Film and method for preparing the same

By introducing hydrocarbon resin into the polyethylene film, the problem of high friction coefficient of the polyethylene film is solved when improving the toughness performance, achieving a lower friction coefficient and higher toughness performance, adapting to a variety of application needs.

CN114269829BActive Publication Date: 2024-10-01EXXONMOBIL CHEMICAL PATENTS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080058449.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-08-20
Filing Date
2020-06-17
Publication Date
2024-10-01
Estimated Expiration
2040-06-17

AI Technical Summary

Technical Problem

While existing polyethylene films have improved toughness properties, they have a high coefficient of friction (COF), which leads to adverse performance conflicts in some applications. They also rely heavily on slip agents, which affects the design and application of the films.

Method used

A specific amount of hydrocarbon resin, such as aliphatic, aromatic or hydrogenated hydrocarbon resin, is introduced into the polyethylene film to form a suitable film structure to improve the tear resistance and falling dart impact performance of the film while reducing the friction coefficient.

Benefits of technology

By introducing hydrocarbon resins, the friction coefficient of the film is significantly reduced, toughness-related properties such as Elmendorf tear height and falling dart impact properties are improved, achieving better performance distribution and reducing the reliance on slip agents. , adapt to different application needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003510120010000271
    Figure BDA0003510120010000271
Patent Text Reader

Abstract

Disclosed are films and methods of making such films, the films comprising a first polyethylene and a hydrocarbon resin that can provide improved friction properties. The hydrocarbon resin can be incorporated in neat form or as a blend, for example, with a second polyethylene, which can be the same as or different from the first polyethylene.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of U.S. Provisional Application No. 62 / 889,322, filed on August 20, 2019, entitled “Polyethylene Blend Film Compositions Comprising Hydrocarbon Resin (Oppera) with improved Toughness and Coefficient of Friction,” the entirety of which is incorporated herein by reference. Field of the Invention

[0003] The present invention relates to films, and in particular to films comprising polyethylene and a hydrocarbon resin, and methods of making such films. Background of the Invention

[0005] Coextrusion blown films are widely used in various packaging and other applications. Film properties are often affected by the combined effects of coextrusion process conditions and the polymer composition selected for the different layers. In order to address the needs of specific end uses, film producers will need to emphasize certain properties accordingly while maintaining a well-balanced overall performance profile without having to pursue one property at the expense of another property.

[0006] Particularly packaging applications require films with good toughness properties, so as to prevent film failure due to being damaged by tearing, falling darts, puncturing or yielding under stress. Among all polymers for coextrusion blown films, ethylene polymers (such as those prepared by gas phase process by Ziegler-Natta catalyst) and blends thereof are easily obtained with low manufacturing costs, sufficient to prove the rationality of commercial applications. Recently, metallocene polyethylene (mPE) (it is also known to have the versatility of expansion and the potential for reducing thickness) has also been introduced into the film and increased in the film to further enhance the mechanical properties related to toughness. However, the maximum achievable restriction with the currently available selection of ethylene polymers seems to have been reached in many specific applications, and "pure" polyethylene solutions tend to weaken other properties generally. For example, the film made of mPE characterized by enhanced toughness performance shows an unfavorable friction coefficient (COF) in the absence of a slip agent. Therefore, film producers have faced such a challenge, namely by easily changing existing solutions to overcome such conflicts between toughness-related performance and COF, to enhance COF while preventing the significant loss of toughness performance or even allowing further improvement of toughness performance.

[0007] Applicants have discovered that the aforementioned objectives can be achieved by applying a specific amount of hydrocarbon resins as described herein in polyethylene films, especially polyethylene films having a monolayer structure. The presence of hydrocarbon resins can result in a significant reduction in COF, with an increase in toughness-related properties including tear resistance and dart impact. Thus, film producers can get rid of the limitations of achievable toughness-related properties and the heavy reliance on slip agents to reduce friction on the film surface, and can instead benefit from the convenience and flexibility of film design to better accommodate properties that used to conflict with each other. SUMMARY OF THE INVENTION

[0009] Films comprising polyethylene and a hydrocarbon resin, and methods for making such films are provided.

[0010] In one embodiment, the present invention encompasses a film comprising a layer comprising: (a) a first polyethylene having (i) a density of about 0.900 to about 0.925 g / cm 3 (ii) Melt index (MI) 2.16 is about 0.1 to about 10.0 g / 10 min, (iii) melt index ratio (MIR) I 21.6 / I 2.16 is about 15 to about 50, (iv) a weight average molecular weight (M w ) is from about 20,000 to about 200,000, (v) a molecular weight distribution (MWD) is from about 2.0 to about 5.0, and (vi) a z-average molecular weight (M z ) and weight average molecular weight (M w )(M z / M w ) ratio of about 1.7 to about 3.5; and (b) about 5 to about 20 weight percent of a hydrocarbon resin, based on the total weight of the polymer in the layer, the hydrocarbon resin comprising an aliphatic hydrocarbon resin, a hydrogenated aliphatic hydrocarbon resin, an aromatic hydrocarbon resin, a hydrogenated aromatic hydrocarbon resin, an alicyclic hydrocarbon resin, a hydrogenated alicyclic hydrocarbon resin, a polyterpene resin, a terpene phenolic resin, a rosin ester resin, a rosin acid resin, or a combination thereof.

[0011] In another embodiment, the present invention is directed to a method for preparing a film comprising the steps of: (a) preparing a layer comprising: (i) a first polyethylene having (i) a density of about 0.900 to about 0.925 g / cm 3 (ii) MI,I 2.16 is about 0.1 to about 10.0 g / 10 min, (iii) MIR, I 21.6 / I 2.16 is about 15 to about 50, (iv) a weight average molecular weight (M w ) is from about 20,000 to about 200,000, (v) MWD is from about 2.0 to about 5.0, and (vi) z-average molecular weight (Mz ) and weight average molecular weight (M w )(M z / M w ) ratio of about 1.7 to about 3.5; and (ii) about 5 to about 20 weight percent of a hydrocarbon resin, based on the total weight of the polymer in the layer, the hydrocarbon resin comprising an aliphatic hydrocarbon resin, a hydrogenated aliphatic hydrocarbon resin, an aromatic hydrocarbon resin, a hydrogenated aromatic hydrocarbon resin, an alicyclic hydrocarbon resin, a hydrogenated alicyclic hydrocarbon resin, a polyterpene resin, a terpene phenolic resin, a rosin ester resin, a rosin acid resin, or a combination thereof; and (b) forming a film comprising the layer in step (a).

[0012] Films described herein or made according to any of the methods disclosed herein can have at least one of the following properties: (i) at least about 15% higher Elmendorf Tear in the machine direction (MD), (ii) at least about 25% higher Elmendorf Tear in the cross-machine direction (TD), (iii) at least about 4% higher dart drop impact, (iv) at least about 3% lower static coefficient of friction (COF), and (v) at least about 40% lower dynamic COF, compared to the properties of a film that does not contain a hydrocarbon resin but is otherwise identical in film formulation, thickness, and structure.

[0013] DETAILED DESCRIPTION OF THE INVENTION

[0014] Various specific embodiments, variations of the present invention will now be described, including exemplary embodiments and definitions adopted therein. Although the following detailed description gives specific exemplary embodiments, it will be appreciated by those skilled in the art that these embodiments are merely exemplary, and that the present invention may be implemented in other ways. Any reference to the "invention" may refer to one or more, but not necessarily all, of the present invention as defined by the claims. The use of titles is merely for convenience and does not limit the scope of the present invention.

[0015] As used herein, "polymer" can be used to refer to homopolymers, copolymers, interpolymers, terpolymers, etc. "Polymer" has two or more identical or different monomer units. "Homopolymer" is a polymer with the same monomer unit. "Copolymer" is a polymer with two or more monomer units that are different from each other. "Terpolymer" is a polymer with three monomer units that are different from each other. The term "different" as used to refer to monomer units indicates that the monomer units differ from each other by at least one atom or are isomerically different. Therefore, as used herein, the definition of copolymer includes terpolymers, etc. Similarly, as used herein, the definition of polymer includes copolymers, etc. Therefore, as used herein, the terms "polyethylene", "ethylene polymer", "ethylene copolymer" and "ethylene-based polymer" mean a polymer or copolymer containing at least 50 mol% ethylene units (preferably at least 70 mol% ethylene units, more preferably at least 80 mol% ethylene units, even more preferably at least 90 mol% ethylene units, even more preferably at least 95 mol% ethylene units or 100 mol% ethylene units (in the case of homopolymers)). In addition, the term "polyethylene composition" means a composition containing one or more polyethylene components.

[0016] As used herein, when a polymer is referred to as comprising a monomer, the monomer is present in the polymer in the polymerized form of the monomer or in the form of a derivative of the monomer.

[0017] As used herein, when a polymer is said to contain a certain percentage (weight %) of a monomer, the percentage of the monomer is based on the total amount of monomer units in the polymer.

[0018] For the purposes of this invention and the claims thereto, a carbon steel having a density of 0.910 to 0.940 g / cm 3 Ethylene polymers are called "low density polyethylene" (LDPE); having a density of 0.890 to 0.930 g / cm 3 , usually 0.910-0.930g / cm 3 , ethylene polymers that are linear and do not contain a large amount of long chain branching are called "linear low density polyethylene" (LLDPE) and can be produced using conventional Ziegler-Natta catalysts, vanadium catalysts or using metallocene catalysts in gas phase reactors, high pressure tubular reactors and / or in slurry reactors and / or using any disclosed catalyst in solution reactors ("linear" means that the polyethylene has no or only very few long chain branches, usually referred to as g'vis is above 0.97, preferably above 0.98); and having a density greater than 0.940 g / cm 3 Ethylene polymers are called "high-density polyethylene" (HDPE).

