Polyester polycarbonate polyols and synthetic leather

The use of a polyester polycarbonate polyol with a specific structure and catalyst addresses the issues of sweat and hydrolysis resistance in synthetic leather, achieving improved durability and reduced solvent use.

CN115044029BActive Publication Date: 2024-12-03ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202210215569.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-03-08
Filing Date
2022-03-07
Publication Date
2024-12-03
Estimated Expiration
2042-03-07

AI Technical Summary

Technical Problem

Existing synthetic leathers face issues with insufficient sweat resistance and hydrolysis resistance, particularly in applications requiring high durability, and often require large amounts of organic solvents during polyurethane polymerization, leading to environmental concerns.

Method used

A polyester polycarbonate polyol with a specific structure and catalyst, such as a metal alkoxide, is used to produce a polyurethane with improved properties like softness, chemical resistance, hydrolysis resistance, and heat resistance, which is then used to create synthetic leather.

Benefits of technology

The solution provides synthetic leather with enhanced abrasion resistance, adhesion, and reduced solvent use, while maintaining flexibility and low-temperature characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115044029B_ABST
    Figure CN115044029B_ABST
Patent Text Reader

Abstract

A polyester polycarbonate polyol and a synthetic leather. A polyester polycarbonate polyol and a method for producing the same are provided, wherein the polyester polycarbonate polyol is a raw material for a polyurethane having an excellent balance of softness (touch), chemical resistance, low temperature properties, heat resistance, hydrolysis resistance, adhesion, and wear resistance. A polyester polycarbonate polyol having a repeating unit represented by the following formula (1) and a repeating unit represented by the following formula (2), a hydroxyl group at the molecular end, a hydroxyl value of 37 to 86 mgKOH / g, and a carbonate group content of 15 to 40% by mass. (In formula (1), R1 is a divalent straight-chain aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.) (In formula (2), R2 is a divalent hydrocarbon having 2 to 15 carbon atoms, and R3 is a divalent straight-chain aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to novel polyester polycarbonate polyol and synthetic leather using the same. Background Art

[0002] In the past, synthetic leathers with good softness were obtained by applying a polyurethane resin solution obtained by polymerizing a polyether polyol such as polypropylene glycol and polytetramethylene glycol to a fibrous substrate or a film-forming plate and solidifying it in water. Although these synthetic leathers have excellent softness, they are easily decomposed by components such as sweat, and have problems in durability. In addition, there are synthetic leathers obtained by solidifying the following polyurethane resin solution, which is obtained by using a polyester polyol obtained by reacting a hydroxy compound with a dibasic acid and polymerizing it. This synthetic leather has problems in hydrolysis resistance.

[0003] As a synthetic leather for solving these problems, for example, Patent Document 1 discloses a synthetic leather obtained by using a polyurethane resin polymerized by using polycarbonate diol. Patent Document 1 specifically discloses a porous sheet-like article, which is formed by containing or bonding a urethane composition in and / or on a fiber substrate, wherein the urethane composition includes: a polyurethane formed by polycarbonate diol, an organic isocyanate and a low molecular diol; and a polyurethane formed by a polyester diol, an organic diisocyanate and a low molecular diol.

[0004] Patent document 2 discloses a porous sheet material, which is obtained by applying a solution of a polyurethane resin formed by a polymer diol, an organic isocyanate and an optional chain extender to a substrate and using a wet film-forming method. The porous sheet material is characterized in that the polymer diol is a mixed diol of polycarbonate diol and polyester diol, and the polycarbonate diol is formed by 1,4-butanediol and one or more other alkane diols having 4 to 6 carbon atoms, and the diol contains 50 to 90 mol% of 1,4-butanediol based on the total molar number of the diol, and the number average molecular weight is 500 to 5000, and the coagulation value of the polyurethane resin is 7 to 14.

