Pretreatment method and recycling method of waste battery black powder
Through alkaline leaching treatment and solid-liquid separation technology, the problem of low recovery efficiency of aluminum elements in waste battery black powder is solved, efficient recovery of metal and carbon elements is achieved, the output of waste residue is reduced, and the added value of the product is increased.
Patent Information
- Application Number
- CN202210233705.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-09
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-03-09
AI Technical Summary
Existing waste battery black powder recycling and treatment methods are difficult to effectively recover aluminum elements, resulting in problems such as large waste residue production and low added value of products.
Use an alkaline leaching agent to perform alkaline leaching treatment on waste battery black powder. Light phase slag, liquid phase products and heavy phase slag are obtained through solid-liquid separation. The density difference is used for separation to increase the recovery rate of aluminum elements and pass Bayer The liquid phase product is treated with the method to obtain alumina, the light phase slag is collected as carbon material, and the valuable metals in the heavy phase slag are extracted.
It improves the separation efficiency of metal elements and carbon elements in waste battery black powder, increases the recovery rate of valuable metals and carbon, reduces the output of waste residue, and increases the added value of the product.
Smart Images

Figure BDA0003539447320000071 
Figure BDA0003539447320000082
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of recycling waste batteries, and in particular to a method for pretreating and recycling black powder from waste batteries. Background Art
[0002] Waste battery black powder is a black powder containing metals such as nickel, cobalt, manganese, copper, aluminum, lithium and carbon powder obtained by disassembling, crushing, screening, pyrolysis and sorting of waste lithium-ion batteries.
[0003] Existing literature (publication number CN111519031A) provides a method for recovering nickel, cobalt, manganese and lithium from waste power lithium-ion battery black powder. The method directly performs reduction leaching (sulfuric acid and SO2) on the battery black powder to obtain a leached slag with carbon powder as the main component and a leachate mainly composed of various metals, and then lime milk is added to the leachate to obtain a lithium-containing solution and a nickel, cobalt and manganese enrichment. The lithium-containing solution is added with carbonate to precipitate lithium to obtain crude lithium carbonate, and the nickel, cobalt and manganese enrichment is then leached-iron aluminum removal-P204 manganese extraction-P507 cobalt extraction-P507 nickel extraction-evaporation crystallization, manganese precipitation and other processes to obtain manganese carbonate, cobalt sulfate and nickel sulfate respectively. The method improves the recovery rate of lithium, the process is mature and stable, and the product quality is good. However, the process is subjected to two leaching processes, and the acid and alkali consumption is large. At the same time, most of the aluminum in the black powder enters the iron-aluminum slag, resulting in a large amount of slag and low product added value.
[0004] Existing literature (publication number CN112374511A) provides a method for recycling waste ternary lithium batteries to prepare lithium carbonate and ternary precursors. This method uses graphite and binder in black powder as reducing agents to first leach lithium under alkaline conditions, and the leachate is then concentrated by evaporation and bubbling carbon dioxide to precipitate lithium. The leached residue is subjected to acid leaching-copper removal-iron and aluminum removal-calcium and magnesium removal-extraction to obtain a mixed solution of nickel sulfate, cobalt sulfate and manganese sulfate. This method has a short process flow, a high recovery rate of valuable metals, and good product quality. However, this method produces a large amount of copper slag, iron and aluminum slag and fluoride slag, which puts great pressure on environmental protection.
[0005] The existing document (publication number CN112207119A) discloses a method for treating battery powder. The method first uses diethanolamine to destroy the binder, and then leaches the ore pulp - removes iron and aluminum - extracts to obtain a stripping solution containing nickel, cobalt, and manganese and a raffinate containing lithium. The process flow of this method is short, and valuable elements such as nickel, cobalt, manganese, lithium, copper, and carbon are all recycled. However, the introduction of organic matter in this method causes certain difficulties in subsequent solution treatment, and the aluminum element is not effectively recovered, and the amount of iron and aluminum slag is large.
[0006] In the above-mentioned process using direct acid leaching, due to the large amount of carbon and aluminum elements in the black powder, the concentrations of nickel, cobalt, manganese and other elements in the leaching solution are low, the equipment is large-scale, the investment is high, the subsequent evaporation of water is large, and the operating cost is high; at the same time, due to the presence of aluminum elements in the black powder, a large amount of acid and alkali is consumed during leaching and iron and aluminum removal, and the added value of the product is low.
