Dispersion

By applying mechanical force to the 2D material/graphite nanosheets in water and combining water-soluble abrasive media and wetting agents, the problem of poor dispersion and stability is solved, and a dispersion with high stability and low viscosity is achieved, which extends the Shelf life and reduces health and environmental hazards.

CN114302860BActive Publication Date: 2024-11-15APPL GRAPHENE MATERIALS UK LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080059548.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-09
Filing Date
2020-07-08
Publication Date
2024-11-15
Estimated Expiration
2040-07-08

AI Technical Summary

Technical Problem

2D material/graphite nanosheets have poor dispersion and poor stability in water and aqueous solutions, are prone to aggregation and airborne transmission, and are health hazards, and existing modification methods may damage the performance of the material or use harmful solvents.

Method used

Using mechanical devices to apply shear and crushing forces to the 2D material/graphite nanosheets, mix water-soluble grinding media and wetting agents to form liquid dispersions to improve dispersion and stability, using a combination of grinding media and wetting agents Reduce the aggregation and flocculation of nanosheets.

Benefits of technology

Achieve high stability and low viscosity 2D material/graphite nano-microsheet dispersion in water, extends the storage period, reduces the harm to the environment, avoids the problem of high solubility coating, and improves the storage stability of the dispersion and usability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003515454730000101
    Figure BDA0003515454730000101
  • Figure BDA0003515454730000111
    Figure BDA0003515454730000111
  • Figure BDA0003515454730000112
    Figure BDA0003515454730000112
Patent Text Reader

Abstract

The present invention discloses a method for forming a liquid dispersion of 2D material / graphite nanoplatelets in an aqueous solution. The method comprises the following steps: (1) generating a dispersion medium; (2) mixing the 2D material / graphite nanoplatelets into the dispersion medium; and (3) subjecting the 2D material / graphite nanoplatelets to sufficient shear force and / or crushing force using a mechanical device to reduce the particle size of the 2D material / graphite nanoplatelets. The liquid dispersion comprises the 2D material / graphite nanoplatelets, at least one grinding medium, water and at least one wetting agent, and at least one grinding medium is water-soluble or functionalized to be water-soluble.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to dispersions, in particular to aqueous dispersions comprising two-dimensional (2D) materials and methods of preparing such dispersions. Background Art

[0002] The 2D materials referred to herein include one or more known 2D materials and / or graphite sheets having at least one nanoscale dimension or a mixture thereof. They are collectively referred to herein as "2D materials / graphite nanoplatelets" or "2D materials / graphite nanoplatelets".

[0003] 2D materials (sometimes called monolayer materials) are crystalline materials composed of a single layer of atoms or at most a few layers of atoms. Layered 2D materials consist of 2D layers that are weakly stacked or bonded to form a three-dimensional structure. Nanosheets of 2D materials have a thickness of nanometers or less, and their other two dimensions are usually larger than nanometers.

[0004] Known 2D nanomaterials include, but are not limited to, graphene (C), graphene oxide, reduced graphene oxide, hexagonal boron nitride (hBN), molybdenum disulfide (MoS2), tungsten diselenide (WSe2), silicene (Si), germanene (Ge), graphyne (C), borophene (B), phosphorene (P), or 2D vertical or in-plane heterostructures of the above two materials.

[0005] Graphite flakes having at least one nanoscale dimension contain 10 to 40 layers of carbon atoms and have lateral dimensions in the range of about 100 nm to 100 μm.

[0006] 2D materials / graphite nanoplatelets, especially graphene and hexagonal boron nitride, have many attractive properties in the materials field, and more properties are being discovered. A major challenge in utilizing such materials and their properties is that such materials are dispersed and can be prepared in a commercial process to be commercially attractive. In particular, such compositions must have sufficient shelf life / storage life to allow the material to be sold to be stored for a known period of time and then used. In addition, such compositions need not be harmful to the user and / or the environment, or at least any harm must be within acceptable limits.

[0007] A particular problem faced by 2D materials / graphite nano-microplatelets is that they disperse very poorly in water and aqueous solutions, and once dispersed, the stability of such dispersions is poor. For example, graphene nanoplatelets and / or graphite nanoplatelets with one nanometer size face this problem in water and aqueous solutions. Hexagonal boron nitride nanoplatelets face the same problem.

[0008] For 2D materials / graphite nanoplatelets that are known or suspected to be hazardous, the stability of these 2D materials / graphite nanoplatelets in dispersion is particularly important, especially when not encapsulated in other materials, as they can easily become airborne if they precipitate out of the dispersion and dry when not bound or encapsulated in a non-airborne substance. Airborne graphene nanoplatelets and / or graphite nanoplatelets with at least one nanometer size are considered to be potentially harmful to human and animal health if inhaled into the lungs. The hazards of other 2D materials / graphite nanoplatelets are still being evaluated, but it is prudent to assume that other 2D materials / graphite nanoplatelets will present similar hazards.

[0009] 2D materials / graphite nanoplatelets have high surface area and low functionality, with the result that they have historically proven to be very difficult to wet and / or disperse in water or aqueous solutions. Furthermore, 2D materials / graphite nanoplatelets are known to be very difficult to prevent from agglomerating once dispersed.

[0010] Since the discovery of 2D materials / graphite nanoplatelets and their properties, improved methods for wetting and achieving dispersion stability in non-aqueous solutions such as organic solvents and aqueous solutions have been the subject of intensive research.

