Prediction method and system for high temperature rupture / creep life of coated high temperature alloy
By establishing the Larson-Miller curve and determining the equivalent bearing area, the problem of the mechanical properties of coating-containing high-temperature alloys in the prior art is solved, and the accurate prediction of high-temperature longevity/creep life is achieved, which reduces the testing cost and time. Improve the reliability of the prediction results.
Patent Information
- Application Number
- CN202210335014.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-31
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-03-31
AI Technical Summary
The prior art cannot effectively predict the mechanical properties of coating-containing high-temperature alloys, resulting in repeated tests and waste of data, and the existing methods ignore the high-temperature bearing capacity of the coating, resulting in low lifetime prediction accuracy and poor stability.
By obtaining the performance parameter data of bare alloy, the Larson-Miller curve is established, the durability/creep life test value of the coated alloy is obtained, the equivalent stress and equivalent bearing area are determined, and high-temperature durability/creep life prediction is carried out.
Fast and low-cost high-temperature long-lasting/creep life prediction is achieved, which improves the reliability and accuracy of the prediction results, and can distinguish the impact of different coatings on alloy performance.
Smart Images

Figure CN114566236B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of material science and technology, and in particular to a method and system for predicting the high-temperature rupture / creep life of a coated high-temperature alloy. Background Art
[0002] High-temperature alloys, the most commonly used materials for aircraft engine blades, are exposed to extremely high temperatures during service. To protect these alloys from oxidation during use, a high-aluminum-content, anti-oxidation coating, also known as a metal bond coat, is often applied to their surface. This coating forms a dense aluminum oxide film at high temperatures to protect the underlying material. While the metal bond coat effectively protects the alloy from oxidation, interdiffusion between the coating and the alloy during preparation and use can lead to a degradation of the alloy's mechanical properties.
[0003] Because the decline in mechanical properties is difficult to quantify, the mechanical properties of the original alloy cannot be used to evaluate the mechanical properties of the coated alloy. To ensure the safety of aircraft engines during use, the commonly used method (1) requires retesting the mechanical properties of the coated alloy to obtain accurate results. (2) In addition, some literature points out that it can be considered that the coating has no load-bearing capacity at high temperatures, and thus it is believed that the coating only reduces the load-bearing area (S2) of the base alloy. When predicting the life of the coated alloy, the stress σ1 applied to the cross-section of the coated alloy (cross-sectional area S1) is converted into the actual stress σ2 borne by the alloy, σ2 = σ1 * S1 / S2, and a stress value σ2 higher than the test stress σ1 is obtained. The bare alloy life data at this stress value is used as the predicted value of the coated alloy life.
[0004] The above methods have limitations: Method (1) retests the mechanical properties of the coated alloy. Due to the harsh operating environment of high-temperature alloys, the loss caused by material failure is difficult to estimate. Therefore, many material indicators need to be measured during the alloy screening process, and the testing time and cost are extremely high. After the alloy is coated, the performance data will change. If the mechanical properties of the coated alloy cannot be correctly predicted, a large amount of data accumulated in the early stage will be wasted, and repeated tests will cause a lot of manpower and material resources to be wasted. Method (2) ignores the high-temperature bearing capacity of the coating. This method assumes that the coating simply does not have the bearing capacity. Although the prediction method is simple and efficient, the effects of different types of metal bonding layers on the mechanical properties of the alloy are different. If a certain coating has a certain high-temperature bearing capacity, then the endurance / creep life predicted by this prediction method will be conservative, which is not conducive to fully utilizing the material properties; when a certain coating interacts strongly with the base alloy, in addition to not bearing the load, it may also damage the mechanical properties of the alloy base. At this time, the life predicted by this method is too optimistic. Once the material fails, the consequences are immeasurable. In summary, the prediction stability of this method is poor and the accuracy is low. Summary of the Invention
[0005] The purpose of the present invention is to provide a method and system for predicting the high-temperature rupture / creep life of coated high-temperature alloys, which can solve the problem that bare alloy performance test data cannot be directly used for coating alloy performance evaluation.
