Solid electrolyte doped amorphous carbon coated graphite composite material and preparation method thereof
By doping metal lithium in porous graphite and depositing solid electrolytes on its shell to form a core-shell structure, the problem of taking into account the fast charging performance and energy density of the negative electrode material of lithium-ion battery is solved, and the lithium ion transmission rate and electrons are achieved The improvement of conductivity significantly improves the power and cycling performance of the material.
Patent Information
- Application Number
- CN202411046981.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-15
AI Technical Summary
The existing lithium-ion battery negative electrode materials are difficult to take into account both the fast charging performance and the energy density. The dispersion performance of solid electrolytes is poor and the liquid phase coating has uniformity problems. The atomic vapor deposition process is controllable but the thickness is thin.
Doping metal lithium in porous graphite, solid electrolyte is deposited on its shell to form a core-shell structure, and solid electrolyte is deposited by atomic vapor deposition method to improve the energy density and fast charging performance of the material.
The lithium ion transmission rate and electron conductivity are improved, the synergistic effect improves power performance and energy density, and the uniformity of lithium metal solution and the thin-layer characteristics of the atomic vapor deposition method improve the fast charging performance and cycling performance of the material.
Smart Images

Figure CN118970003A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of secondary battery material preparation, in particular to a solid electrolyte doped amorphous carbon coated graphite composite material and a preparation method thereof. Background Art
[0002] As the market's requirements for the fast-charging performance of lithium-ion batteries increase, the negative electrode materials used are required to have high energy density while also improving their fast-charging performance. At present, the market-oriented negative electrode materials are mainly artificial graphite, and soft carbon or hard carbon is coated on its surface to improve the fast-charging performance of the material. If the coating amount is too high, the energy density of the negative electrode material will be reduced. If the coating amount is too low, the fast-charging performance of the material will be limited. Solid electrolytes have the characteristics of high lithium ion conductivity and good safety performance, but their dispersion performance is poor. If liquid phase coating is used on the graphite surface, the coating uniformity is poor, and the coating thickness is too high to reduce its energy density. The atomic vapor deposition method has the advantages of high deposition density, thin thickness, high consistency, and controllable process. Coating on the graphite surface can improve the fast-charging performance of graphite composites while taking into account energy density. Summary of the invention
[0003] In order to improve the fast charging performance and energy density of its graphite negative electrode material, the present invention improves the initial efficiency of the material by doping metallic lithium into the porous graphite, and deposits a solid electrolyte in its outer shell to improve the energy density of the material and its fast charging performance.
[0004] A solid electrolyte doped amorphous carbon-coated graphite composite material, characterized in that its composite negative electrode material presents a core-shell structure, the core is graphite, and the shells are, from the inside to the outside, a first shell and a second shell, the first shell is lithium-doped amorphous, and the second shell is composed of a solid electrolyte; calculated based on the mass ratio of the composite material as 100%, the mass of the first shell accounts for 1-10wt%, and the mass of the second shell accounts for 1-10wt%.
[0005] A solid electrolyte doped amorphous carbon coated graphite composite material, characterized in that the shell is composed of 1-5wt% lithium oxide, 1-5wt% conductive agent, and 80-98wt% amorphous carbon.
[0006] A method for preparing a solid electrolyte doped amorphous carbon-coated graphite composite material, characterized in that it comprises the following steps:
[0007] Step S1:
[0008] According to the mass ratio of metal lithium: passivator: inert solvent = 1-10: 0.5-2: 500-1000, metal lithium and passivator are added to the inert solvent, and heated at a temperature of 120-200° C. for reaction for 0.5-3 hours to obtain a lithium metal solution;
[0009] The passivating agent is one of tetraethylene glycol dimethyl ether, ethyl propyl sulfide, diethylene glycol dimethyl ether, and propenyl phenyl ether;
[0010] The inert solvent is one of undecane, dodecane and dimethyl silicone oil;
[0011] Step S2:
[0012] According to the mass ratio of porous graphite: lithium metal solution: resin solution: conductive agent solution = 100:500-1000:100:100, in an inert atmosphere, the porous graphite is added to the lithium metal solution and dispersed evenly, and vacuum soaked at a temperature of 50-100° C. for 12-36 hours, filtered, and the obtained material is added to a 1-10wt% resin solution, and 0.5-5wt% conductive agent solution is added, dispersed evenly, filtered, and the obtained filter residue is vacuum dried at 80° C. for 24 hours, and then carbonized at a temperature of 700-1000° C. for 0.5-2 hours to obtain a lithium oxide / amorphous carbon-coated graphite precursor material;
[0013] Step S3:
[0014] By atomic vapor deposition, the ALD chamber is opened, and the lithium oxide / amorphous carbon-coated graphite precursor material is transferred to the vacuum chamber and evacuated to 1-10pa, and the temperature is raised to 100-500°C. Then, the solid electrolyte is introduced for 1S, the pulse time is 115s, nitrogen purge is 60 seconds, nitrogen purge is 5 seconds, nitrogen purge is 50 seconds, and the carrier gas flow rate is 50-500sccm. It is deposited on the surface of the lithium oxide / amorphous carbon-coated graphite precursor material for 10-120min to obtain a solid electrolyte doped amorphous carbon-coated graphite composite material.
