed within opening 504. In one embodiment, layers 302 and 402 are patterned and transparent conductive layer 210 is exposed along the bottom of opening 504. In another embodiment, opening 504 may extend through transparent conductive oxide layer 202 such that substrate 200 is exposed along the bottom of opening 504. After reading this specification, a skilled artisan will be able to determine the depth of opening 504 to meet the needs or expectations of a particular application.
[0062] The method may further include Figure 1A busbar precursor is deposited at frame 144 in the process, and the busbar precursor is fired at frame 146 to form a busbar. The busbar precursor may include silver, and therefore, the busbar may include silver. In one embodiment, the busbar precursor may be a silver paste. The use of an anti-oxidation layer 302 allows the use of more selective silver-containing glass frits and more aggressive firing conditions. For example, silver-containing glass frits that require higher firing temperatures, more reactive environments during firing, or any combination thereof may be used. Prior to the present invention as claimed herein, the selection of silver-containing glass frits and firing conditions were limited because the transparent conductive oxide layer 210 would be adversely affected by firing conditions that could cause the transparent conductive oxide layer 210 to become over-oxidized. For example, the silver-containing glass frit may be fired at a temperature below 390° C. so as not to significantly adversely affect the transparent conductive oxide layer 210. However, firing at this relatively low temperature provides relatively high resistivity of the bus bar and poor adhesion to underlying materials in contact with the bus bar, such as transparent conductive oxide layer 202 and substrate 200 (eg, mineral glass material).
[0063] The anti-oxidation layer 302 can help reduce the likelihood that the transparent conductive oxide layer 210 will be significantly adversely affected by the more aggressive firing conditions. Thus, a variety of silver-containing glass frits and firing conditions can be used. A firing temperature of at least 390° C. can be used and provide bus bars with lower resistivity and better adhesion to the underlying material.
[0064] Figure 6 602 and 610 after forming. Certain deposition and firing parameters may depend on the desired characteristics of the bus bars 602 and 610 after firing. The bus bars 602 and 610 may have a maximum of 8.0×10 -6 In another embodiment, the resistivity is at most 6.0×10 -6 Ω*cm, up to 5.0×10 -6 Ω*cm, up to 4.0×10 -6 Ω*cm or up to 3.0×10 -6 Ω*cm. The firing temperature can provide a lower resistivity. The resistivity will be higher than the resistivity of pure silver reported in the chemical handbook, and therefore, the resistivity will be greater than 1.59×10 -8Ω*cm. The thickness of busbars 602 and 610, in combination with resistivity, affects the sheet resistivity. In one embodiment, the thickness of busbars 602 and 610 may be at least 2 microns, at least 7 microns, or at least 12 microns. Although the theoretical upper limit is unknown, the maximum thickness may depend on the application. In another embodiment, the thickness may be at most 80 microns, at most 60 microns, or at most 40 microns. For many applications, the thickness of busbars 602 and 610 is in the range of 12 microns to 40 microns. After reading this specification, a technician will be able to determine the thickness to provide the required or desired electrical properties of busbars 602 and 610.
[0065] The bus bar precursor may be deposited by printing, screen printing, etc. The bus bar precursor may have a thickness sufficient to achieve the desired thickness of the bus bars 602 and 610 after the bus bar precursor is fired. The bus bar precursor thickness may depend on the amount of solvent, resin or other organic or volatile components in the precursor. The bus bar precursor may be deposited to a thickness of 1.1 to 4 times the thickness of the bus bars 602 and 610 after firing. As a non-limiting example, if the bus bars 602 to 610 have a thickness of 20 microns after firing, the bus bar precursor may be deposited to a thickness in the range of 22 microns to 80 microns.
[0066] The busbar precursor can be fired to form busbars 602 and 610. Firing can be performed at one or more temperatures. In one embodiment, if there is any solvent, resin or other organic material in the busbar precursor, the substrate 200 can be heated to a temperature in the range of about 100°C to 350°C to evaporate the solvent, burn off the resin, volatilize any other organic material or any combination thereof. The temperature of the substrate 200 is raised to the sintering temperature to sinter the silver-based glass frit in the busbar precursor. The temperature of the substrate 200 can be at least 390°C, at least 400°C, at least 425°C, at least 450°C or at least 475°C. Since higher temperatures can now be used for sintering, the resistivity of the busbars 602 and 610 can be reduced, and the adhesion to the underlying material can be increased. During firing, the presence of the anti-oxidation layer 302 helps to reduce the possibility that the transparent conductive oxide layer 210 will be significantly adversely affected during firing. Therefore, various environments can be used during firing. In one embodiment, firing can be performed in an inert gas (N2, Ar, etc.), or can include a combination of an inert gas and an oxidizing gas (O2, N2O, etc.). In a specific embodiment, the environment includes air. In another embodiment, firing can be performed in an oxidizing gas without an inert gas. The time during the sintering portion can be in the range of 2 minutes to 120 minutes. The specific time may depend on the composition of the silver-based glass material, and therefore, the provider can provide a recommended time range for the sintering portion of the firing.