[0019] As used herein, "first" polyethylene and "second" polyethylene are merely identifiers used for convenience and should not be construed as limiting the individual polyethylenes, their relative order, or the number of polyethylene polymers used, unless otherwise specified herein.

[0020] As used herein, a structure or composition "free of" a component refers to a structure or composition that is substantially free of the component, or that contains the component in an amount less than about 0.01% by weight of the total structure or composition.

[0021] Hydrocarbon resin

[0022] In one aspect of the invention, the film described herein may include a hydrocarbon resin in the layer. Suitable hydrocarbon resins include, but are not limited to, aliphatic hydrocarbon resins, at least partially hydrogenated aliphatic hydrocarbon resins, aliphatic / aromatic hydrocarbon resins, at least partially hydrogenated aliphatic aromatic hydrocarbon resins, aromatic resins, at least partially hydrogenated aromatic hydrocarbon resins, alicyclic hydrocarbon resins, at least partially hydrogenated alicyclic resins, alicyclic / aromatic hydrocarbon resins, alicyclic / aromatic at least partially hydrogenated hydrocarbon resins, polyterpene resins, terpene phenolic resins, rosin esters, rosin acids, grafted resins, and a mixture of two or more of the foregoing. Hydrocarbon resins may be polar or non-polar.

[0023] In one embodiment, the hydrocarbon resins available herein are produced by the thermal polymerization of cyclopentadiene (CPD) or substituted CPD, which may also include aliphatic or aromatic monomers as described later. The hydrocarbon resin may be a non-aromatic resin or an aromatic resin. The hydrocarbon resin may have an aromatic content between 0% by weight and 60% by weight, or between 1% by weight and 60% by weight, or between 1% by weight and 40% by weight, or between 1% by weight and 20% by weight, or between 10% by weight and 20% by weight. Alternatively or additionally, the hydrocarbon resin may have an aromatic content between 15% by weight and 20% by weight, or between 1% by weight and 10% by weight, or between 5% by weight and 10% by weight. Preferred aromatic compounds that may be in the hydrocarbon resin include one or more of styrene, indene, derivatives of styrene, and derivatives of indene. Particularly preferred aromatic olefins include styrene, alpha-methylstyrene, beta-methylstyrene, indene, and methylindene, and vinyltoluene. Styrene components include styrene, styrene derivatives, and substituted styrene. Typically, the styrenic component does not include fused rings such as indenics.

[0024] In another embodiment, hydrocarbon resins useful herein are produced by catalytic (cationic) polymerization of linear dienes. Such monomers are primarily derived from steam cracked naphtha (SCN) and include C5 dienes such as piperylene (also known as 1,3-pentadiene). Polymerizable aromatic monomers can also be used to produce resins and can be relatively pure, such as styrene, -methylstyrene, or from C9-aromatic SCN streams. Such aromatic monomers can be used alone or together with the linear dienes described above. "Natural" monomers can also be used to produce resins, such as terpenes such as α-pinene or β-carene, either alone or with other polymerizable monomers in high or low concentrations. Typical catalysts for the preparation of these resins are AlCl3 and BF3, either alone or complexed. Monoolefin modifiers such as 2-methyl, 2-butene can also be used to control the MWD of the final resin. The final resin can be partially or completely hydrogenated.

[0025] In another embodiment, hydrocarbon resin can be at least partially hydrogenated or hydrogenated in large quantities. As used herein, "at least partially hydrogenated" means that the material contains less than 90% olefinic protons, or less than 75% olefinic protons, or less than 50% olefinic protons, or less than 40% olefinic protons, or less than 25% olefinic protons, such as 20%-50% olefinic protons. As used herein, "hydrogenated in large quantities" means that the material contains less than 5% olefinic protons, or less than 4% olefinic protons, or less than 3% olefinic protons, or less than 2% olefinic protons, such as 1%-5% olefinic protons. Hydrogenation is usually carried out to such an extent that the hydrogenation of aromatic bonds is minimized and avoided.

[0026] In yet another embodiment, the hydrocarbon resin may contain one or more oligomers such as dimers, trimers, tetramers, pentamers and hexamers. The oligomers may be derived from petroleum distillates boiling in the range of 30°C to 210°C. The oligomers may be derived from any suitable process and are often derived as a by-product of resin polymerization. Suitable oligomer streams may have M n Between 130 and 500, or between 130 and 410, or between 130 and 350, or between 130 and 270, or between 200 and 350, or between 200 and 320. Examples of suitable oligomer streams include, but are not limited to, oligomers of cyclopentadiene and substituted cyclopentadiene, oligomers of C4-C6 conjugated dienes, C8-C 10 Oligomers of aromatic olefins, and combinations thereof. Other monomers may be present. These include C4-C6 monoolefins and terpenes. The oligomers may contain one or more aromatic monomers and may be at least partially hydrogenated or substantially hydrogenated.

[0027] Preferably, hydrocarbon resin comprises dicyclopentadiene, cyclopentadiene and methylcyclopentadiene derived content is about 60 weight % to about 100 weight % of the total weight of hydrocarbon resin. In any embodiment, hydrocarbon resin can have dicyclopentadiene, cyclopentadiene and methylcyclopentadiene derived content is about 70 weight % to about 95 weight % of the total weight of hydrocarbon resin, or about 80 weight % to about 90 weight % or about 95 weight % to about 99 weight %. Preferably, hydrocarbon resin can be a hydrocarbon resin including dicyclopentadiene derived unit in a major part. The term "dicyclopentadiene derived unit", "dicyclopentadiene derived content" etc. refers to the dicyclopentadiene monomer (i.e., unreacted compound in the form before polymerization) used to form polymer, and can also refer to the monomer after it has been incorporated into the polymer, which usually has less hydrogen atoms than before polymerization due to polymerization.

[0028] Preferred hydrocarbon resins may have a dicyclopentadiene derived content of about 50% to about 100% by weight of the total weight of the hydrocarbon resin, more preferably about 60% to about 100% by weight of the total weight of the hydrocarbon resin, and even more preferably about 70% to about 100% by weight of the total weight of the hydrocarbon resin. Thus, in any embodiment, a suitable hydrocarbon resin may have a dicyclopentadiene derived content of about 50% or more, or about 60% or more, or about 70% or more, or about 75% or more, or about 90% or more, or about 95% or more, or about 99% or more of the total weight of the hydrocarbon resin.

[0029] Useful hydrocarbon resins may include up to 5 wt % indenyl components, or up to 10 wt % indenyl components. Indenyl components include indene and derivatives of indene. Often, hydrocarbon resins include up to 15 wt % indenyl components. Alternatively, hydrocarbon resins are substantially free of indenyl components.

[0030] Preferred hydrocarbon resins have a melt viscosity of 300-800 centipoise (cPs) at 160° C., or more preferably 350-650 cPs at 160° C. Preferably, the melt viscosity of the hydrocarbon resin is 375-615 cPs at 160° C., or 475-600 cPs at 160° C. The melt viscosity can be measured by a Brookfield viscometer with a "J" type spindle according to ASTM D 6267.

[0031] Suitable hydrocarbon resins have M w In any embodiment, the hydrocarbon resin may have an M w The preferred hydrocarbon resins have a weight average molecular weight of about 800 to about 1000 g / mole. Suitable hydrocarbon resins may have a molecular weight of about 600 to about 1400 g / mole, or about 800 g / mole to about 1200 g / mole. nThe hydrocarbon resin may have a molecular weight of about 300 to about 800 g / mole, or about 400 to about 700 g / mole, or more preferably about 500 to about 600 g / mole. z In any embodiment, suitable hydrocarbon resins may have M w / M n 4 or less, preferably 1.3-1.7.

[0032] Preferred hydrocarbon resins have a glass transition temperature (T g ) is about 30°C to about 200°C, or about 0°C to about 150°C, or about 50°C to about 160°C, or about 50°C to about 150°C, or about 50°C to about 140°C, or about 80°C to about 100°C, or about 85°C to about 95°C, or about 40°C to about 60°C, or about 45°C to about 65°C. Preferably, suitable hydrocarbon resins have a T g It is about 60° C. to about 90° C. DSC is used to measure the glass transition temperature at 10° C. / min.

[0033] Specific examples of commercially available hydrocarbon resins include Oppera TM PR 100, 100A, 100N, 101, 102, 103, 104, 105, 106, 111, 112, 115 and 120 materials and Oppera TM PR 131 hydrocarbon resin (all available from ExxonMobil Chemical Company), ARKON TM M90, M100, M115 and M135 and SUPER ESTER TM Rosin esters (available from Arakawa Chemical Company, Japan), SYLVARES TM Phenol-modified styrene- and methylstyrene resins, styrenated terpene resins, ZONATAC terpene-aromatic resins and terpene phenolic resins (available from Arizona Chemical Company), SYLVATAC TM and SYLVALITE TM Rosin esters (available from Arizona Chemical Company), NORSOLENE TM Aliphatic aromatic resin (available from Cray Valley, France), DERTOPHENE TM Terpene phenolic resin (available from DRT Chemical Company, Landes, France), EASTOTAC TM Resin, PICCOTACTTM C5 / C9 resin, REGALITE TM REGALREZ TM AROMATIC AND REGALITE TM Cycloaliphatic / aromatic resins (available from Eastman Chemical Company, Kingsport, Tennessee), WINGTACK TM ET and EXTRA (available from Goodyear Chemical Company), FORAL TM 、PENTALYN TM and PERMALYN TM Rosin and rosin esters (available from Hercules (now Eastman Chemical Company)), QUINTONE TM Acid-modified C5 resin, C5 / C9 resin, and acid-modified C5 / C9 resin (available from Nippon Zeon, Japan) and LX TM Mixed aromatic / cycloaliphatic resins (available from Neville Chemical Company), CLEARON hydrogenated terpene aromatic resins (available from Yasuhara) The foregoing examples are illustrative only and are in no way limiting.