[0015] The preparation method of porous graphite in step S2 is to mix and bond graphite with a binder solution, dry it, then add it to a potassium permanganate aqueous solution with a molar concentration of 1-12 mg / mL, react it at a temperature of 60-100° C. for 1-6 hours, wash and dry it to obtain porous graphite.
[0016] In step S2, the conductive agent solution is a carbon nanotube conductive liquid, a graphene conductive liquid, or a carbon black conductive liquid, with a mass concentration of 0.5-5wt%, and the solvent is deionized water.
[0017] In step S2, the resin solution is one of urea-formaldehyde resin, melamine formaldehyde resin and polyurethane resin, and the solvent is deionized water.
[0018] The solid electrolyte in step S3 is Li 7 La 3 b Zr 2 Mb 12, where M=Bi or Y and 0<b<1.
[0019] Beneficial effects:
[0020] 1) The metallic lithium doped in the graphite core is used to reduce the defects of the material and improve the initial efficiency. At the same time, the porous graphite has more holes and channels to improve the lithium ion transmission rate of the material, and the hard carbon obtained after the carbonization of the outer resin improves the electronic conductivity of the material. The synergistic effect between the metallic lithium and the hard carbon is brought into play to improve the power performance and energy density of the material.
[0021] 2) Using lithium metal solution to supplement lithium in its graphite oxide has good uniformity, high initial efficiency, and the unreacted lithium can provide sufficient lithium ions during the charge and discharge process, thereby improving the cycle performance;
[0022] 3) The atomic vapor deposition method is used to deposit solid electrolyte on the graphite, relying on the high ion conductivity, stable structure and thin deposition thickness of the solid electrolyte itself to improve the fast charging performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a SEM image of the solid electrolyte-doped amorphous carbon-coated graphite composite material of Example 1. DETAILED DESCRIPTION
[0024] Preparation method of porous graphite:
[0025] 95g of artificial graphite was mixed with 100g of LA132 binder solution with a mass concentration of 5wt%, dried at 80℃ under vacuum for 24h, ground, and then added to a 500ml potassium permanganate aqueous solution with a molar concentration of 6mg / mL, and reacted at 80℃ for 3h, washed with deionized water, and dried at 80℃ under vacuum for 24h to obtain porous graphite.
[0026] Example 1
[0027] A method for preparing a solid electrolyte doped amorphous carbon-coated graphite composite material comprises the following steps:
[0028] Step S1:
[0029] 5 g of metallic lithium and 1 g of tetraethylene glycol dimethyl ether were added to 800 g of undecane inert solvent, and heated at 150° C. for 1 h to obtain a lithium metal solution;
[0030] Step S2:
[0031] Under an argon inert atmosphere, 100 g of porous graphite is added to 800 g of lithium metal solution and dispersed evenly, and vacuum-immersed at 80° C. for 24 hours, filtered, and the obtained material is added to 100 g of 5 wt% urea-formaldehyde resin aqueous solution, and 100 g of 1 wt% carbon nanotube conductive agent solution is added, dispersed evenly, filtered, and the obtained filter residue is vacuum-dried at 80° C. for 24 hours, and then carbonized at 800° C. for 1 hour to obtain a lithium oxide / amorphous carbon-coated graphite precursor material; Step S3:
[0032] Using atomic vapor deposition, the ALD chamber was opened, and the lithium oxide / amorphous carbon-coated graphite precursor material was transferred into the vacuum chamber and evacuated to 5 Pa, and then the temperature was raised to 300 ° C, and then Li 7 La 2.5 Zr 2 Bi 0.5 O 12 The time is 1S, the pulse time is 10s, nitrogen purge is 60 seconds, nitrogen purge is 5 seconds, nitrogen purge is 50 seconds, the carrier gas flow rate is 200sccm, and it is deposited on the surface of lithium oxide / amorphous carbon-coated graphite precursor material for 60 minutes to obtain a solid electrolyte doped amorphous carbon-coated graphite composite material.
