Silicone-functionalized polyurethanes for improving surface hydrophobicity
Through the NCO-capped polysiloxane prepolymer of general formula (I), the problems of insufficient compatibility and hydrophobicity loss of silicone structural units in the coating are solved, and high compatibility and durability are achieved, ensuring that High surface hydrophobicity and reflux properties of the coating.
Patent Information
- Application Number
- CN202080078986.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-15
- Filing Date
- 2020-11-09
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-11-09
AI Technical Summary
The compatibility of the existing silicone structural units in the coating is insufficient, resulting in the silicone chains that accumulate on the surface area of the coating, easily contact with water and peel off, loss of hydrophobicity, and insufficient surface hydrophobic strength.
Using the NCO-capped polysiloxane prepolymer of the general formula (I), the polysiloxane polyol is reacted with diisocyanate and polyisocyanate to form a NCO-capped polysiloxane with high compatibility, followed by the polyol and Other isocyanate reactions to prepare a curing agent with high surface hydrophobicity.
The surface hydrophobicity of the paint is improved, the bonding force with the matrix is enhanced, and the hydrophobicity is not affected by surface scratches or water, providing better durability and reflux performance.
Smart Images

Figure 676139DEST_PATH_IMAGE010
Abstract
Description
[0001] The present invention relates to NCO-terminated polysiloxane prepolymers, a process for their preparation, formulations comprising NCO-terminated polysiloxane prepolymers and the use of such NCO-terminated polysiloxane prepolymers in paint formulations.
[0002] It is known that NCO-terminated prepolymers can be used as curing components in polyurethane paint or coating systems. These prepolymers are usually obtained by reacting polyols with diisocyanates or polyisocyanates. As curing components, the prepolymers are subsequently reacted in the paint or coating system with other polyols, for example with polyacrylate polyols, to form the corresponding polyurethanes. It is desirable that the surfaces of these coatings have hydrophobic properties, for example to minimize the adhesion of water and / or dirt.
[0003] The incorporation of siloxane units into coatings in order thus to increase the hydrophobicity of the corresponding surfaces is known in the prior art.
[0004] Document WO 2018 / 146016 A1 describes a copolymer comprising at least three structural units, one component having at least one biuret or isocyanurate substructure, another component being a polysiloxane, and another hydrocarbon having at least 6 carbon atoms, which is different from the second component, being used to impart hydrophobic properties to textiles.
[0005] WO 2017 / 151621 A1 discloses non-isocyanate functionalized, siloxane-modified glycidyl carbamates for coatings. Glycidyl carbamates are obtained by reacting an organic polyisocyanate, glycidol and at least one bis(hydroxyalkyl)-terminated polydimethylsiloxane.
[0006] Document US 2008 / 0213599 A1 describes a polymer material obtained by reaction of a mixture comprising amino-functional polyorganosiloxane, polyisocyanate and polyol. This material can be used as an antifouling coating.
[0007] US 2014 / 0275410 A1 discloses an isocyanate-terminated polysiloxane copolymer which can be used as a curing agent or co-reactant in coatings. To produce such a copolymer, a methoxy-functionalized polysiloxane, such as methylphenyl polysiloxane, is reacted with a polyisocyanate to obtain the desired copolymer. In the coating, such a copolymer is subsequently reacted with an isocyanate-reactive group to form the corresponding polyurethane.
[0008] WO 2014 / 149331 A1 likewise relates to an isocyanate-terminated polysiloxane which can be used as a curing agent in coating systems. To produce this polysiloxane, a methoxy-functional polysiloxane is likewise hydrolyzed and then reacted with a polyisocyanate.
[0009] In the systems known in the prior art, the compatibility of the siloxane structural units in the paint system needs to be improved in some cases. Another problem is the accumulation of siloxane chains on the coating surface. If the siloxane chains are mainly present on the surface of the coating, contact with water and scratches on the surface can lead to the peeling of the siloxane layer, so that the required surface hydrophobization provided by the siloxane chains is lost. The polysiloxane structural units present should therefore have a sufficiently strong bond to the substrate. In addition, the strength of the surface hydrophobization itself can also be increased.
[0010] The object of the present invention is therefore to provide polysiloxane-based curing agents for polyurethane-based coatings which have a higher surface hydrophobicity than the coatings known from the prior art. In addition, this hydrophobicity should not be affected by scratching of the surface or the action of water on the surface. A further object of the present invention is therefore to provide correspondingly suitable polysiloxane structural units for use as curing agents in coatings which have a particularly high compatibility and bonding with the substrate.
[0011] These objects are achieved according to the invention by NCO-terminated polysiloxane prepolymers of the general formula (I)
[0012] [(Q) q ]-[(M) m -(P) p -(R) r ] t (I)
[0013] where R, P, M, Q, r, p, m, q and t are defined as follows
[0014] R is in each case independently of one another at least one polyisocyanate unit and / or at least one diisocyanate unit,
[0015] P is in each case independently of one another at least one polyol unit,
[0016] M is in each case independently of one another at least one diisocyanate unit and / or at least one polyisocyanate unit,
[0017] Q is at least one polysiloxane unit,
[0018] r is in each case independently of one another a number from 1 to 10,
[0019] p is in each case independently of one another a number from 1 to 10,
[0020] m is in each case independently of one another a number from 1 to 10,
[0021] q is in each case independently of one another a number from 1 to 10,
[0022] t is an integer from 2 to 5, and
[0023] The existing unit M is directly connected to the unit Q.
[0024] The object is further achieved by a process for preparing the NCO-terminated polysiloxane prepolymers according to the invention, comprising at least the following steps:
[0025] (A) reacting at least one polysiloxane polyol with at least one diisocyanate and / or at least one polyisocyanate to obtain at least one NCO-terminated polysiloxane,
[0026] (B) optionally removing excess of the at least one diisocyanate or at least one polyisocyanate,
[0027] (C) reacting the at least one NCO-terminated polysiloxane from step (A) or (B) with at least one polyol,
[0028] (D) reacting the product obtained in step (C) with at least one polyisocyanate or at least one diisocyanate to obtain an NCO-terminated polysiloxane prepolymer,
[0029] And by the formulations according to the invention comprising at least one NCO-terminated polysiloxane prepolymer according to the invention and by the use of the NCO-terminated polysiloxane prepolymers according to the invention as curing agents in paint formulations.
[0030] The present invention is described in detail below.
[0031] The present invention relates to NCO-terminated polysiloxane prepolymers of general formula (I)
[0032] [(Q) q ]-[(M) m -(P) p -(R) r ] t (I),
[0033] wherein R, P, M, Q, r, p, m, q and t are as defined above.
[0034] The prepolymer of the general formula (I) of the present invention is NCO-terminated. In the present invention, "NCO-terminated" means that preferably 2% to 24% by weight, particularly preferably 4% to 15% by weight, very particularly preferably 5% to 12% by weight of the functional groups present at the terminal are isocyanate groups, i.e. NCO groups.
[0035] The prepolymers of the general formula (I) according to the invention can in principle have any molecular weight known to the person skilled in the art. In a preferred embodiment of the invention, the number average molecular weight Mn of the prepolymers according to the invention is from 445 to 8500 g / mol, particularly preferably from 550 to 6000 g / mol, very particularly preferably from 600 to 5500 g / mol.
[0036] In a preferred embodiment of the present invention, the degree of branching of the prepolymers according to the invention is from 2 to 14, particularly preferably from 3 to 12, very particularly preferably from 4 to 10.
[0037] In the general formula (I), R, P, M, Q, r, p, m, q and t are in particular defined as follows.
[0038] In the general formula (I), M is in each case independently of one another at least one diisocyanate unit and / or at least one polyisocyanate unit. According to the invention, the respective unit M present is directly linked to the unit Q. According to the invention, it is possible that 2 to 5 diisocyanate and / or polyisocyanate units M, preferably 2, 3, 4 or 5 diisocyanate and / or polyisocyanate units M, are linked to the polysiloxane unit Q. In a very particularly preferred embodiment, two diisocyanate and / or polyisocyanate units M are linked to the polysiloxane unit Q.
[0039] According to the invention, M in the general formula (I) particularly preferably means, independently of one another, at least one diisocyanate unit in each case, i.e. there are 2 to 5, preferably 2, 3, 4 or 5, very particularly preferably 2 diisocyanate units M on the polysiloxane unit Q. According to the invention, they can be identical or different; preferably, the diisocyanate units M attached to the polysiloxane unit Q are identical.
[0040] In the present invention, "unit" means that the structural unit present in the compound of general formula (I) is derived from the following reactive compounds. If, for example, a diisocyanate reacts with a diol or a polyol, a carbamate group is formed from each of the isocyanate group and the hydroxyl group. However, the rest of the compound used, for example the 6 methylene groups of hexamethylene diisocyanate, remain unchanged. "Unit" is accordingly understood in the present invention to mean both the compound part that does not participate in the reaction and the functional group formed by the reaction, for example a carbamate group. In the present invention, the corresponding unit is always derived from the compound used in the synthesis.
[0041] In the present invention, "in each case independently of one another" means that if the corresponding unit occurs more than once in the general formula (I), these units are identical or different and are selected in each case from the respective possible units. According to the invention, mixtures of compounds of the general formula (I) may also be present, in which the various possible units are present in the individual molecules.
[0042] The at least one diisocyanate unit M is preferably derived from a diisocyanate according to the invention. The diisocyanate used as unit M is preferably selected from organic aliphatic, alicyclic, araliphatic, aromatic diisocyanates and mixtures thereof. Preferably, aliphatic and / or alicyclic diisocyanates are used as unit M.
[0043] Particularly preferably, according to the invention, a diisocyanate selected from the group consisting of butane 1,4-diisocyanate, pentane 1,5-diisocyanate (pentamethylene diisocyanate, PDI), hexane 1,6-diisocyanate (hexamethylene diisocyanate, HDI), 4,4'-methylenebis(cyclohexyl isocyanate) (H12MDI), 3,5,5-trimethyl-1-isocyanato-3-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1,3- and 1,4-bis(isocyanatomethyl)cyclohexane (H6XDI), naphthalene 1,5-diisocyanate As unit M, diisocyanates include esters, diphenylmethane diisocyanate (2,2'-, 2,4'- and 4,4'-MDI or mixtures thereof), diisocyanatomethylbenzenes (toluene 2,4- and 2,6-diisocyanate, TDI) and technical-grade mixtures of these two isomers as well as 1,3- and / or 1,4-bis(isocyanatomethyl)benzene (XDI), 3,3'-dimethylbiphenyl 4,4'-diisocyanate (TODI), 1,4-p-phenylene diisocyanate (PPDI) and cyclohexyl diisocyanate (CHDI) and mixtures thereof.
[0044] The diisocyanates present according to the invention as unit M are very particularly preferably selected from hexane 1,6-diisocyanate (hexamethylene diisocyanate, HDI), pentane 1,5-diisocyanate (pentamethylene diisocyanate, PDI), 3,5,5-trimethyl-1-isocyanato-3-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 4,4′-methylenebis(cyclohexyl isocyanate) (H12MDI) and mixtures thereof.
[0045] In a less preferred embodiment according to the invention, M in the general formula (I) denotes at least one polyisocyanate unit. The polyisocyanates used for this purpose may be selected from aliphatic, cycloaliphatic, araliphatic, aromatic polyisocyanates and mixtures thereof.
[0046] Examples of polyisocyanates present as units M are selected from triisocyanates such as 3,5,5-trimethyl-1-isocyanato-3-isocyanatomethylcyclohexane or higher molecular weight oligomers with biuret, uretdione, isocyanurate, iminooxadiazinedione, allophanate, urethane and / or carbodiimide / uretonimine structural units obtainable by reaction of diisocyanates or triisocyanates selected from butane 1,4-diisocyanate, pentane 1,5-diisocyanate (pentamethylene diisocyanate, PDI), hexane 1,6-diisocyanate (hexamethylene diisocyanate, HDI), 4-isocyanatomethyloctane 1,8-diisocyanate (nonane triisocyanate, TIN), 4,4'-methylenebis(cyclohexyl isocyanate) ( The following are the main products of the present invention: H12MDI), 3,5,5-trimethyl-1-isocyanato-3-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1,3- and 1,4-bis(isocyanatomethyl)cyclohexane (H6XDI), naphthalene 1,5-diisocyanate, diphenylmethane diisocyanate (2,2'-, 2,4'- and 4,4'-MDI or mixtures thereof), diisocyanatomethylbenzene (toluene 2,4- and 2,6-diisocyanate, TDI) and technical grade mixtures of these two isomers as well as 1,3- and / or 1,4-bis(isocyanatomethyl)benzene (XDI), 3,3'-dimethylbiphenyl 4,4'-diisocyanate (TODI), 1,4-p-phenylene diisocyanate (PPDI), cyclohexyl diisocyanate (CHDI) and mixtures thereof.
[0047] In the compounds of the general formula (I), P denotes, independently of one another, in each case at least one polyol unit. The at least one polyol unit is preferably derived according to the invention from a polyol.
[0048] According to the invention either polymeric polyols or low molecular weight polyols may be present.
[0049] The polyols P used according to the invention may be compounds which contain at least one Zerev-active group, for example a hydroxyl or thiol group.
[0050] Polyols P which are particularly preferred according to the invention have an average OH or SH functionality of at least 1.5.
[0051] Polyols P which are preferred according to the invention are selected from diols, triols, tetraols, polyols and mixtures thereof.
[0052] Particularly preferred polyols as units P are selected from ethane-1,2-diol, propane-1,3-diol, propane-1,2-diol, butane-1,4-diol, glycerol, trimethylolpropane, pentaerythritol, polyols and mixtures thereof.
[0053] According to the invention, preferably, the polyol P is selected from polyether polyols, polyester polyols, polyurethane polyols, polysiloxane polyols, polycarbonate polyols, polybutadiene polyols, polyacrylate polyols, polymethacrylate polyols, copolymers of polyacrylate polyols and polymethacrylate polyols, and mixtures thereof.
[0054] In a preferred embodiment, the at least one polyol P is a polymeric polyol, in particular a polyol. The polyol preferably has a weight-average molecular weight Mw of more than 500 g / mol, more preferably from 800 to 100,000 g / mol, in particular from 1,000 to 50,000 g / mol, in each case measured by gel permeation chromatography (GPC) against polystyrene standards.
[0055] The polyol preferably has an OH number of 30 to 400 mg KOH / g, in particular 100 to 300 KOH / g. The hydroxyl number (OH number) indicates how many milligrams of potassium hydroxide are equivalent to the amount of acetic acid bound to 1 gram of substance in the acetylation. In this determination, the sample is boiled with acetic anhydride-pyridine and the acid formed is titrated with potassium hydroxide solution (DIN 53240-2 2:2007-11).
[0056] The glass transition temperature of the polyols preferred according to the invention, measured by means of DSC measurement in accordance with DIN EN ISO 11357-2-2:2014-07, is preferably from -150 to 100°C, more preferably from -120°C to 80°C.
[0057] According to the present invention, preferably, the at least one polyol P is selected from polyether polyols, polyester polyols, polyurethane polyols, polysiloxane polyols, polyacrylate polyols and mixtures thereof.
[0058] The polyether polyols preferably used according to the invention can be obtained in a manner known per se by alkoxylation of suitable starter molecules under base catalysis or using double metal cyanide compounds (DMC compounds). Examples of suitable starter molecules for preparing polyether polyols are simple low molecular weight polyols, water, organic polyamines having at least two NH bonds or any mixtures of such starter molecules.