[0011] The parameters for forming a good dispersion are well established in the field of colloid science, and the free energy of any colloidal system is determined by the interfacial area and interfacial tension. The theoretical surface area of ​​a single layer of graphene is about 2590 m 2 ·g -1 , so the range of conditions for their dispersion is limited, typically these conditions include ultrasonic treatment and the use of polar aprotic solvents.

[0012] In order to maintain the stability of graphene / graphite nanoplatelets (where graphite nanoplatelets are graphite nanoplatelets with nanoscale dimensions and 10 to 20 layers and lateral dimensions in the range of about 100 nm to 100 μm) once dispersed in a dispersion, an energy barrier needs to be created to prevent those nanoplatelets from aggregating. This can be achieved by electrostatic or steric repulsion. If the energy barrier is high enough, then the Brownian motion will maintain the dispersion. This is achieved by using one or more methods, which can be summarized as:

[0013] a.Solvent selection;

[0014] b. Chemical (covalent) modification of graphene / graphite nanoplatelets; and

[0015] c. Non-covalent modification of graphene / graphite nanosheets.

[0016] a. Solvent selection

[0017] Several solvents, notably N-methyl-2-pyrrolidone (NMP), dimethyl sulfoxide (DMSO), and dimethylformamide (DMF), have been identified as being particularly suitable for dispersing graphene / graphite nanoplatelets. These solvents present health and safety concerns and are preferably not used.

[0018] Solvent interactions have been rationalized based on the use of surface energy and Hansen solubility parameters. Several solvents have been identified as potential carrier media using Hansen solubility parameters, however, their effectiveness depends on the functionality of the graphene / graphite nanoplatelets, the dispersion mode, the dispersion time and / or the dispersion temperature.

[0019] However, water is not a solvent that interacts well with graphene / graphite nanosheets. Water is a solvent with high polarity, while graphene / graphite nanosheets are highly hydrophobic. This makes water and graphene / graphite nanosheets repel each other and causes the graphene / graphite nanosheets to aggregate and flocculate rather than disperse.

[0020] b. Chemical (covalent) modification of graphene / graphite nanosheets

[0021] Functionalization of graphene / graphite nanoplatelets depends greatly on the level of functional group availability. In the presence of oxygen (such as in reduced graphene oxide), one of the most popular routes is to use diazonium salts to introduce functionality.

[0022] Alternatively, in the absence of functionality (pure graphene or graphite) or in the case of very low functionality, plasma modification can be used to introduce functionality. These graphene / graphite nanoplatelets can then be further processed to produce new functional species. The most important process parameter for plasma treatment is the process gas, as this determines the chemical groups introduced, while the process time and power used affect the concentration of the introduced functional groups.

[0023] It has been observed that, although chemical functionalization of graphene / graphite nanoplatelets can improve their dispersibility, said chemical functionalization can also increase the defect levels within the graphene sp2 structure and have a negative impact on properties such as conductivity, which is clearly an undesirable outcome.

[0024] c. Non-covalent modification of graphene / graphite nanosheets

[0025] Non-covalent modification of graphene / graphite nanosheets has several advantages over covalent modification, as it does not involve additional chemical steps and avoids the disruption of sp2 domains within the nanosheets. There are a range of possible interactions, based on π-π, cation-π and the use of surfactants.

[0026] π-π bonds can be achieved through dispersion or electrostatic interactions. A large number of aromatic-based systems have been shown to interact with graphene, such as polycyclic aromatic hydrocarbons (PAHs), pyrene, and polyacrylonitrile (PAN).

[0027] The cation-π bond can use metal or organic cations. Organic cations are generally preferred, with imidazolium cations being preferred because those cations have a planar and aromatic structure.

[0028] Surfactants are widely used due to the wide variety of commercially available surfactants. Typically, surfactants will initially be adsorbed on the substrate edge of the nanosheet and then on the surface. Adsorption is enhanced if there is π-π interaction capability and a planar tail that can be solvated. Both nonionic and ionic surfactants have been shown to be effective, depending on the functionality of the graphene / graphite nanosheet substrate edge and surface and the medium in which the graphene / graphite nanosheet is dispersed.

[0029] To summarize the above discussion, highly specialized additives are required to wet, disperse and stabilize dry powders of graphene / graphite nanoplatelets for liquid formulations using organic solvents. The same is true for other 2D materials / graphite nanoplatelets.

[0030] The use of organic solvents in the environment is a growing concern and there is a general desire to reduce or eliminate organic solvents in the environment as much as possible. Summary of the invention

[0031] According to a first aspect of the present invention, there is provided a method for forming a liquid dispersion of 2D material / graphite nanoplatelets in water or an aqueous solution, comprising the following steps:

[0032] (1) generating a dispersion medium;

[0033] (2) mixing the 2D material / graphite nanoplatelets into a dispersion medium; and

[0034] (3) Using a mechanical device to subject the 2D material / graphite nanosheet to sufficient shear force and / or crushing force to reduce the particle size of the 2D material / graphite nanosheet

[0035] Characterized in that the 2D material / graphite nanoplatelets and dispersion medium mixture comprises 2D material / graphite nanoplatelets, at least one grinding medium, water and at least one wetting agent, and at least one grinding medium is water-soluble or functionalized to be water-soluble.

[0036] Step (2) of the first aspect of the present invention is performed before step (3) to achieve initial wetting of the 2D material / graphite flakes.

[0037] According to a second aspect of the present invention, a dispersion is provided, comprising 2D material / graphite nanoplatelets, at least one grinding medium, water and at least one wetting agent, wherein at least one grinding medium is water-soluble or functionalized to be water-soluble.

[0038] According to a third aspect of the present invention, there is provided a liquid coating system comprising a dispersion according to the second aspect of the present invention.

