Rotating member for fixing and production method thereof, fixing device, and image forming device

By forming an open pore structure in the surface layer of the fixing rotating member and increasing the perfluoropolyether content, the problem of reduced toner releasability is solved and the stability and quality of image formation are improved.

CN114690606BActive Publication Date: 2024-10-29CANON KK
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202111590667.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-23
Publication Date
2024-10-29
Estimated Expiration
2041-12-23

AI Technical Summary

Technical Problem

It is difficult for existing fixing members to maintain high toner releasability during long-term use. Especially when processing thin paper media, toner easily adheres to the surface of the rotating member, affecting image formation quality.

Method used

A fixing rotating member composed of a base layer, an elastic layer and a surface layer is used, wherein the surface layer contains tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, and an open pore structure is formed in the surface layer to increase the perfluoropolymer The ether content and porosity ensure the stable migration and retention of PFPE.

Benefits of technology

It is possible to maintain high toner releasability over a long period of time, reduce adhesion of toner on rotating members, and improve the formation quality and stability of electrophotographic images on tissue paper.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114690606B_ABST
    Figure CN114690606B_ABST
Patent Text Reader

Abstract

The present invention relates to a fixing rotating member and a production method thereof, a fixing device, and an image forming device. A fixing rotating member comprises a base layer, an elastic layer, and a surface layer in order, the surface layer comprises PFA and PFPE, and has pores with openings on the first surface; at least a part of the pores comprises PFPE, wherein after removing the PFPE in the pores, when a first observation area is set on the first surface, the ratio of the sum of the areas of the openings in the first observation area to the area of ​​the first observation area is defined as P1; and when a second observation area is set in a cross section of the surface layer, the ratio of the sum of the areas of the pores in the second observation area to the area of ​​the second observation area is defined as P2, and P2 / P1 is 1.3 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a fixing rotating member, a fixing device, and an electrophotographic image forming apparatus. Background Art

[0002] In a fixing device used in an electrophotographic image forming apparatus such as a copier or a laser printer (hereinafter also referred to as an "image forming apparatus"), rotating members in the form of a pair of heated rollers, a film and a roller, a belt and a roller, or a belt and a belt are pressed against each other. A recording medium such as paper on which an image formed of unfixed toner is held is introduced into a pressed portion (hereinafter referred to as a "fixing nip portion") formed between the rotating members, and the unfixed toner is melted by heating to fix the image on the recording medium. Depending on the member expression form, the fixing rotating member that contacts the unfixed toner image on the recording medium may be referred to as a fixing roller, a fixing film, or a fixing belt.

[0003] In recent years, paper media for forming electrophotographic images have become diversified, such as thin paper, such as paper with a basis weight of 52 g / m 2 However, due to the low rigidity of such thin paper, in conventional fixing members such as fixing rotating members, the molten toner during heat fixing may in some cases adhere to the surface of the fixing rotating member, resulting in the thin paper being wrapped around the fixing rotating member. Therefore, in order to stably form an electrophotographic image on thin paper, it is necessary to impart a higher toner release property to the surface of the fixing rotating member. WO 2019 / 181796 discloses a fixing member, the surface layer of which contains a fluororesin and a perfluoropolyether (hereinafter also referred to as "PFPE"), so that the fixing member can maintain a high toner release property for a long time.

[0004] Studies conducted by the present inventors show that the fixing member according to WO 2019 / 181796 exhibits excellent toner release properties for a long time. However, WO 2019 / 181796 (paragraph

[0018] ) shows that fluorine oil is present in the surface layer of the disclosed fixing member without being separated from the fluorine resin. In such cases, there is a limit to the amount of fluorine oil that can be introduced into the surface layer. Therefore, it is found that in order to impart excellent toner release properties to the fixing rotating member for a long time, it is necessary to develop the following technology, which is intended to provide a fixing rotating member that can hold a large amount of PFPE and can stably supply PFPE to the outer surface of the fixing rotating member. Summary of the invention

[0005] At least one aspect of the present disclosure is directed to providing a fixing rotating member capable of maintaining high toner releasability for a longer period of time than conventional cases, and is intended to provide a method for producing a fixing rotating member. Another aspect of the present disclosure is directed to providing a fixing device and an electrophotographic image forming device capable of stably forming high-quality electrophotographic images for a long period of time.

[0006] According to one aspect of the present disclosure, there is provided a fixing rotating member including a base layer, an elastic layer and a surface layer in sequence,

[0007] The surface layer comprises tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer and perfluoropolyether;

[0008] The surface layer has holes having openings on a first surface thereof constituting an outer surface of a fixing rotating member;

[0009] At least a portion of the pores comprise a perfluoropolyether, wherein

[0010] When a first observation region of 8 μm in length×11 μm in width is provided on the first surface of the surface layer after removing the perfluoropolyether in the pores, and a ratio of the sum of the areas of the openings observed in the first observation region to the area of ​​the first observation region is defined as P1; and

[0011] When a second observation region of 8 μm in length and 11 μm in width is set in the cross section of the surface layer after the perfluoropolyether in the pores is removed, a ratio of the sum of the areas of the pores observed in the second observation region to the area of ​​the second observation region is defined as P2, and the cross section includes the entire thickness portion of the surface layer in the circumferential direction of the rotating member for fixing,

[0012] P2 / P1 is 1.3 or more.

[0013] According to another aspect of the present disclosure, there is provided a fixing device including the above-mentioned fixing rotating member, and a heating means for heating the fixing rotating member.

[0014] According to another aspect of the present disclosure, there is provided a method for producing a fixing rotating member, the method comprising the following steps:

[0015] (i) providing a laminate comprising:

[0016] A base layer having an endless belt shape or a roller shape,

[0017] an elastic layer on the outer peripheral surface of the base layer, and

[0018] a resin layer comprising a tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer on the outer peripheral surface of the elastic layer;

[0019] (ii) immersing the laminate into a first perfluoropolyether at a temperature of 300±50° C. to impregnate the resin layer with the perfluoropolyether;

[0020] (iii) cooling the laminated body obtained in step (ii) in which the resin layer is impregnated with the perfluoropolyether;

[0021] (iv) removing at least a portion of the perfluoropolyether impregnated into the resin layer with a fluorine solvent to form pores in the resin layer having openings on the first surface of the resin layer; and

[0022] (v) introducing the second perfluoropolyether into at least a part of the pores to obtain a fixing rotating member having a surface layer containing the second perfluoropolyether in at least a part of the pores.

[0023] Further features of the present disclosure will become apparent from the following description of exemplary embodiments with reference to the attached drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1A , Figure 1B , Figure 1C Surface observation images of the resin layer of the fixing rotating member according to Example 1 ( Figure 1A ), when observing the cross section along the circumferential direction of the belt, the cross-sectional image of the resin layer ( Figure 1B ) and cross-sectional images of the surface layer ( Figure 1C );

[0025] Figure 2A and Figure 2B They are respectively fixing belt ( Figure 2A ) and the fixing roller ( Figure 2B ) is a cross-sectional schematic diagram;

[0026] Figure 3 A cross-sectional schematic diagram of a fixing device using a fixing belt;

[0027] Figure 4 is a schematic cross-sectional view of a fixing device using a fixing roller; and

[0028] Figure 5 is a schematic cross-sectional view showing one aspect of an electrophotographic image forming apparatus. DETAILED DESCRIPTION

[0029] In addition, in the present disclosure, unless otherwise specified, the expression "from XX to YY" or "XX to YY" indicating a numerical range means a numerical range including a lower limit and an upper limit as endpoints. When a numerical range is provided in stages, the upper and lower limits of each numerical value can be combined in any combination.

[0030] The present inventors have repeatedly studied with the purpose of obtaining a fixing rotating member capable of maintaining excellent toner releasability even in long-term use. As a result, the present inventors have found that the above object can be achieved by stipulating as follows: the surface layer contains a tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA); the surface layer has pores having openings in a first surface constituting the outer surface of the fixing rotating member; at least a part of the pores contains perfluoropolyether; and the opening ratio P1 of the pores in the outer surface and the porosity P2 of the openings in the cross section are set within the above ranges.

[0031] Since the surface layer has pores, the surface layer can contain PFPE in the pores. As a result, a larger amount of PFPE can be retained in the surface layer of the above fixing rotating member than in the surface layer disclosed in WO2019 / 181796, in which PFPE is retained in the fluororesin without phase separation.

[0032] The opening of the hole is located on the first surface of the surface layer, which constitutes the outer surface of the fixing rotating member, so the PFPE in the hole can migrate to the first surface. In addition, the amount of PFPE that migrates from the hole to the outer surface can be controlled by setting the relationship between the ratio P1 of the opening area per unit area of ​​the outer surface of the surface layer and the ratio P2 of the hole area per unit area of ​​the cross section of the surface layer to follow P2 / P1≥1.3. As a result, it is believed that the fixing rotating member according to the present aspect can maintain excellent toner releasability for a longer period of time compared to the fixing member according to WO2019 / 181796.

[0033] The reference numerals in the figures are as follows.

[0034] 1: Resin portion including PFA, 2: Opening, 3: Hole, 4: PFPE, 101: First surface

[0035] The fixing rotating member will be described in detail below.

