A method for detecting the quality of laser welding of soft-pack lithium battery tabs
Through welding seam temperature rise experiments and temperature standard deviation analysis, combined with welding seam pressure drop data, the problems of low detection efficiency and misjudgment risk in the existing technology have been solved, and the quality of laser welding of soft-pack lithium battery tabs has been achieved quickly and accurately. Detection avoids product waste.
Patent Information
- Application Number
- CN202210048108.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-17
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-01-17
AI Technical Summary
The existing technology is inefficient when detecting the laser welding quality of soft-pack lithium battery tabs, and there is a risk of misjudgment and product waste. It cannot effectively verify the welding tension value of each product, especially for weakly welded products, the risk of misjudgment is high.
Through the weld temperature rise experiment, a temperature measuring device is used to measure the temperature of the temperature measuring points on the tab weld, the temperature standard deviation is calculated, and secondary judgment is made based on the weld pressure drop data to quickly and accurately judge the lithium battery tab. Laser welding quality to avoid damaging the product.
It is possible to quickly and accurately judge the welding quality of each lithium battery tab without damaging the product, reducing the risk of misjudgment, avoiding product waste, and improving detection efficiency and accuracy.
Smart Images

Figure CN114486982B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for detecting the laser welding quality of a soft-package lithium battery tab, and belongs to the technical field of welding. Background Art
[0002] Laser welding is an efficient and precise welding method that uses a high-energy-density laser beam as a heat source. It has been widely used in the lithium battery industry due to its advantages of high efficiency, low power consumption, and small welding deformation. However, the welded workpiece may have defects such as cold welding, blown welding, weld penetration, and abnormal welding points, which seriously threaten the safety and quality of the product. Therefore, the weld must be inspected during the production process to promptly detect and eliminate batteries with poor welding to avoid flowing into the next process and causing safety hazards.
[0003] See also Figure 1 and Figure 2 The lithium-ion battery module includes two cells. The first cell 1 is provided with a welding terminal tab 101 of the first cell at one end and a charging terminal tab 102 of the first cell at the other end. The second cell 2 is provided with a welding terminal tab 201 of the second cell at one end and a charging terminal tab 202 of the second cell at the other end. The welding terminal tab 101 of the first cell and the welding terminal tab 201 of the second cell are connected together by laser welding. The welding process is: the welding terminal tab 101 of the first cell and the welding terminal tab 201 of the second cell are placed together on the supporting copper bar 5, and then welded by a laser welding machine. The tab weld 8 formed is a straight weld.
[0004] There are two main methods for detecting the existing pole lug welds, namely X-ray detection and weld tensile detection. X-ray detection is a non-contact detection method that integrates the characteristics of defect detection, positioning, and inverse geometric dimension accuracy. However, due to its narrow application range and high requirements on the quality of production personnel, it has not yet been widely used in the field of lithium battery welding detection. Weld tensile detection is mainly used for random inspection of products. It is a destructive test, which not only causes waste of products, but also has the problem of missed inspections, and it is impossible to verify the welding tensile value of each product. At the same time, for products with weak welds, although the welding molten pool is small, the welding tensile force is not necessarily small, and there is a certain risk of misjudgment. Therefore, it is very necessary to seek a method that can efficiently and accurately detect the quality of laser welding of soft-pack lithium battery pole lugs. Summary of the invention
[0005] The purpose of the present invention is to provide a method for detecting the quality of laser welding of a soft-pack lithium battery tab in view of the drawbacks of the prior art, so as to quickly and accurately judge the welding quality of the lithium battery tab and avoid waste of products.
