A multi-layer coated diaphragm and polymer battery prepared therefrom
By adopting a multi-layer coating design on the battery separator, combined with the mutual complementation of low and high swelling rate polymer coatings, the problems of insufficient separator infiltration rate and safety performance in the existing technology are solved, and higher battery performance and safety performance are achieved. safety and reduced production costs.
Patent Information
- Application Number
- CN202111407755.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-11-24
AI Technical Summary
The functional coating of the existing battery separator slows down the infiltration rate of the cell electrolyte, affects the consistency and stability of the interface, and the preparation process is cumbersome and costly, and it has no safety performance in case of puncture damage such as acupuncture and other internal short circuits. improve.
It adopts a multi-layer coating separator design, including a low swelling rate polymer coating and a high swelling rate polymer coating. The low swelling rate coating is evenly coated through gravure coating and the high swelling rate coating is coated at intervals to enhance the separator. The mechanical strength and electrolyte retention capacity are improved, the wetting ability and interface consistency are improved, and it is firmly combined with the pole piece during the pressure formation process to reduce free electrolyte.
It significantly improves the battery's wettability and cycle performance, improves interface stability, improves battery safety and production efficiency, and reduces the risk of liquid electrolyte corrosion and leakage of aluminum-plastic films.
Smart Images

Figure CN114284642B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a multi-layer coated diaphragm and a polymer battery prepared therefrom. Background Art
[0002] As the popularity of electric vehicles increases year by year, the power battery industry is also developing rapidly, and the demand for batteries with high energy density and safety is increasing. Among the various parts that make up the battery, the performance of the diaphragm material also plays a vital role in improving the stability and safety of the battery. The use of diaphragms with multiple coating layers on the surface and the thermal composite process of diaphragms and pole pieces to improve the battery energy density and optimize the stability and safety of the battery interface has also become a research hotspot in the industry.
[0003] CN111755648A applies an asymmetric coating on the diaphragm, including at least one inorganic ion conductor layer applied on one side of the base membrane, and at least one organic polymer layer applied on the other side of the base membrane. By asymmetrically applying the inorganic ion conductor functional layer and the organic polymer functional layer on both sides of the base membrane, the purpose of reducing the interface impedance between the diaphragm and the electrode, improving the thermal stability, liquid absorption rate and ionic conductivity of the diaphragm and other properties is achieved. CN212230512U is provided with three coating layers on the diaphragm, the third coating layer is connected to the substrate layer, and the second coating layer is a heat-insulating aerogel layer. Through the superposition of the three coating layers, the liquid absorption performance and liquid retention performance of the diaphragm are improved. CN107611314A is coated with a first coating layer and a second coating layer of an adhesive polymer on both sides of the diaphragm, respectively. By designing different diaphragm coatings for the positive and negative electrodes, the lithium-ion battery can meet the requirements for hardness and dynamic characteristics. The CN112952296A diaphragm is composed of a composite base film and a conductive ceramic coating made of a mixture of polyolefin and a first conductive ceramic, and the ionic conductivity is improved by constructing a conductive network. Although the above invention patents can improve the porosity and liquid absorption of the battery to a certain extent, their functional coatings will slow down the electrolyte infiltration rate of the battery core, affect the consistency and stability of the battery core interface, and do not improve the safety performance under puncture damage such as acupuncture and other internal short circuit conditions, and the preparation process is relatively cumbersome and the cost is high. Therefore, the present invention provides a multi-layer coated diaphragm and a polymer battery prepared therefrom to solve the above problems. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention proposes a multi-layer coated diaphragm and a polymer battery prepared therefrom, wherein the low swelling polymer coating can improve the mechanical strength of the diaphragm and ensure the adhesion between the diaphragm and the electrode; the high swelling polymer coating can increase the electrolyte retention in the battery, and through the different functions of each coating, they complement each other, greatly improving the wetting ability of the coated diaphragm, enhancing the adhesion between the electrode and the diaphragm, ensuring the interface consistency, and the prepared polymer battery has no free electrolyte, greatly reducing the risk of liquid electrolyte corrosion and leakage of aluminum-plastic film, and improving the electrochemical performance and safety performance of the battery. Interval coating makes the overall coating amount of the diaphragm less than that of the uniform coating design, and also reduces the production cost.
