A porous adsorption deodorizing masterbatch, preparation method and application thereof
By using porous adsorption powders of alkali metal aluminosilicates and diatomite with specific particle sizes in polypropylene materials, combined with photocatalysts, to form an ordered structure, the problem of the release of volatile organic compounds in polypropylene materials is solved, significantly Improved odor removal effect and air retention performance.
Patent Information
- Application Number
- CN202110711029.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-25
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-06-25
AI Technical Summary
Existing polypropylene materials have problems with the release of volatile organic compounds during use, resulting in incomplete elimination of odors and poor air retention properties.
Using a specific particle size combination of porous adsorption powder with alkali metal aluminosilicates compounded on the surface, diatomite and photocatalyst, by adjusting the particle size and pore size, a more orderly staggered arrangement structure is formed, the adsorption capacity is improved, and in the preparation Photocatalyst is added during the process to evenly distribute the alkali metal aluminosilicate and enhance the air-holding performance.
It effectively reduces the release of volatile organic compounds, significantly improves the odor removal effect and air-holding capacity, is suitable for the adsorption of a variety of gas molecules, and avoids small molecule adsorption defects.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of deodorization, and more specifically, to a porous adsorption-type deodorization masterbatch, a preparation method and an application thereof. Background Art
[0002] In recent years, polypropylene has been widely developed due to its good performance. However, in the process of large-scale use of polypropylene materials, the odor problem has brought negative impacts on the human body and the environment. Therefore, in recent years, the research on deodorizing materials has intensified. CN101817953B provides a low-emission modified polypropylene composite material, which achieves the effect of low odor emission by using polypropylene, mineral fillers, odor adsorbents and additives, but its odor cannot be completely eliminated, especially after the modified polypropylene composite material is placed for a period of time, the release of volatile organic compounds increases, and the practical value is relatively low. CN107022146A provides a low-VOC glass fiber reinforced PP material, which achieves the effect of low VOC by using PP, glass fiber, grafting agent, antioxidant and extractant masterbatch, but also has the problem of poor gas retention performance. Summary of the invention
[0003] In view of some problems existing in the prior art, the first aspect of the present invention provides a porous adsorption deodorizing masterbatch, which includes a porous adsorption powder with an alkali metal aluminosilicate composited on the surface, and the weight ratio of the alkali metal aluminosilicate to the porous adsorption powder is (5-7):4.
[0004] In the present application, the porous adsorption powder with alkali metal aluminosilicate compounded on the surface refers to a masterbatch with alkali metal aluminosilicate adsorbed on the surface of the porous adsorption powder.
[0005] In one embodiment, the weight ratio of the alkali metal aluminosilicate to the porous adsorption powder is 6:4.
[0006] In one embodiment, the alkali metal aluminosilicate has a particle size of less than 70 μm.
[0007] Preferably, the particle size of the alkali metal aluminosilicate is 1-10 μm, more preferably 2-6 μm.
[0008] Preferably, the pore size of the alkali metal aluminosilicate is 3-9 angstroms, more preferably 4 angstroms.
[0009] Preferably, the bulk density of the alkali metal aluminosilicate is greater than or equal to 0.5 g / mL.
[0010] Preferably, the alkali metal aluminosilicate is an alkali metal aluminosilicate with a sodium-type crystal structure.
[0011] The alkali metal aluminosilicate described in the present application was purchased from Zhengzhou Chaorong Nanomaterial Co., Ltd., model number AT-3.
[0012] Generally, the use of alkali metal aluminosilicates with a pore size greater than 10 angstroms can achieve more types of volatile organic compounds. However, the applicant found in the experiment that when the porous adsorption deodorizing masterbatch includes diatomaceous earth with alkali metal aluminosilicates compounded on the surface, if the pore size of the alkali metal aluminosilicate is greater than 10 angstroms, the obtained polypropylene will have a strong odor after a period of time. After a series of research and development, the applicant unexpectedly found in the experiment that when the particle size of the alkali metal aluminosilicate is less than 70μm, especially 2-6μm, and the pore size is 3-9 angstroms, after compounding with diatomaceous earth and extruding and granulating with polypropylene, there is no re-release of volatile organic compounds after a period of time. The applicant believes that the possible reason is that the staggered silicon-oxygen tetrahedral units and aluminum-oxygen tetrahedral units are arranged in a more orderly manner when compounded with diatomaceous earth than the alkali metal aluminosilicates with a pore size greater than 10 angstroms, avoiding the phenomenon of excessively large quasi-crystalline nuclei growth of the alkali metal aluminosilicates leading to a weakening of the interaction with the diatomaceous earth during the later melt extrusion granulation process.
