Droplet Generator Nozzle
By adopting glass-metal sealing technology in the droplet generator nozzle, the problem of poor reliability and stability of existing nozzle seals in high temperature and high pressure environments is solved, higher stiffness and acoustic performance are achieved, and gas contamination is avoided .
Patent Information
- Application Number
- CN202080072568.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-09
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-10-09
AI Technical Summary
The seals of existing droplet generator nozzles have poor reliability and stability in high-temperature and high-pressure environments, are prone to vibration and instability due to deformation of the compliance sleeve, and are easily contaminated by gas.
A direct glass-to-metal seal is formed between the glass capillary tube and the metal fitting. By heating and applying pressure, the shape of the glass capillary tube and the through hole of the metal fitting is conformed to form a seal with high stiffness and high performance.
The overall stiffness and acoustic behavior of the nozzle is improved, gas contamination is avoided, seal reliability and stability are enhanced, and vibration and deformation are reduced.
Smart Images

Figure CN114555537B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to U.S. Application No. 62 / 916,723, filed on October 17, 2019, entitled “DROPLET GENERATOR NOZZLE,” which is incorporated herein by reference in its entirety. Technical Field
[0003] The present invention relates to a droplet generator nozzle for a laser-generated plasma radiation source and, more particularly, to a method of manufacturing the nozzle. Background Art
[0004] A lithographic apparatus is a machine configured to apply a desired pattern onto a substrate. A lithographic apparatus may be used, for example, in the manufacture of integrated circuits (ICs). A lithographic apparatus may, for example, project a pattern from a pattern forming device (e.g., a mask) onto a layer of radiation-sensitive material (e.g., a photoresist or simply a resist) disposed on a substrate.
[0005] To project a pattern on a substrate, a lithographic apparatus may use electromagnetic radiation. The wavelength of this radiation determines the minimum size of features that can be formed on a substrate. Lithographic apparatus using extreme ultraviolet (EUV) radiation having a wavelength in the range of 4-20 nm, such as 6.7 nm or 13.5 nm, can be used to form smaller features on a substrate compared to lithographic apparatus using radiation having a wavelength greater than, for example, 4-20 nm.
[0006] EUV radiation can be generated using plasma. A radiation system for generating EUV radiation may include a laser for exciting a fuel to provide a plasma, and a source collector module for containing the plasma. For example, a plasma can be generated by directing a laser beam to a flow of a fuel, such as particles of a suitable material, such as tin (Sn), or a suitable gas or vapor, such as Xe gas or Li vapor. The resulting plasma emits output radiation, such as EUV radiation, which is collected using a radiation collector. The radiation collector may be a mirror-type vertical incidence radiation collector that receives radiation and focuses the radiation into a beam. The source collector module may include an enclosing structure or chamber arranged to provide a vacuum environment to support the plasma. Such a radiation system is generally referred to as a laser produced plasma (LPP) source.
[0007] The fuel may be directed into the path of the laser beam by a droplet generator. The droplet generator may include a nozzle assembly to eject the fuel as droplets. Such a nozzle assembly may operate in a pressurized and / or high temperature environment, and therefore, may require a temperature and pressure resistant seal (e.g., an airtight seal) to be formed between components of the nozzle assembly. Existing nozzle assemblies may include seals between components that have poor reliability, stability, and performance.
[0008] Figure 1 A prior art nozzle assembly 100 is shown. The nozzle assembly 100 includes a glass capillary 110 for emitting fuel droplets from a fuel emitter. The fuel emitter may be a droplet generator.
[0009] Glass capillary 110 may be coupled to a fitting 120, which may be a component of a fuel emitter, or may be coupled to a fuel emitter. Fitting 120 may include metal.
[0010] It is desirable to form a seal, such as an airtight seal, between the glass capillary 110 and the fitting 120. The glass capillary 110 may be disposed within a through hole of the sleeve 130. The sleeve 130 may include a compliant material relative to the glass capillary 110. That is, the sleeve 130 may generally be elastic and / or compressible.
[0011] exist Figure 1 In the prior art example of FIG. 1 , a sleeve 130 is disposed within a through hole of a fitting 120 . A nut 140 is used to compress the sleeve 130 to form a substantially airtight seal between the fitting 120 and the glass capillary 110 .
[0012] The disadvantages of this arrangement for coupling the glass capillary 110 to the fitting 120 are as follows.
[0013] It has been shown that the maximum pressure that can be maintained by the compliant sleeve 130 in use is significantly limited. As such, the sleeve 130 may be subject to outgassing, such as outgassing of H2O, which may contaminate the fuel discharged by the glass capillary 110 in use.
[0014] Furthermore, the sleeve 130 may deform during use, thereby affecting the reliability, stability, and performance of the seal formed between the glass capillary 110 and the fitting 120. Furthermore, such deformation of the sleeve 130 may affect the acoustic behavior of the nozzle 100.
[0015] Additionally, the compliant sleeve 130 may reduce the overall stiffness of the glass capillary 110 relative to the fitting 120 , which may lead to undesirable and / or excessive vibration and overall instability in the nozzle 100 .
[0016] It is desirable to provide a nozzle assembly having reliable, stable and high performance seals between components that are subjected to temperature and pressure changes during operation of a droplet generator, and an apparatus for making such a nozzle assembly. In addition, it is desirable to provide a seal that is not susceptible to significant deformation during use and is relatively inert when exposed to fluids (such as liquid tin) during use. Summary of the invention
[0017] According to one aspect of the present invention, there is provided a method for manufacturing a nozzle of a droplet generator for a laser-generated plasma radiation source, the method comprising: placing a glass capillary in a through hole of a metal fitting; heating the metal fitting; and applying pressure to the glass capillary so that the glass capillary conforms to the shape of the through hole and forms a direct glass-to-metal seal with the through hole.
[0018] Advantageously, the direct glass-to-metal seal avoids the need to implement a sleeve to form a reliable, stable and high-performance seal between the glass capillary and the metal fitting. In addition, such a glass-to-metal seal can improve the overall stiffness and acoustic behavior of the nozzle.
[0019] At least a portion of the through hole may be frustum-shaped.
[0020] The through-hole may be cylindrical in shape.
[0021] Applying pressure may include applying internal pressure to the glass capillary.
