Regenerated cellulose fiber cheese yarn and reactive dyeing method thereof
By using non-aqueous media and linear feeding technology in dyeing regenerated cellulose fiber yarns, the problems of low dye utilization and uneven dyeing are solved, and efficient dye curing and wastewater treatment are achieved, reducing costs and environmental impacts.
Patent Information
- Application Number
- CN202210264497.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-17
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-03-17
AI Technical Summary
The existing dyeing methods for regenerated cellulose fiber yarn reactive dyes have problems such as low dye utilization, uneven dyeing, waste of water resources and difficult wastewater treatment. Especially in dyeing non-aqueous media, the phenomenon of dyeing is prone to occur. .
The dyeing is performed using non-aqueous medium. Through the steps of pressing water, adding dye liquid, adding alkali liquid and heating, combined with linear feeding method, the dye bath temperature and pH value are controlled to ensure uniform adsorption and curing of dyes, and to reduce the use of water and salt.
The dye fixation rate and dyeing rate of dyeing are improved, the dyeing wastewater generation is reduced, the wastewater treatment is simplified, the dyeing wastewater reuse rate is improved, and the dyeing cost is reduced.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of dyeing and finishing, in particular to a regenerated cellulose fiber cheese yarn and a reactive dyeing method thereof. Background Art
[0002] Regenerated cellulose fiber is made from natural cellulose (cotton, linen, bamboo, trees, shrubs, etc.) without changing its chemical structure, but only changing the physical structure of natural cellulose, thereby producing fibers with better performance. Common regenerated cellulose fibers include viscose, tencel, modal, bamboo fiber, cuprammonium fiber, etc.
[0003] At present, the main dyeing method for dyeing regenerated cellulose fiber cheese yarn with reactive dyes is the dye vat water bath dyeing method. The dyeing water bath ratio of this dyeing method is large, the dyeing rate and fixation rate are not high, and the dye utilization rate is about 70%. In addition, a large part of the dye fails to fix on the regenerated cellulose fiber, and a large amount of water is needed to wash it off to meet the fastness requirements. This dyeing method wastes water resources and pollutes the water environment. In addition, a large amount of salt needs to be added during the dyeing process of this dyeing method to promote dyeing, and a large amount of dye and salt exist in the wastewater, which makes it difficult to treat the wastewater and the proportion of wastewater reuse is low.
[0004] CN107794788A discloses a silicon-based non-aqueous dyeing method suitable for cheese yarn. In this scheme, the dye is directly added as a chemical material. This feeding method will highlight the common problem of reactive dye non-aqueous dyeing. Specifically, since most of the water is adsorbed on the regenerated cellulose fiber cheese yarn, the chance of the dye contacting the regenerated cellulose fiber cheese yarn increases, and the dyeing is too fast, which is prone to uneven dyeing. In addition, the feeding method of this scheme will cause the local pH in the dye bath to rise sharply, resulting in the aggravation of the hydrolysis of the dye under high pH conditions, and will also cause the local dye to react with the fiber too quickly, thus causing uneven dyeing. In non-aqueous dyeing, the amount of water used is small, and this phenomenon will be more obvious. Summary of the invention
[0005] In view of the above-mentioned shortcomings and problems of the prior art, the purpose of the present invention is to provide a regenerated cellulose fiber cheese yarn and a reactive dyeing method thereof, which can improve the utilization rate of the dye and the uniformity of the dyeing when dyeing the regenerated cellulose fiber cheese yarn using a non-aqueous medium, and reduce the generation of dyeing wastewater, and reduce the use of salt, so that the treatment of the dyeing wastewater is simple and the reuse rate of the dyeing wastewater is improved.
[0006] In a first aspect, a colored regenerated cellulose fiber cheese yarn is provided, wherein the regenerated cellulose fiber cheese yarn is dyed with reactive dyes, and the dyeing of the regenerated cellulose fiber cheese yarn has a soap fastness of 4-5 under the "National Standard GB / T 3921-2008", a dry friction fastness of 4-5 under the "National Standard GB / T 3920-2008", a wet friction fastness of 3-4, and a color depth of up to 2 / 1 standard depth under the "National Standard GB / T 4841.7-2006".
[0007] In one embodiment, the regenerated cellulose fiber cheese yarn is any one of viscose cheese yarn, tencel cheese yarn, bamboo fiber cheese yarn, modal cheese yarn, chitin fiber cheese yarn, and cupro fiber cheese yarn.
[0008] In one embodiment, the fixation rate of the reactive dye is not less than 80%, the dyeing rate is not less than 99%, and the levelness is level 4-5; the reactive dye is any one of reactive black G, reactive navy blue L-3G, and reactive red LS, or a combination of at least two of them.
