Lithium ion battery additive, electrode sheet, and lithium battery
By using additives such as phosphate esters and sulfate esters in the positive and negative electrode materials of lithium batteries to form coating layers, the problems of structural instability and poor cycle performance of lithium batteries at high voltages are solved, achieving high energy density and long cycle life. Lithium batteries improve safety and reduce production costs.
Patent Information
- Application Number
- CN202210406977.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-18
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-04-18
AI Technical Summary
The existing lithium battery cathode materials are structurally unstable under high voltage, resulting in rapid capacity decline and reduced cycle performance. The cycle life of the anode materials is not ideal, making it difficult to meet the needs of high energy density and long cycle life.
An additive containing oxygen-containing groups such as phosphate ester and sulfate ester is used in the electrode slurry of positive and negative electrode materials to form a uniform coating layer, improve the structural stability and ionic conductivity of the material, and enhance electrochemical stability sex.
It significantly improves the electrochemical stability and cycle life of lithium batteries under high cut-off voltage, improves energy density and safety, reduces production costs, and is suitable for large-scale commercial production.
Smart Images

Figure CN114843605B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and specifically relates to an additive for stabilizing the electrochemical performance of lithium ion battery electrode materials, as well as an electrode sheet and a lithium ion battery containing the additive. Background Art
[0002] Lithium-ion batteries are widely used in different fields such as 3C electronics, drones, electric vehicles, etc. due to their high energy density and long cycle life, and have become an indispensable part of people's lives. The positive and negative electrode materials used in ideal lithium-ion batteries need to comprehensively consider multiple factors such as specific capacity, electrochemical performance, safety, and cost. As people's requirements for product endurance continue to increase, seeking to improve the energy density and cycle life of lithium batteries, especially improving the cycle performance of positive and negative electrode materials, while improving the safety of lithium batteries, has very important scientific and commercial value, and has become the main difficulty in many research and technological breakthroughs.
[0003] At present, lithium batteries are mainly composed of positive electrodes, negative electrodes, separators, electrolytes and shell packaging. Among them, the positive electrode material is one of the key materials of lithium batteries and is also a key factor in determining the final performance. The capacity of positive electrode materials in lithium batteries is currently low, which is difficult to meet the growing needs. Take the commercial positive electrode material lithium cobalt oxide (LiCoO2, LCO) as an example. As the earliest commercialized positive electrode material, lithium cobalt oxide has a theoretical capacity of up to 274mAh / g and the highest volume energy density, and still firmly occupies the consumer electronics market. However, in practical applications, lithium cobalt oxide positive electrode materials can only release a specific capacity of 140mAh / g at a charging voltage of 4.2V. Even after decades of research and development, high-voltage lithium cobalt oxide positive electrode materials can only obtain a specific capacity of 180mAh / g at a cut-off voltage of 4.45V, which still has a certain development space compared with its theoretical capacity. However, when the cut-off voltage is further increased (>4.5V), the lithium cobalt oxide material faces structural damage caused by the irreversible transformation of the crystal structure from O3 phase to H1-3 phase, as well as a series of interface side reactions that cause the cathode / electrolyte interface to be damaged, the interface lattice oxygen to be released, and the dissolution of the cobalt element, which leads to rapid capacity decay and a decrease in cycle performance, hindering the further development and application of high-voltage lithium cobalt oxide. A charging cut-off voltage of 4.6V can give lithium cobalt oxide a specific capacity of nearly 220mAh / g, which can bring a nearly 23% increase in energy density.
