Resin composition
By adjusting the proportions of polyamide, polypropylene, maleic acid-modified styrene-butadiene elastomer and hollow ball filler in the resin composition, and combining plasticizers and flame retardants, the problems in the existing technology are solved. It achieves an efficient performance balance that is difficult to balance between flame retardancy, flexural modulus and lightweight, and is suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202080093454.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-01-27
- Filing Date
- 2020-11-19
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-11-19
AI Technical Summary
It is difficult to balance flame retardancy, flexural modulus and light weight with the existing technology, and cannot effectively achieve the balance of these three properties in the resin composition.
Use 27 to 38 mass% of polyamide, 6 to 20 mass% of polypropylene, 7 to 17 mass% of maleic acid-modified styrene-butadiene elastomer, and 20 to 29 mass of hollow sphere fillers with a specific gravity of 0.2 to 0.7. %, and a combination of plasticizers and flame retardants, through specific mass ratios and manufacturing methods, to form a resin composition that combines flame retardancy, flexural modulus and lightweight.
It achieves a balance between the flame retardancy, flexural modulus and lightweight of the resin composition, improves the impact strength and surface appearance of the molded product, ensures fluidity and pressure control during molding, and is suitable for components of various complex shapes. .
Smart Images

Figure BDA0003748724660000131
Abstract
Description
Technical Field
[0001] The present disclosure relates to resin compositions. Background Art
[0002] Patent Document 1 discloses a resin composition containing 30-80% by mass of polyamide, 5-60% by mass of modified polyolefin, unmodified polyolefin, fillers such as glass beads, and additives such as flame retardants. The composition forms a core-shell particle structure with polyamide as a matrix, modified polyolefin as a shell, and unmodified polyolefin as a core. The composition also improves dimensional stability, impact resistance, etc.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 9-157519 Summary of the invention
[0006] Patent Document 1 cannot achieve desired balance among flame retardancy, flexural modulus, and lightness.
[0007] An object of the present disclosure is to provide a resin composition that achieves a balance between flame retardancy, flexural modulus, and lightness.
[0008] The resin composition disclosed herein contains 27 to 38% by mass of polyamide, 6 to 20% by mass of polypropylene, 7 to 17% by mass of maleic acid-modified styrene-butadiene elastomer, 20 to 29% by mass of a hollow sphere filler having a specific gravity of 0.2 to 0.7, and the remainder being at least one selected from a plasticizer and a flame retardant.
[0009] According to the resin composition in the present disclosure, flame retardancy, flexural modulus, and lightness can be achieved at the same time. DETAILED DESCRIPTION
[0010] The following is a detailed description of the implementation method. However, sometimes more detailed descriptions than necessary are omitted. For example, sometimes detailed descriptions of well-known matters or repeated descriptions of substantially the same technical features are omitted.
[0011] It should be noted that the following description is provided for those skilled in the art to fully understand the present disclosure, and is not intended to limit the subject matter described in the claims.
[0012] (Implementation Method 1)
[0013] Implementation 1 is described below.
[0014] [1-1. Structure]
[0015] The resin composition of the present embodiment contains 27-38 mass % of polyamide, 6-20 mass % of polypropylene, 7-17 mass % of maleic acid-modified styrene-butadiene elastomer, 20-29 mass % of hollow sphere filler having a specific gravity of 0.2-0.7, and at least one selected from a plasticizer and a flame retardant as the remainder. The polyamide, polypropylene, maleic acid-modified styrene-butadiene elastomer, hollow sphere filler, plasticizer, and flame retardant are described in order below.
[0016] [1-2. Polyamide]
[0017] The type of polyamide is not particularly limited. As specific examples of polyamide, aliphatic polyamides such as nylon 6, nylon 66, nylon 11, nylon 12, nylon 46, nylon 6T (T: terephthalic acid component), nylon 9T, nylon MXD6 (MXD: meta-xylylenediamine component) can be listed. Among them, nylon 6, nylon 66, nylon 11, and nylon 12 are preferably used from the viewpoints of excellent formability, mechanical properties, etc.
[0018] These polyamides may be used alone or in combination of two or more thereof.
