A water-absorbent resin and its preparation method, absorbent

Through the selection of three-stage polymer reaction system and specific monomers, the liquid permeability rate of water-absorbent resin particles is improved, the problem of insufficient liquid permeability rate in the prior art is solved, and the water-absorbent resin in various applications is realized. high performance.

CN118652368BActive Publication Date: 2024-12-03CHINA TIANCHEN ENGINEERING CORPORATION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411139125.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-12-03
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

The poor liquid permeability rate of existing water-absorbing resin particles affects their performance in various application scenarios, resulting in the convergence of liquid on the surface of the material, limiting their further application.

Method used

Using a three-stage polymer reaction system, the first monomer and the second monomer are added to the reaction system in stages, and the first polymerization reaction of the acrylic monomer is introduced with the number of carbon atoms of 4-13 in the main chain. Polyolefins regulate the density of hydrophilic functional groups and improve liquid permeability rate.

Benefits of technology

It significantly improves the absorption amount, absorption rate and liquid permeability rate of water-absorbing resin particles, and has better comprehensive performance. It is suitable for water-absorbing tissues, diapers, sanitary napkins, soil improvement agents and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118652368B_ABST
    Figure CN118652368B_ABST
Patent Text Reader

Abstract

The present invention provides a water-absorbent resin and a preparation method thereof, and an absorbent. The preparation method uses an acrylic monomer as a first monomer, a polyolefin with a main chain carbon number of 4-13 as a second monomer, and adds the first monomer at different cross-linking reaction stages by adopting a staged polymerization method, and adopts a staged polymerization reaction method of the first monomer and the second monomer, thereby ensuring that the performance parameters such as the absorption amount and absorption rate of the water-absorbent resin particles are excellent; in addition, the staged addition of the second monomer can reduce the density of the hydrophilic functional group of the main chain of the water-absorbent resin particles, and effectively improve the liquid permeability of the water-absorbent resin particles. The absorption amount, absorption rate and liquid permeability of the water-absorbent resin prepared are all excellent, and the comprehensive performance is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and in particular to a water-absorbent resin and a preparation method thereof, and an absorbent. Background Art

[0002] Water-absorbent resin particles are also called "super absorbent polymers" or "SAP" (Super Absorbent Polymers). They are mainly used to absorb and store large amounts of liquid, especially water. They have hydrophilic groups and cross-linked structures and have strong water absorption capacity. They can quickly absorb hundreds of times more water than their own weight to form a gel, and this gel can still retain water without separation under a certain pressure. Based on this characteristic, water-absorbent resin particles are widely used in daily absorbent paper towels, cosmetics, soil improvers, water-retaining agents for afforestation and seedling cultivation, dehydrating agents and other fields.

[0003] However, in practical applications, in addition to the absorption capacity and absorption rate of water-absorbent resin particles, the liquid permeability is also a performance parameter that needs to be focused on. The liquid permeability is used to characterize the rate or ability of a material to allow liquid to pass through its structure when it is saturated with water; this parameter is crucial to understanding and evaluating the performance of SAP in a variety of application scenarios. SAP with a high liquid permeability can absorb and disperse liquid faster, while SAP with a low liquid permeability may form a liquid barrier, causing liquid to accumulate on the surface of the material. The liquid permeability of existing water-absorbent resin particles still does not meet expectations, which has affected the performance of downstream products, which to a certain extent limits the further application of water-absorbent resin particles. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention discloses a water-absorbent resin and a preparation method thereof, and an absorbent. The prepared water-absorbent resin has good absorption capacity, absorption rate and liquid permeability, thereby solving the problem of poor liquid permeability of existing water-absorbent resin particles.

[0005] In order to achieve the above technical objectives, on the one hand, the present invention provides a method for preparing a water-absorbent resin, the method comprising the following steps:

[0006] S1: Adoption

[0007] S1.1, adding a first monomer aqueous solution and a first cross-linking agent to obtain a precursor mixture, wherein the precursor mixture is divided into two parts, one part is subjected to a first polymerization reaction in an organic solvent containing a surfactant to obtain a first-stage polymer; and the other part is reserved; S1.2, adding the reserved precursor mixture, a second monomer and a second cross-linking agent to the first-stage polymer to perform a second polymerization reaction to obtain a second-stage polymer;

[0008] Or adopt

[0009] S1.1, dividing the first monomer aqueous solution into two parts, subjecting one part of the first monomer aqueous solution and the first cross-linking agent to a first polymerization reaction in an organic solvent containing a surfactant to obtain a first-stage polymer; S1.2, adding another part of the first monomer aqueous solution, the second monomer and the second cross-linking agent to the first-stage polymer to conduct a second polymerization reaction to obtain a second-stage polymer;

[0010] S2: adding a third crosslinking agent to the second-stage polymer to obtain a third-stage polymer through a crosslinking reaction;

[0011] S3: The third-stage polymer is filtered and dried to obtain the water-absorbent resin;

[0012] Wherein, the step S1 also includes adding an initiator and a thickener in step S1.1, or adding an initiator and a thickener in step S1.1 and step S1.2 respectively; the first monomer is an acrylic monomer, and the first monomer aqueous solution is an acrylic monomer aqueous solution treated with alkali neutralization; the second monomer is a polyolefin with a main chain carbon number of 4-13.

[0013] The above technical solution adopts a three-stage polymer reaction system, by adding the first monomer and the second monomer to the reaction system in stages, and by adjusting the addition of the first monomer in batches in the first polymerization reaction stage and the second polymerization reaction stage, it is ensured that the water-based resin obtains excellent absorption capacity, absorption rate and other properties; on this basis, further, the above technical solution adopts a specific type of first monomer and second monomer for staged cross-linking reaction, and adds the second monomer after completing the first polymerization reaction with acrylic monomers, thereby introducing a polyolefin with a main chain carbon number of 4-13 into the main chain structure of the water-absorbent resin, thereby reducing the density of the hydrophilic functional group and effectively improving the liquid permeability of the water-absorbent resin. The embodiment of the present invention shows that the comprehensive performance of the water-absorbent resin particles prepared by the above technical solution is better, which is conducive to the use of downstream products.

[0014] It should be noted that, considering the situation that the first monomer aqueous solution, the first cross-linking agent, the initiator and the thickener will not undergo a cross-linking reaction at room temperature, the above technical scheme can choose to add the initiator and the thickener in step S1.1, or add the initiator and the thickener in both step S1.1 and step S1.2 respectively, that is, technicians in this field can add initiators and thickeners that are suitable for the first monomer equivalent at an appropriate stage in step S1 through non-creative labor, and will not affect the relevant properties of the prepared water-absorbent resin. Adaptive changes made based on this principle will fall within the scope of protection of the present invention.

