Silicone particles with cross-linked core and preparation thereof
By introducing cross-linked silicone elastomer and reinforcing fillers into silicone elastomer particles, and combining them with the structure of the silica shell, the problems of insufficient skin feel and mechanical stability of existing silicone elastomer particles are solved, and a better solution is achieved. Good silky feel and pressure resistance.
Patent Information
- Application Number
- CN201980103278.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-12-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2039-12-17
AI Technical Summary
Existing silica-coated silicone elastomer particles in cosmetics have undesirable skin feel and low mechanical stability, and are easily damaged by pressure and friction.
Using a core containing a cross-linked silicone elastomer composition and reinforcing fillers, combined with the particle structure of the silica shell, specific emulsification and cross-linking methods ensure that the silica is firmly bound to the particle surface, improving skin feel and mechanical stability. sex.
The skin feel and mechanical stability of the particles are significantly improved, allowing them to exhibit better silkiness and pressure resistance under application conditions, and avoid the problem of traditional particles forming agglomerates under pressure.
Abstract
Description
[0001] The present invention relates to elastomeric particles P consisting of a core comprising a crosslinked silicone elastomer composition and a reinforcing filler, and to a process for their production.
[0002] WO2017142068 A1 describes the advantageous properties of silica-coated silicone elastomer particles, in particular the spherical nature, the possibility of influencing the hydrophobic properties, the friction-reducing properties and the absence of adhesion. Therefore, such silica-coated silicone elastomer particles are used in cosmetics.
[0003] Such particles also have the advantage of being able to absorb functional substances such as care oils or fragrances. This is a significant advantage compared to the resin-based particles disclosed in WO2007113095. However, these particles according to WO2017142068 have a still undesirable skin feel and low mechanical stability. Pressure and friction easily destroy such elastomeric particles.
[0004] The invention provides particles P consisting of a core K comprising a crosslinked silicone elastomer composition X and a reinforcing filler F, and a shell H of silica S.
[0005] Under application conditions, the particles P have a surprisingly improved skin feel compared to known particles without reinforcing fillers in the core. This is particularly surprising since the reinforcing fillers are contained in the core K of the silica-coated silicone elastomer particles and do not modify the shell H of the particles P, which shell produces the immediate skin feel.
[0006] Completely unexpectedly, the particles P according to the invention also have an improved mechanical stability compared to known particles without reinforcing fillers or with non-reinforcing fillers in the core, despite the fact that the shell H of the particles P is not modified.
[0007] The particles P are substantially spherical. Preferably the sphericity SPHT3 is at least 0.8, more preferably at least 0.82, as determined by ISO 9276-6 using a Camsizer X2 from Retsch Technology.
[0008] The particles P are characterized in particular in that the silicon dioxide S used is essentially bound to the surface of the polymer particles P. The distribution of the silicon dioxide S used can be obtained from TEM micrographs of thin sections of the embedded particles according to the invention. The silicon dioxide S is preferably more than 10 nm, more preferably more than 20 nm, very preferably more than 30 nm impregnated into the crosslinked polymerisation product and protrudes from the crosslinked polymerisation product preferably more than 10 nm, more preferably more than 20 nm, very preferably more than 30 nm (measured in each case from the outer boundary of the crosslinked polymerisation product) and is therefore firmly bound to the surface of the particles P. This is a significant advantage compared to commercially available products in which silicone elastomer particles are finished with a silicon dioxide post-treatment. In the case of such products, the silicon dioxide is not impregnated into the silicone elastomer and is therefore not firmly bound to the surface.
[0009] As silicone elastomer composition X, in principle all silicones known in the prior art can be used. Addition-crosslinking, peroxidic-crosslinking, condensation-crosslinking or radiation-crosslinking compositions can be used. Peroxidic or addition-crosslinking components are preferred. Addition-crosslinking compositions are particularly preferred.
[0010] The addition-crosslinking silicone elastomer compositions X used in the present invention are known in the prior art and in the simplest case comprise
[0011] (A) at least one linear compound containing a group having an aliphatic carbon-carbon multiple bond
[0012] (B) at least one linear organopolysiloxane compound having Si-bonded hydrogen atoms,
[0013] Or, instead of (A) and (B),
[0014] (C) at least one linear organopolysiloxane compound comprising SiC-bonded groups having aliphatic carbon-carbon multiple bonds and Si-bonded hydrogen atoms, and
[0015] (D) at least one hydrosilylation catalyst.
[0016] The addition-crosslinking silicone elastomer composition X may be a one-component silicone composition or a two-component silicone composition.
[0017] In the case of a two-component silicone elastomer composition X, both components of the addition-crosslinking silicone elastomer composition X may comprise all components in any desired combination, generally with the proviso that one component does not simultaneously comprise a siloxane having aliphatic multiple bonds, a siloxane having Si-bonded hydrogen and a catalyst, i.e., essentially does not simultaneously comprise components (A), (B) and (D) or (C) and (D).
[0018] As is known, the compounds (A) and (B) or (C) used in the addition-crosslinking silicone elastomer composition X are selected so that crosslinking is possible. Thus, for example, compound (A) comprises at least two aliphatically unsaturated groups and (B) comprises at least three Si-bonded hydrogen atoms, or compound (A) comprises at least three aliphatically unsaturated groups and siloxane (B) comprises at least two Si-bonded hydrogen atoms, or, instead of compounds (A) and (B), a siloxane (C) containing aliphatically unsaturated groups and Si-bonded hydrogen atoms in the above-mentioned ratios is used. Also suitable are mixtures of (A) and (B) and (C) having aliphatically unsaturated groups and Si-bonded hydrogen atoms in the above-mentioned ratios.
[0019] The addition-crosslinking silicone elastomer composition X generally contains 30-99.9% by weight, preferably 35-95% by weight, more preferably 40-90% by weight of (A). The addition-crosslinking silicone elastomer composition X generally contains 0.1-60% by weight, preferably 0.5-50% by weight, more preferably 1-30% by weight of (B). If the addition-crosslinking silicone elastomer composition X comprises component (C), generally 30-95% by weight, preferably 35-90% by weight, more preferably 40-85% by weight of (C) is present in the formulation.
[0020] The compound (A) used in the present invention may include a silicon-free organic compound preferably having at least two aliphatic unsaturated groups, and an organic silicon compound preferably having at least two aliphatic unsaturated groups, or a mixture thereof.
[0021] Examples of the silicon-free organic compound (A) are 1,3,5-trivinylcyclohexane, 2,3-dimethyl-1,3-butadiene, 7-methyl-3-methylene-1,6-octadiene, 2-methyl-1,3-butadiene, 1,5-hexadiene, 1,7-octadiene, 4,7-methylene-4,7,8,9-tetrahydroindene, methylcyclopentadiene, 5-vinyl-2-norbornene, bicyclo[2.2.1]hept-2,5-diene, 1,3-diisopropenylbenzene, vinyl-containing polybutadiene, 1,4-divinylcyclohexane, 1,3,5-triallylbenzene, 1,3,5-trivinylbenzene, 1,2,4-trivinylcyclohexane, 1,3,5-triisopropenylbenzene, 1,4-divinylbenzene, 3-methylhept-(1,5)-diene, 3-benzene. 4,5-dimethyl-4,5-diethyloctane-(1,7)-diene, N,N'-methylenebisacrylamide, 1,1,1-tri(hydroxymethyl)propane triacrylate, 1,1,1-tri(hydroxymethyl)propane trimethacrylate, tripropylene glycol diacrylate, diallyl ether, diallylamine, diallyl carbonate, N,N'-diallyl urea, triallylamine, tri(2-methylallyl)amine, 2,4,6-triallyloxy-1,3,5-triazine, triallyl-s-triazine-2,4,6(1H,3H,5H)-trione, diallyl malonate, polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, poly(propylene glycol) methacrylate.
