Secondary battery
Patent Information
- Application Number
- CN202180009339.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-01-23
- Filing Date
- 2021-01-06
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-01-06
AI Technical Summary
In existing secondary batteries, local deformation of the electrode plates during charging and discharging causes capacity reduction and production stability problems. Increasing the core elongation to suppress deformation may cause concerns about contact between the electrode plates and the outer can.
We designed positive and negative electrode cores with length and width directions, and the active material layer formed on the surface of the core has a higher tensile elongation in the center of the width direction than both ends, and the negative electrode core was heat-treated. High elongation regions are formed to suppress local deformation, while the number of grains is controlled to maintain battery capacity and stability.
It effectively suppresses local plate deformation caused by charging and discharging, avoids capacity reduction and loss of production stability, and improves battery cycle characteristics.
Smart Images

Figure CN114946053B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a secondary battery. Background Art
[0002] Secondary batteries such as lithium-ion batteries have an electrode body formed by stacking a positive electrode and a negative electrode with a separator. Usually, each electrode plate includes a core body composed of a metal foil and an active material layer formed on the surface of the core body. The active material layer expands and contracts during charging and discharging, and the degree of expansion and contraction of batteries with high energy density is particularly large. Therefore, a large load may act on a part of the core body during charging and discharging, causing local deformation of the electrode plate.
[0003] In the past, a technology for alleviating the effects of expansion and contraction of the active material layer associated with charge and discharge has been proposed. For example, Patent Document 1 discloses an electrode for a secondary battery using a core having an elongation of 13% or more. Patent Document 1 describes the effects of suppressing the micronization of active material particles caused by the expansion and contraction of the active material layer and the detachment of the active material layer from the core. In addition, Patent Document 2 discloses a method for manufacturing a negative electrode for a secondary battery, which includes a step of heating a copper foil as a negative electrode core to a temperature above the recrystallization temperature to soften it.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2005-135856
[0007] Patent Document 2: Japanese Patent Application Publication No. 2016-100117 Summary of the invention
[0008] Problem that the invention aims to solve
[0009] However, as a method for suppressing local deformation of the pole plate, increasing the elongation of the core as disclosed in Patent Documents 1 and 2 is an effective method, but if the elongation of the core becomes too high, there is a concern that the pole plate will contact the outer can and the sealing plate when the pole plate expands due to charging and discharging. Therefore, it is necessary to limit the size of the pole plate, which will cause a decrease in capacity. In addition, the tension specified during the manufacture of the pole plate will act on the core, but when the elongation of the core is high, the core will be elongated due to the tension during manufacturing, and production stability will be impaired.
[0010] An object of the present application is to provide a secondary battery that can suppress local deformation of an electrode plate associated with charge and discharge and does not cause disadvantages such as a decrease in capacity and a decrease in production stability.
[0011] Solutions for solving problems
[0012] A secondary battery as one embodiment of the present application is characterized in that it has an electrode body, wherein the electrode body includes a positive electrode, a negative electrode and a separator, and the positive electrode and the negative electrode are stacked with the separator between them. The positive electrode includes: a positive electrode core having a length direction and a width direction, and a positive electrode active material layer formed on the surface of the positive electrode core. The negative electrode includes: a negative electrode core having a length direction and a width direction, and a negative electrode active material layer formed on the surface of the negative electrode core. The tensile elongation of at least one of the positive electrode core and the negative electrode core in the central portion in the width direction is higher than the tensile elongation of the two end portions in the width direction.
[0013] A secondary battery as another embodiment of the present application is characterized in that it has an electrode body, wherein the electrode body includes a positive electrode, a negative electrode and a separator, and the positive electrode and the negative electrode are stacked with the separator between them, the positive electrode includes: a positive electrode core having a length direction and a width direction, and a positive electrode active material layer formed on the surface of the positive electrode core, the negative electrode includes: a negative electrode core having a length direction and a width direction, and a negative electrode active material layer formed on the surface of the negative electrode core, and the number of grains per unit area in the central portion in the width direction of at least one of the positive electrode core and the negative electrode core is less than the number of grains per unit area at both ends in the width direction.