[0009] In a second aspect, a method for dyeing regenerated cellulose fiber cheese yarn with reactive dyes based on a non-aqueous medium is provided, comprising the following steps:
[0010] (1) Squeezing water: Pressurizing and squeezing water from the regenerated cellulose fiber cheese yarn after water treatment in a dyeing vat, wherein the pressurizing pressure is 0.01MPa-0.4MPa, so that the moisture content of the regenerated cellulose fiber cheese yarn is 50%-300% (owf.);
[0011] (2) Adding dyeing liquid: adding a non-aqueous medium to the dye vat in a mass ratio of the non-aqueous medium to the regenerated cellulose fiber cheese yarn of (1.5:1)-(30:1); then, adding a first mixed solution of the non-aqueous medium and the dyeing liquid to the dye vat; wherein, when adding the first mixed solution to the dye vat, the material is added in a first linear feeding method of first slow and then fast, and the dye bath temperature is 5-40°C; wherein, after adding the first mixed solution, the dye bath temperature is controlled to be 5-40°C for 10-60 minutes; after adding the first mixed solution, the mass ratio of the non-aqueous medium to the regenerated cellulose fiber cheese yarn in the dye vat is (2:1)-(30.5:1); wherein, the dyeing liquid is composed of 0.1%-30% (owf.) of active dye and 10%-250% (owf.) of water;
[0012] (3) Adding alkali solution: adding a second mixed solution of a non-aqueous medium and an alkali solution to the dye vat; wherein, when the second mixed solution is added to the dye vat, the temperature of the dye bath is 5-40°C; wherein, after the second mixed solution is added, the temperature of the dye bath is controlled to be 5-50°C for 10-60 minutes; after the second mixed solution is added, the mass ratio of the non-aqueous medium to the regenerated cellulose fiber cheese yarn in the dye vat is (3:1)-(31.5:1); wherein the alkali solution is composed of 0.1%-30% (owf.) alkali and 30%-250% (owf.) water;
[0013] (4) Heating: the heating rate is controlled at 0.1-1.5°C / min, the insulation temperature after heating is controlled at 40-100°C, and the insulation time after heating is 10min-200min;
[0014] (5) Washing: the number of washing times is 2-5 times, the water consumption for a single washing is no more than 4 (owf.), the washing temperature is 20-100°C, and the single washing time is 1min-30min;
[0015] (6) Drying.
[0016] In one embodiment, the first linear feeding method is specifically as follows: the feeding speed at the beginning is 0-10 L / min, the feeding speed at the end is 5-100 L / min, the feeding time is 1-100 min, and the feeding speed increases with time.
[0017] In one embodiment, when adding the second mixed liquid to the dye vat, the feeding is performed in a second linear feeding method of first slow and then fast; the second linear feeding method is specifically: the feeding speed at the beginning is 0-10L / min, the feeding speed at the end is 5-100L / min, the feeding time is 1-100min, and the feeding speed increases with time.
[0018] In one embodiment, the non-aqueous medium is a liquid having a surface tension of 1-60 mN / m at 20°C.
[0019] In one embodiment, the non-aqueous medium is any one of hydrocarbons, silicon-based hydrocarbons, cyclomethylsiloxane, liquid paraffin, or a combination of at least two thereof.
[0020] In one embodiment, the reactive dye is any one of reactive black G, reactive navy blue L-3G, and reactive red LS, or a combination of at least two thereof; the alkali in the alkali solution is one of sodium phosphate, sodium silicate, sodium carbonate, sodium hydroxide, sodium monohydrogen phosphate, sodium dihydrogen phosphate, and sodium bicarbonate, or a combination of at least two thereof; the fixation rate of the reactive dye is not less than 80%, the dyeing rate is not less than 99%, and the levelness is grade 4-5.
[0021] In a third aspect, there is provided a regenerated cellulose fiber cheese yarn dyed according to the method of the second aspect.
[0022] In the dyeing bath of the regenerated cellulose fiber cheese yarn used in the reactive dye dyeing method of the regenerated cellulose fiber cheese yarn provided in the embodiment of the present application, most of the liquid is a non-aqueous medium, the amount of water used is very small, and the dye is only dissolved in water but not in the non-aqueous medium. Most of these waters are adsorbed on the regenerated cellulose fiber cheese yarn, so most of the dyes are adsorbed on the regenerated cellulose fiber cheese yarn, and the dyeing rate can be close to 100%. In addition, since the alkali is also only dissolved in water but not in the non-aqueous medium, the reactive dyes dyed on the regenerated cellulose fiber cheese yarn have suitable alkaline conditions, and the fixation rate is also improved accordingly, and the average fixation rate can reach more than 93%. This effect saves more than 20% of reactive dyes compared with traditional water bath dyeing, and does not need to add salt, which reduces the material cost of dyeing, and also reduces the proportion of floating dyes that need to be washed from about 30% to less than 7%, which is reduced to 1 / 3 of traditional water bath dyeing, thereby reducing the number of washing times and reducing the amount of washing water from about 60 times (owf.) of traditional water bath dyeing to less than 16 times (owf.). In addition, the single-cylinder levelness level of the reactive dye dyeing method for regenerated cellulose fiber cheese yarn provided in the embodiment of the present application can reach level 4-5, which is significantly better than level 3-4 of the non-aqueous medium dyeing method in CN107794788A, and the cylinder difference is small, which is easier to promote and industrialize. Since no salt is added during the dyeing process, the salt content and dye content in the dyeing wastewater are very low, and the subsequent water treatment is simple. DETAILED DESCRIPTION
[0023] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.
