Fluorine resin film

By using vinylidene fluoride/tetrafluoroethylene copolymer and optimized treatment technology in fluororesin film, the contradiction between high insulation breakdown strength and low static friction coefficient is solved, and excellent coiling and reliability.

CN114933768BActive Publication Date: 2024-11-19DAIKIN INDUSTRIES LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210619256.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2017-01-31
Filing Date
2018-01-17
Publication Date
2024-11-19
Estimated Expiration
2038-01-17

AI Technical Summary

Technical Problem

It is difficult to achieve a low static friction coefficient while maintaining high insulation breakdown strength, which affects its winding and reliability.

Method used

A fluororesin film containing vinylidene fluoride/tetrafluoroethylene copolymer is used to optimize the static friction coefficient and insulation breakdown strength by adjusting its surface roughness, inorganic particle content, embossing processing and surface coating.

Benefits of technology

A fluororesin film with low static friction coefficient and high insulation breakdown strength is achieved, which improves the wrapping property and reliability of the film, and improves the operability and productivity of the high dielectric film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003674316180000271
    Figure BDA0003674316180000271
  • Figure BDA0003674316180000281
    Figure BDA0003674316180000281
Patent Text Reader

Abstract

A fluororesin film having a low static friction coefficient and high dielectric breakdown strength is provided. A fluororesin film is a fluororesin film containing a fluororesin, characterized in that at least one surface has a ten-point average roughness of 0.100 μm to 1.200 μm, an arithmetic mean roughness of 0.010 μm to 0.050 μm, and a dielectric breakdown strength of 400 V / μm or more.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application. The Chinese national application number of the application to which it is directed is 201880008655.X, the international application number is PCT / JP2018 / 001180, the application date is January 17, 2018, the date of entry into China is July 26, 2019, and the name of the invention is “Fluororesin Film”. Technical Field

[0002] The present invention relates to a fluororesin film. Background Art

[0003] It is known that a film of a vinylidene fluoride homopolymer or a film of a copolymer composed of vinylidene fluoride and other monomers has a high relative dielectric constant.

[0004] Patent Document 1 describes a high dielectric film formed using a fluororesin containing 95 mol % or more of vinylidene fluoride units and tetrafluoroethylene units in total.

[0005] Patent Document 2 describes a film for a film capacitor comprising a tetrafluoroethylene resin as a film-forming resin, wherein the tetrafluoroethylene resin comprises vinylidene fluoride units and tetrafluoroethylene units in a ratio of vinylidene fluoride units / tetrafluoroethylene units (mol %) of 0 / 100 to 49 / 51.

[0006] In addition, Patent Document 3 describes a biaxially oriented polypropylene film, which is a polypropylene film composed of a polypropylene resin mainly composed of propylene, characterized in that the polypropylene resin is obtained by mixing 0.1% by weight to 1.5% by weight of branched polypropylene (H) in a linear polypropylene, and the melt tension (MS) and melt flow rate (MFR) of the branched polypropylene (H) when measured at 230°C satisfy the relationship of log(MS)>-0.56log(MFR)+0.74, and at least one surface of the film surface has a base layer composed of pear-skin-like rough surface, and the ten-point average roughness (Rz) of the surface is 0.50μm to 1.50μm and the surface gloss is 90% to 135%.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: International Publication No. 2008 / 090947

[0010] Patent Document 2: International Publication No. 2012 / 039424

[0011] Patent Document 3: Japanese Patent No. 4940986 Summary of the invention

[0012] Problems to be solved by the invention

[0013] However, fluororesin films used in film capacitors and the like are required to have a high relative dielectric constant and a low static friction coefficient in addition to high dielectric breakdown strength to improve film windability, etc. However, a fluororesin film having a low static friction coefficient while maintaining high dielectric breakdown strength has not yet been obtained.

[0014] In view of the above-mentioned current situation, an object of the present invention is to provide a fluororesin film having a low static friction coefficient and a high dielectric breakdown strength.

[0015] Means for solving problems

[0016] The present invention relates to a fluororesin film, which is a fluororesin film containing a fluororesin, characterized in that at least one surface has a ten-point average roughness of 0.100 μm to 1.200 μm, an arithmetic mean roughness of 0.010 μm to 0.050 μm, and a dielectric breakdown strength of 400 V / μm or more.

[0017] The fluororesin is preferably a vinylidene fluoride / tetrafluoroethylene copolymer. In addition, the fluororesin further preferably contains a copolymer unit based on an ethylenically unsaturated monomer (except tetrafluoroethylene and vinylidene fluoride).

[0018] The fluororesin film of the present invention preferably further contains inorganic particles. The content of the inorganic particles is preferably 0.01 to 5 parts by mass based on 100 parts by mass of the fluororesin.

[0019] The fluororesin film of the present invention is preferably embossed.

[0020] The fluororesin film of the present invention is preferably surface-coated.

[0021] The fluororesin film of the present invention preferably contains two kinds of fluororesins as the fluororesins.

[0022] The fluororesin film of the present invention preferably contains, as the fluororesin, a non-crosslinked fluororesin and a crosslinked fluororesin.

[0023] In addition, the fluororesin film of the present invention preferably contains two fluororesins having different melt flow rates as fluororesins. Preferably, one of the fluororesins has a melt flow rate of 2.0 to 30.0 g / 10 minutes, and the other has a melt flow rate of 0.1 to 1.9 g / 10 minutes.

[0024] The fluororesin film of the present invention preferably comprises two fluororesins having different composition ratios of polymerized units as fluororesins. Preferably, one of the fluororesins is a vinylidene fluoride / tetrafluoroethylene copolymer having a vinylidene fluoride unit / tetrafluoroethylene unit in a molar ratio of 95.0 / 5.0 to 39.0 / 61.0, and the other is a vinylidene fluoride / tetrafluoroethylene copolymer having a vinylidene fluoride unit / tetrafluoroethylene unit in a molar ratio of 38.9 / 61.1 to 5.0 / 95.0.

[0025] The fluororesin film of the present invention is preferably a biaxially stretched film.

[0026] The thickness of the fluororesin film of the present invention is preferably 1 μm to 100 μm.

[0027] The present invention also relates to a film for a film capacitor, comprising an electrode layer provided on at least one surface of the fluororesin film.

[0028] Furthermore, the present invention also relates to a film capacitor including the above-mentioned film for a film capacitor.

[0029] Effects of the Invention

[0030] Since the fluororesin film of the present invention has the above-mentioned constitution, it has a low static friction coefficient and a high dielectric breakdown strength. DETAILED DESCRIPTION

[0031] Next, the present invention will be described in detail.

[0032] The fluororesin film of the present invention comprises a fluororesin, has a ten-point average roughness of 0.100 μm to 1.200 μm on at least one surface, an arithmetic average roughness of 0.010 μm to 0.050 μm, and a dielectric breakdown strength of 400 V / μm or more, and thus has a low static friction coefficient despite having a high dielectric breakdown strength, thereby also achieving excellent windability.

[0033] In addition, when a fluororesin film is used as a high dielectric film for a film capacitor, if insulation breakdown occurs, gas will be generated and reliability will be reduced. However, since the fluororesin film of the present invention has the above-mentioned structure, the generated gas is easily discharged and it also has excellent reliability (for example, long-term durability, etc.).

[0034] Furthermore, since the fluorine resin is contained, a high capacitance can be obtained even if the film thickness is reduced compared to the case where a resin having a low dielectric constant is used.

[0035] Generally, compared with general-purpose resins, vinylidene fluororesins are high dielectric materials and are resins that are easily charged with static electricity. Therefore, due to the effect of static electricity, the films are easily fitted to each other, and are easily fitted to a roller during film forming, making operation difficult and having low productivity. In addition, if the film surface is smooth (the larger the contact area), van der Waals force (intermolecular force) also plays a role, and the films are easily fitted to each other and are easily fitted to a roller, etc., making operation more difficult.

[0036] The fluorine film of the present invention has a specific dielectric breakdown strength and specific surface properties. Therefore, even if it is a high dielectric material, the films are not tightly attached to each other, and during film production, they do not slide in tight contact with the rollers of the molding machine. Therefore, a high dielectric film can be provided without reducing the operability of the film and the film productivity.

[0037] The fluororesin film of the present invention has at least one surface with a ten-point average roughness of 0.100 to 1.200 μm and an arithmetic mean roughness of 0.010 to 0.050 μm.

[0038] From the perspective of reducing the static friction coefficient of the fluororesin film and improving reliability, the ten-point average roughness is preferably 0.150 μm to 1.150 μm, more preferably 0.170 μm to 1.100 μm, and even more preferably 0.200 μm to 1.000 μm. In addition, the arithmetic mean roughness is preferably 0.011 μm to 0.048 μm, more preferably 0.012 μm to 0.045 μm, and even more preferably 0.013 μm to 0.045 μm.

[0039] The ten-point average roughness and arithmetic mean roughness are values ​​measured based on JIS B-0601-2001 and can be measured using, for example, a "laser microscope" manufactured by KEYENCE CORPORATION.

[0040] The dielectric breakdown strength of the fluororesin film of the present invention is 400 V / μm or more, preferably 420 V / μm or more, more preferably 450 V / μm or more, and particularly preferably 500 V / μm or more. The upper limit of the dielectric breakdown strength is not limited, and for example, it may be 1000 V / μm or less, or 800 V / μm or less. In addition, it may be 700 V / μm or less, or 650 V / μm or less.

