Dielectric loss and capacitance monitoring method for superconducting cable during temperature recovery
Through the power frequency capacitance and dielectric loss testing methods, the capacitance and dielectric loss tan δ changes of the superconducting cable are monitored, which solves the problem of difficult monitoring of internal state changes during the reheating process, ensures a smooth temperature transition of the superconducting cable, and avoids mechanical stress. Damage and extension of time.
Patent Information
- Application Number
- CN202210314925.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-03-28
AI Technical Summary
During the temperature recovery process of superconducting cables, existing technology is difficult to effectively monitor the changes in the internal state of the cable, resulting in drastic changes in temperature that may cause thermal stress and mechanical stress damage to components, affecting the construction schedule and equipment safety.
Using the capacitance and dielectric loss test method at a power frequency of 50Hz, the capacitance value and dielectric loss tan δ change data of the superconducting cable are monitored in real time, and its internal state is analyzed to ensure a smooth transition of the temperature recovery process. Specific steps include withdrawing the superconducting cable from the power grid, stopping the refrigeration system, vaporizing liquid nitrogen, controlling the internal pressure, conducting multiple power frequency capacitance and dielectric loss tests during the temperature recovery process, and analyzing the internal moisture, phase state and temperature changes.
It achieves reliable status monitoring of the superconducting cable's temperature recovery process, prevents mechanical stress damage, detects abnormalities in time, determines the optimal temperature recovery speed, and ensures a smooth transition of cable temperature.
Smart Images

Figure CN114814376B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of superconducting cable detection, and in particular to a method for monitoring dielectric loss and capacitance in a superconducting cable temperature recovery process. Background Art
[0002] High-Temperature Superconducting (HTS) cable is a kind of power facility that uses unimpeded superconducting materials that can transmit high current density as conductors and can transmit large currents. It has the advantages of compact structure, low loss and large transmission capacity, and can achieve low-loss and large-capacity power transmission. At present, there is very little experience in related tests and operation of high-temperature superconducting cables at home and abroad, and the overall technology is at the stage of grid-connected demonstration and small-scale commercial application worldwide.
[0003] The superconducting cable system consists of four main parts: the cable body, cable accessories, refrigeration system, and detection and protection system. High-temperature superconducting cables generally use liquid nitrogen (77K, i.e. -196℃) as a cooling medium and an insulating medium. Inside the high-temperature superconducting cable, multiple layers of high-temperature superconducting tapes are spirally wound without gaps on a flexible cable skeleton to form a superconducting conductor layer, which is the conductive part of the transmission current; an insulating layer and a shielding layer are also wound outside the superconductor; in order to keep the liquid nitrogen in the cable at the critical temperature of the superconductor (77K), an insulating tube with excellent thermal insulation performance is required. Therefore, high-temperature superconducting cables are usually composed of a superconductor layer, an insulating layer, a shielding layer, and an insulating tube. The insulating layer is formed by winding 7mm polypropylene laminated paper (PPLP) outside the superconductor. PPLP is formed by pressing a porous pulp material with a polypropylene (PP) film, which has good impregnation properties and can effectively prevent the generation of air gaps and thus reduce the occurrence of partial discharge; while the PP film has high electrical strength and good mechanical properties at low temperatures.
[0004] The process of a superconducting cable returning from operating temperature to normal temperature is called system warming; for example, if a superconducting cable in operation needs to be repaired, the superconducting cable will be allowed to gradually return to normal temperature after a power outage. During the warming process of a superconducting cable, temperature changes cause the corresponding parts of the cable to expand, among which the cable core deforms the most, with an elongation of up to 0.3%, which can easily generate mechanical stress locally in the cable. Currently, when laying cables, it is necessary to preset a certain offset (expansion arc) according to the different positions of the conductor and insulation material. During the warming process, it is necessary to monitor the longitudinal and lateral offsets of the cable and manually adjust the offset (expansion arc) of the cable to avoid the generation of large mechanical stress, thereby preventing thermal stress and mechanical stress damage to components caused by drastic temperature changes.
[0005] As the length of the superconducting cable increases, its temperature recovery time will also increase accordingly. Too long a temperature recovery time will inevitably affect the maintenance period, while too fast a temperature recovery will cause stress to be released too late and damage the cable. Therefore, in addition to the above-mentioned non-electrical quantities (temperature, pressure, flow, liquid level, expansion and contraction displacement, etc.) monitoring, it is also necessary to monitor the electrical quantities of the superconducting cable during the temperature recovery process to truly reflect the changes in the internal state of the superconducting cable during the temperature recovery process, thereby ensuring that the superconducting cable can achieve a smooth temperature transition during the temperature recovery process and avoid cable damage. Summary of the invention
[0006] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and to provide a method for monitoring dielectric loss and capacitance during the reheating process of a superconducting cable. By carrying out capacitance and dielectric loss tests at an industrial frequency of 50 Hz, the internal state changes of the superconducting cable during the reheating process can be truly reflected to ensure that the superconducting cable can achieve a smooth temperature transition during the reheating process.
