Injection mold and production method thereof and method for producing marble-textured molded parts
By designing a multi-channel hot runner and a screw injection molding machine in the injection mold, the repeatability and detail of the marble molded parts are achieved, and the color gradient inconsistent and complex operation of the molded parts in the prior art is solved. question.
Patent Information
- Application Number
- CN202080072024.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-05-05
- Filing Date
- 2020-10-13
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-10-13
AI Technical Summary
The prior art is difficult to achieve repeatable and controlled color gradients when producing marble molded parts, and the injection mold design is complicated and the operation is cumbersome, which can easily lead to the formation of casting ports and defects on the molded parts.
A hot runner injection mold consisting of at least two channels is designed to add molded compounds separately by time and space, and to ensure that the molded compounds remain free during the injection process using the rotation and nozzle structure of the screw injection molding machine. Flow, avoiding curing, thus achieving repeatability and detail of marble patterns.
The repeatability and high detail of marble molded parts is achieved, the design and operation of injection molds is simplified, the formation of casting ports is reduced, and the quality and consistency of the finished product is improved.
Smart Images

Figure CN114555320B_ABST
Abstract
Description
[0001] describe
[0002] The invention relates to an injection mold for producing marbled molded parts, comprising at least one hot runner, a cavity, an inlet opening into the injection mold and an inlet opening into the cavity, wherein the hot runner has at least two channels, which are connected to the inlet opening into the cavity at a first end of each channel and to the inlet opening into the injection mold at a second end of each channel.
[0003] The invention also relates to a method for producing a marbled molding, wherein a first molding compound and at least one further molding compound are injected from an injection unit of a screw injection molding machine into an injection mold, and the injection mold has at least one hot runner and a cavity.
[0004] Marbled moldings generally have at least one marbled (i.e., patterned) visible surface, showing surface effects such as color shades, color stripes, lines, and structures. In marbled moldings, at least a portion of the colorant present is not evenly distributed. The formation of the marble effect depends on the proportions of the different colors and the base color of the molding. Marbled moldings generally do not look exactly the same. If they show a repeating identifying pattern in the color structure, they can also be referred to as moldings with repeatable marble. Specifically, the base color, shades, and main pattern are present in a repeating form in a repeatable marbled molding, although variations in color brightness may occur.
[0005] The production of molded parts, in particular polymer molded parts made from powders, granules or molding compounds (which can each be in the form of a mixture), is usually done using screw injection molding machines. For the production of colored polymer articles, colored polymer granules are usually used, or granules of neutral color are mixed with colored polymer granules with a high pigment concentration before or during the liquefaction of the polymer in the extruder. Usually, the mixing elements used in the injection unit ensure the production of a mixture comprising an uncolored basic material and colored granules comprising a high concentration of colorant mixed with maximum homogeneity and a part with no streaks on the surface.
[0006] Screw injection molding machines with hot runners and screw injection molds are generally capable of uniform plasticization or processing, wherein the molding compound to be injected is homogeneously mixed and has a uniform temperature. In the production of marbled moldings, the goal is a uniform temperature, but a homogeneous mixture of the molding compound to be injected is undesirable, which would cause the color-changing parts to remain visible in the finished part.
[0007] In particular, for producing repeatable marble patterns, where the goal is uniformly repeatable color gradients and color distributions, the machines used are typically those that supply at least two marbling components separately to an injection mold, for example in two separate injection units.
[0008] Also known are devices for producing marbled mouldings, in particular nozzles, which are able to combine moulding compounds from two separate injection units in one injection mould.
[0009] The production of reproducible marbled mouldings in a two-component injection moulding machine is complicated because two injection units are required and must be operated, each of which has a screw, a barrel, a feeding device and corresponding hydraulics for moving the screw.
[0010] The molding compound is injected from a screw injection molding machine into an injection mold, which may include a hot runner or a hot runner system having a plurality of parallel melt channels, which lead to a plurality of cavities respectively.
[0011] In plastic processing, especially thermoplastic machine injection molding, hot runner or hot runner system refers to a special design of the gate system. Compared with other parts of the injection mold, the hot runner is thermally insulated and its temperature can be controlled independently, especially independently from other parts of the injection mold.
[0012] In injection molds that do not include hot runners, the gate system is not thermally isolated from the other parts of the injection mold. Therefore, here, the injection mold and the gate system (for example, a screw gate, a film gate or a tunnel gate) located therein are kept at a controlled temperature, which is lower than the melt temperature of the molding compound. During the production of the molded part, due to these low temperatures, the molding compound has already solidified in the gate system. In this way, a pouring gate is formed, i.e. a protrusion of the molded part, which does not form part of the desired geometry of the molded part and in an additional processing step, the protrusion must be separated from the produced molded part. In the injection mold or after the production of the molded part, the pouring gate can be removed manually or by machine with the aid of additional functional elements. Removing the pouring gate may leave marks or defects on the molded part, which shows the position where the pouring gate is arranged.
[0013] In addition, with a gate system without a hot runner, part of the molding compound injected into the injection mold remains in the gate system and does not flow to the molded part. The remaining part of the molding compound must be recycled or disposed of, and the shot volume is increased by the remaining gate because more molding compound must be plasticized than is present in the finished molded part. This leads to energy disadvantages and disadvantages with respect to the size of the injection molding machine.
[0014] In contrast, the molding compound in an injection mold with a hot runner remains free-flowing, and no curing of the molding compound occurs in the gating system, so that no gates remain on the molded part. In addition, hot runners enable longer flow paths in the injection mold, since any pressure drop due to cooling of the molding compound and the associated increase in viscosity is avoided.
[0015] The hot runner usually has a hot runner nozzle, which is arranged at the entrance to the cavity and constitutes a transition between a heated area and a non-heated area including the cavity in the injection mold. Therefore, the hot runner nozzle constitutes a boundary between liquid molding compound and solid molding compound.
[0016] The hot runner can be designed as an open system or a closed system. In a closed system, the injection point (i.e., the outlet of the hot runner nozzle) can be closed. For this purpose, the hot runner has an additional component as a closing element. The closing element is usually a needle valve, which can be positioned and moved by means of a discrete actuable mechanism operated pneumatically, hydraulically or electrically.
[0017] WO 2004 / 098759 A1 describes an injection molding device having a channel system including a static mixer. The static mixer has a plurality of passages and a mixing outlet, so that a homogenous flow of molding compound is generated.
[0018] CA2861399 is directed to an injection molding machine comprising a distributor plate and a nozzle extending through the distributor plate. The distributor plate and the nozzle are part of a hot runner arrangement.
[0019] WO2013 / 122789A1 discloses a mold system with a needle valve assembly, which can move a needle in an outlet of a nozzle. The wall of a melt channel in the nozzle has a protrusion for guiding the needle.
[0020] WO2011 / 156436A1 is directed to a mold system comprising a nozzle housing and a valve stem. When the valve stem is in the forward position, a groove structure around the valve stem is arranged in the nozzle tip. A guide for the valve stem is integrated into the nozzle tip, guiding the valve stem and providing a passage for the molding compound.
[0021] US 6,245,278 B1 describes an injection nozzle comprising a longitudinal channel and a large number of angled channels branching from the longitudinal channel. The vortex formed is believed to improve flushing and accelerate color changes with respect to the molding compound.
[0022] WO 2012 / 051079 A1 relates to a mold system with a nozzle tip, wherein the outer surface of the nozzle tip has a plurality of outlets so that the molten streams intersect each other along the outer surface. This reduces weld lines and improves the stress cracking resistance of the produced parts.
[0023] WO 2014 / 133702 A1 discloses a hot runner for an injection molding machine, comprising a conditioning zone, wherein a substantially homogenous thermal profile is generated in the processed melt. Wings or lamellae may be provided, for example, for guiding the needle.
[0024] WO01 / 34365A1 and US6,089,468 relate to melt flow mixers for injection molding machines. The flow channel of the needle for the guide has a spiral groove. The depth of the spiral groove decreases in the direction of the outlet zone, so that the resin flow flows spirally through the spiral groove and flows more and more axially through the bridge of the spiral groove in the direction of the outlet zone. This removes the weld line in the finished product. The spiral groove can also be designed as a double spiral groove, in which case the inner groove section is realized on the outer surface of a separate torpedo-shaped device or valve shaft.
[0025] WO 2009 / 055097 A1 and US Pat. No. 5,405,258 relate to hot runner nozzle systems including a torpedo-shaped device with improved replaceability and for improved temperature distribution. Nozzle housings including a filter screen are also described.
[0026] The subject matter of EP546554 also relates to an injection molding device having a hot runner nozzle comprising a torpedo-shaped device. The torpedo-shaped device is fixed to the hot runner nozzle by welding.
[0027] An object of the present invention is to provide an injection mold and a method for producing a marbled molded part, wherein the produced marble pattern varies in a repeatable and controlled manner while achieving a high degree of detail and reproducibility of the marble pattern. Furthermore, the same injection mold can be used for different patterns with little modification effort and high reproducibility.
