Coating tape for inorganic layer of electrode and method for producing the same

By using a coating tape composed of inorganic materials, adhesives and plasticizers on the electrode surface to form a uniform inorganic layer, it solves the problems of short circuit and uneven coating thickness caused by the shrinkage of the separator in the battery, and improves the performance and safety of the battery. .

CN114846099BActive Publication Date: 2024-10-18LG ENERGY SOLUTION LTD
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
CN202080086945.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-18
Publication Date
2024-10-18
Estimated Expiration
2040-11-18

AI Technical Summary

Technical Problem

In the existing technology, the shrinkage of the separator in the battery causes electrode short circuit, and there are problems such as uneven thickness of the inorganic coating and resistance degradation caused by the adhesive.

Method used

Using a coating tape, the inorganic layer containing inorganic materials, adhesives and plasticizers is attached to the electrode surface through a film to form a uniform inorganic coating, avoiding the need to add adhesives separately, and the plasticizer ratio is 17-50 parts by weight. The weight average molecular weight is 350g/mol-10000g/mol, ensuring adhesion and electrical insulation.

Benefits of technology

It effectively prevents internal short circuits in the battery, reduces resistance, improves battery performance and safety, maintains uniform thickness and hole distribution of the inorganic layer, and simplifies the electrode manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114846099B_ABST
    Figure CN114846099B_ABST
Patent Text Reader

Abstract

The present application relates to a coating tape and a method for manufacturing the same, and more particularly, to: a coating tape in which an inorganic layer formed on one or both surfaces of an electrode is formed in the form of an adhesive tape and attached to a battery; and a method for manufacturing the coating tape.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application claims the benefit of priority to Korean Patent Application No. 2019-0169546, filed on December 18, 2019, and Korean Patent Application No. 2020-0148524, filed on November 9, 2020, the disclosures of which are incorporated herein by reference in their entirety.

[0002] The present invention relates to a coating tape for an inorganic layer for an electrode and a method for manufacturing the same. More specifically, the present invention relates to a coating tape in which an inorganic layer formed on one or both surfaces of an electrode is formed in the form of an adhesive tape and attached to a battery and a method for manufacturing the same. Background Art

[0003] Generally, a secondary battery includes an electrode assembly in which a positive electrode / separator / negative electrode is stacked. The positive electrode and the negative electrode are each manufactured by applying a slurry containing an electrode active material to one or both surfaces of a metal current collector, drying the slurry, and rolling the metal current collector with the dried slurry applied thereto. In addition, the separator is used to separate the positive electrode and the negative electrode to prevent an electrical short circuit between the two electrodes while allowing electrolytes and ions to pass.

[0004] Typically, the separator includes a porous substrate to prevent electrical short circuits between the two electrodes. The polyolefin substrate mainly used as the porous substrate will shrink to the form before stretching at high temperature, causing the problem of short circuit between the positive and negative electrodes. In order to solve this problem, the heat resistance is improved by methods such as giving additional materials to the porous substrate. Alternatively, the heat resistance of the entire separator can be improved by adding a coating to one surface of the porous substrate to improve the heat resistance of the entire separator. At this time, the coating can improve the heat resistance of the separator by adding a heat-resistant material to the coating itself or by changing the physical properties of the coating itself.

[0005] The method of improving the heat resistance of the separator as described above increases the temperature at which the separator shrinks. However, when the temperature eventually exceeds the limit temperature, the separator with improved heat resistance will eventually shrink. The present invention considers a method of adding a layer to the electrode that can prevent electrical short circuits in view of this.

[0006] Patent document 1 discloses a method for forming an inorganic coating on at least one surface of an electrode. When the inorganic coating is directly applied (coated) to the electrode as in Patent document 1, the inorganic powder such as Figure 1 The inorganic powder is shown to penetrate into the pores of the electrode, thereby making the thickness of the inorganic coating layer uneven. In addition, the infiltrated inorganic powder acts as a resistor for the electrode, thereby deteriorating the performance of the battery.

[0007] In Patent Document 2, in order to keep the thickness of the inorganic coating constant, a solution containing a dispersion medium and a binder for the inorganic coating is applied to the electrode active material layer. When the binder is added alone, the density of the battery is reduced, and the binder acts as a resistor, deteriorating the battery performance. In the case of forming a separate coating in Patent Document 2, there is a problem that the coating hardens, thereby generating cracks or tears.

[0008] Patent Document 3 adds a plasticizer to the negative electrode active material layer, but this document only proposes a solution for preventing a short circuit inside the battery.

[0009] Patent document 4 discloses a method for improving the processability of a dried coating while improving the flexibility of the coating by mixing a plasticizer in a slurry for a separator. However, in the case of Patent document 4, since the coating is combined with a separate inorganic support, the problem of internal short circuits occurring when the separator shrinks has not been solved. In addition, since sintering is required to attach the coating to the inorganic support, there is a disadvantage that the pore size and distribution of the coating may be different from the pore size and distribution during the initial slurry formation.

[0010] As described above, there is a need for a technology capable of improving the safety and performance of a battery by preventing an internal short circuit of the battery.

[0011] Prior art literature

[0012] Patent Literature

[0013] Korean Patent Application Publication No. 2008-0105853 (December 4, 2008) (Patent Document 1)

[0014] Korean Patent Application Publication No. 2014-0028754 (March 10, 2014) (Patent Document 2)

[0015] Japanese Patent Application Publication No. 2012-238396 (December 6, 2012) (Patent Document 3)

[0016] Korean Patent Application Publication No. 2018-0077030 (July 6, 2018) (Patent Document 4) Summary of the invention

[0017] [Technical issues]

[0018] The present invention has been completed in view of the above problems, and an object of the present invention is to provide a coating tape and a method for manufacturing the same, wherein the coating tape forms an inorganic layer formed on one or both surfaces of an electrode in the form of an adhesive tape for insulation and attaches it to a battery, thereby improving battery performance and preventing internal short circuits.