[0014] Effects of the Invention
[0015] According to the secondary battery involved in the present application, it is possible to suppress the local deformation of the electrode plate accompanying charging and discharging without causing adverse conditions such as a decrease in capacity and a decrease in production stability. If the electrode plate is locally deformed, for example, the uniformity of the battery reaction is impaired and the cycle characteristics are reduced, but according to the secondary battery involved in the present application, the reduction in cycle characteristics caused by the local deformation of the electrode plate can be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a cross-sectional view of a cylindrical battery as an example of an embodiment.
[0017] Figure 2 It is a perspective view of a positive electrode and a negative electrode as an example of an embodiment.
[0018] Hereinafter, with reference to the accompanying drawings, an example of an embodiment of the secondary battery involved in the present application is described in detail. It should be noted that it was originally envisioned to selectively combine the multiple embodiments and variations illustrated below. In addition, in this specification, a description such as "value A to value B" means "above value A and below value B" unless otherwise specified.
[0019] Figure 1 1 is a cross-sectional view of a secondary battery 10 as an example of an embodiment. Figure 1The secondary battery 10 shown has a bottomed cylindrical outer can 16 as an outer body, but the outer body is not limited thereto. The secondary battery involved in the present application can be, for example, a square battery having a bottomed square cylindrical outer can, a coin-shaped battery having a coin-shaped outer can, or a laminated battery having an outer body composed of a laminate sheet including a metal layer and a resin layer.
[0020] like Figure 1 As shown in FIG. 1 , the secondary battery 10 includes a wound electrode body 14 in which a positive electrode 11 and a negative electrode 12 are wound in a spiral shape with a separator 13 interposed therebetween, and a cylindrical outer can 16 that accommodates the electrode body 14. In addition, the secondary battery 10 includes an electrolyte that is accommodated in the outer can 16 together with the electrode body 14. The outer can 16 is a metal container in a bottomed cylindrical shape with one side open in the axial direction, and the opening of the outer can 16 is blocked by a sealing body 17. In the following, for convenience of description, the sealing body 17 side of the battery is set as the upper side, and the bottom side of the outer can 16 is set as the lower side.
[0021] The electrolyte may be an aqueous electrolyte, but is preferably a non-aqueous electrolyte. The non-aqueous electrolyte comprises a non-aqueous solvent and an electrolyte salt that is a solvent in the non-aqueous solvent. Examples of non-aqueous solvents include esters, ethers, nitriles, amides, and mixed solvents of two or more thereof. The non-aqueous solvent may contain a halogen-substituted body formed by replacing at least a portion of the hydrogen of these solvents with a halogen atom such as fluorine. Examples of electrolyte salts include lithium salts such as LiPF6. It should be noted that the electrolyte is not limited to a liquid electrolyte, but may also be a solid electrolyte.
[0022] The positive electrode 11, the negative electrode 12 and the separator 13 constituting the electrode body 14 are all strip-shaped long bodies, which are wound into a spiral shape and alternately stacked in the radial direction of the electrode body 14. In order to prevent the precipitation of lithium, the negative electrode 12 is formed to be one circle larger than the positive electrode 11. In other words, the negative electrode 12 is formed to be longer than the positive electrode 11 in the length direction and the width direction. The two separators 13 are formed to be at least one circle larger than the positive electrode 11, for example, and are arranged in a manner of clamping the positive electrode 11. The electrode body 14 has: a positive electrode lead 20 connected to the positive electrode 11 by welding or the like, and a negative electrode lead 21 connected to the negative electrode 12 by welding or the like.
[0023] Insulating plates 18 and 19 are disposed above and below the electrode body 14 , respectively. Figure 1 In the example shown, the positive electrode lead 20 passes through the through hole of the insulating plate 18 and extends to the sealing body 17 side, and the negative electrode lead 21 passes through the through hole of the insulating plate 19 and extends to the bottom side of the outer can 16. The positive electrode lead 20 is connected to the lower surface of the internal terminal plate 23 of the sealing body 17 by welding or the like, and the cover 27, which is the top plate of the sealing body 17 electrically connected to the internal terminal plate 23, serves as a positive terminal. The negative electrode lead 21 is connected to the bottom inner surface of the outer can 16 by welding or the like, and the outer can 16 serves as a negative terminal.