[0028] This object is achieved by an injection mould for producing a marbled moulded part, the injection mould comprising at least one hot runner, a cavity, an access opening into the injection mould and an inlet into the cavity, wherein the hot runner has at least two channels, the at least two channels are connected to the inlet into the cavity at a first end of each channel and to the access opening into the injection mould at a second end of each channel, wherein the at least two channels each at least partially form a spiral portion and the at least two channels are defined by a single-piece component.
[0029] Additionally proposed is a method for producing marbled molded parts, wherein a first molding compound and at least one further molding compound are each added to an injection unit of a screw injection molding machine in a temporally and / or spatially separated manner and injected from the injection unit of the screw injection molding machine into an injection mold, wherein the injection mold comprises at least one hot runner, a cavity, an entry port into the injection mold and an inlet into the cavity, wherein the hot runner has at least two channels, which are connected to the inlet into the cavity at a first end of each channel and to the entry port into the injection mold at a second end of each channel.
[0030] In the method, preferably an injection unit is used, which comprises a barrel, a screw with a screw tip and a nozzle, wherein the screw is rotatable and arranged in the barrel so as to be movable in the direction of the longitudinal axis of the barrel between a front position and a rear position, the distance between the screw tip and the nozzle being smaller in the front position than in the rear position, and wherein the first molding compound comprises a first polymer compound and a first colorant, and the at least one further molding compound comprises a further polymer compound and optionally at least one further colorant. The method further preferably comprises the following steps:
[0031] a) optionally feeding a first amount of a first molding compound onto the screw when the screw is in the rear position,
[0032] b) optionally advancing the screw from a rear position into a front position,
[0033] c) feeding a second amount of at least one additional molding compound onto the screw,
[0034] d) plasticizing the first molding compound and the at least one further molding compound in the barrel of the screw, rotating the screw and conveying at least a portion of the first molding compound and at least a portion of the at least one further molding compound into the free space in the barrel between the nozzle and the screw tip, and moving the screw from a front position into a rear position,
[0035] e) optionally feeding a new first amount of a first molding compound onto the screw when the screw is in the rear position,
[0036] f) injecting the first molding compound and at least one further molding compound from the free space in the barrel (11) into the cavity of the injection mold, the screw advancing from a rear position to a front position,
[0037] g) cooling the first molding compound and the at least one further molding compound in the injection mold, thereby producing a marbled molding,
[0038] h) removing the marbled moulding from the injection mould,
[0039] wherein steps c) to h) are repeated, step e) is performed before step f) and step a) is optionally performed before step b), and wherein the feeding of a new first amount of the first molding compound in step e) and the optional feeding of a first amount of the first molding compound (1) in step a) are performed temporally and / or spatially separated from the feeding of a second amount of at least one further molding compound in step c).
[0040] Feeding the first molding compound and the at least one further molding compound separately in time and / or space limits the homogenization of the first molding compound and the at least one further molding compound during plasticization, so that in the produced molded part, defined color boundaries and a repeatable marble pattern are visible. The addition of the first molding compound and the at least one further molding compound can also be referred to as continuous or discrete. Thus, before injection into the free space between the nozzle and the screw tip, the first molding compound is distributed non-homogeneously in the at least one further molding compound.
[0041] Depending on the geometry of the at least two channels in the hot runner, a defined repeatable (ie reproducible) pattern is formed on at least one visible face of the produced marbled molding.
[0042] A repeatable marble pattern is understood to be a pattern in which, when different molded parts are produced by the same method and the same apparatus, the human eye does not perceive the differences as significantly different if they are compared with one another. The molded parts produced by the method of the invention or using the injection mold of the invention have a reliably repeatable and recognizable pattern. This is achieved in particular via the defined configuration of the feeding molding compound and the hot runner.
[0043] The marbled molding produced according to the invention can be used for decorative purposes in particular in the consumer goods industry. The marbled molding can be completely marbled or include at least one marbled visible surface. The marbled molding can be three-dimensional or flat. The marbled molding is preferably a household item (such as a dish, a plate, a cup, a cup holder, a handle or a toilet seat), a consumer product (such as a laptop shell or a protective shell for a phone or a smartphone), a toy (such as a turntable or a spinning top), an accessory for the fashion industry (such as a button) or a decorative element for the interior of a vehicle (such as a sun visor or a cover).
[0044] The first molding compound and at least one further molding compound are fed to the barrel of the injection unit and conveyed forward in the conveying direction towards the nozzle by the rotation of the screw of the injection molding machine. This at least partially (preferably completely) plasticizes the first molding compound and at least one further molding compound. The at least one further molding compound and optionally the first molding compound accumulate in the free space between the nozzle and the screw tip and move the screw axially backwards into the rear position of the barrel. Preferably, the screw injection molding machine comprises exactly one injection unit, more preferably exactly one barrel, further preferably exactly one screw.
[0045] Feeding can also be referred to as metering, the first molding compound or at least one further molding compound, for example, via a hopper into the barrel and in particular to the screw. The first molding compound and the at least one further molding compound are supplied in portions separated in time and / or space from one another. "In portions" means that the first molding compound and preferably also the at least one further molding compound are fed to the barrel non-continuously in the form of discrete portions (i.e. in the form of the first amount or the second amount).
[0046] Plasticization is also called dosing. The first molding compound and at least one further molding compound are conveyed by the screw in the direction of the nozzle and are at least partially melted in the process. Preferably, at least a portion of the first molding compound and at least a portion of the at least one further molding compound are completely melted during the plasticization in step d).
[0047] Feeding the second amount of at least one further moulding compound in step c) is preferably performed after advancing the screw in step b).
[0048] Further preferably, the feeding of the new first amount of the first molding compound in step e) and the optional feeding of the first amount of the first molding compound in step a) are completed before the advancement in step b) is started. In addition, the advancement in step b) is preferably completed before the feeding of the second amount of at least one further molding compound is started in step c).
[0049] The first molding compound is preferably first contacted with the screw and then with the at least one further molding compound.
[0050] The first moulding compound and / or the at least one further moulding compound can be fed separately and directly into the barrel and in particular directly onto the screw with the metering system.
[0051] Further preferably, feeding of the second amount of at least one further moulding compound is started when the screw is in the front position.The screw is preferably in the front position when the screw has been moved maximally in the direction of the nozzle.
[0052] The at least one further moulding compound (in particular the second amount of the at least one further moulding compound) may be fed continuously. Preferably, the second amount of the at least one further moulding compound is fed continuously at least during the plasticising in step d).
[0053] In particular, when the feeding of a new first amount of the first molding compound in step e) and optionally the first amount of the first molding compound in step a) and the second amount of at least one further molding compound in step c) are fed in a spatially separated manner, the second amount of at least one further molding compound can be fed continuously during the feeding of the new first amount of the first molding compound in step e) and optionally during the feeding of the first amount of the first molding compound in step a).
[0054] When the feeding of the new first quantity of the first molding compound in step e) and optionally the first quantity of the first molding compound in step a) and the second quantity of at least one further molding compound in step c) are fed in a spatially separated manner, the new first quantity of the first molding compound or the first quantity of the first molding compound is preferably fed at a greater distance from the nozzle than the second quantity of the at least one further molding compound.
[0055] After plasticizing, the rotation of the screw is preferably stopped and the screw is moved forward in the conveying direction to a front position so that the plasticized first molding compound and the plasticized at least one further molding compound are pushed through the nozzle into the cavity of the injection mold.
[0056] Feeding a new first amount of the first molding compound to the screw at the moment when the screw is in the rear position achieves a rhythm or timing synchronization of pattern formation and injection operation, thereby ensuring repeatability of the pattern in continuously produced marbled moldings. More preferably, the screw is stationary in the rear position when feeding the first amount of the first molding compound.
[0057] The volume of plasticized molding compound, which comprises at least one further molding compound and optionally the first molding compound, and which is present between the nozzle and the screw tip before injection into the free space, is also called the metering volume; subtracting the mass buffer (Massepolsters) from the volume of the plasticized molding compound gives the injection volume.
[0058] After the injection in step f), the barrel is filled again. A second amount of at least one further molding compound is fed, plasticization is again achieved, and the screw moves back to the rear position. Thereafter, a first amount of the first molding compound is fed, and injection is again achieved.
[0059] When the first amount of the first molding compound is fed in step a), the plasticization of the at least one further molding compound and optionally the first molding compound has preferably been completed at least once, more preferably at least twice, in particular at least four times. Preferably, when the first amount of the first molding compound is fed in step a), the at least one further molding compound and optionally the first molding compound are present in the barrel.
[0060] Preferably, the first molding compound and / or the at least one further molding compound are fed to the rear part of the barrel. The rear part is understood to mean preferably not more than 50% of the total length of the barrel, more preferably not more than 20% of the total length of the barrel at the end of the barrel remote from the nozzle of the screw injection molding machine. The first molding compound and the at least one further molding compound may be fed to the barrel at the same position or at different positions or at the feed port.