[0022] The addition-crosslinking silicone elastomer composition X preferably comprises as component (A) at least one aliphatic unsaturated organosilicon compound, in which case it is possible to use all aliphatic unsaturated organosilicon compounds which have hitherto been used in addition-crosslinking components, for example silicone block copolymers having urea segments, silicone block copolymers having amide segments and / or imide segments and / or ester-amide segments and / or polystyrene segments and / or silylarylene segments and / or carborane segments, and silicon-grafted copolymers having ether groups.
[0023] As the organosilicon compound (A) containing SiC bonding groups having aliphatic carbon-carbon multiple bonds, it is preferred to use a linear or branched organopolysiloxane composed of units of the general formula (I):
[0024] R 4 a R 5 b SiO (4-a-b) / 2 (I)
[0025] in
[0026] R 4is independently the same or different at each occurrence an organic or inorganic group that does not contain aliphatic carbon-carbon multiple bonds,
[0027] R 5 is independently, the same or different at each occurrence, a monovalent, substituted or unsubstituted SiC-bonded hydrocarbon radical having at least one aliphatic carbon-carbon multiple bond,
[0028] a is 0, 1, 2, or 3, and
[0029] b is 0, 1, or 2,
[0030] The condition is that the sum of a+b is less than or equal to 3 and each molecule has at least 2 groups R 5 .
[0031] Group R 4 Monovalent or polyvalent groups may be present, in which case polyvalent groups such as divalent, trivalent and tetravalent groups, for example, connect two or more, such as two, three or four, siloxy units, for example of formula (I), to one another.
[0032] R 4 Other examples are monovalent groups -F, -Cl, -Br, OR 6 , -CN, -SCN, -NCO, and SiC-bonded, substituted or unsubstituted hydrocarbon radicals which may be interrupted by oxygen atoms or groups -C(O)-; and divalent radicals bonded to Si at both ends according to formula (I). 4 When a SiC-bonded substituted hydrocarbon group is included, preferred substituents are halogen atoms, phosphorus-containing groups, cyano groups, -OR 6 、-NR 6 -、-NR 6 2. -NR 6 -C(O)-NR 6 2. -C(O)-NR 6 2. -C(O)R 6 、-C(O)OR 6 , -SO2-Ph and -C6F5. In these groups, R 6 is independently the same or different at each occurrence a hydrogen atom or a monovalent hydrocarbon group having 1 to 20 carbon atoms, and Ph is phenyl.
[0033] Group R 4Examples of are alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, neopentyl, tert-pentyl, hexyl (such as n-hexyl), heptyl (such as n-heptyl), octyl (such as n-octyl and isooctyl such as 2,2,4-trimethylpentyl), nonyl (such as n-nonyl), decyl (such as n-decyl), dodecyl (such as n-dodecyl) and octadecyl (such as n-octadecyl); cycloalkyl groups such as cyclopentyl, cyclohexyl, cycloheptyl and methylcyclohexyl; aryl groups such as phenyl, naphthyl, anthracenyl and phenanthryl; alkaryl groups such as o-, m-, p-tolyl, xylyl and ethylphenyl; and aralkyl groups such as benzyl, α- and β-phenethyl.
[0034] Substituent R 4 Examples are halogenated alkyl groups such as 3,3,3-trifluoro-n-propyl, 2,2,2,2',2',2'-hexafluoroisopropyl, heptafluoroisopropyl; halogenated aryl groups such as o-, m- and p-chlorophenyl; -(CH2)-N(R 6 )C(O)NR 6 2. -(CH2) o -C(O)NR 6 2. -(CH2) o -C(O)R 6 、-(CH2) o -C(O)OR 6 、-(CH2) o -C(O)NR 6 2. -(CH2)-C(O)-(CH2) p C(O)CH3, -(CH2)-O-CO-R 6 、-(CH2)-NR 6 -(CH2) p -NR 6 2. -(CH2) o -O-(CH2) p CH(OH)CH2OH, -(CH2) o (OCH2CH2) p OR 6 、-(CH2) o -SO2-Ph and -(CH2) o -O-C6F5, where R 6 and Ph correspond to the above definitions, o and p are the same or different integers between 0 and 10.
[0035] R as a divalent group bonded to Si at both ends according to formula (I) 4 Examples of are derived from the above for group R 4The monovalent examples are stated as groups because additional bonding exists through substitution of a hydrogen atom; examples of such groups are -(CH2)-, -CH(CH3)-, -C(CH3)2-, -CH(CH3)-CH2-, -C6H4-, -CH(Ph)-CH2-, -C(CF3)2-, -(CH2) o -C6H4-(CH2) o -、-(CH2) o -C6H4-C6H4-(CH2) o -、-(CH2O) p 、(CH2CH2O) o 、-(CH2) o -O x -C6H4-SO2-C6H4-O x -(CH2) o -, wherein x is 0 or 1, and Ph, o, and p have the above definitions.
[0036] Group R 4 Preferably it comprises a monovalent, SiC-bonded, optionally substituted hydrocarbon radical free of aliphatic carbon-carbon multiple bonds and having 1 to 18 carbon atoms, more preferably a monovalent, SiC-bonded hydrocarbon radical free of aliphatic carbon-carbon multiple bonds and having 1 to 6 carbon atoms, more particularly methyl or phenyl.
[0037] Group R 5 Any desired groups which are capable of undergoing an addition reaction (hydrosilylation) with SiH-functional compounds may be present.
[0038] When the group R 5 When containing SiC-bonded substituted hydrocarbon groups, preferred substituents are halogen atoms, cyano groups and -OR 6 , where R 6 Having the above definition.
[0039] Group R 5 It is preferably an alkenyl group and an alkynyl group having 2 to 16 carbon atoms, such as a vinyl group, an allyl group, a methallyl group, a 1-propenyl group, a 5-hexenyl group, an ethynyl group, a butadienyl group, a hexadienyl group, a cyclopentenyl group, a cyclopentadienyl group, a cyclohexenyl group, a vinylcyclohexylethyl group, a divinylcyclohexylethyl group, a norbornenyl group, a vinylphenyl group and a styryl group, with particular preference being given to using a vinyl group, an allyl group and a hexenyl group.
[0040] The molecular weight of component (A) can vary within a wide range, for example, between 10 2 and 10 6Thus, for example, component (A) may be a relatively low molecular weight alkenyl functional oligosiloxane, such as 1,2-divinyltetramethyldisiloxane; or a molecular weight of, for example, 10 5 g / mol (number average determined by nmR) of high polymer polydimethylsiloxanes with Si-bonded vinyl groups in the chain or at the ends. The structure of the molecules forming component (A) is likewise not fixed; in particular, the structure of relatively high molecular weight siloxanes, i.e. oligomeric or polymeric siloxanes, can be linear, cyclic, branched or resinous, network-like. Linear and cyclic polysiloxanes are preferably of the formula R 4 3SiO 1 / 2 , R 5 R 4 2SiO 1 / 2 , R 5 R 4 SiO 1 / 2 and R 4 2SiO 2 / 2 The unit composition is R 4 and R 5 The branched and network polysiloxanes further comprise trifunctional and / or tetrafunctional units, preferably of the formula R 4 SiO 3 / 2 , R 5 SiO 3 / 2 and SiO 4 / 2 Of course, mixtures of different siloxanes that meet the criteria for component (A) can also be used.