[0015] It should be noted that the present invention does not limit the order of adding the first monomer aqueous solution, the first cross-linking agent, and the thickener and initiator in step S1.1, and does not limit the order of adding the first monomer aqueous solution (or the spare precursor mixture) and the second monomer, or the thickener and initiator in step S1.2. It is also possible to mix some or all of the components first and then add them to the organic solvent. Those skilled in the art can set them according to actual conditions, and the technical solutions formed thereby are all within the protection scope of the present invention.

[0016] In a further example of the present invention, the addition amount of the first monomer and the second monomer is optimized. Optionally, the molar amount of the second monomer is 1% to 20% of the molar amount of the first monomer added in step S1.2. In the embodiment of the present invention, the test results of the absorption amount, absorption rate and liquid permeability of the water-absorbent resin particles obtained when the molar amount of the second monomer in step S1.2 is different from the molar amount of the first monomer added in step S1.2 are shown. Further optionally, the molar amount of the second monomer is 5% to 15% of the molar amount of the first monomer added in step S1.2, further 6% to 14%, further 7% to 13%, and further 9% to 11%.

[0017] In a further example of the present invention, the type of the second monomer is preferably selected. The second monomer can be a 1,ω-divalent aliphatic olefin with 4-13 carbon atoms in the main chain, thereby promoting the rigidity of the prepared water-absorbent resin particles to avoid excessive softness leading to excessive liquid permeability or excessive rigidity affecting the absorption capacity, absorption rate, comfort and other properties. Further optionally, the second monomer can be a 1,ω-divalent aliphatic olefin with 7, 8, 9, or 10 carbon atoms in the main chain.

[0018] In a further example of the present invention, the amount of the first monomer used in the first cross-linking stage and the second cross-linking stage is optimized. Optionally, the molar ratio of the amount of the first monomer used in step S1.1 and step S1.2 is 9:1~1:1; through further exploratory experiments, the molar ratio of the amount of the first monomer used in step S1.1 and step S1.2 can be selected as 8:1~1:1, further selected as 6:1~1:1, and further selected as 3:1~1.5:1; based on a large amount of experimental data, the molar ratio of the amount of the first monomer used in step S1.1 and step S1.2 can be further selected as 2.5:1~1.5:1.

[0019] In the above technical solution, there is no restriction on the type of the acrylic monomer, and those skilled in the art can set it according to the actual situation. In a further example of the present invention, the acrylic monomer may optionally include at least one of (meth)acrylic acid and its salts, 2-hydroxyethyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, and N,N-diethylaminopropyl (meth)acrylate. Among them, (meth)acrylic acid and its salts should be understood as acrylic acid and its salts and methacrylic acid and its salts, and the remaining compounds are understood in the same way as the compound.

[0020] In a further example of the present invention, the concentration of the acrylic acid monomer aqueous solution is explored and optimized, and can be 10wt%-50wt%, further 20wt%-40wt%, and further 25wt%-35wt%, thereby simplifying the process and improving the process operability. It should be noted that the present invention does not limit the specific operation of the alkali neutralization treatment of the first monomer aqueous solution. Those skilled in the art can select a suitable alkali solution for alkali neutralization based on the purpose of achieving the acrylic acid monomer aqueous solution, such as by dripping sodium hydroxide or potassium hydroxide solution, and the technical solutions formed thereby are all within the protection scope of the present invention.

[0021] In a further example of the present invention, the control conditions of the staged cross-linking reaction are explored. Optionally, the temperature of the first polymerization reaction is the azeotropic temperature of water and the organic solvent; and / or, the temperature of the second polymerization reaction is the azeotropic temperature of water and the organic solvent, and / or, the temperature of the cross-linking reaction is the azeotropic temperature of water and the organic solvent, so as to facilitate the cross-linking reaction of each stage to form a uniform and stable cross-linked network, and it is easier to operate. Optionally, the reaction temperature of the first polymerization reaction is 60°C~100°C; and / or, the reaction temperature of the second polymerization reaction is 60°C~100°C; and / or, the reaction temperature of the cross-linking reaction is 60°C~100°C. Optionally, the reaction time of the first polymerization reaction is 0.5h~2h; and / or, the reaction time of the second polymerization reaction is 0.5h~2h; and / or, the reaction time of the cross-linking reaction is 0.5h~2h.

[0022] In a further example of the present invention, the amount of the first crosslinking agent and the second crosslinking agent in step S1 is explored and optimized. Optionally, the molar ratio of the second crosslinking agent to the first monomer added in step S1.2 is recorded as A, and the molar ratio of the first crosslinking agent to the first monomer added in step S1.1 is recorded as B, the value range of B is 1 / 10000~1 / 1000, and the ratio of A to B is (2:1~10:1), thereby organically combining the phased addition of the first monomer of the crosslinking agent and the crosslinking reaction between the first monomer and the second monomer, promoting crosslinking polymerization between the monomers, and improving the strength, rigidity and stability of the prepared water-absorbing resin particles.

[0023] In a further example of the present invention, the molar amount of the third crosslinking agent is 1 / 100000 to 1 / 1000 of the molar amount of the first monomer used in step S1, which increases the hardness and wear resistance of the prepared water-absorbing resin particles and improves their surface properties and overall performance. It should be noted that the present invention does not limit the form of the third crosslinking agent, and the third crosslinking agent can be selected as an aqueous solution, which is conducive to obtaining a uniform and stable crosslinked network through a crosslinking reaction.

[0024] In a further example of the present invention, the types of the first cross-linking agent, the second cross-linking agent and the third cross-linking agent are preferred. Optionally, the first cross-linking agent, the second cross-linking agent and the third cross-linking agent are independently selected from at least one of ethylene glycol, propylene glycol, 1,4-butylene glycol, trimethylolpropane, glycerol, polyethylene glycol, polypropylene glycol, polyglycerol, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, polyglycerol diglycidyl ether, epichlorohydrin, epibromohydrin, α-methyl epichlorohydrin, N,N'-methylenebisacrylamide, trimethylolpropane tri(meth)acrylate, trimethylolmethanol tri(meth)acrylate, trimethylolethanol tri(meth)acrylate, trimethylolpropane triglycidyl ether, triaminomethylmethane tri(meth)acrylamide, triaminomethylethane tri(meth)acrylamide, and triaminomethylpropane tri(meth)acrylamide.