[0061] Depending on the product to be produced, the barrel has different inner diameters. The inner diameter is, for example, in the range of 10 mm to 150 mm, preferably in the range of 25 mm to 50 mm, for example 25 mm or 30 mm. The outlet of the barrel has, for example, a passage with a diameter of 1.5 mm to 10 mm, preferably a passage with a diameter of 3 mm to 6 mm, for example a passage with a diameter of 5 mm.
[0062] The first molding compound and the at least one further molding compound may be fed in the form of powder, granules or plastic chunks.The first molding compound and / or the at least one further molding compound may each be in the form of a homogeneous mixture and / or a heterogeneous mixture.
[0063] Preferably, the first molding compound and / or at least one further molding compound is fed in the form of granules. Granules generally refer to free-flowing solid materials, for example cylindrical or lens-shaped, and preferably have a maximum length of 1 mm to 10 mm, more preferably a maximum length of 3 mm to 6 mm.
[0064] The first molding compound preferably comprises a first granular material, the first granular material comprising a first polymer compound and a first colorant. The first granular material may also be referred to as a colored granular material, which is preferably produced in an upstream step prior to the method of the present invention. The first molding compound may also be referred to as a marble batch or fine material.
[0065] In particular, the at least one further molding compound may comprise a mixture before feeding, the mixture comprising at least two further particulate materials, in particular a second particulate material and a third particulate material. The at least one further polymer compound may be present in the second particulate material and the at least one further colorant may be present in the third particulate material.
[0066] Preferably, the marbled molding comprises a first molding compound and at least one further molding compound.
[0067] The screw of the injection molding machine preferably has a feed zone, a compression zone and a metering zone, which can also be referred to as an injection zone or homogenization zone.
[0068] The screw is preferably a single-blade screw. The screw has, in particular, exactly one passage in which the first molding compound and at least one further molding compound are conveyed. Further preferably, the screw of the screw injection molding machine has flat screw blades. The blade depth in the feed zone is preferably 0.05 to 0.15 times the outer diameter of the screw, and the blade depth in the metering zone is 0.025 to 0.075 times the outer diameter of the screw. The compression ratio refers to the ratio between the channel volume (Gang volumelumen) of the feed zone of the screw and the channel volume of the metering zone of the screw, preferably at least 2, more preferably greater than 2. Preferably, the screw has a length in the range of 20 to 23 times the outer diameter of the screw. Low screw blades have the advantage that less material is accommodated for the same diameter.
[0069] The screw of the screw injection molding machine may comprise a non-return valve, preferably the non-return valve is arranged between the screw tip and the screw blades.The screw tip may have protrusions, in particular 3 to 4 protrusions.
[0070] The injection unit of the injection molding machine preferably comprises a heating device. The heating device can completely surround the barrel, preferably partially surround the barrel. The nozzle of the screw injection molding machine can also comprise a heating device. The heating device helps to melt the first molding compound and at least one additional molding compound.
[0071] Preferably, cooling the first molding compound and the at least one further molding compound in the injection mold in step g) is performed simultaneously with plasticizing the first molding compound and the at least one further molding compound in step d), and optionally, cooling the first molding compound and the at least one further molding compound in the injection mold in step g) is performed at least partially simultaneously with feeding the second amount of the at least one further molding compound in step c).
[0072] Preferably, steps c) to h) are repeated more than once, more preferably more than three times, further preferably more than four times, especially preferably more than five times, thereby continuously producing a plurality of marbled moldings. Preferably, steps a) to f) are performed in the specified order.
[0073] Furthermore, the injection in step f) is preferably repeated at an injection frequency, and each injection or advance can be referred to as a shot. In addition, the feeding of the new first amount of the first molding compound in step e) is preferably repeated at a feeding frequency. The feeding frequency is preferably selected so that it deviates from the injection frequency by no more than 10%, further preferably by no more than 5%, particularly preferably by no more than 1%. Correspondingly, the feeding of the new first amount of the first molding compound in step e) is particularly preferably performed with the injection cycle in step f). In this case, the feeding of the new first amount of the first molding compound in step e) is preferably performed at a different time than the injection in step f). More preferably, the feeding frequency is equal to the injection frequency. In this case, the first amount of the first molding compound is always performed with the same time delay or time advance as the injection.
[0074] For marbled moldings, feeding a new first amount of the first molding compound in step e) and / or feeding a first amount of the first molding compound in step a) can be performed before or after feeding a second amount of at least one further molding compound in step c).
[0075] Like the first molding compound, at least two further molding compounds can also be supplied to the barrel, whereby multi-color molded parts additionally having a marble pattern can be produced. At least one further molding compound can be divided into a plurality of parts, in which case the plurality of parts are preferably each fed continuously or stepwise.
[0076] In addition, after the injection in step f), a holding pressure can be exerted on the molded part in the injection mold by the screw of the screw injection molding machine. Preferably, the holding pressure is applied before the plasticization in step d). When the holding pressure is applied to the molded part in the injection mold by the screw, the screw is preferably in the front position of the barrel or is still moving in the conveying direction, so that more plasticized molding compound is pushed into the mold and thus the material shrinkage is compensated during the cooling of the molded part in the mold.
[0077] Preferably, the second amount of at least one further moulding compound in step c) is fed when applying a holding pressure on the injection mould. More preferably, the second amount of at least one further moulding compound in step c) is fed when starting to apply a holding pressure.
[0078] Preferably, the ratio of the maximum internal free volume in the barrel that can be occupied by the first molding compound and the at least one further molding compound to the internal volume of the cavity is not more than 15, more preferably not more than 10, further preferably not more than 5, in particular from 2 to 5. The maximum internal free volume of the barrel can also be referred to as the melt channel of the injection molding machine.
[0079] Preferably, the internal free volume below the feed opening and in particular above the screw is only filled with the first molding compound and / or the at least one further molding compound or with particles of the first molding compound and / or particles of the at least one further molding compound by 0% to 80% by volume, more preferably by 10% to 50% by volume. This can also be referred to as underfeeding, in which the first molding compound and the at least one further molding compound are fed at a reduced mass flow rate compared to the maximum mass flow rate that can be conveyed by the screw.
[0080] Correspondingly, the barrel and screw of the screw injection molding machine are designed so that, especially before injection, there are preferably no more than 15 shots, more preferably no more than 10 shots, further preferably no more than 5 shots, especially 2 to 5 shots in the injection unit.
[0081] The low internal free volume of the barrel of the screw injection molding machine results in a short residence time of the first molding compound and the at least one further molding compound in the injection unit, which resists homogeneous mixing of the first molding compound with the at least one further molding compound, thereby promoting the production of the marble pattern. The residence time of the first molding compound and / or the at least one further molding compound in the barrel is preferably in the range of 1 second to 15 minutes, more preferably in the range of 0.1 minutes to 4 minutes, particularly preferably in the range of 0.5 minutes to 2 minutes.
[0082] Due to the method according to the invention, the first molding compound contacts the at least one further molding compound in the barrel as late as possible, thereby limiting the degree of mixing as much as possible. Due to the reduced residence time caused by the correspondingly small internal free volume of the barrel, mixing of the first molding compound with the at least one further molding compound is also reduced.
[0083] Preferably, the ratio of the sum of the mass of the first amount of the first molding compound and the mass of the second amount of at least one further molding compound to the mass of the marbled molding is 0.5 to 1.5, more preferably 0.8 to 1.2, further preferably 0.9 to 1, in particular 1. This ratio is, for example, greater than 1 when at least one pouring nozzle is present in the production of the marbled molding, which at least one pouring nozzle also includes the first molding compound as well as the further molding compound, but is removed from the marbled molding after production and is not part of the marbled molding. For example, a ratio of less than 1 can be present when inserts, in particular metal inserts, are integrated into the molding or when a two-component molding is produced which can have different hardnesses, wherein first the first component is injected into the cavity and then the second component is injected into the cavity, the first component and / or the second component having a marbled texture. Since the ratio is close to 1, the marbling (especially individual elements of the marbling pattern, such as rings or vertices) are positioned at similar positions in continuously produced marbled moldings, which means that the repeatability of the marbling on different marbled moldings is optimized, especially because the specific mass ratio is matched to the size of the molding and the rhythm of the injection. This avoids hiding different patterns from different injection operations.
[0084] Correspondingly, each shot is preferably added separately, the first molding compound for one shot and at least one further molding compound for the same shot being supplied spatially and / or locally separately in step e) and optionally in step a) or step c). The addition of the first molding compound and the at least one further molding compound is preferably effected in specific amounts, wherein the first amount and the second amount are each sufficient for exactly one shot.
[0085] Preferably, the mass ratio of the first amount to the second amount is less than 0.1, more preferably less than 0.01 and in particular less than 0.001. The first moulding compound is used to form a marble pattern in at least one further moulding compound constituting the base compound.