[0041] Particularly preferred components (A) are those having a diameter of 0.01 to 500,000 mm 2 / s, more preferably 0.1 to 100000 mm 2 / s, particularly preferably 1 to 10000 mm 2 Vinyl-functional, substantially linear polydiorganosiloxanes having a kinematic viscosity of DIN 53019 of in each case 25° C. / s.
[0042] As organosilicon compounds (B) it is possible to use all hydrogen-functional organosilicon compounds which have also been used hitherto in addition-crosslinkable compositions.
[0043] As the organopolysiloxane (B) containing Si-bonded hydrogen atoms, it is preferred to use a linear, cyclic or branched organopolysiloxane composed of units of the general formula (III):
[0044] R 4 c H d SiO (4-c-d) / 2 (III)
[0045] in
[0046] R 4 With the definitions shown above,
[0047] c is 0, 1, 2, or 3, and
[0048] d is 0, 1, or 2,
[0049] The conditions are that the sum of c+d is less than or equal to 3 and there are at least two Si-bonded hydrogen atoms per molecule.
[0050] The organopolysiloxane (B) used in the present invention preferably contains 0.04 to 1.7 weight % (wt %) of Si-bonded hydrogen based on the total weight of the organopolysiloxane (B).
[0051] The molecular weight of component (B) may vary within a wide range, for example, between 10 2 and 10 6 Thus, for example, component (B) may be a relatively low molecular weight SiH-functional oligosiloxane such as tetramethyldisiloxane, or a high polymer polydimethylsiloxane having SiH groups in the chain or at the ends, or a silicone resin containing SiH groups.
[0052] The structure of the molecules forming component (B) is likewise not fixed; in particular, the structure of relatively high molecular weight SiH-containing siloxanes, i.e. oligomeric or polymeric SiH-containing siloxanes, can be linear, cyclic, branched or resinous or network-like. Linear and cyclic polysiloxanes (B) are preferably of the formula R 4 3SiO 1 / 2 , HR 4 2SiO 1 / 2 , HR 4 SiO 2 / 2 and R 4 2SiO 2 / 2 The unit composition is R 4 The branched and network polysiloxanes further comprise trifunctional and / or tetrafunctional units, preferably of the formula R 4 SiO 3 / 2 ,HSiO 3 / 2 and SiO 4 / 2 Those, among which R 4 Has the definition shown above.
[0053] Of course, mixtures of different siloxanes which meet the criteria for component (B) can also be used. Particular preference is given to using low molecular weight SiH-functional compounds, such as tetrakis(dimethylsiloxy)silane and tetramethylcyclotetrasiloxane, and higher molecular weight SiH-containing siloxanes, such as siloxanes having a kinematic viscosity of 1 to 20 000 mm2 at 25° C. according to DIN 53019. 2 / s, preferably 10 to 1000 mm 2 / s poly(hydrogen methyl) siloxane and poly(dimethyl hydrogen methyl) siloxane, or similar SiH-containing compounds in which some methyl groups have been substituted with 3,3,3-trifluoropropyl or phenyl groups.
[0054] Component (B) is preferably present in the crosslinkable silicone elastomer composition X in such an amount that the molar ratio of SiH groups to aliphatically unsaturated groups from (A) is 0.1 to 20, more preferably 0.3 to 5.0, particularly preferably 0.6 to 2.
[0055] Components (A) and (B) used in the present invention are commercially commonly used products and / or can be prepared by commonly used methods in chemistry.
[0056] Instead of components (A) and (B), the silicone elastomer composition may comprise an organopolysiloxane (C) which contains both aliphatic carbon-carbon multiple bonds and Si-bonded hydrogen atoms. The silicone elastomer composition X may also comprise all three components (A), (B) and (C).
[0057] Siloxanes (C), if used, are preferably those consisting of units of the general formulae (IV), (V) and (VI)
[0058] R 4 f SiO 4 / 2 (IV)
[0059] R 4 g R 5 SiO 3-g / 2 (V)
[0060] R 4 h HSiO 3-h / 2 (VI)
[0061] in
[0062] R 4 and R 5 With the definitions shown above for them
[0063] f is 0, 1, 2, or 3,
[0064] g is 0, 1, or 2, and
[0065] h is 0, 1, or 2,
[0066] The condition is that each molecule has at least 2 groups R 5 At least 2 Si-bonded hydrogen atoms.
[0067] Examples of the organopolysiloxane (C) are SiO 4 / 2 , R 4 3SiO 1 / 2 , R 4 2R 5 SiO 1 / 2 and R 4 2HSiO 1 / 2 Those composed of units are called MP resins. These resins may additionally contain R 4 SiO 3 / 2 and R 4 2SiO units; and substantially R 4 2R 5 SiO 1 / 2 , R 4 2SiO and R 4 A linear organopolysiloxane composed of HSiO units, wherein R 4 and R 5 Having the definitions given above.
[0068] The organopolysiloxane (C) preferably has a molecular weight of 0.01 to 500,000 mm 2 / s, more preferably 0.1 to 100 000 mm 2 / s, particularly preferably 1 to 10000 mm 2 DIN 53019 kinematic viscosity of 200 Å / s, measured in each case at 25° C. The organopolysiloxanes (C) can be prepared by the techniques customary in chemistry.
[0069] As hydrosilylation catalyst (D), all catalysts known in the prior art can be used. Component (D) can be a platinum group metal (e.g., platinum, rhodium, ruthenium, palladium, osmium or iridium), an organometallic compound, or a combination thereof. Examples of component (D) are compounds such as hexachloroplatinic (IV) acid, platinum dichloride, platinum acetylacetonate, and complexes of the compounds encapsulated in a matrix or a core-shell structure. Low molecular weight platinum complexes of organopolysiloxanes include complexes of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane and platinum. Other examples are platinum phosphite complexes or platinum phosphine complexes. For photocurable or UV-curable compositions, for example, derivatives of alkyl platinum complexes such as cyclopentadienyl trimethyl platinum (IV), cyclooctadienyl dimethyl platinum (II), or diketone complexes such as bis-acetylacetonate platinum (II) can be used to initiate addition reactions with the aid of light. These compounds can be encapsulated in a resin matrix.
[0070] Component D is preferably used in a concentration of 0.1 to 1000 parts per million (ppm), more preferably 0.5 to 100 ppm, particularly preferably 1 to 25 ppm, based in each case on the weight of the platinum group metal and the crosslinkable silicone elastomer composition X.
[0071] If the platinum group metal component is present at less than 1 ppm, the curing speed may be low. Using more than 100 ppm of the platinum group metal is uneconomical or may reduce the storage stability of the silicone elastomer composition X.
[0072] The reinforcing filler F is preferably selected from 2 / g BET surface area of pyrogenic or precipitated hydrophobic silica, and carbon black and activated carbon (such as furnace black and acetylene black), and silicone resins, preferably silicone resin F and having a BET surface area of at least 50m 2 Pyrogenic or precipitated hydrophobic silicas having a BET surface area according to DIN 66131 and DIN 66132 (determined with nitrogen) of 1.1 g / g, or mixtures thereof, are used as reinforcing fillers F.
[0073] Examples of silicone resins F are MQ, MT, MDQ, MDT, MTQ and MDTQ silicone resins, wherein M is selected from R3SiO 1 / 2 and HR2SiO 1 / 2 and R 1 R2SiO 1 / 2 , D is selected from R 1 R 1 / 2 and R2SiO 1 / 2 and HRSiO 1 / 2 , T is selected from RSiO 3 / 2 and R 1 SiO 3 / 2 and HSiO 3 / 2 , Q contains SiO 4 / 2 Unit, where R has the above R 4 The definition of R 1 With R 5 Definition of .