[0041] Regarding the above-mentioned dielectric breakdown strength, the above-mentioned film is placed on the lower electrode, a weight of φ25mm and 500g is placed as the upper electrode, and the voltage at both ends is increased at 100V / sec to measure the breakdown voltage. The number of measurements is set to 50 points, and the upper and lower 5 points are removed to calculate the average value, which is divided by the thickness to obtain the dielectric breakdown strength.

[0042] The crystallinity of the fluororesin film of the present invention is preferably 50% or more. By making the crystallinity of the fluororesin film within the above range, a fluororesin film having the above dielectric breakdown strength can be produced. As the above crystallinity, it is more preferably 60% or more, and further preferably 70% or more. The upper limit of the crystallinity is not particularly limited and may be 100%. In order to make the dielectric breakdown strength 400V / μm or more, a resin with high crystallinity is effective.

[0043] The crystallinity is measured by using an X-ray diffraction device and a peak separation method. Specifically, two or more films are overlapped so that the total thickness is 40 μm or more to obtain a measurement sample, and the measurement sample is set in a sample holder. The crystallinity is calculated from the area ratio of the crystalline part to the amorphous part of the diffraction spectrum obtained by the X-ray diffraction device.

[0044] The present invention relates to a fluororesin film comprising a fluororesin.

[0045] Examples of the fluororesin include polytetrafluoroethylene, tetrafluoroethylene / ethylene copolymers, polyvinylidene fluoride, tetrafluoroethylene / perfluoroalkyl vinyl ether copolymers, tetrafluoroethylene / hexafluoropropylene copolymers, etc. As the fluororesin, a melt-processable fluororesin is more preferred.

[0046] Since they exhibit better heat resistance and high dielectric properties, fluorine-containing polymers containing vinylidene fluoride units are preferred, and at least one selected from the group consisting of vinylidene fluoride / tetrafluoroethylene copolymers, vinylidene fluoride / trifluoroethylene copolymers, vinylidene fluoride / hexafluoropropylene copolymers, and vinylidene fluoride / tetrafluoroethylene / hexafluoropropylene copolymers is more preferred.

[0047] The melt flow rate (MFR) of the fluororesin is preferably 0.1 g / 10 min to 100 g / 10 min, more preferably 0.1 g / 10 min to 50 g / 10 min.

[0048] The MFR is determined according to ASTM D3307-01. The mass (g / 10 minutes) of the polymer flowing out from a nozzle having an inner diameter of 2 mm and a length of 8 mm at 297° C. and a load of 5 kg per 10 minutes is the MFR.

[0049] The relative dielectric constant (ε) of the fluororesin at a frequency of 1 kHz and 30° C. is preferably 8 or more, more preferably 9 or more. The upper limit of the relative dielectric constant is not particularly limited, and may be 15, for example.

[0050] The relative dielectric constant is a value calculated as follows: Aluminum is vapor-deposited to a thickness of φ50 mm on the surface of the film formed by molding the fluororesin, and aluminum is vapor-deposited on the entire surface of the opposite surface as a sample, and the capacitance (C) is measured using an LCR meter. The capacitance, electrode area (S), and film thickness (d) are used to calculate the relative dielectric constant using the formula C = ε × ε 0 ×S / d(ε 0 is the vacuum dielectric constant) and the resulting value is the relative dielectric constant.

[0051] The melting point of the fluororesin is preferably 180°C or higher, and the upper limit may be 320°C. The more preferred lower limit is 190°C and the upper limit is 300°C.

[0052] The melting point was measured using a differential scanning calorimeter in accordance with ASTM D-4591 at a heating rate of 10° C. / min, and the temperature corresponding to the peak of the obtained endothermic curve was defined as the melting point.

[0053] The thermal decomposition starting temperature (1% weight loss temperature) of the fluororesin is preferably 360° C. or higher. A more preferred lower limit is 370° C. When the thermal decomposition starting temperature is within the above range, the upper limit can be, for example, 410° C.

[0054] The thermal decomposition starting temperature is the temperature at which 1% by mass of the copolymer in the heating test is decomposed, and is a value obtained by measuring the temperature at which the mass of the copolymer in the heating test decreases by 1% by mass using a differential thermal-thermogravimetric analyzer [TG-DTA].

[0055] The storage modulus (E') of the fluororesin at 170°C measured by dynamic viscoelasticity measurement is preferably 60 MPa to 400 MPa.

[0056] The storage modulus is a value measured at 170°C by dynamic viscoelasticity measurement, more specifically, a value obtained as follows: a sample of 30 mm in length, 5 mm in width, and 0.25 mm in thickness is measured using a dynamic viscoelasticity device in a tensile mode, a clamp width of 20 mm, a measurement temperature of 25°C to 250°C, a heating rate of 2°C / min, and a frequency of 1 Hz, and the value obtained is the storage modulus. The preferred storage modulus (E') at 170°C is 80 MPa to 350 MPa, and the more preferred storage modulus (E') is 100 MPa to 350 MPa.

[0057] The measurement sample can be prepared as follows: for example, the molding temperature is set to a temperature 50°C to 100°C higher than the melting point of the copolymer, a 0.25 mm thick film is molded at a pressure of 3 MPa, and the obtained film is cut into 30 mm long and 5 mm wide to prepare the measurement sample.

[0058] As the fluororesin, a vinylidene fluoride / tetrafluoroethylene copolymer (VdF / TFE copolymer) is preferred from the viewpoint of excellent high dielectric properties, low static friction coefficient, and high dielectric breakdown strength.

[0059] The molar ratio of vinylidene fluoride units to tetrafluoroethylene units in the VdF / TFE copolymer is preferably 5 / 95 to 95 / 5, more preferably 10 / 90 to 90 / 10, and even more preferably 10 / 90 to 49 / 51. It is more preferably 20 / 80 or more (with respect to 100 mol% of the total of the VdF unit and the TFE unit, the VdF unit is 20 mol% or more, and the TFE unit is 80 mol% or less), and even more preferably 45 / 55 or less (with respect to 100 mol% of the total of the VdF unit and the TFE unit, the VdF unit is 45 mol% or less, and the TFE unit is 55 mol% or more).

[0060] The VdF / TFE copolymer preferably further comprises copolymerized units of an ethylenically unsaturated monomer (except tetrafluoroethylene and vinylidene fluoride).

[0061] The content of the copolymerized units of the ethylenically unsaturated monomers may be 0 to 50 mol%, 0 to 40 mol%, 0 to 30 mol%, 0 to 15 mol%, 0 to 10 mol%, or 0 to 5 mol% relative to the total copolymerized units. The content of the copolymer of the ethylenically unsaturated monomers may also be 0.1 mol% or more.

[0062] The ethylenically unsaturated monomer is not particularly limited as long as it is a monomer copolymerizable with tetrafluoroethylene and vinylidene fluoride, but is preferably at least one selected from the group consisting of ethylenically unsaturated monomers represented by the following formulae (1) and (2).

[0063] Formula (1): CX 1 X 2 =CX 3 (CF 2 ) n X 4 (1)

[0064] (Where X 1 , X 2 , X 3 and X 4 The same or different, represents H, F or Cl, and n represents an integer from 0 to 8. However, tetrafluoroethylene and vinylidene fluoride are not included.)

[0065] Formula (2): CF 2 =CF-ORf 1 (2)

[0066] (Where Rf1 represents an alkyl group having 1 to 3 carbon atoms or a fluorinated alkyl group having 1 to 3 carbon atoms.

[0067] The ethylenically unsaturated monomer represented by formula (1) is preferably selected from the group consisting of CF 2 =CFCl, CF 2 =CFCF 3 , at least one of the group consisting of the following formula (3) and the following formula (4), more preferably selected from CF 2 =CFCl, CH 2 =CFCF 3 , CH 2 =CH-C 4 F 9 , CH 2 =CH-C 6 F 13 , CH 2 =CF-C 3 F 6 H and CF 2 =CFCF 3 At least one of the group consisting of, more preferably selected from CF 2 =CFCl, CH 2 =CH-C 6 F 13 and CH 2 =CFCF 3 At least one of .

[0068] CH 2 =CF-(CF 2 ) n X 4 (3)

[0069] (Where X 4 and n are the same as above)

[0070] CH 2 =CH-(CF 2 ) n X 4 (4)

[0071] (Where X 4 and n are the same as above)

[0072] The ethylenically unsaturated monomer represented by formula (2) is preferably selected from the group consisting of CF 2 =CF-OCF 3 CF 2 =CF-OCF 2 CF 3 and CF 2 =CF-OCF 2CF 2 CF 3 At least one of the group consisting of.

[0073] The above-mentioned VdF / TFE copolymer preferably comprises

[0074] 55.0 mol% to 90.0 mol% of tetrafluoroethylene,

[0075] 5.0 mol% to 44.9 mol% of vinylidene fluoride and

[0076] A copolymer containing 0.1 mol% to 10.0 mol% of copolymerized units of an ethylenically unsaturated monomer represented by formula (1).

[0077] CX 1 X 2 =CX 3 (CF 2 ) n X 4 (1)

[0078] (Where X 1 , X 2 , X 3 and X 4 The same or different, represents H, F or Cl, and n represents an integer from 0 to 8. However, tetrafluoroethylene and vinylidene fluoride are not included.)

[0079] More preferably, it comprises

[0080] 55.0 mol% to 85.0 mol% of tetrafluoroethylene,

[0081] 10.0 mol% to 44.9 mol% of vinylidene fluoride and

[0082] A copolymer containing 0.1 mol% to 5.0 mol% of copolymerized units of an ethylenically unsaturated monomer represented by formula (1).