[0086] The ratio of a first concentration of the first colorant in the first molding compound to another concentration of the at least one further colorant in the at least one further molding compound is preferably greater than 20, more preferably greater than 50, in particular greater than 100. Correspondingly, preferably, the first colorant in the first molding compound has a higher concentration than the at least one further colorant optionally present in the at least one further molding compound. Before the at least one further molding compound is brought into contact with the first molding compound, the at least one further molding compound may have been colored by the at least one further colorant.
[0087] Preferably, the first molding compound comprises 10 to 60 wt.-% of the first colorant, more preferably 20 to 40 wt.-% of the first colorant, based on the first molding compound. The at least one further molding compound comprises preferably 0.1 to 6 wt.-% of at least one further colorant, more preferably 0.2 to 4 wt.-% of at least one further colorant, based on the at least one further molding compound.
[0088] By means of the concentration ratios mentioned, good recognizability and definition of the marble pattern is ensured, which contributes to the reproducibility of the pattern.
[0089] The second amount may comprise one or more further moulding compounds.The first polymer compound and / or the at least one further polymer compound are preferably thermoplastic moulding compounds. More preferably, the first polymer compound and / or at least one additional polymer compound comprises a polymer selected from the group consisting of polypropylene (PP), polyethylene (PE), polyoxymethylene (POM), polyethylene terephthalate (PET), polybutylenterephthalat (PBT), polyamide (PA), polycarbonate (PC), polyarylethersulfonen (PSU, PESU, PPSU), thermoplastic polyurethane (TPU), polybutylenadipatterephthalat (PBAT), polybutylene succinate (PBS), polylactide (PLA), polybutylensebacatterephthalat (PBSeT), polyethylene naphthalate (PEN), polymethyl methacrylate (PMMA), polystyrene (PS), styrene-containing polymers (such as acrylonitrile-butadiene-styrene copolymer (ABS) or mixtures thereof). At least one additional molding compound and optionally the first molding compound can be a filling or reinforcing molding compound. More particularly, at least one additional molding compound and optionally the first molding compound can include at least one filler such as talc, glass beads or fibers (such as glass fibers or carbon fibers).
[0090] More preferably, the polymer present in the first polymer compound is also present in at least one additional polymer compound. Further preferably, the first polymer compound and / or at least one additional polymer compound comprises PBT; more preferably, the first polymer compound and at least one additional polymer compound comprises PBT.
[0091] During the method, the first colorant and / or at least one additional colorant may be soluble or insoluble in the first molding compound and / or at least one additional molding compound. The first colorant and / or at least one additional colorant are preferably color pigments. The first colorant is preferably a black colorant. The first colorant preferably comprises industrial carbon black, which is also known as carbon black, or a diaminophenazine compound (such as aniline black). More preferably, the first colorant comprises carbon black or at least one diaminophenazine compound (such as aniline black). At least one additional colorant is preferably a blue colorant, a green colorant, a yellow colorant, a red colorant, a beige colorant, an orange colorant, a white colorant, a gray colorant, a brown colorant or a gold colorant.
[0092] If the barrel is supplied not only with the first molding compound but also with at least two further molding compounds, each further molding compound can comprise a further polymer compound and optionally at least one further colorant. The further molding compound can be added to the barrel together with the at least one further molding compound or the further molding compound can be added to the barrel before or after the at least one further molding compound, optionally directly before or directly after the at least one further molding compound. The at least two further molding compounds can also be fed in consecutively.
[0093] The viscosity of the first molding compound and / or the at least one further molding compound (each in plasticized form) is preferably in the range of 50 Pa·s to 1000 Pa·s. The injection rate of the plasticized molding compound from the nozzle of the screw injection molding machine into the mold is preferably greater than 25 cm 3 / s, more preferably from 50cm 3 / s to 100cm 3 / s, especially from 60cm 3 / s to 80cm 3 / s, for example 70cm 3 The dynamic pressure generally refers to the pressure of the free space in the barrel, and is preferably 1 bar to 100 bar, more preferably 10 bar to 70 bar, further preferably 20 bar to 50 bar.
[0094] The inlet to the injection mold is arranged on a side of the injection mold facing the outlet of the nozzle of the injection unit, so that the plasticized molding compound (especially the first molding compound and at least one additional molding compound) can be pushed from the nozzle of the injection unit into the mold through the inlet. The plasticized molding compound in the injection mold can be pushed from the inlet through at least two channels to the inlet and pushed into the cavity through the inlet. The plasticized molding compound is divided between the at least two channels downstream of the inlet in the conveying direction and recombined upstream of the inlet to the cavity.
[0095] More preferably, the injection mould has exactly one access opening for exactly one injection unit. The injection mould may comprise more than one cavity and one access opening to each cavity. If the injection mould has more than one access opening, the injection mould preferably has at least two channels per access opening or has an insert comprising at least two channels per access opening.
[0096] In the context of the present invention, in the injection mold, at least two channels are arranged in the same hot runner (especially in the same melt channel of the hot runner). If the hot runner system comprises a hot runner distributor with more than one melt channel, preferably there are at least two channels per melt channel of the hot runner for each hot runner nozzle. Within the scope of the present invention, the term "hot runner" refers to the same melt channel of the hot runner or the same section or arm of the hot runner system.
[0097] The at least two channels are preferably connected to the same inlet to the same cavity via a first end of each channel. Further preferably, the at least two channels are connected to an inlet to the injection mold and to the injection molding machine via a second end of each channel. Here, "connected" is understood to mean fluidly connected, and may also be referred to as "in communication".
[0098] The at least two channels are preferably separated from each other between their first end and their second end, in particular separated from each other by a one-piece component. The one-piece component is preferably a rigid component. More preferably, the at least two channels are completely separated from each other between their first end and their second end.
[0099] More specifically, each channel of at least two channels opens to the first end face in the hot runner through their first end separately, and opens to the second end face in the hot runner through their second end. The first end face is arranged to have a smaller distance from the respective entrance to the cavity compared to the second end face, and the second end face is arranged to have a smaller distance from the entrance to the injection mold compared to the first end face. Preferably, at least two channels in the conveying direction start at the second end face correspondingly and end at the first end face. The first end face and / or the second end face are preferably planes. In addition, the first end face and / or the second end face may have an element of a rotation locking device, such as a tongue-and-groove connector or a mating key. In addition, the plane of the first end face and the plane of the second end face preferably form an angle less than 30°, further preferably an angle less than 10° and especially an angle less than 5°, so that the first end face and the second end face are arranged to be substantially parallel to each other in the hot runner.
[0100] In addition, the first end face and / or the second end face is preferably arranged substantially perpendicular to the conveying direction or perpendicular to the longitudinal hot runner axis. "Substantially perpendicular" means an angle in the range of 45° to 135°, more preferably an angle in the range of 70° to 110°, in particular an angle in the range of 80° to 100°, for example 90°.
[0101] At least two channels are preferably arranged at a distance from the inlet (i.e., the tip of the hot runner nozzle) that is preferably 1.5 times the diameter of the hot runner nozzle at the inlet. If the hot runner nozzle diameter at the inlet is 8 mm, the distance is, for example, in the range of 10 mm to 15 mm.
[0102] A section of hot runner defined by a first end face and a second end face can also be considered as a channel section of the hot runner. Correspondingly, in the channel section of the hot runner, replacement of the plasticized molding compound does not occur between at least two channels. The plasticized molding compound comprising the first molding compound and optionally at least one other molding compound is divided and pushed through each of at least two channels in at least two discrete flows. More specifically, at least two channels do not have any passages and / or holes leading to each other between their first ends and their second ends. Correspondingly, mixing of at least two discrete flows does not occur between at least two channels. More specifically, at least two channels are used to reduce mixing of the overall flow of the plasticized molding compound. Therefore, the two discrete channels resist homogeneous mixing of the first molding compound with the other molding compound, so that repeatability is facilitated.
[0103] In the method of the present invention, at least two channels can each, in particular at least partially, form a spiral or extend on a curved path and / or extend straight. When at least two channels in the method pass straight through the hot runner, the at least two channels can also be referred to as straight holes. In this case, at least two channels preferably extend parallel to the longitudinal hot runner axis. It is also possible that at least two straight channels extend obliquely relative to the longitudinal hot runner axis. The inclination imposes a slight distortion on the plasticized molding compound.
[0104] In the injection mould of the invention, at least two channels each at least partially form a spiral.In the context of the present invention, a spiral is understood to mean a three-dimensional spiral which can also be referred to as a helix.
[0105] Due to the helical sections which are formed accordingly by the at least two channels, a distortion is exerted on the plasticized molding compound, which is reflected in the marble pattern of the molded part produced.
[0106] More specifically, at least two channels each have a central axis, wherein the central axis of the respective channel in the form of a spiral is arranged around the longitudinal hot runner axis. Further preferably, the central axes of at least two channels at each position are arranged at the same distance from each other, and further preferably, are arranged at the same distance from the longitudinal hot runner axis. Alternatively, the distance between the central axes of at least two channels can also vary and can increase or decrease in the conveying direction. In each case, the central axis extends through the center of the cross-sectional area of the respective channel.
[0107] The spiral portion can be rotated to the right or to the left in the conveying direction.