[0019] [Technical solution]

[0020] In a first aspect of the present invention, the above and other objects can be achieved by providing a coated tape comprising a film and an inorganic layer attached to one surface of the film, the inorganic layer comprising an inorganic material, a binder, and a plasticizer.

[0021] The plasticizer may contain at least one or more of the following: dibutyl phthalate, propylene glycol, benzyl alcohol, n-butanol, isopropanol, diethyl phosphate, triethyl phosphate, trimethyl phosphate, tributyl phosphate, isopentyl acetate, ethyl lactate, methyl lactate, ethyl butyrate, diethyl carbonate, tributyl orthopropionate, methyl amyl acetate, isopropyl acetate, diisobutyl ketone, methyl ethyl ketone, dipropyl ketone, ethyl butyl ketone and methyl amyl ketone, or a mixture thereof.

[0022] The plasticizer may be greater than 17 parts by weight and less than 50 parts by weight based on 100 parts by weight of the adhesive. In addition, the plasticizer may be greater than 22 parts by weight and less than 40 parts by weight based on 100 parts by weight of the adhesive.

[0023] The weight average molecular weight (M w ) can be 350 g / mol to 10000 g / mol.

[0024] The inorganic material may be an inorganic material having a dielectric constant of 1 or more, an inorganic material having piezoelectricity, an inorganic material having lithium ion transport capability, or a mixture of two or more thereof.

[0025] The inorganic material may be in a particle shape and may have a diameter of 1 nm to 10 μm.

[0026] The binder may be polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber or a mixture thereof.

[0027] The adhesion between the inorganic layer and the electrode may be 20 gf / cm or more, and the adhesion between the inorganic layer and the film may be less than the adhesion between the inorganic material layer and the electrode. In addition to containing the inorganic material, the coated tape according to the present invention may further contain a flame retardant. The flame retardant may be aluminum hydrate or aluminum hydroxide.

[0028] The film may be a release film having different adhesion forces on both surfaces.

[0029] The adhesive force of the inorganic layer attachment surface of the release film may be equal to or lower than the adhesive force of the other surface.

[0030] The adhesive force between the inorganic layer attachment surface of the film and the inorganic layer itself may be greater than a strength capable of bearing the weight of the inorganic layer and lower than an adhesive force between the inorganic layer itself and the electrode.

[0031] The inorganic layer attachment surface of the release film may be coated or surface treated.

[0032] The present invention can provide a method for manufacturing a coated tape, the method comprising: 1) preparing an inorganic slurry by mixing a solvent with an inorganic layer composition comprising an inorganic material, a binder and a plasticizer; 2) applying the inorganic slurry of step 1) to a film; and 3) drying the inorganic slurry applied in step 2) to form an inorganic layer.

[0033] A step of uniformly controlling the amount of inorganic slurry applied may be added between step 2) and step 3).

[0034] In step 2), the inorganic slurry may have a higher binder content in the electrode contact surface portion than in other portions.

[0035] When an inorganic layer is coated on one or both surfaces of an electrode using a coating tape as described above, the present invention can provide a method for manufacturing an electrode, the method comprising: 1) supporting the coating tape on a roller or pressing the coating tape by using a roller so that the inorganic layer contacts the electrode; and 2) removing the film after applying the inorganic layer of the coating tape to the electrode.

[0036] The rollers may include a guide roller, a pressure roller, a heating roller, and a heating pressure roller.

[0037] In step 2), a separate binder may not be added.

[0038] The present invention may be an electrode manufactured by the above-mentioned method for manufacturing an electrode.

[0039] In the present invention, one or more structures that do not conflict with each other can be selected from the above structures and combined. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is an electron microscope photograph of the active material layer of an electrode, where the inorganic layer is directly applied to the electrode in a slurry state.

[0041] Figure 2 A graph showing changes in the number of ignitions and direct current resistance during charge and discharge depending on the composition ratio of the plasticizer in Examples of the present invention and Comparative Examples is shown.

[0042] Figure 3is a graph showing changes in battery capacity expressed as a ratio according to charging and discharging cycles of Examples and Comparative Examples of the present invention. DETAILED DESCRIPTION

[0043] Now, the preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily implement the preferred embodiments of the present invention. However, when describing the working principle of the preferred embodiments of the present invention in detail, when the incorporation of known functions and structures herein may obscure the subject matter of the present invention, the detailed description thereof will be omitted.

[0044] In the case where it is said throughout the specification that one part is connected to another part, not only can the one part be directly connected to the other part, but the one part can be indirectly connected to the other part through another part. In addition, the inclusion of a specific element does not mean the exclusion of other elements, but means that other elements may also be included unless otherwise specified.

[0045] Hereinafter, the present invention will be described in more detail. This is only provided for illustrating the present invention and should not be construed as limiting the scope of the present invention.

[0046] The present invention relates to a coated tape comprising a film and an inorganic layer attached to one surface of the film, the inorganic layer comprising an inorganic material, a binder and a plasticizer.

[0047] Inorganic materials

[0048] The inorganic material may be an inorganic material having a dielectric constant of 1 or more, an inorganic material having piezoelectricity, an inorganic material having lithium ion transport capability, or a mixture of two or more thereof. Preferably, the inorganic material is in a particle form.

[0049] Examples of the inorganic material having a dielectric constant of 1 or more may be SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiC or a mixture thereof, but the present invention is not limited thereto.

[0050] The inorganic material having piezoelectricity refers to a material that is a non-conductor under normal pressure, but when a specific pressure is applied thereto, the internal structure changes and thus becomes conductive. In particular, the inorganic material having piezoelectricity exhibits a high dielectric constant characteristic of 100 or more, and generates electric charge when the particle is stretched or compressed by a specific pressure, so that one surface is charged with positive charge and the other surface is charged with negative charge, thereby having a potential difference between the two surfaces.