[0074] Preferred fumed and precipitated hydrophobic silicas have a diameter of 50 to 800 m 2 / g, more preferably 100 to 500 m 2 / g, particularly preferably 150 to 400 m 2 Particular preference is given to using as solid F pyrogenic hydrophobic silicas having a BET surface area of 150 to 400 m2 / g.
[0075] The reinforced solid F is preferably surface treated and thus hydrophobic. Due to the surface treatment, the preferred solid F has a carbon content of at least 1.5 to no more than 20% by weight, preferably 1.8 to 10% by weight, more preferably 2 to 8% by weight. Particularly preferred are surface treated silicas containing 3 to 6% by weight of Si-bonded aliphatic groups. These groups are, for example, Si-bonded methyl or vinyl groups. Hydrophobic silicas suitable as solid F are characterized in that they are substantially not wetted by water. This means that in the present invention the methanol value of the solid F is greater than 40, preferably greater than 50.
[0076] Hydrophobizing silica is already known to those skilled in the art. Solid F can be hydrophobized in a separate operating step or in situ hydrophobized by adding a suitable hydrophobizing agent to the silicone elastomer composition X. The techniques for surface treatment and hydrophobization of silica are known to the skilled person. Hydrophobization can preferably be carried out by halogen-free silanes, such as described in EP1433749A1.
[0077] An example of a commercially available hydrophobic silica is a silica loaded with -[Si(CH3)2-O] n Partial H18 and H20, loaded with –O-Si(CH3)3 H2000 (commercially available from Wacker Chemie AG, Munich), and 972 and 805 (commercially available from Evonik Degussa GmbH, Frankfurt am Main).
[0078] In a preferred embodiment, the solid F comprises a silicone resin F, more particularly an MDT or MQ resin, preferably an MQ resin. Preferred MQ resins contain less than 10 mol %, preferably less than 2 mol %, particularly preferably less than 0.5 mol % of D or T units. Particularly preferred MQ resins are substantially free of D or T units.
[0079] The silicone resin F is preferably solid at 25° C. and at the pressure of the surrounding atmosphere, ie 1013 hPa.
[0080] Silicone resin F is preferably a resin having a molecular weight Mw of at least 500, preferably at least 900, more preferably at least 1200, and at most 15000, preferably at most 10000, more preferably at most 8000, with a polydispersity of at most 20, preferably at most 18, more preferably at most 16, more particularly at most 15.
[0081] Molecular weight distribution:
[0082] The molecular weight distribution is determined as weight average Mw and number average Mn using the gel permeation chromatography (GPC or size exclusion chromatography (SEC)) technique with polystyrene standards and a refractive index detector (RI detector). Unless otherwise stated, THF is used as eluent and DIN 55672-1 is used. The polydispersity is the ratio Mw / Mn.
[0083] Preferred silicone resins F contain at least 1 mol %, preferably at least 2 mol %, of a group consisting of R 1 R2SiO 1 / 2 , R 1 R 1 / 2 and R 1 SiO 3 / 2 Unit of unit, preferably R 1 R2SiO 1 / 2 unit.
[0084] The silicone resin F preferably contains 0.1 to 10% by weight, more preferably 0.5 to 8% by weight, very preferably 1 to 6% by weight, of alkoxy groups as radicals R. Particularly suitable and therefore preferred are methoxy, ethoxy, isopropoxy and tert-butoxy groups.
[0085] Preferred radicals R are saturated aliphatic radicals, preferably methyl, ethyl and isooctyl, more preferably methyl.
[0086] Preferred groups R 1 It is an unsaturated aliphatic group, preferably a vinyl group.
[0087] Particularly preferred as filler F are MQ resins which contain vinyl groups and contain 45 to 65 mol %, preferably 50 to 60 mol %, of Q units and 30 to 50 mol %, preferably 35 to 45 mol % of M units of the form R3SiO 1 / 2 , and 2 to 10 mol %, preferably 3 to 8 mol %, of M units of the form R 1 R2SiO 1 / 2 , wherein R is preferably methyl and R 1 Vinyl is preferred.
[0088] In the crosslinkable silicone elastomer composition X, the reinforcing filler F is preferably used as an individual filler F or likewise preferably as a mixture of two or more fillers F.
[0089] The silicone elastomer composition X together with the reinforcing filler F forms a mixture B.
[0090] Per 100 parts by weight of the crosslinkable silicone elastomer composition X, the mixture B contains preferably 5 to 200 parts by weight, more preferably 10 to 100 parts by weight, particularly preferably 15 to 50 parts by weight, of reinforcing filler F.
[0091] In addition to the reinforcing fillers F, the mixture B may also contain non-reinforcing fillers. Examples of non-reinforcing fillers are 2 / g BET surface area fillers such as quartz, diatomaceous earth, calcium silicate, zirconium silicate, zeolite, metal oxide powders (such as aluminum oxide, titanium oxide, iron oxide or zinc oxide and / or mixed oxides thereof), barium sulfate, calcium carbonate, gypsum, silicon nitride, silicon carbide, boron nitride, glass powder and plastic powder.
[0092] In addition to at least one siloxane or silane, the droplets may further comprise a component B selected from the group consisting of catalysts, fillers, inhibitors, thermal stabilizers, solvents, plasticizers, color pigments, sensitizers, photoinitiators, adhesion promoters, and the like.
[0093] The silicon dioxide S preferably comprises partially water-wettable pyrogenic and precipitated silicon dioxides or mixtures thereof having a BET specific surface area of 30 to 500 m2 / g, more preferably 100 to 300 m2 / g, wherein pyrogenic silicon dioxide is particularly preferred. The BET surface area is measured according to known methods, preferably according to Deutsche Industrie Norm [German Industrial Standard] DIN 66131 and DIN 66132.
[0094] Silicon dioxide S is preferably surface treated with a suitable hydrophobizing agent, and the result is hydrophobic. Hydrophobization is carried out so that the silicon dioxide S is still partially wettable by water. This means that the methanol value of silicon dioxide S is less than 40, preferably less than 30 in the present invention. Due to surface treatment, preferred silicon dioxide S has a carbon content of at least 0.2 to no more than 1.5 weight %, preferably 0.4 to 1.4 weight %, more preferably 0.6 to 1.3 weight %. Hydrophobic groups are methyl or vinyl groups such as Si bonding. The hydrophobization technology of silicon dioxide is well known to those skilled in the art.
[0095] Preferred silicon dioxide S is silanized pyrogenic silicon dioxide having a methanol number of less than 30.
[0096] Particularly preferred are partially water-wettable silicas as described in EP 1433749 A1 and DE 10349082 A1.
[0097] The average particle size of the granular solid F or, where appropriate, of the aggregate of particles is preferably smaller than the average diameter d of the liquid droplets without finely divided particles. 50 .
[0098] The average particle size of the granular solid F is less than 1000 nm, preferably between 10 nm and 800 nm, more preferably between 50 nm and 500 nm, very preferably between 75 nm and 300 nm, in each case measured as the average hydrodynamic equivalent diameter by photon correlation spectroscopy in 173° backscattering using a Nanosizer ZS from Malvern.