[0083] More preferably, it comprises

[0084] 55.0 mol% to 85.0 mol% of tetrafluoroethylene,

[0085] 13.0 mol% to 44.9 mol% of vinylidene fluoride and

[0086] A copolymer containing 0.1 mol% to 2.0 mol% of copolymerized units of an ethylenically unsaturated monomer represented by formula (1).

[0087] From the viewpoint of improving the mechanical strength of the VdF / TFE copolymer at high and low temperatures, the ethylenically unsaturated monomer represented by formula (1) is preferably selected from the group consisting of CH 2 =CH-C 4 F9 , CH 2 =CH-C 6 F 13 and CH 2 =CF-C 3 F 6 More preferably, the ethylenically unsaturated monomer represented by formula (1) is selected from CH 2 =CH-C 4 F 9 , CH 2 =CH-C 6 F 13 and CH 2 =CF-C 3 F 6 H, and the copolymer is composed of at least one monomer of the group

[0088] 55.0 mol% to 80.0 mol% of tetrafluoroethylene,

[0089] 19.5 mol% to 44.9 mol% of vinylidene fluoride and

[0090] A copolymer containing 0.1 mol% to 0.6 mol% of copolymerization units of an ethylenically unsaturated monomer represented by formula (1).

[0091] The above-mentioned VdF / TFE copolymer may also be

[0092] 58.0 mol% to 85.0 mol% of tetrafluoroethylene,

[0093] 10.0 mol% to 41.9 mol% of vinylidene fluoride and

[0094] A copolymer containing 0.1 mol% to 5.0 mol% of copolymerized units of an ethylenically unsaturated monomer represented by formula (1).

[0095] The above-mentioned VdF / TFE copolymer also preferably comprises

[0096] 55.0 mol% to 90.0 mol% of tetrafluoroethylene,

[0097] 9.2 mol% to 44.2 mol% of vinylidene fluoride and

[0098] A copolymer containing 0.1 mol% to 0.8 mol% of copolymerized units of an ethylenically unsaturated monomer represented by formula (2).

[0099] CF 2 =CF-ORf 1 (2)

[0100] (Where Rf 1represents an alkyl group having 1 to 3 carbon atoms or a fluorinated alkyl group having 1 to 3 carbon atoms.

[0101] More preferably, it comprises

[0102] 58.0 mol% to 85.0 mol% of tetrafluoroethylene,

[0103] 14.5 mol% to 39.9 mol% of vinylidene fluoride and

[0104] 0.1 mol% to 0.5 mol% of an ethylenically unsaturated monomer represented by formula (2)

[0105] Copolymers of copolymer units.

[0106] The above-mentioned VdF / TFE copolymer also preferably comprises

[0107] 55.0 mol% to 90.0 mol% of tetrafluoroethylene,

[0108] 5.0 mol% to 44.8 mol% of vinylidene fluoride,

[0109] 0.1 mol% to 10.0 mol% of an ethylenically unsaturated monomer represented by formula (1) and

[0110] A copolymer containing 0.1 mol% to 0.8 mol% of copolymerized units of an ethylenically unsaturated monomer represented by formula (2).

[0111] More preferably, it comprises

[0112] 55.0 mol% to 85.0 mol% of tetrafluoroethylene,

[0113] 9.5 mol% to 44.8 mol% of vinylidene fluoride,

[0114] 0.1 mol% to 5.0 mol% of an ethylenically unsaturated monomer represented by formula (1) and

[0115] A copolymer containing 0.1 mol% to 0.5 mol% of copolymerized units of an ethylenically unsaturated monomer represented by formula (2).

[0116] More preferably, it comprises

[0117] 55.0 mol% to 80.0 mol% of tetrafluoroethylene,

[0118] 19.8 mol% to 44.8 mol% of vinylidene fluoride,

[0119] 0.1 mol% to 2.0 mol% of an ethylenically unsaturated monomer represented by formula (1) and

[0120] A copolymer containing 0.1 mol% to 0.3 mol% of copolymerized units of an ethylenically unsaturated monomer represented by formula (2). When the copolymer has such a composition, the low permeability is particularly excellent.

[0121] The above copolymer may also be

[0122] 58.0 mol% to 85.0 mol% of tetrafluoroethylene,

[0123] 9.5 mol% to 39.8 mol% of vinylidene fluoride,

[0124] 0.1 mol% to 5.0 mol% of an ethylenically unsaturated monomer represented by formula (1) and

[0125] A copolymer containing 0.1 mol% to 0.5 mol% of copolymerized units of an ethylenically unsaturated monomer represented by formula (2).

[0126] The fluororesin film of the present invention may be a film consisting essentially of only fluororesin, or may contain other components than fluororesin. The fluororesin film of the present invention preferably contains 50% by mass or more of fluororesin.

[0127] Next, more preferred embodiments of the present invention will be described.

[0128] The fluororesin film of the present invention may further contain inorganic particles. By mixing inorganic particles in the fluororesin film, a fluororesin film having the above-mentioned ten-point average roughness and arithmetic mean roughness can be produced, and the winding property can be improved. In addition, by containing inorganic particles, the mechanical strength characteristics are improved.

[0129] From the perspective of obtaining a fluororesin film having the above-mentioned ten-point average roughness and arithmetic mean roughness, the content of the inorganic particles is preferably 0.01 to 5 parts by mass relative to 100 parts by mass of the fluororesin, more preferably 0.05 to 4 parts by mass, and even more preferably 0.1 to 3 parts by mass relative to 100 parts by mass of the fluororesin.

[0130] Examples of the inorganic particles include silica, high dielectric inorganic particles, and reinforcing fillers.

[0131] From the perspective of improving the winding property of the film without damaging the mechanical strength of the film, the above-mentioned silicon dioxide is preferred. From the perspective of the winding property and dielectric breakdown strength of the film, the content of silicon dioxide is preferably 0.01 to 1 part by mass, more preferably 0.1 part by mass or more, relative to 100 parts by mass of the fluororesin. In addition, if the amount added is too much, the interface with the additive becomes larger, which may cause defects.

[0132] As the above-mentioned high dielectric inorganic particles, barium titanate oxide particles, strontium titanate oxide particles, etc. can be cited. From the aspect of film winding property and dielectric breakdown strength, the content of high dielectric inorganic particles is preferably 0.1 to 10 parts by mass relative to 100 parts by mass of fluororesin. In addition, if the addition amount is too much, the interface with the additive becomes larger, which may cause defects.

[0133] If the above-mentioned barium titanate oxide particles are contained, the dielectric constant is improved, but an increase in dielectric loss and a decrease in withstand voltage are observed. Therefore, for the content of the above-mentioned barium titanate oxide particles, the upper limit is about 10 parts by mass relative to 100 parts by mass of fluororesin. In addition, from the perspective of the improvement effect of winding and dielectric constant improvement, the content of barium titanate oxide particles is preferably 0.1 parts by mass or more. In addition, if the addition amount is too much, the interface with the additive becomes larger, which may cause defects.

[0134] It is also one of the preferred methods to emboss the fluororesin film of the present invention. By embossing, a fluororesin film having the above-mentioned ten-point average roughness and arithmetic mean roughness can be manufactured, the static friction coefficient can be reduced, and the winding property can be improved. In addition, by embossing, the generation of wrinkles during film processing can be suppressed, thereby reducing defects and improving reliability. The above-mentioned embossing can be performed in a manner that the fluororesin film satisfies the above-mentioned ten-point average roughness, arithmetic mean roughness and dielectric breakdown strength, and conventional embossing can be used.

[0135] Specifically, an embossing roller having irregularities such as stripes, pear-skin roughness, square, wave, trapezoid, diamond, cloth pattern, silk pattern, oblique lines, dots, etc. is pressed against the film at room temperature and humidity, thereby embossing the film surface.

[0136] If excessively deep depressions are formed during embossing, the film thickness becomes thinner and the dielectric breakdown strength of the portion decreases. Therefore, the depressions during embossing are preferably within 5% of the film thickness.

[0137] It is also one of the preferred embodiments that the fluororesin film of the present invention is surface coated. By surface coating, a fluororesin film having the above-mentioned ten-point average roughness and arithmetic mean roughness can be manufactured, the static friction coefficient can be reduced, and the winding property can be improved. In addition, by surface coating, the characteristics of the dielectric breakdown strength are improved. As long as the above-mentioned surface coating can be carried out in a manner that satisfies the above-mentioned ten-point average roughness, arithmetic mean roughness and dielectric breakdown strength, existing surface coating can be used.

[0138] Specifically, the solution dispersed with nanoparticles is applied to the film surface, and dried above the boiling point of the solvent, so that it can be applied to the film surface. As nanoparticles, preferably the particle diameter is below 500nm, and silicon dioxide, aluminum oxide, zirconium oxide, titanium oxide, zinc oxide, etc. can be cited. And the solvent is not limited, but if it cannot be evenly applied to the film surface, it will cause unevenness, so it is preferred that the ether-based and ketone-based solvents that are not easy to shrink on the fluororesin film. In addition, only by sharing nanoparticles and solvents, the surface coating does not adhere to the film surface, and thus it is necessary to add a binder. As an example of a binder, polyvinylidene fluoride can be cited.

[0139] It is one of the preferred embodiments that the fluororesin film of the present invention contains two fluororesins as the fluororesins. By containing two fluororesins, a fluororesin film having the above-mentioned ten-point average roughness and arithmetic mean roughness can be manufactured, the static friction coefficient can be reduced, and the winding property can be improved. In addition, when containing two fluororesins, it is not easy to tear when processed into a film, and a fluororesin film with excellent mechanical strength can be obtained.

[0140] The two fluororesins are preferably mutually compatible polymers. By using mutually compatible polymers, it is more difficult to tear and a fluororesin film with excellent mechanical strength can be obtained.