[0004] Although the commonly used means for preparing high-voltage lithium cobalt oxide commercially, including doping and coating, can improve the structure and interface stability of lithium cobalt oxide positive electrode materials to a certain extent, thereby improving the electrochemical performance of lithium cobalt oxide at high voltage. However, these modification methods are difficult to further improve the cut-off voltage of lithium cobalt oxide positive electrode materials, especially the cycle stability of the cut-off voltage at 4.6V. And these modification methods usually increase the complexity of the process and bring additional costs to production. This problem is also reflected in other positive electrode materials. Therefore, developing a simple and effective modification method that can improve the stability of lithium cobalt oxide positive electrode materials at a cut-off voltage of 4.6V, obtain positive electrode materials with high energy density, and will not bring a lot of additional costs to industrial production has become the direction of seeking technological breakthroughs in the field of lithium batteries. In addition, the commonly used negative electrode materials are mainly carbon materials based on graphite, but they have problems such as low actual specific capacity, poor rate performance, and unsatisfactory cycle life.
[0005] Therefore, how to improve the electrochemical stability of positive electrode materials at a high cut-off voltage of 4.6V and improve the cycle performance of negative electrode materials are issues that need to be urgently addressed in the lithium battery industry. Summary of the invention
[0006] The purpose of the present invention is to provide an additive that can improve the energy density and cycle performance of lithium batteries under high voltage.
[0007] Another object of the present invention is to provide an electrode sheet comprising the additive.
[0008] Another object of the present invention is to provide a lithium battery comprising the electrode sheet.
[0009] In order to achieve one of the above purposes, the present invention adopts the following technical solution:
[0010] An additive for a lithium-ion battery, the additive is used in an electrode slurry for a positive electrode sheet and / or a negative electrode sheet, and the additive is a compound of the following structural formula:
[0011]
[0012] Among them, R 1 Selected from phosphates, metal salts of phosphates, sulfates, metal salts of sulfates;
[0013] R 2 , R 3 , R 4 , R 5 , R 6 Each is independently selected from alkyl, hydroxyl, carboxyl, phosphate, metal salt of phosphate, phosphite, metal salt of phosphite, pyrophosphate, metal salt of pyrophosphate, sulfate, metal salt of sulfate, sulfonic acid, metal salt of sulfonic acid, sulfinic acid, metal salt of sulfinic acid.
[0014] Furthermore, the R 1 Selected from sulfate esters and metal salts of sulfate esters.
[0015] Furthermore, the R 2 , R 3 , R 4 , R 5 , R 6 Each is independently selected from hydroxyl, phosphate, metal salt of phosphate, sulfate, metal salt of sulfate.
[0016] Furthermore, the additive is cyclohexanehexol hexaphosphate, a metal salt of cyclohexanehexol hexaphosphate, cyclohexanehexol triphosphate, a metal salt of cyclohexanehexol triphosphate, inositol hexasulfate or a metal salt of inositol hexasulfate.
[0017] Furthermore, the additive is inositol hexasulfate or a metal salt of inositol hexasulfate.
[0018] Cyclohexanol triphosphate includes cyclohexanol 1,2,3-triphosphate, cyclohexanol 1,2,4-triphosphate and cyclohexanol 1,3,5-triphosphate.
[0019] Furthermore, the metal salt is a lithium salt, a sodium salt or a potassium salt.
[0020] Furthermore, the additive is cyclohexanehexol hexaphosphate, cyclohexanehexol hexaphosphate dodecalinium, inositol triphosphate, inositol triphosphate hexalithium, inositol hexasulfate or inositol hexasulfate dodecalinium.
[0021] Inositol triphosphate refers to inositol-1,3,5-triphosphate.
[0022] Furthermore, the additive is inositol hexasulfate or inositol hexasulfate dodecalinium.
[0023] Furthermore, the additive is added to the electrode slurry in an amount of 0.1 to 20 wt %.
[0024] A lithium battery electrode sheet comprises a positive electrode sheet and / or a negative electrode sheet, wherein the electrode sheet contains the above-mentioned additive.
[0025] The components of the positive electrode slurry include a positive electrode active material, a binder, a conductive agent, additives and a solvent.
[0026] The positive electrode active material is selected from at least one of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium nickel oxide, lithium nickel cobalt manganese ternary composite oxide, and lithium-rich manganese-based lithium oxide; the proportion of the positive electrode active material in the positive electrode slurry is 80-95wt%.