[0013] In one embodiment, the porous adsorption powder is diatomaceous earth.
[0014] Preferably, the particle size of the porous adsorption powder is 325-400 mesh.
[0015] The diatomaceous earth with a particle size of 325 mesh in this application was purchased from Gongyi Haoxin Water Purification Materials Co., Ltd., and the diatomaceous earth with a particle size of 400 mesh was purchased from Lingshou County Yuanbo Mineral Products Processing Plant.
[0016] The applicant unexpectedly discovered that when the particle size of the porous adsorption powder is 325-400 mesh, after being compounded with the specific alkali metal aluminosilicate of the present application, it can be suitable for the adsorption of molecules of various diameters emitted from polypropylene, and effectively reduce volatile organic compounds. The applicant believes that the possible reason is that after the porous adsorption powder of a specific particle size in the present application is treated with the specific concentration of sulfuric acid in the present application, micropores of different sizes are formed in the porous adsorption powder. After being compounded with the alkali metal aluminosilicate and the photocatalyst again, the composite morphology is relatively uniform, resulting in the deodorizing masterbatch at this time. When acting on volatile organic compounds, volatile organic compounds of different molecular sizes are orderly and graded for adsorption, thereby avoiding the adsorption of relatively small molecular volatile organic compounds on the porous adsorption powder, which leads to the adsorption defect of larger molecular volatile organic compounds.
[0017] In one embodiment, the porous adsorption deodorizing masterbatch comprises a porous adsorption powder with alkali metal aluminosilicate and a photocatalyst compounded on the surface.
[0018] Preferably, the weight ratio of the porous adsorption powder to the photocatalyst is (2-4):1, more preferably 2.6:1.
[0019] The weight ratio of the alkali metal aluminosilicate to the porous adsorption powder and the weight ratio of the porous adsorption powder to the photocatalyst described in the present application are the weight ratios of the raw materials added during the preparation process.
[0020] In one embodiment, the photocatalyst is titanium dioxide.
[0021] Preferably, the particle size of the photocatalyst is 5-30 nm, more preferably 15 nm.
[0022] The second aspect of the present application provides a method for preparing the porous adsorption deodorizing masterbatch, comprising: soaking the porous adsorption powder in an acidic solution at 80-100°C for 2-4 hours, adding water to dilute the reaction, then adding a photocatalyst liquid, continuing to soak for 0.5-1.5 hours, then drying at 160-180°C, adding alkali metal aluminosilicate and ethanol, stirring, standing, discarding the supernatant, and drying to obtain the masterbatch.
[0023] The applicant found that when the alkali metal aluminosilicate and the porous adsorption powder are directly compounded, the adsorption form of the alkali metal aluminosilicate on the surface of the porous adsorption powder in the deodorizing masterbatch obtained is extremely uneven, and is only locally distributed, which affects the use effect of the deodorizing masterbatch. The applicant unexpectedly found that when a specific amount of photocatalyst is additionally compounded, and the particle size of the photocatalyst is 5-30nm, especially 15nm, this not only overcomes the uneven adsorption form of the alkali metal aluminosilicate on the surface of the porous adsorption powder caused by the compounding method, but also improves the gas retention capacity of the porous adsorption powder to a certain extent, and also improves the effect of removing VOC. The applicant believes that the possible reason is that after being treated with a photocatalyst liquid of a specific particle size, the photocatalyst particles of this particle size are compounded on the surface of the porous adsorption powder of a specific particle size. In the process of adding and stirring the alkali metal aluminosilicate molecules, the alkali metal aluminosilicate molecules slide on the surface of the porous adsorption powder and are relatively evenly distributed on its surface after standing.
