Ionic liquid-based liquid compositions for protecting lithium metal components, related coating and polymerization methods, and electrochemical storage systems
By depositing a polymer coating composed of ionic liquids on the lithium battery anode, the problem of dendrites and surface defects in the lithium battery anode is solved, low-cost and efficient lithium metal protection is achieved, the formation of dendrites is delayed and the efficiency is improved. Battery safety and performance.
Patent Information
- Application Number
- CN202080060715.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-07-31
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-07-31
AI Technical Summary
The lithium metal anode of lithium batteries is prone to forming dendrites and surface defects during charge and discharge cycles, resulting in reduced battery life and safety issues. Existing technical solutions are costly or rely on expensive lithium salts, and there are physical blocking methods for solid electrolytes. limitations.
Using a liquid composition based on ionic liquids, including polymerizable ionic liquids, non-polymerizable ionic liquids, cross-linker type ionic liquids, lithium salts and ionic polymers, a polymer coating is formed through deposition and polymerization to protect Lithium metal anode, the coating is composed of all ionic components and has good mechanical, chemical and electrochemical stability.
A simpler, lower-cost lithium metal anode protection is achieved, which improves the anode's mechanical properties and ionic conductivity, delays dendrite formation, avoids the risk of short circuits, and maintains good electrochemical performance at high temperatures.
Smart Images

Figure CN114730857B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to liquid compositions based on ionic liquids for use in protecting lithium metal components, particularly anodes, in lithium electrochemical generators.
[0002] The invention also relates to a method for coating metal parts, the implementation of such a composition, the subsequent polymerization of the composition and an electrochemical storage system having an anode coated thereby. Background Art
[0003] Lithium metal is the preferred negative electrode material for lithium batteries because it has the highest theoretical capacity and the lowest electrochemical potential among all candidates. However, charge and discharge cycles of lithium metal anode batteries can lead to the formation of dendrites and other surface defects, which can reduce battery life and also cause short circuits, which can lead to serious safety issues (thermal runaway, explosion, fire).
[0004] Due to Li + Due to the highly negative electrochemical potential of the Li / Li redox couple, current liquid electrolytes are reduced on the lithium surface to form a solid electrolyte interface (SEI) [1]. This passivation allows the operation of electrochemical cells. The SEI must be an ion conductor and an electrical insulator with uniform composition and morphology. It must also have good flexibility and elasticity [2]. Additives are used in electrolytes. They decompose and participate in the formation of the SEI to improve the properties of the electrochemical cell and thus improve performance.
[0005] Very high concentrations of lithium salts in the electrolyte can also suppress dendrite growth. However, this solution is very lithium salt-intensive and therefore very expensive.
[0006] One approach is to deposit a protective layer (artificial SEI) on the lithium by various thin-film deposition techniques before cycling.
[0007] Solid electrolytes have been developed and used as a means to physically prevent dendrite growth. They can be organic (polymers), inorganic (ceramics), or hybrid.
[0008] EP 3 049 471 B1 discloses a lithium ion conductive polymer composition for a lithium electrochemical generator, which comprises at least one non-ionic polymer.
[0009] WO2016205653A “Multilayer polymer-coated Li anode for high-density Li metal batteries” discloses two layers of polymers.
[0010] US9627713B2 "Composite electrolyte comprising a polymer ionic liquid matrix and embedded nanoparticles, and method for preparing the same" discloses a composite electrolyte comprising inorganic nanoparticles, thus being a hybrid organic / inorganic composition. This layer protects both the lithium and the electrolyte. The resulting battery does not contain a liquid electrolyte.
[0011] US20160164102A1 discloses a metal, organic / inorganic hybrid (inorganic part = ceramic nanoparticles) protective coating. The coating contains an ionic liquid and is obtained by UV polymerization.
[0012] US5961672B discloses a stabilized anode for lithium polymer batteries. The technology for depositing the lithium protective film is vacuum deposition.