[0108] The spirals formed by at least one of the two channels each preferably have the same geometry, such as slope and number of turns, and are offset from each other by a radial angle relative to the longitudinal hot runner axis. The slope (especially the slope angle, for example with a constant slope and a constant diameter) is defined as follows:
[0109]
[0110] Wherein, α: slope angle, S: distance of a complete circle in the longitudinal hot runner axis direction, which can be called pitch height, and D: diameter of the spiral portion.
[0111] The helical portion preferably has a slope of less than 70° at at least one location.
[0112] The spiral portion (formed in each case by one of the at least two channels) can have a constant slope. The constant slope is preferably in the range of 5° to less than 60°, further preferably in the range of 10° to 40°, particularly preferably in the range of 15° to 30°. For example, the constant slope is 20°.
[0113] Preferably, the spiral has a different slope at each of the at least two different positions. Preferably, at least two different positions on the spiral have different distances from the entrance to the cavity. Preferably, a first slope of the spiral at a first position differs from a second slope of the spiral at a second position by at least 20°; preferably, the difference (especially the maximum difference) between the first slope and the second slope is greater than 30° and less than 90°, for example 60°.
[0114] Preferably, the slope of the spiral portion decreases in the direction from the entry opening to the inlet. For example, such as in the conveying direction of the plasticized molding compound, the slope of the spiral portion can change from more than 70° in a first position (e.g. at the second end face, respectively close to the entry opening) to less than 30° in a second position at the first end face (close to the cavity). The change (especially continuous change) from a high slope to a gentle slope in the conveying direction of the plasticized molding compound can achieve good entry in terms of flow while applying a significant distortion at the outlet of at least two channels.
[0115] Preferably, the helix has a number of turns, which may also be referred to as turns, and the number of turns is further preferably in the range of greater than 0.25 to 5. Correspondingly, the helix preferably covers a rotation angle of greater than 90° to 180°. Further preferably, the number of turns is in the range of greater than 0.25 to 3, in particular in the range of greater than 0.50 to 3, for example in the range of 0.51 to 2.
[0116] The hot runner (preferably for each melt channel) preferably has two to eight, more preferably three to eight, further preferably three to six, such as three, four or six channels, which may also be referred to as holes, passages or holes.
[0117] The shape, number and arrangement of the at least two channels affect the geometry of the marble pattern produced. The at least two channels have different cross-sectional geometries and / or different cross-sectional dimensions. For each hot runner, the at least two channels preferably have the same cross-sectional geometry and the same cross-sectional dimensions.
[0118] When the at least two channels each at least partially form a helix, the at least two channels can each be designed, for example, as a screw blade or as a twisted bore, which can also be referred to as a curved bore.
[0119] If at least two channels are designed as screw blades, a portion of a single-piece component that separates the at least two channels from each other may form a plurality of blades. More preferably, the number of blades is equal to the number of at least two channels, in which case the at least two channels are separated from each other in cross section by a bridge. The design of each of the at least two channels (such as screw blades) may also be described as being such that a multi-blade bridge (preferably rotating in a radial direction along a central longitudinal hot runner axis) is arranged in a flow channel hole of a cylinder. Further preferably, at least two channels are defined by two coaxially arranged cylinders, each of which is part of a corresponding outer face. More preferably, at least two channels are defined by the same two coaxially arranged cylinders.
[0120] Preferably, at least two channels each have a circular, elliptical, segment-shaped or polygonal (such as, hexagonal or triangular) cross section on the radial cross section of the hot runner. The triangular cross section may have at least one curved sideline. A triangular cross section or segment-shaped cross section with at least one curved sideline preferably exists when at least two channels are each designed as a spiral blade. The annular segment preferably covers an angle in the range of 100° to 180°. Specifically, when the number of at least two channels is at least four, the angle of the annular segment may be less than 100°. If the channel has a triangular cross section and the intermediate wall between at least two channels is designed as a spiral blade, this can also be described as making the hot runner have a cylindrical central melt channel hole, in which a main shaft corresponding to a blade is arranged, and the blade separates at least two channels from each other. If at least two channels are each designed as a twisted hole, at least two channels each preferably have a circular, elliptical or polygonal (such as, hexagonal) cross section.
[0121] The cross-sectional area of the channel portion of the hot runner (arranged with at least two channels) preferably has an opening ratio The porosity is the ratio of the area available for flow to the total area and is 40% to 80%, further preferably 50% to 75%. The calculation of the porosity is preferably based on the cross-sectional area (especially the circular cross-sectional area), and the radius corresponds to the maximum distance of the wall of at least two channels from the central longitudinal axis of the hot runner. For example, in the case of two channels, the porosity can be 68%, each channel forming a spiral with a slope varying from 90° to 30° with spiral blades, and in the case of three channels, the porosity can be 51%, each channel forming a spiral with a slope varying from 90° to 30° with spiral blades. Preferably, the flow area of the first end face and the second end face that flow into or out of at least two channels has substantially the same size. Correspondingly, in each case based on the inlet area, the inlet area and the outlet area of at least two channels preferably differ from each other by less than 30%, more preferably less than 10%, and particularly preferably less than 5%. This involves the sum of the individual channels of the at least two channels and the inlet area or outlet area of the at least two channels.
[0122] The hot runner (especially the channel portion of the hot runner) can be in a single-piece form or in a multi-piece form. In a multi-piece embodiment, the single-piece component forms the direct boundary of at least two channels. The single-piece component can be formed by a part or a section of the hot runner; more specifically, the channel section of the hot runner or a part of the channel section can be realized in a single-piece form and can be a single-piece component. Alternatively, the insert can be accommodated in the channel section as a single-piece component. In addition, at least two channels can be arranged, for example, directly arranged in a single-piece hot runner nozzle cap (also referred to as a screw-in part).
[0123] Specifically, the outer surfaces of at least two channels (preferably all outer surfaces) are preferably completely closed and defined by a single-piece component. In the cross section of the at least two channels, the first end face and the second end face are not affected by the material from the single-piece component, so that the plasticized molding compound can pass through the first end face and the second end face.
[0124] A one-piece component, in particular an insert, can be part of a hot runner. More particularly, "one-piece" means that the one-piece component is produced from a continuous material, in particular without any connections (e.g., welds and / or welding seams). For example, the walls of at least two channels (in particular, when they are designed as blades) can be molded on the hollow cylindrical basic shape of the insert, or on a centrally positioned solid cylindrical part of the insert. Continuous material is understood to mean a material with a homogeneous composition throughout the one-piece component. The one-piece component is in particular not composed of multiple layers or multiple components, and / or does not have a coating made of other materials.
[0125] The use of one-piece components, in particular produced by additive methods, enables the production of the injection mold to be simplified.
[0126] The hot runner preferably comprises an insert as a single-piece component, which preferably has a cylindrical outer contour. More specifically, at least two channels are arranged in the insert. Correspondingly, the hot runner can use different inserts, each of which has channels of different geometries, which allows a high degree of flexibility in designing the marble pattern with only one injection mold. By using inserts, different marble patterns can be quickly produced one after the other using the same injection mold. Different inserts can be replaced in the hot runner as required. The insert is preferably designed to precisely match a preferably central cylindrical hole in the hot runner, in particular the melt channel, which forms the actual flow channel outside the insert.
[0127] The length-diameter ratio of the insert is preferably from 4: 1 to 1: 1, for example 2: 1, and the length-diameter ratio of the at least two channels is preferably from 20: 1 to 2: 1, more preferably from 10: 1 to 8: 1. The wall thickness between the at least two channels (especially the thickness of the blades or the thickness of the bridge) is preferably 10% to 30%, preferably 15% to 20%, based on the diameter of one of the at least two channels.
[0128] In addition to the insert, the hot runner may also have one, two or more disks, which are used to position and / or fix the insert in the hot runner. Particularly preferably, the insert is arranged between two disks. The disk preferably has a central hole.
[0129] Furthermore, a method for producing an injection mold according to the invention is proposed, wherein at least a portion of the hot runner (preferably a single-piece component, in particular at least an insert) is produced using an additive method (in particular using 3D printing). The production of at least two channels using an additive method enables the production of more complex (in particular more complex spiral) channels. Furthermore, similar to the cast component, this mode of production produces a surface roughness that has a positive influence on the marble pattern. Preferably, the layers produced by the additive method have a layer height of 0.08 mm to 0.2 mm, for example a layer height of 0.1 mm.
[0130] Furthermore, the production of a one-piece component, in particular an insert, by an additive method enables the production of undercuts, thereby achieving a larger flow area of at least two channels. In the context of the present invention, undercuts are understood to mean that the diameter of the insert melt channel increases in the conveying direction. More specifically, the centrally arranged insert melt channel (arranged at the second end face) can have an increasing diameter in the conveying direction.
[0131] The additive method can also produce channels, wherein at least two channels have an undercut and in particular each channel has a turn greater than 0.5. Undercuts of at least two channels are particularly understood to mean that the cross-sections of the channels do not overlap on the axial projection at the first end face and the second end face.