[0067] In one embodiment, firing as previously described may be performed as a separate operation, or may occur during a thermal cycle performed for another purpose. Thus, the time at which firing is performed is flexible, allowing the user to more autonomously integrate firing into an existing process flow. Furthermore, different portions of the firing operation may be performed at different points in the process flow. For example, solvent may be evaporated from the busbar precursor, resin may be burned off, any other organic material may be volatilized, or any combination thereof may be performed during a thermal cycle; and sintering may be performed during different thermal cycles. If needed or desired, one or more other process operations may be performed between different thermal cycles.
[0068] The method may also include Figure 1 The finishing operation is performed at block 162 in the embodiment. The specific finishing operation may depend on the specific application. Figure 7 As shown, portions of layers 210, 302, and 402 are removed at opening 702 such that bus bar 602 is not electrically connected to a majority of transparent conductive oxide layer 210. Thus, bus bar 602 is the primary connector for transparent conductive oxide layer 202, and bus bar 610 is the primary connector for transparent conductive oxide layer 210. At this point in the method, electrochromic device 700 is formed. In another embodiment (not shown), bus bar 602 is formed so that it does not contact the sides of the stack within opening 502, as shown in FIG. Figure 5 In this embodiment, no portions of layers 210, 302, and 402 need to be removed.
[0069] In another embodiment, the electrochromic device 700 can be at least a portion of a vehicle window. In vehicle applications, the electrochromic device 700 can be bent or otherwise shaped to conform to the physical shape of the vehicle. The temperature at which the electrochromic device is bent or otherwise shaped can be at a temperature of at least 600°C. In a specific embodiment, the temperature is in the range of 600°C to 700°C. Heat can be applied locally. The anti-oxidation layer 302 can help reduce the possibility of significantly adversely affecting the transparent conductive oxide layer 210 during bending or otherwise forming. The sintering portion of the firing for forming the busbar can be performed during a thermal cycle for bending the electrochromic device.
[0070] In one embodiment, the insulating glass unit 800 may be formed as Figure 8As shown. The electrochromic device 700 can be coupled to a counter substrate 802 that is transparent to visible light. The counter substrate 802 can include tempered or strengthened glass. In a specific embodiment, an adhesive (not shown) can be used between the electrochromic device 700 and the counter substrate 802. The insulating glass unit 800 can also include a glass panel 804, a spacer 822, and a sealing material 824. Similar to the counter substrate 802, the glass panel 804 can also include tempered or strengthened glass. In addition, the glass panel 804 can be part of a laminate that can include a solar control layer, similar to the solar control layer described previously with respect to the substrate 200. The insulating glass unit can include a solar control layer located in the substrate 200 instead of in the glass panel 804, a solar control layer located in the glass panel 804 or attached to the glass panel 804, or can use a solar control layer with each substrate 200 and in the glass panel 804 or attached to the glass panel 804. In this last alternative, the solar control layer can provide different functions. For example, a solar control layer near the exterior of the building can help suppress near infrared radiation, and another solar control layer near the interior of the building can include low-e materials or help suppress ultraviolet radiation. During the sealing operation, an inert gas (e.g., argon, N2, etc.) can fill the gap 806.
[0071] Optionally, after forming the electrochromic device 700, the electrochromic device 700 can be annealed to relieve stress or for other purposes. Annealing can be performed separately from firing. In another embodiment, the sintering portion of the firing can be combined with the annealing operation. The anti-oxidation layer 302 can allow for higher temperatures for annealing, oxidizing environments such as air, or the use of both without significantly adversely affecting the transparent conductive oxide layer 210. Annealing can be performed at a temperature range of 100°C to 600°C.