[0013] WO2018 / 122428A1 discloses a coating composition comprising an ionic liquid and a cross-linked polymer ionic liquid, wherein the cross-linked polymer ionic liquid and the ionic liquid are not bound by covalent bonds, and wherein the cross-linked polymer ionic liquid is bound to the surface of a substrate.
[0014] The object of the present invention is to overcome these drawbacks by providing a liquid composition for protecting lithium metal which is simpler and less expensive to implement than currently available protection compositions. Summary of the invention
[0015] This object is achieved by the following ionic liquid-based composition, which is used to protect the lithium metal anode of a lithium-based electrochemical energy storage system and comprises:
[0016] - a polymerizable ionic liquid (or an ionic liquid monomer), the cation or anion of which carries at least one polymerizable functional group,
[0017] - non-polymerizable ionic liquids,
[0018] - ionic liquids of the "crosslinker" type, the cations or anions of which carry at least two polymerizable functional groups,
[0019] - lithium salts, and
[0020] -Ionic polymers.
[0021] Such ionic polymers can help improve the mechanical properties of the anode.
[0022] The liquid composition according to the invention may also advantageously comprise a UV or thermal polymerization initiator. Such polymerization initiators degrade during the polymerization and are present in negligible amounts.
[0023] According to another aspect of the present invention, there is provided a method for coating a lithium metal sheet, such as a lithium anode of an electrochemical generator, with a liquid protective composition obtained by depositing and polymerizing the liquid formulation of the present invention, comprising the following steps:
[0024] - depositing a liquid solution having said composition on said metal part,
[0025] - polymerizing the liquid solution thus deposited under the action of UV radiation or heat.
[0026] The deposition step may be performed by applying a film of a liquid solution or by immersing the metal part in the liquid solution.
[0027] The polymer coatings thus obtained differ from those of the prior art in that all components of the formulation are ionic.
[0028] According to another aspect of the present invention, there is provided a lithium-based electrochemical storage system (e.g., a lithium sulfur battery, a lithium metal battery, a lithium ion battery, a lithium ion capacitor), comprising a lithium anode covered with such a deposited layer having the ionic composition of the present invention.
[0029] In the present invention, there is only one polymer layer (between the metallic Li and the electrolyte). These are only ion-based polymers and components.
[0030] The composition according to the invention is only organic. It is a protective layer for lithium, and this "protected" lithium can form the anode of a battery containing a liquid electrolyte.
[0031] The coating used in the present invention is simply deposited, whereas in the prior art, the coating is covalently bonded to the surface of the lithium metal. All components are ionic and therefore participate in the overall ionic conductivity.
[0032] Due to the combination of ionic elements and lithium salts, the protective coating thus obtained constitutes a lithium ion conducting membrane.
[0033] The membrane is mechanically, chemically, and electrochemically stable when in contact with metallic lithium.
[0034] It has very good ionic conductivity (6x10 -2 mS / cm, 4.9x10 at 80°C -1 mS / cm), which is lower than that of the prior art document EP3049471B1 (5x10 -2 mS / cm) is one order of magnitude higher.
[0035] All components of the membrane are ionic, which provides good conductivity, while other formulations of the prior art still have neutral components.
[0036] The protective composition according to the invention can produce a variety of combinations of materials in order to optimize the composition according to the cathode material to be selected. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] The accompanying drawings will detail some examples of embodiments of the present invention, in particular:
[0038] · Figure 1 It shows the coating process of the ionic liquid-based polymer composition on the surface of the metallic lithium foil;
[0039] · Figure 2 Figure 2 shows the stripping and deposition tests of a symmetric cell with bare lithium and lithium protected by an ionic liquid-based polymer at 0.5 mA cm in the first cycle. -1 The current density was maintained for 4 h and then at 0.5 mA cm -1 The current density lasted for 2 hours.
[0040] · Figure 3 SEM images showing a) top view and b) cross section of a bare lithium surface; c) top view and d) cross section of a lithium surface covered with a polymer protective composition.
[0041] · Figure 4 Schematic diagram showing a lithium metal based electrochemical cell of the present invention.