[0005] In order to achieve the above-mentioned objectives, the first aspect of the present invention provides a multi-layer coated diaphragm, which includes a diaphragm substrate and a multi-layer polymer coating coated on the diaphragm substrate; the multi-layer polymer coating includes a low swelling rate polymer coating and a high swelling rate polymer coating; the low swelling rate polymer coating is uniformly coated on the surface of the diaphragm substrate; the high swelling rate polymer coating is coated at intervals on the low swelling rate polymer coating.
[0006] The second aspect of the present invention provides a polymer battery, which includes positive and negative electrodes and a separator, and the separator is the multi-layer coated separator.
[0007] A third aspect of the present invention provides a method for preparing a polymer battery, comprising:
[0008] (1) using a gravure coating method, uniformly coating a slurry of a low swelling rate polymer coating on the surface of the diaphragm substrate, and then coating a slurry of a high swelling rate polymer coating thereon in stripes and diagonal lines to obtain a multi-layer coated diaphragm;
[0009] (2) neatly stacking or winding a certain number of positive and negative electrode sheets and the multi-layer coated separator together, and encapsulating them into a polymer battery using an aluminum-plastic film;
[0010] (3) placing the battery into a pressure forming cabinet for heating and pressure forming after liquid injection, so that the coating of the multi-layer coated diaphragm swells and is firmly bonded to the electrode under pressure;
[0011] (4) After the hot-pressed battery is connected to a charging and discharging device for capacity separation, the battery is degassed and tightened until there is no free electrolyte in the battery core.
[0012] The multi-layer coated diaphragm designed by the present invention and the polymer battery prepared therefrom have the following advantages:
[0013] 1) Significantly improve the battery liquid retention capacity, and can greatly improve the wettability compared to conventional polymer coated diaphragms. Its wetting rate is comparable to that of ceramic diaphragms. The gel layer formed is uniform and stable, which can improve the interface stability and has excellent cycle performance;
[0014] 2) When the battery is short-circuited by needle puncture, the diaphragm gel layer can fit tightly on the electrode surface and maintain a certain toughness, which can effectively increase the contact internal resistance, reduce the temperature rise, and improve the battery safety;
[0015] 3) The preparation process is simple and the production cost is reduced;
[0016] 4) There is no free electrolyte inside the prepared polymer battery, which greatly reduces the risk of liquid electrolyte corrosion and leakage of the aluminum-plastic film.
[0017] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The above and other objects, features and advantages of the present invention will become more apparent through a more detailed description of exemplary embodiments of the present invention with reference to the accompanying drawings.
[0019] Figure 1 Schematic diagram of the cross-section and planar structure of the diaphragm.
[0020] Figure 2 Schematic diagram of the composite membrane of soft-pack battery.
[0021] Figure 3 The cycle curves at 45° C. are shown for the soft-pack batteries assembled in the comparative example and examples 1-6 after compounding.
[0022] Figure 4 This is a disassembly interface diagram of the soft-pack batteries assembled in the comparative example and Examples 1-6 after 10 cycles of standard charge and discharge.
[0023] Figure 5 This is a graph showing the height of the liquid level after the diaphragms of comparative examples and embodiments 1-6 are clamped with a glass slide and immersed in the electrolyte at the same height for 40 seconds.
[0024] Description of reference numerals:
[0025] 1-diaphragm substrate, 2-low swelling rate polymer coating, 3-high swelling rate polymer coating, 4-front clamp, 5-rear clamp, 6-silicone pad, 7-battery. DETAILED DESCRIPTION
[0026] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited to the embodiments set forth herein.
[0027] The present invention provides a multi-layer coated diaphragm, the diaphragm comprising a diaphragm substrate and a multi-layer polymer coating coated on the diaphragm substrate; the multi-layer polymer coating comprises a low swelling rate polymer coating and a high swelling rate polymer coating; the low swelling rate polymer coating is uniformly coated on the surface of the diaphragm substrate; the high swelling rate polymer coating is coated on the low swelling rate polymer coating at intervals. The cross-sectional and planar structural schematic diagram of the diaphragm is shown in FIG. Figure 1 shown.
[0028] Optionally, the maximum swelling and liquid absorption capacity of the high swelling rate polymer coating component in the electrolyte is 20-100% of its mass, and the maximum swelling and liquid absorption capacity of the low swelling rate polymer coating component in the electrolyte should be less than 20%.
[0029] Optionally, the membrane substrate is at least one of PE, PP, cellulose, PET, PI, non-woven fabric and electrospinning membrane.