[0024] In one embodiment, the preparation method of the porous adsorption deodorizing masterbatch comprises: soaking the porous adsorption powder in a 75wt% sulfuric acid solution at 90°C for 3 hours, adding water to dilute the reaction for 1 hour, discarding the supernatant, and then adding a photocatalyst liquid, continuing to soak for 1 hour, then drying at 170°C for 3 hours, adding to an alkali metal aluminosilicate, placing in ethanol and stirring for 1-3 hours, standing for 24 hours, discarding the supernatant, and drying to obtain.
[0025] Preferably, the water is added in a standard amount at a liquid-to-solid weight ratio of 15:1.
[0026] The photocatalyst liquid described in this application was purchased from Hangzhou Jiupeng New Materials Co., Ltd., model number CY-TA33.
[0027] In the present application, the contents of 75 wt % sulfuric acid solution and ethanol are not particularly limited, and those skilled in the art may make conventional selections.
[0028] The third aspect of the present application provides an application of the porous adsorption deodorizing masterbatch in polypropylene or modified polypropylene.
[0029] The fourth aspect of the present application provides a method for using the porous adsorption deodorizing masterbatch, comprising: adding polypropylene, talcum powder, porous adsorption deodorizing masterbatch, and thermal stabilizer into a mixer and mixing for 1-10 minutes, then placing in a twin-screw machine for melt extrusion and granulation to obtain.
[0030] The polypropylene, talc and heat stabilizer described in the present application are not particularly limited, and those skilled in the art can make routine selections.
[0031] The process of melt extrusion in the present application is not particularly limited, and those skilled in the art can make conventional selections, for example: the process is: zone 1 200-210°C, zone 2 210-220°C, zone 3 210-220°C, zone 4 205-215°C; the residence time is 1-5 minutes, and the pressure is 12-18Mpa.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] The present application forms a porous adsorption deodorizing masterbatch by double-adsorbing alkali metal aluminosilicate on the surface of porous adsorption powder through a specific process, thereby improving the adsorption capacity and gas retention of the deodorizing masterbatch, being suitable for a variety of gas molecular diameters, and having a significant odor removal effect. The use of specific alkali metal aluminosilicates avoids the accumulation and growth of alkali metal aluminosilicates on the surface of porous adsorption powders; in the preparation process, the distribution of alkali metal aluminosilicates on the surface of porous adsorption powders is changed by adding a specific amount of photocatalyst liquid, which not only overcomes the uneven adsorption form of alkali metal aluminosilicates on the surface of porous adsorption powders caused by the compounding of alkali metal aluminosilicates and porous adsorption powders, but also improves the gas retention capacity of porous adsorption powders to a certain extent, and also improves the effect of removing VOCs. DETAILED DESCRIPTION
[0034] The present invention is described below by specific implementation methods, but is not limited to the specific embodiments given below.
[0035] Example
[0036] Example 1
[0037] Example 1 of the present invention provides a porous adsorption-type deodorizing masterbatch, which is diatomaceous earth with alkali metal aluminosilicate and photocatalyst having a sodium-type crystal structure on the surface.
[0038] The weight ratio of the alkali metal aluminosilicate with a sodium-type crystal structure to diatomaceous earth is 5:4; the weight ratio of the diatomaceous earth to the photocatalyst is 2:1.
[0039] The alkali metal aluminosilicate with a sodium-type crystal structure has a particle size of 2-6 μm, a pore size of 4 angstroms, and a bulk density greater than or equal to 0.5 g / mL. It is purchased from Zhengzhou Chaorong Nanomaterial Co., Ltd. and has a model number of AT-3.
[0040] The particle size of the diatomaceous earth is 325 mesh, which is purchased from Gongyi Haoxin Water Purification Materials Co., Ltd.
[0041] The photocatalyst is titanium dioxide with a particle size of 5 nm.
[0042] The preparation method of the porous adsorption deodorizing masterbatch is as follows: soaking the porous adsorption powder in a 75wt% sulfuric acid solution at 90°C for 3h, adding water to dilute and react for 1h, discarding the supernatant, then adding the photocatalyst liquid, continuing to soak for 1h, then drying at 170°C for 3h, adding the alkali metal aluminosilicate, placing in ethanol and stirring for 2h, standing for 24h, discarding the supernatant, and drying to obtain the masterbatch.