[0042] · Figure 5 Impedance spectroscopy measurements in a symmetric cell after 30 min and 1240 min of OCV are shown.
[0043] · Figure 6 Shown are the charge and discharge voltage curves of LFP in combination with bare lithium as the negative electrode or protected by a polymer composition. DETAILED DESCRIPTION
[0044] An example of the formulation of the polymer protective composition according to the present invention will now be described.
[0045] All components of the formulations are known from the prior art.
[0046] The deposition of liquid solutions onto solid surfaces can be performed by different liquid solution deposition techniques (film coating, immersion, etc.).
[0047] The polymerization of the liquid solution layer can be performed by UV or heat.
[0048] The electrochemical cell according to the invention can be manufactured according to known techniques. The use of such a protected lithium anode allows the use of an electrolyte that has not been modified by the various additives mentioned above, or simply serves as both electrolyte and separator.
[0049] The polymerizable ionic liquid whose cation or anion carries at least one polymerizable functional group may have the following form (Table 1), as a non-limiting example, with a concentration of 50 to 70 wt %, typically 60 wt %.
[0050]
[0051] Table 1: Examples of different cations carrying at least one polymerizable functional group and possible associated anions
[0052] As shown in Table 1, different anions can be selected from hexafluorophosphate (PF6 - ), perchlorate ClO4 - ), tetrafluoroborate (BF4 - ), hexafluoroarsenate (AsF6 - ), trifluoromethanesulfonate (CF3SO3 - ), bis(trifluoromethanesulfonyl)imide (known as TFSI)N[SO2CF3]2, bis(fluorosulfonyl)imide (known as FSI)LiN[SO2F]2 - 、Bis(pentafluoroethanesulfonyl)imide、N(C2F5SO2)2 - (known by the abbreviation BETI), 4,5-dicyano-2-(trifluoromethyl)imidazoline (known by the abbreviation TDI) and mixtures thereof, preferably LiTFSI, LiFSI and LiTDI.
[0053] Other examples may include other types of cations such as imidazolium, pyrrolidinium, ammonium, pyridinium, pyridazinium, pyrimidinium, pyrazinium, pyrazolium, thiazolium, oxazolium, triazolium, phosphonium, sulfonium. Some such cations are shown below:
[0054]
[0055]
[0056] The non-polymerizable ionic liquid may be in the form, by way of non-limiting example, of a concentration of 30% to 50% by weight, typically 40% by weight.
[0057]
[0058] Table 2: Examples of different cations and anions associated with obtaining non-polymerizable ionic liquids
[0059] Other examples may include other types of cations, such as imidazolium, pyrrolidinium, ammonium, pyridinium, pyridazinium, pyrimidinium, pyrazinium, pyrazolium, thiazolium, oxazolium, triazolium, phosphonium, sulfonium. As shown in Table 2, different anions may be selected from hexafluorophosphate (PF6 - ), perchlorate ClO4 - ), tetrafluoroborate (BF4 - ), hexafluoroarsenate (AsF6 - ), trifluoromethanesulfonate (CF3SO3 - ), bis(trifluoromethanesulfonyl)imide (known as TFSI)N[SO2CF3]2, bis(fluorosulfonyl)imide (known as FSI)LiN[SO2F]2 - 、Bis(pentafluoroethanesulfonyl)imide、N(C2F5SO2)2 - (known by the abbreviation BETI), 4,5-dicyano-2-(trifluoromethyl)imidazoline (known by the abbreviation TDI) and mixtures thereof, preferably LiTFSI, LiFSI and LiTDI.