[0025] In the above technical scheme, there is no restriction on the type of the organic solvent, and those skilled in the art can set it according to actual conditions. In a further example of the present invention, the organic solvent can be selected from one or more of chain aliphatic hydrocarbons, alicyclic hydrocarbons, and aromatic hydrocarbons; wherein the chain aliphatic hydrocarbons can be further selected from chain aliphatic hydrocarbons with 6-8 carbon atoms, the alicyclic hydrocarbons can be further selected from alicyclic hydrocarbons with 6-8 carbon atoms, and the aromatic hydrocarbons can be further selected from at least one compound of aromatic hydrocarbons such as benzene, toluene, and xylene, for example: chain aliphatic hydrocarbons can be n-hexane, n-heptane, 2-methylhexane, 3-methylhexane, 2,3-dimethylpentane, 3-ethylpentane, n-octane, etc.; alicyclic hydrocarbons can be cyclohexane, methylcyclohexane, cyclopentane, methylcyclopentane, trans-1,2-dimethylcyclopentane, cis-1,3-dimethylcyclopentane, trans-1,3-dimethylcyclopentane, etc. Those skilled in the art may use any one of the above organic solvents alone or in any combination, which is not restrictive; preferably, the organic solvent is cyclohexane to ensure that the quality of the obtained cyclohexane is stable, thereby effectively ensuring the absorption amount and absorption rate of the prepared water-absorbent resin particles.

[0026] In a further example of the present invention, the molar amount of the organic solvent is 1 to 3 times the molar amount of the first monomer used in step S1, thereby ensuring that the resin is fully mixed and reacted during the synthesis process to obtain a uniform molecular structure and network structure.

[0027] In the above technical scheme, there is no restriction on the type of the surfactant, and those skilled in the art can set it according to the actual situation. In a further example of the present invention, the surfactant includes sucrose fatty acid ester, polyglycerol fatty acid ester, sorbitan fatty acid ester, polyoxyethylene sorbitan fatty acid ester, polyoxyethylene glycerol fatty acid ester, sorbitol fatty acid ester, polyoxyethylene sorbitol fatty acid ester, polyoxyethylene alkyl ether, polyoxyethylene alkylphenyl ether, polyoxyethylene castor oil, polyoxyethylene hydrogenated castor oil, alkyl allyl formaldehyde condensation polyoxyethylene ether, polyoxyethylene polyoxypropylene block copolymer, polyoxyethylene polyoxypropyl alkyl ether, polyethylene glycol fatty acid ester, alkyl glucoside, N- At least one of alkyl glucose amide, polyoxyethylene fatty acid amide, polyoxyethylene alkylamine, phosphate ester of polyoxyethylene alkyl ether, and phosphate ester of polyoxyethylene alkyl allyl ether; further can be selected from at least one of sucrose fatty acid ester, polyglycerol fatty acid ester, sorbitan fatty acid ester, polyoxyethylene sorbitan fatty acid ester, polyoxyethylene glycerol fatty acid ester, sorbitol fatty acid ester, and polyoxyethylene sorbitol fatty acid ester; those skilled in the art can use any of the above surfactants alone or in any combination, which is not restrictive. In an optional embodiment of the present invention, the surfactant is sorbitan stearate to effectively ensure the dispersion stability of the monomer.

[0028] In a further example of the present invention, the molar amount of the surfactant can be selected to be 1 / 1000~5 / 1000 of the molar amount of the organic solvent; further, it can be selected to be 2 / 1000~4 / 1000, which facilitates the simplification of the process flow and improves stability.

[0029] In the above technical solution, there is no restriction on the type of the initiator, and those skilled in the art can set it according to actual conditions. In a further example of the present invention, the initiator can be a water-soluble free radical initiator, specifically, the initiator includes at least one of persulfate, peroxide, and azo water-soluble free radical initiator; further optionally, the persulfate includes potassium persulfate, ammonium persulfate, and sodium persulfate; further optionally, the peroxide includes methyl ethyl ketone peroxide, methyl isobutyl ketone peroxide, di-tert-butyl peroxide, tert-butyl isopropyl peroxide, tert-butyl acetate peroxide, tert-butyl isobutyrate peroxide, tert-butyl pivalate peroxide, and hydrogen peroxide; further optionally, Optionally, the azo water-soluble free radical initiator includes 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(N-phenylamidino)propane] dihydrochloride, 2,2'-azobis[2-(N-allylamidino)propane] dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} dihydrochloride, 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide], and 4,4'-azobis(4-cyanovaleric acid).

[0030] In a further example of the present invention, the molar ratio of the first monomer to the initiator in step S1 can be selected as 1:(0.0002-0.001), and further can be selected as 1:(0.0003-0.0005), thereby improving the stability and polymerization reaction rate of the prepared water-absorbing resin particles, etc., and helping to improve process efficiency.

[0031] In the above technical solution, there is no restriction on the type of the thickener, and those skilled in the art can set it according to actual conditions. In a further example of the present invention, the thickener includes at least one of hydroxyethyl cellulose, hydroxypropyl cellulose, methyl cellulose, carboxymethyl cellulose, polyacrylic acid, partially neutralized polyacrylic acid, polyethylene glycol, polyacrylamide, polyethyleneimine, dextrin, sodium alginate, polyvinyl alcohol, polyvinyl pyrrolidone, and polyethylene oxide.

[0032] In a further example of the present invention, the molar ratio of the acrylic monomer to the thickener is 1:(0.05-0.2), and can further be 1:(0.1-0.15), so as to regulate the viscosity of the overall mixture and further regulate the particle size of the obtained water-absorbent resin particles and other related performance parameters.

[0033] On the other hand, the present invention provides a water-absorbent resin, which is prepared by the above method.

[0034] In another aspect, the present invention provides an absorbent body comprising the above-mentioned water-absorbent resin.

[0035] Furthermore, the present invention proposes the use of the above-mentioned water-absorbent resin or absorbent in absorbent paper towels, diapers, sanitary napkins, soil conditioners, water-retaining agents, and dehydrating agents.

[0036] Compared with the prior art, the beneficial effects of the present invention are as follows: the preparation method of the water-absorbent resin of the present invention adopts a staged polymerization method to add the first monomer at different cross-linking reaction stages, and adopts a staged cross-linking reaction method between the first monomer and the second monomer, thereby ensuring that the performance parameters such as the absorption amount and absorption rate of the water-absorbent resin particles are excellent; in addition, the introduction of the second monomer can reduce the density of the hydrophilic functional groups of the main chain of the obtained water-absorbent resin particles, and effectively improve the liquid permeability of the water-absorbent resin particles. The absorption amount, absorption rate and liquid permeability of the obtained water-absorbent resin are all excellent, and the comprehensive performance is excellent. The obtained water-absorbent resin and the absorbent containing the water-absorbent resin can be widely used in absorbent paper towels, diapers, sanitary napkins, soil conditioners, water-retaining agents, dehydrating agents and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0038] Figure 1 The schematic diagrams of the structures of the water-absorbent resins prepared in Example 1 and Comparative Example 1 of the present invention are shown;

[0039] Among them, "~" represents the main chain and "○" represents the hydrophilic functional group;

[0040] Figure 2 A photograph of the water-absorbent resin prepared in Example 3.1 is shown. DETAILED DESCRIPTION

[0041] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively below, and preferred embodiments of the present invention are given. However, it should be understood that these embodiments are only used for more detailed description and should not be understood as limiting the present invention in any form, i.e., not intended to limit the scope of protection of the present invention.