[0141] In this specification, "mutually compatible" means that two fluororesins are melted and uniformly mixed with each other.

[0142] The fluororesin preferably includes an uncrosslinked fluororesin and a crosslinked fluororesin. When the uncrosslinked fluororesin and the crosslinked fluororesin are included, since they are not a composite of other materials but the same fluoromaterial, a film with few defects and little interface formation can be obtained.

[0143] The cross-linked fluororesin can be produced, for example, by irradiating an uncross-linked fluororesin with electron beams. That is, the cross-linked fluororesin can be a substance irradiated with electron beams. For cross-linking using electron beams, the absorbed dose is preferably in the range of 20 kGy to 100 kGy at room temperature. By irradiating with electron beams, a three-dimensional network is formed between molecular chains, which can increase the yield point stress and elastic modulus.

[0144] In addition, the crosslinked fluororesin can also be produced by adding a crosslinking agent and subjecting it to heat curing or ultraviolet curing. Examples of the crosslinking agent include dialkyl peroxides, triallyl isocyanurate, and peroxyesters.

[0145] Since a fluororesin film with good compatibility and excellent mechanical strength can be obtained, the uncrosslinked fluororesin and the crosslinked fluororesin are preferably fluororesins having the same polymerization unit, more preferably fluororesins both having VdF units, and preferably both being VdF / TFE copolymers. In addition, the uncrosslinked fluororesin and the crosslinked fluororesin preferably have the same composition ratio. The composition ratio can be the composition ratio described for the fluororesin.

[0146] In this specification, "crosslinking" refers to a state in which molecular chains are connected to form a three-dimensional network.

[0147] From the perspective of dielectric breakdown strength and mechanical strength of the fluororesin film, the cross-linked fluororesin is preferably 0.01% to 10% by mass relative to the total of the cross-linked fluororesin and the uncross-linked fluororesin. It is more preferably 0.03% by mass or more, further preferably 0.05% by mass or more, and particularly preferably 0.1% by mass or more. In addition, if the amount added is too much, the interface with the additive becomes larger, which may cause defects, and is therefore more preferably 10% by mass or less, further preferably 8% by mass or less, and particularly preferably 5% by mass or less.

[0148] It is also one of the preferred embodiments that the fluororesin film of the present invention contains two types of fluororesins having different melt flow rates as the fluororesins.

[0149] From the perspective of dielectric breakdown strength and mechanical strength of the fluororesin film, the fluororesin preferably has a melt flow rate of 2.0 g / 10 min to 30.0 g / 10 min for one and a melt flow rate of 0.1 g / 10 min to 1.9 g / 10 min for the other. In addition, preferably, the melt flow rate of one is 2.0 g / 10 min to 20.0 g / 10 min and the melt flow rate of the other is 0.1 g / 10 min to 1.9 g / 10 min. More preferably, the melt flow rate of one is 2.1 g / 10 min to 10.0 g / 10 min and the melt flow rate of the other is 0.5 g / 10 min to 1.8 g / 10 min.

[0150] From the viewpoint of dielectric breakdown strength and mechanical strength of the fluororesin film, the amount of the other fluororesin having a smaller melt flow rate is preferably 0.1 to 10 mass %, more preferably 0.5 to 8 mass %, and still more preferably 1 to 5 mass %, relative to 100 mass % of the total fluororesin.

[0151] It is also one of the preferred embodiments that the fluororesin film of the present invention contains, as the fluororesin, two types of fluororesins having different composition ratios of polymerized units.

[0152] From the viewpoint of dielectric breakdown strength and mechanical strength of the fluororesin film, the fluororesin contains polymerized units derived from VdF, and preferably contains two polymers having polymerized units derived from VdF in different proportions.

[0153] In the case of fluororesins containing polymer units based on VdF in different proportions, the content of the polymer containing polymer units based on VdF in a small proportion is preferably 0.1 to 10% by mass, more preferably 0.5 to 8% by mass, based on the total amount of the fluororesin, from the aspects of the dielectric breakdown strength and mechanical strength of the fluororesin film and from the aspect that if the amount added is too large, the interface with the additive becomes large and defects occur.

[0154] From the aspects of dielectric breakdown strength and mechanical strength of the fluororesin film, it is more preferred that one of the fluororesins is a VdF / TFE copolymer in which the molar ratio of vinylidene fluoride (VdF) units / tetrafluoroethylene (TFE) units is 35.0 / 65.0 to 50.0 / 50.0, and the other is a VdF / TFE copolymer in which the molar ratio of VdF units / TFE units is 10.0 / 90.0 or more and less than 35.0 / 65.0 (relative to 100 mol % of the total of VdF units and TFE units, the VdF units are 10.0 mol % or more and less than 35.0 mol %, and the TFE units are 90.0 mol % or less and more than 65.0 mol %).

[0155] It is also preferred that one of the fluororesins is a vinylidene fluoride / tetrafluoroethylene copolymer having a vinylidene fluoride unit / tetrafluoroethylene unit molar ratio of 95.0 / 5.0 to 39.0 / 61.0, and the other is a vinylidene fluoride / tetrafluoroethylene copolymer having a vinylidene fluoride unit / tetrafluoroethylene unit molar ratio of 38.9 / 61.1 to 5.0 / 95.0.

[0156] It is also preferred that one of the fluororesins is a vinylidene fluoride / tetrafluoroethylene copolymer having a vinylidene fluoride unit / tetrafluoroethylene unit molar ratio of 50.0 / 50.0 to 39.0 / 61.0, and the other is a vinylidene fluoride / tetrafluoroethylene copolymer having a vinylidene fluoride unit / tetrafluoroethylene unit molar ratio of 38.9 / 61.1 to 10.0 / 90.0.

[0157] The vinylidene fluoride / tetrafluoroethylene copolymers preferably further contain copolymerization units of ethylenically unsaturated monomers (except tetrafluoroethylene and vinylidene fluoride), and the content of the copolymerization units of the ethylenically unsaturated monomers is preferably 0.1 mol % to 5.0 mol % based on all copolymerization units.

[0158] The fluororesin film of the present invention also preferably contains a vinylidene fluoride / tetrafluoroethylene copolymer and polyvinylidene fluoride as the fluororesin. When the vinylidene fluoride / tetrafluoroethylene copolymer and polyvinylidene fluoride are used in combination, the mechanical properties of the fluororesin film are further improved.

[0159] The content of polyvinylidene fluoride is preferably 0.1% to 10% by mass, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more, more preferably 8% by mass or less, and particularly preferably 6% by mass or less, relative to the total of the vinylidene fluoride / tetrafluoroethylene copolymer and polyvinylidene fluoride.

[0160] In this specification, polyvinylidene fluoride refers to a polymer composed only of monomer units based on vinylidene fluoride.

[0161] The fluororesin film of the present invention also preferably contains a vinylidene fluoride / tetrafluoroethylene copolymer and a hexafluoropropylene / tetrafluoroethylene copolymer (FEP) as the fluororesin. When a vinylidene fluoride / tetrafluoroethylene copolymer and a hexafluoropropylene / tetrafluoroethylene copolymer are used in combination, the mechanical properties of the fluororesin film are further improved.

[0162] For the hexafluoropropylene / tetrafluoroethylene copolymer, if the addition amount is too much, the interface with the additive becomes larger, which may cause defects, so the total amount of the vinylidene fluoride / tetrafluoroethylene copolymer and the hexafluoropropylene / tetrafluoroethylene copolymer is preferably 0.1% to 10% by mass, more preferably 0.5% by mass or more, and further preferably 1% by mass or more. In addition, it is more preferably 8% by mass or less, and particularly preferably 6% by mass or less.

[0163] The above-mentioned hexafluoropropylene / tetrafluoroethylene copolymer (FEP) contains tetrafluoroethylene (TFE) units and hexafluoropropylene (HFP) units.

[0164] The mass ratio (TFE / HFP) of the TFE unit to the HFP unit in the FEP is preferably 70 to 99 / 1 to 30 (mass %), and more preferably 85 to 95 / 5 to 15 (mass %).

[0165] The FEP is also preferably a TFE / HFP / PAVE copolymer further comprising a perfluoroalkyl vinyl ether (PAVE) unit in addition to the TFE unit and the HFP unit. Examples of the PAVE unit contained in the FEP include at least one unit selected from the group consisting of general formula (5) and general formula (6).

[0166] CF 2 =CFO(CF 2 CFY 1 O) p -(CF 2 CF2 CF 2 O) q -R f (5)

[0167] (Where Y 1 Indicates F or CF 3 , R f represents a perfluoroalkyl group having 1 to 5 carbon atoms. p represents an integer of 0 to 5, and q represents an integer of 0 to 5. )

[0168] CFX=CXOCF 2 OR 1 (6)

[0169] (wherein, X is the same or different, representing F or CF 3 , R 1 represents a linear or branched perfluoroalkyl group having 1 to 6 carbon atoms, or a cyclic perfluoroalkyl group having 5 or 6 carbon atoms.

[0170] Specific examples thereof include perfluoro(methyl vinyl ether) [PMVE], perfluoro(ethyl vinyl ether) [PEVE], perfluoro(propyl vinyl ether) [PPVE], and perfluoro(butyl vinyl ether) [PBVE].

[0171] Among them, as the above-mentioned PAVE, substances having a bulky side chain are preferred, and specifically, PPVE is preferred.

[0172] For the above-mentioned FEP, the total amount of the polymerization units based on TFE, HFP and PAVE is preferably 90 mol% or more, more preferably 95 mol% or more relative to the total polymerization units. The above-mentioned FEP may be composed only of polymerization units based on TFE and HFP, or may be composed only of polymerization units based on TFE, HFP and PAVE.

