Foldable covering article with reduced dangerous splinters
By combining polymer layer and hard coating on the glass substrate, optimizing material performance, the problem of insufficient fatigue resistance and mechanical reliability when bending is solved, reducing the number of lobes and improving impact resistance is achieved. Sexual effect.
Patent Information
- Application Number
- CN201980102733.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-12-03
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2039-12-03
AI Technical Summary
The existing foldable glass substrates are insufficient in fatigue resistance and mechanical reliability when bending, and are prone to generate a large number of lobes during impact or bending, resulting in damage, and it is difficult to take into account sufficient hardness and flexibility.
Using glass or glass-ceramic substrates with a total thickness of 300μm and below, combined with an optimized polymer layer and hard coating, control Young's modulus and central tension of the material, reduce the number of lobes, and through chemical tempering and ion exchange Deeply optimize the fracture behavior of glass substrates.
A foldable cover product without a large number of lobes is achieved when the bending radius is small, maintaining flexibility while improving mechanical properties, reducing the risk during breaking, and enhancing impact resistance and fatigue resistance.
Smart Images

Figure CN114746269B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a foldable covering product, which is used for a substrate or cover sheet of a display, a fragile sensor, a fingerprint sensor module or a thin film battery, a semiconductor package or an application in a foldable display. Background Art
[0002] Recently, with the development of technology, glass is gradually used as a cover product for consumer devices such as televisions and mobile phones due to its transparent nature, light weight, enhanced toughness, etc. Optical transparency and thermal stability are often important properties for flexible display applications. In addition, flexible displays, especially flexible displays with touch screen functions and / or foldable, should have high fatigue resistance and high puncture resistance, including damage resistance at small bending radii.
[0003] Conventional flexible glass materials offer many desirable properties for flexible substrate and / or display applications. However, efforts to use glass materials for these applications have been largely unsuccessful to date. Generally, glass substrates can be manufactured at very low thickness levels (<25 μm) to achieve smaller and smaller bending radii, but these "thin" glass substrates have limited puncture resistance. At the same time, thicker (>150 μm) and more puncture-resistant glass substrates can be manufactured, but these substrates lack appropriate fatigue resistance and mechanical reliability when bent.
[0004] In addition, due to aesthetic reasons, it is required that the cover article can be folded into a dome shape or an arc shape. Although the foldable glass substrate for foldable electronic device applications is superior to polymer foil in terms of transparency, stability and wear resistance, it may be limited in impact resistance. More specifically, the impact resistance problem of the foldable glass substrate may manifest as damage to the substrate and / or underlying electronic components when impacted or bent.
[0005] Foldable cover products made of glass in the prior art are generally chemically toughened. However, when chemically toughened foldable glass breaks, the stored tensile energy is mainly dissipated through cracks and splinters, which may cause damage or injury to the user. The reason is that the new surface energy generated by the cracks is very limited and splinters seem inevitable, so it is necessary to reduce the splinters during the fracture. It has been found that an effective method for dissipating the released tensile energy during the fracture process is to introduce another material, namely a polymer. Then, the tensile energy can be dissipated by delamination of polymer films, plastic deformation of polymer films located around the force concentration area, viscoelastic deformation of polymer films located between small glass fragments, etc. However, the hardness of typical polymers is very low. Therefore, it is necessary to provide a foldable cover product with sufficient hardness to prevent scratches. Subsequently, it was proposed to introduce a hard material coating to increase the hardness of the foldable cover product. However, when a small bending radius is reached, flexibility may become a problem for the hard material coating. In summary, the thickness of the polymer layer and the hard coating is very important for flexibility and mechanical properties. When a small bending radius is reached, a small thickness may not provide sufficient protection or bonding to dissipate the tensile energy released; a large thickness may cause large strains and lead to failure of the hard coating. Therefore, it is necessary to provide a foldable cover article with sufficient hardness and flexibility, which can also reduce the generation of splinters when breaking due to bending or impact. Summary of the invention
[0006] An object of the present invention is to provide a foldable cover article mainly made of a glass substrate, which reduces the generation of fragments when broken due to bending or impact.
[0007] Another object of the present invention is to provide an optimized polymer layer / hard coating applied to the glass substrate to control the brittleness of the foldable cover article while maintaining or even improving the desired mechanical properties (such as flexibility) of the ultra-thin flexible display cover.
[0008] The above objectives are achieved through the following technical solutions.
[0009] In one aspect, the present invention provides a foldable cover article having a total thickness of t≤300 μm, preferably t≤250 μm, more preferably t≤200 μm, in particular t≤150 μm, particularly preferably t≤100 μm, particularly more preferably t≤85 μm, most preferably t≤70 μm, 50 μm, 40 μm, 30 μm, 20 μm, 10 μm, or within a range with any two of these values as endpoints. For example, the thickness t of the foldable cover article may be 300 μm to 10 μm, 300 μm to 20 μm, or 300 μm to 30 μm, or 300 μm to 40 μm, or 300 μm to 50 μm, or 300 μm to 70 μm, or 300 μm to 85 μm, or 300 μm to 100 μm, or 300 μm to 150 μm, or 300 μm to 2 The foldable cover article can be bent to a minimum bending radius r≤20mm, preferably r≤15mm, more preferably r≤10mm, in particular r≤8mm, particularly preferably r≤6mm, particularly more preferably r≤5mm, most preferably r≤4mm, 3mm, 2mm or 1.5mm without breaking, and its pencil hardness HR≥HB. The foldable cover article comprises a glass or glass-ceramic substrate with a thickness of 5 μm ≤ t1 ≤ 150 μm; and a polymer layer and / or a hard material coating with a total thickness of 5 μm ≤ t2 ≤ 150 μm. For each 20 mm width of the foldable cover article, when the foldable cover article is broken due to bending in a direction perpendicular to the width, the number of slivers with a longest linear stretch of L ≥ 5 mm is less than 10, preferably less than 8, more preferably less than 6, especially less than 5, particularly more preferably less than 4 and most preferably less than 3; and / or the number of slivers with a longest linear stretch of L < 5 mm is less than 50, preferably less than 40, more preferably less than 30, especially less than 25, particularly more preferably less than 20 and most preferably less than 15.
[0010] The inventors of the present invention have found that, compared with glass, due to the lower Young's modulus of the polymer layer, the polymer layer will shift the neutral plane during bending and cause a larger strain in the outermost layer. In order to maintain flexibility and greatly reduce the dangerous cracks of the chemically tempered ultra-thin glass from the foldable cover product, the typical thickness of the foldable cover product is t≤300μm, preferably t≤250μm, more preferably t≤200μm, especially t≤150μm, particularly preferably t≤100μm, particularly more preferably t≤85μm, most preferably t≤70μm, 50μm, 40μm, 30μm, 20μm, or in a range with any two of these values as endpoints. For example, the thickness t of the foldable cover article may be 300 μm to 10 μm, 300 μm to 20 μm, or 300 μm to 30 μm, or 300 μm to 40 μm, or 300 μm to 50 μm, or 300 μm to 70 μm, or 300 μm to 85 μm, or 300 μm to 100 μm, or 300 μm to 150 μm, or 300 μm to 2 The thickness t1 of the glass or glass-ceramic substrate should be 5 μm≤t1≤150 μm, and the total thickness of the polymer layer and / or the hard material coating should be 5 μm≤t2≤150 μm.