[0030] Optionally, the raw material for forming the polymer coating is a polymer binder slurry, or a mixed slurry of a polymer binder and an inorganic material;
[0031] The inorganic material is at least one of aluminum oxide, magnesium hydroxide, layered composite hydroxide, layered composite oxide, boehmite, silicon dioxide, and silicon carbide;
[0032] The polymer binder includes a high swelling rate polymer binder and a low swelling rate polymer binder;
[0033] The high swelling rate polymer binder is preferably at least one of polyvinylidene fluoride and polyacrylonitrile, and the low swelling rate polymer binder is preferably at least one of polyethyl acrylate, polymethyl methacrylate, and ethylene-tetrafluoroethylene copolymer;
[0034] The mass fraction of the inorganic material in the mixed slurry is 0%-90%, and the mass fraction of the polymer binder is 10%-100%.
[0035] Optionally, the multi-layer polymer coating comprises at least two layers;
[0036] The multi-layer polymer coating is coated on one or both sides of the separator substrate.
[0037] Optionally, the total thickness of the low swelling rate polymer coating and the high swelling rate polymer coating is no more than 6 μm;
[0038] The low swelling polymer coating has a thickness of 1-2 μm;
[0039] The thickness of the high swelling polymer coating is 2-4 μm;
[0040] The high swelling ratio polymer coating is preferably coated in stripe-shaped oblique lines with a coating interval of 500 μm-2 mm.
[0041] The slurry of the low swelling rate polymer coating is uniformly coated on the surface of the diaphragm substrate by gravure coating, and then the slurry of the high swelling rate polymer coating is coated thereon to obtain a multi-layer coated diaphragm.
[0042] In the present invention, the low swelling rate polymer coating can improve the mechanical strength of the diaphragm and ensure the adhesion between the diaphragm and the electrode; the high swelling rate polymer coating can increase the electrolyte retention in the battery. Through the different effects of each coating, they complement each other, greatly improving the wetting ability of the coated diaphragm, enhancing the adhesion between the electrode and the diaphragm, ensuring interface consistency, and improving the electrochemical performance and safety performance of the battery.
[0043] The present invention also provides a polymer battery, which comprises positive and negative electrodes and a separator, wherein the separator is the multi-layer coated separator.
[0044] The present invention also provides a method for preparing a polymer battery, comprising:
[0045] (1) using a gravure coating method, uniformly coating a slurry of a low swelling rate polymer coating on the surface of the diaphragm substrate, and then coating a slurry of a high swelling rate polymer coating thereon at intervals to obtain a multi-layer coated diaphragm;
[0046] (2) neatly stacking or winding a certain number of positive and negative electrode sheets and the multi-layer coated separator together, and encapsulating them into a polymer battery using an aluminum-plastic film;
[0047] (3) placing the battery into a pressure forming cabinet for heating and pressure forming after liquid injection, so that the coating of the multi-layer coated diaphragm swells and is firmly bonded to the electrode under pressure;
[0048] (4) After the hot-pressed battery is connected to a charging and discharging device for capacity separation, the battery is degassed and tightened until there is no free electrolyte in the battery core.
[0049] Optionally, the slurry of the high swelling rate polymer coating comprises an inorganic material, a high swelling rate polymer binder and an organic solvent;
[0050] The slurry of the low swelling polymer coating comprises an inorganic material, a low swelling polymer binder and an organic solvent;
[0051] The organic solvent is preferably NMP; the inorganic material is preferably at least one of aluminum oxide, magnesium hydroxide, layered composite hydroxides, layered composite oxides, boehmite, silicon dioxide, and silicon carbide.
[0052] Optionally, the positive and negative electrode sheets are in direct contact with the high swelling rate polymer coating;
[0053] The temperature range for preparing the polymer battery is 60-85° C., and the pressure range is 0.1-0.8 MPa;
[0054] The polymer battery is at least one of a soft pack battery, a cylindrical battery and a square aluminum shell battery, preferably a soft pack battery. Figure 2 shown.
[0055] In the present invention, when the battery is short-circuited by needle puncture, the diaphragm gel layer can be tightly attached to the electrode surface and maintain a certain toughness, which can effectively improve the contact internal resistance, reduce the temperature rise, and improve the battery safety; the prepared polymer battery has no free electrolyte inside, which greatly reduces the risk of liquid electrolyte corrosion and leakage of the aluminum-plastic film.