[0024] The embodiment of the present application provides a regenerated cellulose fiber cheese yarn, which is dyed with reactive dyes. The dyeing of the regenerated cellulose fiber cheese yarn has a soap fastness of 4-5 under the "National Standard GB / T 3921-2008", a dry friction fastness of 4-5 under the "National Standard GB / T 3920-2008", and a wet friction fastness of 3-4. At the same time, the color depth under the "National Standard GB / T 4841.7-2006" can reach 2 / 1 standard depth.
[0025] The regenerated cellulose fiber cheese yarn can be prepared by the non-aqueous medium dyeing method of the regenerated cellulose fiber cheese yarn with reactive dyes described below.
[0026] The embodiment of the present application provides a non-aqueous medium dyeing method of reactive dyes for regenerated cellulose fiber cheese yarns, which can be used to dye reactive dyes for regenerated cellulose fiber cheese yarns. By adopting this method, when the regenerated cellulose fiber cheese yarns are dyed with reactive dyes, the utilization rate of the reactive dyes can be increased to more than 93%, that is, the color fixation rate (the color fixation rate refers to the percentage of the dye that undergoes a covalent bond reaction with the cellulose fiber to the total dye input) is more than 93%. In other words, more than 93% of the reactive dyes are fixed to the regenerated cellulose fibers, and less than 7% of the reactive dyes are not fixed to the regenerated cellulose fibers, so there is no need for a large amount of water washing, which reduces the generation of dyeing wastewater. In addition, during the dyeing process, no additional salt is required, which makes the treatment of dyeing wastewater simple and can improve the reuse rate of dyeing wastewater. Moreover, the method has a high color fixation rate and can prepare regenerated cellulose fiber cheese yarn with a soap fastness of 4-5 under the "National Standard GB / T3921-2008", a dry friction fastness of 4-5 under the "National Standard GB / T 3920-2008", and a wet friction fastness of 3-4. At the same time, the color depth under the "National Standard GB / T 4841.7-2006" can reach 2 / 1 standard depth.
[0027] In summary, in the regenerated cellulose fiber cheese yarn dyeing method provided in the embodiment of the present application, pre-dyeing water squeezing is introduced to accurately control the moisture content of the regenerated cellulose fiber cheese yarn before dyeing. While improving the dyeing effect of the subsequent dyeing process, it can also solve the cylinder difference problem caused by the different moisture content of the regenerated cellulose fiber cheese yarn before dyeing.
[0028] In the implementation process of the regenerated cellulose fiber cheese yarn dyeing method provided in the embodiment of the present application, the dye liquor is stirred with the non-aqueous medium in the material cylinder, and the material is added linearly while stirring, first slowly and then quickly. This feeding method pre-disperses the dye liquor in the non-aqueous medium, slows down the speed at which the dye liquor contacts the regenerated cellulose fiber cheese yarn, thereby slowing down the dyeing rate, improving the levelness of the non-aqueous medium cheese yarn dyeing, and, in the end, most of the dye liquor is still adsorbed on the regenerated cellulose fiber cheese yarn, which will not have a negative impact on the dyeing rate. And the alkali liquor feeding method in the embodiment of the present application pre-disperses the alkali liquor in the non-aqueous medium, so that the alkali liquor is slowly and evenly adsorbed on the regenerated cellulose fiber cheese yarn, and the pH rises slowly and evenly, which not only slows down the dye hydrolysis, but also makes the alkali energy more quickly and evenly distributed on the regenerated cellulose fiber cheese yarn, and there will be no situation where the local alkali concentration is too high, thereby improving the levelness. After testing, the levelness grade of the finished regenerated cellulose fiber cheese yarn dyed by the dyeing method provided in the embodiment of the present application is not less than 4-5 grades.
[0029] Next, the process flow of the regenerated cellulose fiber cheese yarn dyeing method provided in the embodiment of the present application is described.
[0030] The method comprises the following process steps.
[0031] 1. Prepare dye solution
[0032] The recipe is as follows
[0033] Reactive dyes: 0.1% - 30% (owf.). Exemplarily, the reactive dyes can be any one of reactive black G, reactive navy blue L-3G, reactive red LS, or a combination of at least two of them. It should be noted that the reactive dyes that can be used in the embodiments of the present application are only exemplified here and do not constitute a limitation. In other embodiments, other reactive dyes can also be used, which will not be described one by one here. Among them, owf. represents the percentage relative to the weight of the object to be dyed. For example: under certain conditions, to dye 100 kg of fabric, the amount of dye used is 4% (owf), which means that dyeing these fabrics requires: 100x0.04 = kg of dye.
[0034] The solvent is water, and the amount used is between 10%-250% (owf.).
[0035] 2. Prepare lye
[0036] Alkali: 0.1% - 30% (owf.)