[0043] The photocatalyst liquid was purchased from Hangzhou Jiupeng New Materials Co., Ltd.
[0044] The method for using the porous adsorption deodorizing masterbatch is as follows: polypropylene, talcum powder, porous adsorption deodorizing masterbatch and thermal stabilizer are added into a mixer and mixed for 5 minutes, and then placed in a twin-screw machine for melt extrusion and granulation, and the process is: zone one 200-205°C, zone two 210-215°C, zone three 210-220°C, zone four 205-210°C; the residence time is 3 minutes, and the pressure is 16Mpa.
[0045] The polypropylene was purchased from Shanghai Fuchen Plastic Raw Materials Co., Ltd. with a brand name of MF65; the talcum powder was purchased from Yingkou Meilian Mining Co., Ltd.; and the thermal stabilizer was 3-aryl-benzofuranone.
[0046] Example 2
[0047] Embodiment 2 of the present invention provides a porous adsorption deodorizing masterbatch, which is diatomaceous earth with alkali metal aluminosilicate and photocatalyst having a sodium-type crystal structure on the surface.
[0048] The weight ratio of the alkali metal aluminosilicate with a sodium-type crystal structure to diatomaceous earth is 7:4; the weight ratio of the diatomaceous earth to the photocatalyst is 4:1.
[0049] The alkali metal aluminosilicate with a sodium-type crystal structure has a particle size of 2-6 μm, a pore size of 4 angstroms, and a bulk density greater than or equal to 0.5 g / mL. It is purchased from Zhengzhou Chaorong Nanomaterial Co., Ltd. and has a model number of AT-3.
[0050] The diatomaceous earth has a particle size of 400 meshes and is purchased from Lingshou County Yuanbo Mineral Products Processing Plant.
[0051] The photocatalyst is titanium dioxide with a particle size of 30nm.
[0052] The preparation method of the porous adsorption deodorizing masterbatch is as follows: soaking the porous adsorption powder in a 75wt% sulfuric acid solution at 90°C for 3h, adding water to dilute and react for 1h, discarding the supernatant, then adding the photocatalyst liquid, continuing to soak for 1h, then drying at 170°C for 3h, adding the alkali metal aluminosilicate, placing in ethanol and stirring for 2h, standing for 24h, discarding the supernatant, and drying to obtain the masterbatch.
[0053] The photocatalyst liquid was purchased from Hangzhou Jiupeng New Materials Co., Ltd.
[0054] The method for using the porous adsorption deodorizing masterbatch is as follows: polypropylene, talcum powder, porous adsorption deodorizing masterbatch and thermal stabilizer are added into a mixer and mixed for 5 minutes, and then placed in a twin-screw machine for melt extrusion and granulation, and the process is: zone one 200-205°C, zone two 210-215°C, zone three 210-220°C, zone four 205-210°C; the residence time is 3 minutes, and the pressure is 16Mpa.
[0055] The polypropylene was purchased from Shanghai Fuchen Plastic Raw Materials Co., Ltd. with a brand name of MF65; the talcum powder was purchased from Yingkou Meilian Mining Co., Ltd.; and the thermal stabilizer was 3-aryl-benzofuranone.
[0056] Example 3
[0057] Example 3 of the present invention provides a porous adsorption-type deodorizing masterbatch, which is diatomaceous earth with alkali metal aluminosilicate and photocatalyst having a sodium-type crystal structure on the surface.
[0058] The weight ratio of the alkali metal aluminosilicate with a sodium-type crystal structure to diatomaceous earth is 6:4; the weight ratio of the diatomaceous earth to the photocatalyst is 2.6:1.
[0059] The alkali metal aluminosilicate with a sodium-type crystal structure has a particle size of 2-6 μm, a pore size of 4 angstroms, and a bulk density greater than or equal to 0.5 g / mL. It is purchased from Zhengzhou Chaorong Nanomaterial Co., Ltd. and has a model number of AT-3.
[0060] The particle size of the diatomaceous earth is 325 mesh, which is purchased from Gongyi Haoxin Water Purification Materials Co., Ltd.
[0061] The photocatalyst is titanium dioxide with a particle size of 15 nm.