[0132] Laser welding methods or melt layering methods such as fused deposition modeling (FDM) or fused filament production (FFF) can be used as additive methods. To produce a single-piece component (particularly an insert), a metal injection molding feedstock (MIM feedstock) (e.g. ) as material. The MIM feedstock includes different types of steel, such as stainless steel or tool steel, so that the produced single-piece components (particularly inserts) can be specifically matched to the final use.
[0133] Preferably, the single-piece component and / or at least the insert is produced from a metal-containing powder. More preferably, the single-piece component and / or at least the insert is produced from a composition, the components of which include: 30% to 70% by weight, more preferably 40% to 60% by weight of at least one inorganic powder; 30% to 70% by weight, more preferably 40% to 60% by weight of at least one binder. The particle size of at least one inorganic powder is preferably from 0.5 μm to 50 μm, more preferably from 0.1 μm to 30 μm. In addition, at least one inorganic powder preferably includes a precursor compound of a metal, a metal alloy, a ceramic material, and a mixture thereof. More preferably, at least one inorganic powder preferably includes a precursor compound of a metal, a metal alloy, a ceramic material, or a mixture thereof. At least one binder preferably includes a polymer composition (particularly, POM). More preferably, at least one binder includes POM. The composition can be used in the form of particles or filaments.
[0134] The hot runner (including the hot runner distributor) is heated to a temperature at which the molding compound can be plastically processed, ie above the melting temperature of the molding compound. Typically, a closed-loop control with permanent temperature measurement is used.
[0135] In particular, the hot runner has a hot runner nozzle arranged at the inlet into the respective cavity. The temperature of the hot runner nozzle is preferably in the range of 150° C. to 450° C., more preferably in the range of 180° C. to 400° C. The first molding compound and the at least one further molding compound at the inlet into the cavity preferably have a temperature in the range of 150° C. to 450° C., more preferably in the range of 180° C. to 400° C. The injection pressure or holding pressure in the cavity is preferably 400 bar to 2000 bar. The hot runner nozzle preferably comprises a particularly heat-conducting material.
[0136] Hot runner nozzles can be configured as needle valve nozzles, open nozzles with torpedo-shaped devices, open nozzles with straight passages, or open nozzles with tips that may include multiple inlets into the cavity. Since the hot runner is heated to a temperature higher than the temperature of the rest of the injection mold, heat is constantly removed from the hot runner. Although heat is removed, in an open hot runner nozzle, the torpedo-shaped device is used to maintain the free-flowing molding compound to a uniform temperature. The torpedo-shaped device is usually in direct thermal contact with the heated portion of the hot runner nozzle.
[0137] The needle valve nozzle comprises a receiving and driving device for a closing element, in particular a needle, which is guided, for example, by a guide bushing and connected to the nozzle body of the hot runner nozzle by two brackets. The closing element serves to open and close the hot runner nozzle. The hot runner, more preferably a single-piece component and in particular an insert, preferably has a central hole along the longitudinal hot runner axis for the passage of the closing element. If the single-piece component, in particular the insert, has a central hole in addition to the at least two channels, the single-piece component or the insert can be used in combination with the needle valve nozzle.
[0138] In particular, the needle is guided through the insert, thereby subsequently closing the hot runner nozzle at the inlet into the cavity.The insert or the central hole is used to guide the needle, through which the needle moves relative to the insert and the at least two channels.
[0139] A hot runner with at least two channels can be used in combination with an open nozzle. If an open nozzle is present, the hot runner, preferably a one-piece component, in particular an insert, can have a central solid cylinder, which is arranged between the at least two channels, in particular instead of a central hole in a needle valve nozzle. In addition to the at least two channels, the hot runner can also have a torpedo-shaped device, which can be arranged downstream of the at least two channels in the conveying direction.
[0140] At least two channels (specifically with inserts) may be arranged in the hot runner nozzle of the hot runner, in the distributor of the hot runner and / or adjacent to or directly in the inlet into the injection mold leading to the hot runner. More preferably, the hot runner nozzle has a hot runner nozzle head, which is also referred to as a nozzle cap or a screw-in part, and at least two channels are preferably arranged in the nozzle head. The hot runner nozzle head may include an insert, which includes at least two channels. In addition, the hot runner nozzle can be connected to other components of the hot runner by means of a screw connection. The screw connection means that the hot runner nozzle can be replaced with a wear part, and the screw connection means that the insert can be fixed in the hot runner.
[0141] The arrangement of at least two channels in an injection mold, in particular in a hot runner nozzle, offers the advantage that the at least two channels are arranged as close to the cavity as possible, so that distortions exerted on the molding compound are transferred more directly to the molded part and the separation of the different melt portions is maintained for as long as possible.
[0142] Any type of hot runner nozzle can be used to carry out the method according to the invention for producing a reproducible marbled moulding. Depending on the configuration of the hot runner nozzle (in particular, an open nozzle or a needle valve nozzle with different supports for the needles), different marble patterns can be produced in the moulding. The use of needle valve nozzles has produced very pronounced marble patterns. The specific form of the marble pattern is influenced by the geometry of the support for the needles, which the insert can form.
[0143] In the case of using an open nozzle without at least two channels, a circular uniform distribution of color is visible. The optical effect produced by using only an open nozzle can be described as concentric circles. If at least two (e.g., three, four or six) channels are used, the circular structure is destroyed and a slight turbulence of the first molding compound in at least one further molding compound is visible. The number of stripes corresponding to the number of channels that produce the flow lines is visible.
[0144] By designing at least two channels each in the form of twisted holes, the eddy flow of the first molding compound in the at least one further molding compound is intensified.If at least two channels are each designed in the form of screw blades, the wave portions in the form of stripes are formed as a marble pattern with very good reproducibility.
[0145] Embodiments of the invention are shown in the accompanying drawings and are described in more detail in the following description. The invention is not limited to the exemplary embodiments described herein and the aspects emphasized herein. On the contrary, within the scope described in the claims, there are many possible modifications within the capabilities of those skilled in the art.
[0146] The accompanying drawings show:
[0147] Figure 1 shows a first schematic diagram of an injection molding machine having an injection mold,
[0148] Figure 2 A second schematic diagram of a screw injection molding machine with an injection mold is shown,
[0149] Figure 3 shows a cross section of a screw injection molding machine,
[0150] Figure 4 , Figure 6 and Figure 8 Each shows the details of the hot runner,
[0151] Figure 5 , Figure 7 and Fig. 9 Each shows the Figure 4 , Figure 6 and Figure 8 Detailed cross section of the hot runner,
[0152] Figures 10 to 21 each showing a top view or a perspective view of a plurality of embodiments of at least two channels,
[0153] Figure 22 to Figure 27 a top view, a perspective view or a longitudinal section of two further embodiments, each showing at least two channels, and
[0154] Fig.28 An insert with an undercut is shown.
[0155] Figure 1 A schematic diagram of a screw injection molding machine 7 including an injection unit 5 is shown. The injection unit 5 comprises: a barrel 11 having an internal free volume 31; a screw 13 having a screw tip 15; and a nozzle 17 having a nozzle head 37 and a nozzle body 39. The screw 13 is rotatable and is mounted in the direction of the longitudinal axis 19 of the barrel 11. The screw is in a rear position 23 in the barrel 11, with a distance 25 between the nozzle 17 and the screw tip 15, so that there is a free space 27 in the barrel 11 between the nozzle and the screw tip 15.
[0156] A nozzle 17 with an outlet 40 is adjacent to an injection mold 9 with a hot runner 4 and two cavities 29. The injection mold 9 is shown in an enlarged form. The cavity 29 has an internal volume and is only indicated here. In addition, the injection mold 9 has an entry port 8 leading into the injection mold 9 and two inlets 6 leading into the cavities 29. A hot runner 4 with a hot runner distributor 33 (as a gate) is arranged between the outlet 8 and the inlet 6, and the hot runner distributor 33 can also be called a distributor latch. A melt channel 74 leads from the hot runner distributor 33 to each cavity 29, and each of the two melt channels 74 of the hot runner 4 has an insert 42 with a channel 41, and the melt channel 74 is divided into the channels 41 in the insert 42.
[0157] In the screw injection molding machine 7, the screw 13 has a metering zone 47, a compression zone 49 and a feeding zone 51. The screw 13 can be used to convey the molding compound into the free space 27 in a conveying direction 52. The free space 27 is a part of the interior 35 of the barrel 11, which is bounded by the barrel 11 and the screw 13.
[0158] Figure 2A schematic diagram of a screw injection molding machine 7 with an injection mold 9 is shown, which corresponds essentially to Figure 1 However, according to Figure 2 , the screw 13 is in the front position 21 in the barrel 11. Figure 1 In comparison, due to the advancement of the screw 13, the distance 25 has been reduced.