[0173] When the FEP is a TFE / HFP / PAVE copolymer, the mass ratio (TFE / HFP / PAVE) is preferably 70 to 99.8 / 0.1 to 25 / 0.1 to 25 (mass %). Within the above range, heat resistance is further improved.

[0174] The mass ratio (TFE / HFP / PAVE) is more preferably 75 to 98 / 1.0 to 15 / 1.0 to 10 (mass %).

[0175] The TFE / HFP / PAVE copolymer contains 1% by mass or more of HFP units and PAVE units in total.

[0176] The TFE / HFP / PAVE copolymer preferably has an HFP unit of 25% by mass or less of all monomer units. If the content of the HFP unit is within the above range, the heat resistance is more excellent. The content of the HFP unit is more preferably 20% by mass or less, and further preferably 18% by mass or less. It is particularly preferably 15% by mass or less. In addition, the content of the HFP unit is preferably 0.1% by mass or more, and more preferably 1% by mass or more. It is particularly preferably 2% by mass or more.

[0177] In addition, the content of the HFP unit can be measured by the 19F-NMR method.

[0178] In the above-mentioned TFE / HFP / PAVE copolymer, the content of PAVE units is more preferably 20% by mass or less, and further preferably 10% by mass or less. It is particularly preferably 3% by mass or less. In addition, the content of PAVE units is preferably 0.1% by mass or more, and more preferably 1% by mass or more. It should be noted that the content of PAVE units can be measured by 19F-NMR method.

[0179] The above-mentioned FEP may further contain other ethylenic monomer (α) units.

[0180] The other olefinic monomer (α) units are not particularly limited as long as they are monomer units copolymerizable with the TFE units and the HFP units. In the case of a TFE / HFP / PAVE copolymer, they are not particularly limited as long as they are monomer units copolymerizable with the PAVE units. Examples thereof include fluorinated olefinic monomers such as vinyl fluoride [VF], VdF, and chlorotrifluoroethylene [CTFE], and non-fluorinated olefinic monomers such as ethylene, propylene, and alkyl vinyl ethers.

[0181] When the above copolymer is a TFE / HFP / PAVE / other ethylenic monomer (α) copolymer, the mass ratio (TFE / HFP / PAVE / other ethylenic monomer (α)) is preferably 70 to 98 / 0.1 to 25 / 0.1 to 25 / 0.1 to 25 (mass %), more preferably 70 to 98 / 0.1 to 25 / 0.1 to 20 / 0.1 to 15 (mass %), and further preferably 70 to 98 / 0.1 to 20 / 0.1 to 10 / 0.1 to 5 (mass %).

[0182] The TFE / HFP copolymer contains polymerized units other than TFE units in an amount of 1% by mass or more in total.

[0183] The melting point of the FEP is preferably 200° C. to 300° C., more preferably 210° C. or higher, and even more preferably 220° C. or higher. It is more preferably 280° C. or lower, and particularly preferably 270° C. or lower.

[0184] The melting point is a temperature corresponding to a maximum value in a heat of fusion curve when the temperature is increased at a rate of 10° C. / min using a differential scanning calorimeter [DSC].

[0185] The glass transition temperature (Tg) of the FEP is preferably 60° C. to 110° C., more preferably 65° C. or higher, and more preferably 100° C. or lower. The glass transition temperature is a value measured by dynamic viscoelasticity measurement.

[0186] The FEP can be produced, for example, by appropriately mixing monomers that will serve as structural units thereof and additives such as a polymerization initiator and performing a conventionally known method such as emulsion polymerization, solution polymerization or suspension polymerization.

[0187] The melt flow rate (MFR) of the FEP is preferably 0.1 to 10, more preferably 0.5 or more, and even more preferably 1 or more. It is more preferably 5 or less, and particularly preferably 3 or less.

[0188] The MFR is determined according to ASTM D3307-01. The mass (g / 10 minutes) of the polymer flowing out from a nozzle having an inner diameter of 2 mm and a length of 8 mm at 297° C. and a load of 5 kg per 10 minutes is the MFR.

[0189] In addition, the fluororesin film of the present invention also preferably contains a vinylidene fluoride / tetrafluoroethylene copolymer and a perfluoroalkyl vinyl ether / tetrafluoroethylene copolymer (PFA) as the fluororesin. When a vinylidene fluoride / tetrafluoroethylene copolymer and a perfluoroalkyl vinyl ether / tetrafluoroethylene copolymer are used together, the surface roughness of the film increases and the friction coefficient decreases, thereby improving the handleability of the film.

[0190] Regarding the perfluoroalkyl vinyl ether / tetrafluoroethylene copolymer, if the amount added is too much, the interface with the additive becomes larger, which may cause defects, so the total amount of the vinylidene fluoride / tetrafluoroethylene copolymer and the perfluoroalkyl vinyl ether / tetrafluoroethylene copolymer is preferably 0.1% to 10% by mass, more preferably 0.3% by mass or more, and further preferably 0.5% by mass or more. In addition, it is more preferably 8% by mass or less, and particularly preferably 6% by mass or less.

[0191] Examples of PAVE constituting the PFA include at least one selected from the group consisting of general formula (5) and general formula (6).

[0192] CF 2 =CFO(CF 2 CFY 1 O) p -(CF 2 CF 2 CF 2 O) q -Rf (5)

[0193] (Where Y 1 Indicates F or CF 3 , R f represents a perfluoroalkyl group having 1 to 5 carbon atoms. p represents an integer of 0 to 5, and q represents an integer of 0 to 5. )

[0194] CFX=CXOCF 2 OR 1 (6)

[0195] (wherein, X is the same or different, representing F or CF 3 , R 1 represents a linear or branched perfluoroalkyl group having 1 to 6 carbon atoms, or a cyclic perfluoroalkyl group having 5 or 6 carbon atoms.

[0196] Specific examples thereof include perfluoro(methyl vinyl ether) [PMVE], perfluoro(ethyl vinyl ether) [PEVE], perfluoro(propyl vinyl ether) [PPVE], and perfluoro(butyl vinyl ether) [PBVE].

[0197] Among them, as the above-mentioned PAVE, substances having a bulky side chain are preferred, and specifically, PPVE is preferred.

[0198] The PFA preferably contains 1.0% by mass to 10% by mass of polymerized units based on PAVE relative to all polymerized units.

[0199] The amount of the PAVE-based polymerized units relative to all polymerized units is more preferably 2.0% by mass or more, further preferably 3.5% by mass or more, particularly preferably 4.0% by mass or more, and most preferably 5.0% by mass or more, and more preferably 8.0% by mass or less, further preferably 7.0% by mass or less, particularly preferably 6.5% by mass or less, and most preferably 6.0% by mass or less. It should be noted that the amount of the PAVE-based polymerized units is determined by 19 The measurement was carried out by F-NMR method.

[0200] For the above-mentioned PFA, the total amount of the polymerization units based on TFE and PAVE is preferably 90 mol% or more, and more preferably 95 mol% or more relative to all polymerization units. The above-mentioned PFA is also preferably composed of polymerization units based on TFE and PAVE only. It should be noted that the above-mentioned PFA does not contain HFP units.

[0201] The above PFA can be used with respect to the main chain carbon number 10 6 The unstable terminal groups are -COF, -COOH, -CF2 H. -COOCH 3 、-CH 2 OH, -CONH 2 , -CF=CF 2 The above number is the total number of these unstable terminal groups. The above number can be 20 or less, or 10 or less. The lower limit can be 0. In particular, from the perspective of low dielectric loss tangent in the high frequency region (above 10 GHz), relative to the number of main chain carbon atoms 10 6 PFA having 20 or less unstable terminal groups is preferred.

[0202] The number of the unstable terminal groups can be determined by infrared spectroscopy.

[0203] First, the copolymer is melt-extruded to produce a film with a thickness of 0.25 mm to 0.3 mm. The film is analyzed by Fourier transform infrared spectroscopy to obtain an infrared absorption spectrum of the copolymer, and a differential spectrum with a background spectrum that is completely fluorinated and does not contain unstable terminal groups is obtained. According to the following formula (A), the absorption peak of the specific unstable terminal group appearing in the differential spectrum is used to calculate the number of 10% of the copolymer. 6 The number N of unstable terminal groups per carbon atom.

[0204] N=I×K / t (A)

[0205] I: Absorbance

[0206] K: Correction coefficient

[0207] t: film thickness (mm)

[0208] The melting point of the PFA is preferably 280°C to 322°C.

[0209] The melting point is more preferably 290°C or higher, and more preferably 315°C or lower.

[0210] The melting point is a temperature corresponding to a maximum value in a heat of fusion curve when the temperature is increased at a rate of 10° C. / min using a differential scanning calorimeter [DSC].

[0211] The glass transition temperature (Tg) of the PFA is preferably 70° C. to 110° C. The glass transition temperature is more preferably 80° C. or higher, and more preferably 100° C. or lower.

[0212] The above-mentioned glass transition temperature is a value measured by dynamic viscoelasticity measurement.

[0213] The PFA can be produced, for example, by appropriately mixing monomers that will serve as structural units thereof and additives such as a polymerization initiator and performing a conventionally known method such as emulsion polymerization or suspension polymerization.