[0051] In the case of using an inorganic material having the above characteristics, when a short circuit occurs between the positive electrode and the negative electrode, the positive electrode and the negative electrode may not come into direct contact with each other due to the inorganic material, and a potential difference may occur in the particles due to the piezoelectricity of the inorganic material. Therefore, electron migration, that is, a minute current flow, is achieved between the positive electrode and the negative electrode, so that the voltage of the battery gradually decreases, and thus the safety can be improved.

[0052] Examples of the inorganic material having piezoelectricity may be BaTiO3, Pb(Zr,Ti)O3 (PZT), Pb 1- x La x Zr 1-y Ti y O3 (PLZT), Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3 (PMN-PT), hafnium dioxide (HfO2) or a mixture thereof, but the present invention is not limited thereto.

[0053] The inorganic material having lithium ion transport ability refers to an inorganic material containing lithium element, not storing lithium and transporting lithium ions. The inorganic material having lithium ion transport ability can migrate and transport lithium ions through defects existing in the particle structure. Therefore, the lithium ion conductivity in the battery is improved, and thus the battery performance can be improved.

[0054] Examples of the inorganic material having lithium ion transport ability may be lithium phosphate (Li3PO4), lithium titanium phosphate (Li x Ti y( PO4)3, where 0 < x < 2 and 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, where 0 < x < 2, 0 < y < 1 and 0 < z < 3), (LiAlTiP) x O y -based glass (where 0 < x < 4 and 0 < y < 13) such as 14Li2O-9Al2O3-38TiO2-39P2O5, lanthanum lithium titanate (Li x La y TiO3, where 0 < x < 2 and 0 < y < 3), lithium germanium thiophosphate (Li x Ge y P z S w , where 0 < x < 4, 0 < y < 1, 0 < z < 1 and 0 < w < 5) such as Li 3.25 Ge 0.25 P 0.75 S4, lithium nitride (Li x N y, where 0 < x < 4 and 0 < y < 2), such as Li3N, SiS2-based glass (Li x Si y S z , where 0 < x < 3, 0 < y < 2 and 0 < z < 4), such as Li3PO4-Li2S-SiS2, P2S5-based glass (Li x P y S z , where 0 < x < 3, 0 < y < 3 and 0 < z < 7), such as LiI-Li2S-P2S5 or a mixture thereof, but the present invention is not limited thereto.

[0055] When the above high dielectric constant inorganic material, piezoelectric inorganic material, and inorganic material having lithium ion transport ability are used together, the effects obtained by these components can be further improved.

[0056] There is no particular limitation on the size of the various inorganic materials in particle form. However, in order to form a coating with a uniform thickness and obtain an appropriate porosity, the various inorganic materials may have a size of 0.001 μm to 10 μm. When the size of the various inorganic materials is less than 0.001 μm, the dispersibility decreases, making it difficult to exhibit a uniform insulating effect. When the size of the various inorganic materials is greater than 10 μm, it is difficult to form a thin coating. In addition, since the pore size is too large, short circuits may easily occur in the battery during charging and discharging of the battery.

[0057] Adhesives

[0058] The binder is used to bond the inorganic materials and impart a specific degree of viscosity to the inorganic layer.

[0059] The binder used in the present invention may be a polymer that is commonly used in the art to form an inorganic layer on at least one surface of a porous substrate used as a separator. In particular, the binder may use a polymer having a glass transition temperature (Tg) of -200 °C to 200 °C to improve the mechanical properties such as flexibility and elasticity of the finally formed inorganic layer. Such a binder is used to stably connect and fix between the inorganic materials, thereby preventing a decrease in the mechanical properties of the inorganic layer.

[0060] In addition, the binder does not necessarily need to have ion conductivity, however, a polymer with ion conductivity can be used to improve the performance of the electrochemical device. Therefore, the binder used in the present invention preferably includes a binder with a high dielectric constant. In fact, the degree of dissociation of the salt in the electrolyte depends on the dielectric constant of the electrolyte. Therefore, as the dielectric constant of the polymer becomes higher, the degree of dissociation of the salt in the electrolyte increases. In this regard, in the present invention, the dielectric constant of the binder can be 1.0 to 100 (measurement frequency = 1kHz), preferably 10 or more.

[0061] In addition, when the binder is impregnated with a liquid electrolyte, the binder may gel to show a high degree of swelling in the electrolyte. In this regard, it is preferred that the solubility parameter of the binder polymer is 15 to 45 MPa. 1 / 2 , 15~25MPa 1 / 2 or 30~45MPa 1 / 2 Therefore, it is advantageous to use a hydrophilic polymer having multiple polar groups compared to a hydrophobic polymer such as a polyolefin. When the solubility parameter of the polymer is less than 15 MPa 1 / 2 or higher than 45MPa 1 / 2 When the polymer is used, it is difficult for the polymer to swell with a conventional battery electrolyte.

[0062] Non-limiting examples of the binder may be any one selected from the following or a mixture of two or more thereof: polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-trichloroethylene, polymethyl methacrylate, polybutyl acrylate, polyacrylonitrile, polyvinyl pyrrolidone, polyvinyl acetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, carboxymethyl cellulose and tannic acid.

[0063] Preparation of inorganic layer

[0064] The weight ratio of the inorganic material to the binder may be in the range of 1:1 to 99:1, 60:40 to 90:10, or 70:30 to 80:20.

[0065] In the inorganic layer, the binder adheres the inorganic material so that the inorganic materials can be combined with each other. In addition, the inorganic layer contacts the porous substrate through the binder. In the inorganic layer, the inorganic materials exist in a manner of contacting each other to form a closest packing structure, and the interstitial volume generated by the contact of the inorganic materials with each other becomes the pores of the inorganic layer.