[0036] 1. Rotating member for fixing

[0037] The fixing rotating member is, for example, a fixing roller, a fixing film, a fixing belt, etc. The fixing rotating member has a base layer, an elastic layer, and a surface layer in this order.

[0038] Figure 2A and Figure 2B It is a cross-sectional view showing a different form of the fixing rotating member. Figure 2A A fixing rotating member having an endless belt shape (hereinafter also referred to as a "fixing belt 11") is shown, and Figure 2B A fixing rotating member having a roller shape (hereinafter also referred to as a “fixing roller 12 ”) is shown.

[0039] Figure 2A and Figure 2B Each of the fixing rotating members has a base layer 13, an elastic layer 14 covering the outer surface of the base layer 13, and a surface layer 15 covering the surface of the elastic layer on the side opposite to the side facing the base layer. The surface layer 15 may be bonded to the surface of the elastic layer 14 on the side opposite to the side facing the base layer with the aid of an adhesive not shown.

[0040] (1) Grassroots

[0041] Known materials used as base materials of fixing members such as fixing rotating members can be used without particular limitation as the material of the base material 13. For example, metals or alloys such as aluminum, iron, stainless steel or nickel, or heat-resistant resins such as polyimide are used herein.

[0042] In the fixing belt 11, a base material having an endless belt shape can be used as the base layer 13. In this case, examples of the material of the base layer 13 include materials exhibiting excellent heat resistance, such as nickel, stainless steel, and polyimide. The thickness of the base layer 13 is not particularly limited, but is preferably 20 μm to 100 μm, for example, from the viewpoints of strength, flexibility, and heat capacity.

[0043] In the fixing roller 12, for example, a solid or hollow core metal is used as the base layer 13. Examples of the material of the core metal include metals and alloys such as aluminum, iron, and stainless steel. In the case of using a hollow core metal, a heat source may be provided inside it.

[0044] The outer surface of the base layer 13 may be surface treated to impart adhesion to the elastic layer 14. The surface treatment may be a single physical treatment such as sandblasting, lapping or grinding, or a chemical treatment such as oxidation, coupling agent or primer treatment, or a combination of multiple treatments.

[0045] When the elastic layer 14 made of silicone rubber is provided on the surface of the base layer 13 , it is preferable to perform a primer treatment on the surface of the base layer 13 so as to improve the adhesion between the base layer 13 and the elastic layer 14 .

[0046] Examples of primers used for primer treatment include coatings in which a silane coupling agent, a silicone polymer, a hydromethylsiloxane, an alkoxysilane, a reaction accelerating catalyst, and / or a colorant such as red iron oxide are appropriately mixed and dispersed in an organic solvent.

[0047] The primer can be appropriately selected depending on the material of the base layer 13, the type of the elastic layer 14, and the form of the crosslinking reaction. In particular, when the elastic layer 14 contains a large amount of unsaturated aliphatic groups, it is preferable to use a primer containing hydrosilyl groups in order to impart adhesion derived from the reaction with the unsaturated aliphatic groups. When the elastic layer 14 contains a large amount of hydrosilyl groups, it is preferable to use a primer containing unsaturated aliphatic groups.

[0048] Other primers include primers containing an alkoxy group. Commercially available products can be used as the primer. The primer treatment includes a process of applying the primer to the outer surface of the base layer 13 (the surface bonded to the elastic layer 14) and drying or baking.

[0049] (2) Elastic layer

[0050] The material of the elastic layer 14 is not particularly limited, and a known material used as an elastic layer in a fixing rotating member can be used. Preferably, the elastic layer 14 contains silicone rubber having excellent heat resistance. Addition curing type liquid silicone rubber is preferably used as a raw material of the silicone rubber.

[0051] The thickness of the elastic layer 14 can be appropriately designed in consideration of the surface hardness of the fixing rotating member and the width of the fixing nip portion to be formed. When the fixing rotating member is the fixing belt 11, the thickness of the elastic layer 14 is preferably 100 to 500 μm, more preferably 200 to 400 μm.

[0052] In the case where the fixing rotating member is the fixing roller 12 , the thickness of the elastic layer 14 is preferably 0.1 mm (100 μm) to 3.0 mm, more preferably 0.3 mm (300 μm) to 2.0 mm.

[0053] By setting the thickness of the elastic layer 14 to be within this range, it becomes possible to ensure a sufficient width of the fixing nip portion when assembling the fixing rotating member into the fixing device.

[0054] Due to the fact that the elastic layer contains silicone rubber having poor chemical affinity with fluorine oil, the fluorine oil contained in the surface layer does not easily migrate to the elastic layer even after long-term use, and is supplied only to the surface of the fixing rotating member.

[0055] The elastic layer 14 may contain a filler. The filler is added to control thermal conductivity, heat resistance, and elastic modulus.

[0056] Specific examples include silicon carbide (SiC), silicon nitride (Si3N4), silicon dioxide (SiO2), boron nitride (BN), aluminum nitride (AlN), aluminum oxide (Al2O3), iron oxide (Fe2O3), zinc oxide (ZnO), magnesium oxide (MgO), titanium oxide (TiO2), copper (Cu), aluminum (Al), silver (Ag), iron (Fe), nickel (Ni), carbon black (C), carbon fiber (C) and carbon nanotubes (C).

[0057] (3) Surface layer

[0058] The surface layer 15 comprises tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA) and perfluoropolyether (PFPE). Figure 1B As shown, the surface layer has a hole 3 having an opening in a first surface 101 constituting the outer surface of the fixing rotating member. The outer surface of the fixing rotating member is defined as a surface that contacts the unfixed toner on the recording material during fixing. Preferably, the hole 3 has no shell.

[0059] That is, the wall of the hole 3 is preferably constituted by the solid portion of the surface layer, specifically, the resin portion 1 containing PFA.

[0060] At least a portion of the pores contain perfluoropolyether (PFPE) 4. For example, the pores are filled with PFPE.

[0061] The surface layer further meets the following requirements.

[0062] (Requirement) When a first observation region of 8 μm in length and 11 μm in width is set on the first surface of the surface layer after removing PFPE in the pores from the first surface side with a solvent, the ratio of the sum of the areas of the openings observed in the first observation region to the area of ​​the first observation region (hereinafter also referred to as "opening ratio") is defined as P1. When a second observation region of 8 μm in length and 11 μm in width is set at a predetermined position of a cross section of the surface layer after removing PFPE in the pores from the first surface side with a solvent, the ratio of the sum of the areas of the pores observed in the second observation region to the area of ​​the second observation region (porosity) is defined as P2. P1 and P2 satisfy the following relationship: P2 / P1 is 1.3 or more.

[0063] By stipulating that P1 and P2 follow the above relationship, the surface layer can retain a sufficient amount of PFPE, and the PFPE can be stably transferred to the first surface. Herein, P2 / P1 is preferably 5.0 or more, more preferably 7.0 or more. From the viewpoint of achieving a balance between the amount of PFPE that can be retained by the surface layer and the migration of PFPE to the first surface, the upper limit of P2 / P1 is preferably 20.0 or less, more preferably 15.0 or less. That is, for example, the preferred range of P2 / P1 is 1.3 or more and 20.0 or less.

[0064] Herein, P1 is calculated according to the following method. The first surface of the surface layer constituting the outer surface of the fixing rotating member is observed with a scanning electron microscope to obtain an SEM image (magnification of 10,000 times) of an observation area of ​​8 μm in length and 11 μm in width of the first surface. The resolution (e.g., 717 pixels in the longitudinal direction and 986 pixels in the lateral direction) is set in this article so that a single opening can be identified.

[0065] The SEM image was converted into an 8-bit grayscale image using image processing software (product name: ImageJ, manufactured by the National Institutes of Health (NIH) of the United States). A median filter was applied to the obtained grayscale image, and thereafter a binarization process was further performed using the above image processing software to obtain a binarized image. Herein, the binarization process relied on the YEN method disclosed in "IEEE Transactions on Image Processing", Vol. 4, No. 3, March 1995, pp. 370-378 to distinguish between a portion corresponding to an opening and a portion corresponding to PFA within the SEM image.

[0066] Then calculate the ratio of the number of pixels of the portion corresponding to the opening in the obtained binary image to the number of pixels of the entire image. In the present disclosure, observation areas are set at 10 arbitrary positions on the first surface of the surface layer, and the arithmetic mean of the ratios calculated by each observation area is taken as P1. The 10 positions where the observation areas are set are set to positions where the observation areas do not overlap with each other. The specific method involved will be described in the embodiment described below.

[0067] In addition, P2 is calculated according to the following method. A sample of the surface layer is cut out from the surface layer so that a cross section in the direction of the circumferential direction of the fixing rotating member appears on the sample. The cross section includes the entire thickness portion of the surface layer. A predetermined position of the cross section of the sample thus cut out is observed using a scanning electron microscope to obtain an SEM image of a rectangular observation area of ​​the cross section of 8 μm in length and 11 μm in width. The resolution (e.g., 717 pixels in the longitudinal direction and 986 pixels in the lateral direction) is set so that the holes appearing in the cross section can be identified.