[0007] On this basis, it is necessary to research and develop a pretreatment method and recycling method for waste battery black powder that can effectively recycle aluminum elements, have low waste slag output and high product added value. Summary of the invention
[0008] The main purpose of the present invention is to provide a pretreatment method and a recovery method for waste battery black powder, so as to solve the problems in the prior art that the recovery method for waste battery black powder is difficult to effectively recover aluminum elements, and the waste slag output is large and the product added value is low.
[0009] In order to achieve the above-mentioned object, the present invention provides a method for pretreating waste battery black powder, which comprises: using an alkaline leaching agent to perform alkaline leaching treatment on the waste battery black powder to obtain a slurry; the alkaline leaching agent is a dispersion of a strong alkaline compound, and the weight concentration of the alkaline leaching agent is 20-50%; the waste battery black powder includes active ingredients, aluminum elements, copper elements and carbon elements, wherein the active ingredients include one or more of lithium elements, nickel elements, cobalt elements and manganese elements; the slurry is subjected to solid-liquid separation treatment to obtain light phase slag, liquid phase product and heavy phase slag in sequence from top to bottom, wherein the difference between the density of the liquid phase product and the density of the light phase slag is greater than 0 and less than or equal to 0.3 g / cm 3 The difference between the density of the liquid phase product and the density of the heavy phase slag is 3.3-3.9 g / cm 3 The heavy phase slag includes active components and copper elements; the light phase slag includes carbon elements; the liquid phase product includes 0.3-2.6% aluminum elements in terms of weight percentage of the liquid phase product.
[0010] Furthermore, in terms of weight percentage of the waste battery black powder, the waste battery black powder includes 30-55% active ingredients, 2-8% aluminum elements, 1-3% copper elements, 7-18% carbon elements and the remainder impurity elements.
[0011] Furthermore, the heavy phase slag includes 40-60% active ingredients, 1-4% copper, 0.1-0.5% aluminum, 0.1-0.5% carbon and the remainder impurity elements in terms of weight percentage of the heavy phase slag; the light phase slag includes 0.1-0.5% active ingredients, 0-0.1% copper, 0.5-2% aluminum, 85-95% carbon and the remainder impurity elements in terms of weight percentage of the light phase slag.
[0012] Furthermore, the strong alkaline compound is sodium hydroxide.
[0013] Furthermore, the temperature of the alkaline leaching treatment process is 50-100° C. and the time is 1-4 hours.
[0014] Furthermore, the liquid-to-solid ratio of the alkaline leaching treatment process is (3-6):1.
[0015] Furthermore, the solid-liquid separation process is a centrifugal separation process.
[0016] Furthermore, the centrifugal separation treatment is carried out using a decanter centrifuge, and the separation factor of the decanter centrifuge is 500-3000.
[0017] Furthermore, the particle size of the waste battery black powder is 74 to 178 μm.
[0018] In order to achieve the above-mentioned purpose, another aspect of the present invention further provides a method for recycling waste battery black powder, which comprises: adopting the above-mentioned pretreatment method of waste battery black powder provided in the present application to obtain heavy phase slag, light phase slag and liquid phase product; adopting the Bayer process to treat the liquid phase product to obtain alumina; collecting the light phase slag, and obtaining carbon material after washing; collecting the heavy phase slag, and obtaining nickel sulfate and / or cobalt sulfate and / or manganese sulfate, copper and lithium carbonate after extraction and recovery.
[0019] By applying the technical solution of the present invention and adopting the above-mentioned pretreatment method of waste battery black powder, the separation efficiency of metal elements (such as nickel, cobalt, manganese, lithium and copper) and carbon and aluminum elements in waste battery black powder can be greatly improved, which is convenient for the subsequent further extraction and recovery of the above-mentioned elements, thereby improving the recovery rate of valuable metals and carbon, reducing the output of waste slag, and being beneficial to increasing the added value of waste battery black powder. DETAILED DESCRIPTION
[0020] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0021] As described in the background technology, the existing recycling and treatment methods of waste battery black powder have the problems of difficulty in effectively recovering aluminum elements, large waste slag output and low product added value. In order to solve the above technical problems, the present application provides a pretreatment method for waste battery black powder, which comprises: using an alkaline leaching agent to perform alkaline leaching treatment on the waste battery black powder to obtain a slurry; the alkaline leaching agent is a dispersion of a strong alkaline compound, and the weight concentration of the alkaline leaching agent is 20-50%; the waste battery black powder includes active ingredients, aluminum elements, copper elements and carbon elements, wherein the active ingredients include one or more of lithium elements, nickel elements, cobalt elements and manganese elements; the slurry is subjected to solid-liquid separation treatment to obtain light phase slag, liquid phase product and heavy phase slag from top to bottom, wherein the difference between the density of the liquid phase product and the density of the light phase slag is greater than 0 and less than or equal to 0.3g / cm 3 The difference between the density of the liquid phase product and the density of the heavy phase slag is 3.3-3.9 g / cm 3 The heavy phase slag includes active components and copper elements; the light phase slag includes carbon elements; the liquid phase product includes 0.3-2.6% aluminum elements in terms of weight percentage of the liquid phase product.