[0019] The mass average molecular weight (Mw) of the polyamide is not particularly limited, but is preferably 10,000 to 500,000 from the viewpoint of improving plasticity, particularly improving plasticity when a plasticizer is added. The mass average molecular weight (Mw) can be determined by a GPC method.
[0020] The mass ratio of the polyamide in the resin composition is 27 to 38 mass %, preferably 30 to 34 mass %, more preferably 31 to 33 mass %. By setting the mass ratio within the above range, flame retardancy, flexural modulus, and lightness can be achieved at the same time.
[0021] [1-3. Polypropylene (PP)]
[0022] Unmodified polypropylene is used as polypropylene. The concept of polypropylene includes homopolymers, random copolymers and block copolymers. Homopolymers are homopolymers of propylene. Random copolymers and block copolymers are copolymers of propylene and α-polyolefins other than polypropylene. Specific examples of α-polyolefins include ethylene, 1-butene, etc. From the viewpoint of effectively showing the characteristics of polypropylene, the molar ratio of α-polyolefins other than polypropylene in the random copolymer and the block copolymer is preferably 20 mol% or less.
[0023] The mass average molecular weight (Mw) of polypropylene is not particularly limited, but is preferably in the range of 10,000 to 500,000, and more preferably in the range of 45,000 to 300,000. When the mass average molecular weight (Mw) of polypropylene is 10,000 or more, the rigidity reduction of the molded product can be suppressed. When the mass average molecular weight (Mw) of polypropylene is 500,000 or less, the fluidity of the resin composition during molding can be prevented from being reduced. If the fluidity can be prevented from being reduced, the resin can be easily distributed throughout the mold during molding, and even thin or complex-shaped components can be well molded. In addition, since the pressure increase during melt kneading of the resin or injection molding can be suppressed, the destruction of the hollow sphere filler caused by the pressure increase can be suppressed. The mass average molecular weight (Mw) can be obtained by the GPC method.
[0024] The mass ratio of polypropylene in the resin composition is 6 to 20 mass %, preferably 13 to 17 mass %, and more preferably 14 to 16 mass %. By defining the mass ratio within the above range, flame retardancy, flexural modulus, and lightness can be taken into account. In addition, in order to further improve the impact strength, it is preferably mixed with 6 to 8 mass %. By defining the mass ratio within the above range, a balance is achieved with the mixing amount of the maleic acid-modified styrene-butadiene elastomer, and the impact strength can be improved.
[0025] [1-4. Maleic acid-modified styrene-butadiene elastomer]
[0026] As styrene constituting the maleic acid-modified styrene-butadiene elastomer, halogenated styrene can be used, and as butadiene, isoprene (2-methyl-1,3-butadiene) can be used. In addition, the butadiene skeleton can be hydrogenated to form an olefin. The styrene-butadiene elastomer is modified with maleic acid. Thus, the compatibility of polyamide, polypropylene, and hollow sphere fillers is improved.
[0027] Specific examples of styrene-butadiene elastomers constituting maleic acid-modified styrene-butadiene elastomers include, for example, styrene-butadiene copolymers, styrene-isoprene copolymers, styrene-butadiene-styrene copolymers, acrylonitrile-butadiene-styrene copolymers, styrene-isoprene-butadiene copolymers, styrene-butadiene-butylene-styrene copolymers, styrene-ethylene-propylene-styrene copolymers, styrene-ethylene-butylene-styrene copolymers (SEBS), styrene-ethylene-butadiene-styrene copolymers, styrene-ethylene-ethylene-propylene-styrene copolymers, styrene-isoprene-styrene copolymers, and styrene (butadiene / isoprene) styrene copolymers. Among them, maleic acid-modified styrene-ethylene-butylene-styrene copolymers (SEBS) are preferred from the viewpoint of excellent effects of the resin composition disclosed herein.
[0028] These maleic acid-modified styrene-butadiene elastomers may be used alone or in combination of two or more thereof.
[0029] Examples of commercially available products of maleic acid-modified styrene-butadiene elastomers include Tuftec M series (manufactured by Asahi Kasei Corporation).