[0039] In some embodiments of the first aspect of the invention, the 2D material / graphite nanosheets comprise one or more graphene or graphite nanosheets, wherein the graphene nanosheets comprise one or more of graphene nanosheets, reduced graphene oxide nanosheets, double-layer graphene nanosheets, double-layer reduced graphene oxide nanosheets, triple-layer graphene nanosheets, triple-layer reduced graphene oxide nanosheets, few-layer graphene nanosheets, few-layer reduced graphene oxide nanosheets, and graphene nanosheets with 6 to 10 layers of carbon atoms, and the graphite nanosheets comprise graphite nanosheets with at least 10 layers of carbon atoms.

[0040] In some embodiments of the present invention, one or both of the graphene nanoplatelets and the graphite nanoplatelets have lateral dimensions in the range of about 100 nm to 100 μm.

[0041] In some embodiments of the first aspect of the present invention, the 2D material / graphite nano-micron sheet comprises one or more graphite nano-microsheets, wherein the graphite nano-microsheets are graphite nano-sheets having 10 to 20 layers of carbon atoms, graphite nano-sheets having 10 to 14 layers of carbon atoms, graphite nano-sheets having 10 to 35 layers of carbon atoms, graphite nano-sheets having 10 to 40 layers of carbon atoms, graphite nano-sheets having 25 to 30 layers of carbon atoms, graphite nano-sheets having 25 to 35 layers of carbon atoms, graphite nano-sheets having 20 to 35 layers of carbon atoms, or graphite nano-sheets having 20 to 40 layers of carbon atoms.

[0042] In some embodiments of the first aspect of the present invention, the 2D material / graphite nanosheets comprise one or more 2D material nanosheets, wherein the 2D material nanosheets comprise hexagonal boron nitride (hBN), molybdenum disulfide (MoS2), tungsten diselenide (WSe2), silicene (Si), germanene (Ge), graphyne (C), borophene (B), phosphorene (P) or one or more 2D in-plane or vertical heterostructures of two or more of the above materials.

[0043] The few-layer graphene / reduced graphene oxide nanosheets have 4 to 10 layers of carbon atoms, with a monolayer having a thickness of 0.035 nm and a typical interlayer distance of 0.14 nm.

[0044] In some embodiments of the first aspect of the present invention, the 2D material / graphite nanoplatelets comprises graphene / graphite nanoplatelets and at least one 1D material. In some embodiments, the 1D material comprises carbon nanotubes.

[0045] In some embodiments of the first aspect of the invention, the grinding media is a polymer modified with strong anchoring groups, a grinding resin, an aqueous solution of a modified aldehyde resin having at least one amine group, a low molecular weight styrene / maleic anhydride copolymer, or a mixture of these media.

[0046] In some preferred embodiments, the grinding media of the dispersion of 2D material / graphite nanoplatelets is Laropal (trademark) LR 9008, which is a water-soluble modified aldehyde resin commercially available from BASF Dispersions and Resins Division in North America; ADDITOL (trademark) XL 6515, a modified alkyd polymer; ADDITOL XW 6528, a polyester-modified acrylic polymer; ADDITOL XW 6535, a high polymer, automatic emulsifying pigment grinding media; ADDITOL XW 6565, a high polymer, automatic emulsifying pigment grinding media; ADDITOL XW 6591, a polyester-modified acrylic polymer; ADDITOL products are commercially available from the Allnex Group of Companies.

[0047] In some embodiments of the first aspect of the present invention, the dispersion medium comprises a mixture of at least one grinding medium and water, and the step of generating the dispersion medium comprises:

[0048] (i) mixing at least one grinding medium with water until it is substantially homogeneous.

[0049] In some embodiments of the first aspect of the invention, at least one grinding medium is a liquid and the dispersion medium comprises 50 wt % to 90 wt % of at least one grinding medium and 10 wt % to 50 wt % water, 60 wt % to 80 wt % of at least one grinding medium and 20 wt % to 40 wt % water; 65 wt % to 75 wt % of at least one grinding medium and 25 wt % to 35 wt % water, or about 70 wt % of at least one grinding medium and about 30 wt % water.

[0050] In some embodiments of the first aspect of the invention, the method further comprises the following steps:

[0051] (ii) after step (i), adding the 2D material / graphite nanoplatelets to a mixture of at least one grinding medium and water, and

[0052] (iii) mechanically mixing the 2D material / graphite nanoplatelets and the mixture of at least one grinding medium and water until the 2D material / graphite nanoplatelets are substantially dispersed in the grinding medium solution.

[0053] In some embodiments of the first aspect of the present invention, the dispersion medium further comprises at least one wetting agent, the wetting agent is stored in liquid form, and the step of generating the dispersion medium comprises:

[0054] (i) mixing at least one grinding medium, water, and a wetting agent until the mixture of the grinding medium, water, and wetting agent is substantially homogeneous.

[0055] In some embodiments of the first aspect of the present invention, the dispersion medium further comprises at least one wetting agent, the wetting agent is stored in solid (including powder) form, and the step of producing the dispersion medium comprises:

[0056] (I) mixing at least one grinding medium, water, and a wetting agent until the wetting agent is dissolved and the mixture of the grinding medium, water, and wetting agent is substantially homogeneous.

[0057] In some embodiments of the first aspect of the present invention, at least one wetting agent is added to the dispersion medium substantially simultaneously with the 2D material / graphite nanoplatelets.