[0022] The waste battery black powder is subjected to alkaline leaching treatment using an alkaline leaching agent (a dispersion of a strong alkaline compound) of a specific weight concentration. During the alkaline leaching treatment process, the aluminum element reacts with the strong alkaline compound to generate a soluble aluminum-containing salt, while the carbon element, copper element and positive electrode active material (such as nickel cobalt manganese oxide positive electrode material, nickel cobalt aluminum oxide positive electrode material, lithium cobalt oxide positive electrode material, etc.) in the waste battery black powder do not react with the alkaline leaching agent and exist in a solid phase. The aluminum salt, carbon element, copper element and positive electrode active material jointly participate in forming a slurry. Since an alkaline leaching agent of a specific concentration is used, after solid-liquid separation treatment, light phase slag, heavy phase slag and liquid phase product can be obtained in sequence from top to bottom. Among them, the soluble aluminum-containing salt exists in the liquid phase product, the carbon element exists in the light phase slag, and the positive electrode active material exists in the heavy phase slag.
[0023] Compared with alkaline leaching agents of other concentrations, the use of the above-mentioned specific concentration of alkaline leaching agent is beneficial to increasing the density difference between the liquid phase product and the light phase slag, thereby helping to improve the separation efficiency of the light phase slag containing carbon elements and the liquid phase product containing aluminum elements, and realizing the preferential extraction of aluminum elements; at the same time, it is beneficial to improve the separation efficiency of the heavy phase slag containing active ingredients and copper elements and the liquid phase product containing aluminum elements, and thus helping to improve the subsequent recovery rate of aluminum elements.
[0024] The above-mentioned pretreatment method of waste battery black powder can greatly improve the separation efficiency of metal elements (such as nickel, cobalt, manganese, lithium and copper) from carbon and aluminum in waste battery black powder, which is convenient for the subsequent further extraction and recycling of the above-mentioned elements, thereby improving the recovery rate of valuable metals and carbon, reducing the output of waste residue, and helping to increase the added value of waste battery black powder. The above-mentioned pretreatment method is particularly suitable for the recovery and extraction of aluminum.
[0025] In a preferred embodiment, the waste battery black powder includes 30-55% active ingredients, 2-8% aluminum, 1-3% copper, 7-18% carbon and the remainder of impurity elements, in terms of weight percentage of the waste battery black powder. The pretreatment method of waste battery black powder provided in the present application is more targeted to waste battery black powder containing the above components, which is conducive to further improving the separation efficiency of metal elements (such as nickel, cobalt, manganese, lithium and copper) from carbon and aluminum in the waste battery black powder.
[0026] In a preferred embodiment, the heavy phase slag includes 40-60% active ingredients, 1-4% copper, 0.1-0.5% aluminum, 0.1-0.5% carbon and the remainder of impurity elements, based on the weight percentage of the heavy phase slag. The heavy phase slag has a high content of active ingredients and copper elements, while the aluminum and carbon elements are almost zero, which facilitates the subsequent collection of valuable elements in the heavy phase slag for extraction and recovery, thereby further improving the recovery rate of valuable metals, reducing the output of waste slag, and helping to further increase the added value of waste battery black powder. For example, conventional reduction leaching-chemical purification-extraction-evaporation crystallization methods can be used to obtain battery-grade nickel sulfate, battery-grade cobalt sulfate and battery-grade manganese sulfate respectively; copper elements are collected and cathode copper is obtained by copper extraction-electrodeposition; and a crude product of lithium carbonate is obtained after lithium carbonate precipitation.