[0007] The purpose of the present invention can be achieved by the following technical solution: A method for monitoring dielectric loss and capacitance during the temperature recovery process of a superconducting cable, comprising the following steps:
[0008] S1. The superconducting cable is disconnected from the grid, the refrigeration system stops running, and the internal pressure is controlled in real time;
[0009] S2. The superconducting cable returns to normal temperature by heat exchange with the external environment. During this process, the capacitance and dielectric loss of the superconducting cable are tested at an industrial frequency of 50 Hz to obtain the variation data of the capacitance value and dielectric loss tanδ of the superconducting cable;
[0010] S3. According to the variation data of the capacitance value and dielectric loss tanδ of the superconducting cable, the internal state variation information of the superconducting cable during the temperature recovery process is analyzed and obtained.
[0011] Furthermore, the step S1 specifically includes the following steps:
[0012] S11, superconducting cable trips and exits grid operation;
[0013] S12, the refrigeration system stops running, the liquid nitrogen storage tank is closed, and the liquid nitrogen circulation is stopped;
[0014] S13. Liquid nitrogen gradually vaporizes, and the release valve of the cable refrigeration system is opened to discharge nitrogen into the atmosphere to control the internal pressure.
[0015] Furthermore, the step S2 specifically performs capacitance and dielectric loss tests on the superconducting cable at an operating frequency of 50 Hz for multiple times during the temperature recovery process according to a set monitoring time interval.
[0016] Furthermore, the set monitoring time interval is 4 hours.
[0017] Furthermore, the specific process of performing the capacitance and dielectric loss test at an operating frequency of 50 Hz in step S2 is as follows:
[0018] S21. Apply a test voltage to the superconducting cable, and measure and calculate the capacitance value and dielectric loss tanδ of the superconducting cable;
[0019] S22, executing step S21 multiple times according to the set monitoring time interval to obtain multiple capacitances and dielectric loss tanδ corresponding to different time points.
[0020] Furthermore, the capacitance value and dielectric loss value of the superconducting cable are specifically measured using a dielectric loss meter.
[0021] Furthermore, the effective value of the test voltage is 500V.
[0022] Furthermore, the step S3 specifically includes the following steps:
[0023] S31, performing curve fitting on a plurality of capacitance data corresponding to different time points to obtain a capacitance variation curve;
[0024] Perform curve fitting on multiple dielectric loss tanδ corresponding to different time points to obtain a dielectric loss variation curve;
[0025] S32. According to the capacitance change curve and the dielectric loss change curve, the internal state change result of the superconducting cable during the temperature recovery process is analyzed and obtained.
[0026] Furthermore, the step S32 specifically analyzes and obtains the change results of the moisture, phase and temperature inside the superconducting cable, and the phase includes gas and liquid.
[0027] Compared with the prior art, the present invention proposes a dielectric loss and capacitance monitoring method for the reheating process of the superconducting cable. By detecting and analyzing the capacitance and dielectric loss parameters of the superconducting cable, the internal state change of the superconducting cable during the reheating process can be reliably determined, which is conducive to ensuring that the superconducting cable achieves a smooth temperature transition during the reheating process and effectively preventing thermal stress and mechanical stress damage of components caused by drastic temperature changes.