[0022] Applying pressure (eg, internal pressure) may include sealing at least a first opening of a glass capillary; and pumping a gas into a second opening of the glass capillary.
[0023] Applying pressure may include applying external pressure to the glass capillary. Applying external pressure to the glass capillary may include applying a relative compressive force to at least one of: a portion of the glass capillary extending from the through hole; and / or one or both ends of the glass capillary.
[0024] The relative compressive force may be applied in a longitudinal direction relative to the glass capillary. That is, the relative compressive force may be applied along the longitudinal direction of the glass capillary.
[0025] Prior to applying external pressure, a rigid element such as a core rod or the like may be inserted into the glass capillary.
[0026] Pressure may be applied to the glass capillary during and / or after heating the metal fitting.
[0027] The method of making the nozzle may include heating the glass capillary.
[0028] The thermal expansion coefficient of the glass capillary can be substantially equal to or less than the thermal expansion coefficient of the metal fitting. In particular, in a temperature range including the operating temperature range of the nozzle and the manufacturing temperature range of the nozzle, the thermal expansion coefficient of the glass capillary can be substantially equal to or less than the thermal expansion coefficient of the metal fitting.
[0029] The metal fitting may include at least one of: molybdenum; tantalum; tungsten; or a metal alloy (such as a nickel-cobalt-iron alloy).
[0030] The glass capillary may comprise at least one of borosilicate, aluminosilicate, and / or quartz.
[0031] At least a portion of the metal assembly may include a metal oxide layer. For example, at least a portion of a through hole of a metal assembly forming a glass-to-metal seal may include a metal oxide layer.
[0032] The method may further include annealing the glass capillary and / or the metal fitting after cooling the metal fitting.
[0033] Heating the metal assembly may include induction heating the metal assembly.
[0034] Heating the metal fitting may include heating the metal fitting and the glass capillary in a temperature controlled oven or chamber.
[0035] Heating the metal assembly may include heating the metal assembly in an inert atmosphere or a relative vacuum.
[0036] Disposing the glass capillary in the through hole of the metal fitting may include: disposing the glass capillary in the through hole so that the glass capillary protrudes from both ends of the through hole. At least a portion of the glass capillary that protrudes from the metal fitting may be removed by at least one of the following: sanding, grinding, polishing and / or cutting.
[0037] According to another aspect, a nozzle for a droplet generator for a laser-produced plasma radiation source is provided, the nozzle comprising a glass capillary for emitting a fuel as droplets; a metal fitting for coupling the glass capillary to a body of the droplet generator; the glass capillary conforming to a shape of a through hole of the metal fitting, and wherein the glass capillary forms a direct glass-to-metal seal with the through hole.
[0038] The shape of the through-hole may include uniform cylindrical sections and / or frustum-shaped sections.
[0039] The nozzle may be manufactured according to the following method: placing a glass capillary in a through hole of a metal fitting; heating the metal fitting; and applying pressure to the glass capillary so that the glass capillary conforms to the shape of the through hole and forms a direct glass-to-metal seal with the through hole.
[0040] According to another aspect of the present invention, there is provided a laser produced plasma radiation source comprising a droplet generator configured to provide a stream of fuel droplets, wherein the droplet generator comprises a nozzle, the nozzle comprising: a glass capillary for emitting the fuel as droplets; a metal fitting for coupling the glass capillary to a body of the droplet generator; the glass capillary conforming to a shape of a through hole of the metal fitting, and wherein the glass capillary forms a direct glass-to-metal seal with the through hole. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Embodiments of the invention will now be described, by way of example only, with reference to the accompanying schematic drawings, in which:
[0042] Figure 1 An example of a conventional nozzle for a droplet generator for a laser-produced plasma radiation source is depicted;
[0043] Figure 2 A lithographic system including a lithographic apparatus and a radiation source embodying the present invention is shown;
[0044] Figure 3a to Figure 3c Depicts steps in a method for manufacturing a nozzle for a droplet generator for a laser produced plasma radiation source according to an embodiment of the present invention;
[0045] Figure 3d A nozzle manufactured by a method according to an embodiment of the present invention is shown. DETAILED DESCRIPTION
[0046] Figure 2 A lithographic system is shown comprising a radiation source SO and a lithographic apparatus LA. The radiation source SO is configured to generate an EUV radiation beam B and to provide the EUV radiation beam B to the lithographic apparatus LA. The lithographic apparatus LA comprises an illumination system IL, a support structure MT configured to support a patterning device MA (e.g. a mask or reticle), a projection system PS, and a substrate table WT configured to support a substrate W.
[0047] The illumination system IL is configured to condition the EUV radiation beam B before it is incident on the patterning device MA. Furthermore, the illumination system IL may comprise a facet field mirror arrangement 10 and a facet pupil mirror arrangement 11. The facet field mirror arrangement 10 and the facet pupil mirror arrangement 11 together provide an EUV radiation beam B having a desired cross-sectional shape and a desired intensity distribution. The illumination system IL may comprise other mirrors or arrangements in addition to or as an alternative to the facet field mirror arrangement 10 and the facet pupil mirror arrangement 11.
[0048] After being so conditioned, the EUV radiation beam B interacts with the patterning device MA. As a result of this interaction, a patterned EUV radiation beam B' is produced. The projection system PS is configured to project the patterned EUV radiation beam B' onto the substrate W. For this purpose, the projection system PS may include a plurality of mirrors 13, 14 configured to project the patterned EUV radiation beam B' onto the substrate W held by the substrate table WT. The projection system PS may apply a reduction factor to the patterned EUV radiation beam B' so as to form an image having features that are smaller than corresponding features on the patterning device MA. For example, a reduction factor of 4 or 8 may be applied. Although in Figure 1 The projection system PS is shown with only two mirrors 13, 14, but the projection system PS may comprise a different number of mirrors (eg six or eight mirrors).
[0049] The substrate W may include a previously formed pattern. In this case, the lithographic apparatus LA aligns the image formed by the patterned EUV radiation beam B′ with the pattern previously formed on the substrate W.
[0050] A relative vacuum, ie a small amount of gas (eg hydrogen) at a pressure well below atmospheric pressure, may be provided in the radiation source SO, the illumination system IL and / or the projection system PS.