[0068] The SEM image was binarized using numerical calculation software (product name: MATLAB; manufactured by The MathWorks, Inc.) to obtain a binarized image. The binarization process relies on the Otsu method disclosed in "IEEE Transactions on SYSTEMS, MAN, AND CYBERNETICS", Vol. SMC-9, No. 1, January 1979, pp. 62-66, to distinguish between the portion corresponding to the pore and the portion corresponding to the PFA in the SEM image. The ratio of the number of pixels of the portion corresponding to the pore in the binarized image to the number of pixels of the entire image is then calculated. In the present disclosure, the following applies to the thickness direction of the surface layer in the cross section:

[0069] (1) A position where 1 μm from the first surface side of the cross section toward the second surface on the opposite side is the upper end of the observation region and the long side of the observation region is parallel to the first surface;

[0070] (2) a position where the midpoint between the first surface and the second surface of the cross section coincides with the center of gravity of the observation area and the long side of the observation area is parallel to the first surface, and

[0071] (3) The lower end of the observation region is oriented toward the first surface, 1 μm away from the second surface, and the long side of the observation region is parallel to the second surface.

[0072] The samples used for the above operation were taken from three positions at intervals of 120° in the circumferential direction of the fixing rotating member. Therefore, P2 is the arithmetic mean of the 9 ratios calculated as above from a total of 9 SEM images.

[0073] Herein, P1 is preferably 1.0% or more, more preferably 1.5% or more, and further preferably 3.0% or more. The upper limit of P1 is preferably 15.0% or less, and more preferably 10.0% or less.

[0074] Due to the fact that P1 is 1.0% or more, the migration of PFPE in the pores to the first surface of the surface layer is less likely to be hindered, and stable toner releasability can be imparted to the first surface. When P1 is 15.0% or less, excessive migration of PFPE in the pores to the first surface can be suppressed, which helps to maintain stable toner releasability for a long time. Therefore, for example, the preferred range of P1 is 1.0% or more and 15.0% or less, and the more preferred range of P1 is 1.5% or more and 10.0% or less.

[0075] Herein, P2 is preferably 20.0% or more, more preferably 25.0% or more. The upper limit of P2 is not particularly limited, but is preferably 60.0% or less, more preferably 50.0% or less.

[0076] When P2 is 20.0% or more, the surface layer can hold more PFPE and can impart stable toner release properties to the first surface for a longer period of time. On the other hand, the wear of the surface layer can be better prevented by setting P2 to 60.0% or less. Therefore, for example, the preferred range of P2 is 20.0% or more and 60.0% or less, and the more preferred range of P2 is 25.0% or more and 50.0% or less.

[0077] The average opening diameter of the openings in the outer surface of the surface layer is preferably 1 nm to 5 μm, more preferably 50 nm to 140 nm. Keeping the average opening diameter within the above range helps to stably maintain excellent toner releasability. The average opening diameter of the openings in the first surface is herein the average value of the diameters of circles having the same surface area as the surface area of ​​the portion corresponding to the openings from the binarized image used to calculate the above-mentioned P1. The specific method involved will be further described.

[0078] The thickness of the surface layer is preferably 12 μm to 100 μm, more preferably 15 μm to 85 μm.

[0079] PFA

[0080] Next, PFA contained in the surface layer will be described in detail.

[0081] Herein, PFA is a copolymer of perfluoroalkyl vinyl ether (hereinafter referred to as "PAVE") and tetrafluoroethylene (hereinafter referred to as "TFE"). The number of carbon atoms in the perfluoroalkyl chain of PAVE is preferably 1 to 6, more preferably 1 to 4, and still more preferably 1 to 3.

[0082] Furthermore, PAVE is preferably selected from perfluoromethyl vinyl ether (CF2=CF-O-CF3), perfluoroethyl vinyl ether (CF2=CF-O-CF2CF3) and perfluoropropyl vinyl ether (CF2=CF-O-CF2CF2CF3).

[0083] The melting point of PFA is preferably 280°C to 320°C, more preferably 290°C to 310°C.

[0084] As PFA, a commercially available product can be used; specific examples are given below.

[0085] "451HP-J", "959HP-Plus", "350-J" and "950HP-Plus" (all product names, manufactured by Chemours-Mitsui Fluoroproducts Co., Ltd.);

[0086] "P-66P", "P-66PT" and "P-802UP" (all product names, manufactured by AGC Inc.);

[0087] "AP-230" and "AP-231SH", etc. (both are product names, manufactured by Daikin Industries, Ltd.); and

[0088] "6502N" (product name, manufactured by The 3M Company).

[0089] Perfluoropolyether (PFPE)

[0090] Next, the PFPE contained in at least a portion of the pores will be described in detail. The PFPE in the pores may be referred to as a second PFPE to distinguish it from the PFPE (first PFPE) used to form the pores described below. However, this does not exclude that the second PFPE is the same PFPE as the first PFPE.

[0091] The second PFPE is not particularly limited, and known examples of PFPE can be used.

[0092] As the second PFPE, a PFPE having a structure represented by the following formula (1) can be preferably used: PFPE is preferably in an oily state at the melting point of PFA.

[0093]

[0094] In formula (1), a, b, c, d, e and f are each independently 0 or a positive integer, satisfying 1≤a+b+c+d+e+f≤600, and at least one of a, b, c and d represents a positive integer.

[0095] In addition, the order in which each repeating unit exists in formula (1) is not limited to the above order. In addition, each repeating unit in formula (1) may exist in multiple positions in PFPE. That is, the PFPE represented by formula (1) may be a block copolymer or a random copolymer.

[0096] Examples of commercially available PFPE include, for example, PFPE having a structure represented by the following formula (2) (e.g., Demnum S-200 and Demnum S-65 (both are product names); manufactured by Daikin Industries, Ltd.), PFPE having a structure represented by the following formula (3) (e.g., Krytox XHT-1000, Krytox VPF16256, Krytox GPL-107, Krytox GPL-106, Krytox GPL-105, Krytox GPL-104, Krytox GPL-103, Krytox GPL-102, and Krytox GPL-101 (all are product names); manufactured by The Chemours Company), PFPE having a structure represented by the following formula (4) (e.g., Fomblin M60, Fomblin M100, and Fomblin Z25 (all are product names); manufactured by Solvay Specialty Polymers Co., Ltd.), and PFPE having a structure represented by the following formula (5) (for example, Fomblin Y45 and Fomblin Y25 (both product names); manufactured by Solvay Specialty Polymers Co., Ltd.).

[0097] Preferably, the perfluoropolyether has at least one structure selected from the group consisting of the following formula (2) to formula (5).

[0098]

[0099] In the formula (2), n is a positive number, and n is within a range such that the viscosity of PFPE at a temperature of 40° C. is in a range of 30 to 500 mPa·s.

[0100]

[0101] In the formula (3), n' is a positive number, and n' is within a range such that the viscosity of PFPE at a temperature of 40°C is in a range of 10 to 2500 mPa·s.

[0102]

[0103] In formula (4), n" and m are each independently a positive number, m / n" is a number from 0.5 to 2, and n"+m is a number within a range such that the viscosity of PFPE at a temperature of 40°C ranges from 20 to 1400 mPa·s.

[0104]

[0105] In formula (5), n'' and m' are each independently a positive number, m' / n'' is a number from 20 to 1000, and n''+m' is a number within a range such that the viscosity of PFPE at a temperature of 40° C. is within a range of 20 to 1200 mPa·s.

[0106] The viscosity of the second PFPE is preferably 300 mPa·s to 2500 mPa·s, more preferably 350 mPa·s to 2000 mPa·s. Herein, the PFPE within such a viscosity range facilitates stable migration thereof from the pores to the first surface of the surface layer.

[0107] The term viscosity as used herein refers to the viscosity measured using a rheometer (manufactured by TA Instruments Inc.: DHR-2) mounted to a cone plate having a cone angle of 1° and a cone radius of 20 mm, at a flow rate of 100 s -1 The shear rate and the value of the viscosity obtained after rotating for 60 seconds at a measuring temperature of 40°C.

[0108] Examples of commercially available PFPEs within the above viscosity range include, for example, "Krytox GPL-105" (viscosity 301 mPa·s), "Krytox GPL-106" (viscosity 459 mPa·s), "Krytox GPL-107" (viscosity 852 mPa·s), "Krytox VPF16256" (viscosity 1403 mPa·s), "Krytox XHT-1000" (viscosity 1941 mPa·s), "Fomblin M60" (viscosity 586 mPa·s), and "Fomblin M100" (viscosity 1327 mPa·s).

[0109] The content of the perfluoropolyether in the surface layer is preferably 20% to 60% by mass, more preferably 25% to 45% by mass. When the content is 20% by mass or more, good toner releasability is still maintained during long-term use. When the content is 60% by mass or less, abrasion caused by the use of the surface layer can be more reliably prevented.

[0110] Method for producing a rotating member for fixing

[0111] A non-limiting exemplary method for producing the above-described fixing rotating member according to an aspect of the present disclosure includes the following processes (i) to (v).

[0112] Step (i): a step of providing a laminated body including a base layer having an endless belt shape or a roll shape, an elastic layer on an outer peripheral surface of the base layer, and a resin layer containing PFA on an outer peripheral surface of the elastic layer.