[0037] The alkali can be selected from the group consisting of sodium phosphate, sodium silicate, sodium carbonate, sodium hydroxide, sodium monohydrogen phosphate, sodium dihydrogen phosphate, and sodium bicarbonate, or a combination of at least two of the above.
[0038] The solvent is water, and the amount used is between 30%-250% (owf.).
[0039] 3. Staining
[0040] The dyeing process is as follows
[0041] A. Squeeze water
[0042] The regenerated cellulose fiber cheese yarn after scouring and washing needs to be pressurized and squeezed. This step is achieved by a special dyeing cylinder for non-aqueous medium regenerated cellulose fiber cheese yarn. The pressurization pressure is between 0.01MPa-0.4MPa. After squeezing, the moisture content of the regenerated cellulose fiber cheese yarn is between 50%-300% (owf.). The special dyeing cylinder for non-aqueous medium regenerated cellulose fiber cheese yarn used in this method has a pressurized water squeezing function. Exemplarily, the special dyeing cylinder for non-aqueous medium regenerated cellulose fiber cheese yarn that can be used in this method can be: ultra-low bath ratio, high temperature and high pressure CLEANCOLOUR non-aqueous medium dyeing machine produced by Gaoxun Green Intelligent Equipment (Guangzhou) Co., Ltd.
[0043] B. Staining
[0044] Dyeing is achieved by using the above-mentioned non-aqueous medium regenerated cellulose fiber cheese yarn special dyeing vat, and the dye bath is composed of a large amount of non-aqueous medium and a small amount of water during dyeing. Among them, under the condition that the total bath ratio remains unchanged, the water used for flow and heat conduction in traditional water bath dyeing is replaced by a non-aqueous medium (the non-aqueous medium does not dissolve the reactive dye), leaving only a small amount of water for dissolving the dye and alkali and providing a reaction environment. Under this condition, most of the dyes are adsorbed on the regenerated cellulose fiber cheese yarn without salt-promoting dyeing, thereby improving the dye uptake rate. On this basis, this part of the water has a strong alkalinity, and the dyes dyed on the fibers are more likely to react chemically with the fibers and fix on the fibers, thereby improving the color fixation rate, thereby improving the dye utilization rate.
[0045] After squeezing water from the regenerated cellulose fiber cheese yarn in a dye vat, a non-aqueous medium is added to the dye vat, wherein the mass ratio of the added non-aqueous medium to the regenerated cellulose fiber cheese yarn is between (1.5:1) and (30:1).
[0046] Add dye liquor to the dye vat, wherein the amount of the dye liquor is determined by the dye liquor formula of step 1 and the mass of the regenerated cellulose fiber cheese yarn. Specifically, the dye liquor can be stirred in the material vat of the dye vat together with a non-aqueous medium taken separately (i.e., the non-aqueous medium is not taken from the dye vat) to obtain a dye liquor mixed with a non-aqueous medium. Then, the dye liquor mixed with a non-aqueous medium is added to the red dye. When the dye liquor is added to the dye vat, the dye bath temperature is controlled at 5-40°C. Among them, the lower the temperature, the less the dye is hydrolyzed. Controlling the temperature can achieve the purpose of reducing the hydrolysis of the reactive dye and improving the dyeing rate. When adding dye liquid to the dye vat, the dye liquid is stirred and added in a linear manner (i.e., the dye liquid mixed with a non-aqueous medium), first slowly and then quickly. This operation can make the dye liquid relatively evenly distributed in the non-aqueous medium in the form of small droplets, slow down the contact between the dye liquid and the regenerated cellulose fiber cheese yarn, and slowly dye the regenerated cellulose fiber cheese yarn, achieving a slow dyeing effect, improving the levelness of the regenerated cellulose fiber cheese yarn, thereby improving the shortcoming of poor levelness caused by too fast dyeing of non-aqueous media.
[0047] In this method of adding dye liquid, since the dye vat contains a non-aqueous medium, the dye liquid and the non-aqueous medium are first mixed in the material vat and then added to the dye vat to prevent the dye liquid from directly contacting the fiber before being evenly mixed with the non-aqueous medium after being added to the dye vat, which may easily cause color spots.
[0048] The linear feeding method can be specifically: the feeding speed at the beginning is 0-10L / min, the feeding speed at the end is 5-100L / min, the feeding time is 1-100min, the feeding speed increases with time, and the parameter of the feeding speed change can be adjusted in the range of 0-100. The larger the parameter, the smaller the starting feeding speed, and the smaller the speed change for a period of time at the beginning. The dye vat used in this method has a linear feeding function, and the aforementioned linear feeding method can be implemented.
[0049] After the dye solution is added, the 5-40°C holding time is controlled between 10-60 minutes, at which time the mass ratio of the regenerated cellulose fiber cheese yarn to the non-aqueous medium is 1:2-1:30.5.
[0050] When adding alkali, the dye bath temperature is controlled at 5-40℃. Under alkaline conditions, temperature control is very important. On the one hand, the lower the temperature, the less the dye hydrolyzes. Controlling the temperature can reduce the hydrolysis of active dyes and improve the fixation rate. On the other hand, the alkali solution needs to be evenly dispersed on the regenerated cellulose fiber cheese yarn at low temperature. Otherwise, if the temperature is too high when the alkali solution is uneven, the places with high alkali concentration will react quickly, and the places with low alkali concentration will basically not react, resulting in uneven dyeing.