[0058] The one or more wetting agents of the present invention can be one of a polymeric wetting agent, an ionic wetting agent, a polymeric nonionic dispersing and wetting agent, a cationic wetting agent, an amphoteric wetting agent, a Gemini wetting agent, a polymeric resinous wetting agent and dispersing agent, or a mixture of two or more of these wetting agents. The Gemini wetting agent has two polar centers or head groups in the polyether segment, which are connected by a spacer segment.

[0059] Preferred wetting agents for 2D material / graphite nanoplatelet dispersions include, but are not limited to, ADDITOL (trademark) VXW6208 / 60 (a modified acrylic copolymer), which is a polymeric nonionic dispersing and wetting additive commercially available from Allnex Belgium SA / NV; DISPERBYK-2150 (trademark), a block copolymer with basic pigment-affinity groups commercially available from BYK-Chemie GmbH; Surfynol (trademark) 104, a Gemini wetting agent and molecular defoamer commercially available from Evonik Nutrition & Care GmbH.

[0060] Dried 2D materials / graphite nanoplatelets, such as graphene / graphite nanoplatelets, are usually composed of agglomerates or aggregates of primary particles or nanoplatelets. During the dispersion process, these agglomerates or aggregates must be decomposed as far as possible into primary particles or nanoplatelets, the size of which is suitable for the intended application of the 2D material / graphite nanoplatelets. The decomposition of agglomerates or aggregates of primary particles or nanoplatelets is considered to include an exfoliation process.

[0061] In some embodiments of the invention, the dispersing device is a device suitable for applying a crushing action and mechanical shearing force to the 2D material / graphite microplatelets while those materials are mixed with a dispersion medium. Suitable equipment for achieving this is a known grinding or milling device, such as a dissolver, a bead mill, or a three-roll mill.

[0062] In some embodiments of the present invention, it is preferred that the agglomerates or aggregates are broken down into particles or nanoplatelets of a size that cannot be further broken down. This is beneficial because the manufacture and storage of 2D materials / graphite nanoplatelets prior to use are often in the form of particles larger than those required for the 2D material / graphite nanoplatelet dispersion.

[0063] Once the 2D material / graphite nanoplatelet agglomerates or aggregates are reduced to smaller particles or nanoplatelets, the rapid stabilization of the newly formed surface due to the reduction in the size of the agglomerates or aggregates helps prevent the particles or nanoplatelets from reagglomerating or reaggregating.

[0064] The method of the present invention is particularly beneficial because it has been found that the higher the interfacial tension between the dispersion medium (e.g., a dispersion medium comprising water and 2D material / graphite nanoplatelets), the stronger the force tending to reduce the interfacial area. That is, the stronger the force tending to re-agglomerate or re-aggregate the 2D material / graphite nanoplatelets or form flocs. The interfacial tension between the wetting agent in the dispersion medium and the 2D material / graphite nanoplatelets is lower than the interfacial tension between water and the 2D nanomaterial, so the wetting agent helps stabilize the newly formed surface and prevent the 2D material / graphite nanoplatelets from agglomerating, aggregating and / or flocculating.

[0065] The role of wetting agents in stabilizing newly formed surfaces and preventing agglomeration, aggregation and / or flocculation of 2D materials / graphite nanoplatelets is beneficial, but has been found to be insufficient to allow the formation of improved stable dispersions. This is because while wetting agents will allow 2D nanomaterials to be suspended in an aqueous dispersion medium, one characteristic of 2D materials / graphite nanoplatelets is that they have a high surface area relative to other compounds. Water, with its high polarity, can replace the wetting agent.

[0066] An increase in the proportion of wetting agent in the dispersion medium may ultimately result in all components of the dispersion remaining suspended. However, a problem with this method of forming a dispersion is that a coating formed from the dispersion will be highly soluble in water. This is highly undesirable because it can lead to rapid failure of the coating.

[0067] According to the present invention, applying a disruptive action and mechanical shear force to a dispersion comprising a mixture of 2D material / graphite nanoplatelets in a grinding media, water and a wetting agent mixture produces an improved dispersion.

[0068] This is believed to be because, in addition to the wetting agent, the grinding media will also stabilize the surface of the newly formed 2D material / graphite nanoplatelets because a portion of the 2D material / graphite nanoplatelets is at least partially encapsulated within the coating of the grinding media. The wetting agent can then bind to the combined grinding media / 2D material / graphite nanoplatelet particles and allow the grinding media / 2D material / graphite nanoplatelet particles to be suspended in the dispersion. The grinding media requires less wetting agent than the 2D material / graphite nanoplatelets to allow suspension in the dispersion, thus avoiding the problem of requiring too much wetting agent and the resulting high solubility of any coating formed from the dispersion.

[0069] It is believed that this is because water as a solvent has a high polarity, while in contrast, graphene / graphite nanoplatelets with a high carbon / oxygen ratio have a low polarity and are highly hydrophobic, which causes the two to repel each other. This causes the graphene / graphite nanoplatelets to aggregate and flocculate rather than disperse. In some embodiments of the present invention, where the 2D material / graphite nanoplatelets are graphene / graphite nanoplatelets, the carbon / oxygen ratio of the graphene / graphite nanoplatelets is equal to or greater than 15.

[0070] Another advantage of the method of the present invention is that the grinding performance of the dispersing device when acting on the 2D material / graphite nanoplatelets is further improved by the presence of grinding media in the mixture being ground. This improvement is manifested by faster grinding, lower heat generation during grinding, more uniform particle size in the dispersion, smaller D50 particle size in the dispersion, lower dispersion viscosity, higher storage stability relative to known short-shelf-life dispersions, and the ability to redisperse any combination of grinding media / 2D material / graphite nanoplatelet particles that have precipitated out of the dispersion by simply stirring the dispersion.