[0099] To determine the methanol value, defined mixtures of water and methanol were prepared and the surface tension of these mixtures was then determined using known techniques. In a separate experiment, these water-methanol mixtures were covered with a defined amount of particles and shaken under defined conditions (e.g., gently shaken by hand or with a drum mixer for about 1 minute). The determination was performed on water-alcohol mixtures in which the particles had not yet sunk, and on water-alcohol mixtures with a higher alcohol content in which the particles had just sunk. The surface tension of the latter alcohol-water mixture provides the critical surface energy γ crit , as a measure of the particle surface energy γ. The methanol content in water gives the methanol value.
[0100] The reinforcing filler F is preferably more hydrophobic than the silica S.
[0101] The particles P preferably have a dimension x50 of 1 to 100 mm, preferably 2 to 50 mm, more preferably, in particular 3 to 20 mm, more particularly 3 to 8 mm.
[0102] The particles P are amphiphilic, which means that they are both hydrophilic (i.e. water-loving) and lipophilic (i.e. fat-loving). This means that the particles P are easily dispersible not only in polar solvents, such as water or alcohols, but also in non-polar solvents, such as aliphatic hydrocarbons or polydimethylsiloxane oils, without the addition of further dispersing aids or additives, such as organic emulsifiers or other surface-active substances. This is a significant advantage of the particles P compared to uncoated silicone elastomer particles, which are very hydrophobic and non-dispersible in polar solvents, such as water or alcohols, without the use of unnecessary auxiliaries such as organic emulsifiers. In the case of the particles P, the silica S is firmly bound to the surface and therefore remains amphiphilic when dispersed in the solvent. This is a significant advantage over silicone elastomer particles according to the prior art, which are post-treated with silica after curing, since in the case of such particles not according to the invention the absorbed silica is not permanently bound. One disadvantage of these particles according to the prior art is that, when dispersing the particles in a solvent, the non-permanently bound silica detaches completely or partially, causing the particles to become highly hydrophobic and rendering them no longer dispersible in polar solvents such as water.
[0103] The present invention further provides a process for producing particles P consisting of a core K comprising a crosslinked silicone elastomer composition X and a reinforcing filler F and a shell H of silica S, wherein in a first step, a dispersion A comprising silica S and water is mixed with a mixture B comprising a crosslinkable silicone elastomer composition X and a reinforcing filler F to obtain a continuous phase comprising water and a discontinuous phase comprising the crosslinkable silicone elastomer composition X and the reinforcing filler F, and in a second step, the discontinuous phase is crosslinked to obtain particles P.
[0104] The continuous phase does not change during the crosslinking process of the second step.
[0105] The continuous phase preferably comprises at least 80% by weight, more particularly at least 90% by weight, of water.
[0106] Preferably, a three-phase mixture (Pickering emulsion) of an emulsion containing a sparingly water-soluble and water-immiscible silicone elastomer composition X stabilized in an aqueous phase by partially hydrophobized silica is formed. The silicone elastomer composition X is crosslinked after emulsification in a method suitable for producing particles P. If they contain, for example, alkoxy- or acetoxy-substituted silanes or siloxanes, it may be necessary to hydrolyze the condensable silicone elastomer composition X. If the silicone composition X is sufficiently reactive, the water present is sufficient to optionally cause hydrolysis and subsequent condensation. In the case of a less reactive silicone elastomer composition X, a catalyst is required that optionally causes hydrolysis and condensation of siloxanes and silanes. These catalysts may be acids and may be bases or metal catalysts, such as group IV transition metal catalysts, tin catalysts of the type commonly used to accelerate hydrolysis, condensation reactions or transesterification reactions. In addition to known inorganic acids and metal salts, suitable acids or bases also include acidic or basic silanes or siloxanes.
[0107] Preferred basic catalysts are NaOH, KOH, ammonia and NEt3.
[0108] Preferred acidic catalysts are p-toluenesulfonic acid, aqueous or gaseous HCl, sulfuric acid.
[0109] If the process involves a polymerisation reaction, the reaction may be, for example, a free radical polymerisation of an ethylenically unsaturated siloxane or silane.
[0110] In a particular embodiment, for example a transition metal catalyst, such as a platinum catalyst, is added to mixture B, especially when it comprises siloxanes which are capable of reacting with one another in a hydrosilylation reaction.
[0111] The method will be carried out in such a way in the second step that the silica S which stabilizes the discontinuous phase reacts with the surface of the mixture B forming the core during crosslinking, or at least enters into a stabilizing interaction (such as hydrogen bonds, van der Waals interactions) or another directional interaction with said surface, or a combination of these directional interactions, so that the silica S is permanently anchored on the core formed by the mixture B.
[0112] For example, the size of the particles P can be controlled by the emulsification technique, i.e., for example, by variables such as the introduced shear energy, the volume fraction of the mixture B, the amount of silica S, the pH of the continuous aqueous phase and its ionic strength, the viscosity, the metering sequence, the metering rate, or by the reaction scheme, i.e., for example, by the reaction temperature, the reaction time, the concentration of the raw materials used. The choice and amount of any hydrolysis and condensation catalyst used also has an influence on the particle size.
[0113] When using emulsification techniques which allow relatively small droplets to be produced, the process produces small surface-structured particles P. To this end, for example, different shear energies or different choices of silica S can be used to stabilize the mixture B in water.
[0114] The reinforcing filler F and optionally non-reinforcing fillers or optional further ingredients are preferably mixed homogeneously with the silicone elastomer composition X in a first step before the mixture B is emulsified with the dispersion A in a further step and subsequently crosslinked to form the particles P. This ensures that all fillers and optional further ingredients are located inside the droplets as part of the mixture B after emulsification and inside the core K of the particle P after crosslinking.
[0115] The Pickering emulsion E of mixture B is preferably substantially free of conventional liquid and solid organic surface-active substances which are non-particulate at room temperature and at the surrounding atmospheric pressure, such as nonionic, cationic and anionic emulsifiers ("organic emulsifiers").
[0116] Organic emulsifiers here do not refer to particles and colloids, but rather molecules and polymers that meet the definitions of molecules, polymers, colloids and particles given in Dispersionen und Emulsionen [Dispersions and Emulsions], G. Lagaly, O. Schulz, R. Zindel, Steinkopff, Darmstadt 1997, ISBN 3-7985-1087-3, pp. 1-4.
[0117] Typically, these organic emulsifiers have a size of less than 1 nm, a molar mass of <10 000 g / mol, a carbon content of >50% by weight, determinable by elemental analysis, and a Mohs hardness of less than 1.
[0118] At the same time, the emulsions of the invention are substantially free of organic emulsifiers which generally have a solubility of greater than 1% by weight in water at 20° C. and the pressure of the surrounding atmosphere (ie 900 to 1100 hPa) in homogeneous or micellar form.
[0119] The Pickering emulsion E of mixture B may contain a maximum concentration of such organic emulsifiers that is less than 0.1 times, preferably less than 0.01 times, more preferably less than 0.001 times, more particularly less than 0.0001 times the critical micelle concentration of these organic emulsifiers in the aqueous phase; this corresponds to a concentration of these organic emulsifiers of less than 10% by weight, preferably less than 2% by weight, more preferably less than 1% by weight, more particularly 0% by weight, based on the total weight of the dispersion of the invention.
[0120] To produce the particle-stabilized Pickering emulsion E in the first step, all techniques known to the skilled person for producing the emulsion can be used. However, it has emerged that a particularly suitable emulsion for producing the particles P can be obtained according to the following method:
[0121] Method 1:
[0122] Initial introduction of a highly concentrated dispersion A in a volume such that it comprises the total amount of silicon dioxide S desired and only a partial amount of water.
[0123] The total volume of mixture B is slowly metered in with continuous homogenization, for example by means of a high-speed stirrer, a high-speed dissolver or a rotor-stator system.