[0024] A gasket 28 is provided between the outer can 16 and the sealing body 17 to ensure the airtightness inside the battery. A groove portion 22 is formed in the outer can 16, with a part of the side portion extending inward to support the sealing body 17. The groove portion 22 is preferably formed in an annular shape along the circumferential direction of the outer can 16, and the sealing body 17 is supported on its upper surface. The sealing body 17 is fixed to the upper part of the outer can 16 by using the groove portion 22 and the open end of the outer can 16 riveted to the sealing body 17.
[0025] The sealing body 17 has a structure in which an internal terminal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cover 27 are stacked in order from the electrode body 14 side. The components constituting the sealing body 17 have, for example, a disc shape or a ring shape, and the components except the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected at their respective central portions, and an insulating member 25 is sandwiched between their respective peripheral portions. If the internal pressure of the battery rises due to abnormal heat, the lower valve body 24 is deformed and broken in a manner that pushes the upper valve body 26 toward the cover 27 side, thereby cutting off the current path between the lower valve body 24 and the upper valve body 26. If the internal pressure rises further, the upper valve body 26 breaks, and the gas is discharged from the opening of the cover 27.
[0026] Below, refer to Figure 2 , the positive electrode 11 , the negative electrode 12 , and the separator 13 constituting the electrode body 14 , especially the negative electrode 12 , will be described in detail. Figure 2 It is a perspective view of the positive electrode 11 and the negative electrode 12 , and shows the relative arrangement of each other.
[0027] As described in detail later, in this embodiment, the tensile elongation of the central portion of the width direction of the negative electrode core 40 is higher than the tensile elongation of the two end portions in the width direction. In addition, the number of grains per unit area in the central portion of the width direction of the negative electrode core 40 is less than the number of grains per unit area at the two end portions in the width direction. Regarding the tensile elongation of the positive electrode core 30, it is substantially the same in all regions, and the number of grains per unit area is also substantially the same in all regions, but the same structure as the negative electrode core 40 can be applied to the positive electrode core 30, so that the tensile elongation of the central portion in the width direction is higher than the tensile elongation of the two end portions in the width direction. In addition, the number of grains per unit area in the central portion in the width direction of the positive electrode core 30 can be less than the number of grains per unit area at the two end portions in the width direction. Alternatively, this structure can be applied only to the positive electrode core 30.
[0028] [positive electrode]
[0029] like Figure 2As shown, the positive electrode 11 has a positive electrode core 30 and a positive electrode active material layer 31 formed on the surface of the positive electrode core 30. The positive electrode core 30 can be made of a foil of a metal such as aluminum or an aluminum alloy that is stable within the potential range of the positive electrode 11, or a film having the metal disposed on the surface. A suitable example of the positive electrode core 30 is a metal foil composed of an aluminum alloy containing iron. The thickness of the positive electrode core 30 is, for example, 5 μm to 20 μm. In the positive electrode 11, for example, an exposed portion (not shown) is formed in the central portion in the longitudinal direction where the positive electrode active material layer 31 is not formed and the surface of the positive electrode core 30 is exposed, and the positive electrode lead 20 is connected to the exposed portion.
[0030] The positive electrode active material layer 31 includes a positive electrode active material, a conductive agent, and a binder, and is preferably formed on both sides of the positive electrode core 30. The positive electrode active material layer 31 has a thickness of 60 μm to 100 μm on one side of the positive electrode core 30, for example, and is formed with the same thickness on both sides of the positive electrode core 30. The positive electrode 11 can be manufactured as follows: a positive electrode mixture slurry including a positive electrode active material, a conductive agent, and a binder is applied to the positive electrode core 30, and after the coating is dried, it is compressed to form the positive electrode active material layer 31 on both sides of the positive electrode core 30.
[0031] The positive electrode active material uses, for example, a lithium transition metal composite oxide. As metal elements contained in the lithium transition metal composite oxide, Ni, Co, Mn, Al, B, Mg, Ti, V, Cr, Fe, Cu, Zn, Ga, Sr, Zr, Nb, In, Sn, Ta, W, etc. can be cited. Among them, it is preferred to contain at least one of Ni, Co, and Mn. As an example of a suitable composite oxide, a lithium transition metal composite oxide containing Ni, Co, and Mn and a lithium transition metal composite oxide containing Ni, Co, and Al can be cited.