[0060] An ionic liquid of the "crosslinker" type whose cation carries at least two polymerizable functional groups may have the following form, as a non-limiting example, in a concentration ranging from 1 to 5 mol %, typically 3 mol %, relative to the polymerizable liquid ion: 1,4-butanediyl-3,3'-bis-l-vinylimidazolium cation:
[0061]
[0062] The lithium salt may be selected from hexafluorophosphate (PF6 - ), perchlorate ClO4 - ), tetrafluoroborate (BF4 - ), hexafluoroarsenate (AsF6 - ), trifluoromethanesulfonate (CF3SO3 - ), Lithium bis(trifluoromethanesulfonyl)imide (known as LiTFSI) LiN[SO2CF3]2, Lithium bis(fluorosulfonyl)imide (known as LiFSI) LiN[SO2F]2 - , lithium bis(pentafluoroethanesulfonyl)imide LiN(C2F5SO2)2 (known by the abbreviation LiBETI), lithium 4,5-dicyano-2-(trifluoromethyl)imidazole (known by the abbreviation LiTDI) and mixtures thereof, preferably LiTFSI, LiFSI and LiTDI.
[0063] As a non-limiting example, the lithium salt may be present in the composition in a molar ratio relative to the non-polymerizable ionic liquid in a range from a 1:9 molar ratio to a 2:3 molar ratio.
[0064] The ionic polymer contained in the polymer composition according to the present invention may have the following form, as a non-limiting example, with a concentration of 1 mol % to 5 mol % relative to the polymerizable ionic liquid: poly(diallyldimethylammoniumbis(trifluoromethylsulfonyl)imide) or poly(diallyldimethylammoniumbis(fluorosulfonyl)imide), as shown below:
[0065]
[0066] The polymerization initiator may be selected from the following materials or compositions: phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide is a successfully used example, and its concentration is 1 mol % to 5 mol % relative to the polymerizable ionic liquid.
[0067] Examples of membrane preparation:
[0068] The polymer composition based on ionic liquid was prepared in a glove box filled with argon. To a mixture of 40 wt% of non-polymerizable ionic liquid N,N-diethyl-N-methyl-N-(2-methoxyethyl)ammonium bis(trifluoromethylsulfonyl)imide (DEMETFSI) and 60 wt% of polymerizable ionic liquid l-ethyl-3-vinyl imidazole bis(trifluoromethylsulfonyl)imide (EVIMTFSI), 3 mol% of "crosslinker" type ionic liquid l,4-butanediyl-3,3'-bis-l-vinyl imidazole di-bis(trifluoromethylsulfonyl)imide (BVIMTFSI) was added relative to EVIMTFSI. After all components were dissolved, lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) was added at a molar ratio of 1:9 relative to DEMETFSI. Finally, 2 wt% of poly(diallyldimethylammonium bis(trifluoromethylsulfonyl)imide) (polyDDATFSI) was added relative to EVIMTFSI. For crosslinking polymerization of the polymer ionic liquid mixture, the UV curing agent phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide was added at 3.5 wt% relative to EVIMTFSI.
[0069] After all components are dissolved to form a liquid viscous slurry, the metallic lithium ( Figure 1 ). Lithium covered with this preparation was exposed to UV light for 5 minutes to form a cross-linked polymeric protective layer on the lithium surface. The prepared protection was tested in a symmetrical two-electrode pouch cell. The stripping and deposition cycles were carried out at 0.5 mA / cm in the first cycle. 2 The cycle was repeated for 4 hours, with 0.5 mA / cm 2 In all experiments, an area of 2 cm 2of electrodes.
[0070] Figure 2 Figure 2. Cycling of a symmetric cell showing a bare Li surface and a protected Li surface with an ionic liquid based polymer protective layer. The shape and the way in which the peaks evolve with cycling are different for both surfaces. For both surfaces, the overpotential of the cell increases with cycling. After the 15th cycle, some spikes appear that are related to HSAL formation and short circuits. Short circuiting occurs on the bare Li surface after the 25th cycle and then, for the next cycle potential, the cycling ends. For the protected Li with an ionic liquid based polymer composition, the cycling never ends with a potential cutoff as the potential limit is never reached and the cell is still working even after 70 cycles. It is observed that the coating does not completely avoid the formation of dendrites but it can delay the short circuits caused by them.