[0011] Without the polymer layer, a 10 mm x 20 mm area of the ultra-thin glass or glass-ceramic substrate located around the fracture source may break into more than dozens of individual fragments during bending; however, the use of the polymer layer / hard coating proposed in the present invention can reduce the brittleness of the glass and greatly reduce the number of individual fragments after fracture to only a few fragments.
[0012] In a further preferred embodiment of the present invention, the glass or glass-ceramic substrate is tempered and its minimum bending radius in millimeters is r1≤100000×t1 / CS, preferably r1≤80000×t1 / CS, more preferably r1≤70000×t1 / CS, and most preferably r1≤60000×t1 / CS, where CS is the compressive stress in MPa measured on both surfaces of the glass or glass-ceramic substrate.
[0013] In a further preferred embodiment of the present invention, the central tension of the glass or glass-ceramic substrate is CT≤700MPa, preferably CT≤500MPa, more preferably CT≤300MPa, particularly preferably CT≤100MPa, and most preferably CT≤50MPa, wherein CT is the central tension in MPa on the middle surface of the glass or glass-ceramic substrate.
[0014] Surprisingly, it was found that if the glass substrate is chemically toughened, the fracture behavior of the foldable cover substrate is affected by the ion exchange depth DoL and the central tension CT generated during the ion exchange process. In a further preferred embodiment of the present invention, the glass or glass-ceramic substrate is chemically toughened and the depth of its ion exchange layer is DoL ≥ 1 μm, preferably DoL ≥ 2 μm, more preferably DoL ≥ 3 μm, and / or DoL ≤ t1 / 2, preferably DoL ≤ 30 μm, more preferably DoL ≤ 20 μm.
[0015] In a further preferred embodiment of the present invention, the two-point bending strength of the glass or glass-ceramic substrate is BS≥700 MPa, preferably BS≥800 MPa, more preferably BS≥1000 MPa, most preferably BS≥1200 MPa.
[0016] In a further preferred embodiment of the present invention, for every 20 mm width of the foldable covering article, when the foldable covering article is broken due to bending in a direction perpendicular to the width, the number of cracks with the longest linear tension L≥5 mm is less than 10, preferably less than 8, more preferably less than 6, in particular less than 5, particularly more preferably less than 4 and most preferably less than 3, wherein the glass or glass-ceramic substrate or the side with a thinner polymer layer and / or a hard material coating is located on the convex surface.
[0017] In a further preferred embodiment of the present invention, for every 20 mm width of the foldable cover article, when the foldable cover article is broken due to bending in a direction perpendicular to the width, the number of cracks with the longest linear tension L<5 mm is less than 50, preferably less than 45, more preferably less than 40, in particular less than 35, particularly more preferably less than 30 and most preferably less than 20, wherein the glass or glass-ceramic substrate or the side with a thinner polymer layer and / or a hard material coating is located on the convex surface.
[0018] In a further preferred embodiment of the present invention, the folded covered product is placed on the concave surface of a polypropylene semi-ring with a radius of 4 cm, wherein the glass or glass-ceramic substrate or the side with a thinner polymer layer and / or a hard material coating is located on the convex surface, and then hit from a height of 25 cm with a ballpoint pen with a ball diameter of 0.7 mm and a weight of 6 g, and the entire product remains intact after the test.
[0019] In a further preferred embodiment of the present invention, for a 20 mm × 70 mm sample of the foldable covering product, the foldable covering product is placed on a stainless steel cylinder with a radius of 2.8 cm, wherein the glass or glass-ceramic substrate or one side having a thinner polymer layer and / or a hard material coating is located on a concave surface, and then hit from a height of 10 cm with a ballpoint pen having a ball diameter of 0.7 mm and a weight of 6 g, the weight loss caused by small fragments is less than 10%, preferably less than 9%, more preferably less than 8%, in particular less than 7%, particularly preferably less than 6%, and most preferably less than 5%.
[0020] In a further preferred embodiment of the present invention, the foldable covering product is placed flat on a marble platform, with the glass or glass-ceramic substrate or the side with a thinner polymer layer and / or hard material coating facing downward, and then hit with a 32.5g stainless steel ball from a height of 40cm, and the entire product remains intact.
[0021] In a further preferred embodiment of the present invention, the glass or glass-ceramic substrate is laminated with one or more polymer layers, and the total thickness t3p of the one or more polymer layers is 150μm, 120μm, 100μm, 85μm, 70μm, 50μm, 40μm, 30μm, 20μm, 10μm, 5μm, 1μm, or within a range with any two of these values as endpoints. For example, the total thickness t3p of the one or more polymer layers may be in the range of 150 μm to 5 μm, or 150 μm to 10 μm, or 150 μm to 20 μm, or 150 μm to 30 μm, or 150 μm to 40 μm, or 150 μm to 50 μm, or 150 μm to 70 μm, or 150 μm to 85 μm, or 150 μm to 100 μm, or 150 μm to 120 μm, or 150 μm to 1 μm, or 120 μm to 1 μm, or 100 μm to 1 μm, or 85 μm to 1 μm, or 70 μm to 1 μm, or 50 μm to 1 μm, or 40 μm to 1 μm, or 30 μm to 1 μm, or 20 μm to 1 μm, or 10 μm to 1 μm, or 5 μm to 1 μm.
[0022] In a further preferred embodiment of the present invention, the Young's modulus Ep of the one or more polymer layers is 10 GPa, 7 GPa, 6 GPa, 5 GPa, 4 GPa, 3 GPa, 2 GPa, 0.5 GPa, 0.4 GPa, 0.3 GPa, 0.2 GPa, 0.1 GPa, or in a range with any two of these values as endpoints. For example, the Young's modulus Ep of the one or more polymer layers may be 10 GPa to 0.2 GPa, or 10 GPa to 0.3 GPa, or 10 GPa to 0.4 GPa, or 10 GPa to 0.5 GPa, or 10 GPa to 2 GPa, or 10 GPa to 3 GPa, or 10 GPa to 4 GPa, or 10 GPa to 5 GPa, or 10 GPa to 6 GPa, or 10 GPa to 7 GPa, or 1 In the range of 0GPa to 0.1GPa, or 7GPa to 0.1GPa, or 6GPa to 0.1GPa, or 5GPa to 0.1GPa, or 4GPa to 0.1GPa, or 3GPa to 0.1GPa, or 2GPa to 0.1GPa, or 0.5GPa to 0.1GPa, or 0.4GPa to 0.1GPa, or 0.3GPa to 0.1GPa, or 0.2GPa to 0.1GPa.