[0113] Step (ii): a step of bringing a first PFPE into contact with a surface of the resin layer on the side opposite to the side facing the elastic layer at a temperature close to the melting point of PFA to thereby impregnate the resin layer with the first PFPE;

[0114] Step (iii): a step of cooling the laminate obtained in step (ii) in which the resin layer is impregnated with the first PFPE to room temperature (eg, 20° C. to 35° C., preferably 25° C.);

[0115] Step (iv): a step of removing at least a portion of the first PFPE impregnated into the resin layer from the first surface side of the resin layer with a fluorinated solvent to thereby form, in the resin layer, pores having openings on the first surface of the resin layer; and

[0116] Process (v): a process of introducing a second PFPE into at least a part of the pores to thereby make the resin layer a surface layer according to the present disclosure, and obtaining a fixing rotating member having a surface layer containing the second perfluoropolyether in at least a part of the pores.

[0117] The present inventors presume that the mechanism by which the fixing rotating member according to an aspect of the present disclosure is formed by using the above method is as follows.

[0118] In step (ii), the first surface of the resin layer is brought into contact with the first PFPE at a temperature close to the melting point of PFA contained in the resin layer (temperature of 300°C ± 50°C (preferably 290°C to 325°C)), and as a result, the resin layer becomes impregnated with the first PFPE.

[0119] The resin layer impregnated with the first PFPE in step (ii) is in a high temperature state, and therefore the resin layer is cooled to room temperature, for example, about 25° C., in step (iii) following step (ii). Next, in step (iv), the first PFPE in the resin layer is removed using a solvent, and as a result, pores having openings in the first surface of the resin layer are formed at the sites where the first PFPE in the resin layer exists.

[0120] The surface area ratio P2 of the holes per unit area in the cross section parallel to the circumferential direction of the surface layer after the above steps (iii) and (iv) is higher than the surface area ratio P1 of the openings per unit area in the first surface. The reason is considered to be as follows.

[0121] When the PFA tube that has been thermally expanded due to the heating in step (ii) shrinks during the cooling process in step (iii), the cooling proceeds faster on the first surface of the resin layer, and therefore, the degree of shrinkage is greater than that on the elastic layer side surface of the resin layer. As the first surface side shrinks, the first PFPE present near the first surface of the resin layer is squeezed out of the resin layer from the first surface. As a result, the diameter of the opening in the first surface of the resin layer is reduced. On the other hand, the first PFPE that has penetrated deeply into the resin layer in the thickness direction of the resin layer, for example, to a position near the surface on the elastic layer side, will not be released to the outside of the resin layer even when the resin layer shrinks, but will remain in the resin layer. Therefore, the aggregated portion of the first PFPE that constitutes the void after the first PFPE is removed hardly shows a reduction in size. As a result, the ratio (P2 / P1) of the porosity P2 to the opening ratio P1 of the first surface of the surface layer formed in step (iv) increases.

[0122] Herein, the value of P2 / P1 can be adjusted based on the amount of impregnation of the first PFPE into the resin layer in step (ii). Specifically, increasing the amount of impregnation of PFPE into the resin layer increases the gap formed inside the resin layer, so that the value of P2 increases. Increasing the amount of impregnation into the resin layer is also converted into a larger amount of openings in the first surface of the resin layer, so that the value of P1 is increased in the same manner. Although the root cause is not yet clear, the increase in the degree of P1 caused by the increase in the amount of impregnation in the resin layer is greater than the increase in the degree of P2. Therefore, P2 / P1 can be adjusted to be smaller by increasing the amount of the first PFPE impregnated into the PFA tube.

[0123] In order to achieve the preferred range of P2 described above, the resin layer is preferably impregnated with the first PFPE so that the amount of the first PFPE impregnated into the resin layer in step (ii) is preferably 25 to 60% by mass, and particularly preferably 30 to 45% by mass in terms of the content ratio of the first PFPE relative to the mass of the resin layer containing the first PFPE.

[0124] The amount of the first PFPE impregnated into the resin layer can be adjusted based on, for example, the temperature of the first PFPE during impregnation, the viscosity of the first PFPE, and the contact time between the resin layer and the first PFPE. Specifically, the higher the temperature in the temperature range close to the melting point of PFA (temperature of 250 to 350° C.), the lower the viscosity of the first PFPE, the longer the contact time, and the greater the amount of the first PFPE impregnated into the resin layer.

[0125] The preferred viscosity of the first PFPE is 10 to 400 mPa·s, more preferably 30 to 350 mPa·s.

[0126] Examples of commercially available PFPEs within this viscosity range include "Krytox GPL-101" (viscosity 12 mPa·s), "Krytox GPL-102" (viscosity 26 mPa·s), "Krytox GPL-103" (viscosity 54 mPa·s), "Krytox GPL-104" (viscosity 111 mPa·s), "Fomblin M03" (viscosity 30 mPa·s), and "Krytox GPL-105" (viscosity 301 mPa·s).

[0127] Herein, in a case where, for example, the viscosity of the first PFPE is 301 mPa·s, the thickness of the resin layer containing PFA is 20 μm, the melting point of the resin layer is 296° C., and the temperature of the resin layer when in contact with the first PFPE is 310° C., a PFPE-impregnated resin layer having a first PFPE content of 30% by mass can be produced over a contact time of 1 minute.

[0128] The term content is defined herein as the percentage (%) of the mass of the PFPE impregnated into the resin layer relative to the sum of the mass of the resin layer itself plus the mass of the PFPE impregnated into the resin layer.

[0129] In the above example, when a PFPE having a viscosity of 111 mPa·s is used as the first PFPE and other conditions remain unchanged, a PFPE-impregnated resin layer in which the content of the first PFPE is 41% by mass can be produced. In the above example, when the temperature at the time of contact is set to 300° C. and other conditions remain unchanged, a PFPE-impregnated resin layer in which the content of the first PFPE is 26% by mass can be produced.

[0130] The viscosity of "Krytox GPL106" as PFPE used in the examples of WO 2019 / 181796 is 459 mPa·s. When such PFPE is in contact with a resin layer containing PFA at a temperature of 345°C for 5 minutes, a PFPE-impregnated resin layer having a PFPE content of 24% by mass is obtained. However, when the PFPE content is at this level, there is no PFPE aggregation in the resin layer. Therefore, even when the PFPE is subsequently dissolved using a fluorine-based solvent, pores are not formed in the resin layer.

[0131] As a method of bringing the resin layer into contact with the first PFPE in the production of the fixing rotating member, any method may be used as long as the PFPE can be brought into contact with the resin layer at a temperature close to the melting point of the PFA resin contained in the resin layer.

[0132] In addition, the resin layer in contact with the first PFPE may be a resin layer in a laminate in which a base layer, an elastic layer, and a resin layer are previously laminated with each other; alternatively, a PFA sheet or a PFA tube for the resin layer may be prepared in a state in which the surface to be bonded to the elastic layer is masked. For example, a dipping method is a further example of a contact method.

[0133] In order to remove the first PFPE impregnated into the resin layer in step (iv), the first surface of the resin layer is immersed in a solvent capable of dissolving the first PFPE but not dissolving PFA, so as to wet the first surface of the resin layer. The "PFPE-dissolving solvent" may be, for example, a solvent in which the amount of PFPE dissolved in 100 g of the solvent at 25° C. is 10 g or more. Meanwhile, the term "PFA-insoluble solvent" includes a solvent in which the amount of PFA dissolved in 100 g of the solvent at 25° C. is 1 g or less. Examples of such solvents include hydrofluoroethers (product name: Novec 7600; manufactured by The 3M Company).

[0134] In order to remove the first PFPE from the resin layer in the step (iii), it is preferred to apply ultrasonic waves to the resin layer to promote the removal of the first PFPE from the resin layer.

[0135] Next, a method for producing the fixing rotating member according to an aspect of the present disclosure will be described in more detail.

[0136] Step (i): A laminated body in which a base layer, an elastic layer containing silicone rubber, and a resin layer containing PFA are laminated in this order is mounted on a dipping device.

[0137] Step (ii): The laminate is immersed in a PFPE bath heated to a temperature close to the melting point of PFA (300°C ± 50°C (preferably 290°C to 325°C)) and allowed to stand for preferably 20 seconds to 5 minutes, more preferably 30 seconds to 2 minutes (eg 1 minute) (immersion step-1).

[0138] It was found that in (impregnation process-1), as the contact temperature between the resin layer and the first PFPE increases and as the viscosity of the PFPE decreases, the impregnation amount increases. The contact temperature and the viscosity of the PFPE can be appropriately selected as long as an impregnation amount equal to or greater than a given amount that allows the formation of the above-specified pores is achieved.

[0139] X°C is defined as the heating temperature of the first PFPE in the impregnation step-1 and Y°C is defined as the melting point of PFA, preferably XY is 0°C to 40°C, more preferably 3°C to 20°C.

[0140] Step (iii): The laminate is taken out from the first PFPE bath and cooled to room temperature.

[0141] Step (iv): After cooling, the laminate is impregnated with a solvent capable of dissolving the first PFPE, thereby dissolving the first PFPE impregnated into the resin layer from the openings of the first surface of the resin layer (pore forming step). As a result of this step, pores having openings in the first surface are formed in the resin layer.