[0032] As the conductive agent included in the positive electrode active material layer 31, carbon materials such as carbon black, acetylene black, Ketjen black, and graphite can be exemplified. As the binder included in the positive electrode active material layer 31, fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide resins, acrylic resins, polyolefin resins, etc. can be exemplified. In addition, these resins can be used in combination with cellulose derivatives such as carboxymethyl cellulose (CMC) or its salts, polyethylene oxide (PEO), etc.
[0033] [negative electrode]
[0034] The negative electrode 12 has a negative electrode core 40 and a negative electrode active material layer 41 formed on the surface of the negative electrode core 40. The negative electrode core 40 can be made of a foil of a metal such as copper that is stable within the potential range of the negative electrode 12, or a film having the metal disposed on the surface. A suitable example of the negative electrode core 40 is a metal foil having copper as a main component, which may be a copper foil consisting essentially of only copper. The thickness of the negative electrode core 40 is, for example, thinner than that of the positive electrode core 30, and is 4 μm to 15 μm. In the negative electrode 12, for example, an exposed portion 43 is formed at both ends in the longitudinal direction where the negative electrode active material layer 41 is not formed and the surface of the negative electrode core 40 is exposed. The negative electrode lead 21 ( Figure 2 The exposed portion 43 is connected to the exposed portion 43.
[0035] The negative electrode core 40 may be any of a rolled copper foil produced by hot rolling a high-purity ingot or an electrolytic copper foil produced by electroplating. The electrolytic copper foil is produced by adjusting the type, concentration, precipitation rate, etc. of additives to control the grain diameter. Generally, when the grain diameter of the copper foil is large, the copper foil is easy to stretch, and when the grain diameter is small, the copper foil is difficult to stretch. The grains of the copper foil can be confirmed by a scanning electron microscope (SEM).
[0036] As described above, the negative electrode core 40 is a strip-shaped elongated body, and the tensile elongation of the central portion in the width direction is higher than that of the two end portions in the width direction. The tensile elongation of the central portion in the width direction of the negative electrode core 40 is preferably 1.2 times or more of the tensile elongation of the two end portions in the width direction, more preferably 2 times or more, and particularly preferably 3 times or more. In the present embodiment, the first region 44 is formed in such a manner that the tensile elongation of the central portion in the width direction of the negative electrode core 40 becomes higher. In the negative electrode core 40, there is a first region 44 as a high elongation region, and a second region 45 having a lower tensile elongation than the first region 44. The second region 45 is arranged in a range including the two end portions in the width direction of the negative electrode core 40 in such a manner that the tensile elongation of the central portion in the width direction of the negative electrode core 40 is higher than that of the two end portions in the width direction.
[0037] The first region 44 is preferably formed along the longitudinal direction of the negative electrode core 40 . Figure 2 In the example shown, the first region 44 is formed with a certain width over the entire length of the negative electrode core 40. The first region 44 is formed, for example, in a band shape centered at the center in the width direction of the negative electrode core 40. The width of the first region 44 is preferably 25% or less, more preferably 20% or less, and particularly preferably 15% or less of the entire width of the negative electrode core 40. The lower limit of the width of the first region 44 is preferably 5%, more preferably 8%, and particularly preferably 10%.
[0038] For the central portion in the width direction of the negative electrode core 40, for example, the negative electrode active material layer 41 expands during charging and is pulled to both sides in the width direction. In particular, for the region Z opposite to the edge of the positive electrode active material layer 31, the volume of the portion of the negative electrode active material layer 41 opposite to the positive electrode active material layer 31 changes due to charging and discharging, but the volume of the portion not opposite to the positive electrode active material layer 31 does not change, so a large stress is likely to act on the region Z compared to other regions. By forming the first region 44 as a high elongation region in the central portion in the width direction of the negative electrode core 40, the local deformation of the negative electrode 12 can be efficiently suppressed. It should be noted that if the overall tensile elongation of the negative electrode core 40 is increased, as described above, there is a concern of undesirable conditions such as a decrease in capacity and a decrease in production stability.
[0039] The tensile elongation of the negative electrode core 40 is measured in accordance with IPC-TM-650 by the following method.
[0040] (1) The portion of the negative electrode core 40 to be measured is cut into a size of 100 mm×12.7 mm using a sharp cutter to prepare a sample piece.