[0051] Alkali solution is added to the dye vat. Wherein, the amount of alkali solution added is determined by the alkali solution formula of step 2 and the quality of the regenerated cellulose fiber cheese yarn. Specifically, the alkali solution can be stirred together with the non-aqueous medium taken from the material tank of the dye vat (i.e., the non-aqueous medium is not taken from the dye vat) to obtain an alkali solution mixed with the non-aqueous medium. Then the alkali solution mixed with the non-aqueous medium is added to the red dyeing. Wherein, when adding alkali solution to the dye vat, the alkali solution and the non-aqueous medium in the material tank are stirred while the linear feeding method is used to feed (i.e., the alkali solution mixed with the non-aqueous medium), first slowly and then quickly, so that the alkali solution can be relatively evenly distributed in the non-aqueous medium in the form of small droplets, the contact between the dye solution and the regenerated cellulose fiber cheese yarn is slowed down, and the alkali solution is slowly adsorbed on the regenerated cellulose fiber cheese yarn, so that the pH value of the entire dye bath can be slowly and evenly increased, avoiding color flowers caused by sudden changes in pH value, and improving the levelness of the regenerated cellulose fiber cheese yarn, thereby further improving the shortcomings of poor levelness caused by too fast dyeing of non-aqueous medium dyeing. After adding the alkali, the 5-50°C holding time is controlled between 10-60 minutes, at which time the ratio of the regenerated cellulose fiber cheese yarn to the non-aqueous medium is 1:3-1:31.5.
[0052] Heating: When heating, the heating rate is controlled at 0.1-1.5℃ / min, the insulation temperature after heating is controlled between 40-100℃, and the insulation time after heating is controlled between 10min-200min.
[0053] The linear addition method of the alkali solution can be implemented by referring to the linear addition method of the dye solution, which will not be described in detail here.
[0054] The non-aqueous medium used in the method needs to be liquid, and the surface tension is controlled at 1-60 mN / m (20° C.) The non-aqueous medium used in the method can be any one of hydrocarbons, silicon-based hydrocarbons, cyclomethylsiloxane, liquid paraffin, or a combination of at least two thereof.
[0055] In this specification, unless otherwise specified, the mass of the regenerated cellulose fiber cheese yarn refers to the mass of the dry regenerated cellulose fiber cheese yarn, that is, the mass of the cheese yarn that has not been washed before dyeing.
[0056] C. Washing
[0057] The washing is achieved by the above-mentioned non-aqueous medium regenerated cellulose fiber cheese yarn special dyeing vat. Since the dyeing step improves the utilization rate of dyes, the washing pressure is reduced, the number of washings is reduced, and no salt is added, the content of dyes and salts in the dyeing wastewater is very low, which is convenient for treatment and reuse. The whole washing process includes the number of washings being controlled between 2-5 times, the water consumption for a single washing being no more than 4 times (owf.), the total washing water being controlled below 8-20 times (owf.), the washing temperature being controlled between 20-100°C, and the single washing time being controlled between 1min-30min.
[0058] D. Drying
[0059] Drying is achieved by means of a dryer.
[0060] Next, in a specific example, the method for dyeing regenerated cellulose fiber cheese yarn provided in the example of the present application is illustrated.
[0061] Example 1: Preparation of black viscose cheese yarn.
[0062] Viscose cheese yarn to be dyed: 40s viscose cheese yarn.
[0063] Viscose cheese yarn to be dyed: 288kg.
[0064] Dye solution formula:
[0065] Reactive Black G: 5% (owf.);
[0066] Water for chemical dyeing: 40% (owf.).
[0067] Lye Recipe:
[0068] Soda ash: 15% (owf.);
[0069] Water for alkali treatment: 60% (owf.).
[0070] Dyeing process and parameters
[0071] 11. Weigh and mix materials.
[0072] 12. Before dyeing, the viscose cheese yarn after scouring and squeezing is placed in a non-aqueous medium regenerated cellulose fiber cheese yarn special dyeing vat. When squeezing, the pressure is 0.15 MPa. After squeezing, the moisture content of the viscose cheese yarn is 200% (owf.). In this embodiment, unless otherwise specified, the non-aqueous medium regenerated cellulose fiber cheese yarn special dyeing vat can be referred to as a dyeing vat.
[0073] 13. Add non-aqueous medium and put it into the dyeing vat. At this time, the mass ratio of viscose cheese yarn to non-aqueous medium is 1:3.
[0074] 14. Add dye liquid, add the dye liquid into the material tank of the dye vat through the automatic feeding system, and then add non-aqueous medium, stir, and linearly add material (i.e. dye liquid mixed with non-aqueous medium) into the dye vat. The dye bath temperature is 30℃ when the dye liquid is added to the dye vat, and the heat preservation time at 32℃ after adding the dye liquid is 40 minutes. The ratio of viscose cheese yarn to non-aqueous medium is 1:3.5.