[0124] - optionally with continuous homogenization by means of, for example, a high-speed stirrer, a high-speed dissolver or a rotor-stator system, the desired remaining volume of water is then slowly metered in.
[0125] Method 2:
[0126] Initial introduction of dispersion A in a volume such that it comprises the desired total amounts of silica S and water.
[0127] The total volume of mixture B is slowly metered in with continuous homogenization, for example by means of a high-speed stirrer, a high-speed dissolver, a rotor-stator system or by means of a capillary emulsifier.
[0128] Method 3:
[0129] - The total volume of mixture B is initially introduced.
[0130] - Slow metering of the highly concentrated dispersion A with continuous homogenization, for example by means of a high-speed stirrer, a high-speed dissolver or a rotor-stator system, in a volume such that it comprises the desired total amount of silicon dioxide S and only a partial amount of water.
[0131] - optionally with continuous homogenization by means of, for example, a high-speed stirrer, a high-speed dissolver or a rotor-stator system, the desired remaining volume of water is then slowly metered in.
[0132] Method 4:
[0133] - The total volume of mixture B is initially introduced.
[0134] Dispersion A is slowly metered in, with continuous homogenization by means of, for example, a high-speed stirrer, a high-speed dissolver or a rotor-stator system, in a volume such that it comprises the desired total amount of silicon dioxide S and only a partial amount of water.
[0135] Method 5:
[0136] - Initially introducing a total volume of mixture B and dispersion A such that it contains the desired total amounts of silica S and water.
[0137] - Combined homogenization by means of, for example, high-speed stirrers, high-speed dissolvers or rotor-stator systems.
[0138] Method 6:
[0139] - Initial introduction of a total volume of mixture B and highly concentrated dispersion A, the volume initially introduced being such that it comprises the total amount of silicon dioxide S desired and a partial amount of water.
[0140] - Combined homogenization by means of, for example, high-speed stirrers, high-speed dissolvers or rotor-stator systems.
[0141] - optionally with continuous homogenization by means of, for example, a high-speed stirrer, a high-speed dissolver or a rotor-stator system, the desired remaining volume of water is then slowly metered in.
[0142] Methods 1, 2, 5 and 6 are preferred, among which methods 2 and 5 are particularly preferred, and method 5 is especially preferred.
[0143] Homogenization is preferably carried out in at least one process step for at least 30 seconds, preferably at least 1 minute.
[0144] The preparation of the dispersion A of silicon dioxide S in water which forms the homogeneous phase in the emulsion according to the invention can in principle be carried out according to known methods for preparing particle dispersions, such as incorporation using stirring elements with high shearing action, such as high-speed stirrers, high-speed dissolvers, rotor-stator systems, ultrasonic dispersers or ball mills or bead mills.
[0145] The concentration of silicon dioxide S in dispersion A here is between 1 and 80% by weight, preferably between 10 and 60% by weight, more preferably between 10 and 40% by weight, very preferably between 12 and 30% by weight.
[0146] In an optional process step, the Pickering emulsion E is diluted with water, optionally with continuous homogenization by means of, for example, a high-speed stirrer, a high-speed dissolver or a rotor-stator system.
[0147] The process described can be carried out in a continuous form or in a discontinuous form. The continuous form is preferred.
[0148] The temperature in the first step is between 0°C and 80°C, preferably between 10°C and 50°C, more preferably between 20°C and 40°C.
[0149] The emulsification operation can be carried out at atmospheric pressure (in other words, at 900 to 1100 hPa), at elevated pressure or at reduced pressure. Operation at atmospheric pressure is preferred.
[0150] The concentration of silicon dioxide S in the three-phase mixture comprising dispersion A and mixture B from the first step is between 1 and 80% by weight, preferably between 2 and 50% by weight, more preferably between 3 and 30% by weight, particularly preferably between 4 and 20% by weight.
[0151] The concentration of the silicone elastomer composition X in the three-phase mixture comprising dispersion A and mixture B from the first step is between 1 and 80% by weight, preferably between 20 and 76% by weight, more preferably between 40 and 72% by weight, particularly preferably between 50 and 70% by weight.
[0152] The concentration of water in the three-phase mixture comprising dispersion A and mixture B from the first step is between 5 and 80% by weight, preferably between 10 and 70% by weight, more preferably between 15 and 60% by weight, particularly preferably between 20 and 40% by weight.
[0153] Starting from the above three-phase mixture, particles P can be obtained in a second step by the following method:
[0154] The three-phase mixture is preferably diluted by adding water to a mass fraction of water of 50% to 90% by weight, more preferably 40% to 80% by weight.
[0155] In the second step, the three-phase mixer is preferably agitated with low shear action, for example by means of a slow dissolver, rotor-stator or beam stirrer, until internal crosslinking of the particles P is complete, or by shaking with suitable components.
[0156] The duration of the second process step is preferably shorter than 120 hours, more preferably between 0 hours and 48 hours, very preferably between 0.1 hours and 24 hours and in a specific embodiment, between 0.25 hours and 12 hours.
[0157] The three-phase mixture of dispersion A and mixture B from the first step can optionally be mixed with a catalyst that accelerates and completes crosslinking as described above. This addition can be made directly to the discontinuous phase or the continuous phase before preparing the three-phase mixture; during emulsification, or subsequently, to the completed three-phase mixture.
[0158] The amount of any catalyst added is within the typical quantitative range for catalysts.
[0159] The reaction temperature during the crosslinking stage is between 0°C and 100°C, preferably between 10°C and 80°C, more preferably between 15°C and 60°C.
[0160] The reaction can optionally be carried out under an inert gas atmosphere such as nitrogen, argon or carbon dioxide. In that case, the oxygen fraction is less than 15% by volume, preferably less than 10% by volume, more preferably less than 5% by volume.
[0161] The pH of the reaction mixture is between pH 10 and 1, preferably between pH 9 and 3, more preferably between pH 8 and 4, and in a specific embodiment, between pH 7 and 5.
[0162] The three-phase mixture may optionally be mixed with a water-soluble organic solvent such as an alcohol (e.g. methanol, ethanol or isopropanol) or a ketone (such as acetone or MEK) or an ether (such as THF) or others. These may be added in the first step or before or during the second step.
[0163] The three-phase mixture can optionally be mixed with dispersing aids, protective colloids and / or surfactants. These can be added in the first step or before or during the second step.
[0164] The three-phase mixture contains preferably less than 5 wt. %, more preferably less than 1 wt. %, more particularly less than 0.1 wt. % of dispersing aids, protective colloids and surfactants. In a specific embodiment, the three-phase mixture is free of dispersing aids, protective colloids and surfactants.
[0165] The three-phase mixture optionally contains inorganic or organic electrolytes. These can be added after the first step, during the second step or after the second step has ended.
[0166] In this case, the ionic strength of the three-phase mixture is between 0.01 mmol / l and 1 mol / l, preferably between 0.1 mmol / l and 500 mmol / l, more preferably between 0.5 mmol / l and 100 mmol / l.
[0167] The surface of the particles P can optionally be modified by treatment with reactive silanes or siloxanes. These can be added directly after the preparation of the Pickering emulsion in the first step, during the reaction phase, or after the reaction phase in the second step, before the separation of the particles P, or after the separation of the particles in the liquid or solid phase. This treatment should be carried out so that the silanes or siloxanes are covalently chemically attached to the particles. The corresponding techniques and methods are known to the person skilled in the art.