[0071] The use of grinding media allows for the use of less wetting agent than might be desired in producing the dispersion, thereby minimizing solubility problems of coatings formed from coating systems comprising dispersions prepared according to the present invention.

[0072] According to a second aspect of the present invention, there is provided a liquid dispersion comprising 2D material / graphite nanoplatelets, at least one grinding medium, water and at least one wetting agent.

[0073] In some embodiments of the second aspect of the present invention, the 2D material / graphite nanoplatelets comprise one or more of graphene nanoplatelets, graphite nanoplatelets and 2D material nanoplatelets, and wherein the graphene nanoplatelets comprise one or more of graphene nanoplatelets, reduced graphene oxide nanoplatelets, double-layer graphene nanoplatelets, double-layer reduced graphene oxide nanoplatelets, three-layer graphene nanoplatelets, three-layer reduced graphene oxide nanoplatelets, few-layer graphene nanoplatelets, few-layer reduced graphene oxide nanoplatelets and graphene nanoplatelets with 6 to 10 layers of carbon atoms, and the graphite nanoplatelets comprise graphite nanoplatelets having at least 10 layers of carbon atoms, and the graphite nanoplatelets comprise graphite nanoplatelets having 10 to 20 layers of carbon atoms. sheets, graphite nanosheets with 10 to 14 layers of carbon atoms, graphite nanosheets with 10 to 35 layers of carbon atoms, graphite nanosheets with 10 to 40 layers of carbon atoms, graphite nanosheets with 25 to 30 layers of carbon atoms, graphite nanosheets with 25 to 35 layers of carbon atoms, graphite nanosheets with 20 to 35 layers of carbon atoms or graphite nanosheets with 20 to 40 layers of carbon atoms, and the 2D material nanosheets contain hexagonal boron nitride (hBN), molybdenum disulfide (MoS2), tungsten diselenide (WSe2), silicene (Si), germanene (Ge), graphyne (C), borane (B), phosphorene (P) or one or more of the 2D in-plane or vertical heterostructures of two or more of the above materials.

[0074] In some embodiments of the second aspect of the present invention, the 2D material / graphite nanoplatelets comprises at least one 1D material.

[0075] In some embodiments of the second aspect of the invention, at least one grinding medium is a polymer modified with a strong anchoring group, an aqueous solution of a modified aldehyde resin having at least one amine group, or a low molecular weight styrene / maleic anhydride copolymer.

[0076] In some preferred embodiments, the grinding media of the dispersion of 2D material / graphite nanoplatelets is Laropal (trademark) LR 9008, which is a water-soluble modified aldehyde resin commercially available from BASF Dispersions and Resins Division in North America; ADDITOL (trademark) XL 6515, a modified alkyd polymer; ADDITOL XW 6528, a polyester-modified acrylic polymer; ADDITOL XW 6535, a high polymer, automatic emulsifying pigment grinding media; ADDITOL XW 6565, a high polymer, automatic emulsifying pigment grinding media; ADDITOL XW 6591, a polyester-modified acrylic polymer; ADDITOL products are commercially available from the Allnex Group of Companies.

[0077] In some embodiments of the second aspect of the invention, the wetting agent comprises one of a polymeric wetting agent, an ionic wetting agent, a polymeric nonionic dispersing and wetting agent, a cationic wetting agent, an amphoteric wetting agent, a Gemini wetting agent, a polymeric resinous wetting agent and dispersing agent or a mixture of two or more of these wetting agents.

[0078] Preferred wetting agents include, but are not limited to, ADDITOL (trademark) VXW 6208 / 60 (a modified acrylic copolymer), a polymeric nonionic dispersing and wetting additive commercially available from Allnex Belgium SA / NV; DISPERBYK-2150 (trademark), a block copolymer with basic pigment-affinic groups commercially available from BYK-Chemie GmbH; Surfynol (trademark) 104, a Gemini wetting agent and molecular defoamer commercially available from Evonik Nutrition & Care GmbH.

[0079] In some embodiments of the second aspect of the invention, the liquid dispersion is produced using the method according to the first aspect of the invention.

[0080] Brief Description

[0081] To better understand the various embodiments that are useful in understanding the specific embodiments, reference will now be made to the following examples. DETAILED DESCRIPTION

[0082] Example

[0083] Typical formulations of dispersions according to the invention are listed in Tables 1 and 2 below:

[0084] All dispersions were made on an Eiger Torrance 250 horizontal bead mill. The dispersions were milled at maximum speed in recirculation mode for 15 minutes.

[0085] Characterization of dispersions

[0086] Particle size was measured on a Mastersizer 3000 to determine the effectiveness of the grinding resin and dispersant in deagglomerating and reducing particle size.

[0087] Measuring viscosity helps understand the rheological properties of a dispersion. This is done using a Kinexus rheometer.

[0088] Storage stability is determined by using a Turbiscan Stability Analyzer. The Turbiscan Stability Index (TSI) is a relative stability metric that allows comparison of multiple samples. As a relative metric, it allows quantitative assessment of closely related formulations.

[0089] Stability tests were performed at room temperature and elevated temperature (40°C).

[0090] Table 1

[0091] Element weight% A-GNP35 0.5 Surfynol 104 0.1 water 29.82 Laropal LR9008 69.58

[0092] Table 2

[0093] Element weight% A-GNP10 10 Surfynol 104 2 water 26.4 Laropal LR9008 61.6

[0094] The graphite material A-GNP10 is commercially available from Applied Graphene Materials UK Ltd., UK, and comprises graphite nanoplatelets 25 to 35 atoms thick. The graphite nanoplatelets are provided in powder form and are generally aggregated into agglomerates of nanoplatelets.