[0034] These commercially available compounds typically have a ring and ball softening point (measured according to ASTM E-28 (1996 revised edition)) of about 10°C to about 200°C, more preferably about 50°C to about 180°C, more preferably about 80°C to about 175°C, more preferably about 100°C to about 160°C, more preferably about 110°C to about 150°C, and more preferably about 125°C to about 140°C, wherein any upper limit and any lower limit of the softening point can be combined into a preferred softening point range. For hydrocarbon resins, a convenient approach is the ring and ball softening point determined according to ASTM E-28.

[0035] In one embodiment, the hydrocarbon resin is present in an amount of about 5 to about 20% by weight, such as about 5%, about 5.5%, about 6%, about 6.5%, about 7%, about 7.5%, about 8%, about 8.5%, about 9%, about 9.5%, about 10%, about 10.5%, about 11%, about 11.5%, about 12%, about 12.5%, about 13%, about 13.5%, about 14%, about 15%, about 16%, about 17%, about 18%, about 19%, about 20%, about 21%, about 22%, about 23%, about 24%, about 25%, about 26%, about 27%, about 28%, about 29%, about 30%, about 31%, about 32%, about 33%, about 34%, about 35%, about 36%, about 37%, about 38%, about 39%, %, about 14 wt %, about 14.5 wt %, about 15 wt %, about 15.5 wt %, about 16 wt %, about 16.5 wt %, about 17 wt %, about 17.5 wt %, about 18 wt %, about 18.5 wt %, about 19 wt %, about 19.5 wt %, about 20 wt %, or in an amount within the range of any combination of values ​​recited herein, based on the total weight of polymer in that layer.

[0036] The hydrocarbon resins described herein may be optionally pre-blended with one or more polyethylene polymers described herein or other polymers miscible with the polyethylene polymers as described herein, and then blended with the polyethylene to form the polymer composition in the layer. Frequently, the pre-blend may contain the hydrocarbon resin, ranging from a lower limit of about 10 wt %, 20 wt %, about 30 wt %, about 40 wt %, about 50 wt %, about 60 wt %, or about 70 wt % to an upper limit of about 90 wt %, about 80 wt %, about 70 wt %, about 60 wt %, about 50 wt %, or about 40 wt %, for example, about 10 wt %, about 20 wt %, about 30 wt %, about 40 wt %, about 50 wt %, about 60 wt %, about 70 wt %, about 80 wt %, or about 90 wt %, based on the total weight of the pre-blend, or in any range between two values ​​as described above, as long as the lower limit is less than the upper limit. Alternatively, the hydrocarbon resin described herein is provided in neat form (ie, without being blended with any other polymer) in a layer of the film prior to being blended with the polyethylene described herein to form the polymer composition in the layer.

[0037] Polyethylene polymer

[0038] In one aspect of the invention, the polyethylene that can be used for the film made according to the method described herein is selected from ethylene homopolymers, ethylene copolymers and their compositions. Available copolymers also contain one or more comonomers in addition to ethylene and can be random copolymers, statistical copolymers, block copolymers and / or their compositions. The method for preparing polyethylene is not critical because it can be prepared by slurry, solution, gas phase, high pressure or other suitable methods, and by using catalyst systems suitable for polyethylene polymerization such as Ziegler-Natta type catalysts, chromium catalysts, metallocene type catalysts, other suitable catalyst systems or their combinations, or by free radical polymerization. In an exemplary embodiment, polyethylene is prepared by the catalysts, activators and methods described in U.S. Patent Nos. 6,342,566; 6,384,142; and 5,741,563; and WO 03 / 040201 and WO 97 / 019991. Such catalysts are well known in the art and are described, for example, in ZIEGLER CATALYSTS (Gerhard Fink, Rolf Mülhaupt and Hans H. Brintzinger, eds., Springer-Verlag 1995); Resconi et al.; and I, II METALLOCENE-BASED POLYOLEFINS (Wiley & Sons 2000).

[0039] Polyethylenes useful in the present invention include those sold under the trade name ENABLE TM 、EXACT TM 、EXCEED TM 、ESCORENE TM 、EXXCO TM 、ESCOR TM 、PAXON TM and OPTEMA TM (ExxonMobil Chemical Company, Houston, Texas, USA), DOW TM 、DOWLEX TM ELITE TM 、AFFINITY TM ENGAGE TM and FLEXOMER TM (The Dow Chemical Company, Midland, Michigan, USA), BORSTAR TM and QUEO TM (Borealis AG, Vienna, Austria) and TAFMER TM (Mitsui Chemicals Inc., Tokyo, Japan).

[0040] Preferred ethylene homopolymers and copolymers useful in the present invention generally have one or more of the following properties:

[0041] 1.M w 20,000 g / mol or greater, 20,000 to 2,000,000 g / mol, preferably 30,000 to 1,000,000, preferably 40,000 to 200,000, preferably 50,000 to 750,000, as measured using gel permeation chromatography ("GPC") according to the procedures disclosed herein; and / or

[0042] 2.T m 30°C to 150°C, preferably 30°C to 140°C, preferably 50°C to 140°C, more preferably 60°C to 135°C, as determined by secondary melting curve based on ASTM D3418; and / or

[0043] 3. A crystallinity of 5% to 80%, preferably 10% to 70%, more preferably 20% to 60%, preferably at least 30%, or at least 40%, or at least 50%, as determined by the enthalpy of the crystallization curve based on ASTM D3418 and calculated by the following formula:

[0044] Crystallinity % = enthalpy (J / g) / 298 (J / g) × 100%;

[0045] Wherein 298 (J / g) is the enthalpy of 100% crystalline polyethylene; and / or

[0046] 4. A heat of fusion of 300 J / g or less, preferably 1 to 260 J / g, preferably 5 to 240 J / g, preferably 10 to 200 J / g, as determined based on ASTM D3418-03; and / or

[0047] 5. Crystallization temperature (T c ) is 15°C to 130°C, preferably 20°C to 120°C, more preferably 25°C to 110°C, preferably 60°C to 125°C, as determined based on ASTM D3418-03; and / or

[0048] 6. a heat deflection temperature of 30°C to 120°C, preferably 40°C to 100°C, more preferably 50°C to 80°C, as measured on injection molded flexure bars based on ASTM D648 at a load of 66 psi (455 kPa); and / or

[0049] 7. A Shore hardness (D scale) of 10 or greater, preferably 20 or greater, preferably 30 or greater, preferably 40 or greater, preferably 100 or less, preferably 25-75 (as measured based on ASTM D 2240); and / or

[0050] 8. The percent amorphous content is at least 50%, preferably at least 60%, preferably at least 70%, more preferably between 50% and 95%, or 70% or less, preferably 60% or less, preferably 50% or less, as determined by subtracting the percent crystallinity from 100.

[0051] The polyethylene may be an ethylene homopolymer such as HDPE. In one embodiment, the ethylene homopolymer has a molecular weight distribution (M w / M n ) or (MWD) is up to 40, preferably in the range of 1.5-20, or 1.8-10, or 1.9-5, or 2.0-4. In another embodiment, the 1% secant flexural modulus of the polyethylene (determined based on ASTM D790A, wherein the test specimen geometry is as specified in the "Molding Materials (Thermoplastics and Thermosets)" section of ASTM D790, and the support span is 2 inches (5.08 cm)) falls within the range of 200 to 1000 MPa, and 300-800 MPa in another embodiment, and 400-750 MPa in yet another embodiment, wherein the desired polymer may exhibit any combination of any upper flexural modulus limit with any lower flexural modulus limit. The preferred MI of the ethylene homopolymer ranges from 0.05 to 800 dg / min in one embodiment, and from 0.1 to 100 dg / min in another embodiment, as measured based on ASTM D1238 (190°C, 2.16 kg).

[0052] In exemplary embodiments, the polyethylene comprises less than 20 mol% propylene units (preferably less than 15 mol%, preferably less than 10 mol%, preferably less than 5 mol%, and preferably 0 mol% propylene units).

[0053] In another embodiment of the invention, ethylene and optionally α-olefins are used to form a di(normal) 3-4 The polyethylenes useful herein are produced by polymerization of a cyclopentadienyl) hafnium compound as a catalyst with a transition metal component, wherein the transition metal component preferably comprises from about 95 mol % to about 99 mol % of a hafnium compound, as further described in U.S. Pat. No. 9,956,088.

[0054] In another embodiment of the present invention, polyethylene is ethylene and one or more selected from C3-C 20 α-olefins, usually C3-C 10Preferably, the comonomer is present in 0.1 wt % to 50 wt % of the copolymer in one embodiment, and 0.5 wt % to 30 wt % in another embodiment, and 1 wt % to 15 wt % in yet another embodiment, and 0.1 wt % to 5 wt % in yet another embodiment, wherein the desired copolymer comprises ethylene and C3-C4 O in any combination of any upper wt % limit with any lower wt % limit described herein. 20 Preferably, the ethylene copolymer will have a weight average molecular weight of greater than 8,000 g / mol in one embodiment, and greater than 10,000 g / mol in another embodiment, and greater than 12,000 g / mol in yet another embodiment, and greater than 20,000 g / mol in yet another embodiment, and less than 1,000,000 g / mol in yet another embodiment, and less than 800,000 g / mol in yet another embodiment, wherein the desired copolymer may comprise any upper molecular weight limit with any lower molecular weight limit described herein.