[0028] The present invention analyzes the moisture, phase state and temperature inside the superconducting cable according to the capacitance change curve and the dielectric loss change curve, which can truly reflect the progress of the superconducting cable during the temperature recovery, can timely discover the abnormalities generated during the temperature recovery process, and can also facilitate the subsequent determination of the optimal temperature recovery speed. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic diagram of the method flow of the present invention. DETAILED DESCRIPTION
[0030] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0031] Example
[0032] like Figure 1 As shown, a method for monitoring dielectric loss and capacitance during the temperature recovery process of a superconducting cable comprises the following steps:
[0033] S1. The superconducting cable is out of the grid, the refrigeration system stops running, and the internal pressure is controlled in real time. Specifically:
[0034] First, the superconducting cable tripped and was taken out of grid operation;
[0035] After that, the refrigeration system stops running, the liquid nitrogen storage tank is closed, and the liquid nitrogen circulation is stopped;
[0036] The liquid nitrogen gradually vaporizes, and then the release valve of the cable refrigeration system is opened to discharge the nitrogen into the atmosphere to control the internal pressure;
[0037] S2, the superconducting cable is restored to normal temperature by heat exchange with the external environment. In this process, the capacitance and dielectric loss test of the superconducting cable at an industrial frequency of 50 Hz are performed to obtain the variation data of the capacitance value and dielectric loss tanδ of the superconducting cable. Specifically, according to the set monitoring time interval, the capacitance and dielectric loss test of the superconducting cable at an industrial frequency of 50 Hz are performed multiple times during the temperature recovery process. In this embodiment, the set monitoring time interval is 4 hours;
[0038] When testing, firstly, a test voltage is applied to the superconducting cable (in this embodiment, the effective value of the test voltage is 500V), and the capacitance and dielectric loss tanδ of the superconducting cable are measured and calculated;
[0039] According to the set monitoring time interval, the above test process is performed multiple times to obtain multiple capacitances and dielectric loss tanδ corresponding to different time points;
[0040] S3. According to the change data of superconducting cable capacitance and dielectric loss tanδ, the internal state change information of superconducting cable during the temperature recovery process is analyzed, specifically:
[0041] S31, performing curve fitting on a plurality of capacitance data corresponding to different time points to obtain a capacitance variation curve;
[0042] Perform curve fitting on multiple dielectric loss tanδ corresponding to different time points to obtain a dielectric loss variation curve;
[0043] S32. According to the capacitance change curve and the dielectric loss change curve, the internal state change results of the superconducting cable during the temperature recovery process are analyzed, including the change results of the moisture content, phase (gaseous and liquid) and temperature inside the superconducting cable.
[0044] The insulation structure of HTS cable at low temperature (operating conditions) is solid-liquid composite insulation of PPLP (polypropylene laminated paper) impregnated with liquid nitrogen; the insulation structure at room temperature is PPLP dry insulation; in the warming project, there is a period of time when it appears as solid-liquid-gas composite insulation.
[0045] The relative dielectric constant ε of liquid nitrogen r is 1.43, and the ε of air r is 1, and the ε of nitrogen r The calculation formula of the capacitance value of the superconducting cable insulation medium is as follows:
[0046] C=2*π*ε r *ε / ln(R 2 / R 1 )
[0047] Where ε is the dielectric constant of vacuum, R 2 is the radius of the cable shield, R 1 is the cable conductor radius; the above formula considers the cable insulation as a whole. If each layer of insulating medium is analyzed, the cable insulation is composed of many layers of PPLP and nitrogen in series; the partial pressure of the AC voltage on PPLP and nitrogen (liquid or gaseous) mainly depends on the capacitance of the two, and the capacitance and ε r Closely related, r It is also related to the liquid phase and the gas phase. Therefore, the partial pressure is uneven and changes, and the contribution of each layer of insulation to the total dielectric loss and total capacitance also changes.
[0048] In the process of superconducting cable returning from low temperature to room temperature, the ε of each layer of material in the solid-liquid composite insulation r In this process, capacitance and dielectric loss tests are carried out, and the detected superconducting cable capacitance and tanδ will also change, realizing the reflection of the internal state changes of the superconducting cable during the temperature recovery from the electrical parameters.
[0049] In addition, the tanδ of PPLP under power frequency will also change with temperature. When the temperature difference of superconducting cable from low temperature to room temperature is huge, the change of tanδ is quite considerable.
[0050] Generally speaking, the test voltage for capacitance and dielectric loss measurement is 10kV. The insulation structure of superconducting cables in operation is liquid nitrogen impregnated PPLP, while at room temperature it is only PPLP dry insulation, which is an incomplete insulation structure with low insulation strength. In order to avoid damage to the cable insulation, the test voltage is reduced to 500V.
[0051] In the later stage of temperature recovery, if the internal pressure of the cable is insufficient, external moisture will enter, causing the PPLP (polypropylene laminated paper) to be damp, and the power frequency dielectric loss tanδ will increase significantly. Therefore, by monitoring the power frequency dielectric loss tanδ, it can be determined whether moisture has entered the cable.
[0052] This embodiment applies the above technical solution and is implemented in the Shanghai kilometer-level superconducting cable demonstration project. The Shanghai kilometer-level superconducting cable demonstration project is an AC 35kV three-phase turnkey cable, and the cable shielding layer is grounded inside the cable and not drawn out. During the warming process, the power frequency dielectric loss capacitance and dielectric spectrum measurement are performed once every 4 hours. If it is found that the state quantity changes slowly, the sampling frequency can be adjusted to reduce. The test time of the power frequency dielectric loss capacitance is short, less than 5 minutes for a three-phase cable, and it is easy to implement. The effective value of the test voltage is 500V.