[0056] The present invention is described in more detail below through examples and comparative examples.
[0057] Comparative Example
[0058] 1) Preparation of diaphragm:
[0059] a. The base film is PE, and both sides have a 2μm boehmite coating.
[0060] 2) Assembling soft pack batteries:
[0061] b. Stack 30 NCM622 ternary positive electrode sheets, 31 artificial graphite negative electrode sheets and 32 separators neatly together.
[0062] c. Use aluminum-plastic film to package the battery cells and assemble them into 50Ah soft-pack batteries.
[0063] d. The battery was filled with electrolyte, which was 1M LiPF6 dissolved in EC:EMC=3:7 (w / w), and the filling amount was 3.3g / Ah.
[0064] 3) Thermal compounding of diaphragm and electrode:
[0065] e. Connect the battery to an air bag, place it in a pressure forming cabinet at 30°C, and connect the positive and negative electrodes to the charging and discharging equipment respectively. Adjust the pressure of the pressure forming cabinet to 0.6MPa and press the battery tightly. Set the pre-charge program to charge to 3.55V at 0.05C, let it stand for 1h, charge to 4.35V at 0.1C, let it stand for 10min, and stop.
[0066] f. After the pre-charging process stops, remove the external air bag, release the pressure in the pressure incubator, take out the battery, and use the external extraction tube to extract the gas from the battery.
[0067] g. Connect the positive and negative poles of the battery to the charging and discharging equipment, set the program to discharge at 0.3C to 2.75V, charge at 0.3C to 4.35V, let it stand for 10 minutes, repeat 3 times, and stop.
[0068] h. Remove the battery from the charging and discharging equipment, connect an external extraction tube, extract the free electrolyte from the battery, and record the battery mass.
[0069] Example 1
[0070] 1) Preparation of diaphragm:
[0071] a. Coat one side of the PE diaphragm substrate with a low swelling rate polymer coating slurry (magnesium hydroxide: polyethyl acrylate = 7:3) and a high swelling rate polymer coating slurry (PVDF), wherein the low swelling rate polymer coating is uniformly coated, and the high swelling rate polymer coating is coated on the low swelling rate polymer coating with oblique intervals, and the coating interval is 500 μm. The coating thicknesses of the low swelling rate polymer coating and the high swelling rate polymer coating are 1 μm and 2 μm, respectively. Perform the same treatment on the other side of the diaphragm to prepare a coated diaphragm.
[0072] 2) Assemble soft pack batteries in the same comparison ratio;
[0073] 3) Thermal compounding of diaphragm and electrode:
[0074] b. Connect the battery to an air bag and place it in a pressure forming cabinet at room temperature of 30°C. Connect the positive and negative electrodes to the charging and discharging equipment respectively. Adjust the pressure of the pressure forming cabinet to 0.6MPa and press the battery tightly. Set the pre-charge program to charge at 0.05C to 3.55V, let it stand for 1h, charge at 0.1C to 4.35V, let it stand for 10min, and stop.
[0075] c. After the pre-charging process stops, remove the external air bag, release the pressure in the pressure incubator, take out the battery, and use the external extraction tube to extract the gas from the battery.
[0076] d. Connect the positive and negative poles of the battery to the charging and discharging equipment, set the program to discharge at 0.2C to 2.75V, charge at 0.2C to 3.9V, let it stand for 10 minutes, and then stop.
[0077] e. Remove the battery from the charging and discharging equipment and put it into the hot pressing cabinet. Adjust the temperature of the hot pressing cabinet to 70℃, the pressure to 0.06Mpa, and the hot pressing time to 60min. After the battery cools down, remove the battery, connect the external extraction tube, extract the free electrolyte from the battery, and record the battery quality.
[0078] Example 2
[0079] 1) Preparation of diaphragm:
[0080] a. Coat one side of the PE diaphragm substrate with a low swelling rate polymer coating slurry (boehmite: polyethyl acrylate = 8:2) and a high swelling rate polymer coating slurry (PVDF), wherein the low swelling rate polymer coating is evenly coated, and the high swelling rate polymer coating is coated on the low swelling rate polymer coating in an oblique interval, with a coating interval of 700 μm, and the coating thicknesses of the low swelling rate polymer coating and the high swelling rate polymer coating are 1 μm and 2 μm, respectively. Perform the same treatment on the other side of the diaphragm to prepare a coated diaphragm.