[0041] (2) One end of the sample piece was attached to the lower chuck of a universal testing machine (Autograph AG-IS10KN manufactured by Shimadzu Corporation), and the other end of the sample piece was attached to the upper chuck (distance between chucks: 50 mm).
[0042] (3) At room temperature (about 25°C), the crosshead with the upper chuck fixed thereto is moved at a constant speed to stretch the sample and measure the length of the sample after it is broken. The elongation is calculated from the change in the length of the sample between the chucks before and after the tensile test.
[0043] The tensile elongation of the first region 44 measured by the above method is preferably 9% or more, more preferably 13% or more. The upper limit of the tensile elongation of the first region 44 is preferably 30%, more preferably 20%. The tensile elongation of the second region 45 measured by the above method is, for example, less than 9%, preferably 5% or less. The lower limit of the tensile elongation of the second region 45 is, for example, 1%. When the tensile elongation of the first region 44 and the second region 45 is within this range, local deformation of the negative electrode 12 can be suppressed without causing disadvantages such as reduced capacity.
[0044] The number of grains per unit area in the widthwise central portion of the negative electrode core 40 is smaller than the number of grains per unit area in the widthwise end portions. The number of grains per unit area in the widthwise central portion of the negative electrode core 40 is preferably 1 / 2 or less, more preferably 1 / 5 or less, and particularly preferably 1 / 10 or less of the number of grains per unit area in the widthwise end portions.
[0045] The grains of the negative electrode core 40 can be confirmed by SEM as described above. The number of grains per unit area is obtained by measuring the grains present within the range of a specified square in the cross-sectional SEM image of the negative electrode core 40. The number of grains in the central portion of the width direction of the negative electrode core 40 can be measured, for example, by aligning the center of the specified square with the center of the width direction of the negative electrode core 40. The number of grains at both ends of the width direction of the negative electrode core 40 can be measured, for example, by aligning one side of the specified positive direction with one end or the other end of the width direction of the negative electrode core 40. At this time, the size of the square is preferably determined in such a way that at least one grain is contained in the central portion of the width direction of the negative electrode core 40.
[0046] In this embodiment, the number of crystal grains per unit area of the first region 44, which is a high elongation region, is smaller than the number of crystal grains per unit area of the second region 45, which is a low elongation region. The first region 44 exists in a range including the central portion in the width direction of the negative electrode core 40, and the second region 45 exists in a range including both ends in the width direction of the negative electrode core 40. Therefore, the tensile elongation of the central portion in the width direction of the negative electrode core 40 is higher than that of the both ends in the width direction.
[0047] The first region 44 is formed by locally heat treating a portion including the central portion in the width direction of the negative electrode core 40. The heat treatment method of the negative electrode core 40 is not particularly limited, and preferably a contact heating means is applied. For example, a hot roller, a hot plate, etc. that clamps the negative electrode core 40 from both sides in the thickness direction can be used to locally heat treat a portion of the negative electrode core 40. The heat treatment temperature also varies depending on the metal constituting the negative electrode core 40. In the case of copper foil, it is preferably 160°C to 250°C, and more preferably 180°C to 220°C. It should be noted that the heat treatment of the negative electrode core 40 can also be performed by heating the negative electrode core 40 together with the negative electrode active material layer 41 after the negative electrode active material layer 41 is formed.
[0048] The negative electrode active material layer 41 contains a negative electrode active material and a binder, and is preferably formed on both sides of the negative electrode core 40. The negative electrode active material layer 41 has a thickness of 60 μm to 100 μm on one side of the negative electrode core 40, for example, and is formed with the same thickness on both sides of the negative electrode core 40. The negative electrode 12 can be manufactured as follows: a negative electrode mixture slurry containing a negative electrode active material and a binder is applied to the negative electrode core 40 that has been locally heat-treated in the central portion in the width direction, and after the coating is dried, it is compressed to form the negative electrode active material layer 41 on both sides of the negative electrode core 40.
[0049] The negative electrode active material includes, for example, a carbon-based active material that reversibly absorbs and releases lithium ions. Suitable carbon-based active materials are natural graphites such as flaky graphite, blocky graphite, and earthy graphite, blocky artificial graphite (MAG), and artificial graphites such as graphitized mesophase carbon microbeads (MCMB). In addition, the negative electrode active material can use a Si-based active material composed of at least one of Si and a Si-containing compound, or a carbon-based active material and a Si-based active material can be used in combination. Lithium metal can also be used as the negative electrode active material, in which case the negative electrode active material layer 41 can be formed without using a binder.