[0023] In a further preferred embodiment of the present invention, the one or more polymer layers are made of a polymer selected from but not limited to: polyparaxylene, thermoplastic polyurethane (TPU), polycarbonate (PC), polysulfone (PS), polyethersulfone (PES), polyetheretherketone (PEEK), polyamide (PA), polyamideimide (PAI), polyimide (PI), poly(methyl methacrylate) (PMMA), polymethylsiloxane (PDMS) or a combination thereof.
[0024] In a further preferred embodiment of the present invention, at least one surface of the glass or glass-ceramic substrate is coated with one or more hard material coatings, and the total thickness t3c of the one or more hard material coatings is 150 μm, 120 μm, 100 μm, 85 μm, 70 μm, 50 μm, 40 μm, 30 μm, 20 μm, 10 μm, 5 μm, 1 μm, or within a range with any two of these values as endpoints. For example, the total thickness t3c of the one or more hard material coatings can be 150 μm to 5 μm, or 150 μm to 10 μm, or 150 μm to 20 μm, or 150 μm to 30 μm, or 150 μm to 40 μm, or 150 μm to 50 μm, or 150 μm to 70 μm, or 150 μm to 85 μm, or 150 μm to 100 μm. m, or 150μm to 120μm, or 150μm to 1μm, or 120μm to 1μm, or 100μm to 1μm, or 85μm to 1μm, or 70μm to 1μm, or 50μm to 1μm, or 40μm to 1μm, or 30μm to 1μm, or 20μm to 1μm, or 10μm to 1μm, or 5μm to 1μm.
[0025] In a further preferred embodiment of the present invention, the Young's modulus Eh of the one or more hard material coatings is 15 GPa, 13 GPa, 11 GPa, 9 GPa, 7 GPa, 4 GPa, 2 GPa, 1 GPa, or in a range with any two of these values as endpoints. For example, the Young's modulus Eh of the one or more hard material coatings may be in the range of 15 GPa to 2 GPa, or 15 GPa to 4 GPa, or 15 GPa to 7 GPa, or 15 GPa to 9 GPa, or 15 GPa to 11 GPa, or 15 GPa to 13 GPa, or 15 GPa to 1 GPa, or 13 GPa to 1 GPa, or 11 GPa to 1 GPa, or 9 GPa to 1 GPa, or 7 GPa to 1 GPa, or 4 GPa to 1 GPa, or 2 GPa to 1 GPa.
[0026] In a further preferred embodiment of the present invention, the one or more hard material coatings are made of, but not limited to, the following organic polymer materials: for example, acrylates and their modified forms, or inorganic-organic hybrid polymer materials, such as polysiloxanes and their modified forms, PMMA containing inorganic nanoparticles, and epoxy-siloxane hybrids.
[0027] In a further preferred embodiment of the present invention, the pencil hardness of the foldable cover article on the side laminated with the polymer layer and / or the hard material coating is less than 8H.
[0028] In a further preferred embodiment of the present invention, the fracture height of the foldable covering article is Ha≥Hg×2, preferably Ha≥Hg×3, more preferably Ha≥Hg×4, further preferably Ha≥Hg×5, further preferably Ha≥Hg×6, further preferably Ha≥Hg×7, further preferably Ha≥Hg×8, particularly preferably Ha≥Hg×9, and most preferably Ha≥Hg×10, wherein Hg is the fracture height of the glass substrate, and the fracture height is determined in a pen drop test, and the foldable covering article is placed on a platform consisting of 25μm OCA, 50μm PET, 25μm OCA, 50μm PET and 30cm marble from top to bottom, wherein the glass or glass-ceramic substrate surface or the side with a thinner polymer layer and / or a hard material coating faces downward and is bonded to the OCA layer on the top of the platform, and the pen is a ballpoint pen with a ball diameter of 0.5mm and a weight of 13g.
[0029] In a further preferred embodiment of the present invention, the breaking force of the foldable covering product is Fab≥2Fgb, preferably Fab≥5Fgb, more preferably Fab≥10Fgb, further preferably Fab≥20Fgb, further preferably Fab≥40Fgb, further preferably Fab≥60Fgb, particularly preferably Fab≥80Fgb, and most preferably Fab≥100Fgb, wherein Fgb is the breaking force of the glass substrate, and the breaking force is determined in a downward pressure test of P180 sandpaper, the glass or glass-ceramic substrate surface or the side with a thinner polymer layer and / or hard material coating of the foldable covering product is placed on a steel plate, and a steel bar with a diameter of 3 mm applies a load to the other side of the foldable covering product on its flat front side until it breaks, wherein the P180 sandpaper is attached to the flat front side of the steel bar, and the grinding surface of the sandpaper is in contact with the top surface of the foldable covering product.
[0030] In a further preferred embodiment of the present invention, the fracture height of the foldable cover article is at least the fracture force of the glass substrate multiplied by 2, preferably multiplied by 5, more preferably multiplied by 10, further preferably multiplied by 20, particularly preferably multiplied by 50, particularly more preferably multiplied by 100, particularly further preferably multiplied by 150 and most preferably multiplied by 200, wherein the fracture height is determined in a sandpaper ball drop test, wherein the glass or glass ceramic surface or the surface with a thinner polymer layer and / or a hard material coating of the glass article is placed on a steel plate, and a load is applied to the other surface of the glass article by dropping a 4.5 g acrylic ball from above until it breaks, wherein P180 type sandpaper is placed on the top surface of the foldable cover article, and the abrasive surface of the sandpaper is in contact with the top surface of the foldable cover article.
[0031] On the other hand, the present invention provides the use of the foldable cover article according to any one of the preceding claims in applications such as a substrate or cover sheet of a display, a fragile sensor, a substrate or cover sheet of a fingerprint sensor module, a semiconductor package, a substrate or cover sheet of a thin film battery, and a foldable display. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figures 1a to 1m 1 is a cross-sectional view of a foldable cover article according to an embodiment of the present invention and a foldable cover article for comparison in the prior art.
[0033] Figure 2 Schematic diagram of testing a foldable covering product under the condition of 2PB outward folding.
[0034] Figures 3a to 3k The fracture is caused by the external bending of 2PB. Figures 1a to 1j Schematic diagrams of Examples 1 to 10 of foldable cover articles are shown.
[0035] Figures 4a to 4c The fracture is caused by the external bending of 2PB. Figures 1k to 1m Schematic diagrams of Comparative Examples 1 to 3 of foldable cover articles are shown.
[0036] Figure 5 Schematic diagram of testing a foldable covering product under 2PB inward folding conditions.