[0051] For example, Figure 2 The radiation source SO shown is of a type that may be referred to as a laser produced plasma (LPP) source. A laser system 1, which may, for example, include a CO2 laser, is arranged to deposit energy via a laser beam 2 into a fuel, such as tin (Sn), provided from, for example, a fuel emitter 3. Although tin is mentioned in the following description, any suitable fuel may be used. The fuel may, for example, be in liquid form and may, for example, be a metal or an alloy. The fuel emitter 3 may include a nozzle 200 configured to direct tin (for example in the form of droplets) along a trajectory toward a plasma formation region 4. The laser beam 2 is incident on the tin at the plasma formation region 4. The deposition of laser energy into the tin generates a tin plasma 7 at the plasma formation region 4. During de-excitation and recombination of electrons with ions of the plasma, radiation including EUV radiation is emitted from the plasma 7.
[0052] EUV radiation from the plasma is collected and focused by a collector 5. The collector 5 includes, for example, a near normal incidence radiation collector 5 (sometimes more generally referred to as a normal incidence radiation collector). The collector 5 may have a multi-layer mirror structure arranged to reflect EUV radiation (e.g., EUV radiation having a desired wavelength such as 13.5 nm). The collector 5 may have an elliptical structure with two focal points. The first focal point may be in the plasma formation region 4, and the second focal point may be at an intermediate focus 6, as described below.
[0053] The laser system 1 may be spatially separated from the radiation source SO. In this case, the laser beam 2 may be transferred from the laser system 1 to the radiation source SO by means of a beam delivery system (not shown) comprising, for example, suitable directional mirrors and / or beam expanders and / or other optical devices. The laser system 1, the radiation source SO and the beam delivery system may together be considered a radiation system.
[0054] The radiation reflected by the collector 5 forms an EUV radiation beam B. The EUV radiation beam B is focused at an intermediate focus 6 to form an image at the intermediate focus 6 of a plasma present at the plasma formation region 4. The image at the intermediate focus 6 serves as a virtual radiation source for the illumination system IL. The radiation source SO is arranged such that the intermediate focus 6 is located at or near an opening 8 in an enclosing structure 9 of the radiation source SO.
[0055] although Figure 2 The radiation source SO is depicted as a laser produced plasma (LPP) source, but any suitable source, such as a discharge produced plasma (DPP) source or a free electron laser (FEL), may be used to generate EUV radiation.
[0056] As described above, the fuel emitter 3 may include a nozzle 200 configured to direct the fuel (eg, tin in the form of droplets) along a trajectory towards the plasma formation region 4 .
[0057] Figure 3a A glass capillary 210 is shown. The glass capillary 210 is a hollow glass tube that is open at a first end 225 and a second end 230. The glass capillary 210 may include, for example, borosilicate, aluminosilicate, or quartz. The glass capillary 210 may include, for example, soda-lime glass or alkali-barium glass. The glass capillary 210 may include alkali-barium aluminoborosilicate glass. The glass capillary 210 may be optimized or modified, for example by mixing alkalis (Na and K) and / or alkaline earths (Ca and Mg), etc., to achieve desired physicochemical properties. When disposed in a forming nozzle (e.g. Figure 2 When the glass capillary 210 is in a metal fitting 220 that is a portion of the nozzle 200 as shown, the glass capillary 210 can be a straight tube with constant inner and outer diameters.
[0058] Figure 3a Also shown in FIG. 2 is a metal assembly 220. The metal assembly 220 includes a through hole 235. The metal assembly 220 may be formed of, for example, molybdenum, tantalum, and / or tungsten. In some embodiments, the metal assembly 220 may include, for example, aluminum and / or platinum. In some embodiments, the metal assembly 220 may include a metal alloy, such as stainless steel, etc.
[0059] exist Figure 3aIn an exemplary embodiment of the present invention, a portion 240 of the through hole 235 is substantially frustum-shaped. That is, the frustum-shaped through hole portion 240 has a substantially conical surface. This frustum / conical shape can be formed, for example, by machining the metal assembly 220 with a conical reamer. In other embodiments, the entire through hole can be roughly frustum-shaped. In yet other embodiments, the entire through hole can be cylindrical. It should also be understood that in alternative embodiments falling within the scope of the present invention, the through hole can be straight or substantially straight. That is, in alternative embodiments, all or substantially all of the through holes can be straight, such as a uniform cylindrical shape. The shape of the through hole can include a uniform cylindrical portion and a frustum-shaped portion.
[0060] In one advantageous embodiment, the sidewalls of the substantially frusto-shaped through-hole portion 240 may be angled between approximately 2 and 5 degrees relative to the longitudinal axis X defined by the through-hole 235 and the center of the frusto-shaped through-hole portion 240. Note that for exemplary purposes only, Figures 3a to 3d The angle is magnified. Figures 3a to 3d In other embodiments within the scope of the present invention, the angle of the sidewalls of the substantially frusto-shaped through-hole portion 240 of the through-hole may be between greater than 5 degrees and less than 2 degrees relative to the longitudinal axis X defined by the through-hole 235 and the center of the frusto-shaped through-hole portion 240.
[0061] At least a portion of the metal assembly 220 may advantageously include an oxide layer on the surface forming the through hole 235, and in particular, the substantially frustum-shaped through hole portion 240 of the through hole 235 includes an oxide layer. Such an oxide layer may provide a more robust and / or reliable and / or effective glass-to-metal seal. Advantageously, providing an oxide layer (e.g., a metal oxide layer) provides oxygen atoms that can be used to form an effective glass-to-metal bonding layer.
[0062] It should be understood that providing a metal oxide layer may be applicable to any metal used to form a glass-to-metal seal. For example, a metal assembly 220 including any of molybdenum, tungsten, tantalum, and / or a metal alloy such as nickel-cobalt-iron alloy may include a metal oxide layer. In some example embodiments, at least a portion of the metal assembly 220 (e.g., at least a portion of a through hole of the metal assembly) may be oxidized to ensure that a sufficient and / or adequate oxide layer is present before forming a glass-to-metal seal.
[0063] If such an oxide layer is desired but is found to be initially absent or insufficient, the metal assembly 220 can be treated to form an oxide layer. For example, the metal assembly 220 can be heated in the presence of oxygen to accelerate the formation of such an oxide layer.