[0027] In a preferred embodiment, the light phase slag includes 0.1-0.5% active ingredients, 0-0.1% copper, 0.5-2% aluminum, 85-95% carbon and the remainder of impurity elements, in terms of weight percentage of the light phase slag. The carbon content in the light phase slag is relatively high, while the content of active ingredients, copper and aluminum is almost zero, which facilitates the subsequent collection of carbon in the light phase slag, which can be directly recycled as anode material or directly sold as fuel after washing, which is conducive to further improving the recovery rate of carbon, reducing the output of waste slag, and further improving the added value of waste battery black powder.
[0028] In a preferred embodiment, the strong alkaline compound is sodium hydroxide. The use of the above-mentioned alkaline leaching agent is conducive to more efficiently reacting aluminum with it to generate soluble aluminum salts, while the carbon, copper and positive electrode active materials (such as nickel cobalt manganese oxide positive electrode materials, nickel cobalt aluminum oxide positive electrode materials, lithium cobalt oxide positive electrode materials, etc.) in the waste battery black powder do not react with the alkaline leaching agent and still exist in a solid phase.
[0029] In a preferred embodiment, the temperature of the alkaline leaching treatment process is 50-100°C and the time is 1-4 hours. The temperature and time of the alkaline leaching treatment process include but are not limited to the above ranges. Limiting them within the above ranges is conducive to increasing the reaction rate of the aluminum element and the strong alkaline compound to generate a soluble aluminum salt, thereby helping to improve the efficiency of the pretreatment of waste battery black powder.
[0030] In a preferred embodiment, the liquid-to-solid ratio of the alkaline leaching treatment process is (3-6): 1. The liquid-to-solid ratio of the alkaline leaching treatment process includes but is not limited to the above range. Limiting it within the above range is conducive to the waste battery black powder and the alkaline leaching agent to fully contact and react, which is conducive to making the reaction more thorough, so that more aluminum elements in the waste battery black powder form soluble aluminum salts, which is conducive to the subsequent enrichment and extraction and recovery of aluminum elements.
[0031] In a preferred embodiment, the solid-liquid separation treatment is a centrifugal separation treatment. Compared with other solid-liquid separation treatment methods, the centrifugal separation treatment is conducive to the separation of solid and liquid phases of materials with different densities under the action of centrifugal force. In order to further improve the effect of solid-liquid separation, improve the separation efficiency of light phase slag containing carbon elements and liquid phase products containing aluminum elements, and at the same time, it is conducive to improving the separation efficiency between heavy phase slag containing active ingredients and copper elements and liquid phase products containing aluminum elements. Preferably, the centrifugal separation treatment is carried out using a sedimentation centrifuge, and the separation factor of the sedimentation centrifuge is 500 to 3000.
[0032] In a preferred embodiment, the particle size of the waste battery black powder is 74 to 178 μm. The particle size of the waste battery black powder includes but is not limited to the above range. Limiting it within the above range is conducive to increasing the specific surface area of the waste battery black powder, thereby increasing its contact area with the alkaline leaching agent, making the alkaline leaching process more sufficient; at the same time, it is conducive to speeding up the alkaline leaching treatment speed, thereby saving time and facilitating batch processing of waste battery black powder.
[0033] The second aspect of the present application also provides a method for recycling waste battery black powder, which comprises: adopting the above-mentioned pretreatment method of waste battery black powder provided in the present application to obtain heavy phase slag, light phase slag and liquid phase product; adopting the Bayer process to treat the liquid phase product to obtain alumina; collecting the light phase slag, and obtaining carbon material after washing; collecting the heavy phase slag, and obtaining nickel sulfate and / or cobalt sulfate and / or manganese sulfate, copper and lithium carbonate after extraction and recovery.
[0034] The pretreatment method of the above-mentioned waste battery black powder provided in the present application has good separation efficiency and can well separate the heavy phase slag, light phase slag and liquid phase product. For example, the liquid phase product is treated by the Bayer process to obtain aluminum oxide; the conventional reduction leaching-chemical purification-extraction-evaporation crystallization method can be used to obtain battery-grade nickel sulfate, battery-grade cobalt sulfate and battery-grade manganese sulfate respectively; the copper element is collected and cathode copper is obtained by copper extraction-electrodeposition; the crude product of lithium carbonate is obtained after lithium carbonate precipitation.