[0027] The binder is one or more of polyvinylidene fluoride, cellulose-based binder, polyacrylate-based binder, and rubber-based binder; the proportion of the binder in the positive electrode slurry is 0.5-10 wt%.
[0028] The conductive agent is one or more of acetylene black, conductive carbon black, conductive graphite, carbon fiber, and carbon nanotubes; the proportion of the conductive agent in the slurry is 0.5-10wt%.
[0029] The solvent is one or more of N-methylpyrrolidone, N-dimethylformamide, dimethyl sulfoxide and water.
[0030] The positive electrode sheet includes positive electrode slurry and current collector, the current collector is aluminum foil, and the positive electrode sheet preparation process is: the uniformly mixed positive electrode slurry is coated on the current collector, and is made by vacuum high-temperature drying; the mixing method of the positive electrode slurry is mechanical stirring, ball milling or high-speed vibration mixing.
[0031] The components of the negative electrode slurry include a negative electrode active material, a binder, a conductive agent, additives and a solvent.
[0032] The negative electrode active material is selected from at least one of graphite, silicon, silicon oxide, lithium titanate, and metallic lithium.
[0033] The binder is one or more of polyvinylidene fluoride, cellulose-based binder, polyacrylate-based binder, and rubber-based binder; the proportion of the binder in the positive electrode slurry is 0.5-10 wt%.
[0034] The conductive agent is one or more of acetylene black, conductive carbon black, conductive graphite, carbon fiber, and carbon nanotubes; the proportion of the conductive agent in the slurry is 0.5-10wt%.
[0035] The solvent is one or more of N-methylpyrrolidone, N-dimethylformamide, dimethyl sulfoxide and water.
[0036] Furthermore, the additives in the electrode sheet are added in the form of direct addition, spray drying, ball milling, spin coating or immersion.
[0037] A lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator, an electrolyte and a shell. The positive electrode sheet or the negative electrode sheet is as described above; the separator, the electrolyte and the shell are commonly used and well-known materials in the art and are not particularly limited.
[0038] The negative electrode sheet includes a negative electrode slurry and a current collector, wherein the current collector is a copper foil. The negative electrode sheet preparation process is as follows: the uniformly mixed negative electrode slurry is coated on the current collector and dried at a high temperature in a vacuum; the mixing method of the negative electrode slurry is mechanical stirring, ball milling or high-speed vibration mixing.
[0039] Alkyl refers to a saturated aliphatic hydrocarbon group, which is a straight or branched chain group containing 1 to 20 carbon atoms, preferably an alkyl group containing 1 to 12 carbon atoms, and more preferably an alkyl group containing 1 to 6 carbon atoms. Examples of alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, 2-pentyl, isopentyl, neopentyl, hexyl, 2-hexyl, 3-hexyl, 3-methylpentyl.
[0040] Phosphate finger
[0041] Phosphite refers to
[0042] Pyrophosphate finger
[0043] Sulfate finger
[0044] Sulfonic acid group
[0045] Sulfinate
[0046] The present invention has the following beneficial effects:
[0047] The ester groups containing oxygen atoms such as phosphate ester and sulfate ester of the additive of the present invention can form a uniform coating layer on the surface of the positive electrode material and the negative electrode material particles, which can improve the structural stability of the electrode material, reduce interface side reactions, enhance the electrode ion conductivity, and ultimately improve the high-voltage electrochemical stability of the positive electrode material and the cycle life of the negative electrode material, thereby obtaining a lithium battery with high cut-off voltage, high energy density and long cycle life.
[0048] The additives contain groups such as phosphates and sulfates that are chemically stable under high temperature conditions, which can improve the electrochemical cycle stability of lithium-ion batteries when operating under higher temperature conditions, effectively solve the current safety issues of lithium batteries such as flammability and explosion, and effectively improve the safety of lithium batteries.