[0059] Preferred starter molecules for the preparation of polyether polyols by alkoxylation, in particular by the DMC process, are in particular simple polyols such as ethylene glycol, 1,3-propylene glycol, butane-1,4-diol, hexane-1,6-diol, neopentyl glycol, 2-ethylhexane-1,3-diol, glycerol, trimethylolpropane, pentaerythritol and low molecular weight hydroxyl-containing esters of such polyols with dicarboxylic acids of the type mentioned below, or low molecular weight ethoxylation or propoxylation products of such simple polyols, or any mixtures of such modified or unmodified alcohols. Alkylene oxides suitable for the alkoxylation are in particular ethylene oxide and / or propylene oxide, which can be used for the alkoxylation in any order or in mixed form.
[0060] Suitable polyester polyols according to the invention are described, for example, in EP-A-0 994 1 17 and EP-A-1 273 640. The polyester polyols can be prepared in a known manner by low molecular weight polycarboxylic acid derivatives, for example succinic acid, adipic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, tetrachlorophthalic anhydride, endomethylenetetrahydrophthalic anhydride, glutaric anhydride, maleic acid, maleic anhydride, fumaric acid, dimerized fatty acids, trimerized fatty acids, phthalic acid, phthalic anhydride, isophthalic acid, terephthalic acid, citric acid or trimellitic acid. Polyester polyols can be prepared by polycondensation of hydroxycarboxylic acids with low molecular weight polyols, such as ethylene glycol, diethylene glycol, neopentyl glycol, hexanediol, butanediol, propylene glycol, glycerol, trimethylolpropane, 1,4-hydroxymethylcyclohexane, 2-methylpropane-1,3-diol, butane-1,2,4-triol, triethylene glycol, tetraethylene glycol, polyethylene glycol, dipropylene glycol, polypropylene glycol, dibutylene glycol and polybutylene glycol or by ring-opening polymerization of cyclic carboxylic acid esters, such as ε-caprolactone. In addition, hydroxycarboxylic acid derivatives, such as lactic acid, cinnamic acid or hydroxycaproic acid, can also be polycondensed to form polyester polyols. However, polyester polyols of oleochemical origin can also be used. Such polyester polyols can be prepared, for example, by complete ring opening of epoxidized triglycerides of a fat mixture containing at least partly ethylenically unsaturated fatty acids and one or more alcohols having 1 to 12 carbon atoms and by subsequent partial transesterification of the triglyceride derivatives into alkyl ester polyols having 1 to 12 carbon atoms in the alkyl group.
[0061] Polyurethane polyols suitable according to the invention are preferably prepared by reaction of polyester polyol prepolymers with suitable di- or polyisocyanates and are described, for example, in EP-A-1 273 640 and EP-A-0 148 329. Preference is given to polyurethane polyols prepared using HDI, PDI, IPDI or H12MDI. The number-average molecular weight is preferably 500 to 2000 g / mol, the average functionality is 2.0 to 3.5. Examples of suitable polyester polyols and suitable polyisocyanates are in each case those mentioned above.
[0062] Silicone polyols suitable according to the invention as polyol component P are described, for example, in WO-A-01 / 09260, the silicone polyols listed therein preferably being used in combination with other polyhydroxy compounds, in particular those having a higher glass transition temperature.
[0063] Polyacrylate polyols very particularly preferred according to the invention are generally copolymers of acrylic acid and / or methacrylic acid with hydroxyl-containing ethylenically unsaturated monomers and preferably have a weight-average molecular weight Mw of 270 to 22 000 g / mol, preferably 500 to 18 000 g / mol, more preferably 800 to 12 000, in each case determined by gel permeation chromatography (GPC) against polystyrene standards. The glass transition temperature of these copolymers is generally in the range of -100 to 100° C., in particular -50 to 80° C., in each case determined by DSC measurement in accordance with DIN EN ISO 11357-2-2:2014-07.
[0064] Preferred poly(meth)acrylate polyols have an OH number of 60 to 250 mg KOH / g, in particular 70 and 200 mg KOH / g, and an acid number of 0 and 30 mg KOH / g. The acid number indicates the number of milligrams of potassium hydroxide consumed to neutralize 1 gram of the respective compound (DIN EN ISO 2114:2002-06).
[0065] The preparation of suitable poly(meth)acrylate polyols is known per se to the person skilled in the art. They are obtained by free-radical polymerization of acrylic acid and / or methacrylic acid with hydroxyl-containing ethylenically unsaturated monomers and optionally further ethylenically unsaturated monomers. Examples of suitable ethylenically unsaturated compounds are ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, isopropyl acrylate, isopropyl methacrylate, butyl acrylate, butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, amyl acrylate, amyl methacrylate, hexyl acrylate, hexyl methacrylate, ethylhexyl acrylate, ethylhexyl methacrylate, 3,3,5-trimethylhexyl acrylate, 3,3,5-trimethylhexyl methacrylate, octadecyl acrylate, octadecyl methacrylate, dodecyl acrylate or dodecyl methacrylate, cycloalkyl acrylates and / or methacrylates, such as cyclopentyl acrylate, cyclopentyl methacrylate, isobornyl acrylate, isobornyl methacrylate or, in particular, cyclohexyl acrylate and / or methacrylate.
[0066] Suitable hydroxyl-containing ethylenically unsaturated monomers are, in particular, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl acrylate, 3-hydroxypropyl methacrylate, 3-hydroxybutyl acrylate, 3-hydroxybutyl methacrylate, in particular 4-hydroxybutyl acrylate and / or 4-hydroxybutyl methacrylate.
[0067] Further monomeric building blocks for the polyacrylate polyols may be vinylaromatics, such as vinyltoluene, α-methylstyrene or in particular styrene, amides or nitriles of acrylic or methacrylic acid, vinyl esters or vinyl ethers and, in minor amounts, in particular acrylic acid and / or methacrylic acid.
[0068] Low molecular weight polyols P which are preferred according to the invention are derived, for example, from polyols and / or ether alcohols or ester alcohols having 2 to 14 carbon atoms, preferably 4 to 10 carbon atoms.
[0069] Preferably, the low molecular weight polyol P suitable according to the invention is selected from ethane-1,2-diol, propane-1,2-diol, propane-1,3-diol, isomeric butanediols, pentanediol, hexanediol, heptanediol, octanediol, decan-1,10-diol, dodecane-1,12-diol, cyclohexane-1,2-diol, cyclohexane-1,4-diol, cyclohexane-1,4-dimethanol, 1,4-bis(2-hydroxyethoxy)benzene, 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), 2,2-bis(4-hydroxycyclohexane-1,4-diol ... 1,2,3-propane (perhydrobisphenol), propane-1,2,3-triol, butane-1,2,4-triol, 1,1,1-trimethylolethane, hexane-1,2,6-triol, 1,1,1-trimethylolpropane (TMP), bis(2-hydroxyethyl)hydroquinone, 1,2,4-trihydroxycyclohexane, 1,3,5-trihydroxycyclohexane, 1,3,5-tri(2-hydroxyethyl)isocyanurate, bis(hydroxymethyl)tricyclo[5.2.1.02,6]decane, 4,8-bis(hydroxymethyl)tricyclo[5.2.1.0 2,6 ]decane, 5,8-bis(hydroxymethyl)tricyclo[5.2.1.0(2,6)], di-trimethylolpropane, 2,2-bis(hydroxymethyl)propane-1,3-diol (pentaerythritol), 2,2,6,6-tetra(hydroxymethyl)-4-oxaheptane-1,7-diol (dipentaerythritol), mannitol or sorbitol, low molecular weight ether alcohols such as diethylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol or dibutylene glycol, low molecular weight ester alcohols such as neopentyl glycol hydroxypivalate and mixtures thereof.
[0070] Very particularly preferred polyols P according to the invention are selected from 1,1,1-trimethylolpropane (TMP), polyesters formed from hexane-1,6-diol, neopentyl glycol, butane-1,4-diol, adipic acid, 2,2,4-trimethylpentane-1,3-diol, 2-butyl-2-ethylpropane-1,3-diol, or polyacrylate polyols formed from styrene, 1-decene, methyl methacrylate, acrylic acid, hydroxyethyl methacrylate, hydrophobic vinyl esters and mixtures thereof.
[0071] In the general formula (I), R denotes in each case, independently of one another, at least one polyisocyanate unit and / or at least one diisocyanate unit.
[0072] In the compounds of the general formula (I), at least one polyisocyanate unit is preferably present as unit R according to the invention.
[0073] The at least one polyisocyanate unit R is preferably derived according to the invention from a polyisocyanate. The at least one polyisocyanate is preferably selected from aliphatic, cycloaliphatic, araliphatic, aromatic polyisocyanates and mixtures thereof.
[0074] Particularly preferably, according to the invention, polyisocyanates selected from triisocyanates such as 3,5,5-trimethyl-1-isocyanato-3-isocyanatomethylcyclohexane or preferably higher molecular weight oligomers with biuret, uretdione, isocyanurate, iminooxadiazinedione, allophanate, urethane and / or carbodiimide / uretonimine structural units are preferably used as units R, wherein the diisocyanates or triisocyanates are selected from butane 1,4-diisocyanate, pentane 1,5-diisocyanate (pentamethylene diisocyanate, PDI), hexane 1,6-diisocyanate (hexamethylene diisocyanate, HDI), 4-isocyanatomethyloctane 1,8-diisocyanate (nonane triisocyanate, TIN), 4,4'-methylenebis(cyclohexyl) ... isocyanate) (H12MDI), 3,5,5-trimethyl-1-isocyanato-3-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1,3- and 1,4-bis(isocyanatomethyl)cyclohexane (H6XDI), naphthalene 1,5-diisocyanate, diphenylmethane diisocyanate (2,2'-, 2,4'- and 4,4'-MDI or mixtures thereof), diisocyanatomethylbenzene (toluene 2,4- and 2,6-diisocyanate, TDI) and technical grade mixtures of these two isomers as well as 1,3- and / or 1,4-bis(isocyanatomethyl)benzene (XDI), 3,3'-dimethylbiphenyl 4,4'-diisocyanate (TODI), 1,4-p-phenylene diisocyanate (PPDI), cyclohexyl diisocyanate (CHDI) and mixtures thereof.
[0075] The polyisocyanates used according to the invention as unit R are very particularly preferably selected from the group consisting of preferably higher molecular weight oligomers with biuret, uretdione, isocyanurate, iminooxadiazinedione, allophanate, urethane and / or carbodiimide / uretonimine structural units obtainable by reaction of diisocyanates or triisocyanates selected from the group consisting of pentane 1,5-diisocyanate (pentamethylene diisocyanate, PDI), hexane 1,6-diisocyanate (hexamethylene diisocyanate, PDI), ester, HDI), 4,4'-methylenebis(cyclohexyl isocyanate) (H12MDI), 3,5,5-trimethyl-1-isocyanato-3-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), diphenylmethane diisocyanate (2,2'-, 2,4'- and 4,4'-MDI or mixtures thereof), diisocyanatomethylbenzene (toluene 2,4- and 2,6-diisocyanate, TDI) and technical grade mixtures of these two isomers and their mixtures.
[0076] In a less preferred embodiment of the invention, those used as units R are derived from diisocyanates. They are selected, for example, from organic aliphatic, cycloaliphatic, araliphatic, aromatic diisocyanates and mixtures thereof.
[0077] Examples of diisocyanates used as unit R are selected from butane 1,4-diisocyanate, pentane 1,5-diisocyanate (pentamethylene diisocyanate, PDI), hexane 1,6-diisocyanate (hexamethylene diisocyanate, HDI), 4,4'-methylenebis(cyclohexyl isocyanate) (H12MDI), 3,5,5-trimethyl-1-isocyanato-3-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1,3- and 1,4-bis(isocyanatomethyl)cyclohexane (H6XDI), naphthalene 1 ,5-diisocyanate, diphenylmethane diisocyanate (2,2'-, 2,4'- and 4,4'-MDI or mixtures thereof), diisocyanatomethylbenzenes (toluene 2,4- and 2,6-diisocyanate, TDI) and technical grade mixtures of these two isomers as well as 1,3- and / or 1,4-bis(isocyanatomethyl)benzene (XDI), 3,3'-dimethylbiphenyl 4,4'-diisocyanate (TODI), 1,4-p-phenylene diisocyanate (PPDI), as well as cyclohexyl diisocyanate (CHDI) and mixtures thereof.
[0078] In the general formula (I), Q is at least one polysiloxane unit. The at least one polysiloxane unit Q present in the compound of the general formula (I) is preferably derived according to the invention from polysiloxane polyols, polysiloxane polyamines or polysiloxane polythiols, in particular polysiloxane polyols.
[0079] According to the invention, it is possible in principle to use all polysiloxane polyols, polysiloxane polyamines or polysiloxane polythiols known to the person skilled in the art in order to obtain the corresponding polysiloxane units in the compounds of the general formula (I).
[0080] In a preferred embodiment of the present invention, the polysiloxane units Q present are based on compounds of the general formula (II)
[0081] (II),
[0082] in
[0083] R, R4, R5, R6, n, n 1 ,m,m 1 and k are defined as follows:
[0084] n and n 1 are independently 0 or greater than 0, preferably 10 to 200, more preferably 15 to 100, and (n+n 1 ) is less than 500, preferably less than 200, more preferably less than 100,
[0085] m and m 1 are independently 0 or greater than 0, preferably 0 to 30, more preferably 0.1 to 25, and (m+m 1 ) is less than 60, preferably less than 30, more preferably less than 25,
[0086] k is 0 to 10, preferably 0 to 5, for example 0, 1, 2, 3, 4 or 5,
[0087] R is at least one radical selected from linear, cyclic or branched, aliphatic or aromatic, saturated or unsaturated carbon radicals having 1 to 20 carbon atoms and optionally heteroatoms selected from O, P, S, N, which in each case optionally have a functional group selected from halogen radicals, hydroxyl groups, amine groups, mercapto groups, carboxyl groups, alkoxy groups, epoxy groups, alkylalkoxysilylalkyl groups or alkoxysilylalkyl groups, in particular methyl groups,
[0088] R4, R5, R6 are at least one group selected from linear, cyclic or branched, aliphatic or aromatic, saturated or unsaturated carbon groups having 1 to 20 carbon atoms and optionally heteroatoms selected from O, P, S, N, which in each case optionally have a halogen group, a hydroxyl group, an amine group, a mercapto group, a carboxyl group, an alkoxy group, an epoxy group, an alkylalkoxysilylalkyl group or an alkoxysilylalkyl group, -(CH2) x'' -O-(CH2-CH2O-) x -(CH2-CH(R')O-) y -(SO) z -R" functional group, where
[0089] x is 0 to 100, preferably 1 to 5,
[0090] x'' is 0 to 100, preferably 1 to 4,
[0091] y is 0 to 100, preferably 1 to 5,
[0092] z is 0 to 100, preferably 0 to 1,
[0093] R' is an optionally substituted alkyl or aryl group having 1 to 12 carbon atoms, which is substituted, for example, by an alkyl group, an aryl group or a haloalkyl or haloaryl group, and
[0094] R" is a hydrogen radical or an alkyl radical having 1 to 4 carbon atoms, a -C(O)-R"' radical in which R"'=alkyl, a -CH2-O-R' radical, an alkylaryl radical or a -C(O)NH-R' radical,
[0095] SO is the styrene oxide group -CH(C6H5)-CH2-O-,
[0096] At least two, preferably 2 to 5, more preferably 2 groups selected from R, R4, R5 and / or R6 carry at least one hydroxyl group, amine group and / or thiol group, preferably at least one hydroxyl group.