[0214] The fluororesin film of the present invention may also include other polymers other than the fluororesin. As other polymers, for example, polycarbonate (PC), polyester, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), silicone resin, polyether, polyvinyl acetate, polyethylene, polypropylene (PP) etc. are preferred in order to improve flexibility, poly (methyl) acrylate, epoxy resin, polyoxyethylene, polypropylene oxide, polyphenylene ether (PPO), polyphenylene sulfide (PPS), polyamide (PA), polyimide (PI), polyamide-imide (PAI), PC, polystyrene, polybenzimidazole (PBI) etc. can be cited in order to improve strength, and odd-numbered polyamide, cyanoplulan, copper phthalocyanine polymer etc. can be cited in addition from the aspect of supplementing high dielectric properties.

[0215] The mass ratio of the fluororesin to the other polymer is preferably 50 / 50 to 99 / 1, more preferably 75 / 25 to 99 / 1.

[0216] The fluororesin film of the present invention may also contain an affinity enhancer. Examples of the affinity enhancer include coupling agents, functional group-modified polyolefins, styrene-modified polyolefins, functional group-modified polystyrenes, polyacrylic acid imide, cumylphenol, etc., which may be contained within a range that does not impair the effects of the present invention. It should be noted that, from the perspective of withstand voltage, it is more preferred not to contain these components.

[0217] The thickness of the fluororesin film of the present invention is preferably 100 μm or less, more preferably 50 μm or less, further preferably 30 μm or less, and particularly preferably 10 μm or less. The thickness of the fluororesin film may also be 1 μm or more. The above thickness can be measured using a digital length measuring instrument.

[0218] The relative dielectric constant (ε) of the fluororesin film of the present invention at a frequency of 1 kHz and 30° C. is preferably 9 or more, more preferably 10 or more.

[0219] The relative dielectric constant is a value calculated as follows: Aluminum is vapor-deposited to a thickness of φ50 mm on the surface of the film, and aluminum is vapor-deposited on the entire opposite surface as a sample, and the capacitance (C) is measured using an LCR meter. The capacitance, electrode area (S), and film thickness (d) are calculated using the formula C = ε × ε 0 ×S / d(ε 0 is the vacuum dielectric constant) and the resulting value is the relative dielectric constant.

[0220] The fluororesin film of the present invention has a volume resistivity at 30° C. of preferably 1E+15 Ω·cm or more, more preferably 2E+15 Ω·cm or more.

[0221] Regarding the volume resistivity, aluminum was deposited on one side of the film in vacuum to prepare a sample. The sample was then placed in a thermostatic chamber (30°C, 25% RH) and a voltage of 50 V / μm was applied to the sample using a digital superinsulator / microammeter to measure the volume resistivity (Ω·cm).

[0222] The fluororesin film of the present invention has a dielectric loss tangent at a frequency of 1 kHz and 150° C. of preferably 7% or less, more preferably 6% or less.

[0223] The dielectric loss tangent is measured using an LCR meter.

[0224] The fluororesin film of the present invention has a tensile elastic modulus at 25° C. in the machine direction (MD) of preferably 800 MPa or more, more preferably 900 MPa or more.

[0225] The tensile modulus can be measured in accordance with ASTM D1708.

[0226] The fluororesin film of the present invention may have an elastic modulus of 800 MPa or more at 25°C in the longitudinal direction (MD) and a thickness of 100 μm or less. The elastic modulus is more preferably 900 MPa or more. The thickness is more preferably 30 μm or less, further preferably 10 μm or less, and preferably 1 μm or more.

[0227] The fluororesin film of the present invention can be produced, for example, by a production method comprising the following steps: a step of embossing a pre-processed film containing a fluororesin or a step of surface coating. The pre-processed film can be obtained, for example, by the following steps: melt extrusion molding a fluororesin to obtain a film. In addition, the film obtained by melt extrusion molding can be further stretched. Melt extrusion molding and stretching are described below.

[0228] In addition, when the fluororesin film of the present invention contains two fluororesins as fluororesins, it can be produced by a production method comprising the following steps: a step of mixing the two fluororesins to obtain a fluororesin mixture; a step of melt-extruding the fluororesin mixture to obtain a film; and a step of obtaining a stretched film by stretching the obtained film.

[0229] The step of obtaining the fluororesin mixture and the step of obtaining the film may be performed separately or simultaneously. For example, the mixing and melt extrusion molding of the two fluororesins may be performed simultaneously using a melt extrusion molding machine.

[0230] The melt extrusion molding can be performed at 250°C to 380°C.

[0231] The melt extrusion molding can be performed using a melt extrusion molding machine, preferably with a cylinder temperature of 250°C to 350°C and a die temperature of 300°C to 380°C.

[0232] The production method preferably further comprises a step of winding the film obtained by the extrusion molding with a roll. The temperature of the roll is preferably 0 to 180°C.

[0233] After the extrusion molding, the obtained film is stretched to obtain a stretched film. The stretching may be uniaxial stretching or biaxial stretching.

[0234] In the uniaxial stretching, the film is stretched in the same machine direction (MD) as the direction in which the fluororesin is extruded during extrusion molding.

[0235] The stretching ratio in the uniaxial stretching is preferably 2 to 10 times, more preferably 3 times or more.

[0236] The stretching temperature in the uniaxial stretching is preferably 0 to 180°C, more preferably 30°C or higher, and more preferably 120°C or lower.

[0237] In the biaxial stretching, the film is stretched in the transverse direction (TD) perpendicular to the machine direction (MD).

[0238] The stretching ratio in the biaxial stretching is preferably 2 to 10 times, more preferably 3 times or more, in terms of each of the ratios in MD and TD.

[0239] The stretching temperature in the biaxial stretching is preferably 0 to 200°C, more preferably 30°C or higher, and more preferably 120°C or lower.

[0240] The biaxial stretching may be sequential biaxial stretching or simultaneous biaxial stretching.

[0241] As the biaxial stretching method, a tenter-type biaxial stretching method, a tubular biaxial stretching method, or the like can be used, and a tenter-type biaxial stretching method is preferred.

[0242] The stretching temperature in the biaxial stretching is preferably 0 to 200°C, more preferably 30°C or higher, and more preferably 120°C or lower.

[0243] The sequential biaxial stretching method is a method in which the longitudinal stretching (MD direction) is usually performed using the rotation difference of the rolls, and then the end (TD side) of the roll film is clamped with a clamp in the transverse stretching and stretched in the TD direction. Depending on the situation, the stretching in the MD direction may be performed in the order of longitudinal stretching, transverse stretching, and longitudinal stretching.

[0244] The simultaneous biaxial stretching method is a method in which the end portion (TD side) of a rolled film is clamped with clips, and the interval between the clips is widened in both the MD direction and the TD direction, thereby stretching the film.

[0245] The production method preferably further includes a step of heat-fixing the obtained stretched film after the stretching. Heat-fixing can suppress shrinkage of the film due to the influence of heat or the like, thereby improving durability.

[0246] The temperature of the heat setting is preferably 100° C. to 250° C., more preferably 150° C. or higher, and more preferably 200° C. or lower. The heat setting time is preferably short, and in the case of continuous stretching, is preferably 5 minutes or less.

[0247] From the viewpoint of being able to obtain a fluororesin film having the above-mentioned ten-point average roughness, arithmetic mean roughness and dielectric breakdown strength while being able to improve the volume resistivity, the fluororesin film of the present invention is preferably a biaxially stretched film, and more preferably a biaxially stretched film comprising the above-mentioned two fluororesins as the fluororesin.

[0248] The fluororesin film of the present invention is suitable as a high dielectric film or a piezoelectric film.

[0249] When the film of the present invention is used as a piezoelectric film, the film is preferably subjected to a polarization treatment. The polarization treatment can be performed by corona discharge, for example, by applying a voltage to the film using a linear electrode as described in Japanese Patent Publication No. 2011-181748; or by applying a voltage to the film using a needle electrode. After the polarization treatment, a heat treatment can be performed.

[0250] Furthermore, the fluororesin film of the present invention can be suitably used for a film capacitor, an electrowetting device, or a piezoelectric panel.

[0251] The fluororesin film of the present invention has excellent windability due to its low static friction coefficient and is also excellent in dielectric breakdown strength, and can therefore be particularly suitably used as a high dielectric film for film capacitors.

[0252] A film for a film capacitor including an electrode layer on at least one surface of the fluororesin film is also one aspect of the present invention. A film capacitor including the film for a film capacitor is also one aspect of the present invention.

[0253] As the structure of the film capacitor, for example, there can be cited a laminated type in which electrode layers and high dielectric films are alternately laminated (Japanese Patent Publication No. 63-181411, Japanese Patent Publication No. 3-18113, etc.); a wound type in which a strip-shaped high dielectric film and electrode layer are wound (structures disclosed in Japanese Patent Publication No. 60-262414, etc. in which electrodes are not continuously laminated on the high dielectric film, and structures disclosed in Japanese Patent Publication No. 3-286514, etc. in which electrodes are continuously laminated on the high dielectric film, etc.). The wound type film capacitor in which the electrode layer is continuously laminated on the high dielectric film has a simple structure and is relatively easy to manufacture. In the case of the wound type film capacitor, two sheets of high dielectric films with electrodes laminated on one side are usually stacked and wound so that the electrodes are not in contact with each other for manufacturing. If necessary, the winding is fixed so that it does not become loose.

[0254] The electrode layer is not particularly limited, and is usually a layer composed of conductive metals such as aluminum, zinc, gold, platinum, and copper, and is used as a metal foil or as a vapor-deposited metal film. Either the metal foil or the vapor-deposited metal film can be used, and both can be used together. From the perspective of being able to make the electrode layer thinner, thereby increasing the capacitance relative to the volume; having excellent adhesion to the dielectric; and having a small thickness deviation, a vapor-deposited metal film is generally preferred. The vapor-deposited metal film is not limited to one layer, and can be made into multiple layers as needed, for example, in order to make it moisture-resistant, a semiconductor aluminum oxide layer is further formed on the aluminum layer to form an electrode layer (for example, Japanese Patent Publication No. 2-250306, etc.). The thickness of the vapor-deposited metal film is not particularly limited, and is preferably in the range of 100 angstroms to 2,000 angstroms, and more preferably in the range of 200 angstroms to 1,000 angstroms. When the thickness of the vapor-deposited metal film is within this range, the capacitance and strength of the capacitor are balanced, which is suitable.