[0042] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0043] It should be noted that, in the description of the preferred embodiment, unless otherwise clearly specified and limited, the terms "first", "second" and "third" are used for descriptive purposes only. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances, and therefore they cannot be understood as limitations on the present invention.

[0044] It should be noted that in the following embodiments and comparative examples of the present invention, the absorption amount, absorption rate and liquid permeability are detected by the following method:

[0045] The absorption capacity is tested using 0.9% sodium chloride aqueous solution as simulated urine according to the test method specified in GB / T 22875-2018 (unit: s).

[0046] The absorption rate is measured according to the test method specified in Japanese Industrial Standard JIS-K-7224-1996-R2006.

[0047] The liquid permeability test experiment of water-absorbent resin particles is carried out in a device including an upper cylinder, a middle cylinder and a lower funnel. Among them, the middle cylinder is a cylinder with an inner diameter of 7 cm, and a porous glass plate with equal-diameter filter paper is provided at the bottom; after 60g of water-absorbent resin particle sample is placed in the middle cylinder, it is compacted with a glass plate carrying a 350g weight; after the middle cylinder is loaded, the glass plate is removed and a rapid qualitative filter paper is covered on the top of the middle cylinder, and then the upper cylinder and the middle cylinder are bolted together; the lower part of the middle cylinder is connected to a circular triangular funnel with a circular opening inner diameter of 7cm and a straight barrel inner diameter of 2cm. During the test, 100mL of sodium chloride aqueous solution with a concentration of 0.9% is quickly poured into the upper cylinder, and a graduated measuring cylinder is used to collect the liquid flowing down from the triangular funnel. A stopwatch is used to record the volume of liquid retained in the measuring cylinder within 1 minute from the start of pouring physiological saline, which is recorded as the liquid permeability (unit ml).

[0048] Example 1

[0049] A method for preparing a water-absorbent resin, specifically, adding 350 mL of cyclohexane and 3 g of sorbitan stearate (Span 60) surfactant to a glass jacketed reactor with a volume of 1000 mL, setting the stirring speed to 250 rpm, turning on the heating system, raising the temperature of the liquid in the reactor to 50°C, and dissolving the sorbitan stearate. On the other hand, adding 90 g of acrylic acid (1.25 mol) and 90 g of deionized water to a glass flask, mixing the two uniformly under magnetic stirring, then dropping 120 g of a 32% sodium hydroxide aqueous solution through a constant pressure dropping funnel, and controlling the system temperature to not exceed 30°C by water bath cooling to obtain a first monomer aqueous solution.

[0050] S1.1, under stirring, add 60 mg of crosslinking agent N,N'-methylenebisacrylamide (molecular weight 154.17, relative to acrylic acid monomer 3.2×10 -4 mol), 30 mg thickener hydroxyethyl cellulose, 300 mg potassium persulfate initiator, and after all solids are dissolved, a precursor mixture is obtained; 200 g of the precursor mixture is taken out and added to a glass reactor, and then the heating system is turned on to raise the jacket temperature of the glass jacket reactor to 90°C. After the temperature of the gas phase in the reactor is monitored to be stable, stirring is maintained for 1 hour to obtain the first stage polymer. The heating system is turned off, stirring is maintained, and the temperature in the reactor is cooled to room temperature.

[0051] S1.2, on the other hand, add 60 mg of cross-linking agent N,N'-methylenebisacrylamide to the remaining precursor mixture. After all the solids are dissolved, add all the remaining precursor mixture into the glass reactor, then add 2 g of 1,6-heptadiene (20.8 mmol), turn on the heating system to raise the jacket temperature of the glass jacket reactor to 90°C again. After monitoring the temperature of the gas phase in the reactor and stabilizing it, keep stirring for 1 hour to obtain the second stage polymer.

[0052] S2, open the reflux condensation system, remove water from the polymer by azeotropic distillation of cyclohexane and water, and when the oil-water interface in the oil-water separator no longer changes, add 10g of 5% by mass concentration of ethylene glycol diglycidyl ether aqueous solution into the reactor, keep the jacket at 90°C for cross-linking for 1 hour to obtain the third stage polymer, and then continue to remove the remaining water in the system by azeotropic distillation of cyclohexane and water.

[0053] S3, turn off the heating system, cool the contents of the kettle to room temperature, then filter out the solid product, dry it, and obtain the granular absorbent resin. After testing, the absorbent resin particles have an absorption capacity of 61 g / g, an absorption rate of 28 s, and a liquid permeability of 15.2 ml. The structural diagram of the absorbent resin is shown in FIG. Figure 1 The supporting data for this structural diagram comes from the scanning electron microscope EDS energy scattering spectrum (see Table 1).

[0054] Table 1

[0055]

[0056] Comparative Example 1

[0057] 350 mL of cyclohexane and 3 g of sorbitan stearate (Span 60) surfactant were added to a glass jacketed reactor with a volume of 1000 mL. The stirring speed was set to 250 rpm. The heating system was turned on to raise the temperature of the liquid in the reactor to 50 ° C, and the sorbitan stearate was dissolved. On the other hand, 90 g of acrylic acid and 90 g of deionized water were added to a glass flask. Under magnetic stirring, the two were mixed evenly, and then 120 g of a 32% sodium hydroxide aqueous solution was added dropwise through a constant pressure dropping funnel. The system temperature was controlled not to exceed 30 ° C by water bath cooling.

[0058] Under stirring, 60 mg of crosslinking agent N,N'-methylenebisacrylamide (molecular weight 154.17, relative to acrylic acid monomer 3.2×10 -4 mol), 30 mg thickener hydroxyethyl cellulose, 300 mg potassium persulfate initiator, after all solids are dissolved, 200 g of the first monomer aqueous solution is taken out and added to the glass reactor, and then the heating system is turned on to raise the jacket temperature of the glass jacket reactor to 90° C. After starting reflux, stirring is maintained for 1 hour to obtain the first stage polymer.

[0059] The heating system was turned off, stirring was maintained, and the temperature in the reactor was cooled to room temperature. On the other hand, 60 mg of the cross-linking agent N,N'-methylenebisacrylamide was added to the remaining first monomer aqueous solution. After all the solids were dissolved, the remaining first monomer aqueous solution was added to the glass jacket reactor, and the heating system was turned on to raise the jacket temperature of the glass jacket reactor to 90° C. After reflux began, stirring was maintained for 1 hour to obtain the second stage polymer.

[0060] The reflux condensation system was turned on, and the water in the polymer was removed by azeotropic distillation of cyclohexane and water. When the oil-water interface in the oil-water separator no longer changed, 10 g of 5% mass concentration of ethylene glycol diglycidyl ether aqueous solution was added to the reactor, and the jacket was kept warm at 90°C for 1 hour for crosslinking. After that, the remaining water in the system was continued to be removed by azeotropic distillation of cyclohexane and water. The heating system was turned off, and the solid product was filtered out after cooling to room temperature, and dried to obtain a granular absorbent resin. After testing, the absorbent resin had an absorption capacity of 59 g / g, an absorption rate of 32 s, and a liquid permeability of 3.6 ml. The structural schematic diagram of the absorbent resin is shown in FIG. Figure 1 The supporting data for this structural diagram comes from the scanning electron microscope EDS energy scattering spectrum (as shown in Table 2).