[0006] The problem described in the present invention is solved by the following technical solution:
[0007] A method for detecting the quality of laser welding of a soft-pack lithium battery tab, the method comprising the following steps:
[0008] First, conduct the weld temperature rise test. The specific steps are as follows:
[0009] a. L represents the length of the electrode ear weld of the battery module being tested, and the maximum allowable virtual weld length S is set;
[0010] b. Make an experimental battery module so that the length of the unwelded portion of the entire tab weld is S and the length of the welded portion is LS;
[0011] c. Divide the pole ear weld into n equal parts along its length direction, and use the two end points of the pole ear weld and each equal division point as temperature measurement points to obtain n+1 temperature measurement points;
[0012] d. Connect the two cells of the battery module to the two electrodes at the output end of the constant current source, respectively, so that the current output by the constant current source A continuously flows through the electrode tab weld and the temperature of the electrode tab weld reaches a stable value;
[0013] e. Use the temperature measuring device to measure the temperature of each temperature measuring point on the tab weld, obtain a set of temperature data of the temperature measuring points, and calculate the standard deviation σ of the tab weld temperature of the experimental battery module:
[0014]
[0015] Where t i represents the temperature measurement value of the i-th temperature measurement point, i=1,2,…,n+1, Represents the average value of the temperature data at the temperature measurement point, that is
[0016] f. Changing the position of the unwelded portion in the tab weld, remaking the experimental battery module, and repeating steps c to f until the tab weld temperature standard deviation of m experimental battery modules is obtained;
[0017] g. Calculate the average value of the standard deviation of the welding temperature of the tabs of m experimental battery modules
[0018] Then, the quality of laser welding of the soft-pack lithium battery tabs was tested based on the experimental results:
[0019] When testing the quality of laser welding of the tabs of soft-pack lithium batteries, firstly, the standard deviation of the tab weld temperature σ′ of the tested battery module is obtained according to the method of steps c to e, and then σ′ is compared with For comparison, if It is preliminarily judged that the laser welding quality of the soft-pack lithium battery tab is qualified, otherwise it is judged to be unqualified.
[0020] In the above-mentioned soft-pack lithium battery tab laser welding quality detection method, during the weld temperature rise experiment, while using a temperature measuring device to measure the temperature of each temperature measuring point on the tab weld, a voltmeter is used to measure the voltage between the welding end tabs of two battery cells to obtain the tab weld voltage drop V of the m experimental battery modules. j , j = 1, 2, ..., m, and then find V j The average When testing the quality of laser welding of soft-pack lithium battery tabs, the same method is used to measure the voltage drop V' of the tab weld of the battery module being tested. By comparing V′ with The size of the welding quality is judged again. If the laser welding quality of the soft-pack lithium battery tab is good, it is judged to be unqualified; otherwise, it is judged to be unqualified.
[0021] In the above-mentioned soft-pack lithium battery tab laser welding quality inspection method, when conducting the weld temperature rise experiment, the maximum allowable cold weld length S is set to: S=0.1L~0.12L.
[0022] In the above-mentioned soft-pack lithium battery tab laser welding quality detection method, 21 to 61 temperature measuring points are set on the tab weld.
[0023] In the above-mentioned soft-pack lithium battery tab laser welding quality inspection method, when conducting the weld temperature rise experiment, the number of battery modules produced for the experiment is 5 to 10.
[0024] In the above-mentioned soft-pack lithium battery tab laser welding quality detection method, the temperature measuring device is a laser thermometer.
[0025] In the above-mentioned soft-pack lithium battery tab laser welding quality detection method, the output current of the constant current source is twice the rate discharge current of the battery module being detected.
[0026] The present invention obtains the maximum tab weld temperature standard deviation data of qualified battery modules through a weld temperature rise experiment, and then detects the laser welding quality of the soft-pack lithium battery tab according to the experimental results. It can quickly and accurately judge the welding quality of each lithium battery tab without damaging the product, thereby avoiding product waste. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The present invention will be further described below in conjunction with the accompanying drawings.
[0028] Figure 1 This is a schematic diagram of the welding seam of the pole ear of a soft-pack lithium battery;
[0029] Figure 2 This is the end view of the welding seam of the soft-pack lithium battery ear;
[0030] Figure 3It is a schematic diagram of weld pressure drop measurement;
[0031] Figure 4 It is a schematic diagram of weld temperature measurement.