[0064] The first step in the method of manufacturing the nozzle 200 for a droplet generator may include disposing the glass capillary 210 in the through hole 235 and the frustum-shaped through hole portion 240 of the metal fitting 220 .
[0065] exist Figure 3a , the first end 225 of the glass capillary 210 is shown extending from the metal fitting 220. In other embodiments, the first end 225 of the glass capillary 210 can be substantially flush with the end 245 or face of the metal fitting 220. It can be noted that, prior to the heating step described below, the glass capillary 210 does not have the same shape as the through hole 235 including the frustum-shaped through hole portion 240. Instead, the glass capillary 210 is straight, has a constant outer diameter, and does not conform to the shape of the frustum-shaped through hole portion 240 or the through hole 235 prior to heating, as shown in FIG. Figure 3a shown.
[0066] In various embodiments, the outer diameter of the glass capillary 210 is slightly smaller than the inner diameter of the through hole 235. In this way, the glass capillary 210 can be inserted into the through hole 235. For example, the difference between the outer diameter of the glass capillary 210 and the inner diameter of the through hole 235 can be in the range of 1 mm, 0.1 mm, or less, but other differences in the corresponding diameters can be used in other embodiments.
[0067] Another step of manufacturing the nozzle 200 for the droplet generator may include heating the metal fitting 220 or heating the metal fitting 220 and the glass capillary 210. Heating the metal fitting 220 and the glass capillary 210 may include placing the metal fitting 220 and the glass capillary 210 in a temperature controlled oven or chamber. Heating the metal fitting 220 may include inductively heating the metal fitting 220. By inductively heating the metal fitting 220, the glass capillary may be heated by the metal fitting 220.
[0068] The heating process, together with the application of pressure as described below, causes the glass capillary 210 to conform to the shape of the through hole 235 including the frustum-shaped through hole portion 240 .
[0069] In one particular embodiment, the metal fitting 220 can be heated in a relatively inert atmosphere. For example, the metal fitting 220 can be disposed within a shield, container, chamber, enclosure, etc., and exposed to a relatively inert gas (such as nitrogen or argon). Advantageously, such a relatively inert gas can prevent oxidation of one or more surfaces of the glass capillary 210 or the metal fitting 220. For example, a metal fitting 220 comprising molybdenum can be particularly susceptible to oxidation when heated in the presence of oxygen. Therefore, heating the metal fitting 220 in the presence of a relatively inert gas can prevent or at least minimize such oxidation of an undesirable oxide layer on the surface of the metal fitting 220 and / or the glass capillary 210. For example, it may be desirable to have an oxide layer on only a portion of the surface of the metal fitting 220 that forms the glass-to-metal seal.
[0070] The inert atmosphere can be provided as a gas flow. Thus, the temperature of the atmosphere can be controlled. The temperature of the atmosphere can be controlled or maintained at a relatively constant level. Advantageously, by providing the inert atmosphere as a gas flow, heating of the inert atmosphere can be minimized. Advantageously, the gas flow can have a cooling effect on the portion of the glass capillary 210 exposed to the gas flow. Thus, undesirable deformation of one or more portions of the glass capillary 210 extending or protruding from the metal fitting 220 can be limited.
[0071] In yet another embodiment, the metal fitting 220 can be heated in a relative vacuum environment (e.g., a low pressure environment). For example, the metal fitting 220 can be disposed in a shield, container, chamber, enclosure, etc., and the surrounding gas (e.g., air) can be exhausted from the shield, container, chamber, or enclosure or pumped or pushed in other ways to achieve a relative vacuum, such as a partial vacuum or a low pressure environment. Advantageously, a relative vacuum, such as a partial vacuum or a low pressure environment can prevent oxidation of one or more surfaces of the glass capillary 210 or the metal fitting 220. For example, when heated in the presence of oxygen, a metal fitting 220 comprising molybdenum can be particularly subject to oxidation. Therefore, heating the metal fitting 220 in a relative vacuum or low pressure environment can prevent or at least minimize such oxidation.
[0072] The heating and pressurization described below expands the glass capillary 210 within the metal fitting 220 to conform to the shape of the through hole 235 of the metal fitting. It should be noted that the portion of the glass capillary 210 that expands within the metal fitting 220 includes a thinner sidewall than the portion of the glass capillary 210 that may be exposed to the gas flow. Advantageously, such a gas flow can ensure that the thickness of the sidewall of the portion of the glass capillary 210 that may be exposed to the gas flow is maintained at a desired level and is not subjected to undesirable deformation, such as expansion, that may thin the sidewall of the glass capillary 210.
[0073] In one embodiment, an argon gas flow of between 4 and 8 standard liters per minute is provided, although other flows are used in other embodiments.
[0074] The glass capillary 210 may also be heated directly, for example, while the metal fitting is being heated, such as by a temperature controlled oven or chamber.Alternatively (or additionally), the glass capillary 210 may be heated by the metal fitting 220 as described above.
[0075] By heating the metal fitting 220, the glass capillary 210 can be heated to a degree that the glass capillary 210 becomes soft. That is, the glass capillary 210 can be heated to a level whereby the glass capillary 210 transitions from a rigid state to a softened state, such as a relatively flexible or partially melted state. That is, the glass capillary 210 can be heated directly or through the metal fitting 220 until the viscosity of the glass forming the glass capillary 210 is reduced to a degree that the glass becomes relatively flexible.
[0076] The metal fitting 220 may be heated to a temperature in the range of 800 K to 2000 K. The temperature to which the metal fitting 220 may be heated may depend on the material used for the glass capillary 210. For example, a glass capillary 210 comprising quartz may require a temperature in the range of 1800 K, while a glass capillary 210 comprising borosilicate may require a temperature in the range of 800 K.
[0077] Metal fitting 220 may be heated to at least the operating temperature of glass capillary 210, such as a temperature at which glass capillary 210 becomes pliable. Preferably, metal fitting 220 is not heated to a temperature that would cause glass capillary 210 or metal fitting 220 to deform excessively under its own weight.
[0078] Another step in manufacturing the nozzle 200 for the droplet generator may include applying internal or external pressure to the glass capillary 210 so that the glass capillary 210 conforms to the shape of the through hole 235 and forms a direct glass-to-metal seal with the through hole 235, as will be described with reference to Figure 3b and Figure 3c described.