[0062] The preparation method of the porous adsorption deodorizing masterbatch is as follows: soaking the porous adsorption powder in a 75wt% sulfuric acid solution at 90°C for 3h, adding water to dilute and react for 1h, discarding the supernatant, then adding the photocatalyst liquid, continuing to soak for 1h, then drying at 170°C for 3h, adding the alkali metal aluminosilicate, placing in ethanol and stirring for 2h, standing for 24h, discarding the supernatant, and drying to obtain the masterbatch.
[0063] The photocatalyst liquid was purchased from Hangzhou Jiupeng New Materials Co., Ltd., model number CY-TA33.
[0064] The method for using the porous adsorption deodorizing masterbatch is as follows: polypropylene, talcum powder, porous adsorption deodorizing masterbatch and thermal stabilizer are added into a mixer and mixed for 5 minutes, and then placed in a twin-screw machine for melt extrusion and granulation, and the process is: zone one 200-205°C, zone two 210-215°C, zone three 210-220°C, zone four 205-210°C; the residence time is 3 minutes, and the pressure is 16Mpa.
[0065] The polypropylene was purchased from Shanghai Fuchen Plastic Raw Materials Co., Ltd. with a brand name of MF65; the talcum powder was purchased from Yingkou Meilian Mining Co., Ltd.; and the thermal stabilizer was 3-aryl-benzofuranone.
[0066] Example 4
[0067] Example 4 of the present invention provides a porous adsorption-type deodorizing masterbatch, which is diatomaceous earth with alkali metal aluminosilicate having a sodium-type crystal structure on the surface.
[0068] The weight ratio of the alkali metal aluminosilicate with a sodium-type crystal structure to diatomaceous earth is 6:4.
[0069] The alkali metal aluminosilicate with a sodium-type crystal structure has a particle size of 2-6 μm, a pore size of 4 angstroms, and a bulk density greater than or equal to 0.5 g / mL. It is purchased from Zhengzhou Chaorong Nanomaterial Co., Ltd. and has a model number of AT-3.
[0070] The particle size of the diatomaceous earth is 325 mesh, which is purchased from Gongyi Haoxin Water Purification Materials Co., Ltd.
[0071] The preparation method of the porous adsorption deodorizing masterbatch is as follows: soaking the porous adsorption powder in a 75wt% sulfuric acid solution at 90°C for 3h, adding water to dilute and react for 1h, discarding the supernatant, drying at 170°C for 3h, adding to alkali metal aluminosilicate, adding ethanol, stirring for 2h, standing for 24h, discarding the supernatant, and drying to obtain the masterbatch.
[0072] The method for using the porous adsorption deodorizing masterbatch is as follows: polypropylene, talcum powder, porous adsorption deodorizing masterbatch and thermal stabilizer are added into a mixer and mixed for 5 minutes, and then placed in a twin-screw machine for melt extrusion and granulation, and the process is: zone one 200-205°C, zone two 210-215°C, zone three 210-220°C, zone four 205-210°C; the residence time is 3 minutes, and the pressure is 16Mpa.
[0073] The polypropylene was purchased from Shanghai Fuchen Plastic Raw Materials Co., Ltd. with a brand name of MF65; the talcum powder was purchased from Yingkou Meilian Mining Co., Ltd.; and the thermal stabilizer was 3-aryl-benzofuranone.
[0074] Example 5
[0075] Example 5 of the present invention provides a porous adsorption-type deodorizing masterbatch, which is diatomaceous earth with alkali metal aluminosilicate and photocatalyst having a sodium-type crystal structure on the surface.
[0076] The weight ratio of the alkali metal aluminosilicate with a sodium-type crystal structure to diatomaceous earth is 6:4; the weight ratio of the diatomaceous earth to the photocatalyst is 2.6:1.
[0077] The alkali metal aluminosilicate with a sodium-type crystal structure has a pore size of 10 angstroms and a bulk density of 0.66 g / mL. It was purchased from Qingdao Hengxintian New Material Technology Co., Ltd. and the model is 13X original powder.
[0078] The particle size of the diatomaceous earth is 325 mesh, which is purchased from Gongyi Haoxin Water Purification Materials Co., Ltd.
[0079] The photocatalyst is titanium dioxide with a particle size of 15 nm.