[0032] The numbers in the figure are: 1. first battery cell, 101. welding end ear of the first battery cell, 102. charging end ear of the first battery cell, 2. second battery cell, 201. welding end ear of the second battery cell, 202. charging end ear of the second battery cell, 3. positive electrode of constant current source, 4. negative electrode of constant current source, 5. supporting copper bus, 6. negative electrode of voltmeter, 7. positive electrode of voltmeter, 8. ear weld, 9. temperature measuring point, 10. temperature measuring device, A. constant current source, V. voltmeter. DETAILED DESCRIPTION
[0033] The present invention provides a method for detecting the quality of laser welding of a soft-pack lithium battery tab, which improves the efficiency and accuracy of welding quality detection and solves the problems of low detection efficiency, high labor intensity, risk of misjudgment and product waste in traditional methods.
[0034] The detection equipment used in the present invention includes a weld pressure drop measurement device and a weld temperature measurement device.
[0035] See also Figure 3 The welding seam voltage drop measuring device comprises a constant current source A and a voltmeter V, a positive electrode 3 of the constant current source, a negative electrode 4 of the constant current source, a negative electrode 6 of the voltmeter, and a positive electrode 7 of the voltmeter. The welding seam temperature measuring device comprises a temperature measuring device 10, which is a laser thermometer.
[0036] This method is summarized on the basis of a large number of experiments. The purpose of the experiment is to find out the technical indicators that can reflect the quality of laser welding of the tab, and then construct a scientific and reasonable criterion. As we all know, poor welding quality will lead to increased weld resistance. According to Joule's law, when the current is constant, the resistance increases and the heat generation will increase, and the weld temperature will also rise accordingly. Therefore, the quality of welding can be judged according to the change of weld temperature. However, when the welding defect is small, the change of weld temperature is often not obvious, and for longer straight welds, the selection of the temperature measurement point position will have a great impact on the measurement results. In most cases, weld defects such as cold welding and welding penetration appear locally. Since the current is mainly distributed in the well-welded parts, the current in the defective parts is very small or zero, and its heat generation can be ignored. Therefore, the temperature rise of the parts with welding defects is small or the temperature does not rise (such as the leaking parts), and the temperature of the well-welded parts rises due to the increase of current density. Therefore, the general temperature detection method cannot accurately judge the quality of laser welding of the tab. Compared with normal welds, the temperature rise of the parts with welding defects is smaller, while the temperature rise of the parts with good welding is larger. Therefore, it is impossible to accurately judge the welding quality based on the average temperature of different parts of the weld.
[0037] Through analysis, it can be seen that for the lug welds with local welding defects, the dispersion of weld temperature in different parts is aggravated. Therefore, we judge the welding quality based on the standard deviation of the lug weld temperature.
[0038] Based on the above analysis, we designed the following experiments:
[0039] 1. The total length of the tab weld is 60mm, there are no welding defects, the weld is divided into 60 equal parts, 61 temperature measurement points are set, the temperature measurement points are 1mm apart, numbered 1 to 61, the constant current source provides a current of 100A, and 10 sets of welded modules are used. The voltage drop range of the tab weld measured by the voltmeter is 0.0008 to 0.0012mV. The infrared thermometer collects the temperature of the weld and obtains an average temperature rise of 2.1℃, a maximum temperature rise of 2.2℃, and a minimum temperature rise of 1.8℃. The average value of the calculated standard deviation is 0.013℃.
[0040] 2. The total length of the pole ear weld is 60mm, the normal welding length is 55mm, and the rest is reserved blank. 61 temperature measurement points are set, with a temperature measurement point interval of 1mm, numbered 1 to 61, and the constant current source provides a current of 100A. 10 groups of welded modules are used, and the positions of the reserved blanks are different. The voltage drop range of the pole ear weld measured by the voltmeter is 0.0016 to 0.0019mV. The infrared thermometer collects the temperature of the weld and obtains an average temperature rise of 2.2℃, a maximum of 2.9℃, and a minimum of 0.5℃. The average value of the calculated standard deviation is 0.819℃.