[0075] 15. Add alkali, add the alkali solution to the material tank of the dyeing vat through the automatic feeding system, and then add non-aqueous medium, stir, and linearly add material (i.e. alkali solution mixed with non-aqueous medium) to the dyeing vat. The dye bath temperature is 33°C when the alkali solution is added to the dyeing vat, and the insulation time at 35°C after adding alkali is 30 minutes. At this time, the ratio of viscose cheese yarn to non-aqueous medium is 1:4.
[0076] 16. Heat up, and the heating rate is controlled at 1℃ / min.
[0077] 17. Keep warm: after heating up, the temperature is kept at 60℃ and the time is 70min.
[0078] 18. Washing, washing temperature is 80℃, single washing time is 10min, washing times are 3 times, water consumption for each washing is 4 times (owf.). The total washing water consumption for 3 washing times is 12 times (owf.).
[0079] 19. Drying.
[0080] 20. The test results show that the dye uptake rate (dye uptake rate refers to the ratio of dye adsorbed from dye solution to fiber before dye is fixed by soda ash) is 99%, the fixation rate is 93%, and the levelness is 4-5. The levelness can be measured as follows: the cheese yarn is woven into cloth, and the DE value is measured at a certain number of positions on the cloth surface. If the value is less than 0.8, it is levelness 4-5.
[0081] 21. The various indicators of the finished viscose cheese yarn are shown in Table 1.
[0082] The main fastness of the finished regenerated cellulose fiber cheese yarn was tested according to the National Standard GB / T 3921-2008 and the National Standard GB / T 3920-2008. The test results are shown in Table 1.
[0083] Table 1
[0084] Soap fastness Dry rubbing fastness Wet rubbing fastness Level 4-5 Level 4-5 Level 3-4
[0085] In addition, after testing, the uniformity of the finished viscose cheese yarn can meet customer requirements, and there is no difference between the inner and outer layers; the yarn strength of the finished viscose cheese yarn can meet customer requirements; the yarn softness can meet weaving requirements; the surface effect and feel of the yarn after weaving can also meet customer requirements.
[0086] Example 2, navy blue Tencel cheese yarn.
[0087] Tencel cheese yarn to be dyed: 32-count Tencel cheese yarn.
[0088] The mass of the tencel cheese yarn to be dyed is 288kg.
[0089] Dye solution formula:
[0090] Active navy blue L-3G: 3% (owf.);
[0091] Water for chemical dyeing: 30% (owf.).
[0092] Lye recipe:
[0093] Soda ash: 10% (owf.);
[0094] Water for alkali treatment: 50% (owf.).
[0095] Dyeing process and parameters
[0096] 21. Weigh and prepare materials.
[0097] 22. Before dyeing, the water is squeezed out, and the Tencel cheese yarn after scouring and squeezing is placed in a non-aqueous medium regenerated cellulose fiber cheese yarn special dyeing vat. When squeezing out the water, the pressure is 0.3 MPa, and the moisture content of the Tencel cheese yarn after squeezing out the water is 180% (owf.). In this embodiment, unless otherwise specified, the non-aqueous medium regenerated cellulose fiber cheese yarn special dyeing vat can be referred to as a dyeing vat.
[0098] 23. Add non-aqueous medium and put it into the dyeing vat. At this time, the mass ratio of Tencel cheese yarn to non-aqueous medium is 1:4.
[0099] 24. Add dye liquid, add the dye liquid into the material tank of the dye vat through the automatic feeding system, then add non-aqueous medium, stir, and linearly add material (i.e. dye liquid mixed with non-aqueous medium) into the dye vat. The dye bath temperature is 31°C when the dye liquid is added to the dye vat, and the 34°C insulation time after adding the dye liquid is 20 minutes. The ratio of Tencel cheese yarn to non-aqueous medium is 1:4.5.
[0100] 25. Add alkali, add the alkali solution to the material tank of the dyeing vat through the automatic feeding system, and then add non-aqueous medium, stir, and linearly add material (i.e. alkali solution mixed with non-aqueous medium) to the dyeing vat. The dye bath temperature is 36°C when the alkali solution is added to the dyeing vat, and the heat preservation time at 40°C after adding alkali is 30 minutes. At this time, the ratio of regenerated cellulose fiber cheese yarn to non-aqueous medium is 1:5.
[0101] 26. Heat up, and the heating rate is controlled at 1℃ / min.
[0102] 27. Keep warm: after heating, the temperature is kept at 60℃ and the time is 50min.
[0103] 28. Washing, washing temperature is 60℃, single washing time is 10min, washing times are 2 times, water consumption for each washing is 4 times (owf.). The total washing water consumption for 2 washing times is 8 times (owf.).
[0104] 29. Drying.
[0105] 30. The test results show that the dyeing rate is 99%, the fixing rate is 95%, and the levelness is 4-5.
[0106] 31. The various indicators of the finished Tencel cheese yarn are shown in Table 2.