[0050] As in the case of the positive electrode 11, the binder contained in the negative electrode active material layer 41 can also use fluororesin, PAN, polyimide resin, acrylic resin, polyolefin resin, etc., but preferably styrene-butadiene rubber (SBR) is used. In addition, the negative electrode active material layer 41 preferably further contains CMC or its salt, polyacrylic acid (PAA) or its salt, polyvinyl alcohol (PVA), etc. Among them, it is suitable to use SBR in combination with CMC or its salt, PAA or its salt.
[0051] [Spacer]
[0052] The spacer 13 uses a porous sheet with ion permeability and insulation. Specific examples of porous sheets include microporous films, woven fabrics, non-woven fabrics, etc. As the material of the spacer 13, polyolefins such as polyethylene, polypropylene, copolymers of ethylene and α-olefins, cellulose, etc. are suitable. The spacer 13 can be any of a single-layer structure and a laminated structure. A heat-resistant layer containing inorganic particles, a heat-resistant layer composed of a resin with high heat resistance such as aramid resin, polyimide, polyamide-imide, etc. can be formed on the surface of the spacer 13. Example
[0053] Hereinafter, the present application will be further described by way of examples, but the present application is not limited to these examples.
[0054] <Example 1>
[0055] [Heat treatment of copper foil]
[0056] Lift both ends of the copper foil in the width direction, which is cut into a thickness of 8μm and a width of 40mm×100mm, to relax the copper foil. Use a heat-resistant clamp with a width of 5mm to press the central part of the relaxed copper foil in the width direction against a hot plate heated to 190°C from above. At this time, adjust the force used to lift the copper foil so that the portion of the copper foil in contact with the hot plate is only the portion pressed by the heat-resistant clamp, and so that no crease is generated in the portion that touches the edge of the heat-resistant clamp. This state is maintained for 5 minutes to complete the heat treatment of the copper foil. Thus, the copper foil of Example 1 is obtained, in which a high elongation region with a high elongation is formed in the central part of the width direction over the entire length in the longitudinal direction. It should be noted that the heat treatment is carried out in a drying oven with a dew point below -30°C.
[0057] <Comparative Example 1>
[0058] The copper foil of Example 1 before the heat treatment was used as the copper foil of Comparative Example 1.
[0059] <Comparative Example 2>
[0060] A copper foil of Comparative Example 2 was obtained in the same manner as in Example 1, except that the entire copper foil was pressed on a hot plate heated to 190° C. for heat treatment.
[0061] [Pressure test of copper foil]
[0062] In order to simulate the expansion and contraction of the negative electrode active material layer accompanying the charge and discharge of the battery, a pressure test was performed using a universal testing machine (the above-mentioned Autograph) by the following method. The pressure test was performed on each copper foil of Example 1, Comparative Example 1 and Comparative Example 2.
[0063] A 20 mm square SUS clamp is fixed to the upper part, and a SUS table is fixed to the lower part so as to be horizontal to the ground. The heat-treated copper foil is placed on the table, and a 1 mm thick fluororubber sheet cut into 25 mm square is placed on the copper foil. At this time, the copper foil and the rubber sheet are arranged in such a way that the centers of the clamp, the rubber sheet, and the copper foil are aligned. In this state, a universal testing machine is used to lower the upper clamp at a speed of 0.5 mm / sec until a load of 8 kN is applied to the clamp. Thereafter, the clamp is raised at the same speed until the load on the clamp disappears, and the presence or absence of copper foil breakage is confirmed. In this test, a polypropylene tape (9 mm in width and 30 μm in thickness) is attached to one side of the copper foil, and the test is carried out with the tape facing the table side. The height difference of the tape is to simulate the application of a local load to the electrode body. Figure 2 The tape was attached so that one end in the width direction was located at the center in the width direction of the copper foil.
[0064] [Measurement of tensile elongation of copper foil]
[0065] By the above method, the tensile elongation of each copper foil of Comparative Example 1 and Comparative Example 2 was measured. It should be noted that the central portion in the width direction of the copper foil of Example 1 and the copper foil of Comparative Example 2 were heat treated under the same conditions. In addition, the two end portions in the width direction of the copper foil of Example 1 were not heat treated like the copper foil of Comparative Example 1. Therefore, the tensile elongation of the central portion in the width direction and the two end portions in the width direction in Table 1 respectively uses the measurement results of Comparative Example 2 and Comparative Example 1.