[0006] To achieve the above object, the present invention provides the following solutions:
[0007] The present invention provides a method for predicting the high-temperature rupture / creep life of a coated high-temperature alloy, the method comprising:
[0008] Obtaining bare alloy performance parameter data, and establishing a bare alloy Larson-Miller curve based on the bare alloy performance parameter data; the bare alloy performance parameter data including temperature, stress, and bare alloy rupture / creep life data under corresponding temperature and stress;
[0009] Obtaining a rupture / creep life test value of the coated alloy under test temperature and test stress conditions;
[0010] Determine a Larson-Miller parameter value according to the rupture / creep life test value of the coated alloy to be tested and the Larson-Miller curve of the bare alloy, obtain a stress value corresponding to the Larson-Miller parameter value, and use the stress value as the equivalent stress of the coated alloy to be tested;
[0011] Determine the equivalent load-bearing area of the coated alloy to be tested according to the equivalent stress; the equivalent load-bearing area of the coated alloy to be tested is the load-bearing area of the bare alloy equivalent to that of the coated alloy to be tested;
[0012] According to the equivalent bearing area of the coated alloy to be tested, the rupture / creep life of the coated alloy to be tested under different temperature and stress conditions is predicted.
[0013] Optionally, the expression of the bare alloy Larson-Miller parameter is:
[0014] P = T (C + lgτ);
[0015] Where P is the Larson-Miller parameter of the bare alloy, T is the absolute temperature, τ is the rupture / creep life of the alloy, and C is a constant related to the alloy material.
[0016] Optionally, the calculation formula for the equivalent load-bearing area of the coated alloy to be tested is:
[0017] S′0=S0*σ / σ′;
[0018] S0=S1+S2;
[0019] Wherein, S′0 is the equivalent bearing area of the coated alloy to be tested, S0 is the total cross-sectional area of the coated alloy to be tested, σ is the test stress value of the coated alloy to be tested, σ′ is the equivalent stress value of the coated alloy to be tested, S1 is the coating cross-sectional area of the coated alloy to be tested, and S2 is the substrate cross-sectional area of the coated alloy to be tested.
[0020] To achieve the above objectives, the present invention further provides a prediction system for high-temperature rupture / creep life of coated high-temperature alloys, the prediction system comprising:
[0021] A bare alloy Larson-Miller curve establishment unit, configured to obtain bare alloy performance parameter data and establish a bare alloy Larson-Miller curve based on the bare alloy performance parameter data; the bare alloy performance parameter data including temperature, stress, and bare alloy rupture / creep life data under corresponding temperature and stress;
[0022] A unit for acquiring a rupture / creep life test value of the coated alloy to be tested, for acquiring a rupture / creep life test value of the coated alloy to be tested under test temperature and test stress conditions;
[0023] a coated alloy to be tested equivalent stress determination unit, configured to determine a Larson-Miller parameter value based on a rupture / creep life test value of the coated alloy to be tested and a Larson-Miller curve of the bare alloy, and obtain a stress value corresponding to the Larson-Miller parameter value, and use the stress value as the equivalent stress of the coated alloy to be tested;
[0024] an equivalent bearing area determining unit for the coated alloy to be tested, configured to determine the equivalent bearing area of the coated alloy to be tested according to the equivalent stress; the equivalent bearing area of the coated alloy to be tested is the bearing area of the bare alloy equivalent to that of the coated alloy to be tested;
[0025] The coating-containing alloy to be tested rupture / creep life prediction unit is used to predict the rupture / creep life of the coating-containing alloy to be tested under different temperature and stress conditions according to the equivalent bearing area of the coating-containing alloy to be tested.
[0026] Optionally, the expression of the bare alloy Larson-Miller parameter is:
[0027] P = T (C + lgτ);
[0028] Where P is the Larson-Miller parameter of the bare alloy, T is the absolute temperature, τ is the rupture / creep life of the alloy, and C is a constant related to the alloy material.
[0029] Optionally, the calculation formula for the equivalent load-bearing area of the coated alloy to be tested is:
[0030] S′0=S0*σ / σ′;
[0031] S0=S1+S2;
[0032] Wherein, S′0 is the equivalent bearing area of the coated alloy to be tested, S0 is the total cross-sectional area of the coated alloy to be tested, σ is the test stress value of the coated alloy to be tested, σ′ is the equivalent stress value of the coated alloy to be tested, S1 is the coating cross-sectional area of the coated alloy to be tested, and S2 is the substrate cross-sectional area of the coated alloy to be tested.