[0097] In the compounds of the general formula (II), the various monomer units of the siloxane chain and / or polyoxyalkylene chain may be constructed blockwise with one another or have a random distribution.
[0098] In the present invention, all index numbers and numerical ranges given according to the present invention are to be understood as the average value of the possible statistical distribution of the actually existing structures and / or their mixtures. The index numbers according to the present invention may also be present in the form of decimals (numbers separated by decimal points), for example 1.2. In this case, it is the average value of a mixture containing compounds with different index numbers.
[0099] In a preferred embodiment, R in the general formula (II) is methyl, ethyl and / or phenyl.
[0100] Further preferably, R in the general formula (II) refers to R4, R5 and / or R6, for example
[0101]
[0102]
[0103]
[0104]
[0105] in
[0106] m = 6 to 20, preferably 8 to 18,
[0107] n = 2 to 18, preferably 4 to 8,
[0108] o = 0 to 30, preferably 2 to 20, especially 5 to 15,
[0109] p = 0 to 30, preferably 0 to 10,
[0110] q = 0 to 30, preferably 2 to 20, especially 5 to 15,
[0111] r = 0 to 30, preferably 0 to 10,
[0112] s = 0 to 10, preferably 1 to 5,
[0113] t = 1 to 20, preferably 1 to 10,
[0114] u = 1 to 10, preferably 2 to 4,
[0115] v = 1 to 10, preferably 2 to 5,
[0116] w = 1 to 6, preferably 1 to 3,
[0117] x = 1 to 6, preferably 2 to 4,
[0118] y = 1 to 10, preferably 1 to 3.
[0119] The polysiloxane polyols, polysiloxane polyamines or polysiloxane polythiols preferably used according to the invention have a functionality of, for example, 2 to 6, particularly preferably 2, 3, 4, 5 or 6 and very particularly 2.
[0120] The polysiloxane polyols, polysiloxane polyamines or polysiloxane polythiols preferably used according to the invention contain, for example, 1 to 50, particularly preferably 2 to 30 and very particularly 3 to 20 repeating units. According to the invention, "siloxane" is understood to mean a radical having a base structure containing two or more -SiO- groups.
[0121] According to the invention, very particular preference is given to using as polysiloxane polyols α,ω-hydroxypropyl-terminated polydimethylsiloxanes having an OH content of 1% to 10%, preferably 2 to 8% by weight, a molecular weight of 200 to 2000 g / mol, preferably 400 to 1000 g / mol, and a solids content of 100% by weight, so that after reaction with the NCO groups of the diisocyanate and / or polyisocyanate units M, the corresponding polysiloxane units Q are present.
[0122] The present invention preferably relates to the polysiloxane prepolymers according to the invention, wherein the at least one polysiloxane unit is present in an amount of 0.1% to 5% by weight, based on the entire polysiloxane prepolymer.
[0123] The present invention furthermore preferably relates to the polysiloxane prepolymers according to the invention, wherein the polysiloxane prepolymers according to the invention have a number average molecular weight Mn of <4000 g / mol, preferably >450 g / mol and <3000 g / mol, particularly preferably >650 g / mol and <2500 g / mol, very particularly preferably >800 g / mol and <2500 g / mol. The number average molecular weight Mn is determined by gel permeation chromatography (GPC) in tetrahydrofuran at 23° C. The operation was carried out according to DIN 55672-1:2016-03: "Gel permeation chromatography, part 1 – Tetrahydrofuran as eluent" (SECurityGPC System from PSS Polymer Service, flow rate 0.6 ml / min; columns: 2 × PSS SDV (100A), 2 × PSS SDV (50A), 8 × 300 mm, 5 µm; RID detector (RI-Agilent 1260). Polystyrene samples of known molar mass were used for calibration. The number-average molecular weight was calculated by means of the software.
[0124] In the general formula (I), r describes in each case the number of units R present, R in turn being selected from the abovementioned groups. In the general formula (I), r preferably in each case independently of one another is a number from 1 to 30, particularly preferably from 1 to 20, more preferably from 1 to 5, r very particularly preferably being 1.
[0125] In the general formula (I), m describes in each case the number of units M present, M in turn being selected from the abovementioned groups. In the general formula (I), m preferably in each case independently of one another is a number from 1 to 30, particularly preferably from 1 to 20, more preferably from 1 to 5, m very particularly preferably being 1.
[0126] In the general formula (I), p describes in each case the number of units P present, P in turn being selected from the abovementioned groups. In the general formula (I), p preferably in each case independently of one another is a number from 1 to 30, particularly preferably from 1 to 20, more preferably from 1 to 5, p very particularly preferably being 1.
[0127] In the general formula (I), q describes in each case the number of units Q present, which in turn are selected from the above-mentioned groups. In the general formula (I), q preferably refers in each case independently of one another to a number of 1 to 30, particularly preferably 1 to 20, more preferably 1 to 5, q being very particularly preferably 1.
[0128] In the general formula (I), t in each case describes the presence of a unit -[(M) m -(P) p -(R) r In the general formula (I), t preferably is in each case independently of one another a number of 2 to 5, particularly preferably 2, 3 or 4, t being very particularly preferably 2.
[0129] Monofunctional compounds can additionally also be used according to the invention as compounds containing siloxane groups, for example poly(dimethylsiloxane)propylhydroxy copolymers, in particular heptamethyl-2-(3-hydroxypropyl)trisiloxane having a functionality of 1 and a molecular weight of 280 g / mol.
[0130] The present invention also relates to a process for preparing the NCO-terminated polysiloxane prepolymer of the present invention, comprising at least the following steps:
[0131] (A) reacting at least one polysiloxane polyol, polysiloxane polyamine and / or polysiloxane polythiol with at least one diisocyanate and / or at least one polyisocyanate to obtain at least one NCO-terminated polysiloxane,
[0132] (B) optionally removing excess of the at least one diisocyanate and / or at least one polyisocyanate,
[0133] (C) reacting the at least one NCO-terminated polysiloxane from step (A) or (B) with at least one polyol,
[0134] (D) reacting the product obtained in step (C) with at least one diisocyanate or at least one polyisocyanate to obtain an NCO-terminated polysiloxane prepolymer.
[0135] Each step of the method of the present invention is described in detail below.
[0136] Step (A) of the process of the present invention comprises reacting at least one polysiloxane polyol, polysiloxane polyamine and / or polysiloxane polythiol, preferably at least one polysiloxane polyol, with at least one diisocyanate and / or at least one polyisocyanate, preferably at least one diisocyanate, to obtain at least one NCO-terminated polysiloxane.
[0137] Step (A) of the process of the invention can generally be carried out by all methods known to the person skilled in the art. Preferably, step (A) of the process of the invention can be carried out in an apparatus known to the person skilled in the art, such as a stirred tank reactor with inlets and outlets for reactants and products. Optionally, step (A) of the process of the invention can be carried out under exclusion of water and air, for example in a dry atmosphere of nitrogen or a noble gas, such as helium or argon.
[0138] Step (A) of the process of the invention can be carried out, for example, by mixing the substrates, in particular the at least one diisocyanate and / or the at least one polyisocyanate and the at least one polysiloxane polyol, polysiloxane polyamine and / or polysiloxane polythiol, with one another and reacting them together.
[0139] In a preferred embodiment, step (A) of the process of the invention is carried out by initially charging the at least one diisocyanate and / or the at least one polyisocyanate. The at least one diisocyanate and / or the at least one polyisocyanate can be initially charged according to the invention in a solvent or without a solvent. Suitable solvents for this reaction step are preferably solvents which do not themselves participate in the reaction, such as ethyl acetate, butyl acetate, methoxypropyl acetate, solvent naphtha (Solvesso 100) and / or methyl ethyl ketone. Step (A) of the process of the invention is preferably carried out in the absence of a solvent. The initially charged at least one diisocyanate and / or at least one polyisocyanate is preferably heated according to the invention to a temperature above room temperature, for example 60 to 120° C., preferably 80 to 110° C.
[0140] More preferably, the at least one polysiloxane polyol, polysiloxane polyamine and / or polysiloxane polythiol is added to an initial charge of at least one diisocyanate and / or at least one polyisocyanate.
[0141] The ratio of NCO groups to NCO-reactive groups, ie OH, SH and / or NH groups, present in the reaction mixture is generally from 1 to 50, preferably from 2 to 30, more preferably from 2 to 20 in step (A) of the process of the invention.
[0142] The resulting reaction mixture is usually stirred until the reaction is complete. The reaction mixture is preferably stirred for 1 to 8 hours, preferably 2 to 6 hours.
[0143] The reaction of step (A) of the process according to the invention is preferably carried out at a temperature of 60 to 120°C, more preferably 80 to 110°C.
[0144] After step (A) of the process of the invention, a reaction product comprising the at least one polysiloxane polyol, polysiloxane polyamine and / or polysiloxane polythiol and at least one diisocyanate or at least one polyisocyanate, ie at least one NCO-terminated polysiloxane, is obtained.
[0145] The reaction mixture obtained in step (A) can be used according to the invention directly in step (C) of the process according to the invention. This is preferably done when the ratio of NCO groups to NCO-reactive groups in the reaction mixture has been set so that an NCO-terminated polysiloxane is obtained, but no excess of at least one diisocyanate and / or at least one polyisocyanate is present, i.e. no excess of at least one diisocyanate and / or at least one polyisocyanate is present in the reaction mixture obtained after step (A).
[0146] In a preferred embodiment of the present invention, the reaction mixture obtained in step (A) of the process of the invention is transferred to step (B) of the process of the invention, particularly preferably without further intermediate steps.
[0147] Optional step (B) of the process of the invention comprises removing excess at least one diisocyanate or at least one polyisocyanate.
[0148] Preference is given to carrying out step (B). By removing excess at least one diisocyanate or at least one polyisocyanate in step (B) of the process according to the invention, NCO-terminated polysiloxane polyols are obtained which are not contaminated with at least one diisocyanate and / or at least one polyisocyanate. Carrying out step (B) according to the invention thus makes it possible to obtain the desired target compounds according to the invention, i.e. NCO-terminated polysiloxane prepolymers, with high purity, homogeneity and an increased molecular weight compared to alternative production processes.
[0149] The content of at least one diisocyanate or at least one polyisocyanate, preferably at least one diisocyanate, in the reaction mixture after step (B) is preferably according to the invention at most 5% by weight, preferably 1% to 0.01% by weight.
[0150] Step (B) of the process according to the invention can in principle be carried out by all methods known to the person skilled in the art. The present invention preferably relates to the process according to the invention, wherein step (B) is carried out by thin-film evaporation, phase separation, precipitation or a combination thereof.
[0151] Step (B) of the process of the present invention is preferably carried out by thin film evaporation. More preferably, thin film evaporation is carried out at a temperature of 50 to 200° C., preferably 80 to 120° C. In addition, thin film evaporation is carried out at a pressure of preferably 0.001 to 500 mbar (absolute), more preferably 0.01 to 200 mbar (absolute).
[0152] Step (B) of the process according to the invention can be carried out in all apparatuses known to the person skilled in the art, in particular in thin-film evaporators or apparatuses suitable for phase separation or precipitation.
[0153] The NCO-terminated silicone polyols obtained after step (A) or (B), preferably after step (B), have an NCO content of generally 1% to 20% by weight, preferably 4% to 18% by weight.
[0154] After step (A) or (B), preferably after step (B), the NCO-terminated polysiloxane polyol obtained has a concentration of generally 100% to 50% by weight, preferably 100% to 75% by weight. This means that the desired product is preferably obtained without impurities and solvents.
[0155] After step (A) or (B), preferably after step (B), the NCO-terminated polysiloxane polyol obtained has a viscosity of generally 50 to 4000 mPa·s, preferably 100 to 2500 mPa·s, more preferably 100 to 1000 mPa·s.
[0156] Step (C) of the process of the invention comprises reacting the at least one NCO-terminated polysiloxane from step (A) or (B) with at least one polyol.
[0157] Step (C) of the process according to the invention can generally be carried out by all methods known to the person skilled in the art. The NCO-terminated polysiloxane from step (A) or (B) is preferably mixed and reacted with the at least one polyol according to the invention. Suitable and preferred polyols according to the invention have already been mentioned above.
[0158] The molar ratio of NCO groups present in the reaction mixture of step (C) of the process according to the invention to the OH, NH and / or SH groups present in the at least one polyol used is preferably from 0.001 to 0.9, more preferably from 0.01 to 0.8.
[0159] Step (C) of the process of the present invention can be carried out in the presence of a solvent or in the absence of a solvent. In a preferred embodiment, step (C) of the process of the present invention is carried out in the presence of a solvent. The solvent used in step (C) of the process of the present invention is preferably selected from esters, such as 1-methoxy-2-propyl acetate (MPA), butyl acetate (BA), dibasic esters, ketones, such as methyl ethyl ketone, ethers, such as diethyl ether, and mixtures thereof.
[0160] In the reaction mixture of step (C) of the process according to the invention, the components are present together in a concentration of 20% to 80% by weight, preferably 30% to 70% by weight, in each case based on the solids content of the entire solution.
[0161] The reaction of step (c) of the process according to the invention can be carried out in the presence of at least one catalyst. Suitable catalysts are known per se to those skilled in the art and are selected, for example, from tin organic compounds, particularly suitable being dibutyltin laurate. If a catalyst is used in step (c) of the process according to the invention, it is preferably present in a concentration of 0.01% to 0.1% by weight, based on the reaction mixture.
[0162] Step (C) of the process of the present invention can be carried out in an apparatus known per se to the person skilled in the art, for example a stirred tank reactor with corresponding inlets and outlets. Furthermore, step (C) of the process of the present invention can preferably be carried out in an inert atmosphere, for example in an atmosphere of nitrogen or a noble gas, for example helium or argon.
[0163] Step (C) of the process of the present invention is preferably carried out at a temperature of 20 to 100° C., preferably 40 to 80° C. In general, step (C) of the process of the present invention is carried out at atmospheric pressure or at a pressure slightly above atmospheric pressure by using an inert gas.
[0164] Step (C) of the process according to the invention is generally carried out until all NCO groups present have reacted, i.e. have reacted with OH or SH groups. Preferably, step (C) of the process according to the invention is carried out until the content of NCO groups present in the reaction mixture is less than 0.5% by weight, more preferably less than 0.2% by weight, in each case based on the entire reaction mixture. Very particularly preferably, no more NCO groups are present in the reaction mixture, i.e. the NCO group content is below the analytical detection limit known to the person skilled in the art.
[0165] In a preferred embodiment of the method of the present invention, the reaction mixture obtained after step (C) can be directly transferred to step (D) of the method of the present invention. The reaction mixture can be optionally post-treated after step (C) and before step (D).
[0166] Step (D) of the process of the present invention comprises reacting the product obtained in step (C) with at least one polyisocyanate and / or at least one diisocyanate, preferably with at least one polyisocyanate to obtain an NCO-terminated polysiloxane prepolymer.
[0167] Step (D) of the process of the invention can generally be carried out by all methods known to the person skilled in the art. In a preferred embodiment of the present invention, the at least one polyisocyanate and / or the at least one diisocyanate, preferably the at least one polyisocyanate, is added to the reaction mixture obtained from step (C).