[0081] 2) Assemble soft pack batteries in the same comparison ratio;
[0082] 3) The thermal combination of the diaphragm and the electrode is the same as in Example 1.
[0083] Example 3
[0084] 1) Preparation of diaphragm:
[0085] a. Coat one side of the PE diaphragm substrate with a low swelling rate polymer coating slurry (boehmite: polyethyl acrylate = 6:4) and a high swelling rate polymer coating slurry (PVDF), wherein the low swelling rate polymer coating is evenly coated, and the high swelling rate polymer coating is coated on the low swelling rate polymer coating in an oblique interval, with a coating interval of 1000 μm, and the coating thicknesses of the low swelling rate polymer coating and the high swelling rate polymer coating are 1 μm and 2 μm, respectively. Perform the same treatment on the other side of the diaphragm to prepare a coated diaphragm.
[0086] 2) Assemble soft pack batteries in the same comparison ratio;
[0087] 3) The thermal combination of the diaphragm and the electrode is the same as in Example 1.
[0088] Example 4
[0089] 1) Preparation of diaphragm:
[0090] a. Coat one side of the PE diaphragm substrate with a low swelling rate polymer coating slurry (Al2O3: polyethyl acrylate = 9:1) and a high swelling rate polymer coating slurry (Al2O3: PVDF = 1:9), wherein the low swelling rate polymer coating is evenly coated, and the high swelling rate polymer coating is coated on the low swelling rate polymer coating in an oblique interval, with a coating interval of 1000 μm, and the coating thicknesses of the low swelling rate polymer coating and the high swelling rate polymer coating are 1 μm and 3 μm, respectively. Perform the same treatment on the other side of the diaphragm to prepare a coated diaphragm.
[0091] 2) Assemble soft pack batteries in the same comparison ratio;
[0092] 3) The thermal combination of the diaphragm and the electrode is the same as in Example 1.
[0093] Example 5
[0094] 1) Preparation of diaphragm:
[0095] a. Coat one side of the PE diaphragm substrate with a low swelling rate polymer coating slurry (boehmite: polyethyl acrylate = 8:2) and a high swelling rate polymer coating slurry (PVDF), wherein the low swelling rate polymer coating is evenly coated, and the high swelling rate polymer coating is coated on the low swelling rate polymer coating in an oblique interval, with a coating interval of 2000 μm, and the coating thicknesses of the low swelling rate polymer coating and the high swelling rate polymer coating are 1 μm and 2 μm, respectively. Perform the same treatment on the other side of the diaphragm to prepare a coated diaphragm.
[0096] 2) Assemble soft pack batteries in the same comparison ratio;
[0097] 3) The thermal combination of the diaphragm and the electrode is the same as in Example 1.
[0098] Example 6
[0099] 1) Preparation of diaphragm:
[0100] a. Coat one side of the PE diaphragm substrate with a low swelling rate polymer coating slurry (magnesium aluminum layered composite hydroxide: polyethyl acrylate = 7:3) and a high swelling rate polymer coating slurry (PVDF), wherein the low swelling rate polymer coating is uniformly coated, and the high swelling rate polymer coating is coated on the low swelling rate polymer coating in an oblique interval, with a coating interval of 1000 μm, and the coating thicknesses of the low swelling rate polymer coating and the high swelling rate polymer coating are 2 μm and 2 μm, respectively. Perform the same treatment on the other side of the diaphragm to prepare a coated diaphragm.
[0101] 2) Assemble soft pack batteries in the same comparison ratio;
[0102] 3) The thermal combination of the diaphragm and the electrode is the same as in Example 1.
[0103] Figure 3 The cycle curves at 45°C are shown for the soft-pack batteries assembled in the comparative example and in Examples 1-6 after compounding. Figure 3 From the mid-cycle performance, it can be seen that the capacity retention rates of the embodiments are higher than those of the comparative examples, which shows that multi-layer coating of the diaphragm can significantly improve the battery performance.
[0104] Figure 4 This is a disassembly interface diagram of the soft-pack battery assembled in the comparative example and Examples 1-6 after 10 cycles of standard charge and discharge. Figure 4 It can be seen that the interface consistency of the battery cells in the embodiments is significantly improved compared with the comparative examples.
[0105] Figure 5 The following is a graph showing the height of the liquid level after the diaphragms of Comparative Example and Examples 1-6 were clamped and fixed with a glass slide and immersed in the electrolyte at the same height for 40 seconds. Figure 5It can be seen that the liquid absorption capacity and wettability of the diaphragms of Examples 1-6 are greatly improved compared with the comparative example.