[0033] According to the specific embodiments provided by the present invention, the present invention discloses the following technical effects:
[0034] The present invention provides a method and system for predicting the high-temperature rupture / creep life of a coated high-temperature alloy. The method obtains bare alloy performance parameter data and establishes a Larson-Miller curve for the bare alloy based on the bare alloy performance parameter data. The method then obtains test values of the rupture / creep life of the coated alloy under test temperature and test stress conditions. Based on the test values and the Larson-Miller curve, Larson-Miller parameter values are determined. Stress values corresponding to the Larson-Miller parameter values are then obtained. The stress values are used as the equivalent stress of the coated alloy. Based on the equivalent stress, the equivalent bearing area of the coated alloy is determined. Based on the equivalent bearing area, the rupture / creep life of the coated alloy under different temperature and stress conditions is predicted. The method shortens testing time, reduces costs, and provides highly reliable prediction results. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0036] Figure 1 This is a flow chart of a method for predicting the high-temperature rupture / creep life of a coated high-temperature alloy according to the present invention;
[0037] Figure 2 Schematic diagram of the Larson-Miller curve of the bare alloy of the present invention;
[0038] Figure 3Schematic diagram of the relationship between the coating cross-sectional area, substrate cross-sectional area and total cross-sectional area of the present invention;
[0039] Figure 4 This is a schematic diagram of the module structure of a prediction system for high-temperature rupture / creep life of a coated high-temperature alloy according to the present invention.
[0040] Explanation of symbols:
[0041] Unit 1: Establishing Larson-Miller curve of bare alloy; Unit 2: Obtaining test value of rupture / creep life of coated alloy; Unit 3: Determining equivalent stress of coated alloy; Unit 4: Determining equivalent bearing area of coated alloy; Unit 5: Predicting rupture / creep life of coated alloy. DETAILED DESCRIPTION
[0042] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0043] The purpose of the present invention is to provide a method and system for predicting the high-temperature rupture / creep life of coated high-temperature alloys, which can solve the problem that bare alloy performance test data cannot be directly used for coating alloy performance evaluation.
[0044] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0045] Thermal barrier coatings are functional coatings typically consisting of a thermally insulating ceramic layer and a metal bonding layer. Deposited on the surface of high-temperature metals or high-temperature alloys, they act as a thermal insulator, lowering the substrate's surface temperature and allowing it to operate at higher temperatures for extended periods.
[0046] Metal bonding layer: a metal coating located between the ceramic insulation layer and the base material in the thermal barrier coating. On the one hand, it improves the mismatch in thermal expansion coefficients between the metal base and the ceramic surface layer, and on the other hand, it improves the high-temperature oxidation resistance of the base material.
[0047] High-temperature alloy: refers to a type of metal material based on iron, nickel and cobalt, which can work for a long time at high temperatures above 600°C and under certain stress. It has excellent high-temperature strength, good oxidation resistance and thermal corrosion resistance, good fatigue performance, fracture toughness and other comprehensive properties. It is mainly used in the aerospace and energy fields.
[0048] Endurance / creep life: refers to the time from the beginning of deformation to the occurrence of fracture when a material is subjected to a constant load at a certain temperature.
[0049] Creep: The phenomenon in which a solid material's strain increases over time while maintaining a constant stress. The creep test is similar to the endurance test, except that the strain of the material is recorded over time.
[0050] Larson-Miller method: It is a method for predicting the endurance / creep life of materials. This method believes that the endurance strength of the material is determined by the temperature-time parameter P, which is called the Larson-Miller parameter. Its value P=T(C+lgτ), where T is the absolute temperature, τ is the fracture time, and C is a constant related to the material.
[0051] Larson-Miller curve: The curve obtained by fitting all the endurance / creep data points in the coordinate system with the endurance / creep stress as the vertical coordinate and the Larson-Miller parameter P as the horizontal coordinate.