[0055] In another embodiment, the ethylene copolymer comprises ethylene and one or more other monomers selected from C3-C 20 Linear, branched or cyclic monomers, and in some embodiments C3-C 12 Linear or branched α-olefins, preferably butene, pentene, hexene, heptene, octene, nonene, decene, dodecene, 4-methyl-pentene-1, 3-methylpentene-1, 3,5,5-trimethyl-hexene-1, etc. The monomer may be present in an amount of up to 50 wt%, preferably up to 40 wt%, more preferably from 0.5 wt% to 30 wt%, more preferably from 2 wt% to 30 wt%, more preferably from 5 wt% to 20 wt%, based on the total weight of the ethylene copolymer.

[0056] Preferred linear α-olefins that can be used as comonomers of the ethylene copolymers useful in the present invention include C3-C8 α-olefins, more preferably 1-butene, 1-hexene and 1-octene, even more preferably 1-hexene. Preferred branched α-olefins include 4-methyl-1-pentene, 3-methyl-1-pentene, 3,5,5-trimethyl-1-hexene and 5-ethyl-1-nonene. Preferred monomers containing aromatic groups contain up to 30 carbon atoms. Suitable monomers containing aromatic groups contain at least one aromatic structure, preferably 1-3, more preferably phenyl, indenyl, fluorenyl or naphthyl structural parts. The monomer containing aromatic groups also contains at least one polymerizable double bond, so that after polymerization, the aromatic structure will be pendant to the polymer backbone. The monomer containing aromatic groups can also be further substituted by one or more hydrocarbyl groups, and the hydrocarbyl groups include but are not limited to C1-C 10Alkyl groups. In addition, two adjacent substituents may be joined to form a ring structure. Preferred aromatic group-containing monomers contain at least one aromatic structure attached to a polymerizable olefinic moiety. In particular, preferred aromatic monomers include styrene, α-methylstyrene, p-alkylstyrene, vinyltoluene, vinylnaphthalene, allylbenzene and indene, especially styrene, p-methylstyrene, 4-phenyl-1-butene and allylbenzene.

[0057] Preferred diene monomers useful in the present invention include any hydrocarbon structure having at least two unsaturated bonds, preferably C4-C 30 , wherein at least two of the unsaturated bonds are readily incorporated into the polymer by stereoregular or non-stereoregular catalysts (one or more). It is also preferred that the diene monomers are selected from α,ω-diene monomers (i.e., divinyl monomers). More preferably, the diene monomers are linear divinyl monomers, most preferably those containing 4-30 carbon atoms. Examples of preferred dienes include butadiene, pentadiene, hexadiene, heptadiene, octadiene, nonadiene, decadiene, undecadiene, dodecadiene, tridecadiene, tetradecadiene, pentadecadiene, hexadecadiene, heptadecadiene, octadecadiene, nonadecadiene, eicosadiene, heneicosadiene, docosadiene, tricosadiene, tetracosadiene, pentacosadiene, hexacosadiene, heptacosadiene, octacosadiene, nonacosadiene, triacontadiene, and particularly preferred dienes include 1,6-heptadiene, 1,7-octadiene, 1,8-nonadiene, 1,9-decadiene, 1,10-undecadiene, 1,11-dodecadiene, 1,12-tridecadiene, 1,13-tetradecadiene, and low molecular weight polybutadiene (Mw less than 1000 g / mol). Preferred cyclic dienes include cyclopentadiene, vinyl norbornene, norbornadiene, ethylidene norbornene, divinylbenzene, dicyclopentadiene or higher ring containing dienes with or without substituents at various ring positions.

[0058] In an exemplary embodiment, one or more dienes are present in the polyethylene at up to 10 wt%, preferably at 0.00001 wt% to 2 wt%, preferably 0.002 wt% to 1 wt%, even more preferably 0.003 wt% to 0.5 wt%, based on the total weight of the polyethylene. In some embodiments, the diene is added to the polymerization in an amount from an upper limit of 500 ppm, 400 ppm or 300 ppm to a lower limit of 50 ppm, 100 ppm or 150 ppm.

[0059] Preferred ethylene copolymers useful herein are preferably those comprising at least 50 wt% ethylene and having up to 50 wt%, preferably from 1 wt% to 35 wt%, even more preferably from 1 wt% to 6 wt% of C3-C 20Copolymers of comonomers, preferably C4-C8 comonomers, preferably hexene or octene, based on the weight of the copolymer. Preferably, the polymers are metallocene polyethylenes (mPE).

[0060] Useful mPE homopolymers or copolymers can be produced using mono- or bis-cyclopentadienyl transition metal catalysts in conjunction with activators of aluminoxanes and / or non-coordinating anions in solution, slurry, high pressure or gas phase. The catalyst and activator can be supported or unsupported, and the cyclopentadienyl ring can be substituted or unsubstituted.

[0061] In one embodiment, the films described herein comprise a first polypropylene (being a polyethylene as defined herein) in a layer having (i) a density of about 0.900 to about 0.925 g / cm 3 (ii) MI,I 2.16 is about 0.1 to about 10.0 g / 10 min, (iii) MIR, I 21.6 / I 2.16 is about 15 to about 50, (iv) a weight average molecular weight (M w ) is from about 20,000 to about 200,000, (v) MWD is from about 2.0 to about 5.0, and (vi) z-average molecular weight (M z ) and weight average molecular weight (M w )(M z / M w ) ratio is about 1.7 to about 3.5.

[0062] In another embodiment, the first polyethylene is prepared by using ethylene with a di(normal C 3-4 The invention is produced by gas phase polymerization of an alkylcyclopentadienyl) hafnium compound as a catalyst of a transition metal component, wherein the transition metal component comprises from about 95 mol % to about 99 mol % of the hafnium compound.

[0063] The polyethylene polymer that can be used as the first polyethylene in the film described herein comprises from 70.0mol% to or 100.0mol% of the unit derived from ethylene. The lower limit of the ethylene content range can be from 70.0mol%, 75.0mol%, 80.0mol%, 85.0mol%, 90.0mol%, 92.0mol%, 94.0mol%, 95.0mol%, 96.0mol%, 97.0mol%, 98.0mol% or 99.0mol%, based on the mol% of the polymer unit derived from ethylene. The polyethylene polymer can have an upper limit of 80.0mol%, 85.0mol%, 90.0mol%, 92.0mol%, 94.0mol%, 95.0mol%, 96.0mol%, 97.0mol%, 98.0mol%, 99.0mol%, 99.5mol% or 100.0mol%, based on the polymer unit derived from ethylene. For polyethylene copolymers, the polyethylene polymer may have less than 50.0 mol% of C3-C 20 Polymer units of olefins, preferably α-olefins such as hexene or octene. 20 The lower limit of the olefin content range may be 25.0 mol%, 20.0 mol%, 15.0 mol%, 10.0 mol%, 8.0 mol%, 6.0 mol%, 5.0 mol%, 4.0 mol%, 3.0 mol%, 2.0 mol%, 1.0 mol% or 0.5 mol%, based on the olefin content derived from C3-C 20 Polymer units of olefins. C3-C 20 The upper limit of the olefin content range may be 20.0 mol%, 15.0 mol%, 10.0 mol%, 8.0 mol%, 6.0 mol%, 5.0 mol%, 4.0 mol%, 3.0 mol%, 2.0 mol% or 1.0 mol%, based on the olefin content derived from C3-C 20 Polymer units of olefins. Any lower limit can be combined with any upper limit to form a range. The comonomer content is based on the total content of all monomers in the polymer.

[0064] In one class of embodiments, the first polyethylene may have minimal long chain branching (ie, less than 1.0 long chain branch / 1000 carbon atoms, preferably 0.05 to 0.50 long chain branches / 1000 carbon atoms). Such values ​​are consistent with g' visThe branching index (as defined below) of ≥ 0.980, 0.985, ≥ 0.99, ≥ 0.995, or 1.0 is characteristic of a linear structure. Although such values ​​indicate little to no long chain branching, some long chain branching may be present (i.e., less than 1.0 long chain branch / 1000 carbon atoms, preferably less than 0.5 long chain branch / 1000 carbon atoms, and particularly 0.05 to 0.50 long chain branches / 1000 carbon atoms).

[0065] In some embodiments, the first polyethylene can have a density of about 0.900 to about 0.925 g / cm according to ASTM D-4703 and ASTM D-1505 / ISO 1183. 3 , about 0.910-about 0.921g / cm 3 , about 0.912-about 0.918g / cm 3 , or about 0.914-0.918g / cm 3 .

[0066] The weight average molecular weight (M w ) can be about 15,000 to about 500,000 g / mol, about 20,000 to about 200,000 g / mol, about 25,000 to about 150,000 g / mol, about 150,000 to about 400,000 g / mol, about 200,000 to about 400,000 g / mol, or about 250,000 to about 350,000 g / mol.