[0106] Test Example 1
[0107] The diaphragm samples prepared in the comparative examples and examples 1-6 were tested for liquid retention and air permeability. The test method for liquid retention is: determine the mass m0 of the dry battery cell, use the prepared diaphragms to assemble the soft-pack batteries, inject liquid and compound them, tighten the batteries after 3 cycles of standard charge and discharge, and determine the mass m1 of the battery cell. The battery liquid retention = m1-m0. Air permeability test method: select the diaphragm sample to measure the average time required to pass 100mL of gas. The results are shown in Table 1.
[0108] Table 1
[0109]
[0110] From the data of Examples 1-3 in Table 1, it can be seen that when the thickness of the diaphragm coating remains unchanged, the coating interval of the high swelling rate polymer coating is increased, the air permeability of the diaphragm is improved to a certain extent, and the liquid retention amount is also increased accordingly. However, when the coating interval is further increased to Example 5, the air permeability is improved, but the liquid retention amount decreases. It is speculated that the porosity is too large and the electrolyte is lost. It can be seen from Examples 3, 4, and 6 that when the coating interval remains unchanged, appropriately increasing the thickness of the high swelling rate polymer coating or the low swelling rate polymer coating can effectively increase the liquid retention amount. And the ratio of inorganic materials and binders in the coatings of the embodiments are all preferred examples.
[0111] Test Example 2
[0112] The polymer batteries prepared in the comparative example and Examples 1-6 were subjected to battery needle penetration test. The test method is: at 25°C, a stainless steel needle with a diameter of 1 mm was used to penetrate the battery at a speed of 0.1 mm / s perpendicular to the battery surface to a depth of 6 mm, and the battery voltage drop and temperature rise were monitored. The battery was adjusted to a fully charged state before the test. The results are shown in Table 2.
[0113] Table 2
[0114]
[0115]
[0116] From the data of Examples 1-3 in Table 2, it can be seen that as the coating interval of the high swelling polymer coating increases, the coating amount of the high swelling polymer coating decreases, the pressure drop of the battery needle puncture increases, and the temperature rise increases. It is speculated that the gel layer can effectively increase the contact resistance, reduce the temperature rise, and slow down the occurrence of thermal runaway of the battery. From Examples 3 and 6, it can be seen that increasing the thickness of the low swelling polymer coating also has a certain effect on reducing the pressure drop and temperature rise of needle puncture.
[0117] Test Example 3
[0118] The polymer coating swelling capacity test was conducted by placing a certain amount of polymer slurry in a petri dish and drying it to form a film with a thickness of about 0.5 mm, cutting the film into a shape of 2 cm × 2 cm, and accurately weighing its mass m0, then placing the cut film and 20 mL of electrolyte in a sample tube, heating it to 70°C and keeping it for 24 hours, then taking out the swollen film, wiping off the liquid electrolyte on the surface, and quickly weighing the mass m1, and its swelling degree is τ = 100% × (m1-m0) / m0. The results are shown in Table 2.
[0119] Table 3
[0120]
[0121]
[0122] It can be seen from the test results of the comparative examples and the embodiments that the polymer battery using the multi-layer coated diaphragm of the present invention has improved liquid retention, wettability, interface consistency and safety.
[0123] Compared with the existing diaphragms, in the multi-layer coated diaphragm design of the present invention, the low swelling rate polymer coating can improve the mechanical strength of the diaphragm and ensure the adhesion between the diaphragm and the electrode; the high swelling rate polymer coating can increase the electrolyte retention in the battery. Through the different effects of each coating, they complement each other, greatly improving the wetting ability of the coated diaphragm, enhancing the adhesion between the electrode and the diaphragm, ensuring interface consistency, and improving the electrochemical performance and safety performance of the battery.