[0030] The mass ratio of the maleic acid-modified styrene-butadiene elastomer in the resin composition is 7 to 17 mass %, preferably 7 to 9 mass %. By setting the mass ratio within the above range, flame retardancy, flexural modulus and lightness can be taken into account. In addition, in the case of further improving impact strength, it is preferably mixed with 15 to 17 mass %. By setting the mass ratio within the above range, a balance is achieved with the mixing amount of polypropylene, and the impact strength can be improved.
[0031] [1-5. Hollow sphere filler]
[0032] Hollow spherical fillers can make the resin composition light in specific gravity. Generally, polyamide resins, polypropylene resins, etc., which are thermoplastic resins, have a specific gravity of 0.90 or more. If a considerable amount of flame retardant is added to improve flame retardancy, the specific gravity of the resin composition increases by about 0.1. In order to reduce the apparent specific gravity of the resin composition, in the present disclosure, hollow spherical fillers as light specific gravity structural members are melt-kneaded into the resin composition.
[0033] As the hollow ball filler, any of inorganic hollow ball fillers and organic hollow ball fillers can be used. As the specific example of the inorganic hollow ball filler, glass hollow balls such as hollow glass beads, white sand hollow balls, alumina hollow balls (pearlite hollow balls), silica-alumina hollow balls (fly ash hollow balls), carbon hollow balls, zirconium oxide hollow balls, etc. can be listed. As the specific example of the organic hollow ball filler, thermoplastic organic hollow balls such as thermosetting organic hollow balls such as phenolic resin hollow balls, acrylonitrile hollow balls, etc. can be listed. Among them, from the viewpoint of the ease of forming during manufacture, hollow glass beads are preferably used.
[0034] These hollow sphere fillers may be used alone or in combination of two or more thereof.
[0035] The specific gravity of the hollow sphere filler is 0.2 to 0.7, preferably 0.3 to 0.6, and more preferably 0.4 to 0.5. When the specific gravity of the hollow sphere filler is 0.2 or more, the compressive strength of the hollow sphere filler can be improved. In addition, when the specific gravity of the hollow sphere filler is 0.7 or less, the resin composition can be made lighter.
[0036] The compressive strength of the hollow sphere filler is not particularly limited, but is preferably 40 to 190 MPa, more preferably 110 to 190 MPa. By setting it within the above range, the hollow sphere filler can be prevented from being broken, and the weight of the resin composition can be reduced.
[0037] The mass ratio of the hollow sphere filler in the resin composition is 20 to 29 mass %, preferably 26 to 29 mass %, more preferably 27 to 28 mass %. By setting the mass ratio within the above range, flame retardancy, flexural modulus, and lightness can be achieved at the same time.
[0038] [1-6. Plasticizer]
[0039] The plasticizer is not particularly limited as long as it is applicable to polyamide. Examples of the plasticizer include sulfonamides such as aromatic or aliphatic sulfonamides, hydroxybenzoates, polycyclic aromatic compounds, N-alkyl aliphatic sulfonamides, orthophosphates, esters of aliphatic carboxylic acids, lactams, lactones, cyclic ketones, adducts of hydroxycarboxylic acids and alkylene oxides, pentyl cyclohexanol carbonate and tetrahydrofurfuryl carbonate, chlorinated aromatic hydrocarbons and their ethers, adducts of polyamide and ethylene oxide, condensates of carbamate and formaldehyde, condensates of isocyanates and polyoxy compounds, amorphous polyamides, and the like.
[0040] Specific examples of sulfonamides include N-butylbenzenesulfonamide, N-hexylbenzenesulfonamide, N-decylbenzenesulfonamide, and N-cyclohexylbenzylsulfonamide. Further examples of toluene derivatives thereof include p-toluenesulfonamide, N-ethyl-p-toluenesulfonamide, N-ethyl-o,p-toluenesulfonamide (o,p mixture), N-butyl-p-toluenesulfonamide, N-hexyl-p-toluenesulfonamide, N-decyl-p-toluenesulfonamide, and N-cyclohexyl-p-toluenesulfonamide.
[0041] Specific examples of hydroxybenzoic acid esters include p-hydroxybenzoic acid esters and the like.
[0042] Specific examples of the polycyclic aromatic compound include fluorene derivatives.