[0168] The molar ratio of OH or SH groups present in the reaction mixture used in step (D) to the NCO groups added in step (D) is preferably from 1.1 to 20, more preferably from 2 to 12 according to the invention.
[0169] The step (D) of the method of the present invention is preferably carried out in the presence of a solvent. In a preferred embodiment of the method of the present invention, the reaction mixture used in step (D) already contains the solvent from step (C). In a further preferred embodiment of the present invention, a solvent is added in the step (D) of the method of the present invention. In a preferred embodiment, so much solvent is added in step (D) that the concentration of the dissolved components in the reaction mixture is 20% to 80% by weight, preferably 30% to 70% by weight, in each case based on the entire reaction mixture. The solvent suitable for step (D) has been mentioned for step (C).
[0170] Step (D) of the process of the present invention can be carried out in apparatus known to those skilled in the art, for example in a stirred tank reactor with corresponding inlets and outlets. In addition, step (D) of the process of the present invention can preferably be carried out in an inert atmosphere, for example in an atmosphere of nitrogen or a noble gas, for example helium or argon.
[0171] Step (D) of the process of the present invention is preferably carried out at a temperature of 20 to 100° C., preferably 40 to 80° C. In general, step (D) of the process of the present invention is carried out at atmospheric pressure or at a pressure slightly above atmospheric pressure by using an inert gas.
[0172] After step (D) of the process according to the invention, the desired NCO-terminated polysiloxane prepolymer according to the invention is obtained, in particular a prepolymer of the general formula (I). Step (D) may optionally be followed by a work-up step, for example by separating off the solvent present, such as ethyl acetate, methoxypropyl acetate, butyl acetate, solvent naphtha (Solvesso 100) or a mixture thereof.
[0173] The NCO-terminated polysiloxane prepolymers obtained after step (D) have an NCO content of generally 0.1% to 17% by weight, preferably 2% to 14% by weight.
[0174] The NCO-terminated polysiloxane prepolymer obtained after step (D) has a solids content of generally 20% to 80% by weight, preferably 30% to 70% by weight.
[0175] The NCO-terminated polysiloxane prepolymer obtained after step (D) has a Hazen color index of generally 0 to 300, preferably 10 to 150.
[0176] Another subject of the present invention is an NCO-terminated polysiloxane prepolymer obtainable or produced by the process according to the invention. The NCO-terminated polysiloxane prepolymers according to the invention are characterized in particular in that, on the one hand, the coatings obtainable therefrom have significantly better residual gloss and flowback than similar systems which do not contain the NCO-terminated polysiloxane prepolymers according to the invention, and on the other hand, as surface-active substances, they allow a reduced use of flow additives or the complete omission of flow additives. The measurement of residual gloss and flowback is preferably carried out as shown in the Examples section, and the reduction of leveling additives is preferably observed by visually evaluating the coating to see whether "orange peel" has formed.
[0177] The present invention further relates to formulations which comprise at least one NCO-terminated polysiloxane prepolymer according to the invention, preferably in an amount of 5% to 70% by weight, based on the entire formulation. In particular, the formulation according to the invention is a paint formulation.
[0178] Besides the NCO-terminated polysiloxane prepolymers according to the invention, corresponding formulations are known per se to the person skilled in the art.
[0179] The paint formulations of the invention can preferably be present in the form of two-component formulations known per se to the person skilled in the art.
[0180] The two-component formulations of the invention preferably comprise at least one polyol and optional additives in a first component (component A) and at least one NCO-terminated polysiloxane prepolymer of the invention, at least one polyisocyanate and optional additives in a second component (component B).
[0181] In a preferred embodiment of the present invention, the paint formulation of the invention, in particular the two-component formulation of the invention, is a formulation for a clearcoat and / or a topcoat layer.
[0182] Under varnish of the present invention and / or topcoat layer, there may be a colored paint. The composition, requirements and processing of the colored paint formulation itself are known to those skilled in the art and are described in, for example, the instructions of the automobile company or are for example published in "Farbe und Lack 07 / 2003" (Vincentz-Verlag), in the article "Eine Frage der Einstellung" in the 1st to 3rd page and in U.Poth, "Automotive Coatings Formulation", Vincentz-Verlag 2008, ISBN9783866309043, 137-163 and 213-215 pages or U.Kuttler, "Principles of Automotive OEM Coatings", in Allnex Belgium SA.
[0183] In component A of the two-component formulation of the invention, at least one polyol is preferably present. The polyol is preferably selected from polyester polyols, polyurethane polyols, polysiloxane polyols, polycarbonate polyols, polyacrylate polyols and mixtures thereof, preferably from polyester polyols, polyacrylate polyols, polyurethane polyols and mixtures thereof. The corresponding polyols are known per se to the person skilled in the art and are described, for example, above in this document.
[0184] Polycarbonate polyols that come into consideration are obtainable by reacting carbonic acid derivatives, such as diphenyl carbonate, dimethyl carbonate or phosgene, with diols. Examples of such diols that come into consideration include ethylene glycol, propane-1,2- and 1,3-diol, butane-1,3- and butane-1,4-diol, hexane-1,6-diol, 2-ethylhexane-1,3-diol, octan-1,8-diol, neopentyl glycol, 1,4-bishydroxymethylcyclohexane, 2-methylpropane-1,3-diol, 2,2,4-trimethylpentane-1,3-diol, dipropylene glycol, polypropylene glycol, dibutylene glycol, polybutylene glycol, bisphenol A, tetrabromobisphenol A, and lactone-modified diols. Preferably, the diol component contains 40% to 100% by weight of hexane-1,6-diol and / or hexanediol derivatives, preferably those having not only terminal OH groups but also ether or ester groups, such as the products obtained by reacting 1 mol of hexanediol with at least 1 mol, preferably 1 to 2 mol, of ε-caprolactone or by etherifying hexanediol with itself to give di- or tri-hexanediol. Polyether polycarbonate polyols can also be used.
[0185] Preference is given to polycarbonate polyols based on dimethyl carbonate and hexanediol and / or butanediol and / or ε-caprolactone. Very particular preference is given to polycarbonate polyols based on dimethyl carbonate and hexanediol and / or ε-caprolactone.
[0186] Suitable polyols also include known polyacetal polyols obtainable, for example, by reaction of simple diols, such as diethylene glycol, triethylene glycol, 4,4′-bis((2-hydroxyethoxy)phenyl)dimethylmethane (an adduct of 2 mol of ethylene oxide with bisphenol A), or hexanediol with formaldehyde, or polyacetals prepared by polycondensation of cyclic acetals, such as trioxane.
[0187] Suitable polyols further include those described, for example, in EP-A 0 689 556 and EP-A 0 937 110, for example specific polyols obtainable by epoxidation of fatty acid esters with aliphatic or aromatic polyols under epoxide ring opening.
[0188] Hydroxyl-containing polybutadienes can likewise serve as polyols.
[0189] The polymeric polyols can be used alone or in any desired mixtures with one another. They can be present either without solvent or dissolved in conventional solvents.
[0190] Furthermore, additives may be present in component (A) of the two-component preparations according to the invention. Such additives are known per se to those skilled in the art.
[0191] The optional additives are selected according to the invention from catalysts, solvents, light stabilizers such as UV absorbers and hindered amines (HALS), stabilizers, for example UV stabilizers, fillers, anti-settling agents, defoamers, anti-cratering agents, wetting agents, leveling agents, film-forming aids, reactive diluents, rheology control substances, slip additives, components to prevent staining and / or improve the cleanability of the cured lacquer, matting agents, antioxidants, pigments and mixtures thereof. Preference is given to UV stabilizers, antioxidants, leveling agents, fillers and / or pigments.
[0192] Suitable catalysts according to the invention are suitable for catalyzing the reaction of component A with component B. Such catalysts are known to the person skilled in the art. Suitable are, in particular, tin catalysts, bismuth catalysts, zinc catalysts, zirconium catalysts and amine bases. Particularly suitable are, for example, zinc compounds, such as zinc(II) stearate, zinc(II) n-octoate, zinc(II) 2-ethyl-1-hexanoate, zinc(II) naphthenate, zinc chloride, zinc 2-ethylhexanoate or zinc(II) acetylacetonate, tin compounds, such as tin(II) n-octoate, tin(II) 2-ethyl-1-hexanoate, tin(II) laurate, dibutyltin oxide, dibutyltin dichloride, dibutyltin diacetate, tin(II) ethylhexanoate, dibutyltin(IV) dilaurate, dibutyltin dimaleate or dioctyltin diacetate, zirconium compounds, such as zirconium(IV) 2-ethyl-1-hexanoate, zirconium(IV) isopropoxide, zirconium(IV) n-butoxide, zirconium(IV) 2-ethylhexanoate, zirconium(IV) oxyoctoate, zirconium(IV) neodecanoate, zirconium(IV) naphthenate or zirconium(IV) acetylacetonate, bismuth(III) 2-ethylhexanoate and bismuth(III) octoate.
[0193] The catalyst is preferably used in an amount of 0.01% to 0.5% by weight, more preferably in an amount of 0.01% to 0.3% by weight, based in each case on the total weight of compound A in the first component.
[0194] Component A may further preferably contain at least one solvent. In general, all solvents known to the person skilled in the art are suitable here. Particularly suitable are aromatic and aliphatic solvents, which are preferably selected from butyl acetate, 1-methoxy-2-propyl acetate, 3-methoxy-1-butyl acetate, ethyl acetate, dibasic acid esters, propylene n-butyl ether, methyl ethyl ketone, toluene, xylene, solvent naphtha (hydrocarbon mixture) and mixtures thereof. Preferably, the solvent is contained in an amount of 30% to 90% by weight, more preferably 45% to 70% by weight, based on the total weight of component A.
[0195] The UV stabilizers suitable according to the present invention can be preferably selected from piperidine derivatives, such as 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, 4-benzoyloxy-1,2,2,6,6-pentamethylpiperidine, bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate, bis(1,2,2,6,6-pentamethyl-1-4-piperidyl) sebacate, bis(2,2,6,6-tetramethyl-4-piperidyl) suberate, bis(2,2,6,6-tetramethyl-4-piperidyl) dodecanedioate; benzophenone derivatives, such as 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octyloxybenzophenone. Benzophenone, 2-hydroxy-4-dodecyloxybenzophenone or 2,2'-dihydroxy-4-dodecyloxybenzophenone; benzotriazole derivatives, for example 2-(2H-benzotriazol-2-yl)-4,6-di-tert-amylphenol, 2-(2H-benzotriazol-2-yl)-6-dodecyl-4-methylphenol, 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol, 2-(5-chloro-2H-benzotriazol-2-yl)-6-(1,1-dimethylethyl)-4-methylphenol, 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol, 2- (2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol, 3-(3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenylpropanoate), 2-(2H-benzotriazol-2-yl)-4,6-bis(1,1-dimethylethyl)phenol, 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol, 2-(5-chloro-2H-benzotriazol-2-yl)-4,6-bis(1,1-dimethylethyl)phenol; oxalic acid anilides, for example 2-ethyl-2'-ethoxyoxalyl Aniline or 4-methyl-4'-methoxyoxalanilide; salicylic acid esters, such as phenyl salicylate, 4-tert-butylphenyl salicylate, 4-tert-octylphenyl salicylate; cinnamate derivatives, such as methyl α-cyano-β-methyl-4-methoxycinnamate, butyl α-cyano-β-methyl-4-methoxycinnamate, ethyl α-cyano-β-phenylcinnamate, isooctyl α-cyano-β-phenylcinnamate; and malonate derivatives, such as dimethyl 4-methoxybenzylidenemalonate, diethyl 4-methoxybenzylidenemalonate, dimethyl 4-butoxybenzylidenemalonate, DL-α-tocopherol, tocopherol, cinnamic acid derivatives, cyanoacrylates and mixtures thereof. These preferred UV stabilizers can be used alone or in any combination with each other. Particularly preferred UV stabilizers are available under the trade names Tinuvin® 292 and Tinuvin® 1130 from BASF SE.
[0196] Hindered amines (often also referred to as HALS or HAS compounds; hindered amine (light) stabilizers) may act as suitable free radical scavengers. These are selected from 2,2,6,6-tetramethylpiperidine, 2,6-di-tert-butylpiperidine or derivatives thereof, such as bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and mixtures thereof. These are available, for example, as the Tinuvin® and Chimassorb® brands from BASF SE. Examples of N-alkylated free radical scavengers include bis(1,2,2,6,6-pentamethyl-4-piperidyl)[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butylmalonate (e.g. Tinuvin® 144 from BASF); a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate and methyl(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate (e.g. Tinuvin® 292 from BASF SE); or which are N-(o-alkylated), such as the reaction product of bis(2,2,6,6-tetramethyl-1-(octyloxy)-4-piperidyl)sebacate with 1,1-dimethylethyl hydroperoxide and octane (e.g. Tinuvin® 40 from BASF SE). 123), in particular HALS triazines, reaction products of 2-aminoethanol with cyclohexane and N-butyl-2,2,6,6-tetramethyl-4-piperidinamine-2,4,6-trichloro-1,3,5-triazine peroxide (e.g. Tinuvin® 152 from BASF SE).
[0197] Optionally, one or more UV stabilizers of component A mentioned by way of example are preferably used in an amount of 0.001% to 3.0% by weight, based on the total weight of compound A, more preferably 0.01% to 2% by weight.
[0198] Suitable antioxidants according to the invention are preferably sterically hindered phenols, which can preferably be selected from 2,6-di-tert-butyl-4-methylphenol (ionol), pentaerythritol tetrakis (3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate), octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, triethylene glycol bis (3-tert-butyl-4-hydroxy-5-methylphenyl) propionate, 2,2'-thiobis (4-methyl-6-tert-butylphenol) and bis [3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] 2,2'-thiodiethyl ester. If desired, these can be used both individually and in any combination with one another. The antioxidant is preferably used in an amount of 0.001% by weight to 3.0% by weight, more preferably 0.02% by weight to 2.0% by weight, based on the total weight of compound A, in each case calculated as the total amount of antioxidant used.
[0199] In order to improve substrate wetting, suitable leveling agents may optionally be included, for example organically modified siloxanes, such as polyether-modified siloxanes, polyacrylates and / or fluorosurfactants. These leveling agents are preferably used in an amount of 0.01% to 3% by weight, preferably 0.01% to 2% by weight, more preferably 0.05% to 1.5% by weight, based on the total weight of compound A, calculated as the total amount of leveling agents used. Preferred leveling agents are available from Altana under the trade names BYK 141 and BYK 311.
[0200] The polyisocyanates existing in the component B of two-component preparation of the present invention are for example selected from the group mentioned above for synthesizing polysiloxane prepolymers of the present invention.Preferred polyisocyanates comprise all obtainable higher molecular weight oligomers with biuret, uretdione, isocyanurate, iminooxadiazinedione, allophanate, carbamate and / or carbodiimide / uretonimine structural units by the reaction of the diisocyanates or triisocyanates selected from PDI, HDI, HDI, H12MDI, IPDI and mixture thereof.These polyisocyanates exist usually with 5 % by weight to 50 % by weight, preferably 5 % by weight to 25 % by weight, based on the whole preparation consisting of component A and component B in each case.
[0201] Furthermore, the inventive NCO-terminated polysiloxane prepolymers of the general formula (I) are present in component B of the two-component formulations of the invention. This is present, for example, in an amount of generally 50% to 95% by weight, preferably 75% to 95% by weight, based in each case on component B.