[0033] Example 2
[0034] A method for preparing a solid electrolyte doped amorphous carbon-coated graphite composite material comprises the following steps:
[0035] Step S1:
[0036] 1 g of metallic lithium and 0.5 g of ethyl propyl sulfide were added to 500 g of dodecane inert solvent, and heated at 120° C. for 3 h to obtain a lithium metal solution;
[0037] Step S2:
[0038] Under an argon inert atmosphere, 100 g of porous graphite was added to 500 g of lithium metal solution and dispersed evenly, and vacuum-soaked at 50 ° C for 36 hours, filtered, and the obtained material was added to 100 g of 1 wt% melamine formaldehyde resin aqueous solution, and 100 g of 0.5 wt% graphene conductive agent solution was added, dispersed evenly, filtered, and the obtained filter residue was vacuum-dried at 80 ° C for 24 hours, and then carbonized at 700 ° C for 2 hours to obtain a lithium oxide / amorphous carbon-coated graphite precursor material;
[0039] Step S3:
[0040] Using atomic vapor deposition, the ALD chamber was opened, and the lithium oxide / amorphous carbon-coated graphite precursor material was transferred into the vacuum chamber and evacuated to 1 Pa. The temperature was raised to 100 °C, and then Li 7 La2.5 Zr 2 Y 0.5 O 12 The time is 1S, the pulse time is 1s, nitrogen purge is 60 seconds, nitrogen purge is 5 seconds, nitrogen purge is 50 seconds, the carrier gas flow rate is 50sccm, and it is deposited on the surface of lithium oxide / amorphous carbon-coated graphite precursor material for 10 minutes to obtain a solid electrolyte doped amorphous carbon-coated graphite composite material.
[0041] Example 3
[0042] A method for preparing a solid electrolyte doped amorphous carbon-coated graphite composite material comprises the following steps
[0043] Step S1:
[0044] 10 g of metallic lithium and 2 g of diethylene glycol dimethyl ether were added to 1000 g of dimethyl silicone oil inert solvent, and heated at 200° C. for 0.5 h to obtain a lithium metal solution;
[0045] Step S2:
[0046] Under an argon inert atmosphere, 100 g of porous graphite was added to 1000 g of lithium metal solution and dispersed evenly, and vacuum-soaked at a temperature of 100 ° C for 12 hours, filtered, and the obtained material was added to 100 g of a 10 wt% polyurethane resin aqueous solution, and 100 g of a 5 wt% carbon black solution was added, dispersed evenly, filtered, and the obtained filter residue was vacuum-dried at 80 ° C for 24 hours, and then carbonized at a temperature of 1000 ° C for 0.5 hours to obtain a lithium oxide / amorphous carbon-coated graphite precursor material;
[0047] Step S3:
[0048] Using the atomic vapor deposition method, the ALD chamber was opened, and the lithium oxide / amorphous carbon-coated graphite precursor material was transferred to the vacuum chamber and evacuated to 10 Pa. The temperature was raised to 500 ° C, and then the solid electrolyte was introduced for 1S. The pulse time was 1 15s, nitrogen purge for 60 seconds, nitrogen purge for 5 seconds, nitrogen purge for 50 seconds, and the carrier gas flow rate was 500sccm. It was deposited on the surface of the lithium oxide / amorphous carbon-coated graphite precursor material for 120 minutes to obtain a solid electrolyte doped amorphous carbon-coated graphite composite material.
[0049] Comparative Example 1:
[0050] The difference from Example 1 is that no lithium metal solution is added in step S1 and step S2, and the rest is the same as Example 1.
[0051] Comparative Example 2:
[0052] Unlike Example 1, Li is not deposited by ALD technology. 7 La2.5 Zr 2 Y 0.5 O 12 The preparation process is to use the lithium oxide / amorphous carbon-coated graphite precursor material in step S2 of Example 1 as the negative electrode material.
[0053] Experimental example
[0054] (1) SEM test
[0055] The solid electrolyte doped amorphous carbon-coated graphite composite material prepared in Example 1 was subjected to SEM testing, and the results are as follows: Figure 1 As shown. Figure 1 It can be seen that the obtained composite material presents a granular structure with slight bonding, a particle size between 10-15 μm, and a uniform size distribution.