[0049] The electrode sheet of the present invention has low cost and simple preparation process, and the amount of additive added is controllable. It can be directly adapted to the existing lithium battery production and can be easily implemented in large-scale commercial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Attached Figure 1 It is a cycle diagram of lithium cobalt oxide-lithium metal battery of Examples 1 to 3 and Comparative Example 1;
[0051] Attached Figure 2 It is a high temperature cycle diagram of the lithium cobalt oxide-lithium metal battery of Example 4 and Comparative Example 1;
[0052] Attached Figure 3Graphite-lithium metal battery cycle diagrams of Example 5 and Comparative Example 2;
[0053] Attached Figure 4 It is the cycle diagram of the lithium cobalt oxide-graphite battery of Example 11 and Comparative Example 3. DETAILED DESCRIPTION
[0054] The present invention will be further described below in conjunction with specific embodiments. The following parts are all parts by weight.
[0055] Example 1
[0056] The positive electrode sheet and lithium battery are prepared by using lithium cobalt oxide as the positive electrode material and cyclohexanehexol hexaphosphate as an additive.
[0057] 80 parts of lithium cobalt oxide positive electrode active material, 10 parts of acetylene black, 10 parts of PVDF binder, 5 parts of cyclohexane hexol hexaphosphate and an appropriate amount of N-methylpyrrolidone were mixed at 1600 rpm for 10 minutes using a high-speed centrifugal homogenizer to obtain a uniform oily positive electrode slurry.
[0058] The prepared positive electrode slurry was evenly coated on aluminum foil using a coating machine, and transferred to a blast drying oven for 6 hours at 60°C. It was then transferred to a vacuum drying oven for secondary drying. It was then rolled and cut into pieces to obtain a circular positive electrode sheet with a diameter of 12 mm, which was stored in a glove box for later use.
[0059] The battery uses a CR2032 button cell. The battery is assembled in the order of positive electrode shell, positive electrode sheet, diaphragm, lithium sheet, stainless steel gasket, spring, and negative electrode shell, and the amount of electrolyte added is 30 to 60 microliters. The battery assembly process must be completed in an argon atmosphere glove box.
[0060] Example 2
[0061] The positive electrode sheet and the lithium battery were prepared using the same scheme as in Example 1. The difference from Example 1 was that the additive was cyclohexanehexol hexaphosphate dodecalinium.
[0062] Example 3
[0063] The positive electrode sheet and lithium battery were prepared using the same scheme as in Example 1. The difference from Example 1 was that the additive was inositol triphosphate.
[0064] Example 4
[0065] The positive electrode sheet and the lithium battery were prepared using the same scheme as in Example 1. The difference from Example 1 was that the additive was inositol triphosphate hexalithium.
[0066] Comparative Example 1
[0067] The positive electrode sheet and lithium battery were prepared using the same protocol as in Example 1, but without adding additives.
[0068] Performance Testing
[0069] The lithium cobalt oxide half-cells prepared in Examples 1, 2, 3 and Comparative Example 1 were subjected to constant current charge and discharge tests at room temperature in the range of 3 to 4.6 V at 1C, and the number of test cycles was 100. The evaluation method was capacity retention rate. The capacity retention rate was defined as: capacity retention rate = 100th cycle discharge capacity / 1st cycle discharge capacity × 100%.
[0070] The results are as follows Figure 1 As shown, by comparison, it can be found that the decay rate of comparative example 1 at a high cut-off voltage of 4.6V is very fast, and the capacity has been reduced by more than 30% (only 69%) after 100 cycles, while embodiments 1 to 3 show significantly improved cycle life, and there is still a capacity retention rate of nearly 90% after a long cycle (89% for embodiment 1, 88% for embodiment 2, and 87% for embodiment 3); This shows that the introduction of additives effectively improves the electrochemical cycle stability of lithium cobalt oxide with a high cut-off voltage, thereby obtaining a lithium-ion battery with a higher energy density.
[0071] The lithium cobalt oxide half-cells prepared in Example 4 and Comparative Example 1 were subjected to constant current charge and discharge tests at 1C in the range of 3 to 4.6 V and at 45° C., with the number of test cycles being 100.