[0168] The solids fraction of particles P in the three-phase mixture consisting of all solids used and polymerization products of materials capable of addition polymerization, condensation polymerization or chain polymerization is between 5% and 70% by weight, preferably between 10% and 50% by weight, more preferably between 20% and 40% by weight.
[0169] After the second step, the three-phase mixture can optionally be stored, still with stirring. This can be achieved, for example, by a beam stirrer or an anchor stirrer.
[0170] In a preferred embodiment, the particles P are separated, preferably by sedimentation, filtration or centrifugation, more preferably by filtration or centrifugation, very preferably by centrifugation.
[0171] After they have been separated, the particles P are preferably washed with a washing liquid preferably selected from completely deionized water, methanol, ethanol and mixtures thereof.
[0172] In a preferred embodiment, the particles P are separated from the aqueous phase in powder form. This can be achieved, for example, by filtering, settling, centrifuging or by drying in an oven or dryer or by spray drying or by removing volatile components by applying an appropriate reduced pressure.
[0173] By spray drying, particles P of very high fineness can be obtained without further processing. The particles P dried by static drying tend to form loose agglomerates which can be deagglomerated by suitable grinding methods, for example by ball milling or air jet milling.
[0174] Measurement method
[0175] - Solid content: 10 g of the aqueous dispersion was mixed with an equal amount of ethanol in a porcelain dish and evaporated to constant weight at 150° C. in a drying oven purged with N 2 . s *100 / 10g, mass of dry residue m SThe solids content is given.
[0176] -Average particle size (x50):
[0177] d 50 The determination was carried out using a Camsizer X2 from Retsch Technology (measuring principle: dynamic image analysis according to ISO 13322-2, measuring range: 0.8 μm-30 mm, analysis type: dry measurement of powders and granules, dispersion pressure = 2 bar).
[0178] - Carbon content %C determined by carbon elemental analysis; the sample is burned at above 1000°C in an O2 stream and the resulting CO2 is detected and quantified by IR; Instrument: LECO 244
[0179] - Methanol value: To determine the methanol value, defined mixtures of water and methanol are prepared. In a separate experiment, these water-methanol mixtures are covered with equal volumes of dry particles and shaken under defined conditions (e.g. gently shaken by hand or with a drum mixer for about 1 minute). The determination is carried out for a water-alcohol mixture in which the particles have not yet sunk, and for a water-alcohol mixture with a higher alcohol content in which the particles have just sunk. The latter methanol content in the water gives the methanol value.
[0180] - Kinematic viscosity is measured at 25°C according to DIN 53019.
[0181] In the following examples, all amounts and percentages are by weight, all pressures are 0.10 MPa (absolute pressure) and all temperatures are 20° C. in each case unless otherwise specified. Example
[0182] Example 1: Preparation of Silicon Dioxide Aqueous Dispersion A
[0183] 1300 g of a molten salt having a BET specific surface area of 200 m 2 / g of hydrophilic starting silica (named N20 from Wacker-Chemie GmbH, Munich) with dimethyldichlorosilane according to EP 1433749 A1, partially hydrophobic fumed silica having a residual silanol content of 71% and a carbon content of 0.95% was added in portions with stirring to 5200 g of completely demineralized (FD) water. After complete addition of the silica, dispersion was continued at 650 rpm for a further 60 minutes. This gave a high-viscosity dispersion with a solids content of 20% and a pH of 4.2.
[0184] Example 2: General procedure for mixing dispersion A comprising silicon dioxide S and water with mixture B using a dissolver
[0185] Step 1: The silica dispersion described in Example 1 is weighed into a suitable stirred container and stirred at 6000 rpm for 10 minutes using a Labo-Top planetary dissolver from PC Laborsystem, CH. The viscosity of the dispersion decreases. FD water is optionally added and mixed evenly. The mixed silicone oil component prepared according to one of Examples 5, 6 or 7 is added to the stirred silica dispersion and homogenized in the dissolver at 6000 rpm with a water coolant for 10 minutes. During this period, the temperature of the mixture should not rise more than 35° C. The result is a white substance with high viscosity.
[0186] Step 2: Dilute the high viscosity material from process step 1 to 30% silicone oil content at 1000 rpm by adding FD water in three equal portions. Stir at 1000 rpm for 3 minutes after each portion of FD water. This produces a highly fluid white O / W emulsion.
[0187] Example 3: General procedure for mixing dispersion A comprising silica S and water with mixture B using an Ultra-Turrax
[0188] Step 1: The silica dispersion described in Example 1 is weighed into a suitable 1000 ml / l stainless steel container and stirred at 10000 rpm for 10 minutes using an Ultra-Turrax T50. The viscosity of the dispersion decreases. FD water is optionally added and mixed evenly. The mixed silicone oil component prepared according to one of Examples 5, 6 or 7 is added to the stirred silica dispersion and then homogenized at 10000 rpm for 10 minutes using an Ultra Turrax with ice cooling. During this period, the temperature of the mixture should not rise more than 35°C. The result is a white substance with high viscosity.
[0189] Step 2: Dilute the high viscosity material from step 1 to 30% silicone oil content by adding FD water in three equal portions. Stir at 6000 rpm for 3 minutes after each portion of FD water. This produces a highly fluid white O / W emulsion.
[0190] Example 4: General procedure for producing silica-coated silicone elastomer microparticles P of the present invention from a Pickering emulsion of mixture B
[0191] 250 g of the polyaddition-polymerizable Pickering emulsion prepared according to Example 2 or Example 3 was mixed with 20 ppm of a polyaddition-polymerizable emulsion having a viscosity of 1000 mm 2 / s (25 ° C) of a vinyl-containing polydimethylsiloxane (in which both chain ends are terminated by dimethylvinylsilyl groups) in the form of a 1% by weight solution of Karstedt catalyst (based on the amount of platinum), and the mixture is stirred at 80 ° C for 24 hours. The result is a white, highly fluid dispersion. For isolation, particles P are removed by filtration and dried in a drying cabinet at 80 ° C for 24 hours. This produces a fine white powder.
[0192] Example 5: Silicone Resin Reinforced Mixture B Capable of Addition Polymerization
[0193] Using a paddle stirrer, 375 g of a 1000 mm 2 / s (25°C) of vinyldimethylsiloxy-terminated polydimethylsiloxane and 264g of viscosity of 20 000mm 2 / s (25°C) of vinyldimethylsiloxy-terminated polydimethylsiloxane were uniformly mixed. Then 274 g of [Me3SiO 1 / 2 ] 26.65 [ViMe2SiO 1 / 2 ] 3.72 [SiO 4 / 2 ] 42.78 [HO 1 / 2 ] 1.02 [EtO 1 / 2 ] 5.93 The base substance thus obtained was uniformly mixed with 114 g of a copolymer consisting of dimethylsiloxy, methylhydrogensiloxy and trimethylsiloxy units, the copolymer having a molecular weight of 40 mm 2 / s at a viscosity of 25°C and a SiH content of 0.40%.
[0194] Example 6: Production of Silica-Coated Silicone Resin-Reinforced Silicone Elastomer Particles P
[0195] 320 g of the inventive mixture B from Example 5 and 240 g of the aqueous silicon dioxide dispersion A from Example 1 were emulsified as in Example 2. Subsequently, as in Example 4, pulverulent silicone elastomer particles P having an average particle size of d50=3.4 mm were produced.