[0037] Figures 6a to 6k The fracture is caused by the inward fold of 2PB. Figures 1a to 1j Schematic diagrams of Examples 1 to 10 of foldable cover articles are shown.
[0038] Figures 7a to 7c The fracture is caused by the inward fold of 2PB. Figures 1k to 1m Schematic diagrams of Comparative Examples 1 to 3 of foldable cover articles are shown.
[0039] Figure 8 Schematic diagram of testing a foldable cover product under the condition of an external folding pen.
[0040] Figures 9a to 9k For the pen that has been folded outwards Figures 1a to 1j Schematic diagrams of Examples 1 to 10 of foldable cover articles are shown.
[0041] Figures 10a to 10c The pen is broken due to external folding. Figures 1k to 1m Schematic diagrams of Comparative Examples 1 to 3 of foldable cover articles are shown. DETAILED DESCRIPTION
[0042] The purpose, features and advantages of the present invention will be explained in more detail through the examples and embodiments described below with reference to the accompanying drawings. In the accompanying drawings, the same reference numerals are used to indicate similar or corresponding elements.
[0043] Figures 1a to 1j A cross-sectional view of a foldable cover article according to the present invention and a foldable cover article in the prior art for comparison purposes is shown. Examples according to the present invention and comparative examples are described below. In the following examples, the glass substrate is ultra-thin glass (UTG), which is commercially available under the brand name AS87 eco aluminosilicate glass with a Young's modulus of 73.3 GPa and a pencil hardness of 9H produced by SCHOTT AG of Germany. It should be noted that the glass substrate can be made of different glasses, such as silicate glass, soda-lime glass, borosilicate glass, etc.
[0044] The following examples according to the invention only show preferred examples. However, the foldable covering article may also comprise a different number of layers / coatings on one / both sides as described below.
[0045] Example 1
[0046] Figure 1a A foldable cover article 1 is shown, which includes a glass substrate 200 and a polyparaxylene layer 300 applied on the glass substrate 200 by a chemical vapor deposition (CVD) method. In this example, the thickness of the glass substrate 200 is t2g=0.07 mm, the thickness t3p of the polyparaxylene layer 300 is in the range of 8 to 10 μm and the Young's elastic modulus Ep is in the range of 2 to 3 GPa.
[0047] Example 2
[0048] Figure 1b A foldable cover article 1 is shown, which includes a glass substrate 201 and a hard material coating 301 applied to the glass substrate 201 by a slot die coating method. In this example, the thickness of the glass substrate 201 is t2g=0.07 mm, and the hard material coating 301 is made of a polymer selected from PMMA containing nanoparticles (e.g., SiO2 particles) or epoxy-siloxane hybrids with a Young's modulus Ep in the range of 4 to 6 GPa. The thickness t3c of the hard material coating 301 is in the range of 19 to 22 μm.
[0049] Example 3
[0050] Figure 1cA foldable cover product 1 is shown, which includes a glass substrate 202; and a polyimide (PI) layer 302 and a hard material coating 312 applied to the glass substrate 202 by a roll-to-roll micro-gravure coating method. In this example, the thickness of the glass substrate 202 is t2g=0.07mm, and the hard material coating 312 is made of a polymer selected from a hybrid material of PMMA or PMMA and siloxane, and the Young's modulus Ep2 is in the range of 4 to 6GPa. The Young's modulus Ep1 of the PI layer 302 is in the range of 5 to 8GPa, and the thickness t3p is 50μm. The thickness t3c of the hard material coating is 10μm.
[0051] Example 4-1
[0052] Figure 1d A foldable cover article 1 is shown, which includes a glass substrate 203 and a hard material coating 303 applied to the glass substrate 203 by a spin coating process. In this case, the edge of the glass substrate 203 is encapsulated by the hard material coating 303. In this example, the thickness of the glass substrate 203 is t2g=0.07mm, and the hard material coating 303 is made of a polymer of polymethyl methacrylate containing SiO2 nanoparticles. The hard material coating 303 is applied to the glass substrate 203 by spin coating, and the thickness t3c of the hard material coating 303 is 30μm and the Young's modulus Ec is 3.16GPa.
[0053] Example 4-2
[0054] Figure 1e A foldable cover article 1 is shown, which includes a glass substrate 204 and a hard material coating 304 applied to the glass substrate 204 by a spin coating process. In this case, the edge of the glass substrate 204 is not encapsulated by the hard material coating 304. In this example, the thickness of the glass substrate 204 is t2g=0.07mm, and the hard material coating 304 is made of a polymer of polymethyl methacrylate containing SiO2 nanoparticles. The hard material coating 304 is applied to the glass substrate 204 by spin coating, and the thickness t3c of the hard material coating 304 is 30μm and the Young's modulus Ec is 3.16GPa.
[0055] Example 5
[0056] In Example 5, the structure of the foldable cover article 1 is Figure 1b The structure of Example 2 shown is the same, except that the Young's modulus Ep of the hard coating is in the range of 2 to 3 GPa.
[0057] Example 6
[0058] Figure 1f A foldable cover article 1 is shown, which includes a glass substrate 205; and a hard material coating 305, a polyimide (PI) layer 315 and an optically clear adhesive (OCA) coating 325 applied on the glass substrate 205. In this case, the hard material coating 305 is made of a polymer of polymethyl methacrylate containing SiO2 nanoparticles, and the OCA coating 325 is produced by Tesa, which is commercially available. 69401. In this example, the thickness of the glass substrate 205 is t2g=0.07 mm, the thickness of the hard material coating 305 is 10 μm, and the thickness of the PI layer 315 is 50 μm and the Young's modulus Ep is in the range of 5 to 8 GPa. The Young's modulus Ec of the OCA coating 325 is less than 0.001 GPa and the thickness t3c is 25 μm.
[0059] Example 7
[0060] Figure 1g A foldable cover article 1 is shown, which includes a glass substrate 206; and a hard material coating 306, an optically clear adhesive (OCA) coating 316 and a PET layer 326 applied on the glass substrate 206. In this case, the hard material coating 306 is made of a polymer of polymethyl methacrylate containing SiO2 nanoparticles, and the OCA coating 316 is made of a commercially available Tesa produced 69401. In this example, the thickness of the glass substrate 206 is t2g=0.07 mm, and the thickness of the hard material coating 306 is 30 μm. The thickness of the OCA coating 316 is 25 μm and the Young's modulus Ep is greater than 0.001 GPa. The thickness t3c of the PET layer 326 is 25 μm.
[0061] Example 8
[0062] Figure 1h A foldable cover article 1 is shown, which includes a glass substrate 208 and a hard material coating 308 applied on one side of the glass substrate 208 by a spin coating process. A pressure sensitive adhesive (PSA) coating 318 and a polyethylene terephthalate (PET) layer 328 are on the other side of the glass substrate 208. In this case, the glass substrate 208 is made of SCHOTT AS87eco with a thickness of 70 μm, which is commercially available. The hard material coating 308 has a thickness of 25 μm. The PSA coating 318 has a thickness of 25 μm, and the PET layer 318 has a thickness of 25 μm.
