Bipolar current collector, pole piece and cylindrical battery

By using the insulating film layer of carbon chain polymer in bipolar current collector, the liquid absorption rate and liquid retention volume are improved, the problem of low liquid retention rate in the prior art is solved, and the efficient cycle stability of the battery is achieved and Manufacturing efficiency.

CN118970064APending Publication Date: 2024-11-15SHANGHAI XUANYI NEW ENERGY DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411044281.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing bipolar current collector has a low liquid retention rate, which leads to gaps in the battery during the expansion of the silicon negative electrode, which requires more electrolyte replenishment. In addition, the solid electrolyte in the solid-state battery system is costly and it is difficult to achieve the end seal design.

Method used

Design a bipolar current collector, including a positive electrode metal layer, an insulating film layer and an anode metal layer stacked in sequence. The main chain of the polymer in the insulating film layer is a carbon chain, and the groups on the branched chain have good electrophilicity. The liquid characteristics and swelling rate are controlled within the numerical range of n and m, and the liquid absorption rate and liquid retention volume are increased.

Benefits of technology

The good liquid absorption rate, liquid retention volume, strength and toughness of the bipolar current collector is achieved, the cycle stability and manufacturing efficiency of the battery are improved, and the probability of short-circuiting of the positive and negative electrodes is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970064A_ABST
    Figure CN118970064A_ABST
Patent Text Reader

Abstract

The invention provides a bipolar current collector, a pole piece and a cylindrical battery. The bipolar current collector comprises a positive electrode metal layer, an insulating film layer and a negative electrode metal layer which are sequentially stacked, the insulating film layer comprises a polymer, the structural formula of the polymer is # imgabs0 #, R1 and R2 are independently selected from any one of C1-C10 alkyl groups, C2-C10 carboxylic ester groups and C6-C10 aryl groups, R1 and R2 are different, and n + m is larger than or equal to 100 and larger than or equal to 300. The bipolar current collector has good liquid absorption rate, liquid retention capacity, strength and toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a bipolar current collector, a pole piece and a cylindrical battery. Background Art

[0002] In the full-ear winding process of cylindrical cells, the difficulty in inward diffusion and infiltration due to the cell group domain and cell structure leads to the problem of difficulty in injection. More electrolyte is needed to replenish the gaps in the silicon negative electrode expansion process, and the current bipolar current collector has a low liquid retention coefficient. Bipolar electrodes are currently more often used in series to prepare high-voltage and low-internal resistance batteries. The main problem of liquid battery systems is the difficulty in implementing end seal design, and the cost of solid electrolytes in solid-state battery systems is high. Therefore, it is urgent to develop a new type of bipolar current collector to solve the above problems. Summary of the invention

[0003] The main purpose of the present invention is to provide a bipolar current collector, a pole piece and a cylindrical battery to solve the problem of low liquid retention rate of the bipolar current collector in the prior art.

[0004] In order to achieve the above object, according to one aspect of the present invention, a bipolar current collector is provided, comprising a positive electrode metal layer, an insulating film layer and a negative electrode metal layer stacked in sequence, wherein the insulating film layer comprises a polymer, and the structural formula of the polymer is Among them, R 1 and R 2 Each independently selected from C 1 ~C 10 Alkyl, C 2 ~C 10 The carboxylate group and C 6 ~C 10 Any one of the aryl groups of 1 and R 2 Not the same, 300≥n+m≥100.

[0005] Furthermore, the above n and m are each independently a positive integer; and / or, the ratio of n to m is 3-10:7-20.

[0006] Furthermore, the above R 1 and R 2 Each independently selected from C 1 ~C 6 Alkyl, C 2 ~C 6 The carboxylate group and C 6 ~C 8 Any one of the aromatic groups; preferably R 1 is phenyl; and / or, R 2Any one selected from the group consisting of methyl formate, ethyl formate and ethyl acetate.