[0072] The results are as follows Figure 2 As shown, by comparison, it is found that the capacity retention rate of Example 4 is 68%, and the capacity retention rate of Comparative Example 1 is 49%. Under higher temperature operating conditions, the additive has a significant improvement effect on the cycle stability of the positive electrode material under high voltage, indicating that the introduction of additives can improve the high temperature performance of lithium batteries and improve the safety of lithium batteries, thereby meeting more complex application markets.
[0073] Example 5
[0074] Anode sheets and lithium batteries are prepared using graphite as the negative electrode material and inositol hexasulfate dodecasulfate as an additive.
[0075] 95 parts of graphite negative electrode active material, 5 parts of carbon nanotubes, 5 parts of sodium carboxymethyl cellulose binder, 5 parts of styrene-butadiene rubber binder, 3 parts of lithium inositol hexasulfate and deionized water dispersant were ground for 1 hour to obtain a uniform negative electrode slurry.
[0076] The prepared negative electrode slurry was evenly coated on the copper foil with a coater, and transferred to a blast drying oven, and dried at 60°C for 6 hours, and then transferred to a vacuum drying oven for secondary drying. Then, it was rolled and cut into pieces to obtain a circular negative electrode sheet with a diameter of 12 mm, which was stored in a glove box for later use.
[0077] The battery uses a CR2032 button cell. The battery is assembled in the order of positive electrode shell, negative electrode sheet, diaphragm, lithium sheet, stainless steel gasket, spring, and negative electrode shell, with the amount of electrolyte added being 30 to 60 microliters. The battery assembly process must be completed in an argon atmosphere glove box.
[0078] Comparative Example 2
[0079] The negative electrode sheet and lithium battery were prepared using the same protocol as in Example 5, but without adding additives.
[0080] Performance Testing
[0081] The lithium batteries prepared in Example 5 and Comparative Example 2 were subjected to constant current charge and discharge tests at 0.5C in the range of 0.01-2V, and the number of test cycles was 200. The evaluation method was capacity retention rate.
[0082] The results are as follows Figure 3 As shown in the figure, it is found that after 200 cycles, Example 5 still maintains a capacity of nearly 300 mAh / g, with a retention rate of 88%. Comparative Example 2 decays rapidly, and finally only has a capacity of 260 mAh / g, showing a capacity retention rate of only 78%. This shows that the additive is also beneficial to the improvement of the cycle life of the negative electrode material, and is more conducive to further improving the cycle performance of the full battery.
[0083] Example 6
[0084] The negative electrode sheet and lithium battery were prepared using the same scheme as in Example 5, except that the additive was inositol hexasulfate.
[0085] The test was carried out in the same way and the capacity retention rate was 90%.
[0086] Example 7
[0087] The negative electrode sheet and lithium battery were prepared using the same scheme as in Example 5, except that the additive was hexasodium inositol triphosphate.
[0088] The test was carried out in the same way and the capacity retention rate was 83%.
[0089] Example 8
[0090] The negative electrode sheet and lithium battery were prepared using the same scheme as in Example 5, except that the additive was cyclohexanehexol hexaphosphate.
[0091] The test was carried out in the same way and the capacity retention rate was 82%.
[0092] Example 9
[0093] The positive electrode sheet and lithium battery were prepared using the same scheme as in Example 1, except that the additive was inositol hexasulfate.
[0094] The test was carried out in the same way and the capacity retention rate was 93%.
[0095] Example 10
[0096] The positive electrode sheet and the lithium battery were prepared using the same scheme as in Example 1, except that the additive was inositol hexasulfate dodecapotassium.
[0097] The test was carried out in the same way and the capacity retention rate was 92%.
[0098] Embodiment 11
[0099] The positive electrode sheet of Example 1 and the negative electrode sheet of Example 5 are assembled into a battery.
[0100] Comparative Example 3
[0101] The positive electrode sheet of comparative example 1 and the negative electrode sheet of comparative example 2 are assembled into a battery.