[0142] Step (v-1): The laminated body having the resin layer having pores and obtained as a result of the above step is then immersed in a second PFPE bath and allowed to stand for preferably 5 to 30 minutes, more preferably 10 to 20 minutes (e.g. 15 minutes). As a result, the second PFPE is introduced into the pores in the resin layer (immersion step-2).

[0143] The temperature of the second PFPE at this time is preferably a temperature that allows the impregnation of the second PFPE into the pores to be promoted but does not cause the openings in the first surface of the resin layer to disappear. As a non-limiting example, the lower limit of the temperature of the second PFPE in this process is preferably 180° C. or more, and the upper limit is preferably 280° C. or less, more preferably 230° C. or less.

[0144] Process (v-2): The laminated body obtained as a result of the above process is taken out from the second PFPE bath, and the second PFPE attached to the outer surface is removed to thereby obtain a fixing rotating member according to an aspect of the present disclosure.

[0145] In this process, the method for removing the excess second PFPE attached to the surface is not particularly limited, and examples thereof include cleaning with a fluorine solvent, removing with air, and wiping with non-woven fabric. Examples of the method of cleaning with a fluorine solvent include a removal method using fibers such as non-woven fabric impregnated with a fluorine solvent.

[0146] 2. Fixing equipment

[0147] The fixing device includes a fixing rotating member and a heating means for heating the fixing rotating member. The fixing device includes, for example, a heating rotating member and a pressing rotating member arranged to form a fixing nip portion with the heating rotating member.

[0148] Examples of the combination of the heating rotating member and the pressing rotating member include, for example, a heating roller and an elastic pressing roller arranged to face the heating roller, and a heating film and an elastic pressing roller arranged to contact the heating film. Other examples of the combination of the heating rotating member and the pressing rotating member include a heating belt and an elastic pressing roller arranged to contact the heating belt, and a heating belt and an elastic pressing belt arranged to contact the heating belt.

[0149] (1) Fixing equipment using a fixing belt

[0150] Figure 31 is a cross-sectional view of a fixing device having a heating fixing belt 11 and an elastic pressure roller 19 along the circumferential direction of the fixing belt.

[0151] The fixing belt 11 is the fixing belt described as the fixing rotating member above. The fixing belt 11 is loosely fitted outside the belt guide member 16. The pressurizing rigid post 18 is inserted inside the belt guide member 16. The belt guide member 16 is formed of, for example, a heat-resistant / insulating resin.

[0152] The heating member is, for example, a heater configured to contact the inner peripheral surface of the fixing belt. A ceramic heater 17 as a heat source is provided at a position where the belt guide member 16 and the inner surface of the fixing belt 11 contact each other. The ceramic heater 17 is embedded in a groove portion provided in the length direction of the belt guide member 16 and fixed to the groove portion. The ceramic heater 17 generates heat by energizing with the aid of a component not shown.

[0153] The elastic pressure roller 19 has a core metal 19a made of stainless steel and an elastic layer 19b made of cured silicone rubber, for example, on its circumferential surface. A surface layer 19c made of fluorine resin is provided on the circumferential surface of the elastic layer 19b. The thickness of the surface layer 19c is, for example, 50 μm.

[0154] A downward thrust is applied to the pressurizing rigid column 18 by providing a pressurizing spring (not shown) between both ends of the pressurizing rigid column 18 and a spring receiving member (not shown) on the side of the apparatus chassis. As a result, the lower surface of the ceramic heater 17 disposed under the belt guide member 16 and the upper surface of the elastic pressurizing roller 19 are brought into pressure contact with each other, with the fixing belt 11 sandwiched therebetween, to form a predetermined fixing nip portion N. That is, the lower surface of the ceramic heater 17 is disposed so as to contact the inner peripheral surface of the fixing belt 11.

[0155] The recording medium P as a heated body having an image formed of unfixed toner G thereon is nipped and conveyed at a conveying speed V in the fixing nip portion N. As a result, the toner image is heated and pressurized. As a result, the toner image is melted and mixed, and thereafter the toner image is cooled, and as a result, the toner image is thereby fixed on the recording medium P.

[0156] (2) Heating fixing device using fixing roller

[0157] Figure 4 1 is a cross-sectional view along the circumferential direction of a fixing roller in a heating fixing device provided with a heating fixing roller 12 , an elastic pressure roller 19 arranged to face the fixing roller 12 , and a heater 20 as a heating member for the fixing roller 12 .

[0158] The fixing roller 12 is the fixing roller described as the above fixing rotating member. In the fixing roller 12 , an elastic layer 14 is formed on the outer peripheral surface of the hollow core metal as the base layer 13 , and a mold release surface layer 15 is formed outside the elastic layer 14 .

[0159] The fixing roller 12 and the elastic pressing roller 19 are rotationally pressed toward each other by an unillustrated pressing member, and as a result, a fixing nip portion N is formed.

[0160] Heaters 20 as heat sources for supplying heat required to melt the unfixed toner G are installed inside the fixing roller 12 and inside the elastic pressure roller 19. A halogen heater is generally used as the heater 20. Depending on the size of the recording medium P to be conveyed, a plurality of halogen heaters may be installed inside the rollers.

[0161] With the aid of unillustrated components, each rotational force is applied to the fixing roller 12 and the elastic pressure roller 19 through the base layer (core metal) 13 and the end of the core metal 19a, and the rotation is controlled herein so that the moving speed of the surface of the fixing roller 12 is substantially equal to the conveying speed V of the recording medium P. At this time, the rotational force may be applied to either one of the fixing roller 12 and the elastic pressure roller 19 having elasticity, so that the other roller rotates by being driven; alternatively, the rotational force may be applied to both rollers.

[0162] The recording medium P as a heated body having an image formed by the unfixed toner G thereon is sandwiched and conveyed in the fixing nip portion N of the fixing device formed as described above. As a result, the toner image is heated and pressurized. As a result, the toner image is melted and mixed, and thereafter the toner image is cooled, resulting in the toner image being fixed on the recording medium P.

[0163] 3. Electrophotographic image forming equipment

[0164] A known structure can be used as an electrophotographic image forming device. Such devices include multi-function devices, copiers, fax machines, and printers that utilize an electrophotographic system. In this article, a color laser printer will be used as an example to schematically explain the overall structure of an electrophotographic image forming device.

[0165] Figure 5 is a schematic cross-sectional view of the laser printer 40 . Figure 5 The laser printer 40 shown in FIG. 1 has respective electrophotographic photosensitive member drums 39 (hereinafter referred to as “photosensitive member drums 39”) that rotate at a constant speed for each of the colors including yellow (Y), magenta (M), cyan (C), and black (K). The laser printer 40 further has an intermediate transfer member 38 that holds a color image developed in an image forming portion and obtained by multiple transfer, and transfers the color image to a recording medium P fed from a feeding unit.

[0166] By means of a drive member (not shown), such as Figure 5 As shown in , each photosensitive member drum 39 ( 39Y, 39M, 39C, 39K) is rotationally driven counterclockwise.

[0167] Around each photosensitive member drum 39, there are arranged in sequence according to its rotation direction, charging devices 21 (21Y, 21M, 21C, 21K) for uniformly charging the surface of the photosensitive member drum 39, scanner units 22 (22Y, 22M, 22C, 22K) for irradiating a laser beam based on image information to form an electrostatic latent image on the photosensitive member drum 39, developing units 23 (23Y, 23M, 23C, 23K) for attaching colorant to the electrostatic latent image to thereby develop the colorant in the form of a colorant image, primary transfer rollers 24 (24Y, 24M, 24C, 24K) for transferring the colorant image on the photosensitive member drum 39 to the intermediate transfer member 38 in the primary transfer section T1, and cleaning units 25 (25Y, 25M, 25C, 25K) having a cleaning scraper for removing untransferred colorant remaining on the surface of the photosensitive member drum 39 after transfer.

[0168] At the time of image formation, a belt-shaped intermediate transfer member 38 stretched around rollers 26, 27 and 28 rotates and the respective color toner images formed on the respective photosensitive member drums 39 undergo primary transfer overlapping each other on the intermediate transfer member 38, and as a result, a color image is formed.

[0169] Then, the recording medium P is conveyed to the secondary transfer portion T2 by the conveying means in synchronization with the primary transfer to the intermediate transfer member 38. The conveying means includes a feed cassette 29 that accommodates a plurality of recording media P, a feed roller 30, a separation pad 31, and a registration roller pair 32. When forming an image, the feed roller 30 is driven to rotate according to the image forming operation, and the recording media P in the feed cassette 29 are separated one by one, and conveyed to the secondary transfer portion T2 by the registration roller pair 32 at a timing synchronized with the image forming operation.

[0170] A movable secondary transfer roller 33 is arranged in the secondary transfer section T2. ​​The secondary transfer roller 33 can be moved substantially in the vertical direction. At the time of image transfer, the secondary transfer roller 33 is pressed toward the intermediate transfer member 38 via the recording medium P with a predetermined pressure. At the same time, a bias is applied to the secondary transfer roller 33, and the toner image on the intermediate transfer member 38 becomes transferred to the recording medium P.