[0041] 3. The total length of the pole ear weld is 60mm, the normal welding length is 50mm, and the rest is reserved blank. 61 temperature measurement points are set, with a temperature measurement point interval of 1mm, numbered 1 to 61, and the constant current source provides a current of 100A. 10 groups of welded modules are used, and the positions of the reserved blanks are different. The voltage drop range of the pole ear weld measured by the voltmeter is 0.0021 to 0.0025mV. The infrared thermometer collects the temperature of the weld and obtains an average temperature rise of 2.3℃, a maximum temperature rise of 3.1℃, and a minimum temperature rise of 0.2℃. The average value of the calculated standard deviation is 2.047℃.
[0042] It can be seen that for the lug welds with local welding defects, the average temperature rise of the weld does not change significantly, while the standard deviation of the lug weld temperature will increase by dozens of times. Therefore, it is most accurate to use the standard deviation of the lug weld temperature to judge the quality of welding.
[0043] The present invention adopts the following method to detect the quality of the electrode lug weld:
[0044] First, conduct the weld temperature rise test. The specific steps are as follows:
[0045] a. L represents the length of the electrode ear weld 8 of the detected battery module, and sets the maximum allowable virtual welding length d;
[0046] b. Making an experimental battery module, so that the length of the unwelded portion of the entire ear weld 8 is S, and the length of the welded portion is LS;
[0047] c. Divide the electrode ear weld 8 into n equal parts along its length, and use the two end points of the electrode ear weld 8 and each equal point as the temperature measurement point to obtain n+1 temperature measurement points;
[0048] d. Connect the two cells of the battery module to the two electrodes at the output end of the constant current source A, respectively, so that the current output by the constant current source A continuously flows through the tab weld 8 and the temperature of the tab weld 8 reaches a stable value;
[0049] e. Use the temperature measuring device 10 to measure the temperature of each temperature measuring point on the tab weld 8, obtain a set of temperature data of the temperature measuring points, and calculate the standard deviation σ of the tab weld temperature of the experimental battery module:
[0050]
[0051] Where t i represents the temperature measurement value of the i-th temperature measurement point, i=1,2,…,n+1, Represents the average value of the temperature data at the temperature measurement point, that is
[0052] f. Changing the position of the unwelded portion in the tab weld 8, remaking the experimental battery module, and repeating steps c to f until the standard deviation of the tab weld temperature of m experimental battery modules is obtained;
[0053] g. Calculate the average value of the standard deviation of the welding temperature of the tabs of m experimental battery modules
[0054] Then, the quality of laser welding of the soft-pack lithium battery tabs was tested based on the experimental results:
[0055] When testing the quality of laser welding of the tabs of soft-pack lithium batteries, firstly, the standard deviation of the tab weld temperature σ′ of the tested battery module is obtained according to the method of steps c to e, and then σ′ is compared with For comparison, if It is preliminarily judged that the laser welding quality of the soft-pack lithium battery tab is qualified, otherwise it is judged to be unqualified.
[0056] The above method is highly accurate in detecting the lug weld with local welding defects. However, in special cases, although the entire weld is poorly welded, the resistance value is relatively uniform. At this time, the standard deviation of the lug weld temperature will be very small, which is prone to misjudgment.