[0066] The pores of the inorganic layer are spaces formed by inorganic materials that are in contact with each other in a close packing or dense packing structure of the inorganic materials. The pores of the inorganic layer can provide channels for the movement of lithium ions.

[0067] Plasticizers

[0068] The plasticizer is used to impart flexibility to the inorganic layer and prevent the inorganic layer from cracking or tearing after drying.

[0069] Non-limiting examples of the plasticizer may be at least one or more of the following: dibutyl phthalate, propylene glycol, benzyl alcohol, n-butanol, isopropyl alcohol, diethyl phosphate, triethyl phosphate, trimethyl phosphate, tributyl phosphate, isoamyl acetate, ethyl lactate, methyl lactate, ethyl butyrate, diethyl carbonate, tributyl orthopropionate, methyl amyl acetate, isopropyl acetate, diisobutyl ketone, methyl ethyl ketone, dipropyl ketone, ethyl butyl ketone and methyl amyl ketone or a mixture thereof.

[0070] Based on 100 parts by weight of the adhesive, the plasticizer may be greater than 17 parts by weight to less than 50 parts by weight. In the case where the plasticizer is less than 17 parts by weight based on 100 parts by weight of the adhesive, the inorganic layer may harden and cracks may occur, or the inorganic layer may tear when the inorganic layer is attached using a coating tape. In the case where the plasticizer is more than 50 parts by weight based on 100 parts by weight of the adhesive, the amount of the adhesive in the total weight of the inorganic layer is reduced, so that sufficient adhesion cannot be obtained. As a result, when the inorganic layer is attached using a coating tape, the inorganic layer cannot be attached to the electrode.

[0071] Furthermore, when the plasticizer is excessive, the plasticizer itself may function as a resistor, which may deteriorate the performance of the battery.

[0072] More preferably, the plasticizer may be greater than 22 parts by weight and less than 40 parts by weight based on 100 parts by weight of the adhesive. In the case where the plasticizer is less than 22 parts by weight based on 100 parts by weight of the adhesive, because the proportion of the plasticizer is low, cracks in the inorganic layer or a phenomenon in which a portion of the inorganic layer is damaged when attached using a coating tape cannot be prevented, thereby catching fire due to overcharging. In the case where the plasticizer is more than 40 parts by weight based on 100 parts by weight of the adhesive, the plasticizer acts as a resistor, which may deteriorate the performance of the battery.

[0073] The weight average molecular weight of the plasticizer can be 350g / mol to 10000g / mol. When the weight average molecular weight is less than 350g / mol, there may be a problem that the inorganic layer cannot obtain adhesion that can be attached to the electrode. When the weight average molecular weight is greater than 10000g / mol, there may be a problem that the plasticizer may be locally aggregated. The higher the molecular weight, the better the adhesion and electrical insulation, and the lower the volatility. Therefore, within the above range, a plasticizer that can show appropriate adhesion, electrical insulation, and desired air permeability and porosity can be selected.

[0074] By adding a plasticizer as described above, the inorganic layer can be directly attached to the electrode without causing cracks when the coating tape is attached. In order to attach the inorganic layer to one surface of the electrode, the adhesion between the inorganic layer and the electrode must be more than 20gf / cm. In order to use the inorganic layer as a coating tape used by removing the inorganic layer from the film, the inorganic layer preferably has an adhesion that is easy to peel off from the film. Therefore, it is preferred that the adhesion between the inorganic layer and the film is less than the adhesion between the inorganic layer and the electrode.

[0075] additive

[0076] The inorganic layer according to the present invention may contain additives other than inorganic materials, binders and plasticizers. The additives are materials that are necessary or additionally required to improve the operation and performance of the electrochemical device, and if they need to be continuously replenished due to their consumption during the operation of the electrochemical device, they can be applied without particular limitation.

[0077] Non-limiting examples of the additive may be an additive for suppressing a side reaction occurring in a battery, an additive for improving thermal stability, an additive for suppressing overcharge, a dispersant, and a mixture of two or more thereof.

[0078] As the additive for suppressing the side reactions occurring in the battery, at least one selected from the group consisting of ethylenediaminetetraacetic acid, tetramethylethylenediamine, pyridine, bipyridine, ethylbis(diphenylphosphine), butyronitrile, succinonitrile, iodine, ammonium halide and its derivatives can be used, but the present invention is not limited thereto.

[0079] As the additive for improving thermal stability, at least one selected from the group consisting of hexamethyldisiloxane, hexamethoxycyclotriphosphazene, hexamethylphosphoramide, cyclohexylbenzene, biphenyl, dimethylpyrrole and derivatives thereof or a mixture of two or more thereof may be used, but the present invention is not limited thereto.

[0080] An example of the additive for improving thermal stability may be a flame retardant. The flame retardant may include a phosphorus-based or inorganic-based flame retardant, and may further include a flame retardant synergist capable of improving the flame retardant effect.

[0081] As the additive for suppressing overcharge, at least one selected from the group consisting of n-butylferrocene, a halogen-substituted benzene derivative, cyclohexylbenzene, and biphenyl, or a mixture of two or more thereof may be used, but the present invention is not limited thereto.

[0082] There is no limitation on the dispersant as long as it is a material that improves dispersibility and maintains uniform dispersion. However, it is preferred that the dispersant is a material with high dispersibility. For example, an anionic surfactant can be used. The anionic surfactant can be a component in which an anionic component containing one or more salts selected from the group consisting of carboxylates, phosphates, sulfonates and sulfates constitutes the head. In addition, examples of substances that can be used as dispersants can be selected from any one or more of the following: oil-soluble polyamines, oil-soluble amine compounds, fatty acids, fatty alcohols, sorbitan fatty acid esters, tannic acid, tannic acid and pyrogallic acid.