[0202] Preferably, no further additives are present in component B besides the compounds mentioned.
[0203] According to the invention, the two-component preparation of the invention may also be an aqueous preparation. In this embodiment, the at least one solvent mentioned above in component A and / or in component B of the two-component preparation of the invention is replaced by water.
[0204] Besides the NCO-terminated siloxane prepolymers according to the invention, the polyisocyanate component A) may optionally also contain polyisocyanates having aliphatically, cycloaliphatically, araliphatically and / or aromatically bonded isocyanate groups, which optionally also contain siloxane chains. These additional polyisocyanates are in particular the known lacquer isocyanates containing uretdione, isocyanurate, iminooxadiazinedione, carbamate, allophanate, biuret and / or oxadiazinetriaone structures, as described, for example, in Laas et al., J. Prakt. Chem. 336, 1994, 185-200, DE-A 1 670 666, DE-A 3 700 209, DE-A 3 900 053, EP-A 0 330 966, EP-A 0 336 205, EP-A 0 339 396 and EP-A 0 798 299. For this purpose, preference is given to using the compounds described above as unit R.
[0205] Particularly preferred additional polyisocyanates in the polyisocyanate component A) are those of the mentioned types which have exclusively aliphatically and / or cycloaliphatically bonded isocyanate groups, in particular those based on PDI, HDI and / or IPDI.
[0206] These additional polyisocyanates are optionally used in the coating composition of the invention in an amount of up to 70% by weight, preferably up to 60% by weight, more preferably up to 50% by weight, based on the total amount of the polyisocyanate component A) composed of at least one NCO-terminated siloxane prepolymer and the optional additional polyisocyanate.
[0207] The formulations according to the invention, in particular paint formulations, can comprise as binder component any aqueous polymer dispersions B) which preferably carry groups reactive toward isocyanate groups, particularly preferably hydroxyl and / or amino groups.
[0208] All polymer dispersions customary in aqueous 2K PUR coating technology come into consideration as aqueous polymer dispersions B). These are, for example, the customary aqueous or water-dispersible polyacrylate resins, polyester resins, polyurethane resins, polyurea resins, polycarbonate resins or polyether resins described, for example, in EP-A 0 358 979, EP-A 0 469 389, EP-A 0 496 205, EP-A 0 557 844, EP-A 0 583 728, WO 94 / 03511, WO 94 / 20559, WO 94 / 28043 or WO 95 / 02005. It is also possible to use any hybrid dispersions or any mixtures of different polymer dispersions.
[0209] Examples of suitable hydroxy-functional polyacrylate dispersions B1) are the known so-called secondary polyacrylate dispersions which can be prepared in a manner known per se by copolymerization of hydroxyl-containing ethylenically unsaturated monomers with hydroxyl-free olefin monomers in organic solvents, neutralization of the possibly incorporated ionic groups and dispersion in water.
[0210] Examples of suitable monomers for producing the secondary polyacrylate dispersions B1) are, for example, vinyl and vinylidene monomers, for example styrene, α-methylstyrene, o- and / or p-chlorostyrene, o-, m- or p-methylstyrene, p-tert-butylstyrene, acrylic acid, acrylonitrile, methacrylonitrile, acrylic and methacrylic esters of alcohols having up to 18 carbon atoms, such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, amyl acrylate, hexyl acrylate, 2-ethyl acrylate, 1-butyl acrylate, 2-butyl acrylate, 1-butyl ... 2-ethylhexyl methacrylate, 2-octyl methacrylate, 3,3,5-trimethylhexyl methacrylate, octadecyl acrylate, dodecyl acrylate, cyclopentyl acrylate, cyclohexyl acrylate, 4-tert-butylcyclohexyl acrylate, norbornyl acrylate, isobornyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, amyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, 2-octyl methacrylate, 3,3,5-trimethylhexyl methacrylate -trimethylhexyl ester, octadecyl methacrylate, dodecyl methacrylate, cyclopentyl methacrylate, cyclohexyl methacrylate, 4-tert-butylcyclohexyl methacrylate, norbornyl methacrylate or isobornyl methacrylate, diesters of fumaric acid, itaconic acid or maleic acid with alcohols having 4 to 8 carbon atoms, acrylamide, methacrylamide, vinyl esters of alkanemonocarboxylic acids having 2 to 5 carbon atoms, such as vinyl acetate or vinyl propionate, carboxyl-functional free-radical polymerizable monomers, such as acrylic acid, methacrylic acid, 1-carboxyethyl acrylate, crotonic acid, fumaric acid, Monoalkyl esters of maleic acid (anhydride), itaconic acid, or dibasic acids and / or anhydrides, such as monoalkyl maleates, hydroxyalkyl esters of acrylic acid and methacrylic acid having 2 to 6 carbon atoms in the hydroxyalkyl group, such as 2-hydroxyethyl, 2-hydroxypropyl, 3-hydroxypropyl, 3-hydroxybutyl, 4-hydroxybutyl, trimethylolpropane monoacrylate or monomethacrylate, pentaerythritol monoacrylate or monomethacrylate, hydroxy monomers containing alkylene oxide units, such as addition products of ethylene oxide, propylene oxide or butylene oxide with acrylic acid or methacrylic acid, and any mixtures of these monomers mentioned by way of example.
[0211] Ethylenically unsaturated monomers which are likewise suitable for producing the secondary polyacrylate dispersions B1) are vinyl monomers containing alkylene oxide units, such as condensation products of acrylic acid or methacrylic acid with oligomeric alkylene oxide monoalkyl ethers, and monomers having further functional groups, such as epoxy groups, alkoxysilyl groups, urea groups, urethane groups, amide groups or nitrile groups, and (meth)acrylate monomers and / or vinyl monomers having a functionality of 2 or more, such as hexanediol di(meth)acrylate, which can be co-used in small amounts, for example up to 3% by weight, based on the total amount of monomers.
[0212] Preferred ethylenically unsaturated monomers for producing the secondary polyacrylate dispersions B1) are methyl methacrylate, styrene, acrylic acid, methacrylic acid, butyl acrylate, butyl methacrylate, ethyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate or hydroxybutyl methacrylate.
[0213] In the secondary polyacrylate dispersion B1), the amount of carboxyl-functional monomers is 0.8 to 5% by weight, in particular 1.2 to 4% by weight, and the amount of hydroxyl-functional monomers is 1 to 45% by weight, preferably 6 to 30% by weight.
[0214] Secondary polyacrylate dispersions B1) suitable for the formulations according to the invention are prepared from ethylenically unsaturated monomers in the presence of polymerization initiators known per se. Examples of suitable initiators are peroxide compounds such as diacyl peroxides, alkyl peresters, dialkyl peroxides, peroxydicarbonates, inorganic peroxides or azo compounds.
[0215] In principle, any organic solvent used for producing the secondary polyacrylate dispersion B1) is suitable. These solvents can be used in any amount, but are preferably used in an amount of less than 20% by weight, based on the total amount of monomers. Preference is given to solvent mixtures of at least one hydrophobic solvent, such as solvent naphtha, toluene, xylene, crystal oil, and at least one hydrophilic solvent, such as butyl glycol, butyl diethylene glycol, diethylene glycol, propylene glycol monomethyl ether or dipropylene glycol monomethyl ether.
[0216] Suitable tertiary amines are generally used to neutralize possible ionic groups, in particular carboxyl groups, incorporated into the copolymers. Examples of suitable neutralizing agent amines are tertiary monoamines, such as trimethylamine, triethylamine, tripropylamine, tributylamine, ethyldiisopropylamine, dimethylcyclohexylamine, N-methylmorpholine, N-ethylmorpholine, N-methylpiperidine, N-ethylpiperidine, tertiary diamines, such as 1,3-bis(dimethylamino)propane, 1,4-bis(dimethylamino)butane or N,N´-dimethylpiperazine, or tertiary amines carrying isocyanate-reactive groups, for example alkanolamines, such as dimethylethanolamine, methyldiethanolamine, 2-aminomethyl-2-methylpropanol or, for example, triethanolamine.
[0217] The secondary polyacrylate dispersions B1) can be prepared by any process known from the prior art, for example in a feed process, a batch process or a cascade process.
[0218] After the copolymer solution has been dispersed in water, the solvent used can be removed proportionately or completely by distillation.
[0219] The pH value of the secondary polyacrylate dispersion B1) suitable for the coating composition of the invention is preferably from 5 to 11, more preferably from 6 to 10.
[0220] The solids content of the secondary polyacrylate dispersion B1) is preferably from 20% to 60% by weight, more preferably from 35% to 55% by weight. The average particle size is generally from 20 to 400 nm.
[0221] In the production of secondary polyacrylate dispersions, so-called reactive diluents can be used instead of or in addition to solvents. Suitable reactive diluents are, for example, polyethers with a functionality of 2 or 3 which are liquid at room temperature, low-viscosity polyesters, such as the reaction product of 1 mol of a dicarboxylic acid, such as dimer fatty acid or adipic acid, with 2 mol of a diol or triol or with 2 mol of glycidyl tert-carbonate. Other examples of suitable reactive diluents are the reaction products of ε-caprolactone with low molecular weight alcohols, and hydroxy-functional oils, such as castor oil.
[0222] Suitable aqueous polymer dispersions B) for the coating compositions of the invention are also, for example, so-called hydroxy-functional primary polyacrylate dispersions B2), which can be prepared in a customary manner by copolymerization of hydroxyl-containing ethylenically unsaturated monomers with hydroxyl-free olefin monomers directly in aqueous emulsion in the presence of suitable surface-active substances.
[0223] Suitable primary polyacrylate dispersions B2) and their production are described, for example, in RO Athey jr., Emulsion Polymer Technology, Dekker, New York, 1991.
[0224] Monomers suitable for producing such primary polyacrylate dispersions B2) include in principle the monomers already mentioned above in connection with the production of the secondary polyacrylate dispersions B1).
[0225] In the emulsion polymerization, the polymerization initiator is usually initially charged and / or added in parallel, optionally with the addition of the initial charge and / or the replenishment. Examples of suitable initiators are redox systems, peroxides, persulfates and / or azo compounds, such as dibenzoyl peroxide, diisopropylbenzene peroxide, cumene hydroperoxide, potassium peroxodisulfate, ammonium peroxodisulfate, azobisisobutyronitrile or di-tert-butyl peroxide.
[0226] Hybrid forms of polyacrylate dispersions known per se, such as polyester-polyacrylate dispersions B3), are likewise suitable as aqueous polymer dispersions B for the coating compositions of the invention. These dispersions contain both polyacrylate segments and polyester segments and are prepared, for example, by free-radical (co)polymerization of monomers of the type mentioned above in connection with the production of the secondary polyacrylate dispersions B1) in the presence of a polyester component, either as a bulk polymerization or preferably in an organic solution. Suitable polyester components are described below as possible synthesis components for the production of polyurethane dispersions B4).
[0227] Polyester-polyacrylate dispersions B3) suitable as aqueous polymer dispersions B) preferably contain a polyester proportion of 10% to 75% by weight, more preferably 20% to 60% by weight, based on the total solids content of the dispersion.
[0228] Polyurethane dispersions B4) are also suitable as aqueous polymer dispersions B) for the coating compositions of the invention. These dispersions are the customary self-emulsifying polyurethanes or polyurethane-polyureas known per se in aqueous form.
[0229] Self-emulsifying polyurethanes contain ionic and / or nonionic hydrophilic groups in the polymer chain, wherein these groups may be incorporated directly into the polymer chain or incorporated laterally or terminally.
[0230] Suitable polyurethane dispersions B4) are obtainable by methods known to the person skilled in the art by preparing the polyurethanes or polyurethane prepolymers in the melt or in an organic solution and then dispersing them in water, it being possible, if appropriate, to carry out a chain extension reaction in the organic solution in parallel with or after the dispersion step to increase the molecular weight.
[0231] To produce suitable polyurethane dispersions B4), various compounds reactive toward isocyanate groups, potentially ionic and / or nonionic, can be used to incorporate hydrophilic groups into the polyurethanes, for example by incorporating hydroxycarboxylic acids, such as dimethylolacetic acid, 2,2-dimethylolpropionic acid, 2,2-dimethylbutyric acid, 2,2-dimethylolvaleric acid, dihydroxysuccinic acid, hydroxypivalic acid or mixtures of these acids, aminocarboxylic acids, such as isophoronediamine or Michael adducts of ethylenediamine with acrylic acid, aminosulfonic acids, such as aminoethylethanesulfonic acid, hydroxy- or aminofunctional phosphonic acids and / or mono-, di- or trifunctional polyethylene oxide units having a molecular weight range of 350 to 2500 g / mol; mixtures of such compounds can also be used.
[0232] Particularly suitable hydrophilic units are dimethylolpropionic acid, dimethylolbutanoic acid, mono- or dihydroxyfunctional polyethylene oxide units in the molecular weight range given above, and hydroxy-functional or amino-functional sulfonic acids and / or sulfonates.
[0233] The tertiary amines and / or tertiary amino alcohols described above as suitable neutralizing amines for the secondary polyacrylate dispersions B1) preferably serve as neutralizers for these hydrophilic units.
[0234] To prepare suitable polyurethane dispersions B4), use is made of any aliphatic, cycloaliphatic, araliphatic and / or aromatic diisocyanates and / or polyisocyanates, such as have been mentioned above as starting compounds.
[0235] Preference is given to using isophorone diisocyanate, 4,4′-dicyclohexylmethane diisocyanate and / or hexamethylene diisocyanate.
[0236] Further synthesis components for producing suitable polyurethane dispersions B4) are polyester polyols, polyesteramide polyols, polyacetal polyols, polyether polyols, polysiloxane polyols and / or polycarbonate polyols in the molecular weight range from 500 to 18 000 g / mol and having a functionality of 1 to 5, preferably 2 to 2.5.
[0237] Suitable polyester polyols for producing the polyurethane dispersions B4) are, for example, those having an average functionality of 1.5 to 5, such as can be prepared in a known manner by reacting aliphatic, cycloaliphatic or aromatic dicarboxylic acids and / or polycarboxylic acids and / or their anhydrides, such as succinic acid, glutaric acid, adipic acid, sebacic acid, pimelic acid, suberic acid, azelaic acid, nonanedicarboxylic acid, decanedicarboxylic acid, phthalic acid, isophthalic acid, hexahydrophthalic acid, trimellitic acid, phthalic anhydride, tetrahydrophthalic acid, maleic acid, maleic anhydride, fumaric acid, dimerized and trimerized fatty acids, dimethyl terephthalate and diethylene glycol terephthalate with polyols, such as ethane-1,2-diol, propane-1,2-diol and propane-1,3-diol. It is prepared by reacting 1,2-diol, isomeric butanediol, pentanediol, hexanediol, heptanediol and octanediol, decane-1,10-diol, dodecane-1,12-diol, cyclohexane-1,2-diol and -1,4-diol, cyclohexane-1,4-dimethanol, 4,4'-(1-methylethylidene)bicyclohexanol, diethylene glycol, triethylene glycol, tetraethylene glycol, propane-1,2-diol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, propane-1,2,3-triol, 1,1,1-trimethylolethane, hexane-1,2,6-triol, 1,1,1-trimethylolpropane, 2,2-bis(hydroxymethyl)propane-1,3-diol and / or 1,3,5-tris(2-hydroxyethyl)isocyanurate.