[0007] Furthermore, the porosity of the insulating film layer is 30-60%.

[0008] Furthermore, the ratio of the thickness of the positive electrode metal layer, the thickness of the insulating film layer and the thickness of the negative electrode metal layer is 1:5-10:0.5-1.

[0009] Furthermore, the surface density of the positive electrode metal layer is 260 to 400 g / m 2 ; and / or, the surface density of the negative electrode metal layer is 170 to 260 g / m 2 .

[0010] Furthermore, the positive electrode metal layer and the negative electrode metal layer are each independently copper foil and / or aluminum foil.

[0011] Furthermore, the areas of the positive metal layer and the negative metal layer are both smaller than the area of ​​the insulating film layer; and the projections of the edges of the positive metal layer perpendicular to the insulating film layer are all located on the insulating film layer, and the minimum distance between the position of the projection of at least one edge of the positive metal layer on the insulating film layer and the edge of the insulating film layer is 2 to 4 mm; the projections of the edges of the negative metal layer perpendicular to the insulating film layer are all located on the insulating film layer, and the minimum distance between the position of the projection of at least one edge of the negative metal layer on the insulating film layer and the edge of the negative metal layer is 2 to 4 mm.

[0012] According to another aspect of the present invention, a pole piece is provided, comprising a positive electrode active material layer, a bipolar current collector and a negative electrode active material layer stacked in sequence, the positive electrode active material layer is arranged in contact with the positive electrode metal layer of the bipolar current collector, and the negative electrode active material layer is arranged in contact with the negative electrode metal layer of the bipolar current collector, and the bipolar current collector is the aforementioned bipolar current collector.

[0013] According to another aspect of the present invention, a cylindrical battery is provided, wherein the cylindrical battery comprises the aforementioned pole piece.

[0014] Applying the technical solution of the present invention, the bipolar current collector of the present application includes a positive electrode metal layer, an insulating film layer and a negative electrode metal layer stacked in sequence. The main chain of the polymer in the insulating film layer is a carbon chain, and the type of the side chain is controlled within the above range. On the one hand, the groups on the side chains have good electrophilic electrolyte properties, which helps to improve the liquid absorption rate of the bipolar current collector; on the other hand, the presence of the groups on the side chains makes the high insulating film layer have a higher swelling rate, which helps to improve the liquid retention of the bipolar current collector. It is preferred to control the sum of the values ​​of n and m within the above range, which helps to control the molecular weight of the polymer. Too large a molecular weight of the polymer is not conducive to the processing of the high insulating film layer, and is not conducive to improving the porosity of the insulating film layer. Too small a molecular weight of the polymer is not conducive to improving the strength of the polymer. The molecular weight of the polymer corresponding to the sum of the values ​​of n and m within the above range is more conducive to improving the strength and toughness of the insulating film layer. Therefore, the bipolar current collector of the present application has good liquid absorption rate, liquid retention, strength and toughness. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0016] Figure 1 A schematic cross-sectional view of the bipolar current collector in Example 1 of the present application along the vertical direction is shown, wherein the vertical direction is the direction in which the positive electrode metal layer 1, the insulating film layer 2 and the negative electrode metal layer 3 are stacked in sequence.

[0017] The above drawings include the following reference numerals:

[0018] 1. Positive metal layer; 2. Insulating film layer; 3. Negative metal layer. DETAILED DESCRIPTION

[0019] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0020] As analyzed in the background technology of this application, the bipolar current collector in the prior art has the problem of low liquid retention rate. In order to solve the above problem, this application provides a bipolar current collector, a pole piece and a cylindrical battery.

[0021] In a typical embodiment of the present application, a bipolar current collector is provided, such as Figure 1 As shown, it includes a positive electrode metal layer 1, an insulating film layer 2 and a negative electrode metal layer 3 stacked in sequence, wherein the insulating film layer 2 includes a polymer, and the structural formula of the polymer is Among them, R 1 and R 2Each independently selected from C 1 ~C 10 Alkyl, C 2 ~C 10 The carboxylate group and C 6 ~C 10 Any one of the aryl groups of 1 and R 2 Not the same, 300≥n+m≥100.