[0043] Specific examples of orthophosphates include monooctyldiphenyl phosphate, tolylphenyl phosphate, and xylyldiphenyl phosphate.
[0044] Specific examples of the esters of aliphatic carboxylic acids include dioctyl azelate and dioctyl sebacate.
[0045] Among these plasticizers, sulfonamides, hydroxybenzoic acid esters, and polycyclic aromatic compounds are preferred from the viewpoint of excellent compatibility with polyamide and excellent effect of imparting plasticization to the resin composition.
[0046] These plasticizers may be used alone or in combination of two or more.
[0047] The mass ratio of the plasticizer in the resin composition is preferably 1 to 2.2 mass %, more preferably 1.5 to 2.0 mass %. When the mass ratio of the plasticizer is 1 mass % or more, the plasticizer can be added to the resin composition. In addition, when the mass ratio of the plasticizer is 2.2 mass % or less, the surface appearance can be well maintained.
[0048] [1-7. Flame retardant]
[0049] Examples of the flame retardant include halogen flame retardants, phosphorus flame retardants such as phosphate ester flame retardants and organic phosphorus flame retardants, metal salt flame retardants, siloxane flame retardants, ammonium polyphosphate flame retardants, and triazine flame retardants.
[0050] Specific examples of halogen flame retardants include decabromodiphenyl ether, tetrabromobisphenol A, tetrabromobisphenol S, 1,2-bis(2',3',4',5',6'-pentabromophenyl)ethane, 1,2-bis(2,4,6-tribromophenoxy)ethane, 2,4,6-tris(2,4,6-tribromophenoxy)-1,3,5-triazine, 2,6- or 2,4-dibromophenol, brominated epoxy resins, brominated polycarbonates, brominated polystyrenes, brominated polyacrylates, ethylenebistetrabromophthalimide, Brominated flame retardants containing bromine compounds such as hexabromocyclododecane, hexabromobenzene, pentabromobenzyl acrylate, 2,2-bis[4'(2",3"-dibromopropoxy)-,3',5'-dibromophenyl]-propane, bis(3,5-dibromo-4-dibromopropoxyphenyl)sulfone, tris(2,3-dibromopropyl)isocyanurate, and chlorinated flame retardants containing chlorine compounds such as chlorinated paraffins, chlorinated polyethylene, chlorinated polypropylene, perchloropentacyclodecane, dodecachlorododecahydrodimethyldibenzocyclooctene, dodecachlorooctahydrodimethyldibenzofuran, etc. Here, 1,2-bis(2',3',4',5',6'-pentabromophenyl)ethane (ethylenebis(pentabromophenyl)) is preferred from the viewpoint of exerting a flame retardant effect at a relatively low addition amount.
[0051] Specific examples of phosphorus-based flame retardants include aromatic phosphates such as triphenyl phosphate, tricresyl phosphate, trimethyl phosphate, triethyl phosphate, cresyl diphenyl phosphate, xylyl diphenyl phosphate, and 2-ethylhexyl diphenyl phosphate, phosphate-based compounds such as monophosphate compounds and phosphate oligomer compounds, halogen-containing phosphate compounds such as tris(dichloropropyl)phosphate, trichloroethyl phosphate, and trichloropropyl phosphate, condensed phosphate compounds, polyphosphates, red phosphorus-based compounds, phosphinate compounds, phosphonate compounds, phosphazene oligomer compounds, and phosphonic acid amide compounds.
[0052] Specific examples of metal salt flame retardants include organic metal salt flame retardants such as sodium antimonate, antimony trioxide, antimony pentoxide, etc., which are used in combination with a halogen flame retardant, metal salt flame retardants used as flame retardant aids, organic sulfonic acid alkali (earth) metal salts, boric acid metal salt flame retardants, stannate metal salt flame retardants, etc.
[0053] These flame retardants may be used alone or in combination of two or more.
[0054] Furthermore, an anti-drip agent (polytetrafluoroethylene having fibril-forming ability, etc.) may be blended and used in combination with a flame retardant.
[0055] The mass ratio of the flame retardant in the resin composition is preferably 12.6 to 15.2 mass %, more preferably 13 to 15 mass %. When the mass ratio of the flame retardant is 12.6 mass % or more, flame retardancy can be imparted to the resin composition. In addition, when the mass ratio of the flame retardant is 15.2 mass % or less, lightweighting of the resin composition can be achieved.