[0052] like Figure 1 As shown, the present invention provides a method for predicting the high-temperature rupture / creep life of a coated high-temperature alloy, comprising the following steps:
[0053] S1: Obtain bare alloy performance parameter data, and establish a bare alloy Larson-Miller curve based on the bare alloy performance parameter data; the bare alloy performance parameter data includes temperature, stress and bare alloy endurance / creep life data under corresponding temperature and stress; wherein, at least three sets of temperature / stress / bare alloy endurance / creep life data are included. Bare alloy Larson-Miller curve is as follows Figure 2 shown.
[0054] S2: Obtain the rupture / creep life test value of the coated alloy under the test temperature and test stress conditions. Specifically, before predicting the life of the coated alloy, it is necessary to evaluate the effect of the coating material (coating cross-sectional area S1, substrate cross-sectional area S2, total cross-sectional area S0) on the mechanical properties of the alloy. Therefore, it is necessary to test the rupture / creep life of the coated alloy under at least one temperature / stress (T / σ). The relationship diagram of the coating cross-sectional area, substrate cross-sectional area and total cross-sectional area is shown in the figure below. Figure 3 .
[0055] S3: Determine a Larson-Miller parameter value based on the rupture / creep life test value of the coated alloy to be tested and the Larson-Miller curve of the bare alloy, and obtain a stress value corresponding to the Larson-Miller parameter value, and use the stress value as the equivalent stress of the coated alloy to be tested.
[0056] S4: determining an equivalent load-bearing area of the coated alloy to be tested according to the equivalent stress; the equivalent load-bearing area of the coated alloy to be tested is the load-bearing area of the bare alloy equivalent to that of the coated alloy to be tested.
[0057] S5: Predicting the rupture / creep life of the coated alloy under different temperature and stress conditions based on the equivalent load-bearing area of the coated alloy.
[0058] Furthermore, when the rupture / creep life of multiple coated alloys to be tested is obtained based on multiple sets of temperature / stress (T / σ), the equivalent load-bearing area of the coated alloy to be tested corresponding to each set of data is calculated respectively, and then the equivalent load-bearing area of the coated alloy to be tested obtained in each group is averaged to obtain the average value of the equivalent load-bearing area of the coated alloy to be tested, which is used as the equivalent load-bearing area of the coated alloy to be tested, and the rupture / creep life of the coated alloy to be tested under subsequent different temperature and stress conditions is predicted.
[0059] Furthermore, when predicting the rupture / creep life of the coated alloy under the T1 / σ1 parameter, the equivalent bearing area of the coated alloy has been calculated to be S0'. At this time, the equivalent stress σ1'=σ1*S0 / S0'. After obtaining the equivalent stress σ1', it is only necessary to Figure 2 The P1 value corresponding to σ1' is read on the Larson-Miller curve. Since P1 is a function of temperature T1 and rupture / creep life τ1, the predicted rupture / creep life τ1 of the coated alloy under T1 / σ1 parameters can be calculated if the values of P1 and T1 are known.
[0060] Furthermore, if Figure 4 As shown, the present invention also provides a prediction system for the high-temperature rupture / creep life of a coated high-temperature alloy, the prediction system comprising: a bare alloy Larson-Miller curve establishment unit 1, a rupture / creep life test value acquisition unit 2 for the coated alloy to be tested, an equivalent stress determination unit 3 for the coated alloy to be tested, an equivalent bearing area determination unit 4 for the coated alloy to be tested, and a rupture / creep life prediction unit 5 for the coated alloy to be tested.
[0061] A bare alloy Larson-Miller curve establishing unit 1 is used to obtain bare alloy performance parameter data and establish a bare alloy Larson-Miller curve based on the bare alloy performance parameter data; the bare alloy performance parameter data includes temperature, stress and bare alloy rupture / creep life data under corresponding temperature and stress;
[0062] The coating-containing alloy to be tested rupture / creep life test value acquisition unit 2 is used to obtain the coating-containing alloy to be tested rupture / creep life test value of the coating-containing alloy to be tested under test temperature and test stress conditions.
[0063] The coated alloy to be tested equivalent stress determination unit 3 is used to determine the Larson-Miller parameter value based on the rupture / creep life test value of the coated alloy to be tested and the Larson-Miller curve of the bare alloy, and obtain the stress value corresponding to the Larson-Miller parameter value, and use the stress value as the equivalent stress of the coated alloy to be tested.