[0022] The bipolar current collector of the present application includes a positive electrode metal layer 1, an insulating film layer 2 and a negative electrode metal layer 3 stacked in sequence. The main chain of the polymer in the insulating film layer 2 is a carbon chain, and the type of the side chain is controlled within the above range. On the one hand, the groups on the side chains have good electrophilic electrolyte properties, which helps to improve the liquid absorption rate of the bipolar current collector; on the other hand, the presence of the groups on the side chains makes the high insulating film layer 2 have a higher swelling rate, which helps to improve the liquid retention of the bipolar current collector. It is preferred to control the sum of the values ​​of n and m within the above range, which helps to control the molecular weight of the polymer. Too large a molecular weight of the polymer is not conducive to the processing of the high insulating film layer 2, and is not conducive to improving the porosity of the insulating film layer 2. Too small a molecular weight of the polymer is not conducive to improving the strength of the polymer. The molecular weight of the polymer corresponding to the sum of the values ​​of n and m within the above range is more conducive to improving the strength and toughness of the insulating film layer 2. Therefore, the bipolar current collector of the present application has good liquid absorption rate, liquid retention, strength and toughness.

[0023] In one embodiment of the present application, the above n and m are each independently a positive integer; and / or, the ratio of n to m is 3-10:7-20.

[0024] It is preferred to control the ratio of n to m within the above range, which helps to control R 1 and R 2 The quality ratio of 1 and R 2 The synergistic effect of the bipolar current collector helps to further improve the liquid absorption rate and liquid retention capacity.

[0025] In one embodiment of the present application, the above R 1 and R 2 Each independently selected from C 1 ~C 6 Alkyl, C 2 ~C 6 The carboxylate group and C 6 ~C 8 Any one of the aromatic groups; preferably R 1 is phenyl; and / or, R 2 Any one selected from the group consisting of methyl formate, ethyl formate and ethyl acetate.

[0026] The presence of aromatic groups helps to improve the strength and toughness of the bipolar current collector, and the presence of carboxylate groups helps to improve the electrophilicity of the bipolar current collector. 1 and R 2 The types are within the above range, which helps to further improve the liquid absorption rate, liquid retention, strength and toughness of the bipolar current collector.

[0027] In one embodiment of the present application, the porosity of the insulating film layer 2 is 30-60%.

[0028] The insulating film layer having the above porosity helps to increase the contact area between the polymer and the electrolyte, thereby helping to increase the liquid absorption rate and liquid retention of the bipolar current collector.

[0029] In one embodiment of the present application, the ratio of the thickness of the positive electrode metal layer 1 , the thickness of the insulating film layer 2 , and the thickness of the negative electrode metal layer 3 is 1:5-10:0.5-1.

[0030] It is preferred to control the thickness ratio of the positive metal layer 1, the insulating film layer 2 and the negative metal layer 3 within the above range, which helps to improve the synergistic effect between the three, thereby helping to further improve the liquid absorption rate and liquid retention of the bipolar current collector. In addition, it is preferred to control the thickness ratio of the positive metal layer 1, the insulating film layer 2 and the negative metal layer 3 within the above range, which helps to improve the conductivity of the bipolar current collector and helps to reduce the probability of short circuit between the positive metal layer 1 and the negative metal layer 3.

[0031] In order to further improve the conductivity of the bipolar current collector, in one embodiment of the present application, the surface density of the positive electrode metal layer 1 is 260-400 g / m 2 and / or, the surface density of the negative electrode metal layer 3 is 170 to 260 g / m 2 .