[0079] Figure 3b 2 depicts an internal pressure applied to the glass capillary 210. The step of applying the internal pressure to the glass capillary 210 may include the step of sealing the opening of the first end 225 or the opening of the second end 230 of the glass capillary 210. Figure 3b In the illustrated embodiment, the opening of the second end 230 is sealed with a cap 250 .
[0080] The step of sealing the opening of the first end 225 or the opening of the second end 230 may be performed before or after the step of heating the metal fitting 220. For example, after the metal fitting 220 is heated so that the glass capillary 210 is softened, the opening of the first end 225 or the opening of the second end 230 may be sealed by compressing (e.g., clamping or crimping) a portion of the glass capillary 210 at the opening of the first end 225 or the opening of the second end 230. In addition, the step of sealing the opening of the first end 225 or the opening of the second end 230 may be performed before or after the step of disposing the glass capillary 210 in the through hole 235 and the truncated through hole portion 240 of the metal fitting 220.
[0081] The opening of the first end 225 or the opening of the second end 230 can be sealed by, for example, a plug, a cover or a cap. Additionally or alternatively, the opening of the first end 225 or the opening of the second end 230 can be sealed by, for example, glue or resin (such as a curable resin).
[0082] The opening of the first end 225 or the opening of the second end 230 can be sealed by, for example, heating and at least partially melting the glass capillary 210. For example, the glass capillary 210 can be heated and then crimped to form a seal. The seal can advantageously be an airtight seal, such as a gas-tight seal.
[0083] The step of applying internal pressure to the glass capillary 210 may also include pumping a gas into the other of the opening of the first end 225 or the opening of the second end 230 of the glass capillary 210. That is, if the opening of the first end 225 is sealed, the gas may be pumped into the opening of the second end 230. Conversely, if the opening of the second end 230 is sealed, the gas may be pumped into the opening of the first end 225. Preferably, the gas is a relatively inert gas (relative to the metal fitting 220 and the glass capillary 210), such as nitrogen and / or argon.
[0084] Internal pressure may be applied during and / or after heating the metal fitting 220 and the glass capillary 210 .
[0085] For example purposes only, Figure 3b A cap 250 is shown sealing the second end 230 of the glass capillary 210. Figure 3b In the example shown in FIG. 2 , gas is pumped into the first end 225 of the glass capillary in the direction indicated by arrow 255 .
[0086] A pump or compressor may be communicatively coupled to the glass capillary 210 to pump gas into the first end 225 of the glass capillary. Figure 3bAs shown, a portion of the glass capillary tube protrudes from, e.g., extends outwardly from, an end 245 or face of the metal fitting 220. Thus, a hose or tubing (not shown) may be attached to the protruding portion of the glass capillary tube 210 using any suitable means to form a seal between the hose or tubing and the glass capillary tube 210. A pump or compressor may be communicatively coupled to the hose or tubing and thus configured to apply internal pressure to the glass capillary tube 210.
[0087] As gas is pumped into the glass capillary 210, the pressure increases within the glass capillary 210. In one embodiment, the pressure within the glass capillary 210 may be set to about 0.5 bar, but in other embodiments, the pressure within the glass capillary 210 may be set or increased to between 0.1 bar and 10 bar or higher.
[0088] Due to the applied internal pressure and the relative flexibility of the glass capillary 210 due to the heating of the metal fitting 220 and / or the glass capillary 210, the glass capillary 210 expands and / or deforms within the through hole 235 of the metal fitting 220 and the frustum-shaped through hole portion 240 until it contacts the through hole of the metal fitting 220. In particular, as Figure 3b As shown, the glass capillary 210 expands and / or deforms within the truncated through-hole portion 240 until it contacts the truncated through-hole portion 240 of the through-hole of the metal fitting 220. In this way, the glass capillary 210 expands and / or deforms so that the glass capillary conforms to the shape of the through-hole 235, particularly to the shape of the truncated through-hole portion 240.
[0089] As previously described, the through hole can be straight, or substantially straight, for example, the through hole may not have a truncated portion. That is, in an alternative embodiment, all or substantially all of the through holes can be straight, for example, uniformly cylindrical. In such an embodiment, due to the applied internal pressure and the relative flexibility of the glass capillary 210 caused by heating the metal fitting 220 and / or the glass capillary 210, the straight glass capillary 210 can expand and / or deform within the through hole 235 of the metal fitting 220 and the truncated through hole portion 240 until it contacts the through hole of the metal fitting 220.
[0090] Furthermore, due to the pressure applied by the gas, the temperature of the metal fitting 220 , and the temperature of the glass capillary 210 , a glass-to-metal seal is formed between the glass capillary 210 and the metal fitting 220 .
[0091] After the glass-to-metal seal is formed, the cap 250 or seal may be removed. Removal of the cap 250 or seal may include removal of a portion of the glass capillary 210, such as cutting away.
[0092] Figure 3c An external pressure is shown applied to the glass capillary 210. Applying the external pressure to the glass capillary 210 may include applying an opposing compressive force to at least one of: a portion of the glass capillary 210 extending from the through hole; and / or a first end 225 and a second end 230 of the glass capillary.
[0093] The external pressure may be applied during and / or after heating the metal fitting 220 and the glass capillary 210 .
[0094] exist Figure 3c In the example of FIG. 1 , pressure is applied to the first end 225 and the second end 230 of the glass capillary 210 in the directions indicated by arrows 260 and 265. That is, the directions indicated by arrows 260 and 265 are generally opposite. Thus, the force is a compressive force, which acts to compress the glass capillary 210.
[0095] Due to the applied external pressure and the relative flexibility of the glass capillary 210 due to the heating of the metal fitting 220 and / or the glass capillary 210, the glass capillary 210 expands and / or deforms within the through hole 235 of the metal fitting 220 and the frustum-shaped through hole portion 240 until it contacts the through hole of the metal fitting 220. In particular, as Figure 3c As shown, the glass capillary 210 expands and / or deforms within the truncated through-hole portion 240 until it contacts the truncated through-hole portion 240 of the metal fitting 220. In this way, the glass capillary 210 expands and / or deforms so that the glass capillary conforms to the shape of the through-hole 235, particularly to the shape of the truncated through-hole portion 240.