[0056] (2) Button battery test
[0057] The solid electrolyte-doped amorphous carbon-coated graphite composite material prepared in Examples 1-3 and the graphite composite negative electrode material of Comparative Examples 1-2 were assembled into button batteries according to the following method:
[0058] Add a binder, a conductive agent, and a solvent to the negative electrode material, stir and mix them evenly to form a negative electrode slurry, apply the negative electrode slurry on a copper foil, dry, roll, and cut to obtain a negative electrode sheet. The binder is polyvinylidene fluoride, the conductive agent is SP conductive agent, the solvent is NMP, and the weight ratio of the negative electrode material, SP conductive agent, polyvinylidene fluoride and NMP is 95:1:4:220. A metal lithium sheet is used as a counter electrode, a polyethylene (PE) film, a polypropylene (PP) film or a polyethylene propylene (PEP) composite film is used as a separator, and a Li PF 6 / EC+DEC(Li PF 6 The concentration of EC was 1.3 mol / L, the volume ratio of EC and DEC was 1:1) as the electrolyte, and the battery was assembled in an argon-filled glove box.
[0059] The button cells were installed on the Wuhan Blue Electric CT2001A battery tester, and charged and discharged at a rate of 0.1C. The charge and discharge voltage range was 0.005V to 2.0V, and the first discharge specific capacity and first discharge efficiency were measured. The 2C rate discharge specific capacity was tested, and the rate performance (2C / 0.1C), cycle performance (0.1C / 0.1C, 100 weeks) and initial charge DCR (50% SOC) were calculated.
[0060] According to the national standard GB / T-24533-2019 "Graphite Anode Materials for Lithium-ion Batteries", the tap density, specific surface area, powder conductivity and powder OI value of the above-mentioned anode materials are tested. The test results are shown in Table 1:
[0061] Table 1
[0062]
[0063]
[0064] It can be seen from Table 1 that the discharge specific capacity of the graphite composite negative electrode materials prepared in Examples 1-3 is significantly higher than that of the comparative example; the reason may be that the lithium salt doped in the graphite material of the example reduces the irreversible capacity of the material and improves the initial efficiency, while the solid electrolyte coated on the outer layer improves the ionic conductivity of the material and improves the rate performance and cycle performance.
[0065] (3) Soft pack battery test
[0066] The graphite negative electrode materials prepared in Examples 1-3 and Comparative Examples 1-2 were used as negative electrodes, and the ternary material (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 ) was used as the positive electrode material to prepare the positive electrode, and LiPF 6 (solvent is EC+DEC, volume ratio is 1:1, concentration is 1.3 mol / L) as electrolyte and cel egard2400 as separator to prepare 2Ah soft-pack battery.
[0067] When preparing the negative electrode, a binder, a conductive agent, and a solvent are added to the negative electrode material, stirred and mixed to form a negative electrode slurry, and the negative electrode slurry is coated on a copper foil, dried, rolled, and cut to form a negative electrode sheet. The binder is LA132 binder, the conductive agent is SP conductive agent, the solvent is double distilled water, and the weight ratio of the negative electrode material, SP conductive agent, LA132 binder and double distilled water is 95:1:4:220.
[0068] When preparing the positive electrode, a binder, a conductive agent, and a solvent are added to the positive electrode material, and the mixture is stirred and mixed to form a positive electrode slurry. The positive electrode slurry is coated on an aluminum foil, dried, rolled, and cut to form a positive electrode sheet. The binder is PVDF, the conductive agent is SP, and the solvent is N-methylpyrrolidone. The weight ratio of the positive electrode material, the conductive agent, the binder, and the solvent is 93:3:4:140.
[0069] 1) Rate performance test
[0070] The charge and discharge voltage range is 2.8~4.2V, the test temperature is 25±3.0℃, and the charging is performed at 1.0C, 2.0C, 3.0C, and 5.0C, and the discharge is performed at 1.0C. The constant current ratio and temperature of the battery under different charging modes are tested. The results are shown in Table 2:
[0071] Table 2
[0072]
[0073] As can be seen from Table 2, the rate charging performance of the pack battery of the present invention is significantly better than that of the comparative example, and the charging time is shorter, indicating that the composite negative electrode material of the present invention has good fast charging performance. The reason may be that the lithium compound doped in the material provides sufficient lithium ions during the charging and discharging process, and the solid electrolyte coated on the outer layer increases the lithium ions and increases the diffusion rate of lithium ions, thereby improving the rate performance.
[0074] 2) Cycle performance test
[0075] The soft-pack batteries made of the graphite composite materials in Examples 1-3 and Comparative Examples 1-2 were subjected to the following experiment: 100, 300, and 500 charge and discharge cycles were performed at a 2C / 2C charge and discharge rate and a voltage range of 2.8-4.2V, respectively, to test the capacity retention rate. The results are shown in Table 3:
[0076] Table 3
[0077]
[0078] It can be seen from Table 3 that the cycle performance of the lithium ion battery prepared from the graphite composite material prepared in the present invention is significantly better than that of the comparative example in all stages. The reason may be that the lithium salt compound doped in the graphite has the characteristic of high lithium ions, which provides sufficient lithium ions during the charge and discharge process to improve the cycle performance.