[0064] The equivalent load-bearing area determination unit 4 of the coated alloy to be tested is used to determine the equivalent load-bearing area of the coated alloy to be tested according to the equivalent stress; the equivalent load-bearing area of the coated alloy to be tested is the load-bearing area of the bare alloy equivalent to that of the coated alloy to be tested.
[0065] The coated alloy life prediction unit 5 is used to predict the rupture / creep life of the coated alloy under different temperature and stress conditions according to the equivalent bearing area of the coated alloy.
[0066] Furthermore, the expression of the bare alloy Larson-Miller parameter is:
[0067] P = T (C + lgτ);
[0068] Where P is the Larson-Miller parameter of the bare alloy, T is the absolute temperature, τ is the rupture / creep life of the alloy, and C is a constant related to the alloy material.
[0069] Furthermore, the calculation formula for the equivalent bearing area of the coated alloy to be tested is:
[0070] S′0=S0*σ / σ′;
[0071] S0=S1+S2;
[0072] Wherein, S′0 is the equivalent bearing area of the coated alloy to be tested, S0 is the total cross-sectional area of the coated alloy to be tested, σ is the test stress value of the coated alloy to be tested, σ′ is the equivalent stress value of the coated alloy to be tested, S1 is the coating cross-sectional area of the coated alloy to be tested, and S2 is the substrate cross-sectional area of the coated alloy to be tested. Specific embodiments
[0074] Table 1 Comparison of rupture / creep life and equivalent stress / bearing area of high-temperature alloys with four different metal bonding layers
[0075]
[0076] Table 1 shows the equivalent stress and equivalent bearing area of a coated alloy obtained by calculating the high-temperature rupture / creep life prediction method of the coated high-temperature alloy according to the present invention after coating four different metal bonding layers (with the same thickness) on a certain nickel-based high-temperature alloy. The cross-section of the coated alloy is 3 mm long, 1 mm wide, the coating thickness is 40 μm, and the total cross-sectional area S0 is 3 mm. 2 The test temperature / stress (T / σ) for the coated alloys was 1100°C / 100 MPa. Based on the equivalent areas obtained for the four coated alloys, their rupture and creep lives under other T1 / σ1 conditions can be predicted. The rupture and creep lives of these four coated alloys at 1100°C / 90 MPa were predicted and compared with the measured values. The results are shown in Appendix 2. The results demonstrate that this method accurately predicts the life of the coated alloys, with errors within 5% of the measured values.
[0077] Table 2 Comparison of predicted and measured values of rupture / creep life of high-temperature alloys with four different metal bonding layers
[0078]
[0079] The technical effect of the present invention is that the present invention only needs to test the rupture / creep life of the coated alloy under one temperature / stress. Combined with the rupture / creep life data of the bare alloy, the rupture / creep life of the coated alloy under different temperatures / stresses can be accurately predicted. The test time and cost are low, and in the test examples, excellent prediction accuracy is demonstrated, with relative errors within 4%, and the reliability of the prediction results is high.
[0080] In addition, this method can distinguish the effects of different coatings. (The prior art (2) does not consider the type of coating, but only considers the reduction in the cross-sectional area of the substrate after coating.) The results in Table 1 show that different types of coatings of the same thickness also have different effects on the rupture / creep life of the coated alloy. This method can take this effect into account, and the results are applicable to more coating / alloy systems and have higher accuracy.
[0081] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments. Reference can be made to the common and similar parts between the various embodiments. For the systems disclosed in the embodiments, since they correspond to the methods disclosed in the embodiments, the description is relatively simple, and the relevant parts can be referred to the method description.
[0082] This document uses specific examples to illustrate the principles and implementation methods of the present invention. The above examples are only intended to help understand the method and core concept of the present invention. At the same time, those skilled in the art will find that the specific implementation methods and application scopes may vary based on the concept of the present invention. In summary, the contents of this specification should not be construed as limiting the present invention.