[0072] Embodiments may provide benefits compared to conventional electrochromic devices. Higher temperatures during the sintering portion of the firing of the busbars allow a wider range of silver-based glass frits to be used. Prior to the present invention, the temperature during firing was limited so that the transparent conductive oxide layer 210 was not highly oxidized. As the firing temperature increases, the likelihood of significantly affecting the transparent conductive oxide increases. When an oxidizing environment is used during firing, the transparent conductive oxide may become over-oxidized and the busbar resistivity will be too high. Silver-based glass frits that will not fully sinter at temperatures below 390°C can now be used. Such silver-based glass frits can provide lower resistivity than silver-based glass frits designed to be sintered at temperatures below 390°C, even when the same sintering temperature is used.
[0073] The ability to use higher temperatures during sintering can allow the busbars to better adhere to the underlying material. The busbars can contact the layers and substrates within the electrochromic stack. In the illustrated embodiment, busbars 602 and 610 contact the transparent conductive oxide layer 202 and substrate 200 at a region away from the electrochromic stack. In a specific embodiment, the transparent conductive oxide layer 202 can be a transparent conductive oxide, and the surface of the substrate 200 contacting the busbars 602 and 610 can be a mineral glass including SiO2. ASTM B905-00 (re-approved) 2010 can be used to test the adhesion of SiO2. In an embodiment using Method A of the ASTM standard, the average adhesion strength to SiO2 is at least 3N, at least 5N, or at least 7N based on 20 measurements. Although there is no theoretical adhesion limit that would be problematic, the average adhesion strength (Method A) may be less than 1000N. Very good adhesion strength can be considered to be at least 15N. Although there is no problematic theoretical adhesion limit, the average adhesion strength (Method A) may be less than 1000N. It is considered that very good bond strength may be at least 15 N. In the examples using method B of the ASTM standard, the average bond strength to SiO2 is at least 3 or at least 4 based on 20 measurements.
[0074] Many different aspects and embodiments are possible. Some of those aspects and embodiments are described below. After reading this specification, those skilled in the art will appreciate that those aspects and embodiments are merely illustrative and do not limit the scope of the present invention. Exemplary embodiments may be based on any one or more of the following listed embodiments.
[0075] Embodiment 1. An electrochromic device, comprising:
[0076] substrate;
[0077] a first transparent conductive oxide layer on the substrate; and
[0078] a first bus bar on the substrate, wherein the first bus bar comprises silver and has:
[0079] Up to 8.0×10 -6 Resistivity in Ω*cm;
[0080] Adhesion strength to SiO2 of at least 3N based on 20 measurements as determined by ASTM B905-00, Method A (reapproved in 2010);
[0081] An average bond strength to SiO2 of at least 3 based on 20 measurements as determined by ASTM B905-00, Method B (reapproved 2010); or
[0082] Its combination.
[0083] Embodiment 2. The electrochromic device according to embodiment 1, further comprising (1) an anti-oxidation layer between the substrate and the first transparent conductive oxide layer or (2) an anti-oxidation layer on the first transparent conductive oxide layer.
[0084] Embodiment 3. A method of forming an electrochromic device, comprising:
[0085] forming a first transparent conductive oxide layer on a substrate;
[0086] forming a bus bar precursor on a substrate, wherein the bus bar precursor comprises silver; and
[0087] The bus bar precursor is fired to form a first bus bar, wherein the firing is performed such that the first bus bar is at a temperature of at least 390°C.
[0088] Embodiment 4. The method according to embodiment 3, further comprising forming an anti-oxidation layer, such that the anti-oxidation layer is (1) between the substrate and the first transparent conductive oxide layer or (2) on the first transparent conductive oxide layer.
[0089] Embodiment 5. The method according to embodiment 3 or 4, wherein the anti-oxidation layer is formed by a sputtering deposition technique.
[0090] Embodiment 6. The method of any one of embodiments 3 to 5, wherein firing the bus bar precursor is performed such that the first bus bar is at a temperature greater than 400°C, at least 425°C, at least 450°C, or at least 475°C.
[0091] Embodiment 7. The method of any one of embodiments 3 to 6, further comprising removing organic material from the bus bar precursor after forming the bus bar precursor on the substrate and before firing the bus bar precursor.
[0092] Embodiment 8. The method of embodiment 7, wherein removing the organic material is performed at a temperature of at most 350°C, at most 325°C, or at most 300°C.
[0093] Embodiment 9. The method according to any one of embodiments 2 to 8, wherein firing the bus bar precursor is performed after forming the first transparent conductive oxide layer.