[0255] When a vapor-deposited metal film is used as the electrode layer, the film formation method is not particularly limited, and for example, vacuum vapor deposition, sputtering, ion plating, etc. can be used. Usually, vacuum vapor deposition is used.

[0256] As vacuum deposition methods, there are batch methods for molded products, semi-continuous methods for long products, and continuous methods, etc., and the semi-continuous method is currently the main method used. The semi-continuous metal deposition method is a method in which metal deposition is performed in a vacuum system, winding is performed, and then the vacuum system is returned to the atmospheric system to take out the deposited film.

[0257] The semi-continuous method can be specifically carried out by referring to FIG. 1 of Japanese Patent No. 3664342, for example, and according to the method described therein.

[0258] When a metal thin film layer is formed on the film, the film surface may be subjected to a treatment for improving adhesion, such as a corona treatment or a plasma treatment. When a metal foil is used as an electrode layer, the thickness of the metal foil is not particularly limited, and is usually in the range of 0.1 μm to 100 μm, preferably 1 μm to 50 μm, and more preferably 3 μm to 15 μm.

[0259] The fixing method is not particularly limited, for example, it can be fixed and structurally protected by sealing with resin or enclosing in an insulating housing. The connection method of the lead wire is also not limited, and examples thereof include welding, ultrasonic crimping, hot crimping, and fixing with tape. The lead wire can also be connected to the electrode in advance before winding. For the case of enclosing in an insulating housing, as needed, the opening can be sealed with a thermosetting resin such as a urethane resin or an epoxy resin to prevent oxidation degradation.

[0260] The fluororesin film of the present invention can be suitably used as a high dielectric film of an electrowetting device.

[0261] The electrowetting device may include: a first electrode; a second electrode; a conductive liquid configured to be movable between the first electrode and the second electrode; and a membrane (high dielectric membrane) of the present invention, configured between the first electrode and the conductive liquid to insulate the first electrode from the second electrode. A water-repellent layer may be provided on the membrane of the present invention. Between the first electrode and the second electrode, an insulating liquid is retained in addition to the conductive liquid, and the conductive liquid and the insulating liquid may constitute two layers.

[0262] The above-mentioned electrowetting device can be used in optical elements, display devices (display screens), variable focus lenses, light modulation devices, optical pickup devices, optical recording and reproducing devices, developing devices, droplet operation devices, and analytical instruments (for example, chemical, biochemical, and biological analytical instruments that require the movement of tiny conductive liquids for sample analysis).

[0263] The fluororesin film of the present invention can be suitably used as a piezoelectric film of a piezoelectric panel.

[0264] The piezoelectric panel may include a first electrode, the fluororesin film (piezoelectric film) of the present invention, and a second electrode in this order. The first electrode is directly or indirectly disposed on one main surface of the film, and the second electrode is directly or indirectly disposed on the other main surface of the film.

[0265] The piezoelectric panel may be used in a touch panel. The touch panel may be used in an input device. The input device having the touch panel may perform input based on a touch position, a touch pressure, or both. The input device having the touch panel may have a position detection unit and a pressure detection unit.

[0266] The input device can be used in electronic devices (e.g., mobile phones (e.g., smartphones), portable information terminals (PDAs), tablet computers, ATMs, ticket vending machines, and car navigation systems). Electronic devices having the input device can operate and work based on touch position, touch pressure, or both.

[0267] In addition, it can also be used as a film in environmental power generation such as vibration power generation, touch sensors, touch panels, touch sensors, dielectric bolometers, thin film speakers, tactile feedback (haptics) and other ferroelectric applications, or electrostrictive actuators.

[0268] Example

[0269] Next, the present invention will be described with reference to Examples, but the present invention is not limited to the Examples.

[0270] Each numerical value in the examples was measured by the following method.

[0271] Monomer composition of fluorinated polymers

[0272] The NMR was performed at a temperature of (melting point of polymer + 20)°C. 19 The F-NMR measurement was determined by appropriately combining elemental analysis with the integrated value of each peak and the type of monomer.

[0273] Melting point

[0274] Thermal measurement was performed using a differential scanning calorimeter in accordance with ASTM D-4591 at a heating rate of 10° C. / min, and the melting point was determined from the peak of the obtained endothermic curve.

[0275] thickness

[0276] The film placed on the substrate was measured at room temperature using a digital length measuring instrument.

[0277] Relative dielectric constant

[0278] Aluminum was deposited on both sides of a film in a vacuum to prepare a sample. The electrostatic capacitance of the sample was measured at 30° C. and a frequency of 1 kHz using an LCR meter. The relative dielectric constant was calculated from the obtained electrostatic capacitances.

[0279] Volume resistivity

[0280] Aluminum was deposited on one side of the film in vacuum to prepare a sample. The sample was then placed in a thermostatic chamber (30°C, 25% RH) and a voltage of 50 V / μm was applied to the sample using a digital superinsulator / microammeter to measure the volume resistivity (Ω·cm).

[0281] The dielectric breakdown strength is a value measured based on JIS C2110.

[0282] The film is placed on the lower electrode, and a weight of 25 mm and 500 g is placed as the upper electrode. The voltage is increased at 100 V / sec at both ends to measure the breakdown voltage. The number of measurements is set to 50 points, and the upper and lower 5 points are removed to calculate the average value, which is divided by the thickness to obtain the insulation breakdown strength.

[0283] The values ​​of the ten-point average roughness and the arithmetic mean roughness are values ​​measured based on JIS B-0601-2001.

[0284] Static friction coefficient

[0285] The static friction coefficient was determined using a surface property measuring machine under the following conditions: speed: 150 mm / min, measuring length: 15.0 mm, roller load: 100 g, roller (width: 60 mm, diameter: 30 mm). During the measurement, the film was also attached to the roller, and the static friction coefficient between the two overlapping films was measured. If the static friction coefficient could not be measured due to the lack of sliding, the evaluation result was set to ×.

[0286] Crystallinity

[0287] The crystallinity was measured by using an X-ray diffractometer and a peak separation method. Specifically, two or more films were overlapped so that the total thickness was 40 μm or more, and the obtained measurement sample was placed on a sample holder, and the crystallinity was calculated from the area ratio of the crystalline part to the amorphous part of the diffraction spectrum obtained by the X-ray diffractometer.

[0288] The components used in Examples and Comparative Examples are as follows.

[0289] Fluororesin (1): VdF / TFE copolymer, VdF / TFE=40.0 / 60.0 (molar ratio), MFR: 2.7 g / 10 min, melting point: 216°C (the structural unit of ethylenically unsaturated monomers other than VdF and TFE is 1 wt% or less)

[0290] additive

[0291] Additive A: Cross-linked fluororesin: A VdF / TFE copolymer (VdF / TFE=40.0 / 60.0 (molar ratio), structural units of ethylenically unsaturated monomers other than VdF and TFE are 1 wt% or less, MFR: 0.8 g / 10 min, melting point: 216°C) is irradiated with 20 kGy of electron beams to obtain a cross-linked fluororesin.

[0292] Additive B: PVDF: MFR: 1g / 10min, melting point: 172°C

[0293] Additive C: VdF polymer 1: VdF / TFE copolymer, VdF / TFE=31.0 / 69.0 (molar ratio), MFR: 1.5 g / 10 min, melting point: 240°C (the structural unit of the ethylenically unsaturated monomer other than VdF and TFE is 1 wt% or less)

[0294] Additive D: VdF polymer 2: VdF / TFE copolymer, VdF / TFE=22.0 / 78.0 (molar ratio), MFR: 1.6 g / 10 min, melting point: 270°C (the structural unit of ethylenically unsaturated monomers other than VdF and TFE is 1 wt% or less)

[0295] Additive E: FEP (hexafluoropropylene / tetrafluoroethylene copolymer), MFR: 1g / 10min, melting point: 260°C

[0296] Example 1

[0297] 1 part by mass of additive A was added to 99 parts by mass of fluororesin (1) pellets, and the mixture was extruded at 290°C to 350°C to obtain a film having a thickness of 85 μm. The film having a thickness of 85 μm was stretched 3.5 times at 60°C using a biaxial stretching machine to obtain a stretched film having a thickness of 9 μm.

[0298] Example 2

[0299] 3 parts by mass of additive A were added to 97 parts by mass of fluororesin (1) pellets, and the mixture was extruded at 290° C. to 350° C. to obtain a film having a thickness of 75 μm. The film having a thickness of 75 μm was stretched 3.5 times at 60° C. using a biaxial stretching machine to obtain a stretched film having a thickness of 7 μm.

[0300] Example 3

[0301] 5 parts by mass of additive A were added to 95 parts by mass of fluororesin (1) pellets, and the mixture was extruded at 290°C to 350°C to obtain a film having a thickness of 80 μm. The film having a thickness of 80 μm was stretched 3.5 times at 60°C using a biaxial stretching machine to obtain a stretched film having a thickness of 8 μm.

[0302] Example 4

[0303] 1 part by mass of additive B was added to 99 parts by mass of fluororesin (1) pellets, and the mixture was extruded by a melt extruder at 290°C to 350°C to obtain a film having a thickness of 85 μm. The film having a thickness of 85 μm was stretched 3.5 times by a biaxial stretching machine at 60°C to obtain a stretched film having a thickness of 10 μm.