[0035] In an optional embodiment, the liquid phase product is treated by the Bayer process to obtain an aluminum-extracted liquid, and the aluminum-extracted liquid is returned to the reaction system of the alkaline leaching treatment to participate in the alkaline leaching treatment. In order to improve the recovery rate of the aluminum element, preferably, the aluminum-extracted liquid includes 0.3-2.6% aluminum element in terms of weight percentage of the aluminum-extracted liquid.
[0036] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0037] Example 1
[0038] A method for pretreating waste battery black powder, comprising:
[0039] The particle size of the waste battery black powder used in this embodiment is 150 μm, and the weight percentage of each element is shown in Table 1.
[0040] Table 1
[0041] Element Type Ni Co Mn element Li element Cu Al element C element Content (wt%) 12.5 5.0 7.0 3.0 2.3 6.8 16.0
[0042] The alkaline leaching agent used in this embodiment is sodium hydroxide, the weight concentration of the sodium hydroxide solution is 20%, and the separation factor of the decanter centrifuge is 500.
[0043] The above-mentioned sodium hydroxide solution is used to perform alkaline leaching treatment on the above-mentioned type of waste battery black powder to obtain a slurry. In this process, the temperature of the alkaline leaching process is 100° C., the time is 4 hours, and the liquid-to-solid ratio is 3:1.
[0044] The slurry is centrifuged to obtain light phase slag, liquid phase product and heavy phase slag from top to bottom. The difference between the density of the liquid phase product and the density of the light phase slag is 0.1 g / cm 3 The difference between the density of the liquid phase product and the density of the heavy phase slag is 3.8 g / cm 3 .
[0045] The test results show that the content of aluminum in the liquid phase product is 2.26% in terms of weight percentage of the liquid phase product; the content of each element in the heavy phase slag is shown in Table 2, and the content of each element in the light phase slag is shown in Table 3.
[0046] Example 2
[0047] The difference from Example 1 is that the weight concentration of the sodium hydroxide solution is 50%; the density of the liquid product is 1.5 g / cm 3 .
[0048] The test results show that the content of aluminum in the liquid phase product is 2.26% in terms of weight percentage of the liquid phase product; the content of each element in the heavy phase slag is shown in Table 2, and the content of each element in the light phase slag is shown in Table 3.
[0049] Example 3
[0050] The difference from Example 1 is that the weight concentration of the sodium hydroxide solution is 37%; the difference between the density of the liquid phase product and the density of the light phase slag is 0.2 g / cm 3 The difference between the density of the liquid phase product and the density of the heavy phase slag is 3.7 g / cm 3 .
[0051] The test results show that the content of aluminum in the liquid phase product is 2.26% in terms of weight percentage of the liquid phase product; the content of each element in the heavy phase slag is shown in Table 2, and the content of each element in the light phase slag is shown in Table 3.
[0052] Example 4
[0053] The difference from Example 1 is that the temperature of the alkaline leaching treatment process is 50° C. and the time is 1 hour.
[0054] The test results show that the content of aluminum in the liquid phase product is 2.26% in terms of weight percentage of the liquid phase product; the content of each element in the heavy phase slag is shown in Table 2, and the content of each element in the light phase slag is shown in Table 3.
[0055] Example 5
[0056] The difference from Example 1 is that the temperature of the alkaline leaching treatment process is 30° C. and the time is 0.5 h.
[0057] The test results show that the content of aluminum in the liquid phase product is 1.21% in terms of weight percentage of the liquid phase product; the content of each element in the heavy phase slag is shown in Table 2, and the content of each element in the light phase slag is shown in Table 3.
[0058] Example 6
[0059] The difference from Example 1 is that the liquid-to-solid ratio in the alkaline leaching treatment process is 6:1.
[0060] The test results show that the content of aluminum in the liquid phase product is 1.13% in terms of weight percentage of the liquid phase product; the content of each element in the heavy phase slag is shown in Table 2, and the content of each element in the light phase slag is shown in Table 3.
[0061] Example 7
[0062] The difference from Example 1 is that the liquid-to-solid ratio in the alkaline leaching treatment process is 1:1.
[0063] The test results show that the content of aluminum in the liquid phase product is 6.0% in terms of weight percentage of the liquid phase product; the content of each element in the heavy phase slag is shown in Table 2, and the content of each element in the light phase slag is shown in Table 3.
[0064] Example 8
[0065] The difference from Example 1 is that the separation factor of the decanter centrifuge is 3000.