[0061] Table 2

[0062]

[0063] Comparative Example 2

[0064] 350 mL of cyclohexane and 3 g of sorbitan stearate (Span 60) surfactant were added to a glass jacketed reactor with a volume of 1000 mL. The stirring speed was set to 250 rpm. The heating system was turned on to raise the temperature of the liquid in the reactor to 50 ° C, and the sorbitan stearate was dissolved. On the other hand, 90 g of acrylic acid and 90 g of deionized water were added to a glass flask. Under magnetic stirring, the two were mixed evenly, and then 120 g of a 32% sodium hydroxide aqueous solution was added dropwise through a constant pressure dropping funnel. The system temperature was controlled not to exceed 30 ° C by water bath cooling.

[0065] Under stirring, 60 mg of crosslinking agent N,N'-methylenebisacrylamide (molecular weight 154.17, relative to acrylic acid monomer 3.2×10 -4 mol), 30 mg thickener hydroxyethyl cellulose, 300 mg potassium persulfate initiator, after all solids are dissolved, all the first monomer aqueous solution is added to the glass reactor, and then the heating system is turned on to raise the jacket temperature of the glass jacket reactor to 90°C. After starting reflux, stirring is maintained for 1 hour to obtain the first stage polymer.

[0066] The heating system was turned off, stirring was maintained, and the temperature in the reactor was cooled to room temperature. Then, 4 g of 1,6-heptadiene (41.6 mmol) and 40 mg of potassium persulfate initiator were added, and the heating system was turned on to raise the jacket temperature of the glass jacket reactor to 90° C. After reflux began, stirring was maintained for 1 hour to obtain a second-stage polymer.

[0067] The reflux condensation system was turned on, and the water in the polymer was removed by azeotropic distillation of cyclohexane and water. When the oil-water interface in the oil-water separator no longer changed, 10g of ethylene glycol diglycidyl ether aqueous solution with a mass concentration of 5% was added to the reactor, and the jacket was kept at 90°C for crosslinking for 1 hour. After that, the remaining water in the system was continued to be removed by azeotropic distillation of cyclohexane and water, and the heating system was turned off. After cooling to room temperature, the solid product was filtered out and dried to obtain a granular water-absorbent resin. After testing, the absorption capacity of the water-absorbent resin was 53g / g, the absorption rate was 59s, and the liquid permeability was 5.8ml.

[0068] Example 2

[0069] A method for preparing a water-absorbent resin, specifically, adding 350 mL of cyclohexane and 3 g of sorbitan stearate (Span 60) surfactant to a glass jacketed reactor with a volume of 1000 mL, setting the stirring speed to 250 rpm, turning on the heating system, raising the temperature of the liquid in the reactor to 50°C, and dissolving the sorbitan stearate. On the other hand, adding 90 g of acrylic acid (1.25 mol) and 90 g of deionized water to a glass flask, mixing the two uniformly under magnetic stirring, then dropping 120 g of a 32% sodium hydroxide aqueous solution through a constant pressure dropping funnel, and controlling the system temperature to not exceed 30°C by water bath cooling to obtain a first monomer aqueous solution.

[0070] S1.1, take out 200g of the first monomer aqueous solution, add 40mg of crosslinking agent N,N'-methylenebisacrylamide (molecular weight 154.17, relative to acrylic acid monomer 2.13×10 -4 mol), 20 mg thickener hydroxypropyl cellulose, 200 mg potassium persulfate initiator, after all solids are dissolved, add into the glass reactor, then turn on the heating system to raise the jacket temperature of the glass jacket reactor to 90°C. After monitoring the temperature of the gas phase in the reactor and stabilizing, keep stirring for 1 hour to obtain the first stage polymer.

[0071] S1.2, turn off the heating system, keep stirring, and cool the temperature in the reactor to room temperature. On the other hand, add 80 mg of cross-linking agent N, N'-methylenebisacrylamide, 10 mg of thickener hydroxypropyl cellulose, and 100 mg of potassium persulfate initiator to the remaining first monomer aqueous solution under stirring. After all the solids are dissolved, add all the remaining first monomer aqueous solution to the glass reactor, then add 2 g of 1,6-heptadiene (20.8 mmol), turn on the heating system to raise the jacket temperature of the glass jacket reactor to 90°C again. After monitoring the temperature of the gas phase in the reactor to stabilize, keep stirring for 1 hour to obtain the second stage polymer.

[0072] S2, open the reflux condensation system, remove water from the polymer by azeotropic distillation of cyclohexane and water, and when the oil-water interface in the oil-water separator no longer changes, add 10g of 5% by mass concentration of ethylene glycol diglycidyl ether aqueous solution into the reactor, keep the jacket at 90°C for cross-linking for 1 hour to obtain the third stage polymer, and then continue to remove the remaining water in the system by azeotropic distillation of cyclohexane and water.

[0073] S3, turn off the heating system, cool the contents in the kettle to room temperature, filter out the solid product, dry it, and obtain the water-absorbent resin in granular form. After testing, the water-absorbent resin particles have an absorption capacity of 62 g / g, an absorption rate of 27 s, and a liquid permeability of 14.3 ml.

[0074] Example 3

[0075] A method for preparing a water-absorbent resin, specifically, adding 350 mL of cyclohexane and 3 g of a sorbitol fatty acid ester surfactant to a glass jacketed reactor with a volume of 1000 mL, setting the stirring speed to 250 rpm, turning on the heating system, raising the temperature of the liquid in the reactor to 50° C., and dissolving the sorbitol fatty acid ester. On the other hand, adding 90 g of acrylic acid (1.25 mol) and 90 g of deionized water to a glass flask, mixing the two uniformly under magnetic stirring, then dropping 120 g of a 32% sodium hydroxide aqueous solution through a constant pressure dropping funnel, and controlling the system temperature to not exceed 30° C. by water bath cooling to obtain a first monomer aqueous solution.

[0076] S1.1, under stirring, add 60 mg of crosslinking agent N,N'-methylenebisacrylamide (molecular weight 154.17, relative to acrylic acid monomer 3.2×10 -4 mol), 30 mg thickener hydroxyethyl cellulose, 300 mg potassium persulfate initiator, and after all solids are dissolved, a precursor mixture is obtained; 200 g of the precursor mixture is taken out and added to a glass reactor, and then the heating system is turned on to raise the jacket temperature of the glass jacket reactor to 90°C. After the temperature of the gas phase in the reactor is monitored to be stable, stirring is maintained for 1 hour to obtain the first stage polymer. The heating system is turned off, stirring is maintained, and the temperature in the reactor is cooled to room temperature.