[0083] Coated tape

[0084] The coated tape according to the present invention can be used in the form of a tape by applying an inorganic layer to a film. The inorganic layer is attached to the film in a similar manner to a double-sided tape before being attached to the electrode. For this reason, it is preferred that the adhesion between the inorganic layer attachment surface of the film and the inorganic layer itself is greater than the weight of the inorganic layer and less than the adhesion between the inorganic layer itself and the electrode.

[0085] The coated tape can be wound into a round shape and stored, and then used by hanging it on a roll when used. Alternatively, the coated tape can be in a form that can be used by placing a separate film on a film cut into a specific size and an inorganic layer to cover the exposed surface of the inorganic layer and then removing it.

[0086] As described above, when the coated tape is wound into a round shape and stored or the film is used by removing it, the film may be a release film having different adhesive forces on both surfaces. When the release film is used in a state where the coated tape is multi-layered, the adhesive force between the inorganic layer and the attachment surface may be equal to or lower than the adhesive force of the other surface for ease of use.

[0087] The film may use any material as long as it has low surface roughness and can be easily peeled off so that no residue is left when the inorganic layer is peeled off. Examples of the film may include: synthetic resin films such as polyethylene, polypropylene, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, and polyethylene terephthalate; metal foils, etc.

[0088] The film may be coated or surface treated at least on the inorganic layer attachment surface so that no residue of the inorganic layer remains. Examples of surface treatment include: plasma treatment; surface modification treatment such as sulfonation treatment; or stripping treatment such as silicon treatment, long cycloalkyl treatment and fluorine treatment.

[0089] The film may use a material evaporated by heat treatment, ultraviolet irradiation, or solution treatment.

[0090] The present invention provides a method for manufacturing a coated tape, the method comprising: 1) preparing an inorganic slurry by mixing a solvent with an inorganic layer composition comprising an inorganic material, a binder and a plasticizer; 2) applying the inorganic slurry of step 1) to a film; and 3) drying the inorganic slurry applied in step 2) to form an inorganic layer.

[0091] The inorganic material, binder, plasticizer, mixing ratio thereof, and film are as described above.

[0092] As the solvent, conventional solvents known in the art may be used without limitation. Non-limiting examples of the solvent include acetone, tetrahydrofuran, dichloromethane, chloroform, dimethylformamide, N-methyl-2-pyrrolidone (NMP), cyclohexane, water, and mixtures thereof.

[0093] In the drying step, an oven or a heating chamber may be used within a temperature range that takes into account the vapor pressure of the solvent. Alternatively, a method of volatilizing the solvent by leaving the inorganic slurry at room temperature is also feasible. At this time, a temperature condition in the temperature range of 25° C. to 100° C. and a relative humidity condition of 40% or more may be considered.

[0094] A step of uniformly controlling the amount of inorganic slurry applied may be further included between step 2) and step 3).

[0095] In the step of uniformly controlling the amount of inorganic slurry applied, a roller may be used to uniformly control. Alternatively, a method of cutting the applied surface with a blade may also be used. In addition, a method of placing the film in a container of a desired size, applying the slurry, and then pressing the surface to fit the container may also be used.

[0096] In step 2), the inorganic slurry may have a higher binder content in the electrode contact surface than in other parts. By increasing the binder content, adhesion to the electrode may be improved without adding a separate binder.

[0097] The coated tape according to the present invention can have adhesion even after drying in step 3). This is because the inorganic layer is formed by mixing the plasticizer in the adhesive at a ratio of more than 22 parts by weight and less than 40 parts by weight based on 100 parts by weight of the adhesive. The coated tape that maintains adhesion even after drying as described above can be directly applied to the electrode without adding a separate adhesive.

[0098] Electrode fabrication

[0099] The method for manufacturing an electrode according to the present invention may include: 1) supporting the coated tape according to the above description on a roller or pressing the coated tape by using a roller so that the inorganic layer contacts the electrode; and 2) removing the film after applying the inorganic layer of the coated tape to the electrode.

[0100] The electrode may be a negative electrode or a positive electrode.

[0101] The positive electrode may be manufactured by, for example, applying a positive electrode mixture in which a positive electrode active material composed of positive electrode active material particles, a conductive agent, and a binder are mixed onto a positive electrode current collector. A filler may be further added to the positive electrode mixture as needed.

[0102] Typically, the positive electrode collector is manufactured to have a thickness of 3 μm to 500 μm. There is no particular limitation on the positive electrode collector, as long as the positive electrode collector does not cause any chemical changes in the battery to which the positive electrode collector is applied, and the positive electrode collector exhibits high conductivity. For example, the positive electrode collector may be made of one selected from the following: stainless steel, aluminum, nickel and titanium. Alternatively, the positive electrode collector may be made of one selected from the following: aluminum or stainless steel whose surface is treated with carbon, nickel, titanium or silver. Specifically, aluminum can be used. The collector may have a fine concave-convex pattern formed on its surface to increase the adhesion of the positive active material. The collector may be constructed in various forms such as a film, a sheet, a foil, a mesh, a porous body, a foam body and a non-woven fabric body.

[0103] The positive electrode active material may further include, for example, a layered compound such as lithium nickel oxide (LiNiO2) or a compound substituted by one or more transition metals, a lithium manganese oxide such as Li 1+x Mn 2-x O4 (where x ranges from 0 to 0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, Cu2V2O7; LiNi 1-x M xNi-site lithium nickel oxide represented by LiMn O2 (wherein M = Co, Mn, Al, Cu, Fe, Mg, B or Ga, and x ranges from 0.01 to 0.3); 2-x M x Lithium manganese composite oxides represented by Li2Mn3MO8 (wherein M = Co, Ni, Fe, Cr, Zn or Ta, and x is in the range of 0.01 to 0.1) or Li2Mn3MO8 (wherein M = Fe, Co, Ni, Cu or Zn); LiMn2O4 in which a portion of Li is replaced by alkaline earth metal ions; disulfide compounds; Fe2(MoO4)3, etc., but are not particularly limited thereto.