[0159] Figure 3 Shown according to Figure 1 1 . A section of a feed zone 51 of a screw 13 present in a barrel 11 is shown. The screw 13 is movable along the longitudinal axis 19 of the barrel 11 and is in a rear position 23. A part of the screw 13 is located below a feed opening 53. In the embodiment shown, a first molding compound 1 as well as a further molding compound 3 are fed to the screw 13 through the feed opening 53. The feed opening 53 has a first area 55 for feeding the first molding compound 1 and has a second area 57 for feeding the further molding compound 3. Due to the cover 59, there is a second distance 61 between the first area 55 and the second area 57, by means of which the first molding compound 1 and the further molding compound 3 are fed spatially separated.
[0160] Figure 4 A hot runner nozzle 76 of a hot runner 4 is shown with a hot runner nozzle cap 77. The insert 42 is arranged in the hot runner nozzle cap 77 as a single-piece component 46. A needle 73 is guided through the insert 42 and is movable along the longitudinal hot runner axis 69 and can close the inlet 6 into the cavity 29.
[0161] Figure 5 Shown according to Figure 4 4 shows a cross-sectional view of an insert 42. The insert 42 has a central hole 71 through which a needle 73 is guided. In addition, the insert 42 has a channel 41 in the form of a straight hole and with a circular cross section 63. The channel 41 is a through-hole extending parallel to the longitudinal hot runner axis 69.
[0162] Figure 6 and Figure 7 as well as Figure 8 and Fig. 9 Basically corresponds to Figure 4 and 5 , except that the insert 42 has a different configuration.
[0163] according to Figure 6 and Figure 7 , the insert 42 does not have a central hole 71, since the hot runner nozzle 76 is designed as an open nozzle without a needle 73. The same applies to Figure 8 and Fig. 9 A portion of the hot runner 4.
[0164] according to Figure 6 and Figure 7 The insert 42 of the open hot runner nozzle 76 has three straight channels 41 with a central axis 67 that is arranged parallel to the longitudinal hot runner axis 69 .
[0165] exist Figure 8 and Fig. 9 In FIG. 1 , a hot runner nozzle 76 in the form of an open nozzle is also shown. Figure 8 and Fig. 9 The insert 42 comprises three channels 41, wherein each channel 41 at least partially forms a spiral portion 75 having a greater slope in the first position 44 than in the second position 48. Each channel 41 has a first end 43 and a second end 45, wherein the first end 43 is arranged adjacent to the inlet 6. Each channel 41 has a cross section 63 that is oval or circular.
[0166] Figures 10 to 21 Six additional embodiments of the insert 42 are shown, each of which is shown in a top view or a perspective view. Figures 10 to 21 In the embodiment, the channels 41 each form a spiral 75 , wherein the central axis 67 of each channel 41 is each arranged in the form of a spiral 75 around the longitudinal hot runner axis 69 and has a specific number of turns 50 .
[0167] according to Fig.10 and Fig.11 , the insert 42 has three channels 41 and a central hole 71 for the guide needle. The slope of the spiral portion 75 decreases in the conveying direction 52 (i.e., in the direction from the entry port 8 to the inlet 6 of the injection mold 9 and in the direction from the second end 45 of each channel 41 to the first end 43). There is a greater slope in the first position 44 than in the second position 48. The slope changes from about 90° to a relatively gentle slope of about 30°. This leads to favorable entry in terms of flow and significant distortion, which is applied to the plasticized molding compound at the outlet (i.e., at the first end 43 of each channel 41). Along the longitudinal hot runner axis 69, there is a constant free cross-section 63, thereby a constant aperture ratio. The spiral portions 75 each have a half turn 50, so that the bridge 65 between the two channels 41 is rotated 180° compared to the first end 43 and the second end 45.
[0168] according to Fig.12 and Fig.13 The insert 42 corresponds to the Fig.10 and Fig.11The difference is that this is an insert 42 for an open nozzle, since the channels 41 are separated from each other on the longitudinal hot runner axis 69 by a solid cylinder 79 .
[0169] according to Fig.14 and Fig.15 The insert 42 corresponds to the Fig.12 and Fig.13 of the insert 42 , except that there are only two channels 41 .
[0170] according to Fig.16 and Fig.17 The insert 42 corresponds substantially to Fig.14 and Fig.15 Insert 42 of FIG. 1 except that helical portions 75 have a constant slope and each helical portion 75 has only about one third of a complete turn 50 so that bridge portion 65 is rotated about 120° toward second end 45 compared to first end 43. The slope is about 60°.
[0171] according to Fig.18 and Fig.19 The insert 42 corresponds substantially to Fig.16 and Fig.17 The insert 42 has 1.5 turns 50 except for the helical portion 75, so that there is a slope of about 20°.
[0172] according to Fig. 20 and Fig.21 The insert 42 is similar to that according to Fig.12 and Fig.13 There are three channels 41, each in the form of a spiral 75 having a greater slope in the first position 44 than in the second position 48. Fig. 20 and Fig.21 The channels 41 of the insert 42 each partially form a spiral portion 75, and the first end 43 of the channel 41 opens to the first end face 83. Another part of the channel 41 is straight and opens to the second end face 81 via the second end 45. In addition, the channel 41 has a hexagonal cross section 63.
[0173] Fig. 22 , Fig.23 and Fig.24 The insert 42 shown in plan view, perspective view and longitudinal section in the figure corresponds essentially to the insert 42 according to Fig.25 , Fig.26 and Fig. 27 The insert 42 has, except for the channel 41, a constant elliptical cross section 63. Since the constant cross section 63 is elliptical, a higher open porosity is achieved in the cross section 63 compared to a partially circular cross section 63.
[0174] according to Fig.25 , Fig.26 and Fig. 27 The insert 42 corresponds to the Figure 6 and Figure 7 The insert 42 corresponds substantially to Fig. 22 , Fig.23 and Fig.24 The insert 42 has a variable cross section 63 except that the channel 41 has a circular cross section 63 at the second end 45 and also along the straight portion of the channel 41. In the spiral portion 75, the cross section 63 changes from a circular shape to a flattened elliptical shape because the slope of the central axis 67 of the channel 41 increases relative to the longitudinal hot runner axis 69.
[0175] Fig.28 An insert 42 is shown with an undercut 91. The insert 42 includes three channels 41, each of which forms a spiral 75 with a variable slope. In the insert 42, an insert melt channel 85 terminates at a second end face 81 of the channel 41 in the conveying direction 52. The insert melt channel 85 has an undercut 91, so that a first diameter 87 of the insert melt channel 85 is smaller than a second diameter 89 of the insert melt channel 85 at the second end face 81. Correspondingly, the diameters 87, 89 of the insert melt channel 85 increase in the conveying direction 52. Example
[0176] Production of cup holders
[0177] For the production of the cup holder, a hydraulic injection molding machine with a clamping force of 1000 kN was used, which comprises a barrel with an inner diameter of 25 mm and an injection mold with two cavities and a hot runner system.
[0178] For both cup holders, i.e. for each injection operation, also referred to as cycle or shot, a first quantity of a first molding compound is provided in each case. The first molding compound comprises black particles in the form of cylindrical particles, each having a diameter of 1 mm and a length of 2 mm, comprising a black colorant and having a concentration of 20% by weight in PBT. The first quantity has a mass of 0.03 g, corresponding to 5 particles.
[0179] In addition, a second amount of additional molding compound is provided for each of the two cup holders. The second amount has a mass of 40 g. The additional molding compound includes 39.77 g of uncolored PBT granular material and 0.23 g of colored PBT granular material per second amount, wherein the colored PBT granular material includes an additional colorant in concentrated form. The additional molding compound is in the form of a granular mixture, and the uncolored PBT granules and the colored PBT granules are premixed in the additional molding compound.
[0180] In each cycle, a first quantity of the first molding compound is introduced onto the screw in the rear position. The screw is then moved to the front position towards the nozzle for injection. For adding the molding compound, a metering device with two hoppers mounted on a cylindrical feed opening is used. The hopper for the first molding compound opens via a tube close to the screw blades in the hollow barrel. This ensures the desired placement of the first quantity.
[0181] The plasticized molding compound is injected into a cooled injection mold comprising a hot runner system and two cavities, each having a melt channel with a hot runner nozzle, so that two marbled molded parts are produced in parallel in each cycle. The hot runner keeps the plasticized molding compound in a liquid state before it reaches the cavity (i.e., before molding). The hot runner nozzle used in each case is a hydraulically operated needle valve nozzle.
[0182] Each melt channel of the hot runner comprises an exchangeable insert, each having a central hole for a guide needle. In addition, the inserts each contain at least two channels in which the flows of the plasticized molding compound are separated and then combined again in the melt channel upstream of the outlet of the hot runner nozzle. Using inserts with three or four channels makes it possible to obtain cup holders with a pattern comprising a three-fold or four-fold repeat. An insert with three channels is arranged upstream of one of the two hot runner nozzles, and an insert with four channels is arranged upstream of the other of the two hot runner nozzles. It is thus possible to produce two cup holders of the same color with respectively different reproducible marble patterns in only one injection mold in a single cycle.
[0183] One of the inserts used had a geometry according to Table 1, and the channels were in each case Fig.10 and Fig.11 The form of the screw blades shown.