[0063] Example 9
[0064] Figure 1i A foldable cover product 1 is shown, which includes a glass substrate 209 and a colorless polyimide (CPI) layer 319 bonded to the glass substrate 209 by an OCA coating 309. In this example, the glass substrate 209 is gradually thinned by acid etching, and the thinned portion of the glass substrate 209 is filled with the OCA coating 309. The thickness of the thinnest portion of the glass substrate 209 is t1=50 μm, and the thickness of the glass substrate 209 is 145 μm except for the thinned portion. The thickness of the OCA coating 309 is 25 μm except for the portion of the OCA coating 309 filled in the thinned portion of the glass substrate 209. And, the thickness of the CPI layer 319 is 50 μm. In this case, even if the glass substrate is generally thick, the glass substrate 209 has good foldability at the thinnest portion. Therefore, the foldable cover product 1 has good foldability.
[0065] Example 10
[0066] Figure 1j A foldable cover article 1 is shown, which includes a glass substrate 210 and a colorless polyimide (CPI) layer 310 bonded to the substrate 210. In this example, the glass substrate 209 is completely wrapped by the CPI layer 310 to form a capsule structure. The thickness of the glass substrate is t1=70 μm, and the thickness of the CPI layer 310 is 50 μm.
[0067] Comparative Example 1
[0068] Figure 1k A foldable cover article 1 ' is shown comprising a glass substrate 200' without any polymer layer or coating.
[0069] Comparative Example 2
[0070] Figure 1l A foldable cover article 1' is shown, which includes a glass substrate 201' and a polyparaxylene layer 301' applied on the glass substrate 201' by a physical vapor deposition (PVD) or chemical vapor deposition (CVD) process. In this example, the thickness of the glass substrate is t2'g=0.07 mm, the thickness tp of the polyparaxylene layer 301' is in the range of 3 to 5 μm and the Young's elastic modulus Ep is in the range of 2 to 3 GPa.
[0071] Comparative Example 3
[0072] Figure 1mA foldable cover article 1' is shown, which includes a glass substrate 202' and two hard material coatings 302' applied to the glass substrate 202' by a dip coating process. In this example, the glass substrate 202' has a thickness t2'g=0.07 mm, each of the hard material coatings 302' is made of a polymer selected from PMMA or a hybrid material of PMMA and siloxane, and the Young's modulus Ep2 of the hard material coatings 302' is in the range of 4 to 6 GPa and the thickness t2 is 5 μm.
[0073] It should be noted that in the above examples, for better comparison, the materials of the glass substrate, hard material coating, PET layer, PI layer, CPI layer, PSA layer and OCA are the same, unless otherwise specifically defined. Moreover, if the thickness of the glass substrate is not constant, the thickness t1 of the glass substrate generally refers to the thickness of its thinnest part.
[0074] Test 1: 2PB external fold
[0075] Figure 2 A schematic diagram of a test of a foldable cover article 1, 1' that breaks under a 2PB outward fold is shown. The test is conducted by clamping the foldable cover article 1, 1' using two fixtures, wherein the polymer layer / coating of the foldable cover article 1, 1' faces the fixtures. In the case where there are polymer layers and / or coatings on both sides of the glass substrate 1, 1', the side with a larger thickness of the polymer layer and / or coating faces the fixture when bent. In this test, the fixture is placed 60 cm above a cutting platform with a 1 cm x 1 cm grid, and the results are relative to Figure 1a to Figure 1m The samples of the foldable covering products 1 and 1' shown in the figure are 20 mm x 70 mm x 0.07 mm in size. Figures 3a to 3k and Figures 4a to 4c From Figures 3a to 3k It can be determined from Figures 4a to 4c that when the thickness of the polymer layer and / or coating is large, the number of cracks caused by the fracture of the 2PB after external bending is small. In detail, the specific number of cracks in Examples 1 to 10 and Comparative Examples 1 to 3 is listed in Table 1.
[0076] Table 1
[0077] serial number Number of lobes ≥5 mm Number of lobes < 5 mm Example 1 ~5 ~20 Example 2 ~5 ~28 Example 3 ~3 ~17 Example 4-1 3 ~23 Example 4-2 4 ~32 Example 5 ~3 0 Example 6 1 0 Example 7 1 0 Example 8 1 0 Example 9 1 0 Example 10 1 0 Comparative Example 1 ~30 >100 Comparative Example 2 ~15 ~60 Comparative Example 3 ~12 ~60
[0078] Test 2: 2PB inward fold
[0079] Figure 5A schematic diagram of testing a foldable cover article 1, 1' under the condition of 2PB inward folding is shown. The foldable cover article 1, 1' is clamped by two fixtures to perform the test, wherein the glass substrate of the foldable cover article 1, 1' faces the fixtures. In the case where both sides of the glass substrate 1, 1' have a polymer layer and / or coating, the side with a smaller thickness of the polymer layer and / or coating faces the fixture when bent. In this test, the fixture is placed 60 cm above a cutting platform with a 1 cm×1 cm grid, and the results are relative to Figures 1a to 1m The samples of the foldable covering products 1 and 1' shown in the figure are 20 mm x 70 mm x 0.07 mm in size. Figures 6a to 6k and Figures 7a to 7c From Figures 6a to 6k It can be determined from Tables 7a to 7c that when the thickness of the polymer layer and / or coating is large, the number of cracks caused by the fracture of the 2PB after external bending is small. In detail, the specific number of cracks in Examples 1 to 10 and Comparative Examples 1 to 3 is listed in Table 2.
[0080] Table 2
[0081] serial number Number of lobes ≥5 mm Number of lobes < 5 mm Example 1 ~6 ~31 Example 2 ~6 ~37 Example 3 1 ~33 Example 4-1 4 ~28 Example 4-2 5 ~41 Example 5 ~4 ~12 Example 6 1 ~7 Example 7 1 0 Example 8 1 12 Example 9 1 ~13 Example 10 1 0 Comparative Example 1 ~30 >100 Comparative Example 2 ~20 >100 Comparative Example 3 ~116 >100
[0082] Test 3: Outer Fold Pen
[0083] Figure 8 A schematic diagram of testing a foldable covering product 1, 1' under the condition of an externally folded pen is shown. The test is performed by dropping a pen weighing 6g and having a length of 0.7mm from a height of 10cm onto a sample of the foldable covering product 1, 1', with the polymer layer and / or coating facing the pen. The sample is fixed on a roller with a radius of 2.8cm, and both ends of the sample are fixed with two tapes with a length of 3mm. In the case where the polymer layer and / or coating are present on both sides of the glass substrate 1, 1', the side with a larger thickness of the polymer layer and / or coating faces the pen. In this test, since it is difficult to collect tiny fragments, both ends of the sample attached to the tape are collected and weighed after the test. The weight loss is defined as follows:
[0084] The test results are relative to Figures 1a to 1m The samples of the foldable covering articles 1 and 1' shown are respectively Figures 9a to 9k and Figures 10a to 10c From Figures 9a to 9k and Figures 10a to 10c It can be determined that when the thickness of the polymer layer and / or coating is large, the weight loss caused by the breakage after the outer folding pen is small. In detail, the specific weight loss in Examples 1 to 10 and Comparative Examples 1 to 3 is listed in Table 3.