[0104] The conductive agent is usually added so that the conductive agent accounts for 0.1 wt% to 30 wt% based on the total weight of the mixture containing the positive electrode active material. There is no particular limitation on the conductive agent, as long as the conductive agent exhibits high conductivity without causing any chemical changes in the battery to which the conductive agent is applied. As the conductive agent, for example: graphite such as natural graphite or artificial graphite; carbon black such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black or thermal black; conductive fibers such as carbon fibers or metal fibers; fluorocarbon powder; metal powder such as aluminum powder or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive substances such as polyphenylene derivatives.

[0105] The binder contained in the positive electrode is a component that helps the combination between the active material and the conductive agent and the combination with the current collector. Based on the total weight of the mixture containing the positive electrode active material, the addition amount of the binder is generally 0.1 wt % to 30 wt %. Examples of the binder can be polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber and various mixtures.

[0106] The negative electrode may be manufactured by coating a negative electrode active material onto a negative electrode current collector and drying the coated negative electrode current collector. The negative electrode may further optionally include the above-mentioned components as required.

[0107] Generally, the negative current collector is manufactured to have a thickness of 3 μm to 500 μm. There is no particular limitation on the negative current collector as long as the negative current collector exhibits high conductivity and does not cause any chemical changes in the battery to which the negative current collector is applied. For example, the negative current collector can be made of copper, stainless steel, aluminum, nickel, titanium, or sintered carbon. Alternatively, the negative current collector can be made of the following substances: copper or stainless steel treated on the surface with carbon, nickel, titanium, or silver; or an aluminum-cadmium alloy. Additionally, in the same manner as the positive current collector, the negative current collector can have a fine uneven pattern formed on its surface to improve the adhesion of the negative active material. The negative current collector can be constructed in various forms such as films, sheets, foils, meshes, porous bodies, foams, and non-woven fabric bodies.

[0108] The negative active material can include, for example: carbon such as non-graphitized carbon and graphitic carbon; metal composite oxides such as Li x Fe2O3 (0 ≤ x ≤ 1), Li x WO2 (0 ≤ x ≤ 1), Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements in Groups 1, 2, and 3 of the periodic table, halogens; 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8); lithium metal; lithium alloy; silicon-based alloy; tin-based alloy; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, and Bi2O5; conductive polymers such as polyacetylene; or Li-Co-Ni-based materials.

[0109] The rollers can include guide rollers, heating rollers, and heating and pressing rollers. The rollers can press or heat-press the coated tape according to the adhesion of the coated tape. The intensity of this pressure can vary according to the adhesion of the coated tape. However, preferably, the intensity of this pressure is the same as or stronger than the intensity at which the coated tape can form an inorganic layer on one or both surfaces of the electrode.

[0110] In the method for manufacturing an electrode according to the present invention, an inorganic coating is formed on the electrode by utilizing the adhesion of the inorganic layer itself without adding a separate binder.

[0111] The electrode of the present invention can form an electrode assembly by stacking the electrodes of the present invention thereon. As another example, a separator made only of a porous substrate, a separator coated with a separate inorganic coating on the porous substrate, or the electrode of the present invention can be stacked on the electrode of the present invention.

[0112] As the porous substrate, any porous substrate used for battery separators can be used, but a porous substrate with excellent ion conductivity is preferably used. The pore size of the porous substrate is generally 0.01 μm to 10 μm, and its thickness is generally 5 μm to 300 μm. Examples of such porous substrates include sheets or non-woven fabrics made of olefin polymers such as polypropylene, glass fibers or polyethylene having chemical resistance and hydrophobicity. When a solid electrolyte such as a polymer is used as an electrolyte, the solid electrolyte can also serve as a diaphragm. The separate inorganic coating on the porous substrate may be the same as the inorganic coating defined in the present invention. Alternatively, the separate inorganic coating on the porous substrate may be a coating excluding a plasticizer from the inorganic coating defined in the present invention.

[0113] The electrode assembly stacked as described above may be subjected to a roll-pressing process after being stacked.

[0114] At this time, the rolling temperature may be 90°C to 130°C. The preferred temperature is 100°C or 125°C. When the rolling temperature is lower than 90°C, the adhesion between the electrode and the separator does not reach the desired level, which is not preferred. When the rolling temperature is higher than 130°C, the performance of the adhesive deteriorates, resulting in reduced adhesion, and the separator may be deformed, which is not preferred.

[0115] The pressure during rolling may be about 1 to about 3 tons. At this time, the most preferred range may be about 1.5 to about 2 tons. When the pressure during rolling exceeds 3 tons, damage such as tearing may occur, and when the pressure during rolling is less than 1 ton, the desired level of adhesion between the electrode and the separator cannot be obtained.

[0116] The rolling time during rolling can be about 1 minute to about 3 minutes. At this time, the most preferred range can be about 1.5 minutes to about 2.5 minutes. When the rolling time is greater than 3 minutes, structural deformation of the separator may occur. When the rolling time is less than 1 minute, the desired level of adhesion cannot be obtained between the electrode and the separator.

[0117] The present invention also provides a battery pack comprising a unit cell as a unit battery and a device comprising the battery pack as a power source. The unit cell of the present invention itself can be a power supply device for an unmanned aerial vehicle or a laptop computer, and can be used in the form of stacked unit cells. Specifically, the battery pack can be used as a power source for devices that require high temperature, long life, high rate characteristics, etc. Preferred examples of the device may include mobile electronic devices, wearable electronic devices, electric tools driven by electric motors powered by batteries, electric vehicles (EV), hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV) and energy storage systems. However, the present invention is not limited thereto.