[0184] Table 1
[0185]
[0186] 20 coasters were produced in 10 consecutive cycles, thus repeating the process several times. A good reproducibility of the obtained marble pattern was found.
[0187] Reference Number List
[0188] 1 First Molding Compound
[0189] 3 At least one additional molding compound
[0190] 4 Hot runner
[0191] 5 Injection unit
[0192] 6 Entrance
[0193] 7 Screw injection molding machine
[0194] 8 Entrance
[0195] 9Injection mold
[0196] 11 Barrel
[0197] 13 Screw
[0198] 15 Screw tip
[0199] 17 Nozzle
[0200] 19 Longitudinal axis of barrel
[0201] 21 front position
[0202] 23 Rear position
[0203] 25 Distance
[0204] 27 Freespace
[0205] 29 chambers
[0206] 31 Internal free volume
[0207] 33 Hot runner distributor
[0208] 35 Internal
[0209] 37 Nozzle Tip
[0210] 39 Nozzle body
[0211] 40 Exit
[0212] 41 channels
[0213] 42 Inserts
[0214] 43 First end
[0215] 44 First Position
[0216] 45 Second end
[0217] 46 Single Components
[0218] 47 Metering Area
[0219] 48 Second position
[0220] 49 Compression Zone
[0221] 50 laps
[0222] 51 Feeding Area
[0223] 52 Transmission direction
[0224] 53 Feeding port
[0225] 55 First Area
[0226] 57 Second Area
[0227] 59 Cover
[0228] 61 Second Distance
[0229] 63 Cross section
[0230] 65 Bridge
[0231] 67 Central Axis
[0232] 69 Longitudinal hot runner axis
[0233] 71 Center hole
[0234] 73 pins
[0235] 74 Melt channel
[0236] 75 Spiral
[0237] 76 Hot runner nozzle
[0238] 77 Hot runner nozzle cap
[0239] 79 Solid Cylinder
[0240] 81 Second end surface
[0241] 83 First end surface
[0242] 85 Insert melt channel
[0243] 87 First diameter
[0244] 89 Second diameter
[0245] 91 Undercut
Claims
1. An injection mold (9) for producing a marble-textured molded part, comprising: at least one hot runner (4), a cavity (29), an inlet (8) leading to the injection mold (9), and an inlet (6) leading to the cavity (29), wherein the hot runner (4) has at least two channels (41), the at least two channels are connected to the inlet (6) leading to the cavity (29) at a first end (43) of each channel (41) and are connected to the inlet (8) leading to the injection mold (9) at a second end (45) of each channel (41), wherein the at least two channels (41) are each at least partially The at least two channels (41) are delimited by a single-piece component (46), wherein the at least two channels (41) are separated from each other by the single-piece component (46) between their first end (43) and their second end (45), wherein the at least two channels (41) each have a central axis (67), and the central axis (67) is arranged around the longitudinal hot runner axis (69) in the form of a spiral (75), and the spiral (75) has a different slope at each of at least two different positions; The spiral portion (75) has a plurality of turns (50), and the number of the turns (50) is in the range of greater than 0.5 to 3; wherein the spiral portion (75) has a slope of less than 60° at at least one position.
2. The injection mold (9) according to claim 1, characterized in that The hot runner (4) has three to eight channels (41).
3. The injection mold (9) according to claim 1, characterized in that A first slope of the helical portion (75) at the first position (44) differs from a second slope of the helical portion (75) at the second position (48) by at least 20°.
4. The injection mold (9) according to claim 1, characterized in that The slope of the spiral portion (75) decreases in the direction from the inlet opening (8) to the inlet (6).
5. The injection mold (9) according to claim 1, characterized in that The hot runner (4) has a central hole (71) along the longitudinal hot runner axis (69).
6. The injection mold (9) according to claim 1, characterized in that The hot runner (4) has a closing element along the longitudinal hot runner axis (69).
7. The injection mold (9) according to claim 6, characterized in that The closing element is a needle (73).
8. The injection mold (9) according to claim 1, characterized in that The at least two channels (41) each have a circular, elliptical, ring segment-shaped or polygonal cross section (63) in a radial cross section of the hot runner (4).
9. The injection mold (9) according to claim 8, characterized in that The polygonal cross section (63) is a hexagon or a triangle.
10. The injection mold (9) according to claim 1, characterized in that The one-piece component (46) is an insert (42) arranged in the hot runner (4), and the at least two channels (41) are arranged in the insert (42).
11. A method for producing an injection mold (9), characterized in that The injection mold (9) is used to produce a marble-textured molded part, comprising: at least one hot runner (4), a cavity (29), an inlet (8) leading to the injection mold (9), and an inlet (6) leading to the cavity (29), wherein the hot runner (4) has at least two channels (41), the at least two channels are connected to the inlet (6) leading to the cavity (29) at a first end (43) of each channel (41) and are connected to the inlet (8) leading to the injection mold (9) at a second end (45) of each channel (41), wherein the at least two channels are connected to the inlet (6) leading to the cavity (29) at a first end (43) of each channel (41) and are connected to the inlet (8) leading to the injection mold (9) at a second end (45) of each channel (41). The two channels (41) each at least partially form a spiral portion (75), and the at least two channels (41) are delimited by a single-piece component (46), wherein the at least two channels (41) are separated from each other by the single-piece component (46) between their first end (43) and their second end (45), wherein at least the single-piece component (46) is produced by an additive method; wherein the spiral portion (75) has a plurality of turns (50), and the number of turns (50) is in the range of greater than 0.5 to 3; wherein the spiral portion (75) has a slope of less than 60° at at least one position.
12. The method according to claim 11, characterized in that The one-piece component (46) is an insert (42) arranged in the hot runner (4), and the at least two channels (41) are arranged in the insert (42).
13. The method according to claim 11 or 12, characterized in that: The additive method is 3D printing.
14. A method for producing a marbled molded part, wherein a first molding compound (1) and at least one further molding compound (3) are each added temporally and / or spatially separately to an injection unit (5) of a screw injection molding machine (7) and injected from the injection unit (5) of the screw injection molding machine (7) into an injection mold (9), wherein the injection mold (9) comprises at least one hot runner (4), a cavity (29), an inlet opening (8) into the injection mold (9) and an inlet (6) into the cavity (29), wherein the hot runner (4) has at least two channels (41) which are connected at a first end (43) of each channel (41). connected to the inlet (6) leading into the cavity and connected at the second end (45) of each channel (41) to the entry port (8) leading into the injection mold, wherein the at least two channels (41) each at least partially form a spiral portion (75), and the at least two channels (41) are defined by a single-piece component (46), wherein the at least two channels (41) are separated from each other by the single-piece component (46) between their first end (43) and their second end (45); wherein the spiral portion (75) has a plurality of turns (50), and the number of the turns (50) is in the range of greater than 0.5 to 3; wherein the spiral portion (75) has a slope of less than 60° at at least one position.
15. The method according to claim 14, characterized in that The injection unit (5) comprises a barrel (11), a screw (13) having a screw tip (15) and a nozzle (17), and the screw (13) is rotatable and arranged in the barrel (11) so as to be movable in the direction of the longitudinal axis (19) of the barrel (11) between a front position (21) and a rear position (23), the distance (25) between the screw tip (15) and the nozzle (17) being smaller in the front position (21) than in the rear position (23), and wherein the first molding compound (1) comprises a first polymer compound and a first colorant, and the at least one further molding compound (3) comprises a further polymer compound, comprising the following steps: a) feeding a first amount of the first molding compound (1) onto the screw (13) when the screw (13) is in the rear position (23), b) advancing the screw (13) from the rear position (23) to the front position (21), c) feeding a second amount of the at least one further molding compound (3) onto the screw (13), d) plasticizing the first molding compound (1) and the at least one further molding compound (3) in the barrel (11) of the screw (13), rotating the screw (13) and conveying at least a portion of the first molding compound (1) and at least a portion of the at least one further molding compound (3) into a free space (27) in the barrel (11) between the nozzle (17) and the screw tip (15), and moving the screw (13) from the front position (21) to the rear position (23), e) feeding a new first amount of the first molding compound (1) onto the screw (13) when the screw (13) is in the rear position (23), f) injecting the first molding compound (1) and the at least one further molding compound (3) from the free space (27) in the barrel (11) into the cavity (29) of the injection mold (9), the screw (13) advancing from the rear position (23) to the front position (21), g) cooling the first molding compound (1) and the at least one further molding compound (3) in the injection mold (9), thereby producing a marbled molding, h) removing the marbled moulding from the injection mould (9), wherein steps c) to h) are repeated, step e) is performed before step f), and wherein the feeding of a new first amount of the first molding compound (1) in step e) and the feeding of the first amount of the first molding compound (1) in step a) are performed temporally and / or spatially separated from the feeding of the second amount of the at least one additional molding compound (3) in step c).
16. The method according to claim 15, characterized in that The at least one further moulding compound (3) comprises at least one further colourant.