[0096] As previously described, the through hole can be straight, or substantially straight, for example, the through hole may not have a truncated portion. That is, in an alternative embodiment, all or substantially all of the through holes can be straight, for example, a uniform cylindrical shape. In such an embodiment, due to the applied external pressure and the relative flexibility of the glass capillary 210 caused by heating the metal fitting 220 and / or the glass capillary 210, the straight glass capillary 210 can expand and / or deform within the through hole 235 of the metal fitting 220 and the truncated through hole portion 240 until it contacts the through hole of the metal fitting 220.
[0097] Furthermore, due to the applied external pressure, the temperature of the metal fitting 220 and the temperature of the glass capillary 210 , a glass-to-metal seal is formed between the glass capillary 210 and the metal fitting 220 .
[0098] like Figure 3cAs shown, the relative compressive force indicated by arrows 260, 265 is applied in the longitudinal direction relative to the glass capillary 210. Such external force can be applied by any suitable means, such as by placing the glass capillary 210 in a machine press. Such a machine press can be mechanical, hydraulic or pneumatic. Such external force can be applied by placing the glass capillary 210 between intermediate components (such as plates) and then applying external pressure to the intermediate components. Such external force can be applied by clamping one or more parts of the glass capillary, such as by one or more clamps, and moving the one or more clamps relative to the metal assembly 220.
[0099] The step of applying external pressure to the glass capillary 210 may further include inserting a rigid member 290 (eg, a core rod) into the glass capillary 210 before applying the external pressure. Such a rigid member may prevent the through hole of the glass capillary 210 from collapsing or excessively deforming in an undesirable direction due to the applied external force.
[0100] Figure 3d A nozzle manufactured by a method according to an embodiment of the present invention is depicted. Figure 3b and Figure 3c In contrast, the portion of the glass capillary 210 that protrudes (e.g., protrudes) from the end 245 or face of the metal fitting 220 has been removed. The removal of the portion may include at least one of sanding, grinding, polishing, and / or cutting. In other embodiments, the portion of the glass capillary 210 that protrudes from the end 245 or face of the metal fitting 220 may be left in place and / or formed as an edge.
[0101] Another step in the method of manufacturing a nozzle 200 for a droplet generator may include cooling the metal fitting 220. Such cooling may be active cooling, such as by refrigeration or with the aid of a cooling gas flow, or by natural cooling, such as allowing the metal fitting 220 to cool to ambient temperature. Such cooling may follow or adhere to a predetermined temperature profile. Advantageously, such cooling may at least partially anneal the glass capillary, thereby reducing internal stresses within the glass capillary.
[0102] In addition, the end of the glass capillary (e.g., after removing the above-mentioned protruding portion) and / or the end 245 or face of the metal fitting 220 can be ground and / or polished. Such grinding and / or polishing can provide a smooth surface so that the end of the glass capillary 210 is flush with the end 245 or face of the metal fitting 220. In addition, such grinding or polishing can remove unwanted debris or oxide layers. In particular, for a metal fitting 220 including molybdenum, a molybdenum oxide layer can be formed on the end 245 or face of the metal fitting 220. Such polishing and / or grinding can remove such an oxide layer.
[0103] The method may include the step of annealing the glass capillary 210 and / or the metal fitting 220. The specific temperature and / or heating and / or cooling rate required for annealing the glass capillary 210 may depend on the specific glass type and / or glass composition. For example, the glass capillary 210 may be heated to about 600K to 800K before cooling to ambient temperature, although other temperatures may be used in other embodiments. This annealing step may be repeated one or more times.
[0104] The step of annealing the glass capillary 210 may be performed before and / or after the step of removing the portion of the glass capillary 210 that protrudes (eg, bulges) from the end 245 or face of the metal fitting 220 .
[0105] Advantageously, Figures 3a to 3d The frustum-shaped through-hole of the exemplary embodiment shown in FIG. 2 provides an enhanced seal between the glass capillary 210 and the metal fitting 220 during use. That is, during use, as the pressurized fuel enters the glass capillary 210 at the first opening 275 and is ejected or released from the glass capillary 210 at the second opening 280, pressure may be applied to the inner surface, such as the inner sidewall, of the glass capillary 210. Such pressure applied by the fuel may, to some extent, further expand the glass capillary 210, thereby pressing the glass capillary 210 against the metal fitting 220. Therefore, the glass-to-metal seal between the glass capillary 210 and the metal fitting 220 may form a self-energizing seal at least to some extent, such as an improved seal due to the pressure applied to the inner surface of the glass capillary 210 during use.
[0106] Advantageously, the coefficient of thermal expansion (CTE) of the metal fitting 220 is substantially the same as the CTE of the glass capillary 210 over the operating temperature range of the nozzle 200, or is within a predetermined range relative to the CTE of the glass capillary 210. Further, it is also advantageous that the CTE of the metal fitting 220 is substantially the same as the CTE of the glass capillary 210, or is within a predetermined range relative to the CTE of the glass capillary 210, over a temperature range that includes the temperature required to form a glass-to-metal seal, such as over the manufacturing temperature range of the nozzle. That is, the glass-to-metal seal is formed at a temperature at which the glass softens and is subsequently cooled to room temperature. Thus, it is advantageous that the CTE of the metal fitting 220 is substantially the same as the CTE of the glass capillary 210, or is within a predetermined range relative to the CTE of the glass capillary 210, over the entire temperature range that includes the temperature at which the glass softens and room temperature, and preferably also includes the operating temperature range of the nozzle 200, which may include temperatures below room temperature.
[0107] For example, a metal fitting including molybdenum may have a CTE of approximately 5.5 ppm / K. Thus, the predetermined range of the CTE of the glass capillary may be, for example, + / -0.5 ppm / K. Various borosilicate or aluminosilicate glasses include CTEs that match molybdenum within + / -0.5 ppm / K. A glass capillary having a CTE lower than the CTE of the metal fitting may be selected to create an interference fit between the metal fitting and the glass capillary. For example, one embodiment may include a metal fitting including molybdenum and a glass capillary including borosilicate having a CTE of approximately 3.3 ppm / K. Such pressure may advantageously cause the glass-to-metal seal to additionally and / or at least partially form an interference fit between the metal fitting and the glass capillary. That is, in use, pressure may be applied to the inner surface of the glass capillary 210, whereby the pressure may further expand the glass capillary 210 to a certain extent, thereby pressing the glass capillary 210 against the metal fitting 220.