[0118] The structure and manufacturing method of the device are well known in the art to which the present invention pertains, and thus a detailed description thereof will be omitted.

[0119] Hereinafter, the present invention will be described with reference to the following examples. These examples are provided only for easier understanding of the present invention and should not be construed as limiting the scope of the present invention.

[0120] Example 1 (binder:plasticizer (weight ratio) = 1:0.22)

[0121] 20 g of inorganic powder, 10 g of acetone as a solvent, 2.5 g of CMC (carboxymethyl cellulose) as a dispersant were pre-dispersed, and then 20 g of PVdF-HFP binder and 4.4 g of dibutyl phthalate were added and dispersed. The composition was applied to a PET film and then dried to prepare a coating tape.

[0122] The coating tape was applied to a negative electrode using graphite as an active material on lithium metal and a positive electrode using NCMA as an active material on aluminum.

[0123] Thereafter, a polyolefin porous substrate was stacked between the negative electrode and the positive electrode, and then roll-pressed at 90° C. and a pressure of 100 MPa for 10 seconds to form a unit cell.

[0124] Example 2 (binder:plasticizer (weight ratio) = 1:0.26)

[0125] In Example 1, dibutyl phthalate was changed to 5.2 g to prepare a coating tape. The subsequent steps were the same as in Example 1.

[0126] Example 3 (binder:plasticizer (weight ratio) = 1:0.28)

[0127] In Example 1, dibutyl phthalate was changed to 5.6 g to prepare a coating tape. The subsequent steps were the same as in Example 1.

[0128] Example 4 (binder:plasticizer (weight ratio) = 1:0.36)

[0129] In Example 1, dibutyl phthalate was changed to 7.2 g to prepare a coating tape. The subsequent steps were the same as in Example 1.

[0130] Example 5 (binder:plasticizer (weight ratio) = 1:0.40)

[0131] In Example 1, dibutyl phthalate was changed to 8 g to prepare a coating tape. The subsequent steps were the same as in Example 1.

[0132] Comparative Example 1 (Binder:Plasticizer (weight ratio) = 1:0)

[0133] In Example 1, dibutyl phthalate was changed to 0 g to prepare a coating tape. The subsequent steps were the same as those of Example 1. The slurry was applied to the positive electrode and the negative electrode of Example 1, respectively. Thereafter, a unit monomer was formed by stacking a polyolefin porous substrate between the negative electrode and the positive electrode.

[0134] Comparative Example 2 (Binder:Plasticizer (weight ratio) = 1:0.17)

[0135] In Example 1, dibutyl phthalate was changed to 3.4 g to prepare a coating tape. The subsequent steps were the same as in Example 1.

[0136] Comparative Example 3 (Binder:Plasticizer (weight ratio) = 1:0.50)

[0137] In Example 1, dibutyl phthalate was changed to 10 g to prepare a coating tape. The subsequent steps were the same as in Example 1.

[0138] At this time, in the case of Comparative Example 2, when the composition was dried, the coating hardened and cracks appeared, or the coating was torn when the composition was applied to the electrode. As a result, the unit cell could not be produced. In the case of Comparative Example 3, coating on the negative electrode could not be performed due to poor adhesion.

[0139] Overcharge fire evaluation

[0140] The unit cells of Examples 1 to 5 and Comparative Example 1 were formed into 3A pouch-type battery cells and then charged to 4.2V at a constant current. Figure 2 The state after the lithium secondary battery is fully charged to 100% SOC under the condition of 8.4 V / 1 C is shown.

[0141] like Figure 2 As shown, in the case of Comparative Example 1, fire was observed in all 5 batteries. However, fire was observed in 4 of the 5 batteries of Example 1, and in 2 of the 5 batteries of Example 2. In Examples 3 to 5, fire was not observed in any of the 5 batteries. It can be seen that the safety of the battery formed by the method of the example is more excellent.

[0142] Resistance evaluation

[0143] When a 3C pulse was applied to the unit cells of Examples 1 to 5 and Comparative Example 1 at SOC 50 for 10 seconds, the voltage change was measured. The results are shown in Figure 2 middle.

[0144] like Figure 2As shown, the resistance value of Example 1 is 4.19mΩ, the resistance value of Example 2 is 4.685475mΩ, the resistance value of Example 3 is 4.86mΩ, the resistance value of Example 4 is 13.29595mΩ, the resistance value of Example 5 is 14.52mΩ, and the resistance value of Comparative Example 1 is 3.89mΩ. It can be seen that the resistance value increases with the increase in the amount of plasticizer. In particular, it can be seen that the resistance value between Example 2 and Example 3 increases significantly. Therefore, it can be confirmed that when the amount of plasticizer relative to the adhesive exceeds the range of Example 5, the resistance value becomes too large and the performance of the battery deteriorates seriously.

[0145] Battery cell capacity retention rate evaluation experiment

[0146] The unit cells of Example 1, Example 3, Example 5 and Comparative Example 1 were charged at 25° C. and 1C to reach 4.2 V, and discharged at a constant current of 1C to reach 3.0 V. The charge and discharge were cycled 100 times, and the discharge capacity after 1 cycle and the discharge capacity after 100 cycles were measured. Thereafter, the capacity retention rate was measured according to the following formula (1).

[0147] Formula (1): Capacity retention rate (%) = {discharge capacity after cycle / discharge capacity after first cycle} × 100

[0148] The capacity retention rate measured according to the above experiment is shown in Figure 3 middle.

[0149] like Figure 3 As shown, similar capacity retention rates were shown in the cases of Examples 1 and 3 and Comparative Example 1. However, in the case of Example 5, it can be seen that the capacity decreased as well as the resistance value.