[0304] Example 5

[0305] 3 parts by mass of additive B were added to 97 parts by mass of fluororesin (1) pellets, and the pellets were extruded at 290°C to 350°C to obtain a film having a thickness of 80 μm. The film having a thickness of 80 μm was stretched 3.5 times at 60°C using a biaxial stretching machine to obtain a stretched film having a thickness of 9 μm.

[0306] Example 6

[0307] 5 parts by mass of additive B were added to 95 parts by mass of fluororesin (1) pellets, and the mixture was extruded at 290°C to 350°C to obtain a film having a thickness of 85 μm. The film having a thickness of 85 μm was stretched 3.5 times at 60°C using a biaxial stretching machine to obtain a stretched film having a thickness of 10 μm.

[0308] Example 7

[0309] 1 part by mass of additive C was added to 99 parts by mass of fluororesin (1) pellets, and the mixture was extruded by a melt extruder at 290°C to 350°C to obtain a film having a thickness of 80 μm. The film having a thickness of 80 μm was stretched 3.5 times by a biaxial stretching machine at 60°C to obtain a stretched film having a thickness of 8 μm.

[0310] Example 8

[0311] 3 parts by mass of the additive D were added to 97 parts by mass of the fluororesin (1) pellets, and the film was formed by melt extrusion at 290° C. to 350° C. to obtain a film having a thickness of 80 μm. The 80 μm film was stretched 3.5 times at 60° C. by a biaxial stretching machine to obtain a stretched film having a thickness of 8 μm.

[0312] Example 9

[0313] 5 parts by mass of additive C were added to 95 parts by mass of fluororesin (1) pellets, and the mixture was extruded at 290°C to 350°C to obtain a film having a thickness of 85 μm. The 85 μm film was stretched 3.5 times at 60°C using a biaxial stretching machine to obtain a stretched film having a thickness of 9 μm.

[0314] Example 10

[0315] 1 part by mass of the additive D was added to 99 parts by mass of the fluororesin (1) pellets, and the film was formed by melt extrusion at 290°C to 350°C to obtain a film with a thickness of 75 μm. The 75 μm film was stretched 3.5 times at 60°C by a biaxial stretching machine to obtain a stretched film with a thickness of 7 μm.

[0316] Embodiment 11

[0317] 3 parts by mass of the additive D were added to 97 parts by mass of the fluororesin (1) pellets, and the film was formed by melt extrusion at 290° C. to 350° C. to obtain a film having a thickness of 75 μm. The 75 μm film was stretched 3.5 times at 60° C. by a biaxial stretching machine to obtain a stretched film having a thickness of 7 μm.

[0318] Example 12

[0319] 5 parts by mass of the additive D were added to 95 parts by mass of the fluororesin (1) pellets, and the film was formed by melt extrusion at 290°C to 350°C to obtain a film with a thickness of 85 μm. The 85 μm film was stretched 3.5 times at 60°C by a biaxial stretching machine to obtain a stretched film with a thickness of 9 μm.

[0320] Embodiment 13

[0321] 1 part by mass of additive E was added to 99 parts by mass of fluororesin (1) pellets, and the film was formed by melt extrusion at 290°C to 350°C to obtain a film with a thickness of 85 μm. The 85 μm film was stretched 3.5 times at 60°C by a biaxial stretching machine to obtain a stretched film with a thickness of 9 μm.

[0322] Embodiment 14

[0323] 1.5 parts by mass of additive E was added to 99 parts by mass of fluororesin (1) pellets, and the film was formed by melt extrusion at 290°C to 350°C to obtain a film with a thickness of 85 μm. The 85 μm film was stretched 3.5 times at 60°C by a biaxial stretching machine to obtain a stretched film with a thickness of 9 μm.

[0324] Embodiment 15

[0325] 1 part by mass of additive E was added to 99 parts by mass of fluororesin (1) pellets, and the film was formed by melt extrusion at 290°C to 350°C to obtain a film with a thickness of 85 μm. The 85 μm film was stretched 4.0 times at 60°C by a biaxial stretching machine to obtain a stretched film with a thickness of 7 μm.

[0326] Comparative Example 1

[0327] The pelletized resin of fluororesin (1) was formed into a film by a melt extruder at 290°C to 350°C and a film by a T-die extruder to obtain a film with a thickness of 85 μm. The 30 μm film was stretched 3.0 times by a uniaxial stretcher at 60°C to obtain a stretched film with a thickness of 10 μm. The static friction coefficient could not be measured because there was no sliding.

[0328] Comparative Example 2

[0329] 0.05 parts by mass of additive B was added to 99.95 parts by mass of fluororesin (1) pellets, and the film was formed by melt extrusion molding at 290°C to 350°C to obtain a film with a thickness of 29 μm. The 29 μm film was stretched 3.0 times by a uniaxial stretching machine at 60°C to obtain a stretched film with a thickness of 10 μm. The static friction coefficient could not be measured because there was no sliding.

[0330] Comparative Example 3

[0331] 11 parts by mass of additive B was added to 89 parts by mass of fluororesin (1) pellets, and the mixture was extruded by a melt extruder at 290°C to 350°C to obtain a film having a thickness of 30 μm. The 30 μm film was stretched 3.0 times by a uniaxial stretcher at 60°C to obtain a stretched film having a thickness of 11 μm.

[0332] Tables 1 and 2 show the physical properties of the films obtained in Examples and Comparative Examples.

[0333]

[0334]

Table 2

[0335]

Claims

1. A fluororesin film comprising a fluororesin, characterized in that: comprising, as the fluororesin, two fluororesins having different composition ratios of polymerized units, The two fluororesins having different composition ratios of polymerized units are two fluororesins containing polymerized units based on vinylidene fluoride and having different ratios of polymerized units based on vinylidene fluoride, and the content of the fluororesin having a smaller ratio of polymerized units based on vinylidene fluoride is 0.1% by mass to 5% by mass relative to the total amount of the fluororesins. Of the two fluororesins, one is a vinylidene fluoride / tetrafluoroethylene copolymer having a vinylidene fluoride unit / tetrafluoroethylene unit in a molar ratio of 95.0 / 5.0 to 39.0 / 61.0, and a melt flow rate of 2.0 g / 10 minutes to 30.0 g / 10 minutes; and the other is a vinylidene fluoride / tetrafluoroethylene copolymer having a vinylidene fluoride unit / tetrafluoroethylene unit in a molar ratio of 38.9 / 61.1 to 5.0 / 95.0, and a melt flow rate of 0.1 g / 10 minutes to 1.9 g / 10 minutes. The ten-point average roughness of at least one surface is 0.100 μm to 1.200 μm and the arithmetic average roughness is 0.010 μm to 0.050 μm, and the dielectric breakdown strength is 400 V / μm or more.

2. The fluororesin film according to claim 1, wherein The fluororesin is a vinylidene fluoride / tetrafluoroethylene copolymer.

3. The fluororesin film according to claim 2, wherein The fluororesin further comprises a copolymer unit based on an ethylenically unsaturated monomer, wherein the ethylenically unsaturated monomer does not include tetrafluoroethylene and vinylidene fluoride.

4. The fluororesin film according to claim 1, 2 or 3, wherein The fluororesin film further contains inorganic particles.

5. The fluororesin film according to claim 4, wherein The content of the inorganic particles is 0.01 to 5 parts by mass based on 100 parts by mass of the fluororesin.

6. The fluororesin film according to claim 1, 2 or 3, wherein This fluororesin film is embossed.

7. The fluororesin film according to claim 1, 2 or 3, wherein This fluororesin film is surface-coated.

8. The fluororesin film according to claim 1, 2 or 3, wherein The fluororesin film is a biaxially stretched film.

9. The fluororesin film according to claim 1, 2 or 3, wherein The thickness of the fluororesin film is 1 μm to 100 μm.

10. The fluororesin film according to claim 1, 2 or 3, wherein Of the two fluororesins, one is a vinylidene fluoride / tetrafluoroethylene copolymer having a vinylidene fluoride unit / tetrafluoroethylene unit molar ratio of 50.0 / 50.0 to 39.0 / 61.0, and the other is a vinylidene fluoride / tetrafluoroethylene copolymer having a vinylidene fluoride unit / tetrafluoroethylene unit molar ratio of 38.9 / 61.1 to 10.0 / 90.

0.

11. The fluororesin film according to claim 1, 2 or 3, wherein The content of the fluororesin having a small proportion of polymerized units based on vinylidene fluoride is 1% by mass to 5% by mass based on the total amount of the fluororesin.

12. The fluororesin film according to claim 1, 2 or 3, wherein The melting point of the fluororesin is 190°C to 300°C.

13. The fluororesin film according to claim 1, 2 or 3, wherein The fluororesin film has a thickness of 1 μm to 10 μm.

14. The fluororesin film according to claim 1, 2 or 3, wherein The fluororesin film has a ten-point average roughness of at least one surface of the fluororesin film of 0.200 μm to 1.000 μm.

15. The fluororesin film according to claim 1, 2 or 3, wherein The fluororesin film has an arithmetic mean roughness of 0.013 μm to 0.045 μm.

16. The fluororesin film according to claim 1, 2 or 3, wherein The dielectric breakdown strength of the fluororesin film is 500V / μm to 650V / μm.

17. A film for a film capacitor, comprising an electrode layer on at least one surface of the fluororesin film according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 or 16. 18 . A film capacitor comprising the film for a film capacitor according to claim 17 .