Claims
1. A method for predicting high temperature rupture / creep life of a coated high temperature alloy, characterized in that: The prediction method comprises: Obtaining bare alloy performance parameter data, and establishing a bare alloy Larson-Miller curve according to the bare alloy performance parameter data; the bare alloy performance parameter data includes temperature, stress and bare alloy rupture / creep life data under corresponding temperature and stress; Obtaining a rupture / creep life test value of the coated alloy under test temperature and test stress conditions; Determine the Larson-Miller parameter value according to the rupture / creep life test value of the coated alloy to be tested and the Larson-Miller curve of the bare alloy, obtain the stress value corresponding to the Larson-Miller parameter value, and use the stress value as the equivalent stress of the coated alloy to be tested; According to the equivalent stress, determining the equivalent load-bearing area of the coated alloy to be tested; the equivalent load-bearing area of the coated alloy to be tested is the load-bearing area of the bare alloy equivalent to the coated alloy to be tested; According to the equivalent load-bearing area of the coated alloy to be tested, predicting the rupture / creep life of the coated alloy to be tested under different temperature and stress conditions; The calculation formula for the equivalent bearing area of the coated alloy to be tested is: S0′=S0*σ / σ′; S0=S1+S2; Wherein, S0′ is the equivalent bearing area of the coated alloy to be tested, S0 is the total cross-sectional area of the coated alloy to be tested, σ is the test stress value of the coated alloy to be tested, σ′ is the equivalent stress value of the coated alloy to be tested, S1 is the coating cross-sectional area of the coated alloy to be tested, and S2 is the substrate cross-sectional area of the coated alloy to be tested.
2. The method for predicting high temperature rupture / creep life of coated high temperature alloy according to claim 1, characterized in that: The expression of the bare alloy Larson-Miller parameter is: P = T (C + lgτ); Wherein, P is the Larson-Miller parameter of bare alloy, T is the absolute temperature, τ is the rupture / creep life of alloy, and C is a constant related to alloy material.
3. A prediction system for high temperature rupture / creep life of coated high temperature alloys, characterized in that: The prediction system comprises: A bare alloy Larson-Miller curve establishing unit, used for acquiring bare alloy performance parameter data, and establishing a bare alloy Larson-Miller curve according to the bare alloy performance parameter data; the bare alloy performance parameter data includes temperature, stress and bare alloy rupture / creep life data under corresponding temperature and stress; A unit for acquiring a rupture / creep life test value of the coated alloy to be tested, used for acquiring a rupture / creep life test value of the coated alloy to be tested under test temperature and test stress conditions; The coated alloy to be tested equivalent stress determination unit is used to determine the Larson-Miller parameter value according to the rupture / creep life test value of the coated alloy to be tested and the Larson-Miller curve of the bare alloy, and obtain the stress value corresponding to the Larson-Miller parameter value, and use the stress value as the equivalent stress of the coated alloy to be tested; The equivalent load-bearing area determination unit of the coated alloy to be tested is used to determine the equivalent load-bearing area of the coated alloy to be tested according to the equivalent stress; the equivalent load-bearing area of the coated alloy to be tested is the load-bearing area of the bare alloy equivalent to the coated alloy to be tested; the calculation formula of the equivalent load-bearing area of the coated alloy to be tested is: S0′=S0*σ / σ′; S0=S1+S2; Wherein, S0′ is the equivalent bearing area of the alloy to be tested containing the coating, S0 is the total cross-sectional area of the alloy to be tested containing the coating, σ is the test stress value of the alloy to be tested containing the coating, σ′ is the equivalent stress value of the alloy to be tested containing the coating, S1 is the coating cross-sectional area of the alloy to be tested containing the coating, and S2 is the substrate cross-sectional area of the alloy to be tested containing the coating; The coating-containing alloy to be tested rupture / creep life prediction unit is used to predict the rupture / creep life of the coating-containing alloy to be tested under different temperature and stress conditions according to the equivalent load-bearing area of the coating-containing alloy to be tested.
4. The prediction system for high temperature rupture / creep life of coated high temperature alloy according to claim 3, characterized in that: The expression of the bare alloy Larson-Miller parameter is: P = T (C + lgτ); Wherein, P is the Larson-Miller parameter of bare alloy, T is the absolute temperature, τ is the rupture / creep life of alloy, and C is a constant related to alloy material.
Citation Information
Patent Citations
Fatigue creep interaction damage gas turbine blade service life evaluation model
CN112001046A
Heat-resistant steel creep life prediction method based on M-H method
CN113252465A
Lifetime estimation method of nickel-based alloy component
JP2009074857A