[0066] [Observation of crystal grains of copper foil]
[0067] The number of crystal grains existing in a predetermined square range of each of the copper foils of Example 1, Comparative Example 1, and Comparative Example 2 was measured from a cross-sectional SEM image of the copper foil.
[0068] [Table 1]
[0069]
[0070] As shown in Table 1, the copper foil of Example 1 having a high elongation region formed in the central part in the width direction has the same fracture resistance as the case where the entire copper foil is heat treated (Comparative Example 2). That is, the high elongation region absorbs the local load, so the local deformation of the negative electrode of the copper foil of Example 1 associated with charging and discharging is suppressed. The copper foil of Comparative Example 1, which does not have a high elongation region, broke in the above-mentioned pressure test. Furthermore, since the copper foil of Example 1 has a low tensile elongation at both ends in the width direction, the stretching of the copper foil caused by the tension during manufacturing and charging and discharging is suppressed compared to Comparative Example 2 in which the tensile elongation of the entire copper foil is high. Therefore, it is possible to avoid undesirable situations such as a reduction in production stability and a reduction in battery capacity caused by limitations on the size of the electrode plate.
[0071] Description of Reference Numerals
[0072] 10 secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 16 outer can, 17 sealing body, 18, 19 insulating plate, 20 positive electrode lead, 21 negative electrode lead, 22 groove portion, 23 internal terminal plate, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cover, 28 gasket, 30 positive electrode core, 31 positive electrode active material layer, 40 negative electrode core, 41 negative electrode active material layer, 43 exposed portion, 44 first region, 45 second region
Claims
1. A secondary battery comprising an electrode body, wherein the electrode body comprises a positive electrode, a negative electrode and a separator, and the positive electrode and the negative electrode are stacked with the separator interposed therebetween. The positive electrode comprises: a positive electrode core having a length direction and a width direction, and a positive electrode active material layer formed on a surface of the positive electrode core. The negative electrode includes: a negative electrode core having a length direction and a width direction, and a negative electrode active material layer formed on a surface of the negative electrode core. At least one of the positive electrode core body and the negative electrode core body has a higher tensile elongation at the center portion in the width direction than at both ends in the width direction. The tensile elongation of at least one of the positive electrode core body and the negative electrode core body in the central portion in the width direction is 1.2 times or more the tensile elongation of both end portions in the width direction.
2. The secondary battery according to claim 1, wherein The electrode body has a winding structure in which the positive electrode and the negative electrode are spirally wound with the separator interposed therebetween. The negative electrode active material layer is formed in a larger area than the positive electrode active material layer and is arranged to face the entire area of the positive electrode active material layer. The tensile elongation of the negative electrode core body at a center portion in a width direction is higher than that of both end portions in the width direction.
3. A secondary battery comprising an electrode body, wherein the electrode body comprises a positive electrode, a negative electrode and a separator, and the positive electrode and the negative electrode are stacked with the separator interposed therebetween. The positive electrode comprises: a positive electrode core having a length direction and a width direction, and a positive electrode active material layer formed on a surface of the positive electrode core. The negative electrode includes: a negative electrode core having a length direction and a width direction, and a negative electrode active material layer formed on a surface of the negative electrode core. The number of crystal grains per unit area in the central portion in the width direction of at least one of the positive electrode core and the negative electrode core is smaller than the number of crystal grains per unit area in both ends in the width direction. The number of crystal grains per unit area in the center portion in the width direction of at least one of the positive electrode substrate and the negative electrode substrate is less than or equal to 1 / 2 of the number of crystal grains per unit area in both end portions in the width direction.
4. The secondary battery according to claim 3, wherein The electrode body has a winding structure in which the positive electrode and the negative electrode are spirally wound with the separator interposed therebetween. The negative electrode active material layer is formed in a larger area than the positive electrode active material layer and is arranged to face the entire area of the positive electrode active material layer. The number of crystal grains per unit area in the center portion in the width direction of the negative electrode core is smaller than the number of crystal grains per unit area in both end portions in the width direction.