[0094] Embodiment 10. The method of any one of embodiments 2 to 9, further comprising shaping the electrochromic device after firing the bus bar precursor, wherein the bending is performed at a temperature of at least 600°C.
[0095] Embodiment 11. An electrochromic device or method according to any one of Embodiments 2 and 4 to 9, wherein the anti-oxidation layer comprises silicon nitride, aluminum nitride, titanium nitride, tungsten nitride, tantalum nitride, titanium silicon nitride, tungsten silicon nitride or tantalum silicon nitride.
[0096] Embodiment 12. The electrochromic device or method according to any of the preceding embodiments, wherein the first bus bar has a maximum of 6.0×10 -6 Ω*cm, up to 5.0×10 -6 Ω*cm, up to 4.0×10 -6 Ω*cm or up to 3.0×10 -6 Resistivity of Ω*cm.
[0097] Embodiment 13. The electrochromic device or method according to any of the preceding embodiments, wherein the first bus bar has a current greater than 1.59×10 -8 Resistivity of Ω*cm.
[0098] Embodiment 14. An electrochromic device or method according to any of the preceding embodiments, as determined by Method A of ASTM B905-00 (reapproved in 2010), based on 20 measurements, wherein the average adhesion strength of the first bus bar to SiO2 is at least 3N, at least 5N or at least 7N.
[0099] Embodiment 15. The electrochromic device or method of any of the preceding embodiments, as determined by Method B of ASTM B905-00 (Reapproved 2010), wherein the first bus bar has at least 3 or at least 4 categories.
[0100] Embodiment 16. An electrochromic device or method according to any of the preceding embodiments, wherein the average adhesion strength of the first bus bar to SiO2 is at most 1000 N based on 20 measurements as determined by Method A of ASTM B905-00 (reapproved in 2010).
[0101] Embodiment 17. The electrochromic device or method of any preceding embodiment, wherein the first transparent conductive oxide layer comprises a doped metal oxide.
[0102] Embodiment 18. The electrochromic device or method of any preceding embodiment, wherein the doped metal oxide comprises tin oxide doped with a Group 13 element, zinc oxide doped with a Group 13 element, or any combination thereof.
[0103] Embodiment 19. The electrochromic device or method according to any one of the preceding embodiments, further comprising:
[0104] a first electrode which is an electrochromic electrode or a counter electrode;
[0105] a second electrode, which is the other of the electrochromic electrode or the counter electrode;
[0106] a ceramic electrolyte layer disposed between the first electrode and the second electrode; and
[0107] a second transparent conductive oxide layer which is closer to the second electrode than the first electrode,
[0108] The first transparent conductive oxide layer is closer to the first electrode than the second electrode.
[0109] Embodiment 20. The electrochromic device or method of Embodiment 19, further comprising a second bus bar comprising silver, wherein the first bus bar is electrically connected to the first transparent conductive oxide layer, and the second bus bar is electrically connected to the second transparent conductive oxide layer.
[0110] Embodiment 21. The electrochromic device or method according to any one of the preceding embodiments, further comprising an insulating layer covering the anti-oxidation layer, wherein the insulating layer comprises an oxide.
[0111] Embodiment 22. The electrochromic device or method according to Embodiment 21, further wherein the insulating layer comprises SiO2.
[0112] Embodiment 23. The electrochromic device or method of any preceding embodiment, wherein the substrate comprises up to 1 wt. % alkali metal oxide.
[0113] Embodiment 24. The electrochromic device or method of Embodiment 22, wherein the substrate comprises a mineral glass layer.
[0114] Embodiment 25. The electrochromic device or method of Embodiment 24, wherein the mineral glass layer has a thickness of at most 300 microns.
[0115] Embodiment 26. An electrochromic device or method according to any of the preceding embodiments, wherein the substrate is flexible.
[0116] It should be noted that not all activities described in the general description or examples above are required, a portion of a specific activity may not be required, and one or more other activities in addition to the activities described may be performed. In addition, the order of activities listed is not necessarily the order in which the activities are performed.
[0117] For the sake of clarity, certain features described herein in the context of separate embodiments may also be provided in combination in a single embodiment. Conversely, for the sake of brevity, various features described in the context of a single embodiment may also be provided individually or in any sub-combination. In addition, references to values stated in ranges include every value within the stated range.