[0238] Suitable polyester polyols are also those which can be prepared, for example, in a conventional manner from lactones and individual polyols, such as those listed above, for example, as starter molecules under ring opening. Examples of lactones suitable for preparing these polyester polyols are β-propiolactone, γ-butyrolactone, γ- and δ-valerolactone, ε-caprolactone, 3,5,5- and 3,3,5-trimethylcaprolactone or any mixtures of such lactones.
[0239] Suitable polycarbonate polyols for producing polyurethane dispersion B4) are in particular diols, such as those mentioned above in the list of polyols, and the reaction products known per se of diaryl carbonates, such as diphenyl carbonate, dimethyl carbonate or phosgene. Other suitable polycarbonate polyols are those containing not only carbonate structures but also ester groups. These are in particular polyester carbonate diols known per se, which can be obtained, for example, according to the teaching of DE-B 1 770 245, by the reaction of diols with lactones, in particular, for example, ε-caprolactone and the subsequent reaction of the resulting polyester diols with diphenyl carbonate or dimethyl carbonate. Polycarbonate polyols containing not only carbonate structures but also ether groups are equally suitable. These are in particular polyether carbonate polyols known per se, which can be obtained, for example, by the catalytic reaction of alkylene oxide and carbon dioxide in the presence of H-functional initiator molecules according to the method of EP-A 2046861.
[0240] Suitable polyether polyols for producing polyurethane dispersions B4) are those obtainable, for example, by alkoxylation of suitable initiator molecules in a manner known per se. In order to prepare these polyether polyols, any polyols can be used as initiator molecules, for example those of the type described above for the preparation of polyester polyols in a molecular weight range of 62 to 400. Suitable alkylene oxides for alkoxylation are in particular ethylene oxide and propylene oxide, which can be used for alkoxylation in any order or in a mixture. Other equally suitable polyether polyols are polytetramethylene ether glycols prepared, for example, by polymerization of tetrahydrofuran according to Angew. Chem. 72, 927 (1960) and having a number-average molecular weight of 400 g / mol to 4000 g / mol.
[0241] To prepare suitable polyurethane dispersions B4), it is further possible to use block copolymers based on the polyols mentioned, for example polyether-polyester copolymers, polycarbonate-polyester copolymers or polycarbonate / polyether copolymers.
[0242] Preferred polyols for producing suitable polyurethane dispersions B4) are polyester polyols, polycarbonate polyols and / or C3 and / or C4 polyether polyols.
[0243] In the production of suitable polyurethane dispersions B4), it is also possible to use low molecular weight alcohols having a functionality of 2 to 4. These are, in particular, compounds having a molecular weight of 500 g / mol, for example simple polyols of the type mentioned above as synthesis components for the polyester polyols, or amino alcohols such as diethanolamine, ethanolamine, diisopropanolamine, propanolamine, which may optionally also be present in ethoxylated and / or propoxylated form, and any desired mixtures of these alcohols.
[0244] In the production of suitable polyurethane dispersions B4), known compounds are generally used as chain extenders. These chain extenders are, in particular, diamines, polyamines and / or amino alcohols, for example diethanolamine, 1,2-diaminopropane, 1,4-diaminobutane, 2,5-diamino-2,5-dimethylhexane, 1,5-diamino-2-methylpentane, 1,6-diaminohexane, 2,2,4- and / or 2,4,4-trimethyl-1,6-diaminohexane, 1,11-diaminoundecane, 1,12-diaminododecane, triaminononane, ethylenediamine, isophoronediamine, diethylenetriamine, hydrazine, adipic acid dihydrazide, hydroxyethylethylenediamine, bishydroxyethylethylenediamine, aminopropanol, aminoalkoxysilanes and any desired mixtures of these compounds.
[0245] Suitable polyurethane dispersions B4) can be produced using suitable solvents. Examples of suitable solvents are acetone, methyl ethyl ketone, N-methylpyrrolidone and / or N-ethylpyrrolidone.
[0246] Suitable polyurethane dispersions B4) can be produced in order to accelerate the reaction or to achieve specific effects, also using catalysts customary in polyurethane chemistry, such as dibutyltin dilaurate, dibutyltin oxide, tin dioctoate, tin chloride and / or tertiary amines.
[0247] In the production of polyurethane dispersions in the melt or in organic solution, diisocyanates and / or polyisocyanates are generally reacted with polyols and hydrophilic units of the type mentioned to form isocyanate-functional prepolymers, which are subsequently further reacted in the melt, in organic solution or in aqueous dispersion with chain extenders of the type indicated to form high molecular weight polyurethanes which are dispersible and / or dispersed in water.
[0248] Any solvent used can be distilled off completely or partly after dispersion.
[0249] Polyurethane dispersions B4) suitable for the coating composition of the invention preferably have a solids content of 25% to 60% by weight, a pH value of 5.5 to 11 and / or an average particle size of 20 to 500 nm.
[0250] Further suitable aqueous polymer dispersions B) for the formulations according to the invention are polyester dispersions and polyester solutions B5), such as are obtained by dispersing suitable water-dilutable polyester polyols in water.
[0251] Examples of suitable water-dilutable polyester polyols are dispersion resins known, for example, from paint technology, which have very good pigment-wetting and / or pigment-affinity qualities and an acid number in the range of 25 to 75 mg KOH / g, a hydroxyl content of 2.5 to 10% by weight, a molecular weight in the range of 750 to 5000 g / mol and / or fatty acid components in an amount of 15 to 50% by weight.
[0252] Polyester dispersions and solutions B5) suitable for the preparations according to the invention are obtained, for example, by reacting polyester polyols, for example the polyester polyols described above as synthesis components for producing polyurethane dispersions B4), with anhydrides, such as phthalic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, maleic anhydride, trimellitic anhydride or pyromellitic anhydride, wherein the reaction is carried out so that the anhydride reacts with a portion of the hydroxyl groups, with concomitant ring opening of the anhydride and incorporation into the polyester. In this way, hydroxyl-functional and simultaneously carboxyl-functional polyesters are obtained which, after complete or proportional neutralization of the carboxyl groups, can be dissolved or dispersed in water. Aqueous polyester dispersions or solutions B5) are obtained with an average particle size of 10 to 200, preferably 25 to 100 nm.
[0253] In general, the aqueous polymer dispersions B) used in the coating compositions of the invention are hydroxy-functional and / or amino-functional dispersions of the types mentioned. However, it is also possible to use nonfunctional polymer dispersions B) as binder component in the coating compositions of the invention.
[0254] The aqueous polymer dispersion B) used in the coating composition of the invention preferably comprises at least one aqueous secondary polyacrylate dispersion B1), a polyester-polyacrylate dispersion B3) based on polyester polyols, polycarbonate polyols and / or C3 or C4 polyether polyols.
[0255] In the coating compositions of the invention, preference is given to using hydroxyl-functional aqueous polymer dispersions B) having a hydroxyl content of 0.5 to 7.0% by weight, preferably 0.5 to 6.0% by weight, more preferably 1.0 to 5.0% by weight, based on resin solids, an acid number of less than 50 mg KOH / g, preferably less than 40 mg KOH / g, more preferably less than 30 mg KOH / g and / or a number average molecular weight Mn, as determined by gel permeation chromatography, of 500 to 30 000 g / mol, preferably 1 000 to 15 000 g / mol, more preferably 1 500 to 10 000 g / mol.
[0256] In embodiments of the invention in which an aqueous two-component formulation is present, at least one emulsifier may additionally be present in component B. Suitable external and internal emulsifiers are known per se to the person skilled in the art and are described, for example, in "Polyurethanes - Coatings, Adhesives and Sealants", 2019, Meier-Westhues, Danielmeier, Kruppa, Squiller, Vincentz Network GmbH, pages 48-51. Particularly suitable emulsifiers contain functional groups and / or cationic groups which can be converted into cations by neutralizing agents and / or quaternizing agents, or functional groups and / or anionic groups which can be converted into anions by neutralizing agents and / or nonionic hydrophilic groups.
[0257] The present invention further relates to the use of the NCO-terminated polysiloxane prepolymers of the invention as curing agents in paint formulations. What has been said about the two-component formulations of the invention applies here correspondingly with regard to the amounts and other components present. Example
[0258] Unless otherwise stated, all experiments were conducted at 23°C and 50% relative humidity.
[0259] The NCO content is determined titrimetrically in accordance with DIN EN ISO 11909:2007-05.
[0260] The OH value is determined by titration according to DIN 53240-2:2007-11.
[0261] The acid number is determined according to DIN EN ISO 2114:2002-06.
[0262] The indicated OH contents are calculated from the analytically determined OH numbers. The indicated values are in each case based on the total weight of the respective composition, including any solvents used concomitantly.
[0263] The residual monomer content is measured by gas chromatography using an internal standard in accordance with DIN EN ISO 10283:2007-11.
[0264] The solids content was determined according to DIN EN ISO 3251:2008-06.
[0265] The drying times (T1, T3 and T4) were determined according to DIN EN ISO 9117-5:2010-07 (Drying tests – Part 5: Modified Bandow-Wolff method).
[0266] The viscosity is determined in accordance with DIN EN ISO 3219 / A:1994-10 at 23° C. Unless stated otherwise, this is the dynamic viscosity.
[0267] The number-average molecular weight Mn was determined by gel permeation chromatography (GPC) in tetrahydrofuran at 23°C. The operation was carried out according to DIN 55672-1:2016-03: "Gel permeation chromatography, part 1 – Tetrahydrofuran as eluent" (SECurity GPC System from PSS Polymer Service, flow rate 0.6 ml / min; columns: 2 × PSS SDV (100A), 2 × PSS SDV (50A), 8 × 300 mm, 5 µm; RID detector (RI-Agilent 1260). Polystyrene samples of known molar mass were used for calibration. The number-average molecular weight was calculated by means of the software.
[0268] The 20° gloss of the resulting coatings was measured in reflection according to DIN EN ISO 2813:2015-02.
[0269] Condensation water test according to DIN EN ISO 6270-2 CH:2018-04.
[0270] The contact angle was determined in accordance with DIN 55660-2:2011-12. For each value, the contact angle with water was checked at 10 points on the plate and the average of these measurements is given.
[0271] The wet scratch resistance of the coatings was tested using a laboratory washing apparatus according to DIN EN ISO 20566:2013-06. The gloss loss in gloss units (GU) after scratching (10 cycles) is given. The lower the gloss loss in GU, the more resistant the coating is to wet scratching.
[0272] The dry scratch resistance is determined using a linear reciprocating device (friction decolorizer) according to DIN 55654:2015-08. Here, a weight (950 g) whose flat bottom is stretched on polishing paper (company 3M, grade: 9 MIC) is placed on the coating without scratching the coating and then mechanically guided in a path on the coating. 10 or 20 reciprocating strokes are implemented each time. After exposure to the scratching medium, the test area is cleaned with a soft cloth and the gloss is then measured at three different positions transverse to the scratching direction. The lower the gloss loss GU calculated from the average value of this measurement, the more scratch-resistant the coating is.
[0273] The König pendulum damping was determined on glass panels in accordance with DIN EN ISO 1522:2007-04.
[0274] The coatings were applied by spraying. The dry film thickness for all films was 35 to 40 µm.
[0275] The solvent and water resistance is determined in accordance with DIN EN ISO 4628-1:2016-07. The solvent resistance test is carried out using the solvents xylene (hereinafter also abbreviated as "Xy"), methoxypropyl acetate (MPA), ethyl acetate (EA) and acetone (Ac). The contact time is in each case 5 minutes. For the measurement of water resistance, the contact time is in each case 24 hours. The inspection is carried out in accordance with the specified standards. The test surface is evaluated visually and by scratching, the following classification being used: 0 = no changes can be detected; 1 = swollen ring, hard surface, only visible changes; 2 = swollen ring, slight softening; 3 = marked softening (possible slight blistering); 4 = marked softening (possible severe blistering), scratching can penetrate to the substrate; 5 = complete destruction of the coating without external stress.
[0276] The reflow behavior (reflow) describes the recovery of a scratched coating surface after the effect of temperature, based on the gloss value. The coating composition is scratched by wet or dry scratching. The residual gloss is determined after the scratching cycle. The coating is placed in an oven at 60° C. for 2 hours and the gloss is then determined according to the above procedure. The reflow is indicated as a percentage, i.e. the ratio of the residual gloss to the reflow value.
[0277] The contact angle is determined according to DIN 55660-2:2011-12.
[0278] The following reagents were used in the examples and comparative examples:
[0279] Diisocyanate:
[0280] Hexamethylene 1,6-diisocyanate (HDI) and isophorone diisocyanate (PDI) were obtained from Covestro and used without purification.
[0281] Polyols:
[0282] Polyol 1 is based on a polyether diol (Dianol® 320 HP, solid) which contains secondary OH groups and has a hydroxyl number of 325 mgKOH / g. The reaction with propylene oxide gives Polyol 1 with a molecular weight of 550 g / mol.
[0283] Polyol 2 is a polyester polyol formed from hexanediol, butanediol, adipic acid and propylene glycol, having a functionality of 2, a molecular weight of about 400 g / mol, an OH content of about 8% by weight and a viscosity of 80 mPa∙s.
[0284] Polyol 3 is a polyacrylate polyol formed from methyl methacrylate, acrylic acid, styrene and hydroxyethyl methacrylate, having an OH content of 2.8% by weight, based on solids, dissolved in butyl acetate at a solids content of 75% by weight. The viscosity is 5000 mPa∙s.
[0285] Polyol 4 is an α,ω-hydroxypropyl terminated polydimethylsiloxane (Baysilone OF OH 702 (4 wt %)) having an OH content of 4 wt % and a molecular weight of 600 to 800 g / mol. The clear liquid has a molecular weight of 37 mm 2 ∙s -1 kinematic viscosity.
[0286] Polyol 5 is an aliphatic hydroxyl functional polycarbonate polyester polyurethane dispersion. It was obtained from Covestro and has the following characterization data:
[0287] Viscosity: 300-1500 mPa∙s
[0288] Non-volatile matter ratio: 50.0-54.0%
[0289] OH content: about 1%.
[0290] Polyol 6 is a polyester polyacrylate dispersion. It was obtained from Covestro and has the following characteristic data:
[0291] Viscosity: 700-7200 mPa∙s
[0292] Non-volatile matter ratio: 41-43%
[0293] OH content: 3.8%.
[0294] Polyol 7 is a polyacrylate polyol. It is available from Allnex and sold under the trade name Setalux DA 870 BA and has the following characteristic data:
[0295] Viscosity: 3500 mPa∙s
[0296] Non-volatile matter ratio: 70%
[0297] OH content: 4.2% (based on solids).
[0298] Amine 1 is a secondary amine prepared from 4,4'-methylenebis(cyclohexylamine) and diethyl maleate and has the following characteristic data:
[0299] Amine value: 200 mg KOH / g
[0300] Viscosity (25℃): 900-2000 mPa∙s
[0301] Color value (Hason): ≤ 250.
[0302] TMP stands for 1,1,1-trimethylolpropane, a trifunctional polyol with a molecular weight of 134 g / mol.
[0303] Polyisocyanate:
[0304] Polyisocyanate 1 is a trimer of hexamethylene 1,6-diisocyanate having a functionality of 2.8 to 3.6, an NCO content of 23% by weight, an equivalent weight of 183 g / mol and a viscosity of 1200 mPa∙s.
[0305] Polyisocyanate 2 is a trimer of hexamethylene 1,6-diisocyanate having a functionality of 2.8 to 3.6, an NCO content of 21.8% by weight, a viscosity of 3000 mPa∙s and an equivalent weight of 193 g / mol.