[0079] Although the preferred embodiments of the present invention have been described above in conjunction with the accompanying drawings, they are not intended to limit the scope of protection of the present invention. For those skilled in the art, the present invention may have various modifications and variations, and any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A solid electrolyte doped amorphous carbon-coated graphite composite material, characterized in that: Its composite negative electrode material presents a core-shell structure, with the core being graphite, and the shells being the first shell and the second shell from the inside to the outside, the first shell being lithium-doped amorphous, and the second shell being composed of a solid electrolyte; calculated based on the mass ratio of the composite material being 100%, the mass of the first shell accounts for 1-10wt%, and the mass of the second shell accounts for 1-10wt%.
2. The solid electrolyte doped amorphous carbon-coated graphite composite material according to claim 1, characterized in that: The shell is composed of 1-5wt% of lithium oxide, 1-5wt% of conductive agent and 80-98wt% of amorphous carbon.
3. The method for preparing a solid electrolyte doped amorphous carbon-coated graphite composite material according to claim 1, characterized in that: The steps include: Step S1: According to the mass ratio of metal lithium: passivator: inert solvent = 1-10: 0.5-2: 500-1000, metal lithium and passivator are added to the inert solvent, and heated at a temperature of 120-200° C. for reaction for 0.5-3 hours to obtain a lithium metal solution; The passivating agent is one of tetraethylene glycol dimethyl ether, ethyl propyl sulfide, diethylene glycol dimethyl ether, and propenyl phenyl ether; The inert solvent is one of undecane, dodecane and dimethyl silicone oil; Step S2: According to the mass ratio of porous graphite: lithium metal solution: resin solution: conductive agent solution = 100:500-1000:100:100, in an inert atmosphere, the porous graphite is added to the lithium metal solution and dispersed evenly, and vacuum soaked at a temperature of 50-100° C. for 12-36 hours, filtered, and the obtained material is added to a 1-10wt% resin solution, and 0.5-5wt% conductive agent solution is added, dispersed evenly, filtered, and the obtained filter residue is vacuum dried at 80° C. for 24 hours, and then carbonized at a temperature of 700-1000° C. for 0.5-2 hours to obtain a lithium oxide / amorphous carbon-coated graphite precursor material; Step S3: By atomic vapor deposition, the ALD chamber is opened, and the lithium oxide / amorphous carbon-coated graphite precursor material is transferred to the vacuum chamber and evacuated to 1-10pa, and the temperature is raised to 100-500°C. Then, the solid electrolyte is introduced for 1S, the pulse time is 115s, nitrogen purge is 60 seconds, nitrogen purge is 5 seconds, nitrogen purge is 50 seconds, and the carrier gas flow rate is 50-500sccm. It is deposited on the surface of the lithium oxide / amorphous carbon-coated graphite precursor material for 10-120min to obtain a solid electrolyte doped amorphous carbon-coated graphite composite material.
4. The method for preparing a solid electrolyte doped amorphous carbon-coated graphite composite material according to claim 3, characterized in that: The preparation method of porous graphite in step S2 is to mix and bond graphite with a binder solution, dry it, then add it to a potassium permanganate aqueous solution with a molar concentration of 1-12 mg / mL, react it at a temperature of 60-100° C. for 1-6 hours, wash and dry it to obtain porous graphite.
5. The method for preparing a solid electrolyte doped amorphous carbon-coated graphite composite material according to claim 3, characterized in that: In step S2, the conductive agent solution is a carbon nanotube conductive liquid, a graphene conductive liquid, or a carbon black conductive liquid, with a mass concentration of 0.5-5wt%, and the solvent is deionized water.
6. The method for preparing a solid electrolyte doped amorphous carbon-coated graphite composite material according to claim 3, characterized in that: In step S2, the resin solution is one of urea-formaldehyde resin, melamine formaldehyde resin and polyurethane resin, and the solvent is deionized water.
7. The method for preparing a solid electrolyte doped amorphous carbon-coated graphite composite material according to claim 3, characterized in that: The solid electrolyte in step S3 is Li7La 3b Zr2MbO 12 , where M=Bi or Y and 0<b<1.
Citation Information
Cited By
Negative active material and preparation method thereof, negative plate and lithium ion battery
CN121726374A
A negative electrode active material, a preparation method thereof, a negative electrode sheet, and a lithium ion battery
CN121726374B