[0150] Regarding the discharge capacity after 100 cycles, Example 1 was 97.6%, Example 3 was 98.5%, Example 5 was 88.5%, and Comparative Example 1 was 99.23%. As described above, when the amount of plasticizer relative to the binder was the same as that of Example 5, it can be seen that the battery capacity was within a good range while ensuring battery safety. When a plasticizer outside the range of Example 5 was used, it can be confirmed that the capacity retention rate was also poor.

[0151] Those skilled in the art will appreciate that the present invention may be implemented in a specific manner other than that set forth herein without departing from the spirit and essential features of the present invention. Therefore, the above-described embodiments should be interpreted in all respects as illustrative rather than restrictive. The scope of the present invention should be determined by the appended claims and their legal equivalents, rather than by the above description, and all changes within the meaning and equivalent range of the appended claims are intended to be included therein.

[0152] [Industrial Applicability]

[0153] The present invention provides an adhesive coating tape for an inorganic layer, wherein the inorganic layer can be attached to one or both surfaces of an electrode for insulation, thereby preventing a short circuit inside a battery due to shrinkage of a diaphragm, and the phenomenon that the electrode layer is impregnated with inorganic layer particles is reduced compared to the case of using a slurry. Therefore, compared to the shrinkage reduction rate of the diaphragm, the resistance of the battery is reduced, thereby obtaining a battery with excellent performance and safety.

[0154] Furthermore, since a separate binder is not added between the electrode and the inorganic layer, the capacity relative to the size of the battery is increased, and the manufacturing method of the electrode is simple.

[0155] Furthermore, by adding it in the form of a tape, the thickness of the inorganic layer becomes uniform and the resistance and ion conductivity become uniform, thereby improving the capacity and output of the battery.

[0156] The pore distribution and pore size of the inorganic layer can also be kept constant.

Claims

1. A coating tape for a secondary battery, the coating tape comprising: membrane; and an inorganic layer attached to one surface of the film, the inorganic layer comprising an inorganic material, a binder and dibutyl phthalate as a plasticizer, wherein the weight ratio of the inorganic material to the binder is 1:1 to 90:10, wherein the binder is at least one selected from polyvinylidene fluoride-hexafluoropropylene and polyvinylidene fluoride-trichloroethylene, Wherein, based on 100 parts by weight of the adhesive, the content of the plasticizer is greater than 22 parts by weight and less than 40 parts by weight. 2 . The coated tape for secondary batteries according to claim 1 , wherein the inorganic material is an inorganic material having a dielectric constant of 1 or more, an inorganic material having piezoelectricity, an inorganic material having lithium ion transporting ability, or a mixture of two or more thereof. 3 . The coated tape for secondary batteries according to claim 2 , wherein the inorganic material is in a particle form and has a diameter of 1 nm to 10 μm.

4. The coating tape for secondary battery according to claim 1, wherein The adhesion between the inorganic layer and the electrode is 20 gf / cm or more, and An adhesive force between the inorganic layer and the film is smaller than an adhesive force between the inorganic layer and the electrode.

5. The coated tape for secondary batteries according to claim 1, wherein the inorganic layer, in addition to containing the inorganic material, the binder and the plasticizer, further comprises any one of the following: an additive for suppressing side reactions occurring in the battery, an additive for improving thermal stability, an additive for suppressing overcharge, and a mixture of two or more thereof. 6 . The coated tape for secondary batteries according to claim 1 , wherein the film is a release film having different adhesive forces on both surfaces. 7 . The coated tape for secondary batteries according to claim 6 , wherein the adhesive force of the inorganic layer-attached surface of the release film is equal to or lower than the adhesive force of the other surface. 8 . The coated tape for secondary batteries according to claim 1 , wherein the adhesion between the inorganic layer attachment surface of the film and the inorganic layer itself is greater than the strength capable of bearing the weight of the inorganic layer and lower than the adhesion between the inorganic layer itself and the electrode. 9 . The coated tape for secondary batteries according to claim 6 , wherein the inorganic layer attachment surface of the release film is coated or surface treated.

10. A method for manufacturing the coating tape for secondary batteries according to claim 1, the method comprising: 1) preparing an inorganic slurry by mixing a solvent with an inorganic layer composition including an inorganic material, a binder, and a plasticizer; 2) applying the inorganic slurry of step 1) onto a membrane; and 3) Drying the inorganic slurry applied in step 2) to form an inorganic layer. 11 . The method according to claim 10 , further comprising uniformly controlling the amount of the inorganic slurry applied between step 2) and step 3). 12 . The method according to claim 10 , wherein in step 2), the inorganic slurry has a higher binder content in the electrode contact surface portion than in other portions.

13. A method for manufacturing an electrode by coating the inorganic layer on one surface or both surfaces of an electrode using the coating tape for a secondary battery according to any one of claims 1 to 9, the method comprising: 1) supporting the coated tape on a roller or pressing the coated tape by using a roller so that the inorganic layer contacts the electrode; and 2) After applying the inorganic layer of the coating tape to the electrode, removing the film.

14. The method according to claim 13, wherein the roller comprises a guide roller, a pressure roller, a heating roller and a heating pressure roller.

15. The method according to claim 13, wherein in step 2), no separate binder is added.

16. An electrode manufactured using the method according to claim 13.

Citation Information

Patent Citations

  • Negative electrode paste, negative electrode and manufacturing method thereof, as well as nonaqueous electrolyte secondary battery

    JP2012238396A

  • Non-woven cloth increasing micropore polymer diaphragm and usage as well as preparation method thereof

    CN101226994A

  • Thermally conductive pressure-sensitive adhesive composition, thermally conductive pressure-sensitive adhesive sheet, and electronic component

    CN102165028A

  • Paste for forming an etching mask pattern and method for manufacturing a solar cell using same

    CN102648245A

  • Internal and external adhesive tape for pipeline anticorrosion

    CN103602278A