[0066] The test results show that the content of aluminum in the liquid phase product is 2.26% in terms of weight percentage of the liquid phase product; the content of each element in the heavy phase slag is shown in Table 2, and the content of each element in the light phase slag is shown in Table 3.
[0067] Example 9
[0068] The difference from Example 1 is that the separation factor of the decanter centrifuge is 300.
[0069] The test results show that the content of aluminum in the liquid phase product is 2.02% in terms of weight percentage of the liquid phase product; the content of each element in the heavy phase slag is shown in Table 2, and the content of each element in the light phase slag is shown in Table 3.
[0070] Example 10
[0071] The difference from Example 1 is that the weight concentration of the sodium hydroxide solution is 45%; the separation factor of the decanter centrifuge used is 2000; the temperature of the alkaline leaching process is 75° C., the time is 2 h, and the liquid-to-solid ratio is 4:1.
[0072] The test results show that the content of aluminum in the liquid phase product is 1.7% in terms of weight percentage of the liquid phase product; the content of each element in the heavy phase slag is shown in Table 2, and the content of each element in the light phase slag is shown in Table 3.
[0073] Embodiment 11
[0074] The difference from Example 1 is that the weight concentration of the sodium hydroxide solution is 50%; the separation factor of the decanter centrifuge used is 3000; the temperature of the alkaline leaching process is 50° C., the time is 1 hour, and the liquid-to-solid ratio is 6:1.
[0075] The test results show that the content of aluminum in the liquid phase product is 1.13% in terms of weight percentage of the liquid phase product; the content of each element in the heavy phase slag is shown in Table 2, and the content of each element in the light phase slag is shown in Table 3.
[0076] Example 12
[0077] The difference from Example 1 is that the separation factor of the decanter centrifuge is 300; the temperature of the alkaline leaching process is 30° C., the time is 0.5 h, and the liquid-to-solid ratio is 5:1.
[0078] The test results show that the content of aluminum in the liquid phase product is 0.81% in terms of weight percentage of the liquid phase product; the content of each element in the heavy phase slag is shown in Table 2, and the content of each element in the light phase slag is shown in Table 3.
[0079] Comparative Example 1
[0080] The difference from Example 1 is that the weight concentration of the sodium hydroxide solution is 10%; the density of the liquid product is 1.1 g / cm 3 The difference between the density of the liquid phase product and the density of the light phase slag is 0.1 g / cm 3 The difference between the density of the liquid phase product and the density of the heavy phase slag is 4.0 g / cm 3 .
[0081] The test results show that the content of aluminum in the liquid phase product is 1.23% in terms of weight percentage of the liquid phase product; the content of each element in the heavy phase slag is shown in Table 2, and the content of each element in the light phase slag is shown in Table 3.
[0082] Table 2
[0083]
[0084]
[0085] Table 3
[0086]
[0087] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:
[0088] By comparing Examples 1 and 2 and Comparative Example 1, it can be seen that, compared with other concentrations of sodium hydroxide, the use of the above-mentioned specific concentration of sodium hydroxide is beneficial to increasing the density difference between the liquid phase product and the light phase slag, thereby helping to improve the separation efficiency of the light phase slag containing carbon elements and the liquid phase product containing aluminum elements, and achieving preferential extraction of aluminum elements; at the same time, it is beneficial to improve the separation efficiency of the heavy phase slag containing active ingredients and copper elements and the liquid phase product containing aluminum elements.
[0089] By comparing Examples 1 and 3 and Comparative Example 1, it can be seen that limiting the difference between the density of the liquid phase product and the density of the light phase slag, as well as the difference between the density of the liquid phase product and the density of the heavy phase slag within the preferred range of the present application is beneficial to improving the separation efficiency of the liquid phase product, light phase slag and heavy phase slag, thereby improving the recovery rate of valuable metals and carbon, reducing the output of waste slag, and is beneficial to increasing the added value of waste battery black powder.
[0090] By comparing Examples 1, 4 and 5, it can be seen that the temperature and time of the alkaline leaching treatment process include but are not limited to the preferred range of the present application. Limiting it within the preferred range of the present application is beneficial to increasing the reaction rate of the aluminum element and the strong alkaline compound to form a soluble aluminum salt (sodium aluminate), which in turn helps to improve the efficiency of the pretreatment of waste battery black powder.