[0056] [1-8. Method for producing resin composition]
[0057] The resin composition (pellets) can be manufactured by a dry method as described below. That is, polyamide, polypropylene, maleic acid-modified styrene-butadiene elastomer, hollow sphere filler with a specific gravity of 0.2 to 0.7, and at least one selected from a plasticizer and a flame retardant are put into a mixing extruder such as a twin-screw mixing extruder with a specified blend. In the mixing extruder, polyamide, polypropylene, and maleic acid-modified styrene-butadiene elastomer are melted. The hollow sphere filler and the flame retardant are dispersed in the molten mixed resin under the condition that the fluidity of the polyamide is improved and the shear stress is reduced by the plasticizer. Furthermore, in the mixing extruder, the hollow sphere filler and the flame retardant are subjected to shearing and are evenly dispersed in the molten mixed resin. The molten mixture extruded by the mixing extruder is, for example, water-cooled to form pellets. There is no particular limitation on the size of the pellets.
[0058] [1-9. Method for manufacturing molded product]
[0059] Various molded products can be manufactured by using the resin composition (pellets) as a molding material and using known molding methods such as injection molding, extrusion molding, and casting molding. The resin composition contains polyamide, polypropylene, maleic acid-modified styrene-butadiene elastomer, hollow sphere filler, and at least one selected from a plasticizer and a flame retardant as the remainder, so the obtained molded product has flame retardancy, flexural modulus, and lightness.
[0060] [1-10. Effects, etc.]
[0061] As described above, the resin composition of the present embodiment contains 27 to 38% by mass of polyamide, 6 to 20% by mass of polypropylene, 7 to 17% by mass of maleic acid-modified styrene-butadiene elastomer, 20 to 29% by mass of hollow sphere filler having a specific gravity of 0.2 to 0.7, and at least one selected from a plasticizer and a flame retardant as the remainder. Thus, flame retardancy, flexural modulus, and lightness can be achieved.
[0062] In addition, in this embodiment, 30 to 34% by mass of polyamide, 13 to 17% by mass of polypropylene, 7 to 9% by mass of maleic acid-modified styrene-butadiene elastomer, and 26 to 29% by mass of hollow sphere filler may be used, thereby achieving better flame retardancy, flexural modulus, and weight reduction.
[0063] In addition, in this embodiment, 31-33% by mass of polyamide, 14-16% by mass of polypropylene, 7-9% by mass of maleic acid-modified styrene-butadiene elastomer, and 27-28% by mass of hollow sphere filler may be used, thereby achieving further excellent flame retardancy, flexural modulus, and weight reduction.
[0064] In addition, in the present embodiment, the polyamide may be 31 to 33% by mass, the polypropylene may be 6 to 8% by mass, the maleic acid-modified styrene-butadiene elastomer may be 15 to 17% by mass, and the hollow sphere filler may be 27 to 28% by mass. Thus, the blending amount of the polypropylene and the blending amount of the maleic acid-modified styrene-butadiene elastomer is balanced, thereby improving the impact strength.
[0065] In addition, in this embodiment, the plasticizer may be 1 to 2.2 mass % and the flame retardant may be 12.6 to 15.2 mass %. This can maintain the surface appearance of the resin composition well and improve plasticity. In addition, the resin composition can be lightweight and flame retardant can be improved.
[0066] In addition, in the present embodiment, the mass average molecular weight of the polyamide may be 10,000 to 500,000. This can improve plasticity, and in particular, can improve plasticity when a plasticizer is added.
[0067] In addition, in the present embodiment, the mass average molecular weight of the polypropylene can be 10,000 to 500,000. Thus, the rigidity of the molded product can be suppressed from decreasing. In addition, the fluidity of the resin composition during molding can be prevented from decreasing. If the fluidity can be prevented from decreasing, the resin can be easily spread throughout the mold during molding, so even thin or complex-shaped components can be well molded. In addition, since the pressure increase during melt kneading or injection molding of the resin can be suppressed, the destruction of the hollow sphere filler accompanied by the pressure increase can be suppressed.