[0095] Graphene / graphite material A-GNP35 is commercially available from Applied Graphene Materials UK Ltd., UK, and comprises 5 to 15 atomically thick graphene / graphite nanoplatelets. The graphite nanoplatelets are provided in powder form and are typically aggregated into agglomerates of nanoplatelets.

[0096] Each dispersion was prepared using the following steps:

[0097] 1. Add Surfynol 104 and Laropal LR9008 to water. Stir until the mixture is basically homogeneous;

[0098] 2. Add A-GNP-10 or A-GNP-35 to the mixture and stir until the powder is evenly dispersed in the mixture;

[0099] 3 Recirculate the mixture in a bead mill using the beads for 15 minutes.

[0100] discuss

[0101] Graphene (A-GNP10) dispersed only in water

[0102] A-GNP10 was dispersed in water at 4 different concentrations: 0.1%, 1%, 5% and 10%. The samples were stored at ambient conditions for 4 weeks.

[0103] The 5% and 10% samples settled within 2 to 3 days after manufacture.

[0104] The 0.1% and 1% samples had no significant sedimentation 4 weeks after manufacture.

[0105] The severe degree of sedimentation seen in the addition of 5% and 10% by weight of graphene (A-GNP10) reinforces the need to identify suitable pigment dispersing resins (i.e., grinding media) and / or surfactants (i.e., wetting agents) to improve the shelf life and storage stability of the product.

[0106] Graphene (A-GNP10) dispersed in water containing a dispersing resin (i.e., grinding media)

[0107] Decentralized testing

[0108] 10% A-GNP 10 was dispersed in a series of media with increasing loading of grinding media Laropal LR9008:

[0109] 1. Water only

[0110] 2. A mixture of 10% Laropal and 90% water

[0111] 3. A mixture of 20% Laropal and 80% water

[0112] 4. A mixture of 30% Laropal and 70% water

[0113] 5. A mixture of 40% Laropal and 60% water

[0114] 6. A mixture of 50% Laropal and 50% water

[0115] Viscosity of A-GNP 10 aqueous dispersion

[0116] As shown in Table 3 below, all dispersions have very low viscosities (less than 1 PaS). Overall, the rheological properties of these dispersions do not vary significantly. However, the dispersion of 10% Laropal LR9008 and 90% water shows a particularly high viscosity.

[0117] Table 3: Viscosity of A-GNP 10 aqueous dispersion

[0118]

[0119] Particle size distribution of A-GNP 10 aqueous dispersion

[0120] The particle size distribution of all samples was monitored and the results are shown below in Table 4. Except for the dispersion with 10% Laropal loading, all dispersions showed a D90 in the range of 15-25 μm.

[0121] Table 4: Particle size distribution of A-GNP 10 aqueous dispersion

[0122]

[0123] Storage stability of A-GNP 10 aqueous dispersion

[0124] The samples were tested at room temperature and at elevated temperature (40°C). In general, the addition of Laropal LR 9008 usually improves the sedimentation stability.

[0125] Turbiscan measurement – ​​multiple light scattering

[0126] Static multiple light scattering was performed on the sample and the results are shown in Table 5 below. Static multiple light scattering is an optical method used to characterize concentrated liquid dispersions. Depending on the concentration and the primary particle size, light is transmitted into the sample and either backscattered or transmitted by dispersion. TSI numbers are used to indicate the degree of variation within the sample, with high numbers indicating a high degree of variation within the sample, i.e., instability.

[0127] Table 5: Turbiscan evaluation

[0128]

[0129] Comment

[0130] For A-GNP10 dispersions in water, as tested by Turbiscan, the presence of Laropal was shown to improve stability, with the only exception being the dispersion containing 10% Laropal LR9008. In the absence of Laropal LR9008, settling of the dispersion began to be seen after 2 to 3 days of storage. With the use of a dispersion resin, the settling stability increased to 6 weeks.

[0131] Graphene (A-GNP35) dispersed in water containing a dispersing resin (i.e., grinding media)

[0132] Decentralized testing

[0133] 0.5% A-GNP 35 was dispersed in water / solvent and subjected to recirculating bead milling for 15 min.

[0134] 0.5% A-GNP35 in the following

[0135] Water only

[0136] ·10% Laropal 90% water

[0137] ·20% Laropal 80% water

[0138] ·30% Laropal 70% water

[0139] ·40%Laropal 60%Water

[0140] ·50%Laropal 50%Water

[0141] Viscosity of A-GNP 35 aqueous dispersion

[0142] As shown in Table 6 below, A-GNP 35 dispersions in water tend to show only very high viscosities. For all systems tested, the viscosity decreases after the addition of Laropal LR9008. The lowest viscosity is reached at a loading of 20% Laropal.

[0143] Table 6: Viscosity of A-GNP 35 aqueous dispersion

[0144]

[0145] Particle size distribution of A-GNP 35 aqueous dispersion

[0146] The particle size distribution of all samples was evaluated and the results are shown in Table 7 below. The use of Laropal LR9008 was shown to significantly reduce the particle size. For the systems containing Laropal, the dispersion with a 10% Laropal loading showed the smallest reduction in particle size distribution. Between 20% and 50% Laropal loading, the particle size distribution did not change much. For these systems, the D90 was half of that when no dispersing resin (i.e., grinding media) was used.