[0077] S1.2, on the other hand, add 20 mg of cross-linking agent N,N'-methylenebisacrylamide to the remaining precursor mixture. After all the solids are dissolved, add all the remaining precursor mixture into the glass reactor, then add an appropriate amount of 1,6-heptadiene, turn on the heating system to raise the jacket temperature of the glass jacket reactor to 90°C again. After monitoring the temperature of the gas phase in the reactor to stabilize, keep stirring for 1 hour to obtain the second stage polymer.

[0078] S2, open the reflux condensation system, remove water from the polymer by azeotropic distillation of cyclohexane and water, and when the oil-water interface in the oil-water separator no longer changes, add 10g of 5% by mass concentration of ethylene glycol diglycidyl ether aqueous solution into the reactor, keep the jacket at 90°C for cross-linking for 1 hour to obtain the third stage polymer, and then continue to remove the remaining water in the system by azeotropic distillation of cyclohexane and water.

[0079] S3, turning off the heating system, allowing the material in the kettle to cool to room temperature, then filtering out the solid product, drying it, and obtaining the granular water-absorbent resin.

[0080] In this embodiment, other parameters remain unchanged, only the molar ratio of the second monomer to the first monomer added in step S1.2 is changed. The specific parameter adjustments of Examples 3.1-3.3 and Comparative Examples 3.1-3.2 and the absorption capacity, absorption rate and liquid permeability of the prepared water-absorbent resin are shown in Table 3. The photo of the water-absorbent resin prepared in Example 3.1 is shown in Figure 2 , the particle size of the water-absorbent resin is 500-800 microns.

[0081] Table 3

[0082]

[0083] Example 4

[0084] A method for preparing a water-absorbent resin, specifically, adding 350 mL of cyclohexane and 3 g of sorbitan stearate (Span 60) surfactant to a glass jacketed reactor with a volume of 1000 mL, setting the stirring speed to 250 rpm, turning on the heating system, raising the temperature of the liquid in the reactor to 50°C, and dissolving the sorbitan stearate. On the other hand, adding 90 g of acrylic acid (1.25 mol) and 90 g of deionized water to a glass flask, mixing the two uniformly under magnetic stirring, then dropping 120 g of a 32% sodium hydroxide aqueous solution through a constant pressure dropping funnel, and controlling the system temperature to not exceed 30°C by water bath cooling to obtain a first monomer aqueous solution.

[0085] S1.1, under stirring, add 60 mg of crosslinking agent N,N'-methylenebisacrylamide (molecular weight 154.17, relative to acrylic acid monomer 3.2×10 -4 mol), 30 mg of thickener carboxymethyl cellulose, 300 mg of potassium persulfate initiator, and after all solids are dissolved, a precursor mixture is obtained; 200 g of the precursor mixture is taken out and added to a glass reactor, and then the heating system is turned on to raise the jacket temperature of the glass jacket reactor to 90°C. After the temperature of the gas phase in the reactor is monitored to be stable, stirring is maintained for 1 hour to obtain the first stage polymer. The heating system is turned off, stirring is maintained, and the temperature in the reactor is cooled to room temperature.

[0086] S1.2, on the other hand, add 60 mg of cross-linking agent N,N'-methylenebisacrylamide to the remaining precursor mixture. After all the solids are dissolved, add all the remaining precursor mixture into the glass reactor, then add the second monomer, turn on the heating system to raise the jacket temperature of the glass jacket reactor to 90°C again. After monitoring the temperature of the gas phase in the reactor to stabilize, keep stirring for 1 hour to obtain the second stage polymer.

[0087] S2, open the reflux condensation system, remove water from the polymer by azeotropic distillation of cyclohexane and water, and when the oil-water interface in the oil-water separator no longer changes, add 10g of 5% by mass concentration of ethylene glycol diglycidyl ether aqueous solution into the reactor, keep the jacket at 90°C for cross-linking for 1 hour to obtain the third stage polymer, and then continue to remove the remaining water in the system by azeotropic distillation of cyclohexane and water.

[0088] S3, turning off the heating system, allowing the material in the kettle to cool to room temperature, then filtering out the solid product, drying it, and obtaining the granular water-absorbent resin.

[0089] In this embodiment, other parameters remain unchanged, only the type and amount of the second monomer added are changed. The specific parameter adjustments and the absorption capacity, absorption rate and liquid permeability of the prepared water-absorbent resin are shown in Table 4.

[0090] Table 4

[0091]

[0092] Example 5

[0093] A method for preparing a water-absorbent resin, specifically, adding 350 mL of cyclohexane and 3 g of a polyoxyethylene sorbitol fatty acid ester surfactant to a glass jacketed reactor with a volume of 1000 mL, setting the stirring speed to 250 rpm, turning on the heating system, raising the temperature of the liquid in the reactor to 50° C., and dissolving the polyoxyethylene sorbitol fatty acid ester. On the other hand, adding 90 g of acrylic acid (1.25 mol) and 90 g of deionized water to a glass flask, mixing the two uniformly under magnetic stirring, then dropping 120 g of a 32% sodium hydroxide aqueous solution through a constant pressure dropping funnel, and controlling the system temperature to not exceed 30° C. by water bath cooling to obtain a first monomer aqueous solution.

[0094] S1.1, under stirring, add 60 mg of crosslinking agent N,N'-methylenebisacrylamide (molecular weight 154.17, relative to acrylic acid monomer 3.2×10 -4 mol), 30 mg thickener hydroxyethyl cellulose, 300 mg potassium persulfate initiator, and after all solids are dissolved, a precursor mixture is obtained; a portion of the precursor mixture is taken out and added to a glass reactor, and then the heating system is turned on to raise the jacket temperature of the glass jacket reactor to 90°C. After the temperature of the gas phase in the reactor is monitored to be stable, stirring is maintained for 1 hour to obtain the first stage polymer.

[0095] S1.2, turn off the heating system, keep stirring, and cool the temperature in the reactor to room temperature. On the other hand, add a 1.28×10 -3Add the corresponding amount of cross-linking agent N,N'-methylenebisacrylamide, and after all the solids are dissolved, add all the remaining precursor mixture into the glass reactor, then add the corresponding amount of 1,6-heptadiene at a molar amount of the second monomer of 3.33% of the molar amount of the first monomer added in step S1.2, and turn on the heating system to raise the jacket temperature of the glass jacket reactor to 90°C again. After monitoring the temperature of the gas phase in the reactor to stabilize, keep stirring for 1 hour to obtain the second stage polymer.