[0005] Patent document 3 discloses a synthetic leather surface coating layer formed by using a polyurethane resin, wherein the polyurethane resin is formed by polyester polycarbonate diol, polyisocyanate and chain extender, wherein the polyester polycarbonate diol is obtained by an ester exchange reaction between an aliphatic oligocarbonate diol and a polyester polyol, wherein the aliphatic oligocarbonate diol is obtained by an ester exchange reaction between an aliphatic diol and a dialkyl carbonate, and wherein the polyester polyol is obtained by using a compound having an active hydrogen group as an initiator and subjecting a cyclic ester compound to ring-opening addition polymerization.

[0006] Patent document 4 discloses a porous sheet material obtained by wet coagulation, characterized in that it is formed by reacting a polymer diol, an organic isocyanate and a chain extender, wherein the polymer diol comprises a polycarbonate diol (a1) formed by an alkane diol having a carbon number of 4 or more and 6 or less and a polycarbonate diol (a2) formed by an alkane diol having a carbon number of 7 or more and 12 or less, wherein the aforementioned polycarbonate diols are copolymerized polycarbonate diols, and the percentage weight % of (a1) relative to the total weight of (a1) and (a2) is greater than 10% and less than 80%.

[0007] Patent document 5 discloses a synthetic leather comprising a surface layer formed by a surface layer material forming composition for a fiber laminate and a fiber cloth, characterized in that, in the surface layer material forming composition for a fiber laminate composed of a main agent and a curing agent, the main agent is a polycarbonate diol obtained from 1,6-hexanediol and a low molecular weight carbonate, the curing agent comprises a modified polyisocyanate (B1) of hexamethylene diisocyanate having a number average molecular weight of 350 to 500 and an average functional group number (f) of 2≤f<3 and an isocyanurate-modified polyisocyanate (B2) of hexamethylene diisocyanate with f≥3, (B1):(B2) = 50:50 to 95:5 (weight ratio), and both the main agent and the curing agent do not contain an organic solvent.

[0008] However, although the synthetic leathers disclosed in Patent Documents 1 to 5 have hydrolysis resistance, their sweat resistance is insufficient for applications requiring high durability such as automobile seats.

[0009] Therefore, Patent Document 6 proposes synthetic leather using a specific polycarbonate diol (copolycarbonate diol derived from 1,5-pentanediol and 1,6-hexanediol) in order to provide a synthetic leather having an excellent balance of physical properties such as sweat resistance and softness and not generating cracks or wrinkles during storage. However, the polycarbonate diol described in Patent Document 6 requires the use of a large amount of organic solvent during polyurethane polymerization, and further improvement is desired from the perspective of environmental burden.

[0010] Patent document 7 proposes a synthetic leather polyurethane having excellent balance of properties of flexibility, chemical resistance, low temperature characteristics, heat resistance, and touch. Here, a synthetic leather polyurethane is proposed, characterized in that it is a synthetic leather polyurethane obtained by reacting at least (a) a compound containing two or more isocyanate groups in one molecule, (b) a chain extender, and (c) a polycarbonate diol, wherein the (c) polycarbonate diol has a hydroxyl value of 20 mg-KOH / g or more and 45 mg-KOH / g or less, a glass transition temperature of -30°C or less as measured by a differential scanning calorimeter, and an average carbon number of 3 or more and 5.5 or less of a dihydroxy compound obtained by hydrolyzing the polycarbonate diol. However, the synthetic leather polyurethane disclosed in Patent document 7 also requires the use of a large amount of organic solvent during polyurethane polymerization, which is not ideal in terms of environmental burden.

[0011] In recent years, environmentally friendly polyurethanes have been proposed. For example, Patent Document 8 proposes a urethane prepolymer composition, which is a urethane prepolymer composition used to increase the molecular weight by reacting a crosslinking agent with active hydrogen in its components, and contains at least 20 to 80% by mass of a hydroxyl-terminated urethane prepolymer having a hydroxyl value of 10 to 100 mgKOH / g, and further contains 20 to 80% by mass of an oligomer having no urethane bond and a hydroxyl value of 20 to 400 mgKOH / g as a medium for the polymer, and has a substantially non-volatile component of 100%, and is liquid at least at a temperature of 30°C; and a two-component solvent-free polyurethane for synthetic leather is proposed, which is characterized in that it contains 90 to 150 equivalent % of a polyisocyanate crosslinking agent having an NCO content of 5 to 35% by mass relative to the average hydroxyl value of the urethane prepolymer composition.