[0171] The intermediate transfer member 38 and the secondary transfer roller 33 are each driven, so that the recording medium P sandwiched between the intermediate transfer member 38 and the secondary transfer roller 33 is moved along the Figure 5 The recording medium P is conveyed in the direction of the left arrow in FIG. 3 at a predetermined conveying speed V; and then the recording medium P is further conveyed to the fixing unit 35 of the next process by the conveying belt 34. In the fixing unit 35, the transferred toner image is fixed on the recording medium P by applying heat and pressure. Then, the recording medium P is discharged to the discharge tray 37 above the apparatus by the discharge roller pair 36.

[0172] Therefore, by Figure 3 and Figure 4 The fixing device shown in FIG. Figure 5 The fixing unit 35 of the electrophotographic image forming apparatus shown in FIG. 1 realizes an image forming apparatus capable of delivering high-quality images with excellent image uniformity.

[0173] Example

[0174] Next, the present disclosure will be specifically described with reference to Examples.The present disclosure is not limited to the following Examples.

[0175] In this embodiment, a fixing member as a rotating member for fixing was produced using the following PFA resin and perfluoropolyether.

[0176] Fluorine resin

[0177] PFA-1: "959HP-Plus" (product name, manufactured by Chemours-Mitsui Fluoroproducts Co., Ltd.)

[0178] PFA-2: "451HP-J" (product name, manufactured by Chemours-Mitsui Fluoroproducts Co., Ltd.)

[0179] Perfluoropolyether

[0180] PFPE-1: "Krytox GPL104" (product name, manufactured by The Chemours Company, 111 mPa·s (40° C.)

[0181] PFPE-2: "Krytox GPL105" (product name, manufactured by The Chemours Company, 301 mPa·s (40° C.)

[0182] PFPE-3: "Krytox VPF16256" (product name, manufactured by The Chemours Company, 1403 mPa·s (40° C.)

[0183] PFPE-4: "Krytox XHT-1000" (product name, manufactured by The Chemours Company, 1941 mPa·s (40° C.)

[0184] PFPE-5: "Fomblin M100" (product name, manufactured by Solvay Specialty Polymers Co., Ltd., 1327 mPa·s (40° C.)

[0185] PFPE-6: "Krytox GPL106" (product name, manufactured by The Chemours Company, 459 mPa·s (40° C.)

[0186] Example 1

[0187] Fusing belt production

[0188] Preparation of a laminate having a base layer, an elastic layer and a resin layer containing PFA

[0189] As a base layer, a substrate having an inner diameter of 30 mm, a width of 400 mm and a thickness of 40 μm obtained by nickel electroforming and having an endless belt shape was prepared. The outer peripheral surface of this substrate was subjected to primer treatment.

[0190] As a raw material for forming the elastic layer, an addition-curing liquid silicone rubber (product name: SE1886, manufactured by Dow Corning Toray Co., Ltd.) containing no filler was prepared. To 61 parts by volume of the liquid silicone rubber, 38 parts by volume of spherical alumina (product name: Alunabeads CB-A30S, manufactured by Showa Denko KK) as a spherical filler and 1 part by volume of vapor-grown carbon fiber (product name: VGCF-S, manufactured by Showa Denko KK, aspect ratio = 100, average fiber length = 10 μm) as a non-spherical filler were added.

[0191] Thus, an addition-curable silicone rubber composition for forming an elastic layer was prepared in this manner. The above composition was applied to the outer peripheral surface of the above substrate by ring coating, and then heated at a temperature of 200° C. for 4 hours to cause crosslinking of the layer of the addition-curable silicone rubber composition, and thereby an elastic layer having a thickness of 300 μm was formed.

[0192] While the substrate on which the elastic layer was formed was rotated at a moving speed of 20 mm / sec, the surface of the elastic layer was irradiated with ultraviolet rays in the atmosphere using an ultraviolet lamp arranged at a position 10 mm from the surface of the elastic layer. The ultraviolet lamp used herein was a low-pressure mercury ultraviolet lamp (product name: GLQ500US / 11, manufactured by Toshiba Lighting & Technology Corporation), and irradiation was performed so that the cumulative light amount at a wavelength of 185 nm on the irradiated surface was 800 mJ / cm 2 .

[0193] Then, the surface of the elastic layer was substantially uniformly coated with an addition curing type silicone rubber adhesive (product name: SE1819CV, an equal mixture of "A liquid" and "B liquid", manufactured by Dow Corning Toray Co., Ltd.) to a thickness of about 20 μm.

[0194] Next, the inner surface was covered with a hydrophilically treated fluororesin tube (PFA-1, 20 μm thick, melting point 296° C.), and the belt surface was uniformly pressed from above the fluororesin tube to thereby remove excess adhesive from between the elastic layer and the fluororesin tube.

[0195] Then, the base layer covered with the elastic layer and the fluororesin tube was placed in an electric furnace set to a temperature of 200° C. and the whole was heated for 1 hour to cure the adhesive and bond the fluororesin tube to the elastic layer, after which both ends were cut to obtain a 343 mm wide laminate for a fixing belt.

[0196] First PFPE contact impregnation

[0197] Dipping process-1

[0198] The first PFPE (PFPE-1) was placed in a measuring cylinder made of borosilicate glass. An electric heating wire covered with a heat insulating material was wound around the entire measuring cylinder, and the measuring cylinder was heated to a PFPE temperature of 310° C. The pre-imaged tape thus produced was mounted on a dipping device, and the laminate was immersed in the heated PFPE for 1 minute and then removed.

[0199] Evaluation A-1: ​​Measurement of the content of the first PFPE in the resin layer impregnated with the first PFPE

[0200] The content of the first PFPE in the obtained resin layer impregnated with the first PFPE is measured according to the following method. Specifically, a multilayer sample of the elastic layer and the resin layer is cut out from the laminate. Next, the elastic layer is removed from the multilayer sample by dissolving the silicone rubber in the elastic layer from the multilayer sample by immersing the multilayer sample in a silicone resin dissolving agent (product name: e-Solve 21RS, manufactured by Kaneko Chemical Co., Ltd.). In this way, a measurement sample made of only the entire thickness portion of the resin layer is prepared. The measurement sample is measured under the following conditions using a thermogravimetric analyzer (TGA), and the content (mass %) of the first PFPE relative to the resin layer containing the first PFPE is calculated.

[0201] Instrument: TGA851 (product name, manufactured by Mettler-Toledo International Inc.)

[0202] Atmosphere: In the air

[0203] Temperature: 425℃

[0204] In the measurement time-weight reduction rate curve obtained based on the above thermogravimetric analysis, a linear least squares approximate expression is obtained from the region where the slope is constant and only PFA is reduced. The intercept of the linear least squares approximate expression is taken as the PFA content (mass %), and the first PFPE content is calculated according to the first PFPE content (mass %) = 100-PFA content.

[0205] Hole Forming Process

[0206] After the laminate obtained in the impregnation process-1 is cooled to room temperature (25°C), the laminate is immersed in a measuring cylinder containing a separately prepared fluorine solvent (product name: Novec 7300, manufactured by The 3M Company) for 10 minutes. Next, the measuring cylinder is placed in a water tank of an ultrasonic cleaning device (product name: Bransonic (model 2510J-DTH); manufactured by Emerson Japan, Ltd.) and irradiated with ultrasound for 60 minutes. After treatment, the laminate is taken out of the measuring cylinder and dried by allowing it to stand for 60 minutes in an environment at a temperature of 25°C. A laminate in which the PFPE present on the surface and inside of the resin layer is removed is thus obtained. The visual appearance of the obtained laminate is white, and holes are observed to be formed in the resin layer.

[0207] Figure 1A and Figure 1B Schematic diagram showing an observation image with a scanning electron microscope of a first surface of a resin layer of the obtained laminate and a cross section of the laminate in a direction along the circumferential direction.

[0208] Figure 1A Schematic diagram of a SEM image of the first surface. The resin portion 1 and the opening 2 made of PFA are observed. Figure 1B Schematic diagram of a SEM image of a cross section of the resin layer in the direction along the circumferential direction of the laminate. The resin portion 1 containing PFA and the pores 3 are observed here. It is found that the pores 3 have openings in the first surface 101 and thus have openings in the first surface.

[0209] Evaluation A-2: Calculation of the opening ratio P1, average opening diameter, and porosity P2 on the first surface of the surface layer (resin layer)

[0210] The opening ratio P1 and the average opening diameter of the first surface of the surface layer (resin layer) are calculated as follows.

[0211] A scanning electron microscope was used to observe the surface of the laminate from which the first PFPE was removed and obtained in the above hole forming process, that is, the surface of the resin layer on the side opposite to the side facing the elastic layer, and a SEM image (magnification 10000 times) of a rectangular observation area of ​​8 μm in length × 11 μm in width was obtained. The resolution was set to 717 pixels in the longitudinal direction and 986 pixels in the lateral direction so that the opening could be identified. The acquired SEM image was converted into an 8-bit grayscale image using image processing software (product name: ImageJ, manufactured by the National Institutes of Health (NIH) of the United States). After applying a median filter to the obtained grayscale image, a binarization process was further performed using the above image processing software to obtain a binarized image. The binarization process relies on the YEN method to distinguish between the portion corresponding to the opening and the portion corresponding to the PFA in the SEM image. The ratio of the number of pixels corresponding to the portion of the opening in the obtained binarized image to the number of pixels of the entire image is then calculated. Observation areas were set at 10 arbitrary positions on the surface of the resin layer with an opening, and the arithmetic mean of the ratio calculated by each observation area was taken as P1. The observation areas are set to positions where the observation areas do not overlap with each other.