[0071] Film uniformity and thickness
[0072] The polymerizable protective composition was characterized using a field emission scanning electron microscope (FE SEM) Supra 35VP (Zeiss, Germany). The samples were prepared and attached to a custom vacuum transfer holder in an argon-filled glove box that was opened in the SEM chamber under reduced pressure. SEM images of the bare lithium surface and the lithium surface covered with the polymerizable protective composition are shown in Figure 2. Figure 3 shown.
[0073] The bare lithium surface is rough and uneven (3a, b). When the polymerizable protective composition is applied on the Li surface (3c, d), the uneven surface is covered by a smooth, dense and very uniform layer with some pores due to direct polymerization on the lithium surface. In the cross-sectional view (3d), it can be observed that the polymerizable protective composition adheres well to the lithium surface. An estimated thickness of 60 μm was determined.
[0074] The composition based on ionic liquids according to the invention is applied to one of the two faces of the lithium sheet by a deposition technique known to the person skilled in the art (e.g. a knife coater, e.g. reference K Control Coater from RK Print, Figure p. 14). Polymerization then takes place, producing a lithium protective film. When the battery is assembled, the protected face of the lithium faces the second electrode (cathode), e.g. Figure 4 shown.
[0075] Conductivity of polymerizable protective composition
[0076] To determine the ionic conductivity, a 200-cm thick, 87-μm-thick, 0.78-cm-thick 2 A free-standing polymeric protective composition film is sandwiched between two copper foils. Nyquist plots are obtained at different temperatures. Ionic conductivity The value is obtained from the impedance measurement using the following formula: where t and S are the thickness and surface of the film, respectively, and R is the ohmic resistivity. The ionic conductivity obtained is 3.6x10 -2 mS.cm -1 , at 80℃ is 4.9x10 -1 mS.cm -1 .
[0077] Stability and compatibility of protective polymer compositions with lithium metal
[0078] The stability and compatibility of the ionic liquid-based polymer membranes with metallic Li were measured by impedance spectroscopy in symmetric cells after 30 and 1240 min at OCV. Figure 5 The measured spectrum shown in Figure 1 is matched to the equivalent circuit in the inset. For this circuit, R1 corresponds to the electrolyte resistance, and the sum of R2 and R3 corresponds to the resistance of the lithium surface: the charge transfer resistance and the resistance of the SEI at the lithium electrode.
[0079] For bare lithium, the sum of R2 and R3 increases from 49Ω for the cell 30 minutes after assembly to 76Ω after 1240 minutes. This 55% increase is related to the formation of the SEI layer as the metallic lithium surface is exposed to the electrolyte when the cell is stored at OCV. In contrast, the resistance of the lithium symmetric cell with ionic liquid-based polymer@Li changes from 37W at 30 minutes after assembly to 35W after 1240 minutes.
[0080] The film protects the metal surface from continued consumption of the electrolyte, thereby preventing the SEI from growing over time when the battery is stored at OCV. As a result, the impedance barely changes during the measurement. Once the lithium surface is covered with the protective ionic liquid-based polymer film, the growth of the passivation film is not as fast as on a bare lithium surface.
[0081] Charging and discharging curves of a complete battery
[0082] Figure 6 The charge and discharge voltage curves of LFP assembled with bare lithium as the negative electrode or with lithium protected by a polymer composition are shown. The cathode is made of LFP and the anode is made of lithium metal and coated with a protective polymer composition.
[0083] The voltage curves are slightly different, but the capacities are almost the same. The voltage evolution at the beginning of a half-cycle (charge or discharge) is slower for cells with lithium protected by the polymer composition as anode than for cells with bare Li, so the LFP / Li protected cells take longer to reach the voltage plateau. These can be attributed to the effects caused by the delayed mass transport of lithium protected by the polymer composition samples discussed previously. However, this does not seem to have a negative impact on the cycling of full cells using LFP as cathode at low current density at room temperature. In this study, independent of the choice of anode, the charge and discharge curves of both cells as well as the cell capacity (155 mAh g -1 ) are almost the same. However, using lithium protected by a polymer composition as the negative electrode can achieve more stable cycling and better Coulombic efficiency.