[0096] S2, open the reflux condensation system, remove water from the polymer by azeotropic distillation of cyclohexane and water, and when the oil-water interface in the oil-water separator no longer changes, add 10g of 5% by mass concentration of ethylene glycol diglycidyl ether aqueous solution into the reactor, keep the jacket at 90°C for cross-linking for 1 hour to obtain the third stage polymer, and then continue to remove the remaining water in the system by azeotropic distillation of cyclohexane and water.

[0097] S3, turning off the heating system, allowing the material in the kettle to cool to room temperature, then filtering out the solid product, drying it, and obtaining the granular water-absorbent resin.

[0098] In this embodiment, other parameters remain unchanged, and only the molar ratio of the first monomer in step S1.1 and step S1.2 is changed. The specific parameter adjustments and the absorption capacity, absorption rate and liquid permeability of the prepared water-absorbent resin are shown in Table 5.

[0099] Table 5

[0100]

[0101] Example 6

[0102] A method for preparing a water-absorbent resin, specifically, adding 350 mL of cyclohexane and 3 g of sorbitan stearate (Span 60) surfactant to a glass jacketed reactor with a volume of 1000 mL, setting the stirring speed to 250 rpm, turning on the heating system, raising the temperature of the liquid in the reactor to 50°C, and dissolving the sorbitan stearate. On the other hand, adding 90 g of acrylic acid (1.25 mol) and 90 g of deionized water to a glass flask, mixing the two uniformly under magnetic stirring, then dropping 120 g of a 32% sodium hydroxide aqueous solution through a constant pressure dropping funnel, and controlling the system temperature to not exceed 30°C by water bath cooling to obtain a first monomer aqueous solution.

[0103] S1.1, under stirring, add 3.2×10 -4mol of the first crosslinking agent, 30 mg of the thickener hydroxyethyl cellulose, 300 mg of potassium persulfate initiator were added, and after all the solids were dissolved, a precursor mixture was obtained. 200 g of the precursor mixture was taken out and added to a glass reactor, and then the heating system was turned on to raise the jacket temperature of the glass jacket reactor to 90° C. After the temperature of the gas phase in the reactor was monitored to be stable, stirring was maintained for 1 hour to obtain a first-stage polymer.

[0104] S1.2, turn off the heating system, keep stirring, and cool the temperature in the reactor to room temperature. On the other hand, add 10% of the first monomer to the remaining precursor mixture. -3 After all the solids are dissolved, the remaining precursor mixture is added to the glass reactor, followed by 4 g of 1,6-heptadiene (41.6 mmol), and the heating system is turned on to raise the jacket temperature of the glass jacket reactor to 90°C again. After the temperature of the gas phase in the reactor is monitored and stabilized, stirring is maintained for 1 hour to obtain the second stage polymer.

[0105] S2, open the reflux condensation system, remove water from the polymer by azeotropic distillation of cyclohexane and water, and when the oil-water interface in the oil-water separator no longer changes, add 10g of 5% by mass concentration of trimethylolpropane triacrylate aqueous solution into the reactor, keep the jacket at 90°C for cross-linking for 1 hour to obtain the third stage polymer, and then continue to remove the remaining water in the system by azeotropic distillation of cyclohexane and water.

[0106] S3, turning off the heating system, allowing the material in the kettle to cool to room temperature, then filtering out the solid product, drying it, and obtaining the granular water-absorbent resin.

[0107] In this embodiment, other parameters remain unchanged, and only the types of the first cross-linking agent and the second cross-linking agent are changed. The specific parameter adjustments and the absorption capacity, absorption rate and liquid permeability of the prepared water-absorbent resin are shown in Table 6.

[0108] Table 6

[0109]

[0110] Example 7

[0111] A method for preparing a water-absorbent resin, specifically, adding 350 mL of cyclohexane and 3 g of sorbitan stearate (Span 60) surfactant to a glass jacketed reactor with a volume of 1000 mL, setting the stirring speed to 250 rpm, turning on the heating system, raising the temperature of the liquid in the reactor to 50°C, and dissolving the sorbitan stearate. On the other hand, adding 90 g of acrylic acid (1.25 mol) and 90 g of deionized water to a glass flask, mixing the two uniformly under magnetic stirring, then dropping 120 g of a 32% sodium hydroxide aqueous solution through a constant pressure dropping funnel, and controlling the system temperature to not exceed 30°C by water bath cooling to obtain a first monomer aqueous solution.

[0112] S1.1, under stirring, add trimethylolpropane triglycidyl ether (molecular weight 302.4, relative to 1×10 acrylic acid monomer) to the first monomer aqueous solution. -4 mol), 30 mg thickener hydroxyethyl cellulose, 300 mg potassium persulfate initiator, and after all solids are dissolved, a precursor mixture is obtained; 200 g of the precursor mixture is taken out and added to a glass reactor, and then the heating system is turned on to raise the jacket temperature of the glass jacket reactor to 90°C. After the temperature of the gas phase in the reactor is monitored to be stable, stirring is maintained for 1 hour to obtain a first-stage polymer.

[0113] S1.2, turn off the heating system, keep stirring, and cool the temperature in the reactor to room temperature. On the other hand, add tris(acrylamidemethyl)methane to the remaining precursor mixture. After the solid is completely dissolved, add the remaining precursor mixture to the glass reactor, then add 4g of 1,6-heptadiene (41.6 mmol), turn on the heating system to raise the jacket temperature of the glass jacket reactor to 90°C again. After monitoring the temperature of the gas phase in the reactor to stabilize, keep stirring for 1 hour to obtain the second stage polymer.

[0114] S2, open the reflux condensation system, remove water from the polymer by azeotropic distillation of cyclohexane and water, and when the oil-water interface in the oil-water separator no longer changes, add 10g of 5% by mass concentration of glycerol diglycidyl ether aqueous solution into the reactor, keep the jacket at 90°C for cross-linking for 1 hour to obtain the third stage polymer, and then continue to remove the remaining water in the system by azeotropic distillation of cyclohexane and water.

[0115] S3, turning off the heating system, allowing the material in the kettle to cool to room temperature, then filtering out the solid product, drying it, and obtaining the granular water-absorbent resin.

[0116] In this embodiment, other parameters remain unchanged, and only the relative amounts of the first cross-linking agent and the second cross-linking agent are changed. The specific parameter adjustments and the absorption capacity, absorption rate and liquid permeability of the prepared water-absorbent resin are shown in Table 7.

[0117] Table 7

[0118]

[0119] It should be noted that the above contents are further detailed descriptions of the present invention in combination with specific implementation methods, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions; the dimensional data of this embodiment does not necessarily limit the technical solution, but only shows one of the specific working conditions. For ordinary technicians in the technical field to which the present invention belongs, several simple improvements and modifications can be made without departing from the concept of the present invention, which should be regarded as falling within the scope of protection of the present invention.