[0212] The surface area of ​​the portion corresponding to the opening in each binarized image is approximated to each perfect circle having the same surface area therewith, and the arithmetic mean of the diameters of the perfect circles (hereinafter referred to as the circle equivalent diameter) is taken as the average opening diameter.

[0213] The porosity P2 is calculated as follows.

[0214] A cross-sectional sample was cut out from the resin layer of the laminate from which the first PFPE was removed using a Cryo-Ultra-microtome (manufactured by Leica Microsystems GmbH) so that a cross section of the resin layer in the direction along the circumferential direction of the laminate appeared on the sample. The cross section was set to include the entire thickness portion of the resin layer. Next, the cross section was observed under a scanning electron microscope, and an SEM image of an observation area of ​​8 μm long × 11 μm wide was acquired. The resolution was set to 717 pixels in the longitudinal direction and 986 pixels in the lateral direction so that the holes appearing in the cross section could be identified. The SEM image was binarized using numerical calculation software (product name: MATLAB; manufactured by The MathWorks, Inc.) to obtain a binarized image. The binarization process relies on Otsu's method to distinguish between the portion corresponding to the hole and the portion corresponding to the PFA in the SEM image. The ratio of the number of pixels of the portion corresponding to the hole in the binarized image to the number of pixels of the entire image is then calculated. The acquisition position of the SEM image along the thickness direction in the cross section of each cross-sectional sample is set to three positions as specified in (i) to (iii) below.

[0215] (i) In the cross section of the cross-sectional sample, 1 μm from the surface on one side of the surface layer (hereinafter also referred to as the "first surface") to the surface on the other side (hereinafter also referred to as the "second surface") is the upper end of the observation area and the long side of the observation area is parallel to the first surface.

[0216] (ii) In the cross section of the cross-sectional sample, a position where the midpoint between the first surface and the second surface of the surface layer coincides with the center of gravity of the observation region and the long side of the observation region is parallel to the first surface.

[0217] (iii) In the cross section of the cross-sectional sample, 1 μm from the first surface toward the second surface is the lower end of the observation region and the long side of the observation region is parallel to the second surface.

[0218] Samples for the above operation were obtained from three positions at intervals of 120° along the circumferential direction of the laminate. Thus, a total of 9 SEM images were obtained according to the above operation, and 9 ratios were calculated based on the binarized images created from each SEM image. The arithmetic mean of these 9 ratios was taken as the porosity P2.

[0219] Dipping process-2

[0220] The laminated body provided with the resin layer having pores and obtained as a result of the above pore forming step was then subjected to the following operation: Specifically, the second PFPE (PFPE-3) was placed in a measuring cylinder made of borosilicate glass.

[0221] A heating wire covered with a heat insulating material was wound around the entire measuring cylinder, and the measuring cylinder was heated so that the PFPE temperature was 200° C. Next, the stack was mounted to a dipping device, and the entire stack was immersed in the heated second PFPE for 15 minutes and then taken out.

[0222] Next, the second PFPE attached to the outer surface of the taken-out laminated body was removed using a nonwoven fabric impregnated with a fluorine-based solvent (product name: Novec 7300; manufactured by The 3M Company). In this way, a fixing belt according to the present embodiment was obtained. Figure 1C A schematic diagram showing an observation image by means of a scanning electron microscope of a cross section of the surface layer in the direction along the circumferential direction of the obtained fixing belt. It was found that as a result of the immersion step-2, Figure 1B The pores observed in 3 become filled with the second PFPE 4.

[0223] Evaluation A-3: Measurement of the content of the second PFPE in the surface layer

[0224] Similar to Evaluation A-1, a measurement sample of the obtained fixing belt consisting only of the entire thickness portion of the surface layer was prepared. The measurement sample was measured using a thermogravimetric analyzer (TGA) under the following conditions, and the content ratio (mass %) of the second PFPE in the surface layer relative to the total mass of the surface layer including the mass of the second PFPE in the pores was calculated.

[0225] Instrument: TGA851 (product name, manufactured by Mettler-Toledo International Inc.)

[0226] ·Atmosphere: In the air

[0227] Temperature: 425℃

[0228] In the measurement time-weight reduction rate curve obtained as a result of the above thermogravimetric analysis, a linear least squares approximate expression is obtained from the region where the slope is constant and only PFA is reduced. The intercept of the linear least squares approximate expression is taken as the PFA content (mass %), and the second PFPE content is calculated according to the second PFPE content (mass %) = 100-PFA content.

[0229] Performance evaluation as a fixing belt

[0230] The obtained fixing belt was subjected to the following evaluations B-1 and B-2.

[0231] Evaluation B-1: Evaluation of the presence or absence of toner smear

[0232] The fixing belt was mounted to an electrophotographic image forming apparatus (product name: imageRUNNER-ADVANCE C5051; manufactured by Canon Inc.) in which the angle of the paper separation claw had been adjusted.

[0233] Then, A4 size paper (manufactured by International Paper Co., Ltd., basis weight 75 g / m 2 ) was formed on a sheet of paper having a 10 cm×10 cm cyan solid image. The fixing temperature was set to 180° C., and the paper conveying speed was set to 300 mm / sec.

[0234] Once the number of solid cyan images formed reached 1 sheet, 10,000 sheets, and 300,000 sheets, respectively, a sheet of A4-sized plain thin paper (product name: CS-520, basis weight 52 g / m 2 , manufactured by Canon Inc.) to form a cyan solid image of 10 cm×10 cm. The solid image formed on the plain thin paper was observed visually and under a microscope, and evaluated according to the following criteria.

[0235] Evaluation Criteria

[0236] Rank A: There is neither toner smear nor missing toner.

[0237] Rank B: Very slight toner smear and missing toner were observed.

[0238] Rank C: Both toner smear and missing toner were observed.

[0239] Rank D: Ordinary thin paper becomes stuck to the fixing belt.

[0240] Evaluation B-2: Measurement of surface free energy

[0241] In Evaluation 1, the surface free energy of the outer surface of the fixing belt immediately before forming a solid image on ordinary thin paper was calculated according to the "Kitazaki-Hata method" described in the document "Journal of the Japan Adhesive Society", Japan Society for Adhesion, 1972, Vol. 8, No. 3, pp. 131-141. Specifically, the contact angles of the outer surface of the fixing belt with water, n-hexadecane and diiodomethane were measured (measurement environment: temperature 23° C., relative humidity 55%).

[0242] Then, the surface free energy was calculated based on the "Extended Fowkes equation" according to the "Kitazaki-Hata theory" described in the above document using the measurement results of each contact angle.

[0243] A contact angle meter (product name: DM-501, manufactured by Kyowa Interface Science Co., Ltd.) was used for measurement, and analysis software (product name: FAMAS, manufactured by Kyowa Interface Science Co., Ltd.) was used to analyze surface free energy.

[0244] Example 2

[0245] A laminated body provided with a resin layer having pores was produced in the same manner as in Example 1, except that the contact temperature between the resin layer and the first PFPE in the impregnation process-1 was set to the temperature given in Table 1. After the impregnation process-2, a fixing belt No. 2 was produced in the same manner as in Example 1. The results of evaluations A-1 to A-3 and evaluations B-1 and B-2 for the obtained fixing belt No. 2 are given in Tables 1 and 2.

[0246] Example 3

[0247] A laminated body provided with a resin layer having pores was produced in the same manner as in Example 1 except that the first PFPE in the impregnation process-1 was changed to the first PFPE shown in Table 1. After the impregnation process-2, a fixing belt No. 3 was produced in the same manner as in Example 1. The results of evaluations A-1 to A-3 and evaluations B-1 and B-2 for the obtained fixing belt No. 2 are shown in Tables 1 and 2.

[0248] Examples 4 to 5

[0249] The kind of the second PFPE used in the dipping process-2 was changed as shown in Table 1. Except for this, fixing belts No. 4 and 5 were produced in the same manner as in Example 3. The results of evaluations A-1 to A-3 and evaluations B-1 and B-2 for the obtained fixing belts No. 4 and 5 are shown in Tables 1 and 2.

[0250] Examples 6 and 7

[0251] A laminated body provided with a resin layer having pores was produced in the same manner as in Example 1 except that the thickness of the resin layer was changed as shown in Table 2. After the impregnation step-2, fixing belts No. 6 and 7 were produced in the same manner as in Example 3. The results of evaluations A-1 to A-3 and evaluations B-1 and B-2 for the obtained fixing belts No. 6 and 7 are shown in Tables 1 and 2.

[0252] Example 8

[0253] A laminated body having a resin layer having pores was produced in the same manner as in Example 1 except that the material kind of the resin layer in the impregnation process-1 and the contact temperature with the first PFPE were changed as shown in Table 1. After the impregnation process-2, a fixing belt No. 8 was produced in the same manner as in Example 1. The results of evaluations A-1 to A-3 and evaluations B-1 and B-2 for the obtained fixing belt No. 8 are shown in Tables 1 and 2.