[0068] In addition, in the present embodiment, the plasticizer may be at least one selected from sulfonamides, hydroxybenzoates, and polycyclic aromatic compounds. This can achieve an excellent effect of imparting plasticization to the resin composition.
[0069] [2. Other embodiments]
[0070] As described above, as an example of the technology disclosed in this application, embodiment 1 is described. However, the technology in the present disclosure is not limited thereto, and can also be applied to embodiments that have been changed, replaced, added, omitted, etc. In addition, it is also possible to combine the various components described in the above embodiment 1 to form a new embodiment.
[0071] Therefore, other embodiments are exemplified below.
[0072] The above embodiment may contain one or more additives other than the above within the range that does not inhibit the characteristics of the resin composition of the present disclosure. Specific examples of the additives include colorants, fillers, antioxidants, ultraviolet absorbers, antistatic agents, and the like.
[0073] It should be noted that the above-described embodiments are intended to illustrate the technology in the present disclosure, and therefore various changes, substitutions, additions, omissions, etc. may be made within the scope of the claims or their equivalents.
[0074] Example
[0075] The present disclosure will be specifically described below through examples, but the present disclosure is not limited to the following examples.
[0076] (Example 1)
[0077] Polyamide, polypropylene, maleic acid-modified styrene-butadiene elastomer, hollow sphere filler, plasticizer, and flame retardant were weighed and dry-blended in the ratio (mass %) shown in Table 1. Then, the mixture was melt-kneaded and dispersed using a twin-screw kneading extruder (manufactured by TECHNOVEL CORPORATION, model: KZW15TW) at a kneading temperature of 240° C., and then water-cooled to produce pellets.
[0078] Polyamide: Amilan CM1007 (manufactured by Toray Industries, Inc., nylon 6, mass average molecular weight 250,000)
[0079] Polypropylene: NOVATEC PP BC03B (manufactured by Japan Polypropylene Corporation, mass average molecular weight 150,000)
[0080] Maleic acid-modified styrene-butadiene elastomer: Tuftec M1913 (manufactured by Asahi Kasei Corporation, maleic acid-modified SEBS)
[0081] Hollow ball filler: Glass Bubbles iM16K (manufactured by 3M, hollow glass filler, specific gravity 0.46, compressive strength 110 MPa)
[0082] Plasticizer: OGSOL MF-11 (manufactured by Osaka Gas Chemicals Co., Ltd., bis-phenol-ethanol-fluorene (BPEF))
[0083] Flame retardant: Saytex 8010 (manufactured by ALBEMARLE JAPAN CORPORATION, ethylene bis(pentabromophenyl))
[0084] (Examples 2 to 9)
[0085] Pellets made of a resin composition were produced in the same manner as in Example 1 except that the weights were measured so as to be in the ratios shown in Table 1.
[0086] (Comparative Examples 1 to 3)
[0087] Pellets made of a resin composition were produced in the same manner as in Example 1 except that polypropylene, a plasticizer, and a flame retardant were not used and the components were weighed in the ratios shown in Table 1.
[0088] (Comparative Examples 4 and 5)
[0089] Pellets made of a resin composition were produced in the same manner as in Example 1 except that a plasticizer and a flame retardant were not used and the components were weighed in the ratios shown in Table 1.
[0090] (Comparative Examples 6, 7, 9, 10)
[0091] Pellets made of a resin composition were produced in the same manner as in Example 1 except that the weights were measured so as to be in the ratios shown in Table 1.
[0092] (Comparative Example 8)
[0093] Pellets made of a resin composition were produced in the same manner as in Example 1 except that no flame retardant was used and the components were weighed to have the ratios shown in Table 1.
[0094] (Flexural modulus)
[0095] The pellets of each example and comparative example were used to prepare test pieces specified in ISO 178. Each test piece was subjected to a bending test specified in JIS K 7171. Table 1 shows the measurement results of the bending modulus.
[0096] (Charpy impact test)
[0097] The Charpy impact test is an impact test for breaking a prismatic test piece with a notch formed therein by applying an impact at high speed to the test piece, thereby evaluating the energy required for the breakage and the toughness of the test piece. The Charpy impact test is performed in accordance with the provisions of JIS K7111. The results of the impact strength obtained by the Charpy impact test are shown in Table 1.