[0085] Table 3
[0086] serial number Weight loss (%) Number of major cracks Example 1 0 ~11 Example 2 ~5 / Example 3 0 ~22 Example 4-1 0 15 Example 4-2 0 21 Example 5 ~3 / Example 6 ~0 ~15 Example 7 0 18 Example 8 0 26 Example 9 0 12 Example 10 0 25 Comparative Example 1 ~45 / Comparative Example 2 ~11 / Comparative Example 3 ~16 /
[0087] The preferred embodiments of the present invention are described above. However, many changes and modifications may be made to the above embodiments of the present invention without departing from the spirit and various principles of the present invention. These modifications and changes should be included within the scope of the present invention and protected by the appended claims.
Claims
1. A foldable covering article having a total thickness of t ≤ 300 μm, the foldable covering article being bendable to a minimum bending radius of r ≤ 20 mm without breaking, and having a pencil hardness of ≥ HB, the foldable covering article comprising: A glass or glass-ceramic substrate having a thickness of 5 μm ≤ t1 ≤ 150 μm; And A polymer layer and / or a hard material coating having a total thickness of 5 μm < t2 ≤ 150 μm; Wherein, for every 20 mm width of the foldable covering article, when the foldable covering article breaks due to bending along a direction perpendicular to the width, a) The number of裂片 with a longest linear stretch L ≥ 5 mm is less than 10; and / or b) The number of裂片 with a longest linear stretch L < 5 mm is less than 50, And wherein the Young's modulus of the polymer layer is Ep ≤ 7 GPa, Wherein at least one surface of the glass or glass-ceramic substrate is coated with one or more hard material coatings, the total thickness of the one or more hard material coatings being t3c ≥ 1 μm, and Wherein the one or more hard material coatings are made of PMMA containing inorganic nanoparticles, and wherein the Young's modulus of the hard material coating is 1 GPa ≤ Eh ≤ 15 GPa.
2. The foldable cover article according to claim 1, characterized in that The total thickness of the foldable covering article is t ≤ 250 μm, the foldable covering article being bendable to a minimum bending radius of r ≤ 15 mm without breaking, Wherein, for every 20 mm width of the foldable covering article, when the foldable covering article breaks due to bending along a direction perpendicular to the width, a) The number of裂片 with a longest linear stretch L ≥ 5 mm is less than 8; and / or b) The number of裂片 with a longest linear stretch L < 5 mm is less than 40.
3. The foldable cover article according to claim 1, characterized in that The total thickness of the foldable covering article is t ≤ 200 μm, the foldable covering article being bendable to a minimum bending radius of r ≤ 10 mm without breaking, Wherein, for every 20 mm width of the foldable covering article, when the foldable covering article breaks due to bending along a direction perpendicular to the width, a) The number of裂片 with a longest linear stretch L ≥ 5 mm is less than 6; and / or b) The number of裂片 with a longest linear stretch L < 5 mm is less than 30.
4. The foldable cover article according to claim 1, characterized in that The total thickness of the foldable covering article is t ≤ 150 μm, the foldable covering article being bendable to a minimum bending radius of r ≤ 8 mm without breaking, Wherein, for every 20 mm width of the foldable covering article, when the foldable covering article breaks due to bending along a direction perpendicular to the width, a) The number of裂片 with a longest linear stretch L ≥ 5 mm is less than 5; and / or b) The number of裂片 with a longest linear stretch L < 5 mm is less than 25.
5. The foldable cover article according to claim 1, characterized in that The total thickness of the foldable covering article is t ≤ 100 μm, the foldable covering article being bendable to a minimum bending radius of r ≤ 6 mm without breaking, Wherein, for every 20 mm width of the foldable covering article, when the foldable covering article breaks due to bending along a direction perpendicular to the width, a) the number of slits with the longest linear extension L ≥ 5 mm is less than 4; and / or b) The number of lobes with the longest linear tension L<5 mm is less than 20.
6. The foldable cover article according to claim 1, characterized in that The total thickness of the foldable covering article is t≤85 μm, and the foldable covering article can be bent to a minimum bending radius of r≤5 mm without breaking, Wherein, for each 20 mm width of the foldable cover article, when the foldable cover article breaks due to bending in a direction perpendicular to the width, a) the number of slivers with the longest linear extension L ≥ 5 mm is less than 3; and / or b) The number of lobes with the longest linear tension L<5 mm is less than 15.
7. The foldable cover article according to claim 1, characterized in that The total thickness of the foldable cover article is t≤70 μm, and the foldable cover article can be bent to a minimum bending radius of r≤4 mm without breaking.
8. The foldable cover article according to claim 1, characterized in that The total thickness of the foldable cover article is t≤50 μm, and the foldable cover article can be bent to a minimum bending radius of r≤3 mm without breaking.
9. The foldable cover article according to claim 1, characterized in that The total thickness of the foldable cover article is t≤40 μm, and the foldable cover article can be bent to a minimum bending radius of r≤2 mm without breaking.
10. The foldable cover article according to claim 1, characterized in that The total thickness of the foldable cover article is t≤30 μm, and the foldable cover article can be bent to a minimum bending radius of r≤1.5 mm without breaking.
11. The foldable cover article according to claim 1, characterized in that The total thickness of the foldable cover article is t≤20 μm.
12. The foldable cover article according to claim 1, characterized in that The total thickness of the foldable cover article is t≤10 μm.
13. A foldable covering article according to any one of claims 1 to 12, characterised in that The glass or glass-ceramic substrate is tempered and has a minimum bending radius r1 in millimeters of r1≤100000×t1 / CS, where CS is the compressive stress in MPa measured on both surfaces of the glass or glass-ceramic substrate.
14. The foldable cover article according to claim 13, characterized in that The glass or glass-ceramic substrate is tempered and has a minimum bending radius r1 in millimeters of r1≤80000×t1 / CS.
15. The foldable cover article according to claim 13, characterized in that The glass or glass-ceramic substrate is tempered and has a minimum bending radius r1 in millimeters of r1≤70000×t1 / CS.
16. The foldable cover article according to claim 13, characterized in that The glass or glass-ceramic substrate is tempered and has a minimum bending radius r1 in millimeters of r1≤60000×t1 / CS.
17. The foldable cover article according to claim 13, characterized in that CT≤700 MPa, wherein CT is the central tension in MPa at the mid-plane of the glass or glass-ceramic substrate.