[0254] Comparative Example 1

[0255] A laminate having a base layer, an elastic layer, and a resin layer containing PFA was produced in the same manner as in Example 1 and used as a fixing belt No. C-1 according to this comparative example. Table 2 lists the results of evaluations B-1 and B-2 for this fixing belt No. C-1. Fixing belt No. C-1 was not subjected to the impregnation process-1, the pore forming process, or the second impregnation process, and therefore evaluations A-1 to A-3 were not performed.

[0256] Comparative Example 2

[0257] A laminated body having a resin layer having pores was produced in the same manner as in Example 1 except that the material of the first PFPE in the method described in Example 1 was changed to the material given in Table 1. This laminated body was used as a fixing belt No. C-2 according to this comparative example. Tables 1 and 2 list the results of evaluations A-1 and A-2 and evaluations B-1 and B-2 conducted on the obtained fixing belt No. C-2. The fixing belt No. C-2 according to this comparative example did not undergo the immersion process-2, and therefore the evaluation A-3 was not conducted.

[0258] Comparative Example 3

[0259] Here, the material type of the first PFPE and the contact temperature in the impregnation step-1 of the method described in Example 1 were changed as shown in Table 1. The results of Evaluation A-1 for the obtained laminate, that is, the content ratio of PFPE in the resin layer containing the first PFPE obtained in the impregnation step-1 was 24% by mass.

[0260] When the laminate was subjected to the pore forming process described in Example 1, the first PFPE in the resin layer could not be removed. Although the underlying cause is not clear, it is considered that the first PFPE could not aggregate and connect in the resin layer due to the small impregnation amount, and the first PFPE therefore invaded between the molecules of PFA; as a result, the first PFPE could not be dissolved out with the solvent. Therefore, the impregnation process-2 was not performed, and the laminate obtained up to the impregnation process-1 was used as the fixing belt No. C-3 of this comparative example. Tables 1 and 2 list the results of Evaluation A-1 and Evaluations B-1 and B-2 performed on the obtained fixing belt No. C-3. As described above, even in the pore forming process, pores could not be formed in the resin layer, so the impregnation process-2 was not performed; therefore, Evaluation A-2 or Evaluation A-3 was not performed.

[0261] Comparative Examples 4 and 5

[0262] A substrate whose outer peripheral surface was subjected to primer treatment was prepared in the same manner as in Example 1. The primer-treated surface of the substrate was covered with a stretched porous PTFE tube (product name: Poreflon HP-010-30; manufactured by Sumitomo Electric Fine Polymer Inc.) to obtain a laminate having a porous resin layer. The second PFPE was introduced into the pores of the resin layer in the same manner as in the impregnation process-2 of Example 1, except that the laminate was used here. The contact time with the second PFPE was 3 minutes in Comparative Example 4 and 9 minutes in Comparative Example 5. The laminate obtained by impregnating the resin layer with the second PFPE was used as fixing belts No. C-4 and C-5. Tables 1 and 2 list the results of evaluations A-2 and A-3 and evaluations B-1 and B-2 for fixing belts No. C-4 and C-5.

[0263] Comparative Example 6

[0264] A substrate having a primer-treated peripheral surface is prepared in the same manner as in Example 1. Next, a non-crystalline fluoropolymer (product name: Teflon AF2400, manufactured by The Chemours Company) is dissolved in a fluorine solvent (product name: Novec 7300, manufactured by The 3M Company) to prepare a 2.0 mass % solution. The substrate is immersed in the above solution and then coated according to the dipping method so that the film thickness is 20 μm. The dipping time is 10 sec, and the pulling-up speed is 30 mm / sec. The substrate having a coating film of the solution formed on the peripheral surface is then dried in an oven at a temperature of 160° C. for 15 minutes to obtain a laminate having a porous polytetrafluoroethylene (PTFE) film on the surface. In addition to using this laminate, the pores of the porous PTFE membrane are impregnated with PFPE-3 in the same manner as in the dipping process-2 of Example 1 to obtain a fixing belt according to this comparative example. Tables 1 and 2 list the results of Evaluations A-2 and A-3 and Evaluations B-1 and B-2 of the obtained fixing belts.

[0265] Table 1 lists the formulations of the fixing belts produced in Examples 1 to 8 and Comparative Examples 1 to 6.

[0266] [Table 1-1]

[0267]

[0268] *[Mass of impregnated PFPE / (Mass of impregnated PFPE+Mass of the resin layer itself)]×100

[0269] *1 is the content ratio of the first PFPE in the PFPE-impregnated resin layer obtained in the impregnation step-1.

[0270] [Table 1-2]

[0271]

[0272] *[Mass of impregnated PFPE / (Mass of impregnated PFPE+Mass of the resin layer itself)]×100

[0273] *2 is the content ratio of the second PFPE in the surface layer.

[0274] Table 2 lists the evaluation results of the rotating members for fixing produced in Examples 1 to 8 and Comparative Examples 1 to 6.

[0275] [Table 2]

[0276]

[0277] Table 2 shows that in the fixing rotating members of Examples, excellent toner releasability can be maintained even after long-term use, and as a result, high-quality electrophotographic images can be formed.

[0278] One aspect of the present disclosure makes it possible to obtain a fixing rotating member that can maintain high toner releasability for a long time. Other aspects of the present disclosure make it possible to realize a fixing device and an electrophotographic image forming device that can stably form high-quality electrophotographic images for a long time.

[0279] While the present disclosure has been described with reference to exemplary embodiments, it is to be understood that the present disclosure is not limited to the disclosed exemplary embodiments.The scope of the following claims is to be accorded the broadest interpretation so as to encompass all such modifications and equivalent structures and functions.

Claims

1. A fixing rotating member, which comprises a base layer, an elastic layer and a surface layer in sequence, The surface layer comprises tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer and perfluoropolyether; The surface layer has holes having openings on a first surface thereof constituting an outer surface of the fixing rotating member; At least a portion of the pores comprise the perfluoropolyether, characterized in that When a first observation region of 8 μm in length×11 μm in width is provided on the first surface of the surface layer after the perfluoropolyether in the pores is removed, and a ratio of the sum of the areas of the openings observed in the first observation region to the area of ​​the first observation region is defined as P1; and When a second observation area of ​​8 μm in length and 11 μm in width is set in the cross section of the surface layer after the perfluoropolyether in the holes is removed, a ratio of the sum of the areas of the holes observed in the second observation area to the area of ​​the second observation area is defined as P2, and the cross section includes the entire thickness portion of the surface layer in the circumferential direction of the fixing rotating member, P2 / P1 is 1.3 or more.

2. The fixing rotating member according to claim 1, wherein P1 is between 1.0% and 15.0%; and P2 is 20.0% to 60.0%.

3. The fixing rotating member according to claim 1 or 2, The content of the perfluoropolyether in the surface layer is 20% by mass to 60% by mass. 4 . The fixing rotation member according to claim 1 , wherein an average opening diameter of the openings in the outer surface of the surface layer is 1 to 5 μm. 5 . The fixing rotating member according to claim 1 , wherein the surface layer has a thickness of 12 to 100 μm.

6. The fixing rotating member according to claim 1 or 2, wherein the perfluoropolyether has a structure represented by the following formula (1); In formula (1), a, b, c, d, e and f are each independently 0 or a positive integer, satisfying 1≤a+b+c+d+e+f≤600, and at least one of a, b, c and d represents a positive integer.

7. The fixing rotating member according to claim 1 or 2, The perfluoropolyether has at least one structure selected from the group consisting of formula (2) to formula (5): In formula (2), n is a positive number, and n is within a range such that the viscosity of PFPE at a temperature of 40° C. is in a range of 30 to 500 mPa·s; In formula (3), n′ is a positive number, and n′ is within a range such that the viscosity of PFPE at a temperature of 40° C. is in a range of 10 to 2500 mPa·s; In formula (4), n″ and m are each independently a positive number, m / n″ is a number from 0.5 to 2, and n″+m is a number within a range such that the viscosity of PFPE at a temperature of 40° C. is within a range of 20 to 1400 mPa·s; and In formula (5), n'' and m' are each independently a positive number, m' / n'' is a number from 20 to 1000, and n''+m' is a number within a range such that the viscosity of PFPE at a temperature of 40° C. is within a range of 20 to 1200 mPa·s.

8. The fixing rotating member according to claim 1 or 2, wherein P2 / P1 is 5.0 or more.

9. The fixing rotating member according to claim 1 or 2, wherein the fixing rotating member is a fixing belt having an endless belt shape.

10. The fixing rotating member according to claim 1 or 2, wherein P2 / P1 is 20.0 or less.

11. A fixing device, characterized in that: It comprises the fixing rotating member according to any one of claims 1 to 10, and a heating means for heating the fixing rotating member.

12. The fixing device according to claim 11, wherein The fixing rotating member is a fixing belt having an endless belt shape; and The heating member is a heater disposed in contact with the inner peripheral surface of the fixing belt.

13. An electrophotographic image forming device, characterized in that: It comprises the fixing device according to claim 11 or 12.

Citation Information

Patent Citations

  • Fixing member, fixing device, and electrophotographic image-forming apparatus

    WO2019181796A1

  • Heating fixing belt, fixing device and process for forming heating fixing belt

    CN102799094A

  • Intermediate transfer members containing fluorinated polyamic acids

    CN103454887A