[0067] The first polyethylene can have a molecular weight distribution (MWD) or (MWD) of about 1.5 to about 5.0, about 2.0 to about 5.0, about 3.0 to about 4.5, or about 2.5 to about 4.0. w / M nMWD was measured using gel permeation chromatography ("GPC") on a Waters 150 gel permeation chromatograph equipped with a differential refractive index ("DRI") detector and a Chromatix KMX-6 on-line light scattering photometer. The system used 1,2,4-trichlorobenzene as the mobile phase at 135°C and Shodex (Showa Denko America, Inc.) polystyrene gel columns 802, 803, 804, and 805. This technique is discussed in "Liquid Chromatography of Polymers and Related Materials III," J. Cazes, ed., Marcel Dekker, 1981, p. 207, which is incorporated herein by reference. Polystyrene was used for calibration. No correction for column diffusion was made; however, data on recognized standards, such as (U.S.) National Bureau of Standards polyethylene 1484 and anion-generated hydrogenated polyisoprene (alternating ethylene-propylene copolymer), indicate that such corrections to MWD are less than 0.05 units. M w / M n Calculated from the elution time. Numerical analysis was performed using commercially available Beckman / CIS customized LALLS software in conjunction with a standard gel permeation package. w / M n Means M w is the value reported using the LALLS detector and M n is the value reported using the DRI detector described above.

[0068] The first polyethylene may have a z-average molecular weight (M z ) and weight average molecular weight (M w )(M z / M w ) ratio is greater than about 1.5, or greater than about 1.7, or greater than about 2.0. In some embodiments, this ratio is about 1.7 to about 3.5, about 2.0 to about 3.0, or about 2.2 to about 3.0.

[0069] The first polyethylene may have a melt index (MI) or (MI) as measured by ASTM D-1238-E (190° C., 2.16 kg). 2.16) is from about 0.1 to about 300 g / 10 min, from about 0.1 to about 100 g / 10 min, from about 0.1 to about 50 g / 10 min, from about 0.1 g / 10 min to about 10.0 g / 10 min, from about 0.1 g / 10 min to about 5.0 g / 10 min, from about 0.1 g / 10 min to about 3.0 g / 10 min, from about 0.1 g / 10 min to about 2.0 g / 10 min, from about 0.1 g / 10 min to about 1.2 g / 10 min, from about 0.2 g / 10 min to about 1.5 g / 10 min, from about 0.2 g / 10 min to about 1.1 g / 10 min, from about 0.3 g / 10 min to about 1.0 g / 10 min, from about 0.4 g / 10 min to about 1.0 g / 10 min, or from about 0.5 g / 10 min to about 1.0 g / 10 min.

[0070] The first polyethylene may have a MIR(I 21.6 (190℃, 21.6kg) / I 2.16 (190° C., 2.16 kg)) is about 15 to about 50, about 20 to about 40, about 22 to about 38, about 25 to about 35, about 35 to about 50, or about 40 to about 50.

[0071] In one class of embodiments, the first polyethylene may contain less than 5.0 ppm hafnium, less than 2.0 ppm hafnium, less than 1.5 ppm hafnium, or less than 1.0 ppm hafnium. In other embodiments, the polyethylene polymer may contain from about 0.01 ppm to about 2 ppm hafnium, from about 0.01 ppm to about 1.5 ppm hafnium, or from about 0.01 ppm to about 1.0 ppm hafnium.

[0072] Generally, the amount of hafnium in the polyethylene polymer is greater than the amount of zirconium. In the embodiment of a particular class, the ratio (ppm / ppm) of hafnium to zirconium is at least about 2.0, at least about 10.0, at least about 15, at least about 17.0, at least about 20.0, at least about 25.0, at least about 50.0, at least about 100.0, at least about 200.0 or at least about 500.0 or larger. Although zirconium is usually present as an impurity in hafnium, it will be appreciated that in some embodiments using a catalyst containing particularly pure hafnium, the amount of zirconium can be extremely low, resulting in almost undetectable or undetectable zirconium in the polyethylene polymer. Therefore, the upper limit of the ratio of hafnium to zirconium in the polymer can be quite large.

[0073] In several classes of embodiments, the first polyethylene can have at least a first peak and a second peak in a comonomer distribution analysis, wherein the first peak has a maximum at log(M w) value is 4.0 to 5.4, 4.3 to 5.0, or 4.5 to 4.7; and the TREF elution temperature is 70.0°C to 100.0°C, 80.0°C to 95.0°C, or 85.0°C to 90.0°C. In the comonomer distribution analysis, the second peak has a maximum at the following position, log(M w ) value is 5.0 to 6.0, 5.3 to 5.7, or 5.4 to 5.6; and the TREF elution temperature is 40.0°C to 60.0°C, 45.0°C to 60.0°C, or 48.0°C to 54.0°C.

[0074] In several classes of embodiments, the first polyethylene may have a composition distribution breadth index (CDBI) of 20% to 35%. The CDBI may be determined using techniques for separating individual fractions of a resin sample. A preferred technique is the Temperature Rising Elution Fraction ("TREF") described in Wild et al. J. Poly. Sci., Poly. Phys. Ed., Vol. 20, p. 441 (1982), which is incorporated herein for purposes of U.S. practice.

[0075] In several classes of embodiments described above, the first polyethylene can have a broad orthogonal comonomer distribution or "BOCD". "BOCD" refers to a broad orthogonal composition distribution in which the comonomers of the copolymer are primarily incorporated into high molecular weight chains or species of the polyolefin polymer or composition. The distribution of short chain branches can be measured, for example, using temperature rise elution fractionation (TREF) in conjunction with a light scattering (LS) detector to measure the weight average molecular weight of molecules eluted from a TREF column at a given temperature. The combination of TREF and LS (TREF-LS) produces information about the width of the composition distribution and whether the chain comonomer content of different molecular weights across the polymer chain is increased, decreased, or uniform. BOCD has been described, for example, in U.S. Pat. No. 8,378,043, column 3, line 34, spanning column 4, line 19, and U.S. Pat. No. 8,476,392, line 43, spanning column 16, line 54.

[0076] The TREF-LS data reported in this paper were measured using an analytical size TREF instrument (Polymerchar, Spain) with a column of the following dimensions: inner diameter (ID) 7.8 mm and outer diameter (OD) 9.53 mm and column length 150 mm. The column was packed with steel beads. 0.5 mL of a 6.4% (w / v) polymer solution in o-dichlorobenzene (ODCB) (containing 6 g BHT / 4 L) was added from the column and cooled from 140° C. to 25° C. at a constant cooling rate of 1.0° C. / min. Subsequently, ODCB was pumped through the column at a flow rate of 1.0 ml / min, and the column temperature was increased at a constant heating rate of 2° C. / min to elute the polymer. The 2857 cm-1 The polymer concentration in the eluent is detected by absorption at the wavelength. The concentration of ethylene-α-olefin copolymer in the eluent is calculated from the absorption and plotted as a function of temperature. The molecular weight of the ethylene-α-olefin copolymer in the eluent is measured by light scattering using a Minidawn Tristar light scattering detector (Wyatt, California, USA). The molecular weight is also plotted as a function of temperature.

[0077] The width of the composition distribution is determined by T 75 -T 25 Value characterization, where T 25 is the temperature at which 25% of the eluted polymer is obtained in a TREF experiment as described herein, and T 75 is the temperature at which 75% of the eluted polymer is obtained. The composition distribution is further determined by F 80 The F value is characterized by the fraction of polymer that elutes below 80°C in a TREF-LS experiment as described herein. 80 A value of M indicates a higher comonomer fraction in the polymer molecule. An orthogonal composition distribution consists of M values ​​greater than 1. 60 / M 90 Value definition, where M 60 is the molecular weight of the polymer fraction eluted at 60°C in a TREF-LS experiment as described herein and M 90 is the molecular weight of the polymer fraction eluted at 90°C in the TREF-LS experiment.

[0078] In one class of embodiments, the first polyethylene as described herein may have a BOCD characterized by T 75 -T 25 is 1 or greater, 2.0 or greater, 2.5 or greater, 4.0 or greater, 5.0 or greater, 7.0 or greater, 10.0 or greater, 11.5 or greater, 15.0 or greater, 17.5 or greater, 20.0 or greater, or 25.0 or greater, wherein T 25 is the temperature at which 25% of the eluted polymer is obtained in a TREF experiment as described herein and T 75 is the temperature at which 75% of the eluted polymer is obtained.

[0079] The first polyethylene as described herein may also have a BOCD characterized in that M 60 / M 90 is 1.5 or greater, 2.0 or greater, 2.25 or greater, 2.50 or greater, 3.0 or greater, 3.5 or greater, 4.0 or greater, 4.5 or greater, or 5.0 or greater, wherein M 60 is the molecular weight of the polymer fraction eluted at 60°C in a TREF-LS experiment as described herein and M90 is the molecular weight of the polymer fraction eluted at 90°C in the TREF-LS experiment.

[0080] Additionally, the first polyethylene as described herein may also have a BOCD characterized in that F 80 The value is 1% or more, 2% or more, 3% or more, 4% or more, 5% or more, 6% or more, 7% or more, 10% or more, 11% or more, 12% or more, or 15% or more, wherein F 80 is the fraction of polymer eluting below 80°C.

[0081] Alternatively, a Gottfert Rheotens melt strength instrument may be used to measure the melt strength of the first polyethylene at a particular temperature. Unless otherwise indicated, to measure melt strength, a polymer melt strand extruded from a capillary die is sandwiched between two counter-rotating wheels on the instrument. The melt strength is measured at 2.4 mm / sec. 2 The winding speed is increased with a constant acceleration of . The maximum traction force (in cN) reached before the line breaks or starts to show tensile resonance is determined as the melt strength. The temperature of the rheometer is set at 190°C. The capillary die has a length of 30 mm and a diameter of 2 mm. The polymer melt is extruded from the die at a speed of 10 mm / sec. The distance between the die outlet and the wheel contact point should be 122 mm.