18. The foldable cover article according to claim 17, characterized in that CT≤500MPa.
19. The foldable cover article according to claim 17, characterized in that CT≤300MPa.
20. The foldable cover article of claim 17, wherein: CT≤100MPa.
21. The foldable cover article of claim 17, wherein: CT≤50MPa.
22. The foldable cover article of claim 13, wherein: The depth of the ion exchange layer of the glass or glass-ceramic substrate is DoL≥1 μm, and / or DoL≤t1 / 2.
23. The foldable cover article according to claim 22, characterized in that The depth of the ion exchange layer of the glass or glass-ceramic substrate is DoL≥2 μm and / or DoL≤30 μm.
24. The foldable cover article of claim 22, wherein: The depth of the ion exchange layer of the glass or glass-ceramic substrate is DoL≥3 μm and / or DoL≤20 μm.
25. The foldable cover article of claim 13, wherein: The two-point bending strength BS of the glass or glass-ceramic substrate is ≥700 MPa.
26. The foldable cover article according to claim 25, characterized in that The two-point bending strength BS of the glass or glass-ceramic substrate is ≥800 MPa.
27. The foldable cover article of claim 25, wherein: The two-point bending strength BS of the glass or glass-ceramic substrate is ≥1000 MPa.
28. The foldable cover article of claim 25, wherein: The two-point bending strength BS of the glass or glass-ceramic substrate is ≥1200 MPa.
29. A foldable covering article according to any one of claims 1 to 12, characterised in that For every 20 mm width of the foldable cover article, when the foldable cover article is broken due to bending in a direction perpendicular to the width, the number of cracks with the longest linear tension L≥5 mm is less than 10, wherein the glass or glass-ceramic substrate or the side with a thinner polymer layer and / or a hard material coating is located on the convex surface.
30. The foldable cover article of claim 29, wherein: The number of lobes with the longest linear stretch L≥5 mm is less than 8.
31. The foldable cover article of claim 29, wherein: The number of lobes with the longest linear stretch L≥5 mm is less than 6.
32. The foldable cover article of claim 29, wherein: The number of lobes with the longest linear stretch L≥5 mm is less than 5.
33. The foldable cover article of claim 29, wherein: The number of lobes with the longest linear stretch L≥5 mm is less than 4.
34. The foldable cover article of claim 29, wherein: The number of lobes with the longest linear stretch L≥5 mm is less than 3.
35. A foldable cover article according to any one of claims 1 to 12, characterised in that For every 20 mm width of the foldable cover article, when the foldable cover article is broken due to bending in a direction perpendicular to the width, the number of cracks with the longest linear tension L<5 mm is less than 50, wherein the glass or glass-ceramic substrate or the side with a thinner polymer layer and / or a hard material coating is located on the convex surface.
36. The foldable cover article of claim 35, wherein: The number of lobes with the longest linear tension L<5 mm is less than 45.
37. The foldable cover article of claim 35, wherein: The number of lobes with the longest linear tension L<5 mm is less than 40.
38. The foldable cover article of claim 35, wherein: The number of lobes with the longest linear tension L<5 mm is less than 35.
39. The foldable cover article of claim 35, wherein: The number of lobes with the longest linear stretch L<5 mm is less than 30.
40. The foldable cover article of claim 35, wherein: The number of lobes with the longest linear stretch L<5 mm is less than 20.
41. A foldable covering article according to any one of claims 1 to 12, characterised in that The folded covered product is placed on the concave surface of a polypropylene half ring with a radius of 4 cm, wherein the glass or glass-ceramic substrate or the side with a thinner polymer layer and / or a hard material coating is located on the convex surface, and then hit from a height of 25 cm with a ballpoint pen with a ball diameter of 0.07 mm and a weight of 6 g. The entire product remains intact after the test.
42. A foldable covering article according to any one of claims 1 to 12, characterised in that For a 20 mm×70 mm sample of the foldable cover product, the foldable cover product is placed on a stainless steel cylinder with a radius of 2.8 cm, wherein the glass or glass-ceramic substrate or the side having a thinner polymer layer and / or a hard material coating is located on the concave surface, and then hit from a height of 10 cm with a ballpoint pen having a ball diameter of 0.7 mm and a weight of 6 g, and the weight loss caused by small cracks is less than 10%.
43. The foldable cover article according to claim 42, characterized in that The amount of weight loss due to small fragments was less than 9%.
44. The foldable cover article of claim 42, wherein: The amount of weight loss due to small fragments was less than 8%.
45. The foldable cover article of claim 42, wherein: The amount of weight loss due to small fragments was less than 7%.
46. The foldable cover article of claim 42, wherein: The amount of weight loss due to small fragments was less than 6%.
47. The foldable cover article of claim 42, wherein: The amount of weight loss due to small fragments was less than 5%.
48. A foldable cover article according to any one of claims 1 to 12, characterised in that The foldable covered product is placed flat on a marble platform, with the glass or glass-ceramic substrate or the side with a thinner polymer layer and / or hard material coating facing downward, and then hit with a 32.5 g stainless steel ball from a height of 40 cm, and the entire product remains intact.
49. A foldable cover article according to any one of claims 1 to 12, characterised in that The glass or glass-ceramic substrate is laminated with one or more polymer layers, the total thickness of the one or more polymer layers being t3p≥1 μm and / or t3p≤150 μm.
50. The foldable cover article of claim 49, wherein: The glass or glass-ceramic substrate is laminated with one or more polymer layers, the total thickness of the one or more polymer layers being t3p≥5 μm.
51. The foldable cover article of claim 49, wherein: The glass or glass-ceramic substrate is laminated with one or more polymer layers, the total thickness of the one or more polymer layers being t3p≥10 μm.
52. The foldable cover article of claim 49, wherein: The glass or glass-ceramic substrate is laminated with one or more polymer layers, the total thickness of the one or more polymer layers being t3p≥20 μm.
53. The foldable cover article of claim 49, wherein: The glass or glass-ceramic substrate is laminated with one or more polymer layers, the total thickness of the one or more polymer layers being t3p≥40 μm.
54. The foldable cover article of claim 49, wherein: The Young's modulus of the one or more polymer layers is Ep≤6 GPa, and / or Ep≥0.1 GPa.
55. The foldable cover article of claim 54, wherein: The Young's modulus of the one or more polymer layers is Ep≤5 GPa, and / or Ep≥0.2 GPa.
56. The foldable cover article of claim 54, wherein: The Young's modulus of the one or more polymer layers is Ep≤4 GPa, and / or Ep≥0.3 GPa.
57. The foldable cover article of claim 54, wherein: The Young's modulus of the one or more polymer layers is Ep≤3 GPa, and / or Ep≥0.4 GPa.