[0098] (Specific gravity of resin composition)
[0099] The specific gravity of the resin composition was determined by the water displacement method described in JIS K 7112. Table 1 shows the results of the specific gravity measurement.
[0100] (Flame retardancy test)
[0101] The flame retardancy evaluation of the UL-94 standard of Underwriter's Laboratories Inc. was performed. In the Vertical Burning Test, the long strip test piece is first made vertical, held at the upper end, and its lower end is in contact with the flame of the gas burner for 10 seconds. Then, after the flame of the gas burner is separated, if the flame is extinguished, it is immediately further in contact with the flame of the gas burner for 10 seconds and the flame is separated. For the judgment, according to the total flame burning time and the presence or absence of ignition caused by dripping (particles falling from the test piece), it is graded in the order of easy combustion as UL94V-2, UL94V-1, and UL94V-0. In this test, the case of meeting the UL94V-2 benchmark is judged as "qualified", and the case of not meeting the conditions is judged as "unqualified". The flame retardancy measurement results are shown in Table 1.
[0102] The test pieces were set to have a length of 127 mm, a width of 12.7 mm, and five thicknesses ranging from the smallest to the largest 12.7 mm. The thickness increase was no more than 3.18 mm.
[0103] (Injection pressure)
[0104] The maximum pressure during molding at an injection temperature of 240° C. using a dumbbell-shaped mold was measured. Table 1 shows the results of the injection pressure measurement.
[0105] [Table 1]
[0106]
[0107] It was confirmed that the molded products obtained by the resin composition of each embodiment all had the specified flame retardancy, the bending modulus was 1500MPa or more, and the specific gravity was 0.99 or less, so a resin composition that takes into account flame retardancy, bending modulus and lightness can be obtained. In addition, the injection pressure of each embodiment is less than 135MPa, and the fluidity during molding is good. In addition, the impact strength of each embodiment obtained by the Charpy impact test is 3.0kJ / m 2 As described above, the molded product is excellent in impact strength.
[0108] The resin composition of the present disclosure can be used for applications such as parts of household electrical appliances such as dust collectors, electric tools, dryers, hair irons, curling irons, kettles, and portable cookers.
Claims
1. A resin composition comprising 27 to 38% by weight of polyamide, 6 to 20% by weight of polypropylene, 7 to 17% by weight of a maleic acid-modified styrene-butadiene elastomer, 20 to 29% by weight of a hollow sphere filler having a specific gravity of 0.2 to 0.7, and at least one selected from a plasticizer and a flame retardant as the remainder.
2. The resin composition according to claim 1, wherein The polyamide accounts for 30 to 34% by mass, the polypropylene accounts for 13 to 17% by mass, the maleic acid-modified styrene-butadiene elastomer accounts for 7 to 9% by mass, and the hollow sphere filler accounts for 26 to 29% by mass.
3. The resin composition according to claim 2, wherein The polyamide accounts for 31 to 33% by mass, the polypropylene accounts for 14 to 16% by mass, the maleic acid-modified styrene-butadiene elastomer accounts for 7 to 9% by mass, and the hollow sphere filler accounts for 27 to 28% by mass.
4. The resin composition according to claim 1, wherein The polyamide accounts for 31 to 33% by mass, the polypropylene accounts for 6 to 8% by mass, the maleic acid-modified styrene-butadiene elastomer accounts for 15 to 17% by mass, and the hollow sphere filler accounts for 27 to 28% by mass.
5. The resin composition according to any one of claims 1 to 4, wherein The plasticizer is 1 to 2.2% by mass, and the flame retardant is 12.6 to 15.2% by mass.
6. The resin composition according to any one of claims 1 to 4, wherein The mass average molecular weight of the polyamide is 10,000 to 500,000.
7. The resin composition according to any one of claims 1 to 4, wherein The mass average molecular weight of the polypropylene is 10,000 to 500,000.
8. The resin composition according to any one of claims 1 to 4, wherein The plasticizer is at least one selected from sulfonamides, hydroxybenzoates and polycyclic aromatic compounds.