[0091] By comparing Examples 1, 6 and 7, it can be seen that the liquid-to-solid ratio of the alkaline leaching treatment process includes but is not limited to the preferred range of the present application. Limiting it within the preferred range of the present application is beneficial to allowing the waste battery black powder to fully contact and react with the alkaline leaching agent, which is beneficial to making the reaction more thorough, so that more aluminum elements in the waste battery black powder can form soluble aluminum salts (sodium aluminate), which is beneficial to the subsequent enrichment and extraction and recovery of the aluminum element.
[0092] Comparing Examples 1, 8 and 9, it can be seen that, compared with other ranges, limiting the separation factor of the decanter centrifuge within the preferred range of the present application is beneficial to further improving the effect of solid-liquid separation.
[0093] By comparing Examples 1, 4, 8 and 12, it can be seen that, compared with other value ranges, the use of the preferred technical solution in the present application is beneficial to improving the separation efficiency of light-phase slag containing carbon elements and liquid-phase products containing aluminum elements; at the same time, it is beneficial to improve the separation efficiency of liquid-phase products containing active ingredients and aluminum elements, and thus is beneficial to improving the subsequent recovery rate of aluminum elements.
[0094] According to all the above embodiments of the present application, compared with the prior art, the pretreatment method of the above waste battery black powder provided by the present application has better separation efficiency, and can well separate the heavy phase slag, light phase slag and liquid phase products.
[0095] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.
[0096] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for pretreating waste battery black powder, characterized in that: The pretreatment methods of waste battery black powder include: The waste battery black powder is subjected to alkaline leaching treatment with an alkaline leaching agent to obtain a slurry; the alkaline leaching agent is a dispersion of a strong alkaline compound, and the weight concentration of the alkaline leaching agent is 20-50%; the waste battery black powder includes active ingredients, aluminum elements, copper elements and carbon elements, wherein the active ingredients include one or more of lithium elements, nickel elements, cobalt elements and manganese elements; the temperature of the alkaline leaching treatment process is 50-100° C., and the time is 1-4 hours; The slurry is subjected to solid-liquid separation treatment, wherein the solid-liquid separation treatment is a centrifugal separation treatment; from top to bottom, a light phase slag, a liquid phase product and a heavy phase slag are obtained in sequence, wherein the difference between the density of the liquid phase product and the density of the light phase slag is greater than 0 and less than or equal to 0.3 g / cm 3 The difference between the density of the liquid phase product and the density of the heavy phase slag is 3.3 to 3.9 g / cm 3 ; The heavy phase slag includes the active component and the copper element; the light phase slag includes the carbon element; the liquid phase product includes 0.3-2.6% of the aluminum element in terms of weight percentage of the liquid phase product; Calculated by weight percentage of the waste battery black powder, the waste battery black powder includes 30-55% of the active ingredient, 2-8% of the aluminum element, 1-3% of the copper element, 7-18% of the carbon element and the remainder of impurity elements; The heavy phase slag comprises, in terms of weight percentage of the heavy phase slag, 40-60% of the active ingredient, 1-4% of the copper element, 0.1-0.5% of the aluminum element, 0.1-0.5% of the carbon element and the remainder of the impurity elements; Calculated by weight percentage of the light phase slag, the light phase slag includes 0.1-0.5% of the active ingredient, 0-0.1% of the copper element, 0.5-2% of the aluminum element, 85-95% of the carbon element and the remainder of the impurity elements.
2. The method for pretreating waste battery black powder according to claim 1, characterized in that: The strong alkaline compound is sodium hydroxide.
3. The method for pretreating waste battery black powder according to claim 1, characterized in that: The liquid-to-solid ratio of the alkaline leaching treatment process is (3-6):
1.
4. The method for pretreating waste battery black powder according to claim 1, characterized in that: The centrifugal separation treatment is carried out by using a decanter centrifuge, and the separation factor of the decanter centrifuge is 500-3000.
5. The method for pretreating waste battery black powder according to any one of claims 1 to 4, characterized in that: The particle size of the waste battery black powder is 74 to 178 μm.
6. A method for recycling black powder from waste batteries, characterized in that: The method for recovering waste battery black powder comprises: The heavy phase slag, the light phase slag and the liquid phase product are obtained by the pretreatment method of waste battery black powder according to any one of claims 1 to 5; The liquid phase product is treated by the Bayer process to obtain aluminum oxide; collecting the light phase residue and washing it to obtain a carbon material; The heavy phase slag is collected and extracted and recovered to obtain nickel sulfate and / or cobalt sulfate and / or manganese sulfate, copper and lithium carbonate respectively.