[0108] The operating temperature range may depend on the fuel injected or sprayed by the nozzle 200. For example, the operating temperature range of liquid tin as a fuel may be approximately 300K to 530K.
[0109] Furthermore, in use, the fuel provided by the droplet generator may be, for example, a tin compound, such as SnBr4, SnBr2, SnH4, or a tin alloy, such as a tin-gallium alloy, a tin-indium alloy, a tin-indium-gallium alloy, or a combination thereof. Depending on the material used, the target material may be provided by the droplet generator at a variety of temperatures, including at or near room temperature (e.g., tin alloy, SnBr4), at an elevated temperature (e.g., pure tin), or at a temperature below room temperature (e.g., SnH4). Therefore, it is particularly advantageous to form a glass-to-metal seal between the glass capillary 210 and the metal fitting 220 that is relatively temperature invariant in terms of performance over the entire operating temperature range.
[0110] By closely matching the CTE of the glass capillary 210 to the CTE of the metal fitting 220, cracking of the glass capillary can be avoided after the nozzle is heated to operating temperature (eg, 500 to 500 K for molten tin).
[0111] The CTE of the glass capillary 210 can be closely matched to the CTE of the metal fitting 220, or slightly lower but not slightly higher than the CTE of the metal fitting 220. For example, during the manufacture of the nozzle, and / or in use, if the CTE of the glass capillary 210 is higher than the metal fitting 220, the glass capillary 210 will shrink faster than the metal fitting 220 during cooling of the nozzle 200. This difference in shrinkage between the glass capillary 210 and the metal fitting 220 can be detrimental to the integrity of the glass-metal seal. That is, this difference in shrinkage between the glass capillary 210 and the metal fitting 220 can cause the glass capillary to separate from the metal fitting 220. Therefore, it is beneficial to have a shrinkage of the glass capillary 210 that is less than or equal to a shrinkage of the metal fitting 220.
[0112] The term “inert” as used throughout the specification should be interpreted to mean chemically inert with respect to the glass capillary 201 and the metal fitting 220 .
[0113] The term "glass-to-metal" seal refers to a seal, such as a hermetic seal, between glass and metal, wherein metal is interpreted to include metals, metal alloys, and / or metal oxides. That is, the term "glass-to-metal seal" should be understood to include a seal between glass and metal, wherein the metal may include an oxide layer. For example, in a particular embodiment of the present invention, wherein the metal fitting comprises molybdenum, the term "glass-to-metal seal" includes a seal between a glass capillary 210 and a surface of the metal fitting, wherein the surface of the metal fitting 220 to be sealed to the glass capillary 210 may already include an oxide layer prior to forming the seal.
[0114] Although specific reference may be made herein to the use of lithographic apparatus in IC manufacturing, it should be understood that the lithographic apparatus described herein may have other applications. Possible other applications include the manufacture of integrated optical systems, guidance and detection patterns for magnetic domain memories, flat panel displays, liquid crystal displays (LCDs), thin film magnetic heads, etc.
[0115] Although specific reference is made above to the use of embodiments of the present invention in the context of a droplet generator for a laser-generated plasma radiation source, it should be understood that nozzles made according to the claimed and described methods may have utility and / or be adapted for use in a variety of other applications. For example, such nozzles may be generally applicable to any fluid delivery application, particularly any fluid delivery application in which the fluid to be delivered is under pressure.
[0116] Although specific reference has been made above to the use of embodiments of the invention in the context of optical lithography, it will be appreciated that the invention is not limited to optical lithography and may be used in other applications, such as imprint lithography, where the context permits.
[0117] Further aspects of the invention are set out in the following numbered clauses.
[0118] 1. A method for manufacturing a nozzle for a droplet generator, the method comprising:
[0119] placing a glass capillary in a through hole of a metal fitting;
[0120] heating the metal assembly; and
[0121] Pressure is applied to the glass capillary so that the glass capillary conforms to the shape of the through hole and forms a direct glass-to-metal seal with the through hole.
[0122] 2. The method of clause 1, wherein at least a portion of the through-hole is frustum-shaped.
[0123] 3. The method of clause 1, wherein the disposing the glass capillary in the through hole of the metal fitting comprises: disposing the glass capillary in the form of a tube having a constant diameter, and wherein the heating and applying pressure changes the shape of the capillary.
[0124] 4. The method according to any one of clauses 1 to 3, wherein applying the pressure comprises applying internal pressure to the glass capillary and comprises at least:
[0125] sealing the first opening of the glass capillary; and
[0126] Gas is pumped into the second opening of the glass capillary.
[0127] 5. The method according to any one of clauses 1 to 3, wherein the step of applying the pressure comprises applying external pressure to the glass capillary by applying a relative compressive force to at least one of:
[0128] a portion of the glass capillary extending from the through hole; and
[0129] One end or both ends of the glass capillary.
[0130] 6. The method according to clause 5, wherein the relative compressive force is applied along the longitudinal direction of the glass capillary.
[0131] 7. The method according to clause 5, further comprising the step of inserting a rigid element into the glass capillary before applying the external pressure.
[0132] 8. The method according to any of the preceding clauses, wherein the pressure is applied to the glass capillary during and / or after heating the metal fitting.
[0133] 9. A method according to any of the preceding clauses, wherein within a temperature range that includes an operating temperature range of the nozzle and a manufacturing temperature range of the nozzle, the thermal expansion coefficient of the glass capillary is less than or equal to the thermal expansion coefficient of the metal fitting.
[0134] 10. A method according to any of the preceding clauses, wherein the metal fitting comprises molybdenum, tantalum, tungsten or a metal alloy, and / or the glass capillary comprises borosilicate, aluminosilicate or quartz.
[0135] 11. A method according to any preceding clause, wherein at least a portion of the metal fitting comprises a metal oxide layer.
[0136] 12. The method according to any of the preceding clauses, further comprising annealing the glass capillary and / or the metal fitting after allowing the metal fitting to cool.
[0137] 13. The method of any preceding clause, wherein heating the metal assembly comprises inductively heating the metal assembly.
[0138] 14. The method of clause 13, further comprising providing a flow of an inert gas during the inductive heating, the flow of inert gas being directed to the glass capillary.