[0118] The benefits, other advantages and solutions to problems described above have been described with respect to specific embodiments. However, these benefits, advantages, solutions to problems, and any features that may make any benefit, advantage or solution occur or become more significant should not be construed as key, necessary or essential features of any or all claims.
[0119] The description and the schematic diagram of the embodiments described herein provide an overall understanding of the structure of various embodiments. The description and the illustration are not intended to be used to exhaustively and comprehensively describe all the elements and characteristics of the equipment and system using the structure or method described herein. A separate embodiment may also be provided in combination in a single embodiment, and on the contrary, for the sake of brevity, the various features described in the context of a single embodiment may also be provided separately or in any sub-combination form. In addition, the reference to the value described in the range includes each value within the range. Only after reading this specification, the technician can be aware of many other embodiments. Other embodiments may be used and the embodiments may be derived from the present disclosure, so that structural substitution, logical substitution or another change may be performed without departing from the scope of the present disclosure. Therefore, the present disclosure should be regarded as illustrative rather than restrictive.
Claims
1. An electrochromic device, comprising: substrate; a first bus bar on the substrate, wherein the first bus bar comprises silver and has: Determined by Method A of ASTM B905-00 reapproved in 2010 and based on 20 tests An average bonding strength of at least 3N to SiO2; a first electrode which is an electrochromic electrode or a counter electrode; a second electrode, which is the other of the electrochromic electrode or the counter electrode; a first transparent conductive oxide layer on the substrate; and A second transparent conductive oxide layer is closer to the second electrode than the first electrode. pole, The first bus bar contacts the second transparent conductive oxide layer, the first electrode and the second electrode.
2. The electrochromic device of claim 1, wherein the first bus bar has a classification of at least 4N as measured by Method B of ASTM B905-00, reapproved in 2010.
3. The electrochromic device of claim 1, wherein the average adhesion strength of the first bus bar to SiO2 is at least 5N as determined by Method A of ASTM B905-00 reapproved in 2010 and based on 20 measurements.
4. The electrochromic device of claim 1, wherein the average adhesion strength of the first bus bar to SiO2 is at least 7N as determined by Method A of ASTM B905-00 reapproved in 2010 and based on 20 measurements.
5. The electrochromic device according to claim 1, further comprising: an anti-oxidation layer, wherein the anti-oxidation layer is (1) between the substrate and the first transparent conductive oxide layer or (2) on the first transparent conductive oxide layer. 6 . The electrochromic device of claim 5 , wherein the anti-oxidation layer comprises silicon nitride, aluminum nitride, titanium nitride, tungsten nitride, tantalum nitride, titanium silicon nitride, tungsten silicon nitride, or tantalum silicon nitride.
7. The electrochromic device of claim 1, wherein the first transparent conductive oxide layer comprises a doped metal oxide.
8. The electrochromic device according to claim 1, wherein the first bus bar has a maximum of 6.0×10 -6 Resistivity of Ω*cm.
9. The electrochromic device according to claim 1, wherein the first bus bar has a maximum of 5.0×10 -6 Resistivity of Ω*cm. 10 . The electrochromic device of claim 5 , wherein the first transparent conductive oxide layer is closer to the first electrode than to the second electrode.
11. An electrochromic device comprising: substrate; a first bus bar on the substrate, wherein the first bus bar comprises silver and has: Up to 8.0×10 -6 Resistivity in Ω*cm, a first electrode which is an electrochromic electrode or a counter electrode; a second electrode, which is the other of the electrochromic electrode or the counter electrode; a first transparent conductive oxide layer on the substrate; and a second transparent conductive oxide layer, which is closer to the second electrode than to the first electrode, The first bus bar contacts the second transparent conductive oxide layer, the first electrode and the second electrode.
12. The electrochromic device according to claim 11, further comprising: an anti-oxidation layer, wherein the anti-oxidation layer is (1) between the substrate and the first transparent conductive oxide layer or (2) on the first transparent conductive oxide layer.
13. The electrochromic device of claim 12, wherein the anti-oxidation layer comprises silicon nitride, aluminum nitride, titanium nitride, tungsten nitride, tantalum nitride, titanium silicon nitride, tungsten silicon nitride, or tantalum silicon nitride.
14. The electrochromic device of claim 12, wherein the first transparent conductive oxide layer comprises a doped metal oxide.
15. The electrochromic device of claim 14, wherein the doped metal oxide comprises tin oxide doped with a Group 13 element, zinc oxide doped with a Group 13 element, or any combination thereof.