[0147] Table 7: Particle size distribution of aqueous dispersion of A-GNP 10

[0148]

[0149] Storage stability

[0150] Samples were tested at room temperature and at elevated temperatures. A-GNP 35 dispersions in water generally have high viscosity and the consistency of a thick paste. Therefore, they tend to be more stable than equivalent dispersions of A-GNP 10. After a week of testing, there was no discernible difference in the stability of the samples whether stored at room temperature or at elevated temperature (40°C).

[0151] As shown in Table 8 below, Turbiscan evaluation of the samples showed no significant differences in the stability index of the samples at either room temperature or elevated temperature. The Turbiscan Stability Index (TSI) is a relative stability metric that allows for comparison of multiple samples. As a relative metric, it allows for quantitative evaluation of closely related formulations.

[0152] Table 8: Turbiscan evaluation

[0153]

[0154] Comment

[0155] For the A-GNP35 dispersion in water, the presence of Laropal significantly reduced the viscosity of the dispersion, making the dispersion more convenient to use and easier to handle. The inclusion of Laropal also achieved a greater degree of particle size reduction.

[0156] Graphene (A-GNP3) dispersed in water, including dispersion resin (i.e. grinding media) and wetting agent (Surfynol)

[0157] The stability of the dispersions in Table 1 was monitored over a 4 month period. Changes in particle size and degree of sedimentation were monitored. Four batches of stable formulations were tested. Surfynol (wetting agent) was introduced to further improve pigment wettability and act as a defoamer. The stable formulations are shown in Table 1 above.

[0158] Turbiscan – Multiple Light Scattering

[0159] Static multiple light scattering is an optical method used to characterize concentrated liquid dispersions. Depending on the concentration and primary particle size, light is transmitted into the sample and either backscattered or transmitted via dispersion. Any instabilities occurring in a given sample will have an effect on the backscattered and / or transmitted signal intensities during aging. Formulations with high intensity variations are changing significantly and can be considered unstable.

[0160] Four batches of the dispersion of Table 1 were tested to understand the stability of the dispersion. After 46 days of storage, surface separation formed, as evidenced by the appearance of a transmissive (clear) layer near the surface. Immediately below the forming clear layer was a slightly thicker layer with increased backscattering.

[0161] Monitoring particle size changes

[0162] The dispersions of Table 1 were evaluated for particle size distribution and the results are shown in Table 9 below.

[0163] Changes in particle size can indicate agglomeration, aggregation, or flocculation.

[0164] Table 9

[0165]

[0166] After 4 months, the initial D90 decreased slightly. The initial increase from 16.2 to 17.7 is considered to be within the measurement error.

[0167] Degree of sedimentation

[0168] The degree of sedimentation is shown in Table 10 below.

[0169] Table 10

[0170] Degree of sedimentation Ease of mixing initial No settling easy 1 month No settling easy 4 months No settling easy

[0171] Shelf life recommendations

[0172] The dispersion of Table 1 should be stored at room temperature (15 to 25° C.) for a period of 3 months. Some separation may occur, but this can be mixed back to a homogeneous dispersion with mild mechanical agitation.

Claims

1. A method for forming a liquid dispersion of 2D material / graphite nanoplatelets in an aqueous solution, The following steps are involved: (1) producing a dispersion medium by mixing at least one grinding medium, water, and at least one wetting agent until the mixture of the grinding medium, water, and wetting agent is substantially homogeneous, wherein the at least one grinding medium is water soluble or functionalized to be water soluble and comprises an aqueous solution of a modified aldehyde resin having at least one amine group; (2) Mixing 2D materials / graphite nanosheets into a dispersion medium; and (3) using a mechanical device to subject the 2D material / graphite nanosheets to sufficient shear force and / or crushing force to reduce the particle size of the 2D material / graphite nanosheets, Characterized in that the liquid dispersion comprises the 2D material / graphite nanoplatelets, the at least one grinding medium, the water and the at least one wetting agent, wherein the 2D material / graphite nanosheets comprise one or more of graphene nanosheets, graphite nanosheets and 2D material nanosheets, and wherein The graphene nanosheets include graphene nanosheets, and the graphite nanosheets include graphite nanosheets having at least 10 layers of carbon atoms, and the 2D material nanosheets include hexagonal boron nitride, molybdenum disulfide, tungsten diselenide, silicene, germanene, graphyne, borophene, phosphorene or one or more of the 2D in-plane or vertical heterostructures of two or more of the above materials.

2. The method according to claim 1, wherein the graphene nanosheets are composed of one or more of double-layer graphene nanosheets and triple-layer graphene nanosheets.

3. The method according to claim 1, wherein the graphene nanoplatelets consist of reduced graphene oxide nanoplatelets.

4. The method according to claim 3, wherein the graphene nanosheets are composed of one or more of double-layer reduced graphene oxide nanosheets and triple-layer reduced graphene oxide nanosheets. The method according to claim 1 , wherein the graphite nanoplatelets consist of graphite nanoplatelets having 10 to 20 layers of carbon atoms. The method according to claim 1 , wherein the graphite nanoplatelets consist of graphite nanoplatelets having 10 to 14 layers of carbon atoms. 7 . The method according to claim 1 , wherein the graphite nanoplatelets consist of graphite nanoplatelets having 10 to 35 layers of carbon atoms.

8. The method according to claim 1, wherein the graphite nanoplatelets consist of graphite nanoplatelets having 10 to 40 layers of carbon atoms.

9. The method according to claim 1, wherein the graphite nanoplatelets consist of graphite nanoplatelets having 25 to 30 layers of carbon atoms.

10. The method according to claim 1, wherein the graphite nanoplatelets consist of graphite nanoplatelets having 25 to 35 layers of carbon atoms.