[0057] Considering that the resistance value of the weld will inevitably increase when the weld is poorly welded, the voltage drop when the current of the constant current source flows through will increase significantly, but the resistance value of the weld is very small, at 10 to the -5th power ohms, and the current resistance meter cannot accurately measure it. Therefore, the present invention uses the temperature measuring device 10 to measure the temperature of each temperature measuring point on the tab weld 8, and uses the voltmeter V to measure the voltage between the welding end tabs of the two battery cells to obtain the tab weld voltage drop V of the m experimental battery modules. j , j = 1, 2, ..., m, and then find V j The average When testing the quality of laser welding of soft-pack lithium battery tabs, the same method is used to measure the voltage drop V' of the tab weld of the battery module being tested. By comparing V′ with The size of the welding quality is judged again. If the laser welding quality of the soft-pack lithium battery tab is good, it is judged to be unqualified; otherwise, it is judged to be unqualified.
[0058] Since some electrical characteristics of the weld are more obvious under high current, the output current of the constant current source is 2C of the cell or module capacity.
Claims
1. A method for detecting the quality of laser welding of a soft-pack lithium battery tab, characterized in that: The method comprises the following steps: First, conduct the weld temperature rise test. The specific steps are as follows: a. L represents the length of the electrode ear weld of the battery module being tested, and the maximum allowable virtual weld length S is set; b. Make an experimental battery module so that the length of the unwelded portion of the entire tab weld is S and the length of the welded portion is LS; c. Divide the pole ear weld into n equal parts along its length direction, and use the two end points of the pole ear weld and each equal division point as temperature measurement points to obtain n+1 temperature measurement points; d. Connect the two cells of the battery module to the two electrodes at the output end of the constant current source, respectively, so that the current output by the constant current source continuously flows through the electrode tab weld and the temperature of the electrode tab weld reaches a stable value; e. Use the temperature measuring device to measure the temperature of each temperature measuring point on the tab weld, obtain a set of temperature data of the temperature measuring points, and calculate the standard deviation σ of the tab weld temperature of the experimental battery module: Where t i represents the temperature measurement value of the i-th temperature measurement point, i=1,2,…,n+1, Represents the average value of the temperature data at the temperature measurement point, that is f. Changing the position of the unwelded portion in the tab weld, remaking the experimental battery module, and repeating steps c to f until the tab weld temperature standard deviation of m experimental battery modules is obtained; g. Calculate the average value of the standard deviation of the welding temperature of the tabs of m experimental battery modules Then, the quality of laser welding of the soft-pack lithium battery tabs was tested based on the experimental results: When testing the quality of laser welding of the tabs of soft-pack lithium batteries, firstly, the standard deviation of the tab weld temperature σ′ of the tested battery module is obtained according to the method of steps c to e, and then σ′ is compared with For comparison, if It is preliminarily judged that the laser welding quality of the soft-pack lithium battery tab is qualified, otherwise it is judged to be unqualified; During the weld temperature rise experiment, while measuring the temperature of each temperature measuring point on the tab weld using a temperature measuring device, a voltmeter is used to measure the voltage between the welding tabs of the two cells to obtain the tab weld voltage drop V of the m experimental battery modules. j , j = 1, 2, ..., m, and then find V j The average When testing the quality of laser welding of soft-pack lithium battery tabs, the same method is used to measure the voltage drop V' of the tab weld of the battery module being tested. By comparing V′ with The size of the welding quality is judged again. The laser welding quality of the soft-pack lithium battery tab is judged to be qualified, otherwise it is judged to be unqualified; When the weld temperature rise experiment is performed, the maximum allowable cold weld length S is set to: S=0.1L~0.12L.
2. The method for detecting the quality of laser welding of a soft-pack lithium battery tab according to claim 1, characterized in that: The number of temperature measuring points on the electrode tab weld is 21 to 61.
3. The method for detecting the quality of laser welding of a soft-pack lithium battery tab according to claim 1, characterized in that: When conducting the weld temperature rise experiment, the number of battery modules produced for the experiment is 5 to 10.
4. The method for detecting the quality of laser welding of a soft-pack lithium battery tab according to claim 1, characterized in that: The temperature measuring device is a laser thermometer.
5. The method for detecting the quality of laser welding of a soft-pack lithium battery tab according to claim 1, characterized in that: The output current of the constant current source is a double rate discharge current of the detected battery module.