[0124] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A multi-layer coated diaphragm, characterized in that: The diaphragm includes a diaphragm substrate and a multi-layer polymer coating coated on the diaphragm substrate; The multi-layer polymer coating comprises a low swelling rate polymer coating and a high swelling rate polymer coating; The low swelling polymer coating is uniformly coated on the surface of the diaphragm substrate; The high swelling rate polymer coating is coated on the low swelling rate polymer coating at intervals; The total thickness of the low swelling rate polymer coating and the high swelling rate polymer coating is no more than 6 μm; The low swelling polymer coating has a thickness of 1-2 μm; The thickness of the high swelling polymer coating is 2-4 μm; The high swelling rate polymer coating is coated in stripe-shaped oblique lines at intervals, and the coating interval is 500 μm-2 mm; The maximum swelling and liquid absorption capacity of the high swelling rate polymer coating component in the electrolyte is 20-100% of its mass, and the maximum swelling and liquid absorption capacity of the low swelling rate polymer coating component in the electrolyte is less than 20% of its mass; The raw material for forming the polymer coating is a polymer binder slurry, or a mixed slurry of a polymer binder and an inorganic material; The polymer binder includes a high swelling rate polymer binder and a low swelling rate polymer binder; The mass fraction of the inorganic material in the mixed slurry is 0%-90%, and the mass fraction of the polymer binder is 10%-100%; The slurry of the low swelling polymer coating comprises an inorganic material, a low swelling polymer binder and an organic solvent.
2. The multi-layer coated diaphragm according to claim 1, characterized in that: The membrane substrate is at least one of PE, PP, cellulose, PET, PI, non-woven fabric and electrospinning membrane.
3. The multi-layer coated diaphragm according to claim 1, characterized in that: The inorganic material is at least one of aluminum oxide, magnesium hydroxide, layered composite hydroxide, layered composite oxide, boehmite, silicon dioxide, and silicon carbide; The high swelling rate polymer binder is at least one of polyvinylidene fluoride and polyacrylonitrile, and the low swelling rate polymer binder is at least one of polyethyl acrylate, polymethyl methacrylate, and ethylene-tetrafluoroethylene copolymer.
4. The multi-layer coated diaphragm according to claim 1, characterized in that: The multi-layer polymer coating comprises at least two layers; The multi-layer polymer coating is coated on one or both sides of the separator substrate.
5. A polymer battery, comprising positive and negative electrodes and a separator, wherein the separator is a multi-layer coated separator as described in any one of claims 1 to 4.
6. The method for preparing the polymer battery according to claim 5, comprising the following steps: (1) using a gravure coating method, uniformly coating a slurry of a low swelling rate polymer coating on the surface of the diaphragm substrate, and then coating a slurry of a high swelling rate polymer coating thereon at intervals to obtain a multi-layer coated diaphragm; (2) neatly stacking or winding a certain number of positive and negative electrode sheets and the multi-layer coated separator together, and encapsulating them into a polymer battery using an aluminum-plastic film; (3) placing the battery into a pressure forming cabinet for heating and pressure forming after liquid injection, so that the coating of the multi-layer coated diaphragm swells and is firmly bonded to the electrode under pressure; (4) After the hot-pressed battery is connected to a charging and discharging device for capacity separation, the battery is degassed and tightened until there is no free electrolyte in the battery core.
7. The polymer battery prepared by the multi-layer coated diaphragm according to claim 6, characterized in that: The slurry of the high swelling polymer coating comprises an inorganic material, a high swelling polymer binder and an organic solvent; The slurry of the low swelling polymer coating comprises an inorganic material, a low swelling polymer binder and an organic solvent.
8. The polymer battery prepared by the multi-layer coated diaphragm according to claim 7, characterized in that: The organic solvent is NMP; the inorganic material is at least one of aluminum oxide, magnesium hydroxide, layered composite hydroxides, layered composite oxides, boehmite, silicon dioxide, and silicon carbide.
9. The polymer battery prepared by the multi-layer coated diaphragm according to claim 6, characterized in that: The positive and negative electrode sheets are in direct contact with the high swelling rate polymer coating; The temperature range for preparing the polymer battery is 60-85° C., and the pressure range is 0.1-0.8 MPa; The polymer battery is at least one of a soft-pack battery, a cylindrical battery and a square aluminum shell battery.
10. The polymer battery prepared by the multi-layer coated diaphragm according to claim 9, characterized in that: The polymer battery is a soft-pack battery.
Citation Information
Patent Citations
Lithium ion battery and coating separator thereof
CN107611314A
Asymmetric coating composite diaphragm and preparation method and application thereof
CN111755648A
Ionic membrane, preparation method thereof and semi-solid electrolyte battery
CN112952296A
Diaphragm for lithium ion battery and lithium ion battery
CN212230512U
Composite battery diaphragm, preparation method and battery
CN108711605A