[0102] Performance Testing
[0103] The lithium batteries prepared in Example 11 and Comparative Example 3 were subjected to a long-cycle charge and discharge test at 0.5C. The results are as follows: Figure 4 As shown, after 100 cycles, the battery capacity retention rate of Example 11 reached 95%, and the remaining capacity of the battery of Comparative Example 3 was only 72%. It is proved that adding additives to both the negative electrode and the positive electrode can comprehensively improve the long-cycle stability of lithium-ion batteries at high cut-off voltages, and the effect of improving the cycle performance is more significant than adding additives only to the negative electrode or the positive electrode, or not using additives. Compared with current commercial lithium batteries, due to the increase in the charge cut-off voltage, the electrochemical stability is improved, thereby obtaining a lithium-ion battery with higher energy density.
[0104] Example 12
[0105] The positive electrode sheet was prepared by the same scheme as in Example 1, the negative electrode sheet was prepared by the same scheme as in Example 5, and then assembled into a lithium battery. The additive was
[0106]
[0107] When tested in the same manner, the capacity retention rate was 89%.
[0108] Example 13
[0109] The positive electrode sheet was prepared by the same scheme as in Example 1, the negative electrode sheet was prepared by the same scheme as in Example 5, and then assembled into a lithium battery. The additive was
[0110]
[0111] When tested in the same manner, the capacity retention rate was 93%.
[0112] Embodiment 14
[0113] The positive electrode sheet was prepared by the same scheme as in Example 1, the negative electrode sheet was prepared by the same scheme as in Example 5, and then assembled into a lithium battery. The additive was
[0114]
[0115] When tested in the same manner, the capacity retention rate was 89%.
[0116] Embodiment 15
[0117] The positive electrode sheet was prepared by the same scheme as in Example 1, the negative electrode sheet was prepared by the same scheme as in Example 5, and then assembled into a lithium battery. The additive was
[0118]
[0119] When tested in the same manner, the capacity retention rate was 94%.
[0120] Example 16
[0121] The positive electrode sheet was prepared by the same scheme as in Example 1, the negative electrode sheet was prepared by the same scheme as in Example 5, and then assembled into a lithium battery. The additive was
[0122]
[0123] When tested in the same manner, the capacity retention rate was 91%.
[0124] Embodiment 17
[0125] The positive electrode sheet was prepared by the same scheme as in Example 1, the negative electrode sheet was prepared by the same scheme as in Example 5, and then assembled into a lithium battery. The additive was
[0126]
[0127] The test was carried out in the same manner and the capacity retention rate was 85%.
[0128] Embodiment 18
[0129] The positive electrode sheet was prepared by the same scheme as in Example 1, the negative electrode sheet was prepared by the same scheme as in Example 5, and then assembled into a lithium battery. The additive was
[0130]
[0131] The test was carried out in the same manner and the capacity retention rate was 90%.
[0132] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A lithium battery electrode sheet, including a positive electrode sheet, characterized in that: The positive electrode sheet contains the following additives; The positive electrode active material of the positive electrode sheet is selected from at least one of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium nickel oxide, lithium nickel cobalt manganese ternary composite oxide, and lithium-rich manganese-based lithium oxide; The additive is a metal salt of cyclohexanehexol hexaphosphate, cyclohexanehexol triphosphate, a metal salt of cyclohexanehexol triphosphate, inositol hexasulfate or a metal salt of inositol hexasulfate.
2. The electrode sheet according to claim 1, characterized in that: The metal salt is a lithium salt, a sodium salt or a potassium salt.
3. The electrode sheet according to claim 1, characterized in that: The additive is added to the electrode slurry in an amount of 0.1 to 20 wt %.
4. A lithium ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator, an electrolyte and a casing, characterized in that: The positive electrode sheet is as described in any one of claims 1 to 3.
Citation Information
Patent Citations
Battery negative electrode material, preparation method and application thereof and lithium ion battery
CN112635719A