[0082] The melt strength of the first polyethylene can range from about 1 to about 100 cN, about 1 to about 50 cN, about 1 to about 25 cN, about 3 to about 15 cN, about 4 to about 12 cN, or about 5 to about 10 cN.

[0083] Materials and methods for preparing the first polyethylene are described in, for example, U.S. Patent No. 6,956,088 (particularly Example 1), U.S. Publication No. 2009 / 0297810 (particularly Example 1); U.S. Publication No. 2015 / 0291748 (particularly PE1-PE5 in the examples); and WO2014 / 099356 (particularly PE3 in the examples and mentioned on page 12), including, for example, the use of a silica-supported hafnium transition metallocene / methylaluminoxane catalyst system described in U.S. Patent No. 6,242,545 and U.S. Patent No. 6,248,845 (particularly Example 1).

[0084] Polyethylene polymers suitable for use as the first polyethylene are commercially available from ExxonMobil Chemical Company in Houston, Texas, and are marketed as Exceed XP TM Performance Polymer Sales. Exceed XP TMPerformance Polymer provides outstanding performance in areas such as dart impact strength, flex crack resistance, and machine direction (MD) tear, while maintaining stiffness at lower density. Exceed XP TM mPE also offers an optimal solution with a good balance of melt strength, toughness, stiffness and sealing ability, which makes this type of polymer very suitable for blown / cast film solutions.

[0085] In another exemplary embodiment, the hydrocarbon resin described herein is present in the film described herein in the form of a pre-blend with a second polyethylene (being a polyethylene described herein). Preferably, the second polyethylene has (i) a density of about 0.900 to about 0.925 g / cm 3 (ii) MI,I 2.16 is about 0.1 to about 10.0 g / 10 min, (iii) MIR, I 21.6 / I 2.16 is about 15 to about 50, (iv) a weight average molecular weight (M w ) is from about 20,000 to about 200,000, (v) MWD is from about 2.0 to about 5.0, and (vi) z-average molecular weight (M z ) and weight average molecular weight (M w )(M z / M w ) ratio is about 1.7 to about 3.5. In various embodiments, the second polyethylene can meet the characteristics listed above for the first polyethylene. The second polyethylene can be the same as the first polyethylene or different from the first polyethylene. Preferably, the second polyethylene is the same as the first polyethylene.

[0086] In the films described herein, the first and second polyethylene polymers (if present) may each optionally be in a blend with one or more other polymers, such as polyethylene as defined herein, the blend being referred to as a polyethylene composition. In particular, the polyethylene composition described herein may be a physical blend or in-situ blend of more than one type of polyethylene or a composition of polyethylene with a polymer other than the polyethylene, wherein the polyethylene component is the major component, such as greater than 50% by weight of the total weight of the composition.

[0087] In an exemplary embodiment, the first polyethylene is present in an amount of about 50 wt % to about 95 wt %, e.g., about 50 wt %, about 55 wt %, about 60 wt %, about 65 wt %, about 70 wt %, about 75 wt %, about 80 wt %, about 85 wt %, about 90 wt %, about 95 wt %, or within the range of any combination of values ​​recited herein, based on the total weight of polymers in the layer. In an exemplary embodiment in which the hydrocarbon resin in the layer is present in a pre-blend with a second polyethylene described herein, the weight ratio between the hydrocarbon resin and the second polyethylene is from about 1 :2 to about 2:1, e.g., about 1 :2, about 3:5, about 2:3, about 3:4, about 4:5, about 1 :1, about 5:4, about 4:3, about 3:2, about 5:3, about 2:1, or anywhere between any combination of values ​​recited herein.

[0088] In one class of embodiments, in addition to the polyethylene as described above, the films of the present invention may include other polymers in any layer of the film, including but not limited to other polyolefins, polar polymers, and cationic polymers.

[0089] additive

[0090] Film described herein can also contain various additives as known in the art in at least one layer. The example of such additives includes slip agent, antiblocking agent, filler, antioxidant, UV stabilizer, heat stabilizer, pigment, processing aid, crosslinking catalyst, flame retardant and foaming agent etc., and their combination. In particular, the film made according to the present invention can also include functional additives suitable for specific packaging applications, such as tackifier, antifungal agent and ultraviolet absorber (for silage film). Preferably, additives can be each individually present in an amount of about 0.01 % by weight to about 50 % by weight, or about 0.1 % by weight to about 15 % by weight, or 1 % by weight-10 % by weight, based on the gross weight of the film layer.

[0091] Any additive useful in the film may be provided together with other additive(s) of the same or different type or separately in a pre-blended masterbatch wherein the target concentration of the additive is achieved by combining each neat additive component in the appropriate amounts to make the final composition.

[0092] In a preferred embodiment, the film layer comprising the hydrocarbon resin described herein does not contain any slip agents.

[0093] Membrane Structure

[0094] In addition to the layer comprising the hydrocarbon resin described herein, the film of the present invention may comprise additional layer(s), which may be any layer typically included in a multilayer film construction. For example, the additional layer(s) may be made of:

[0095] 1. Polyolefins. Preferred polyolefins include C2-C 40 Olefins, preferably C2-C 20 Homopolymers or copolymers of olefins, preferably copolymers of α-olefins and other olefins or α-olefins (ethylene is defined as an α-olefin for the purposes of the present invention). Preferred are homopolyethylene, homopolypropylene, copolymers of propylene with ethylene and / or butene, copolymers of ethylene with one or more of propylene, butene or hexene and optionally diene. Preferred examples include thermoplastic polymers such as ultra-low density polyethylene, very low density polyethylene, linear low density polyethylene, low density polyethylene, medium density polyethylene, high density polyethylene, polypropylene, isotactic polypropylene, highly isotactic polypropylene, syndiotactic polypropylene, random copolymers of propylene and ethylene and / or butene and / or hexene, elastomers such as ethylene propylene rubber, ethylene propylene diene monomer rubber, chloroprene rubber, and compositions of thermoplastic polymers and elastomers, such as thermoplastic elastomers and rubber toughened plastics.

[0096] 2. Polar polymers. Preferred polar polymers include homopolymers and copolymers of esters, amides, acetates, and anhydrides. 20 Copolymers of olefins (e.g. ethylene and / or propylene and / or butene) and one or more polar monomers (e.g. acetates, anhydrides, esters, alcohols and / or acrylic compounds). Preferred examples include polyesters, polyamides, ethylene vinyl acetate copolymers and polyvinyl chloride.

[0097] 3. Cationic polymers. Preferred cationic polymers include polymers or copolymers of geminal disubstituted olefins, α-heteroatom olefins and / or styrene monomers. Preferred geminal disubstituted olefins include isobutylene, isopentene, isoheptene, isohexene, isooctene, isodecenes and isododecene. Preferred α-heteroatom olefins include vinyl ethers and vinyl carbazoles, and preferred styrene monomers include styrene, alkyl styrene, para-alkyl styrene, α-methyl styrene, chlorostyrene and bromo-para-methyl styrene. Preferred examples of cationic polymers include butyl rubber, copolymers of isobutylene and para-methyl styrene, polystyrene and poly-α-methyl styrene.

[0098] 4. Miscellaneous. Other preferred layers may be paper, wood, cardboard, metal, metal foil (such as aluminum foil and tin foil), metallized surfaces, glass (including silicon oxide (SiO2) applied by evaporation of silicon oxide onto the film surface), x ) coatings), fabrics, spunbond fibers, and nonwoven materials (especially polypropylene spunbond fibers or nonwoven materials) and substrates coated with inks, dyes, pigments, etc.

[0099] In particular, the films described herein may also include layers comprising materials such as ethylene vinyl alcohol (EVOH), polyamide (PA), polyvinyl chloride (PVDC) or aluminum, in order to obtain barrier properties of the film where appropriate.

[0100] The thickness of the film can generally range from 10 to 200 μm and is determined primarily by the intended use and the properties of the film. Stretch films can be thin; shrink films or heavy-duty bags are much thicker. Conveniently, the film has a thickness of no greater than about 150 μm, such as 10 to 150 μm, 20 to 120 μm, 30 to 100 μm, or 40 to 80 μm. In an exemplary embodiment where the film is a monolayer film, the film can have a thickness of no greater than about 50 μm.

[0101] In an exemplary embodiment, the film has a monolayer structure, comprising: (a) a first polyethylene having (i) a density of about 0.900 to about 0.925 g / cm based on the total weight of the polymer in the monolayer film; 3 (ii) MI,I 2.16 is about 0.1 to about 10.0 g / 10 min, (iii) MIR, I 21.6 / I 2.16 is about 15 to about 50, (iv) a weight average molecular weight (M w ) is from about 20,000 to about 200,000, (v) MWD is from about 2.0 to about 5.0, and (vi) z-average molecular weight (M z ) and weight average molecular weight (M w )(M z / M w ) ratio is about 1.7 to about 3.5; and (b) a blend of a hydrocarbon resin and a first polyethylene, the hydrocarbon resin comprising an aliphatic hydrocarbon resin, a hydrogenated aliphatic hydrocarbon resin, an aromatic hydrocarbon resin, a hydrogenated aromatic hydrocarbon resin, an alicyclic hydrocarbon resin, a hydrogenated alicyclic hydrocarbon resin, a polyterpene resin, a terpene phenolic resin, a rosin ester resin, a rosin acid resin, or a combination thereof; wherein the hydrocarbon resin is present in an amount of about 5 to about 20 weight percent, based on the total weight of polymers in the monolayer film; wherein the weight ratio between the hydrocarbon resin and the first polyethylene in the blend is about 1:2 to about 2:1.