[0032] In order to control the cost of the positive metal layer 1 and the negative metal layer 3 and improve the conductivity of the bipolar current collector, in one embodiment of the present application, it is preferred that the positive metal layer 1 and the negative metal layer 3 are each independently copper foil and / or aluminum foil.

[0033] In one embodiment of the present application, the areas of the positive metal layer 1 and the negative metal layer 3 are both smaller than the area of ​​the insulating film layer 2; and the projections of the edges of the positive metal layer 1 perpendicular to the insulating film layer 2 are all located on the insulating film layer 2, and the minimum distance between the position of the projection of at least one edge of the positive metal layer 1 on the insulating film layer 2 and the edge of the insulating film layer 2 is 2 to 4 mm; the projections of the edges of the negative metal layer 3 perpendicular to the insulating film layer 2 are all located on the insulating film layer 2, and the minimum distance between the position of the projection of at least one edge of the negative metal layer 3 on the insulating film layer 2 and the edge of the negative metal layer 3 is 2 to 4 mm.

[0034] Preferably, the coating area of ​​the positive metal layer 1 and the negative metal layer 3 is within the above range, and the positive metal layer 1 and the negative metal layer 3 are staggered, and the ear welding is performed on the opposite sides of the bipolar current collector, which helps to reduce the probability of short circuit between the positive and negative electrodes during welding and makes the welding more reliable.

[0035] In another typical embodiment of the present application, a pole piece is provided, comprising a positive electrode active material layer, a bipolar current collector and a negative electrode active material layer stacked in sequence, the positive electrode active material layer is arranged in contact with the positive electrode metal layer 1 of the bipolar current collector, and the negative electrode active material layer is arranged in contact with the negative electrode metal layer 3 of the bipolar current collector, and the bipolar current collector is the aforementioned bipolar current collector.

[0036] Since the pole piece contains the bipolar current collector of the present application, the pole piece has excellent cycle stability.

[0037] In another typical embodiment of the present application, a cylindrical battery is provided, wherein the cylindrical battery comprises the aforementioned electrode sheet.

[0038] Since the cylindrical battery contains the pole piece prepared by the bipolar current collector of the present application, the cylindrical battery has excellent cycle stability. In addition, since the electrode can be a bipolar electrode, compared with a single electrode, a separator and a positive electrode or a negative electrode can be discarded in the process of preparing the battery cell, and winding is faster, more convenient and more efficient.

[0039] The beneficial effects of the present application will be further illustrated below in conjunction with embodiments.

[0040] Example 1

[0041] Styrene and ethyl acrylate in a molar ratio of 7:15 were mixed and reacted at 80°C for 2 hours under the action of cumene hydroperoxide initiator to obtain a polymer: Where n = 70, m = 150, R 1 is phenyl, R 2 The polymer is ethyl formate-based, and the porosity of the polymer is 60%. The above polymer is extruded to prepare an insulating film layer 2, and copper foil is coated on one side of the insulating film layer 2, and aluminum foil is coated on the other side of the insulating film layer 2 to obtain a bipolar current collector, wherein the thickness of the insulating film layer 2 is 7 μm, the thickness of the positive electrode metal layer 1 is 1 μm, the thickness of the negative electrode metal layer 3 is 0.7 μm, and the surface density of the positive electrode metal layer 1 is 300 g / m 2 The surface density of the negative electrode metal layer 3 is 200 g / m 2 , the positive electrode metal layer 1 is aluminum foil, and the negative electrode metal layer 3 is copper foil, wherein, Figure 1 Schematic diagram of the cross section of the bipolar current collector along the vertical direction.

[0042] Example 2

[0043] The difference from Example 1 is that methyl acrylate is used to replace ethyl acrylate, and a bipolar current collector is finally obtained.

[0044] Example 3

[0045] The difference from Example 1 is that the molar ratio of styrene to ethyl acrylate is 3:20, and a bipolar current collector is finally obtained.