[0139] 15. The method of clause 1, wherein the through-hole is cylindrical.
[0140] 16. The method of any of the preceding clauses, wherein the step of heating the metal fitting comprises heating the metal fitting in an inert atmosphere or a relative vacuum.
[0141] 17. The method according to any of the preceding clauses, wherein the step of arranging the glass capillary in the through hole of the metal fitting comprises: arranging the glass capillary in the through hole so that the glass capillary protrudes from both ends of the through hole.
[0142] 18. The method according to clause 17, wherein at least a portion of the glass capillary protruding from the metal fitting is removed by at least one of: sanding, grinding, polishing and / or cutting.
[0143] 19. A nozzle for a droplet generator of a laser-generated plasma radiation source, the nozzle comprising:
[0144] a glass capillary for launching the fuel as a droplet;
[0145] a metal fitting for coupling the glass capillary to a body of the droplet generator;
[0146] The glass capillary is conformal to the shape of the through hole of the metal fitting, and wherein the glass capillary forms a direct glass-to-metal seal with the through hole.
[0147] 20. The nozzle according to clause 19, wherein the shape of the through hole comprises a uniform cylindrical section and / or a frustum-shaped section.
[0148] 21. The nozzle according to clause 19, wherein the nozzle is manufactured according to the following method:
[0149] placing the glass capillary in the through hole of the metal fitting;
[0150] heating the metal assembly; and
[0151] Pressure is applied to the glass capillary so that the glass capillary conforms to the shape of the through hole and forms a direct glass-to-metal seal with the through hole.
[0152] Although specific embodiments of the present invention have been described above, it should be understood that the present invention may be practiced in a manner other than that described. The above description is intended to be illustrative rather than limiting. Therefore, it will be apparent to those skilled in the art that modifications may be made to the described invention without departing from the scope of the claims set forth below.
Claims
1. A method for manufacturing a nozzle for a droplet generator, the method comprising: placing a glass capillary in a through hole of a metal fitting; heating the metal assembly; as well as Pressure is applied to the glass capillary so that the glass capillary conforms to the shape of the through hole and forms a direct glass-to-metal seal with the through hole. The method of claim 1 , wherein at least a portion of the through hole is frustum-shaped.
3. The method of claim 2, wherein disposing the glass capillary in the through hole of the metal fitting comprises: The glass capillary is provided in the form of a tube of constant diameter, and wherein the heating and application of pressure changes the shape of the capillary.
4. The method of claim 3, wherein applying the pressure comprises applying internal pressure to the glass capillary, and comprises at least: sealing the first opening of the glass capillary; as well as Gas is pumped into the second opening of the glass capillary.
5. The method of claim 1 , wherein applying the pressure comprises applying internal pressure to the glass capillary, and comprises at least: sealing the first opening of the glass capillary; as well as Gas is pumped into the second opening of the glass capillary.
6. The method of claim 3, wherein the step of applying the pressure comprises applying external pressure to the glass capillary by applying a relative compressive force to at least one of: a portion of the glass capillary extending from the through hole; and One end or both ends of the glass capillary.
7. The method of claim 1, wherein the step of applying the pressure comprises applying external pressure to the glass capillary by applying a relative compressive force to at least one of: a portion of the glass capillary extending from the through hole; and One end or both ends of the glass capillary. The method of claim 7 , wherein the relative compressive force is applied along a longitudinal direction of the glass capillary.
9. The method of claim 7, further comprising the step of inserting a rigid member into the glass capillary prior to applying the external pressure.
10. The method of claim 1, wherein pressure is applied to the glass capillary during and / or after heating the metal fitting.
11. The method of claim 1, wherein the glass capillary has a coefficient of thermal expansion less than or equal to a coefficient of thermal expansion of the metal fitting within a temperature range that includes an operating temperature range of the nozzle and a manufacturing temperature range of the nozzle.
12. The method of claim 1, wherein the metal fitting comprises molybdenum, tantalum, tungsten, or a metal alloy, and the glass capillary comprises borosilicate, aluminosilicate, or quartz.
13. The method of claim 12, wherein at least a portion of the through hole is frustum-shaped, and disposing the glass capillary in the through hole of the metal fitting comprises: The glass capillary is provided in the form of a tube of constant diameter, and wherein the heating and application of pressure changes the shape of the capillary.
14. The method of claim 1, wherein at least a portion of the metal assembly comprises a metal oxide layer.
15. The method of claim 1, further comprising annealing the glass capillary and / or the metal fitting after cooling the metal fitting.
16. The method of claim 1, wherein heating the metal assembly comprises inductively heating the metal assembly.
17. The method of claim 16, further comprising providing a flow of an inert gas during the inductive heating, the flow of inert gas being directed to the glass capillary. The method according to claim 1 , wherein the through hole is cylindrical in shape.
19. The method of claim 1, wherein the step of heating the metal assembly comprises heating the metal assembly in an inert atmosphere or a relative vacuum.
20. The method of claim 1, wherein the step of disposing the glass capillary in the through hole of the metal fitting comprises: The glass capillary is disposed in the through hole so that the glass capillary protrudes from both ends of the through hole.
21. The method of claim 20, wherein at least a portion of the glass capillary protruding from the metal fitting is removed by at least one of: sanding, grinding, polishing and / or cutting.
22. A nozzle for a droplet generator of a laser-generated plasma radiation source, the nozzle comprising: a glass capillary for launching the fuel as a droplet; a metal fitting for coupling the glass capillary to a body of the droplet generator; The glass capillary is conformal to the shape of the through hole of the metal fitting, and wherein the glass capillary forms a direct glass-to-metal seal with the through hole.
23. The nozzle of claim 22, wherein the shape of the through hole comprises a uniform cylindrical section and / or a frustum-shaped section.
24. The nozzle of claim 22, wherein the nozzle is manufactured according to the following method: placing the glass capillary in the through hole of the metal fitting; heating the metal assembly; as well as Pressure is applied to the glass capillary so that the glass capillary conforms to the shape of the through hole and forms a direct glass-to-metal seal with the through hole.
Citation Information
Patent Citations
Systems and methods for target material delivery in a laser produced plasma EUV light source
CN101978792A
Target material supply apparatus for an extreme ultraviolet light source
CN104885161A