Claims

1. A method for preparing a water-absorbent resin, characterized in that: The following steps are involved: S1: Adoption S1.1, adding a first monomer aqueous solution and a first cross-linking agent to obtain a precursor mixture, wherein the precursor mixture is divided into two parts, one part is subjected to a first polymerization reaction in an organic solvent containing a surfactant to obtain a first-stage polymer; and the other part is reserved; S1.2, adding the reserved precursor mixture, a second monomer and a second cross-linking agent to the first-stage polymer to perform a second polymerization reaction to obtain a second-stage polymer; Or adopt S1.1, dividing the first monomer aqueous solution into two parts, subjecting one part of the first monomer aqueous solution and the first cross-linking agent to a first polymerization reaction in an organic solvent containing a surfactant to obtain a first-stage polymer; S1.2, adding another part of the first monomer aqueous solution, the second monomer and the second cross-linking agent to the first-stage polymer to conduct a second polymerization reaction to obtain a second-stage polymer; S2: adding a third crosslinking agent to the second-stage polymer to obtain a third-stage polymer through a crosslinking reaction; S3: The third-stage polymer is filtered and dried to obtain the water-absorbent resin; Wherein, the step S1 further comprises adding an initiator and a thickener in step S1.1, or adding an initiator and a thickener in both step S1.1 and step S1.2 respectively; The first monomer is an acrylic acid monomer, and the acrylic acid monomer includes (meth) acrylic acid and its salt; the first monomer aqueous solution is an acrylic acid monomer aqueous solution treated with alkali neutralization; the second monomer is a polyolefin with 4-13 carbon atoms in the main chain; The molar amount of the second monomer is 1% to 20% of the molar amount of the first monomer added in step S1.2; the molar ratio of the first monomer used in step S1.1 to step S1.2 is 9:1 to 1:

1.

2. The method for preparing a water-absorbent resin according to claim 1, characterized in that: The second monomer is a 1,ω-divalent aliphatic olefin having 4 to 13 carbon atoms in the main chain.

3. The method for preparing a water-absorbent resin according to claim 1, characterized in that: The acrylic monomer further includes at least one of 2-hydroxyethyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, and N,N-diethylaminopropyl (meth)acrylate.

4. The method for preparing a water-absorbent resin according to claim 1, characterized in that: The concentration of the acrylic acid monomer aqueous solution is 10wt%-50wt%.

5. The method for preparing a water-absorbent resin according to claim 1, characterized in that: The temperature of the first polymerization reaction is the azeotropic temperature of water and the organic solvent; And / or, the temperature of the second polymerization reaction is the azeotropic temperature of water and the organic solvent; And / or, the temperature of the cross-linking reaction is the azeotropic temperature of water and the organic solvent.

6. The method for preparing a water-absorbent resin according to claim 1, characterized in that: The reaction temperature of the first polymerization reaction is 60°C to 100°C; And / or, the reaction temperature of the second polymerization reaction is 60° C. to 100° C.; And / or, the reaction temperature of the cross-linking reaction is 60°C to 100°C; And / or, the reaction time of the first polymerization reaction is 0.5h~2h; And / or, the reaction time of the second polymerization reaction is 0.5h~2h; And / or, the reaction time of the cross-linking reaction is 0.5h~2h.

7. The method for preparing a water-absorbent resin according to claim 1, characterized in that: The molar ratio of the second cross-linking agent to the first monomer added in step S1.2 is recorded as A, and the molar ratio of the first cross-linking agent to the first monomer added in step S1.1 is recorded as B. The value range of B is 1 / 10000~1 / 1000, and the ratio of A to B is (2:1~10:1).

8. The method for preparing a water-absorbent resin according to claim 1, characterized in that: The molar amount of the third cross-linking agent is 1 / 100000 to 1 / 1000 of the molar amount of the first monomer used in step S1.

9. The method for preparing a water-absorbent resin according to claim 1, characterized in that: The first cross-linking agent, the second cross-linking agent, and the third cross-linking agent are independently selected from at least one of ethylene glycol, propylene glycol, 1,4-butanediol, trimethylolpropane, glycerol, polyethylene glycol, polypropylene glycol, polyglycerol, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, polyglycerol diglycidyl ether, epichlorohydrin, epibromohydrin, α-methyl epichlorohydrin, N,N'-methylenebisacrylamide, trimethylolpropane tri(meth)acrylate, trimethylolmethanol tri(meth)acrylate, trimethylolethanol tri(meth)acrylate, trimethylolpropane triglycidyl ether, triaminomethylmethane tri(meth)acrylamide, triaminomethylethane tri(meth)acrylamide, and triaminomethylpropane tri(meth)acrylamide.

10. The method for preparing a water-absorbent resin according to claim 1, characterized in that: The organic solvent includes one or more of chain aliphatic hydrocarbons, alicyclic hydrocarbons, and aromatic hydrocarbons; And / or, the molar amount of the organic solvent is 1 to 3 times the molar amount of the first monomer used in step S1.

11. The method for preparing a water-absorbent resin according to claim 1, characterized in that: The surfactant comprises at least one of sucrose fatty acid ester, polyglycerol fatty acid ester, sorbitan fatty acid ester, polyoxyethylene sorbitan fatty acid ester, polyoxyethylene glycerol fatty acid ester, sorbitol fatty acid ester, polyoxyethylene sorbitol fatty acid ester, polyoxyethylene alkyl ether, polyoxyethylene alkylphenyl ether, polyoxyethylene castor oil, polyoxyethylene hydrogenated castor oil, alkyl allyl formaldehyde condensation polyoxyethylene ether, polyoxyethylene polyoxypropylene block copolymer, polyoxyethylene polyoxypropyl alkyl ether, polyethylene glycol fatty acid ester, alkyl glucoside, N-alkyl glucose amide, polyoxyethylene fatty acid amide, polyoxyethylene alkylamine, phosphate ester of polyoxyethylene alkyl ether, and phosphate ester of polyoxyethylene alkyl allyl ether; And / or, the molar amount of the surfactant is 1 / 1000 to 5 / 1000 of the molar amount of the organic solvent.

12. The method for preparing a water-absorbent resin according to claim 1, characterized in that: The initiator includes at least one of persulfate, peroxide, and azo water-soluble free radical initiator; And / or, in step S1, the molar ratio of the first monomer to the initiator is 1:(0.0002-0.001).

13. The method for preparing a water-absorbent resin according to claim 1, characterized in that: The thickener includes at least one of hydroxyethyl cellulose, hydroxypropyl cellulose, methyl cellulose, carboxymethyl cellulose, polyacrylic acid, partially neutralized polyacrylic acid, polyethylene glycol, polyacrylamide, polyethyleneimine, dextrin, sodium alginate, polyvinyl alcohol, polyvinyl pyrrolidone, and polyethylene oxide; And / or, the molar ratio of the acrylic monomer to the thickener is 1:(0.05-0.2).

14. A water-absorbent resin, characterized in that: The preparation method is described in any one of claims 1 to 13.

15. An absorbent body, characterized in that: Contains the water-absorbent resin according to claim 14.