[0084] Of course, the invention is not limited to the embodiment that has just been described, and many other embodiments of the polymer composition according to the invention can be envisaged. In particular, several polymerizable liquid ions whose cations or anions carry at least one polymerizable functional group, a plurality of non-polymerizable ionic liquids, several ionic liquids of the "crosslinker" type whose cations or anions carry at least two polymerizable functional groups, several lithium salts and several ionic polymers can be provided in the composition.
[0085] References
[0086] 1. Peled, E. The electrochemical behavior of alkali and alkaline earthmetals in nonaqueous battery systems—the solid electrolyte interphase model. J. Electrochem. Soc. 126, 2047-2051 (1979).
[0087] 2.Aurbach,D.Review of selected electrode-solution interactions whichdetermine the performance of Li and Li ion batteries.J.Power Sources 89,206-218(2000).Cohen,Y.S.,Cohen,Y.&Aurbach,D.Micromorphological studies of lithiumelectrodes in alkyl carbonate solutions using in situ atomic forcemicroscopy.J.Phys.Chem.B 104,12282-12291(2000).
Claims
1. An ionic liquid-based composition for protecting a lithium anode of an electrochemical storage cell, comprising: - a polymerizable ionic liquid or an ionic liquid monomer, the cation or anion of which carries at least one polymerizable functional group, - non-polymerizable ionic liquids, - ionic liquids of the "crosslinker" type, the cations or anions of which carry at least two polymerizable functional groups, - lithium salts, and -Ionic polymers.
2. The ionic liquid-based composition according to claim 1, It is characterized in that The polymerizable ionic liquid or ionic liquid monomer whose cation and / or anion carries at least one polymerizable functional group has the following form, wherein R 1 , R 2 , R 3 and R 4 Is a polymerizable chemical functional group:
3. The ionic liquid-based composition according to claim 1 or 2, It is characterized in that The non-polymerizable ionic liquid has the following form, the cations and anions of which do not carry any polymerizable chemical functional groups:
4. The ionic liquid-based composition according to claim 1 or 2, It is characterized in that The type of ionic liquid crosslinker whose cation or anion carries at least two polymerizable functional groups has the following form, wherein R 5 , R 6 , R 7 and R 8 Is a polymerizable chemical functional group:
5. The ionic liquid-based composition according to claim 1 or 2, It is characterized in that The lithium salt is selected from the following forms:
6. The ionic liquid-based composition according to claim 1 or 2, It is characterized in that The ionic polymer is selected from polymers of the form: wherein n and m are the number of repeating monomer units:
7. The ionic liquid-based composition according to claim 1, It is characterized in that It also contains a UV or thermal polymerization initiator.
8. A method for coating a lithium anode of an electrochemical storage cell, said method implementing a protective polymer composition obtained by depositing and polymerizing a composition based on an ionic liquid as claimed in any one of claims 1 to 7, said method The following steps are involved: - depositing a liquid solution having said composition on a lithium anode of said electrochemical storage cell, - polymerizing said liquid solution thus deposited.
9. The method according to claim 8, It is characterized in that The deposition step is performed by applying the liquid solution to one of the two faces of a lithium sheet, and the polymerization step produces a protective film of lithium.
10. The method according to claim 8, It is characterized in that The deposition step is performed by immersing the lithium sheet into the liquid solution.
11. A lithium-based electrochemical storage device, include: A lithium anode coated with a polymer composition obtained by depositing and polymerizing the ionic liquid-based composition of any one of claims 1 to 7, the lithium anode facing the cathode.
Citation Information
Patent Citations
Polymer compositions that conduct lithium ions for electrochemical lithium generator
EP3049471B1
Protective coating of metal
US20160164102A1
Stabilized anode for lithium-polymer batteries
US5961672A
Composite electrolyte including polymeric ionic liquid matrix and embedded nanoparticles, and method of making the same
US9627713B2
Multi-layer polymer coated li anode for high density li metal battery
WO2016205653A1