[0107] The main fastness of the finished Tencel cheese yarn was tested according to the National Standard GB / T 3921-2008 and the National Standard GB / T 3920-2008. The test results are shown in Table 2.
[0108] Table 2
[0109] Soap fastness Dry rubbing fastness Wet rubbing fastness Level 4-5 Level 4-5 Level 3-4
[0110] In addition, after testing, the uniformity of the finished Tencel cheese yarn can meet customer requirements, and there is no difference between the inner and outer layers; the yarn strength of the finished Tencel cheese yarn can meet customer requirements; the yarn softness can meet weaving requirements; the surface effect and feel of the yarn after weaving can also meet customer requirements.
[0111] Example 3, red bamboo fiber cheese yarn.
[0112] Bamboo fiber cheese yarn to be dyed: 40s bamboo fiber cheese yarn.
[0113] The mass of bamboo fiber cheese yarn to be dyed is 288kg.
[0114] Dye solution formula:
[0115] Reactive Red LS: 0.5% (owf.);
[0116] Water for chemical dyes: 10% (owf.).
[0117] Lye recipe:
[0118] Soda ash: 5% (owf.);
[0119] Water for alkali treatment: 30% (owf.).
[0120] Dyeing process and parameters
[0121] 31Weigh and prepare materials.
[0122] 32 The bamboo fiber cheese after scouring and squeezing is placed in a non-aqueous medium regenerated cellulose fiber cheese special dyeing vat. When squeezing, the pressure is 0.4 MPa. After squeezing, the moisture content of the bamboo fiber cheese is 130% (owf.). In this embodiment, unless otherwise specified, the non-aqueous medium regenerated cellulose fiber cheese special dyeing vat can be referred to as a dyeing vat.
[0123] 33. Add non-aqueous medium and put the non-aqueous medium into the dyeing vat. At this time, the ratio of bamboo fiber cheese yarn to non-aqueous medium is 1:4.
[0124] 34. Add dye solution, add the dye solution to the material tank of the dye vat through the automatic feeding system, and then add non-aqueous medium, stir, and linearly add material (i.e. dye solution mixed with non-aqueous medium) to the dye vat. The dye bath temperature is 25℃ when the dye solution is added to the dye vat, and the heat preservation time at 27℃ after adding the dye solution is 20 minutes. The ratio of bamboo fiber cheese yarn to non-aqueous medium is 1:4.3.
[0125] 35. Add alkali, add the alkali solution to the material tank of the dye vat through the automatic feeding system, then add non-aqueous medium, stir, and linearly add material (i.e. alkali solution mixed with non-aqueous medium) to the dye vat. The dye bath temperature is 34°C when the alkali solution is added to the dye vat, and the insulation time at 36°C after adding alkali is 20 minutes. At this time, the ratio of bamboo fiber cheese yarn to non-aqueous medium is 1:4.6.
[0126] 36.Heat up, and the heating rate is controlled at 1℃ / min.
[0127] 37. Keep warm. After heating, the temperature is kept at 60℃ and the keeping time is 20min.
[0128] 38. Washing, washing temperature is 30℃, single washing time is 10min, washing times are 2 times, water consumption for each washing is 4 times (owf.). The total washing water consumption for 2 washing times is 8 times (owf.).
[0129] 39. Drying.
[0130] The test results show that the dyeing rate is 99%, the fixing rate is 97%, and the levelness is 4-5.
[0131] 41. The various indicators of the finished bamboo fiber cheese yarn are shown in Table 3.
[0132] The main fastness of the finished bamboo fiber cheese yarn was tested according to the National Standard GB / T 3921-2008 and the National Standard GB / T 3920-2008. The test results are shown in Table 3.
[0133] Table 3
[0134] Soap fastness Dry rubbing fastness Wet rubbing fastness Level 4-5 Level 4-5 Level 4-5
[0135] In addition, after testing, the uniformity of the finished bamboo fiber cheese yarn can meet customer requirements, and there is no difference between the inner and outer layers; the yarn strength of the finished bamboo fiber cheese yarn can meet customer requirements; the yarn softness can meet weaving requirements; the surface effect and feel of the yarn after weaving can also meet customer requirements.
[0136] In the dyeing bath of the regenerated cellulose fiber cheese yarn used in the reactive dye dyeing method of the regenerated cellulose fiber cheese yarn provided in the embodiment of the present application, most of the liquid is a non-aqueous medium, the amount of water used is very small, and the dye is only dissolved in water but not in the non-aqueous medium. Most of these waters are adsorbed on the regenerated cellulose fiber cheese yarn, so most of the dyes are adsorbed on the regenerated cellulose fiber cheese yarn, and the dyeing rate can be close to 100%. In addition, since the alkali is also only dissolved in water but not in the non-aqueous medium, the reactive dyes dyed on the regenerated cellulose fiber cheese yarn have suitable alkaline conditions, and the fixation rate is also improved accordingly, and the average fixation rate can reach more than 93%. This effect saves more than 20% of reactive dyes compared with traditional water bath dyeing, and does not need to add salt, which reduces the material cost of dyeing, and also reduces the proportion of floating dyes that need to be washed from about 30% to less than 7%, which is reduced to 1 / 3 of traditional water bath dyeing, thereby reducing the number of washing times and reducing the amount of washing water from about 60 times (owf.) of traditional water bath dyeing to less than 16 times (owf.). In addition, the single-cylinder levelness level of the reactive dye dyeing method for regenerated cellulose fiber cheese yarn provided in the embodiment of the present application can reach level 4-5, which is significantly better than level 3-4 of the non-aqueous medium dyeing method in CN107794788A, and the cylinder difference is small, which is easier to promote and industrialize. Since no salt is added during the dyeing process, the salt content and dye content in the dyeing wastewater are very low, and the subsequent water treatment is simple.