[0306] Polyisocyanate 3 is an allophanate based on hexamethylene 1,6-diisocyanate and propanol / butanol with a functionality of 2.0 to 2.8, an equivalent weight of 215 g / mol and a viscosity of 500 mPa∙s.
[0307] Polyisocyanate 4 is a trimer of isophorone diisocyanate having a functionality of 2.8 to 3.6, an NCO content of 11.9 wt %, a solids content of 70%, solvent naphtha 100 (30 wt %), an equivalent weight of 360 g / mol, and a viscosity of 1600 mPa∙s.
[0308] Polyisocyanate 5 is an ionically hydrophilized polyisocyanate based on HDI trimer and a sulfonate-based hydrophilizing agent, having a functionality of ≤ 2.8, an NCO content of 20.3% by weight and a viscosity of 3500 mPa∙s.
[0309] Additives and Catalysts:
[0310] Tinuvin 292, a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate (509 g / mol) and methyl 1,2,2,6,6-pentamethyl-4-piperidinyl sebacate (370 g / mol), is a light stabilizer based on hindered amines. The viscosity is 400 mPa∙s. The product was obtained from BASF and used without further purification.
[0311] Tinuvin 1130, a mixture of β-[3-(2H-benzotriazol-2-yl)-4-hydroxy-5-tert-butylphenyl]propionic acid poly(ethylene glycol) 300 ester (637 g / mol) and bis{b-[3-(2H-benzotriazol-2-yl)-4-hydroxy-5-tert-butylphenyl]propionic acid poly(ethylene glycol) 300 ester (975 g / mol), is a UV absorber. The viscosity is 7400 mPa∙s. The product was obtained from BASF and used without further purification.
[0312] BYK® 141 (solid, as supplied: 96.8%), BYK® 331 (solid, as supplied: 100%) and BYK® 348 (solid, as supplied: 100%) are silicone-containing leveling agents formed from covalently linked siloxanes and polyethers. The products are available from BYK.
[0313] Addocat® 201 is a standard catalyst based on dibutyltin dilaurate (DBTL) and is used in a concentration of 0.03% by weight based on solid binder. The catalyst is available from Lanxess.
[0314] Lucrafoam® DNE 01 is a mineral oil based defoamer for use in all pH ranges. This defoamer is available from Levaco Chemicals.
[0315] Tego®-Wet KL 245 is a silicone-based wetting agent with an active content of 100%. It is available from Evonik Industries.
[0316] Aquacer 513 is a VOC-free HDPE-based wax emulsion for improved surface protection in aqueous media. The wax emulsion is available from BYK.
[0317] Decosoft Transparent® 7 D is a highly crosslinked aliphatic polyurethane particle (100%) which imparts a soft feel and matte finish to the coating. The product is available from Microchem.
[0318] Matting Agent Acematt® 3300 ACEMATT 3300 is fumed silica that has been post-treated with a special polymer. This matting agent is characterized by a very high matting efficiency and high transparency.
[0319] Solvents such as butyl acetate (BA) and methoxypropyl acetate (MPA) were obtained from Azelis.
[0320] Example 1 (the present invention)
[0321] 441 g of HDI were initially charged and heated to 105° C. After addition of 280 g of Baysilone OFOH 702, the reaction mixture was stirred at 100° C. for 3 hours under a nitrogen atmosphere. After stirring for a further 2 hours at 110° C., the unreacted HDI monomer was separated off in a thin-film evaporator at a temperature of 150° C. and a pressure of 0.1 mbar. An almost colorless, clear NCO-terminated prepolymer with the following characteristic data was obtained.
[0322] NCO content: 6.65 wt%
[0323] Solid content: 100%
[0324] Viscosity 320 mPa∙s
[0325] HDI: < 0.3 wt%.
[0326] Example 2 (the present invention)
[0327] 583 g of IPDI were initially charged and heated to 105° C. After addition of 280 g of Baysilone OFOH 102, the reaction mixture was stirred at 100° C. for 3 hours under a nitrogen atmosphere. After stirring for a further 2 hours at 110° C., the unreacted HDI monomer was separated off in a thin-film evaporator at a temperature of 150° C. and a pressure of 0.1 mbar. An almost colorless, clear NCO-terminated prepolymer (425 g) was obtained with the following characteristic data.
[0328] NCO content: 7.35 wt%
[0329] Solid content: 100%
[0330] Viscosity 3500
[0331] IPDI: < 0.3 wt%.
[0332] Example 3 (Comparative Example, One-pot Reaction)
[0333] 756 g of Desmodur H were initially charged and heated to 105° C. A mixture of 8 g of TMP, 33 g of polyol 1 and 120 g of polyol 4 was then added, and the reaction mixture was stirred at 110° C. for 2 hours under a nitrogen atmosphere. After stirring at 110° C. for a further 2 hours, unreacted monomeric HDI was separated off in a thin-film evaporator at a temperature of 130° C. and a pressure of 0.1 mbar. An almost colorless, clear NCO-terminated prepolymer having the following characteristic data was obtained.
[0334] NCO content: 9.5%
[0335] Solid content: 100%
[0336] Viscosity 960 mPa∙s.
[0337] Example 4 (the present invention)
[0338] 30.5 g of the product from Example 1 were reacted with 21.3 g of polyol 2 (50% by weight solution in MPA) in the presence of Addocat 201 (0.03% by weight). The reaction was carried out at 60° C. under a nitrogen atmosphere. After the NCO content was determined to be less than 0.1% by weight, 55.5 g of Desmodur N3600 were added and the reaction mixture was adjusted to a solids content of 50% by weight with MPA. The reaction was carried out at 60° C. until an NCO content of 4.9% by weight was reached. An almost colorless, clear NCO-terminated prepolymer with the following characteristic data was obtained.
[0339] NCO content: 4.9%
[0340] Solid content: 50%
[0341] Viscosity 190 mPa∙s.
[0342] Example 5 (the present invention)
[0343] 15.25 g of the product from Example 1 were reacted with 3.35 g of 1,1,1-trimethylolpropane (50% by weight solution in MPA) in the presence of Addocat 201 (0.03% by weight). After a determined NCO content of less than 0.1% by weight, 82.5 g of polyisocyanate 3 were added and the reaction mixture was adjusted to a solids content of 50% by weight with MPA. The reaction was carried out at 60° C. with stirring until an NCO content of 6.8% by weight was reached. An almost colorless, clear NCO-terminated prepolymer having the following characteristic data was obtained.
[0344] NCO content: 6.75 wt%
[0345] Solid content: 50% by weight
[0346] Viscosity 232 mPa∙s.
[0347] Example 6 (the present invention)
[0348] 15.3 g of the product from Example 1 were reacted with 3.35 g of 1,1,1-trimethylolpropane (50% by weight solution in MPA) in the presence of Addocat 201 (0.03% by weight). After the NCO content was determined to be less than 0.1% by weight, 92.5 g of polyisocyanate 1 were added and the reaction mixture was adjusted to a solids content of 50% by weight with MPA. The reaction was carried out at 60° C. with stirring until an NCO content of 8.5% by weight was reached. An almost colorless, clear NCO-terminated prepolymer with the following characteristic data was obtained:
[0349] NCO content: 8.5 wt%
[0350] Solid content: 50% by weight
[0351] Viscosity 110 mPa∙s.
[0352] Example 7 (Present invention)
[0353] 5.28 g of the product from Example 2 were reacted with 1.08 g of 1,1,1-trimethylolpropane (50% by weight solution in MPA) in the presence of Addocat 201 (0.03% by weight). After the NCO content was determined to be less than 0.1% by weight, 29.3 g of polyisocyanate 1 were added. The reaction mixture was adjusted to a solids content of 50% by weight with MPA. The reaction was carried out at 60° C. with stirring until an NCO content of 8.48% by weight was reached. An almost colorless, clear NCO-terminated prepolymer with the following characteristic data was obtained:
[0354] NCO content: 8.48 wt%
[0355] Solid content: 50% by weight
[0356] Viscosity 175 mPa∙s.
[0357] Example 8 (the present invention)
[0358] 5.28 g of the product from Example 2 were reacted with 1.08 g of 1,1,1-trimethylolpropane (50% by weight solution in MPA) in the presence of Addocat 201 (0.03% by weight). After the NCO content was determined to be less than 0.1% by weight, 32.8 g of polyisocyanate 5 were added and the reaction mixture was adjusted to a solids content of 50% by weight with MPA. The reaction was carried out at 60° C. with stirring until an NCO content of 6.75% by weight was reached. An almost colorless, clear NCO-terminated prepolymer with the following characteristic data was obtained:
[0359] NCO content: 6.75 wt%
[0360] Solid content: 50% by weight
[0361] Viscosity 145 mPa∙s.
[0362] Example 9 (Present invention)
[0363] 11.02 g of the product from Example 2 were reacted with 2.24 g of 1,1,1-trimethylolpropane (50% by weight solution in MPA) in the presence of Addocat 201 (0.03% by weight). After the NCO content was determined to be less than 0.1% by weight, 120 g of polyisocyanate 4 were added and the reaction mixture was adjusted to a solids content of 50% by weight with MPA. The reaction was carried out at 60° C. with stirring until an NCO content of 6.48% by weight was reached. An almost colorless, clear NCO-terminated prepolymer with the following characteristic data was obtained:
[0364] NCO content: 6.48 wt%
[0365] Solid content: 50% by weight
[0366] Viscosity 180 mPa∙s.
[0367] Example 10 (Present invention)
[0368] 11.02 g of the product from Example 2 were reacted with 108 g of polyol 2 (50% by weight solution in MPA) in the presence of Addocat 201 (0.03% by weight). After the NCO content was determined to be less than 0.1% by weight, 120 g of polyisocyanate 4 were added and the reaction mixture was adjusted to a solids content of 50% by weight with MPA. The reaction was carried out at 60° C. with stirring until an NCO content of 5.71% by weight was reached. An almost colorless, clear NCO-terminated prepolymer with the following characteristic data was obtained:
[0369] NCO content: 5.71 wt%
[0370] Solid content: 50% by weight
[0371] Viscosity 30 mPa∙s.
[0372] Example 11 (Present invention)
[0373] 11.02 g of the product from Example 2 were reacted with 40.5 g of polyol 3 (50% by weight solution in MPA) in the presence of Addocat 201 (0.03% by weight). After the NCO content was determined to be less than 0.1% by weight, 120 g of polyisocyanate 4 were added and the reaction mixture was adjusted to a solids content of 50% by weight with MPA. The reaction was carried out at 60° C. with stirring until an NCO content of 5.96% was reached. An almost colorless, clear NCO-terminated prepolymer with the following characteristic data was obtained:
[0374] NCO content: 5.96 wt%
[0375] Solid content: 50% by weight
[0376] Viscosity 160 mPa∙s.
[0377] Example 12 (Present invention)
[0378] 6.76 g of the product from Example 1 were reacted with 1.49 g of 1,1,1-trimethylolpropane (50% by weight solution in MPA) in the presence of Addocat 201 (0.03% by weight). After the NCO content was determined to be less than 0.1% by weight, 44.9 g of polyisocyanate 5 were added and the reaction mixture was adjusted to a solids content of 50% by weight with MPA. The reaction was carried out at 60° C. with stirring until an NCO content of 7.82% by weight was reached. An almost colorless, clear NCO-terminated prepolymer with the following characteristic data was obtained:
[0379] NCO content: 7.82 wt%
[0380] Solid content: 50.0% by weight
[0381] Viscosity 115 mPa∙s.
[0382] Example 13 (Present invention)
[0383] 6.76 g of the product from Example 1 were reacted with 27.0 g of polyol 3 BA (50% by weight solution in MPA) in the presence of Addocat 201 (0.03% by weight). After the NCO content was determined to be less than 0.1% by weight, 44.9 g of polyisocyanate 5 were added and the reaction mixture was adjusted to a solids content of 50% by weight with MPA. The reaction was carried out at 60° C. with stirring until an NCO content of 5.84% by weight was reached. An almost colorless, clear NCO-terminated prepolymer with the following characteristic data was obtained:
[0384] NCO content: 5.84 wt%
[0385] Solid content: 50% by weight
[0386] Viscosity 100 mPa∙s.
[0387] Example 14 (Present invention)
[0388] 6.76 g of the product from Example 1 were reacted with 7.17 g of polyol 2 (50% by weight in MPA) in the presence of Addocat 201. After a measured NCO content of less than 0.1% by weight, 44.9 g of polyisocyanate 5 (0.03% by weight) were added and the reaction mixture was adjusted to a solids content of 50% by weight with MPA. The reaction was carried out at 60° C. with stirring until an NCO content of 7.14% by weight was reached. An almost colorless, clear NCO-terminated prepolymer with the following characteristic data was obtained:
[0389] NCO content: 7.14 wt%
[0390] Solid content: 50% by weight
[0391] Viscosity 70 mPa∙s.
[0392] Example 15 (Present invention)
[0393] 6.09 g of the product from Example 1 were reacted with 24.3 g of polyisocyanate 3 (50% by weight in MPA) in the presence of Addocat 201 (0.03% by weight). After the measured NCO content was less than 0.1% by weight, 38.6 g of polyisocyanate 2 were added and the reaction mixture was adjusted to a solid content of 50% by weight with MPA. The reaction was carried out at 60° C. with stirring until an NCO content of 6.75% by weight was reached. An almost colorless, clear NCO-terminated prepolymer with the following characteristic data was obtained:
[0394] NCO content: 6.75 wt%
[0395] Solid content: 50% by weight
[0396] Viscosity 110 mPa∙s.
[0397] Example 16 (Present invention)
[0398] 6.09 g of the product from Example 1 were reacted with 1.34 g of 1,1,1-trimethylolpropane (50% by weight in MPA) in the presence of Addocat 201 (0.03% by weight). After the NCO content was determined to be less than 0.1% by weight, 38.6 g of polyisocyanate 2 were added and the reaction mixture was adjusted to a solids content of 50% by weight with MPA. The reaction was carried out at 60° C. with stirring until an NCO content of 6.75% by weight was reached. An almost colorless, clear NCO-terminated prepolymer with the following characteristic data was obtained:
[0399] NCO content: 6.75 wt%
[0400] Solid content: 50% by weight
[0401] Viscosity 200 mPa∙s.
[0402] Example 17 (Present invention)
[0403] 6.09 g of the product from Example 1 were reacted with 6.45 g of polyol 2 (50% by weight in MPA) in the presence of Addocat 201 (0.03% by weight). After a measured NCO content of less than 0.1% by weight, 38.6 g of polyisocyanate 2 were added and the reaction mixture was adjusted to a solids content of 50% by weight with MPA. The reaction was carried out at 60° C. with stirring until an NCO content of 6.75% by weight was reached. An almost colorless, clear NCO-terminated prepolymer with the following characteristic data was obtained:
[0404] NCO content: 6.75 wt%
[0405] Solid content: 50% by weight
[0406] Viscosity 90 mPa∙s.
[0407] Example 17 (Present invention)
[0408] 12.63 g of the product from Example 1 were stirred with 16.56 g of amine 1 at room temperature for 8 hours. 77.20 g of polyisocyanate 2 were then added and stirred at room temperature likewise for 8 hours. An almost colorless, clear NCO-terminated prepolymer having the following characteristic data was obtained:
[0409] NCO content: 7.01 wt%
[0410] Solid content: 50% by weight
[0411] Viscosity 100 mPa∙s.