[0046] Example 4

[0047] The difference from Example 1 is that the molar ratio of styrene to ethyl acrylate is 10:7, and a bipolar current collector is finally obtained.

[0048] Example 5

[0049] The difference from Example 1 is that the molar ratio of styrene to ethyl acrylate is 11:6, and a bipolar current collector is finally obtained.

[0050] Example 6

[0051] The difference from Example 1 is that the ratio of the thickness of the positive electrode metal layer 1, the thickness of the insulating film layer 2 and the thickness of the negative electrode metal layer 3 is 1:5:1, and a bipolar current collector is finally obtained.

[0052] Example 7

[0053] The difference from Example 1 is that the ratio of the thickness of the positive electrode metal layer 1, the thickness of the insulating film layer 2 and the thickness of the negative electrode metal layer 3 is 1:10:0.5, and a bipolar current collector is finally obtained.

[0054] Example 8

[0055] The difference from Example 1 is that the ratio of the thickness of the positive electrode metal layer 1, the thickness of the insulating film layer 2 and the thickness of the negative electrode metal layer 3 is 1:11:0.4, and a bipolar current collector is finally obtained.

[0056] Comparative Example 1

[0057] The difference from Example 1 is that the reaction temperature is 200°C, the reaction time is 10h, and the obtained polymer is Among them, n=7000, m=15000, and finally a bipolar current collector is obtained, wherein the porosity of the insulating film layer 2 is 23%.

[0058] Comparative Example 2

[0059] The difference from Example 1 is that polypropylene is used as the insulating film layer 2, and a bipolar current collector is finally obtained.

[0060] Performance Testing

[0061] Liquid absorption performance test

[0062] Select two locations on the current collector marked h1 and h2 and draw white lines, with the distance between h1 and h2 being 14mm. Add a few drops of purple litmus solution to the white lines, prepare a certain amount of electrolyte and pour it into a transparent container, making sure that the size of the container allows for observation of the electrolyte rising to the h2 mark. Before starting to immerse the current collector, start the timer. Then quickly insert the electrode into the electrolyte, making sure to start the timing at the moment of insertion. Observe the electrolyte rising along the electrode. When the electrolyte reaches the white line at h2, the purple litmus solution will come into contact with the electrolyte and turn red, and record the absorption time.

[0063] Electrical performance test

[0064] The positive electrode material is coated on the positive electrode metal layer of the current collector, and the negative electrode material is coated on the negative electrode metal layer of the current collector to form a pole piece. After rolling and slitting, the pole piece is wound together with the polyethylene separator to obtain a 18650 type. The winding core and the corresponding gasket are then placed in the cylindrical battery steel shell of the corresponding model and size. After welding the pole ears, injecting and sealing, it is finally assembled into a 18650 cylindrical battery. Charge to 4.20V at a constant current rate of 2.0C, and then switch to constant voltage charging until the current is <0.01C. After standing for 10 minutes, discharge to 2.50V at a constant current rate of 5.0C, and repeat the above charge and discharge process for 300 cycles.

[0065] The bipolar current collectors prepared in the above examples and comparative examples were subjected to liquid absorption performance tests and electrical performance tests. The results of liquid absorption time and capacity retention rate after 300 cycles of battery are shown in Table 1.

[0066] Table 1

[0067] Implementation / Comparative Example Absorption time / min Capacity retention rate / % Example 1 15 85 Example 2 17 83 Example 3 18 84 Example 4 20 83 Example 5 25 79 Example 6 16 85 Example 7 19 83 Example 8 24 77 Comparative Example 1 48 63 Comparative Example 2 50 60