[0053] In practical applications, for example, before the implementation of a large-scale superconducting cable project, a short sample of a superconducting cable with the same structure can be made, and a reheating experiment can be carried out in the laboratory. At the same time, non-electrical quantities (temperature, pressure, flow, liquid level, cold shrinkage displacement) and electrical quantities (dissipation capacitance obtained by using this technical solution) in the reheating process can be collected to obtain the fingerprint data of the cable reheating and form a reheating database of multi-dimensional state quantities of the superconducting cable. In addition, the laboratory reheating speed can be changed to monitor the changes in various state quantities of the cable to obtain the optimal reheating speed.
[0054] When the temperature is restored at the project site, the measured electrical and non-electrical quantities of the superconducting cable system are interpolated and fitted with the data in the temperature restoration database using mathematical tools, so as to understand the current internal state of the cable and determine whether the temperature restoration process is smooth.
[0055] In addition, in actual applications, the monitoring data between three-phase single-core cables can be compared, and any abnormalities can be analyzed immediately.
Claims
1. A method for monitoring dielectric loss and capacitance during the temperature recovery process of a superconducting cable, characterized in that: The following steps are involved: S1. The superconducting cable is disconnected from the grid, the refrigeration system stops running, and the internal pressure is controlled in real time; S2. The superconducting cable returns to normal temperature by heat exchange with the external environment. During this process, the capacitance and dielectric loss of the superconducting cable are tested at an industrial frequency of 50 Hz to obtain the variation data of the capacitance value and dielectric loss tanδ of the superconducting cable; S3. Analyze and obtain the internal state change information of the superconducting cable during the temperature recovery process according to the change data of the superconducting cable capacitance value and dielectric loss tanδ; Among them, step S2 specifically performs capacitance and dielectric loss tests on the superconducting cable at a power frequency of 50 Hz for multiple times during the temperature recovery process according to the set monitoring time interval. The process of performing capacitance and dielectric loss tests at a power frequency of 50 Hz in step S2 is as follows: S21. Apply a test voltage to the superconducting cable, and measure and calculate the capacitance value and dielectric loss tanδ of the superconducting cable; S22, executing step S21 multiple times according to the set monitoring time interval to obtain multiple capacitances and dielectric loss tanδ corresponding to different time points; Step S3 includes the following steps: S31, performing curve fitting on a plurality of capacitance data corresponding to different time points to obtain a capacitance variation curve; Perform curve fitting on multiple dielectric loss tanδ corresponding to different time points to obtain a dielectric loss variation curve; S32, analyzing and obtaining the result of the internal state change of the superconducting cable during the temperature recovery process according to the capacitance change curve and the dielectric loss change curve, specifically analyzing and obtaining the result of the change of the internal moisture, phase state and temperature of the superconducting cable, wherein the phase state includes gaseous state and liquid state, thereby realizing the reflection of the internal state change of the superconducting cable during the temperature recovery process from the electrical parameters; Specifically, a reheating experiment is conducted in the laboratory in advance, and non-electrical quantities and electrical quantities in the reheating process are collected simultaneously. The non-electrical quantities include temperature, pressure, flow, liquid level, and cold shrinkage displacement, and the electrical quantity is dielectric loss capacitance, thereby obtaining the fingerprint data of the cable reheating, and forming a reheating database of multi-dimensional state quantities of superconducting cables; When the temperature is restored at the project site, the measured electrical and non-electrical quantities of the superconducting cable system are interpolated and fitted with the data in the temperature restoration database using mathematical tools, so as to understand the current internal state of the cable and determine whether the temperature restoration process is smooth.
2. The method for monitoring dielectric loss and capacitance during the temperature recovery process of a superconducting cable according to claim 1, characterized in that: The step S1 specifically includes the following steps: S11, superconducting cable trips and exits grid operation; S12, the refrigeration system stops running, the liquid nitrogen storage tank is closed, and the liquid nitrogen circulation is stopped; S13. Liquid nitrogen gradually vaporizes, and the release valve of the cable refrigeration system is opened to discharge nitrogen into the atmosphere to control the internal pressure.
3. The method for monitoring dielectric loss and capacitance during the temperature recovery process of a superconducting cable according to claim 1, characterized in that: The set monitoring time interval is 4 hours.
4. The method for monitoring dielectric loss and capacitance during the temperature recovery process of a superconducting cable according to claim 1, characterized in that: The capacitance value and dielectric loss value of the superconducting cable are specifically measured by using a dielectric loss measuring instrument.
5. A method for monitoring dielectric loss and capacitance during the temperature recovery process of a superconducting cable according to any one of claims 1 to 4, characterized in that: The effective value of the test voltage is 500V.