[0102] Membrane properties and applications

[0103] The films of the present invention can be suitable for forming flexible packaging laminate films, including stand-up pouches, and a variety of other applications such as cling films, low stretch films, non-stretch wrap films, pallet shrink films, overwrap films, agricultural films, and collation shrink films. Film structures that can be used for bags, such as big bags, trash bags and liners, industrial liners, produce bags, and heavy-duty bags are prepared. The films can be used for flexible packaging, food packaging, such as fresh-cut product packaging, frozen food packaging, bundling, packaging, and integration of various products.

[0104] The inventive films described herein may have at least one of the following properties: (i) at least about 15% higher Elmendorf Tear in MD, (ii) at least about 25% higher Elmendorf Tear in TD, (iii) at least about 4% higher Dart Drop Impact, (iv) at least about 3% lower Static COF, and (v) at least about 40% lower Dynamic COF, compared to the properties of a film that does not contain a hydrocarbon resin but is otherwise identical in film formulation, thickness, and structure.

[0105] It has been unexpectedly discovered that film designs as set out herein, by virtue of incorporating into the films specific amounts of hydrocarbon resins described herein, can advantageously and economically mitigate the COF deficiencies commonly seen in films made from mPE having outstanding toughness properties by simultaneously improving both COF and toughness-related properties, thereby resulting in a better achieved overall property profile of the films so obtained, which is favored by a range of promising end uses.

[0106] Method for preparing membrane

[0107] A method for preparing the film of the present invention is also provided. The method for preparing the film may include the following steps: (a) preparing a layer comprising: (i) a first polyethylene having (i) a density of about 0.900 to about 0.925 g / cm 3 (ii) MI,I 2.16 is about 0.1 to about 10.0 g / 10 min, (iii) MIR, I 21.6 / I 2.16 is about 15 to about 50, (iv) a weight average molecular weight (M w ) is from about 20,000 to about 200,000, (v) MWD is from about 2.0 to about 5.0, and (vi) z-average molecular weight (M z ) and weight average molecular weight (M w )(M z / M w ) ratio of about 1.7 to about 3.5; and (ii) about 5 to about 20 weight percent of a hydrocarbon resin, based on the total weight of the polymer in the layer, the hydrocarbon resin comprising an aliphatic hydrocarbon resin, a hydrogenated aliphatic hydrocarbon resin, an aromatic hydrocarbon resin, a hydrogenated aromatic hydrocarbon resin, an alicyclic hydrocarbon resin, a hydrogenated alicyclic hydrocarbon resin, a polyterpene resin, a terpene phenolic resin, a rosin ester resin, a rosin acid resin, or a combination thereof; and (b) forming a film comprising the layer in step (a).

[0108] Film described herein can be formed by any conventional technique known in the art in step (b), including blown extrusion, cast extrusion, coextrusion, blow molding, cast and extrusion blow molding. For example, the composition of the film can be extruded in a molten state through a flat die and then cooled to form a film. Alternatively, the composition can be extruded in a molten state through an annular die and then blown and cooled to form a tubular blown film, which can then be axially cut and expanded to form a flat film. Film of the present invention can be unoriented, uniaxially oriented or biaxially oriented. The physical properties of the film can be different from those of the polymer blend, depending on the film formation technology used.

[0109] In one embodiment of the present invention, the film described herein is formed by using a blowing technique, i.e., forming a blown film. For example, the polymer composition prepared as described herein can be extruded in a molten state through an annular die and then blown and cooled to form a tubular blown film, which can then be axially cut and unfolded to form a flat film. As a specific example, the blown film can be prepared as follows. The polymer composition is introduced into the feed hopper of an extruder (e.g., water-cooled, resistance-heated, and having a 65mm extruder with an L / D ratio of 30:1). A 16cm die with a 1.5mm die gap can be used together with a double air ring and an internal bubble cooling production film. The film is extruded into a film through a die, and the film is cooled by blowing air onto the surface of the film. The film is extracted from the die, usually forming a cylindrical film, which is cooled, flattened, and optionally subjected to desired auxiliary processing such as cutting, processing, sealing, or printing. Typical melt temperatures are about 180°C to about 240°C. The blown film rate is typically about 3 to about 25 kg / hour / inch of die circumference (about 4.35 to about 26.11 kg / hour / cm of die circumference). The finished film can be wound into a roll for subsequent processing. Specific blown film methods and apparatus suitable for forming films according to embodiments of the present invention are described in U.S. Patent No. 5,569,693. Of course, other blown film formation methods may also be used.

[0110] In blown film extrusion, the film can be pulled upward by, for example, nip rolls after leaving the die, and simultaneously blown and laterally stretched to a degree that can be quantified by the blow-up ratio (BUR). Blowing provides transverse (TD) stretching, while being pulled upward by the nip rolls provides longitudinal (MD) stretching. As the polymer cools after leaving the die and blowing, the polymer crystallizes and reaches a point where the crystallization in the film is sufficient to prevent further MD or TD orientation. The position where further MD or TD orientation stops is usually referred to as the "frost line" because haze appears at this position.

[0111] The variables in this process that determine the final film properties include die gap, BUR and TD stretch, take-up speed and MD stretch, and frost line height. Certain factors tend to limit production speed and are largely determined by polymer rheology, including shear sensitivity, which determines maximum output and melt tension that limits bubble stability, BUR, and take-up speed.

[0112] In another embodiment of the present invention, cast film can be prepared using the following pilot-scale commercial cast film production line machine. The pellets of the polymer blend are melted at a temperature ranging from about 200°C to about 300°C, wherein a specific melt temperature is selected to match the viscosity of various resins. The melt is transported to a coextrusion adapter, which combines the melt flow into a multilayer coextrusion structure. This laminar flow is distributed to a desired width by a single manifold film extrusion die. The die gap opening is generally about 0.6mm to about 1mm. The material is then stretched to final film thickness. For a film of about 50 μm, the material stretch ratio is generally about 21:1. A vacuum box or air knife can be used to fix the melt leaving the die opening on the main cooling roller maintained at about 30°C.

[0113] Multilayer films can be formed by methods known in the art. The materials forming each layer can be coextruded through a coextrusion feed block and a die assembly to produce a film having two or more layers that adhere together but have different compositions. Coextrusion can be applied to cast film or blown film processes. Multilayer films can also be formed by extrusion coating, in which the substrate material contacts the hot molten polymer when the polymer leaves the die. Extrusion coating is usually processed at a higher temperature than cast film, usually about 200°C to about 300°C, so as to promote adhesion of the extruded material to the substrate. Other extrusion coating processes are known in the art, including those described in, for example, U.S. Patent Nos. 5,268,230, 5,178,960 and 5,387,630. The coating can be a monolayer film or a multilayer film. The substrate can also be a raw material for milk boxes, juice containers, films, etc. For example, when another polyethylene film is extruded through a die, the polyethylene film that has been formed can be extrusion coated with the other polyethylene film. Multilayer films can also be formed by combining two or more monolayer films prepared as described above. The total thickness of the multilayer film can vary based on the desired application. Total film thicknesses of about 5 to about 100 μm, more typically about 10 to about 50 μm, are suitable for most applications. One skilled in the art will appreciate that the thickness of the individual layers of the multilayer film can be adjusted based on desired end-use properties, resins or copolymers used, equipment capabilities, and other factors. Example

[0114] The present invention may be better understood with reference to the following examples and tables, but the present invention is not intended to be limited thereto.

[0115] The examples illustrate toughness-related properties and COF exhibited by four inventive film samples (Samples 2-3 and 5-6) each comprising a hydrocarbon resin as described herein and two different polyethylene polymers formulated as listed herein, compared to two comparative film samples (Sample 1 compared to Samples 2-3 and Sample 4 compared to Samples 5-6, respectively) that do not contain a hydrocarbon resin but are otherwise identical in film formulation, thickness, and structure. All samples were produced on a coextrusion blown film line according to the methods described herein, with a monolayer structure of 50 μm. The polyethylene and resin products used in the samples include: OPPERA TM PR100N modifier (being a hydrocarbon resin as described herein) (ExxonMobil Chemical Company, Houston, Texas, USA), PE-1 polymer (being the first and second polyethylenes as described herein) (prepared with a bis(n-propylcyclopentadienyl)hafnium dichloride metallocene catalyst as further described in U.S. Pat. No. 6,956,088, density: 0.916 g / cm 3 , MI: 0.20g / 10min, MIR: 49.4, M w :131,704,MWD:3.25,M z / M w : 1.97) (ExxonMobil Chemical Company, Houston, Texas, USA), and PE-2 polymer (being the first and second polyethylenes described herein) (prepared with a bis(n-propylcyclopentadienyl)hafnium dichloride metallocene catalyst, as further described in U.S. Pat. No. 6,956,088, density: 0.916 g / cm 3 , MI: 0.50g / 10min, MIR: 30.1, M w :152,197,MWD:4.02,M z / M w : 2.48) (ExxonMobil Chemical Company, Houston, Texas, USA). TM OPPERA PR100N modifier and 50 wt. % of either PE-1 (referred to as masterbatch-1) or PE-2 polymer (referred to as masterbatch-2) were used in the form of pre-blended masterbatches of the four inventive samples. TM PR 100N modifier, based on the total weight of the masterbatch.