[0068] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0069] The bipolar current collector of the present application includes a positive electrode metal layer, an insulating film layer and a negative electrode metal layer stacked in sequence. The main chain of the polymer in the insulating film layer is a carbon chain, and the type of the side chain is controlled within the above range. On the one hand, the groups on the side chains have good electrophilic electrolyte properties, which helps to improve the liquid absorption rate of the bipolar current collector; on the other hand, the presence of the groups on the side chains makes the high insulating film layer have a higher swelling rate, which helps to improve the liquid retention of the bipolar current collector. It is preferred to control the sum of the values ​​of n and m within the above range, which helps to control the molecular weight of the polymer. Too large a molecular weight of the polymer is not conducive to the processing of the high insulating film layer, and is not conducive to improving the porosity of the insulating film layer. Too small a molecular weight of the polymer is not conducive to improving the strength of the polymer. The molecular weight of the polymer corresponding to the sum of the values ​​of n and m within the above range is more conducive to improving the strength and toughness of the insulating film layer. Therefore, the bipolar current collector of the present application has good liquid absorption rate, liquid retention, strength and toughness.

[0070] The above are only embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A bipolar current collector, comprising a positive electrode metal layer (1), an insulating film layer (2) and a negative electrode metal layer (3) stacked in sequence, characterized in that: The insulating film layer (2) comprises a polymer, and the structural formula of the polymer is Wherein, R1 and R2 are each independently selected from C1 to C 10 Alkyl, C2~C 10 The carboxylate group and C6~C 10 any one of the aromatic groups, and the R1 and the R2 are different, 300≥n+m≥100.

2. The bipolar current collector according to claim 1, characterized in that: The n and the m are each independently a positive integer; and / or the ratio of the n to the m is 3-10:7-20.

3. The bipolar current collector according to claim 1 or 2, characterized in that: The R1 and R2 are each independently selected from any one of a C1-C6 alkyl group, a C2-C6 carboxylate group, and a C6-C8 aryl group; preferably, the R1 is a phenyl group; And / or, R2 is selected from any one of methyl formate, ethyl formate and ethyl acetate.

4. The bipolar current collector according to any one of claims 1 to 3, characterized in that: The porosity of the insulating film layer (2) is 30-60%.

5. The bipolar current collector according to any one of claims 1 to 4, characterized in that: The ratio of the thickness of the positive electrode metal layer (1), the thickness of the insulating film layer (2) and the thickness of the negative electrode metal layer (3) is 1:5-10:0.5-1.

6. The bipolar current collector according to any one of claims 1 to 5, characterized in that: The surface density of the positive electrode metal layer (1) is 260 to 400 g / m 2 ; and / or, the surface density of the negative electrode metal layer (3) is 170 to 260 g / m 2 .

7. The bipolar current collector according to any one of claims 1 to 6, characterized in that: The positive electrode metal layer (1) and the negative electrode metal layer (3) are each independently copper foil and / or aluminum foil.

8. The bipolar current collector according to any one of claims 1 to 7, characterized in that: The areas of the positive metal layer (1) and the negative metal layer (3) are both smaller than the area of ​​the insulating film layer (2); and the projections of the edges of the positive metal layer (1) perpendicular to the insulating film layer (2) are all located on the insulating film layer (2), and the minimum distance between the position of at least one edge of the positive metal layer (1) projected on the insulating film layer (2) and the edge of the insulating film layer (2) is 2 to 4 mm; the projections of the edges of the negative metal layer (3) perpendicular to the insulating film layer (2) are all located on the insulating film layer (2), and the minimum distance between the position of at least one edge of the negative metal layer (3) projected on the insulating film layer (2) and the edge of the negative metal layer (3) is 2 to 4 mm.

9. A pole piece, comprising a positive electrode active material layer, a bipolar current collector and a negative electrode active material layer stacked in sequence, wherein the positive electrode active material layer is arranged in contact with the positive electrode metal layer (1) of the bipolar current collector, and the negative electrode active material layer is arranged in contact with the negative electrode metal layer (3) of the bipolar current collector, characterized in that: The bipolar current collector is the bipolar current collector according to any one of claims 1 to 8.

10. A cylindrical battery, characterized in that: The cylindrical battery comprises the pole piece according to claim 9.