[0080] The preparation method of the porous adsorption deodorizing masterbatch is as follows: soaking the porous adsorption powder in a 75wt% sulfuric acid solution at 90°C for 3h, adding water to dilute and react for 1h, discarding the supernatant, then adding the photocatalyst liquid, continuing to soak for 1h, then drying at 170°C for 3h, adding the alkali metal aluminosilicate, placing in ethanol and stirring for 2h, standing for 24h, discarding the supernatant, and drying to obtain the masterbatch.
[0081] The photocatalyst liquid was purchased from Hangzhou Jiupeng New Materials Co., Ltd., model number CY-TA33.
[0082] The method for using the porous adsorption deodorizing masterbatch is as follows: polypropylene, talcum powder, porous adsorption deodorizing masterbatch and thermal stabilizer are added into a mixer and mixed for 5 minutes, and then placed in a twin-screw machine for melt extrusion and granulation, and the process is: zone one 200-205°C, zone two 210-215°C, zone three 210-220°C, zone four 205-210°C; the residence time is 3 minutes, and the pressure is 16Mpa.
[0083] The polypropylene was purchased from Shanghai Fuchen Plastic Raw Materials Co., Ltd. with a brand name of MF65; the talcum powder was purchased from Yingkou Meilian Mining Co., Ltd.; and the thermal stabilizer was 3-aryl-benzofuranone.
[0084] Performance Evaluation
[0085] Odor test: After the polypropylene obtained in Examples 1-5 was placed for one month, whether there was an odor was recorded, wherein level 0 means no obvious odor; level 1 means a slight odor; level 2 means an obvious odor. The higher the level, the more obvious the odor.
[0086] Morphology observation: The morphologies of the porous adsorption deodorizing masterbatches obtained in Examples 1-5 were observed using a scanning electron microscope, and the composite morphologies of diatomaceous earth and its surface substances were observed. The composite morphologies were divided into three categories according to their uniformity: the first category was relatively uniform in morphology, the second category was moderately uniform in morphology, and the third category was relatively non-uniform in morphology.
[0087] Table 1
[0088] Smell test Morphology observation Example 1 Level 0 First Class Example 2 Level 0 First Class Example 3 Level 0 First Class Example 4 Level 2 Third Class Example 5 Level 1 Second Class
Claims
1. A porous adsorption deodorizing masterbatch, characterized in that: It includes a porous adsorption powder with alkali metal aluminosilicate and photocatalyst compounded on the surface; The porous adsorption powder is diatomaceous earth with a particle size of 325 mesh, purchased from Gongyi Haoxin Water Purification Material Co., Ltd. The weight ratio of the alkali metal aluminosilicate to the porous adsorption powder is (5-7):4; The alkali metal aluminosilicate is an alkali metal aluminosilicate with a sodium crystal structure, the particle size of the alkali metal aluminosilicate with a sodium crystal structure is 2-6 µm, the pore size is 4 angstroms, and the bulk density is greater than or equal to 0.5 g / mL. It is purchased from Zhengzhou Chaorong Nanomaterial Co., Ltd. and the model is AT-3; The photocatalyst is titanium dioxide with a particle size of 5-30nm; The weight ratio of the porous adsorption powder to the photocatalyst is (2-4):1; The preparation method of the porous adsorption deodorizing masterbatch comprises: soaking the porous adsorption powder in a 75wt% sulfuric acid solution at 90°C for 3h, adding water to dilute and react for 1h, discarding the supernatant, then adding a photocatalyst liquid, continuing to soak for 1h, then drying at 170°C for 3h, adding an alkali metal aluminosilicate, placing in ethanol and stirring for 1-3h, standing for 24h, discarding the supernatant, and drying to obtain the masterbatch; The method for using the porous adsorption deodorizing masterbatch comprises: adding polypropylene, talcum powder, porous adsorption deodorizing masterbatch and thermal stabilizer into a mixer and mixing for 1-10 minutes, then placing in a twin-screw machine for melt extrusion and granulation to obtain the masterbatch; The extrusion process is: zone 1 200-210°C, zone 2 210-220°C, zone 3 210-220°C, zone 4 205-215°C; residence time is 1-5 minutes, and pressure is 12-18MPa.