[0116] Elmendorf tear strength was measured based on ASTM D1922-06a using a TearTester 83-11-01 from TMI Group of Companies in both MD and TD and measured the energy required to continue a pre-cut rip in the test sample, expressed as a tear force in grams. The samples were cut across the web using a constant radius tear die and were free of any visible defects (e.g., die lines, gels, etc.).

[0117] The dart impact is measured on a dart impact tester model C from Davenport Lloyd Instruments by the method according to ASTM D1709, where a pneumatically operated ring clamp is used to obtain a uniform flat specimen and an electromagnet automatically releases the dart once sufficient air pressure is reached on the ring clamp. A dart with a 38.10±0.13 mm diameter hemispherical head dropped from a height of 0.66±0.01 m is used. The dart impact measures the energy that causes film failure under specified conditions of a free-falling dart impact. This energy is expressed in terms of the weight (mass, g) of a dart dropped from a specified height that will cause 50% failure of the tested specimens. The specimen has a minimum width of 20 cm and a recommended length of 10 m.

[0118] The coefficient of friction (COF) was determined according to ASTM 1894 and involves determining the initial (static) and sliding (dynamic) coefficients of friction of a plastic film when it slides on itself. A sample prepared with a length of 150 mm and a width of 65 mm was connected to a 200 g slider pulled at a speed of 150 mm / min. The forces to start the slider (static) and to maintain motion (dynamic) were measured separately. The static COF is represented by the initial friction force reading divided by the slider weight, while the dynamic COF is represented by the average friction force reading obtained during uniform sliding of the surface divided by the slider weight.

[0119] The samples were conditioned at 23°C ± 2°C and 50% ± 10% relative humidity for at least 40 hours before all properties were measured.

[0120] The film formulations (based on the total weight of polymer in the film) and thus the corresponding test results are described in the table.

[0121] As shown in the table, film samples of the present invention characterized by specific amounts of hydrocarbon resins described herein can outperform comparative samples without the hydrocarbons in terms of reduced COF, particularly as reflected by a significant reduction in dynamic COF of at least about 40%, with toughness-related properties, including Elmendorf tear strength and dart impact, improved to even more pronounced levels. Moreover, it can be seen that such property enhancement effects work in an incremental manner as the amount of hydrocarbon increases within the ranges listed herein. This suggests that the films of the present invention have promising potential to conveniently and economically improve friction properties in tandem with toughness properties by using the hydrocarbon resins described herein in place of conventional slip agents. Thus, without being bound by theory, by controlling the addition of hydrocarbon resins, better achieved overall properties of films made primarily of polyethylene polymers with outstanding toughness as desired for different end uses can be expected.

[0122] Table: Film formulation (weight %) and test results of samples in the examples

[0123]

[0124] All documents described herein are incorporated herein by reference, including any priority documents and / or test procedures. When numerical lower limits and numerical upper limits are listed herein, the scope from any lower limit to any upper limit is contained. As is apparent from the general description above and the specific embodiments, although the form of the present invention has been set forth and described, various changes can be made without departing from the spirit and scope of the present invention. Therefore, it is not intended to limit the present invention thus.

Claims

1. A film comprising a layer, the layer comprising: (a) 50 to 90 weight percent of a first polyethylene, based on the total weight of the polymers in the layer, the first polyethylene having (i) a density of 0.900 to 0.925 g / cm 3 (ii) Melt index (MI) 2.16 0.1-10.0 g / 10 min, (iii) melt index ratio (MIR) I 21.6 / I 2.16 15-50, (iv) weight average molecular weight (M w ) is 20,000-200,000, (v) a molecular weight distribution (MWD) is 2.0-5.0, and (vi) a z-average molecular weight (M z ) and weight average molecular weight (M w )(M z / M w ) ratio is 1.7-3.5; and (b) 10 to 20 weight percent of a hydrocarbon resin, based on the total weight of the polymer in the layer, the hydrocarbon resin comprising an aliphatic hydrocarbon resin, a hydrogenated aliphatic hydrocarbon resin, an aromatic hydrocarbon resin, a hydrogenated aromatic hydrocarbon resin, an alicyclic hydrocarbon resin, a hydrogenated alicyclic hydrocarbon resin, a polyterpene resin, a terpene phenolic resin, a rosin ester resin, a rosin acid resin, or a combination thereof; wherein the layer does not contain any slip agent and the film has at least one of the following properties: (i) at least 15% higher Elmendorf Tear in the machine direction (MD), (ii) at least 25% higher Elmendorf Tear in the transverse direction (TD), (iii) at least 4% higher dart drop impact, (iv) at least 3% lower static coefficient of friction (COF), and (v) at least 40% lower dynamic COF, compared to the properties of a film not containing the hydrocarbon resin but having the same film formulation, thickness and structure in other aspects.

2. The film of claim 1, wherein the first polyethylene is present in an amount of 50 wt% to 85 wt%, based on the total weight of polymers in the layer.

3. A film according to claim 1 or claim 2 wherein the hydrocarbon resin is present in neat form.

4. A film according to claim 1 or claim 2 wherein the hydrocarbon resin is present in a pre-blend with the second polyethylene.

5. The film of claim 4, wherein the second polyethylene has (i) a density of 0.900 to 0.925 g / cm 3 (ii) Melt index (MI) 2.16 0.1-10.0 g / 10 min, (iii) melt index ratio (MIR) I 21.6 / I 2.16 15-50, (iv) weight average molecular weight (Mw ) is 20,000-200,000, (v) a molecular weight distribution (MWD) is 2.0-5.0, and (vi) a z-average molecular weight (M z ) and weight average molecular weight (M w )(M z / M w ) ratio is 1.7-3.

5. The film of claim 5 , wherein the second polyethylene is the same as the first polyethylene.

7. The film according to claim 4, wherein the weight ratio between the hydrocarbon resin and the second polyethylene is 1:2 to 2:

1.

8. The film of claim 1 or claim 2, wherein the film has a thickness of no greater than 50 μm.

9. The film of claim 1 or claim 2, wherein the film is a single layer film.

10. Single-layer film, comprising: (a) 50 to 90 weight percent of a first polyethylene, based on the total weight of the polymers in the monolayer film, the first polyethylene having (i) a density of 0.900 to 0.925 g / cm 3 (ii) Melt index (MI) 2.16 0.1-10.0 g / 10 min, (iii) melt index ratio (MIR) I 21.6 / I 2.16 15-50, (iv) weight average molecular weight (M w ) is 20,000-200,000, (v) a molecular weight distribution (MWD) is 2.0-5.0, and (vi) a z-average molecular weight (M z ) and weight average molecular weight (M w )(M z / M w ) ratio is 1.7-3.5; and (b) a blend of a hydrocarbon resin and a first polyethylene, the hydrocarbon resin comprising an aliphatic hydrocarbon resin, a hydrogenated aliphatic hydrocarbon resin, an aromatic hydrocarbon resin, a hydrogenated aromatic hydrocarbon resin, an alicyclic hydrocarbon resin, a hydrogenated alicyclic hydrocarbon resin, a polyterpene resin, a terpene phenolic resin, a rosin ester resin, a rosin acid resin, or a combination thereof; wherein the hydrocarbon resin is present in an amount of 10 to 20 weight percent, based on the total weight of polymers in the monolayer film; wherein the weight ratio between the hydrocarbon resin and the first polyethylene in the blend is 1:2 to 2:1; wherein the monolayer film does not contain any slip agent and has at least one of the following properties: (i) at least 15% higher Elmendorf Tear in MD, (ii) at least 25% higher Elmendorf Tear in TD, (iii) at least 4% higher Dart Drop Impact, (iv) at least 3% lower Static COF, and (v) at least 40% lower Dynamic COF, compared to the properties of a film without hydrocarbon resin but otherwise identical in film formulation, thickness, and structure.

11. A method for preparing a membrane, comprising the steps of: (a) preparing a layer comprising: (i) 50 to 90 weight percent of a first polyethylene, based on the total weight of the polymers in the layer, the first polyethylene having (i) a density of 0.900 to 0.925 g / cm 3 (ii) Melt index (MI) 2.16 0.1-10.0 g / 10min, (iii) melt index ratio (MIR) I 21.6 / I 2.16 15-50, (iv) weight average molecular weight (M w ) is 20,000-200,000, (v) a molecular weight distribution (MWD) is 2.0-5.0, and (vi) a z-average molecular weight (M z ) and weight average molecular weight (M w )(M z / M w ) ratio of 1.7 to 3.5; and (ii) 10 to 20 weight percent of a hydrocarbon resin, based on the total weight of the polymer in the layer, the hydrocarbon resin comprising an aliphatic hydrocarbon resin, a hydrogenated aliphatic hydrocarbon resin, an aromatic hydrocarbon resin, a hydrogenated aromatic hydrocarbon resin, an alicyclic hydrocarbon resin, a hydrogenated alicyclic hydrocarbon resin, a polyterpene resin, a terpene phenolic resin, a rosin ester resin, a rosin acid resin, or a combination thereof; and (b) forming a film comprising the layer of step (a); wherein the layer does not contain any slip agent and the film has at least one of the following properties: (i) at least 15% higher Elmendorf Tear in MD, (ii) at least 25% higher Elmendorf Tear in TD, (iii) at least 4% higher Dart Drop Impact, (iv) at least 3% lower Static COF, and (v) at least 40% lower Dynamic COF, compared to the properties of a film without hydrocarbon resin but otherwise identical in film formulation, thickness, and structure.

12. The method according to claim 11, wherein the film in step (b) is formed by blown extrusion, cast extrusion, coextrusion, blow molding, casting or extrusion blow molding.