[0137] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for dyeing regenerated cellulose fiber cheese yarn with reactive dyes based on a non-aqueous medium, It is characterized in that The method is used for dyeing regenerated cellulose fiber cheese yarn with reactive dyes, wherein the dyeing of the regenerated cellulose fiber cheese yarn has a soap fastness of 4-5 under the national standard GB / T 3921-2008, a dry rubbing fastness of 4-5 under the national standard GB / T3920-2008, a wet rubbing fastness of 3-4, and a color depth of 2 / 1 standard depth under the national standard GB / T4841.7-2006; the fixation rate of the reactive dye is not less than 80%, the dyeing rate is not less than 99%, and the levelness is 4-5; the method comprises the following steps: (1) squeezing water: squeezing water from the washed regenerated cellulose fiber cheese yarn in a dye vat, wherein the pressurized pressure is 0.01MPa-0.4MPa, so that the moisture content of the regenerated cellulose fiber cheese yarn is 50%-300% (owf.); (2) Add dyeing liquid: the mass ratio of non-aqueous medium to regenerated cellulose fiber cheese yarn is (1.5:1)-(30: 1), adding a non-aqueous medium to the dye vat; then, adding a first mixed solution of a non-aqueous medium and a dye liquor to the dye vat; wherein, when adding the first mixed solution to the dye vat, the material is added in a first linear feeding method of first slow and then fast, and the dye bath temperature is 5-40°C; wherein, after adding the first mixed solution, the dye bath temperature is controlled to be 5-40°C for 10-60 minutes; after adding the first mixed solution, the mass ratio of the non-aqueous medium to the regenerated cellulose fiber cheese yarn in the dye vat is (2:1)-(30.5:1); wherein the dye liquor is composed of 0.1%-30% (owf.) of active dyes and 10%-250% (owf.) of water; (3) Adding alkali solution: adding a second mixed solution of a non-aqueous medium and alkali solution to the dye vat; wherein, when the second mixed solution is added to the dye vat, the temperature of the dye bath is 5-40°C; wherein, after the second mixed solution is added, the temperature of the dye bath is controlled to be 5-50°C for 10-60 minutes; after the second mixed solution is added, the mass ratio of the non-aqueous medium to the regenerated cellulose fiber cheese yarn in the dye vat is (3:1)-(31.5:1); wherein the alkali solution is composed of 0.1%-30% (owf.) alkali and 30%-250% (owf.) water; (4) Heating: The heating rate is controlled at 0.1-1.5℃ / min, and the insulation temperature is controlled at 40-100℃ after heating. After heating, the insulation time is 10min-200min; (5) Washing: the number of washing times is 2-5 times, the water consumption for a single washing is no more than 4 (owf.), the washing temperature is 20-100°C, and the single washing time is 1min-30min; (6) Drying.
2. The method according to claim 1, It is characterized in that The first linear feeding method is specifically as follows: the feeding speed is 0-10 L / min at the beginning, the feeding speed is 5-100 L / min at the end, the feeding time is 1-100 min, and the feeding speed increases with time.
3. The method according to claim 1, It is characterized in that When adding the second mixed liquid to the dye vat, the feeding is performed in a second linear feeding method of first slow and then fast; the second linear feeding method is specifically: the feeding speed at the beginning is 0-10L / min, the feeding speed at the end is 5-100L / min, the feeding time is 1-100min, and the feeding speed increases with time.
4. The method according to any one of claims 1 to 3, It is characterized in that The non-aqueous medium is a liquid and has a surface tension of 1-60 mN / m at 20°C.
5. The method according to claim 4, It is characterized in that The non-aqueous medium is any one of hydrocarbons, silicon-based hydrocarbons, cyclomethylsiloxane, and liquid paraffin, or a combination of at least two thereof.
6. The method according to any one of claims 1 to 3, It is characterized in that The reactive dye is any one of reactive black G, reactive navy blue L-3G, and reactive red LS, or a combination of at least two of them; the alkali in the alkali solution is one of sodium phosphate, sodium silicate, sodium carbonate, sodium hydroxide, sodium monohydrogen phosphate, sodium dihydrogen phosphate, and sodium bicarbonate, or a combination of at least two of them.
7. Regenerated cellulose fiber cheese yarn dyed by the method according to any one of claims 1 to 3.