58. The foldable cover article of claim 54, wherein: The Young's modulus of the one or more polymer layers is Ep≤2 GPa, and / or Ep≥0.5 GPa.
59. The foldable cover article of claim 49, wherein: The one or more polymer layers are made of a polymer selected from the group consisting of parylene, TPU, PC, PS, PES, PEEK, PA, PAI, PI, PMMA, PDMS, or combinations thereof.
60. A foldable cover article according to any one of claims 1 to 12, characterised in that At least one surface of the glass or glass-ceramic substrate is coated with one or more hard material coatings, and the total thickness of the one or more hard material coatings is t3c≥5μm and / or t3c≤150μm.
61. The foldable cover article of claim 60, wherein: At least one surface of the glass or glass-ceramic substrate is coated with one or more hard material coatings, and the total thickness of the one or more hard material coatings is t3c≥10 μm.
62. The foldable cover article of claim 60, wherein: At least one surface of the glass or glass-ceramic substrate is coated with one or more hard material coatings, and the total thickness of the one or more hard material coatings is t3c≥15 μm.
63. The foldable cover article of claim 60, wherein: At least one surface of the glass or glass-ceramic substrate is coated with one or more hard material coatings, and the total thickness of the one or more hard material coatings is t3c≥20 μm.
64. The foldable cover article of claim 60, wherein: The Young's modulus of the one or more hard material coatings is Eh≥2 GPa, and / or Eh≤13 GPa.
65. The foldable cover article of claim 64, wherein: The Young's modulus of the one or more hard material coatings is Eh≥4 GPa, and / or Eh≤11 GPa.
66. The foldable cover article of claim 64, wherein: The Young's modulus of the one or more hard material coatings is Eh≤9 GPa.
67. A foldable covering article according to any one of claims 1 to 12, characterised in that The pencil hardness of the foldable cover article on the side laminated with the polymer layer and / or the hard material coating is less than 8H.
68. A foldable cover article according to any one of claims 1 to 12, characterised in that The fracture height Ha of the foldable covering product is ≥Hg×2, where Hg is the fracture height of the glass substrate, and the fracture height is determined in a pen drop test, wherein the foldable product is placed on a platform consisting of 25μm OCA, 50μm PET, 25μm OCA, 50μm PET and 30cm marble from top to bottom, wherein the glass or glass-ceramic substrate surface or the side with a thinner polymer layer and / or a hard material coating faces downward and is bonded to the OCA layer on the top of the platform, and the pen is a ballpoint pen with a ball diameter of 0.5mm and a weight of 13g.
69. The foldable cover article of claim 68, wherein: The foldable covering product has a breaking height Ha≥Hg×3.
70. The foldable cover article of claim 68, wherein: The foldable covering product has a breaking height Ha≥Hg×4.
71. The foldable cover article of claim 68, wherein: The foldable covering product has a breaking height Ha≥Hg×5.
72. The foldable cover article of claim 68, wherein: The foldable covering product has a breaking height Ha≥Hg×6.
73. The foldable cover article of claim 68, wherein: The foldable covering product has a breaking height Ha≥Hg×7.
74. The foldable cover article of claim 68, wherein: The foldable covering product has a breaking height Ha≥Hg×8.
75. The foldable cover article of claim 68, wherein: The foldable covering product has a breaking height Ha≥Hg×9.
76. The foldable cover article of claim 68, wherein: The foldable covering product has a breaking height Ha≥Hg×10.
77. A foldable cover article according to any one of claims 1 to 12, characterised in that The rupture force Fab of the foldable covering product is ≥ 2Fgb, wherein Fgb is the rupture force of the glass substrate, and the rupture force is determined in a downward pressure test of P180 sandpaper, wherein the glass or glass-ceramic substrate surface or the surface having a thinner polymer layer and / or a hard material coating of the foldable product is placed on a steel plate, and a load is applied to the other surface of the foldable covering product by a steel bar with a diameter of 3 mm on its flat front side until it breaks, wherein P180 sandpaper is attached to the flat front side of the steel bar, and the grinding surface of the sandpaper is in contact with the top surface of the foldable covering product.
78. The foldable cover article of claim 77, wherein: The foldable cover article has a breaking force Fab ≥ 5Fgb.
79. The foldable cover article of claim 77, wherein: The foldable cover article has a breaking force Fab ≥ 10Fgb.
80. The foldable cover article of claim 77, wherein: The foldable cover article has a breaking force Fab ≥ 20 Fgb.
81. The foldable cover article of claim 77, wherein: The foldable cover article has a breaking force Fab≥40Fgb.
82. The foldable cover article of claim 77, wherein: The foldable cover article has a breaking force Fab ≥ 60 Fgb.
83. The foldable cover article of claim 77, wherein: The foldable cover article has a breaking force Fab ≥ 80 Fgb.
84. The foldable cover article of claim 77, wherein: The foldable cover article has a breaking force Fab ≥ 100 Fgb.
85. A foldable cover article according to any one of claims 1 to 12, characterised in that The fracture height of the foldable cover article is at least the fracture force of the glass substrate multiplied by 2, wherein the fracture height is determined in a sandpaper ball drop test, wherein the glass surface or the surface having a thinner polymer layer and / or a hard material coating of the glass article is placed on a steel plate, and a load is applied to the other surface of the glass article by dropping a 4.5 g acrylic ball from above until it breaks, wherein P180 type sandpaper is placed on the top surface of the foldable cover article, and the abrasive surface of the sandpaper is in contact with the top surface of the foldable cover article.
86. The foldable cover article of claim 85, wherein: The foldable cover article has a fracture height of at least five times the fracture force of the glass substrate.
87. The foldable cover article of claim 85, wherein: The foldable cover article has a fracture height of at least 10 times the fracture force of the glass substrate.
88. The foldable cover article of claim 85, wherein: The foldable cover article has a fracture height of at least 20 times the fracture force of the glass substrate.
89. The foldable cover article of claim 85, wherein: The foldable cover article has a fracture height of at least 50 times the fracture force of the glass substrate.
90. The foldable cover article of claim 85, wherein: The foldable cover article has a fracture height of at least 100 times the fracture force of the glass substrate.
91. The foldable cover article of claim 85, wherein: The foldable cover article has a fracture height of at least 150 times the fracture force of the glass substrate.
92. The foldable cover article of claim 85, wherein: The foldable cover article has a fracture height of at least 200 times the fracture force of the glass substrate.
93. A foldable cover article according to any one of claims 1 to 12, characterised in that The glass or glass-ceramic substrate is completely encapsulated by the polymer layer and / or the hard material coating.
94. The foldable cover article according to claim 1, characterized in that The nanoparticles are SiO2 particles.
95. Use of the foldable cover article according to any one of claims 1 to 94 in applications such as substrates or cover sheets of displays, fragile sensors, substrates or cover sheets of fingerprint sensor modules, semiconductor packages, substrates or cover sheets of thin film batteries, and foldable displays.