11. The method according to claim 1, wherein the graphite nanoplatelets consist of graphite nanoplatelets having 20 to 35 layers of carbon atoms. 12 . The method according to claim 1 , wherein the graphite nanoplatelets consist of graphite nanoplatelets having 20 to 40 layers of carbon atoms.

13. The method of claim 1, wherein the 2D material / graphite nanoplatelets comprises at least one 1D material.

14. The method of any one of claims 1 to 13, wherein the at least one wetting agent comprises a polymeric wetting agent.

15. The method of any one of claims 1 to 13, wherein the at least one wetting agent comprises one of an ionic wetting agent or an amphoteric wetting agent.

16. The method of claim 15, wherein the ionic wetting agent is a cationic wetting agent.

17. The method of any one of claims 1 to 13, wherein the at least one wetting agent comprises a polymeric nonionic dispersing and wetting agent.

18. The method of any one of claims 1 to 13, wherein the at least one wetting agent comprises a Gemini wetting agent.

19. The method of any one of claims 1 to 13, wherein the at least one wetting agent comprises a polymeric resinous wetting and dispersing agent.

20. The method according to any one of claims 1 to 13, wherein the at least one wetting agent is stored in liquid form.

21. The method according to any one of claims 1 to 13, wherein the at least one wetting agent is stored in solid form and the step of producing the dispersion medium include: (i) mixing the at least one grinding medium, water, and a wetting agent until the wetting agent is dissolved and the mixture of the grinding medium, water, and wetting agent is substantially homogeneous.

22. The method of any one of claims 1 to 13, wherein the at least one wetting agent is added to the dispersion medium substantially simultaneously with the 2D material / graphite nanoplatelets.

23. The method according to any one of claims 1 to 13, wherein the step (3) of subjecting the 2D material / graphite nanoplatelets to sufficient shear force and / or crushing force to reduce the particle size of the 2D material / graphite nanoplatelets is carried out using one or more of a dissolver, a bead mill or a triple roll mill.

24. Liquid dispersions, It is characterized in that The liquid dispersion comprises 2D material / graphite nanoplatelets, at least one grinding medium, water, and at least one wetting agent, and wherein the at least one grinding medium is water-soluble or functionalized to be water-soluble and comprises an aqueous solution of a modified aldehyde resin having at least one amine group, wherein the 2D material / graphite nanosheets comprise one or more of graphene nanosheets, graphite nanosheets and 2D material nanosheets, and wherein The graphene nanosheets include graphene nanosheets, and the graphite nanosheets include graphite nanosheets having at least 10 layers of carbon atoms, and the 2D material nanosheets include hexagonal boron nitride, molybdenum disulfide, tungsten diselenide, silicene, germanene, graphyne, borophene, phosphorene or one or more of the 2D in-plane or vertical heterostructures of two or more of the above materials. 25 . The liquid dispersion according to claim 24 , wherein the graphene nanoplatelets consist of one or more of double-layer graphene nanoplatelets and triple-layer graphene nanoplatelets.

26. The liquid dispersion of claim 24, wherein the graphene nanoplatelets consist of reduced graphene oxide nanoplatelets.

27. The liquid dispersion according to claim 26, wherein the graphene nanoplatelets consist of one or more of double-layer reduced graphene oxide nanoplatelets and triple-layer reduced graphene oxide nanoplatelets.

28. The liquid dispersion according to claim 24, wherein the graphite nanoplatelets consist of graphite nanoplatelets having 10 to 20 layers of carbon atoms.

29. The liquid dispersion according to claim 24, wherein the graphite nanoplatelets consist of graphite nanoplatelets having 10 to 14 layers of carbon atoms.

30. The liquid dispersion of claim 24, wherein the graphite nanoplatelets consist of graphite nanoplatelets having 10 to 35 layers of carbon atoms.

31. The liquid dispersion according to claim 24, wherein the graphite nanoplatelets consist of graphite nanoplatelets having 10 to 40 layers of carbon atoms.

32. The liquid dispersion according to claim 24, wherein the graphite nanoplatelets consist of graphite nanoplatelets having 25 to 30 layers of carbon atoms.

33. The liquid dispersion according to claim 24, wherein the graphite nanoplatelets consist of graphite nanoplatelets having 25 to 35 layers of carbon atoms.

34. The liquid dispersion of claim 24, wherein the graphite nanoplatelets consist of graphite nanoplatelets having 20 to 35 layers of carbon atoms.

35. The liquid dispersion according to claim 24, wherein the graphite nanoplatelets consist of graphite nanoplatelets having 20 to 40 layers of carbon atoms.

36. The liquid dispersion of claim 24, wherein the 2D material / graphite nanoplatelets comprises at least one 1D material.

37. The liquid dispersion of any one of claims 24 to 36, wherein the wetting agent comprises a polymeric wetting agent.

38. The liquid dispersion of any one of claims 24 to 36, wherein the wetting agent comprises one of an ionic wetting agent or an amphoteric wetting agent.

39. The liquid dispersion of claim 38, wherein the ionic wetting agent is a cationic wetting agent.

40. The liquid dispersion of any one of claims 24 to 36, wherein the wetting agent comprises a polymeric nonionic dispersing and wetting agent.

41. The liquid dispersion of any one of claims 24 to 36, wherein the wetting agent comprises a Gemini wetting agent.

42. The liquid dispersion of any one of claims 24 to 36, wherein the at least one wetting agent comprises a polymeric resinous wetting and dispersing agent.

43. A liquid coating composition comprising the liquid dispersion according to any one of claims 24 to 36.