[0196] Example 7: Silica-reinforced mixture B capable of undergoing addition polymerization
[0197] Initially introduced in a commercial laboratory kneader 917 g with a viscosity of 1000 mm 2 / s (25 ° C) of vinyl dimethylsiloxy-terminated polydimethylsiloxane, which was heated to 150 ° C and mixed with 621 g of a specific surface area of 125 m 2 / g (measured by the BET method) and a carbon content of 1.6-2.0% by weight of hydrophobic fumed silica. This gives a high-viscosity mass, which is subsequently diluted with 618 g of the above-mentioned polydimethylsiloxane. Kneading at 150° C. under reduced pressure (10 mbar) frees the resulting mass from water and excess residues of fillers (especially volatile components) within one hour. 123 g of a 100 mm thick slurry of 100 mm thick is then added. 2 A copolymer composed of dimethylsiloxy, methylhydrogensiloxy and trimethylsiloxy units having a viscosity of 0.147 / s at 25° C. and an SiH content of 0.47% was prepared and uniformly mixed.
[0198] Example 8: Production of Silica-Coated Silica-Reinforced Silicone Elastomer Particles P
[0199] 156 g of the inventive mixture B from Example 7 and 149 g of the aqueous silicon dioxide dispersion A from Example 1 were emulsified as in Example 3. Subsequently, as in Example 4, pulverulent silicone elastomer particles P having an average particle size of d50=12 mm were produced.
[0200] Comparative Example C1: Silicone elastomer composition capable of addition polymerization without reinforcing filler
[0201] Without adding reinforcing additives, 1535 g of a viscosity of 1000 mm 2 / s (25°C) of vinyl-containing polydimethylsiloxane (wherein both chain ends are capped with dimethylvinylsilyl groups) and 123 g of 100 mm 2 A copolymer composed of dimethylsiloxy, methylhydrogensiloxy and trimethylsiloxy units having a viscosity of 1000 g / s at 25° C. and an SiH content of 0.47% was uniformly mixed.
[0202] Comparative Example C2: Production of silica-coated silicone elastomer particles without reinforcing filler
[0203] According to Example 2, 320 g of the silicone elastomer composition not according to the invention from Comparative Example C1 and 240 g of the aqueous silicon dioxide dispersion from Example 1 were emulsified. Subsequently, according to Example 4, pulverulent silicone elastomer particles P having an average particle size of d50=18 mm were produced.
[0204] Comparative Example C3: Silicone elastomer composition capable of addition polymerization without reinforcing filler
[0205] Without adding reinforcing additives, 479 g of a 200 mm viscosity 2 / s (25°C) of a vinyl-containing polydimethylsiloxane (wherein both chain ends are capped with dimethylvinylsilyl groups) and 21% by weight of a viscosity of 65 mm 2 / s (25°C) of a trimethylsilyl-terminated methylhydrogensiloxane-dimethylsiloxane copolymer containing 0.73 wt% of Si-bonded hydrogen.
[0206] Comparative Example C4: Production of silica-coated silicone elastomer particles without reinforcing filler
[0207] 320 g of the silicone elastomer composition not according to the invention from comparative example C3 and 240 g of the aqueous silicon dioxide dispersion from example 1 were emulsified according to example 2. Subsequently, according to example 4, pulverulent silicone elastomer particles P having an average particle size of d50=9 mm were produced.
[0208] Example 9: Sensory Evaluation of Granules P
[0209] A sensory evaluation of the inventive silica-coated silicone elastomer particles P from Examples 6 and 8 and the particles not according to the invention from Comparative Examples C2 and C4 was carried out by a trained panel of five testers.
[0210] For evaluation, the testers washed their hands and lower arms with soap and water. On the lower arms, a circular test area with a diameter of 4 cm was drawn for each sample, and 0.04 g of the corresponding particles were applied and sprayed each time.
[0211] The parameters evaluated by the testers were the silky feel during spreading and the skin feel after spreading the powder, with a rating from 0 (poor) to 4 (very good). The results are listed in Table 1.
[0212] Table 1
[0213] Example Silky feel Skin feel Example 6 4 3 Example 8 3 4 Comparative Example C2* 1 2 Comparative Example C4* 1 2
[0214] *Not according to the present invention
[0215] Example 10: Mechanical integrity of particles P
[0216] In contrast to Example 9, the tester spread the particles on the skin with strong pressure. The results for the inventive silica-coated silicone elastomer particles P from Examples 6 and 8 were unchanged, whereas the particles not according to the invention from Comparative Examples C2 and C4 formed clumps during spreading, which is undesirable in cosmetic applications.
[0217] Table 2
[0218] Example Silky feel Skin feel Example 6 4 3 Example 8 3 4 Comparative Example C2* 0 0 Comparative Example C4* 0 0
[0219] *Not according to the present invention
[0220] Example 11: Evaluation of mechanical strength
[0221] The silica-coated silicone elastomer particles P according to the invention from Examples 6 and 8 and the particles not according to the invention from Comparative Examples C2 and C4 were each mixed with 100% by weight of a 2 mm thick silica elastomer. 2 / s (25°C) of polydimethylsiloxane. The particles swell and completely absorb the silicone oil.
[0222] The swollen particles were then tested on the skin analogously to Example 9. Surprisingly, it was found that the silica-coated silicone elastomer particles according to the invention from Examples 6 and 8 exhibited a very good velvety skin feel after spreading, whereas the particles not according to the invention from Comparative Examples C2 and C4 had a waxier and more hysteretic skin feel after spreading.
[0223] Table 3
[0224] Example Silky feel Skin feel Example 6 4 4 Example 8 4 4 Comparative Example C2* 3 0 Comparative Example C4* 3 0
[0225] *Not according to the present invention
Claims
1. particles P consisting of a core K comprising a crosslinkable silicone elastomer composition X and a shell H of silicon dioxide S, Features The core K comprises a reinforcing filler F, wherein the reinforcing filler F is selected from a 2 / g DIN66131 BET surface area of pyrogenic or precipitated hydrophobic silica, as well as carbon black and activated carbon and silicone resin, The reinforcing filler F has a methanol value greater than 40 due to surface treatment, and the silica S has a methanol value less than 40.
2. The particle P according to claim 1, wherein the crosslinkable silicone elastomer composition X is addition crosslinked and comprises (A) at least one linear compound containing a group having an aliphatic carbon-carbon multiple bond (B) at least one linear organopolysiloxane compound having Si-bonded hydrogen atoms, Or, instead of (A) and (B), (C) at least one linear organopolysiloxane compound comprising SiC-bonded groups having aliphatic carbon-carbon multiple bonds and Si-bonded hydrogen atoms, and (D) at least one hydrosilylation catalyst. 3 . The particle P according to claim 1 , wherein the core K comprises 5 to 200 parts by weight of reinforcing filler F per 100 parts by weight of the crosslinkable silicone elastomer composition X. 4 .
4. The particle P according to claim 1 or 2, wherein the silicon dioxide S is selected from 2 / g of BET surface area of fumed or precipitated hydrophobic silica.
5. A method for producing particles P as claimed in any one of claims 1 to 4, wherein: In the first step, mixing a dispersion A comprising silica S and water with a mixture B comprising a crosslinkable silicone elastomer composition X to obtain a continuous phase comprising water and a discontinuous phase comprising the crosslinkable silicone elastomer composition X, and in a second step, crosslinking the discontinuous phase to obtain the particles P, Characterized in that the mixture B and the discontinuous phase contain reinforcing filler F.
6. The process of claim 5, wherein the continuous phase comprises at least 80% by weight water.
7. The method according to claim 5 or 6, wherein: In a first step, the mixture B and the dispersion A are initially introduced in a total volume such that it contains the desired total amounts of silica S and water.
8. The method according to claim 5 or 6, wherein in the first step, A catalyst is added to crosslink the crosslinkable silicone elastomer composition X.