[0412] Application Examples:
[0413] Table 1 shows the various paint systems. The components of the paint formulations were mixed with one another and applied to the glass and the color paint by means of a spraying method (multilayer construction). The painted specimens were dried at 60° C. for 30 minutes.
[0414] Table 1
[0415] Table 1: Formulations were sprayed and baked at 60°C for 30 minutes. All analytical values were determined after 7 days.
[0416] Paint 1 Paint 2 Paint 3 Paint 4 Paint 5 Paint 6 Paint 7 (Vgl.) Paint 8 (Vgl.) Paint 9 (Vgl.) product Solid content[%] Weight(g) Weight(g) Weight(g) Weight(g) Weighing (g) Weight(g) Weight(g) Weight(g) Weight(g) Polyol 7 70 48.33 48.33 47.96 47.96 48.37 48.37 49.21 49.21 47.82 Byk 141 96.8 0.25 - 0.25 - 0.25 - 0.25 - 0.25 Byk 331 10 1.50 - 1.50 - 1.50 - 1.50 - 1.50 Tinuvin 292 50 1.00 1.00 1.00 1.00 1.00 1.00 1.00 1.00 1.00 Tinuvin 1130 50 2.00 2.00 2.00 2.00 2.00 2.00 2.00 2.00 2.00 Addocat 201 1 1.50 1.50 1.50 1.50 1.50 1.50 1.50 1.50 1.5 Butyl acetate 0 10.60 10.60 10.09 10.09 9.95 9.95 11.08 11.08 11.23 MPA 0 6.44 6.44 6.15 6.15 6.06 6.06 6.74 6.74 6.86 Xylene 0 10.60 10.60 10.09 10.09 9.95 9.95 11.08 11.08 11.23 Example 3 50 - - - - - - - - 2.39 Example 4 50 3.07 3.07 - - - - - - Example 5 50 - - 5.91 5.91 - - - - Example 6 50 - - - - 6.39 6.39 - - Polyisocyanate 1 100 14.71 14.71 13.55 13.55 13.03 13.03 15.63 15.63 14.11
[0417] Vgl. = Comparative ratio.
[0418] For the various paint formulations, the contact angle for H2O was determined after spraying. For paint 1 (with leveling agent) compared with paint 2 (without leveling agent), it is shown here as an example that the silicone-containing leveling agent used has no influence on the contact angle, since the values are of the same order of magnitude (97° and 100°, respectively) and are therefore comparable. For paints 1 to 5, it has been shown that the addition of NCO-terminated prepolymers containing siloxane chains enables an increase in the contact angle to be achieved without influencing conventional paint parameters such as gloss.
[0419] Furthermore, only slight fluctuations in the contact angle were observed after dry rubbing and surprisingly in the condensation water test (SWT). The results found show a significant difference from the comparative lacquers 8 and lacquers 9 which do not contain NCO-terminated siloxane-containing prepolymers; these have contact angles that are approximately 20° lower. Comparative example lacquer 9 also contains a siloxane-terminated prepolymer, but it has a different composition. Therefore, a decrease in the contact angle is observed in the condensation water test.
[0420] Table 2: Determination of the contact angles of various varnishes before and after being stressed by the scratch and condensation water test (SWT).
[0421] <![CDATA[Contact angle H2O [°]]]> <![CDATA[Paint 1 [1] > Paint 2 <![CDATA[Paint 3 [1] > <![CDATA[Paint 5 [1] > <![CDATA[Paint 7 [1] (See also)]]> Paint 8 (Vgl.) Paint 9 (Vgl.) Paint (before) 97 100 96 96 83 80 101 After PP and reflow (2 h 60 °C) 94 93 95 94 82 80 - <![CDATA[After SWT [2] > 97 95 96 95 73 74 <![CDATA[91 [3] ]]> Δ 0 5 0 3 30 6 10
[0422] [1]With levelling agent. [2] SWT = Condensation Water Test.
[0423] Surprisingly, it was observed that the siloxane-containing coatings have a better reflow compared to the comparative example. This is explained by comparing Paint 3 with Paint 7 as an example. After dry scratching, the gloss of both varnishes dropped - from the same starting value - to about 11 gloss units. After reflow, Paint 3 achieved a value of 87 gloss units, while for Paint 7, a value of only 77 gloss units was observed.
[0424] Table 3: Dry rubbing with a hammer for various paint systems. Reflow: 2 h, 60 °C. All paint systems contain a leveling agent.
[0425] Dry scratching with a hammer Paint 1 Paint 3 Paint 5 Paint 7 Paint 9 Previous glossiness 20° 91.1 91.1 91.4 91.4 89.6 After gloss 20° 11.2 11.5 11.5 11.0 9.9 Residual gloss after PP [%] 12.3 12.6 12.6 12.0 11.0 Gloss 20° Reflow 86.1 87.3 85.8 70.4 77.3 Residual gloss after reflow [%] 94.5 95.8 93.9 77.0 86.3
[0426] Table 4 compares paint systems that all contain a leveling additive. Here again, it is clear that the siloxane-containing systems have significantly better residual gloss and flowback (eg paint 6 vs. paint 8).
[0427] Table 4: Dry rubbing using the abrasion meter for various paint systems. Reflow: 2 h, 60 °C. All paint systems do not contain leveling agent.
[0428] Dry rubbing using a frizz tester Paint 2 Paint 4 Paint 6 Paint 8 Previous glossiness 20° 91 91 91 92 After gloss 20° 42 34 38 15 Residual gloss after PP [%] 46 37 42 16 Gloss 20° Reflow 81 69 63 29 Residual gloss after reflow [%] 89 76 70 46
[0429] Another unexpected beneficial effect observed by the addition of the NCO-terminated siloxane prepolymers is the improved appearance: Coatings of standard formulations form surface orange peel in the absence of leveling additives. If the NCO-terminated siloxane prepolymers of the invention are used and the leveling additives are omitted, no orange peel is observed. By adding the NCO-terminated siloxane prepolymers of the invention, no additives are therefore required for the clearcoat, wherein at the same time no orange peel is formed.
[0430] Furthermore, the compatibility of the NCO-terminated polysiloxane prepolymers was investigated. This was illustrated using the formulations in Table 5 as an example.
[0431] Table 5: Paint formulations with increased NCO-terminated siloxane content.
[0432] Paint 10 Paint 11 Paint 12 PIC / NCO-Siloxane (Binder Solid-Solid) 8:2 7:3 6:4 Polyol 7 50.86 47.54 44.23 Tinuvin 292 1.08 1.04 0.99 Tinuvin 1130 2.16 2.08 1.98 Addocat 201 1.62 1.55 1.38 BA / MPA / XY 33.28 29.27 27.51 Example 4 7.40 11.10 14.80 Polyisocyanate 1 14.80 12.95 11.10 Solid content (%) 50% 50% 50%
[0433] As shown in Table 6, the novel paint raw material can be used in a wide concentration range.
[0434] Table 6: Spraying of Paint 10 and Paint 11
[0435] Paint 10 Paint 11 Paint 12 Optical properties Clear Clear Clear Spray appearance smooth smooth smooth Gloss (20° / 60°) 91 / 94 92 / 95 90 / 94 Haze 11 11 10 Solvent resistance Xy-MPA-EA-Ac (5 min) 2 2 4 4 2 2 4 4 2 2 4 4
[0436] In the following examples, the suitability of the novel siloxane-containing coating raw materials in water-based coatings was examined. The corresponding formulations are given in Table 7.
[0437] Table 7: 2K water-based paints for soft-feel coatings
[0438] Paint 13 (Vgl.) Paint 14 product Solid content[%] Weight [g] Weight(g) Polyol 5 52 25 25 Polyol 6 42 31 31 Distilled water 0 13.7 13.7 Lucrafoam DNE 01 100 0.2 0.2 Tego-Wet KL 245 50 0.4 0.4 Byk 348 100 0.6 0.6 Aquacer 513 35 1.7 1.7 Decosoft Transparent 7 D 100 7.7 7.7 Matting agent Acematt 3300 100 3.1 3.1 Polyisocyanate 5 100 4.98 4.98 Example 4 50 - 1.87 Polyisocyanate 1 100 11.62 11.62
[0439] In these studies, the guide formulation remained unchanged and was supplemented with a new highly compatible NCO-terminated siloxane. Tests showed that the same matte paint appearance was obtained. Contact angle measurements showed that the contact angle could be increased from 90° to 110°.
[0440] Table 8: Waterborne paint applied by spraying, glass substrate.
[0441] Paint 13 (Vgl.) Paint 14 Film appearance Matt, similar to paint 14 Matt, similar to paint 13 <![CDATA[Contact angle H2O [°]]]> 89.6 111
Claims
1. NCO-terminated polysiloxane prepolymer of general formula (I) [(Q) q ]-[(M) m -(P) p -(R) r ] t (I) where R, P, M, Q, r, p, m, q and t are defined as follows R is in each case independently of one another at least one polyisocyanate unit and / or at least one diisocyanate unit, wherein the at least one polyisocyanate unit R is selected from triisocyanates or higher molecular weight oligomers obtainable by reaction of diisocyanates or triisocyanates having biuret, uretdione, isocyanurate, iminooxadiazinedione, allophanate, urethane and / or carbodiimide / uretonimine structural units, P is in each case independently of one another at least one polyol unit, wherein the at least one polyol unit P is selected from the group consisting of polyether polyols, polyester polyols, polyurethane polyols, polysiloxane polyols, polycarbonate polyols, polybutadiene polyols, polyacrylate polyols, polymethacrylate polyols, copolymers of polyacrylate polyols and polymethacrylate polyols, and mixtures thereof, M is in each case independently of one another at least one diisocyanate unit, Q is at least one polysiloxane unit, wherein the at least one polysiloxane unit Q is derived from a polysiloxane polyol, a polysiloxane polyamine or a polysiloxane polythiol, r is in each case independently of one another a number from 1 to 10, p is in each case independently of one another a number from 1 to 10, m is in each case independently of one another a number from 1 to 10, q is in each case independently of one another a number from 1 to 10, t is an integer from 2 to 5, and The existing unit M is directly connected to the unit Q.
2. The polysiloxane prepolymer according to claim 1, characterized in that The diisocyanate or triisocyanate is selected from butane 1,4-diisocyanate, pentane 1,5-diisocyanate (pentamethylene diisocyanate, PDI), hexane 1,6-diisocyanate (hexamethylene diisocyanate, HDI), 4-isocyanatomethyloctane 1,8-diisocyanate (nonane triisocyanate, TIN), 4,4'-methylenebis(cyclohexyl isocyanate) (H12MDI), 3,5,5-trimethyl-1-isocyanato-3-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1,3- and 1, ... Bis(isocyanatomethyl)cyclohexane, naphthalene 1,5-diisocyanate, 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate and 4,4'-diphenylmethane diisocyanate, toluene 2,4-diisocyanate and toluene 2,6-diisocyanate and technical grade mixtures of these two isomers as well as 1,3- and / or 1,4-bis(isocyanatomethyl)benzene, 3,3'-dimethylbiphenyl 4,4'-diisocyanate (TODI), 1,4-p-phenylene diisocyanate (PPDI), cyclohexyl diisocyanate (CHDI) and mixtures thereof.
3. The polysiloxane prepolymer as claimed in claim 2, characterized in that The at least one polyisocyanate unit R is selected from 3,5,5-trimethyl-1-isocyanato-3-isocyanatomethylcyclohexane.
4. The polysiloxane prepolymer according to any one of claims 1 to 2, characterized in that The at least one diisocyanate unit M is selected from butane 1,4-diisocyanate, pentane 1,5-diisocyanate (pentamethylene diisocyanate, PDI), hexane 1,6-diisocyanate (hexamethylene diisocyanate, HDI), 4,4'-methylenebis(cyclohexyl isocyanate) (H12MDI), 3,5,5-trimethyl-1-isocyanato-3-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1,3- and 1,4-bis(isocyanatomethyl)cyclohexane, naphthalene 1, 5-diisocyanate, 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate and 4,4'-diphenylmethane diisocyanate, toluene 2,4-diisocyanate and toluene 2,6-diisocyanate and technical grade mixtures of these two isomers as well as 1,3- and / or 1,4-bis(isocyanatomethyl)benzene, 3,3'-dimethylbiphenyl 4,4'-diisocyanate (TODI), 1,4-p-phenylene diisocyanate (PPDI) and cyclohexyl diisocyanate (CHDI) and mixtures thereof.
5. The polysiloxane prepolymer according to any one of claims 1 to 2, characterized in that The at least one polysiloxane unit Q is derived from a polysiloxane polyol.
6. The polysiloxane prepolymer according to any one of claims 1 to 2, characterized in that The at least one polysiloxane unit is present in an amount of 0.1 wt % to 5 wt % based on the entire polysiloxane prepolymer.
7. The polysiloxane prepolymer according to any one of claims 1 to 2, characterized in that The polysiloxane prepolymer has a number average molecular weight Mn of <4000 g / mol.
8. The polysiloxane prepolymer as claimed in claim 7, characterized in that The polysiloxane prepolymer has a number average molecular weight Mn of >450 g / mol and <3000 g / mol.
9. The polysiloxane prepolymer as claimed in claim 7, characterized in that The polysiloxane prepolymer has a number average molecular weight Mn of >650 g / mol and <2500 g / mol.
10. The polysiloxane prepolymer according to claim 7, characterized in that The polysiloxane prepolymer has a number average molecular weight Mn of >800 g / mol and <2500 g / mol.
11. A method for preparing an NCO-terminated polysiloxane prepolymer as claimed in any one of claims 1 to 10, comprising at least the following steps: (A) reacting at least one polysiloxane polyol, polysiloxane polyamine and / or polysiloxane polythiol with at least one diisocyanate and / or at least one polyisocyanate to obtain at least one NCO-terminated polysiloxane, (B) optionally removing excess at least one diisocyanate and / or at least one polyisocyanate, (C) reacting the at least one NCO-terminated polysiloxane from step (A) or (B) with at least one polyol, (D) reacting the product obtained in step (C) with at least one diisocyanate or at least one polyisocyanate to obtain an NCO-terminated polysiloxane prepolymer.
12. The method as claimed in claim 11, characterized in that Step (B) is performed by thin film evaporation, phase separation, precipitation or a combination thereof.
13. The method according to claim 11 or 12, characterized in that After step (B), the content of at least one diisocyanate or at least one polyisocyanate in the reaction mixture is at most 5% by weight.
14. The method according to claim 13, characterized in that After step (B), the reaction mixture contains at least one diisocyanate or at least one polyisocyanate in an amount of from 1% to 0.01% by weight.
15. The method according to claim 13, characterized in that After step (B), the reaction mixture contains at least one diisocyanate in an amount of at most 5% by weight.
16. The method of claim 13, wherein After step (B), the reaction mixture contains at least one diisocyanate in an amount of 1% to 0.01% by weight.
17. Formulation comprising at least one NCO-terminated polysiloxane prepolymer as claimed in any one of claims 1 to 10.
18. The formulation as claimed in claim 17, wherein the at least one NCO-terminated polysiloxane prepolymer is present in an amount of 5 to 70 wt. %, based on the entire formulation.
19. The formulation as claimed in claim 17, characterized in that It is a paint formulation.
20. The formulation as claimed in claim 19, characterized in that It is a two-component preparation.
21. Use of the NCO-terminated polysiloxane prepolymers as claimed in any one of claims 1 to 10 as curing agents in paint formulations.