[0012] However, the polyurethane prepolymer composition for synthetic leather disclosed in Patent Document 8 is to be solvent-free, and therefore, an ether polyol such as poly-THF or THF-neopentyl glycol copolymer having a hydroxyl value of 20 to 400 mgKOH / g is used as an oligomer having no urethane bond, which results in reduced heat resistance and limited applications.

[0013] Prior art literature

[0014] Patent Literature

[0015] Patent Document 1: Japanese Patent No. 3142102

[0016] Patent Document 2: Japanese Patent Application Publication No. 2003-119314

[0017] Patent Document 3: Japanese Patent Application Publication No. 2004-346094

[0018] Patent Document 4: Japanese Patent No. 4177318

[0019] Patent Document 5: Japanese Patent Application Publication No. 2009-185260

[0020] Patent Document 6: Japanese Patent Application Publication No. 2013-108196

[0021] Patent Document 7: Japanese Patent Application Publication No. 2016-8234

[0022] Patent Document 8: Japanese Patent Application Publication No. 2014-105250 Summary of the invention

[0023] Problem that the invention aims to solve

[0024] In view of the above problems, an object of the present invention is to provide a polyester polycarbonate polyol capable of obtaining a polyurethane having an excellent balance of physical properties such as softness (touch), chemical resistance, hydrolysis resistance, low-temperature characteristics, and heat resistance, and a method for producing the same.

[0025] Solutions for solving problems

[0026] As a result of intensive research, the present inventors have found that by using a polyester polycarbonate polyol having a predetermined structure, a polyurethane having an excellent balance of physical properties such as softness (touch), chemical resistance, hydrolysis resistance, low temperature characteristics, and heat resistance can be provided, and a synthetic leather having an excellent balance of physical properties such as abrasion resistance and adhesion can be provided. In addition, it has been found that a specific catalyst is useful in the production of the polyester polycarbonate polyol, thereby completing the present invention.

[0027] That is, the present invention includes the following aspects.

[0028] [1] A polyester polycarbonate polyol having a repeating unit represented by the following formula (1) and a repeating unit represented by the following formula (2), wherein the molecular ends of the polyester polycarbonate polyol are hydroxyl groups, the hydroxyl value is 37 to 86 mgKOH / g, and the carbonate group content is 15 to 40% by mass.

[0029]

[0030] (In formula (1), R1 is a divalent straight-chain aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.)

[0031]

[0032] (In formula (2), R2 is a divalent hydrocarbon having 2 to 15 carbon atoms, and R3 is a divalent straight-chain aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.)

[0033] [2] The polyester polycarbonate polyol according to [1], wherein the molar ratio of the structural unit represented by formula (1) to the structural unit represented by formula (2) is 50 / 50 to 95 / 5.

[0034] [3] The polyester polycarbonate polyol according to [1] or [2], wherein 50 mol % or more of the repeating units represented by formula (1) contain at least two repeating units selected from the group consisting of formula (3), formula (4) and formula (5).

[0035]

[0036] [4] The polyester polycarbonate polyol according to [3], wherein 50 mol % or more of the repeating units represented by formula (1) contain repeating units of formula (4) and formula (5).

[0037] [5] The polyester polycarbonate polyol according to [3], wherein 50 mol % or more of the repeating units represented by formula (1) include repeating units of formula (3) and formula (5), and the carbonate group content is 21 to 40 mass %.

[0038] [6] A synthetic leather produced using the polyester polycarbonate polyol according to any one of [1] to [5].

[0039] [7] A method for producing a polyester polycarbonate polyol, characterized in that it is a method for producing the polyester polycarbonate polyol described in [1] or [2], using a metal alkoxide as a catalyst.

[0040] [8] The method for producing a polyester polycarbonate polyol according to [7], wherein the metal alkoxide is an alkoxide of a metal of Group 4 of the Periodic Table.

[0041] Effects of the Invention

[0042] By using the polyester polycarbonate polyol of the present invention, a polyurethane having excellent physical property balance of softness (touch), chemical resistance, low temperature characteristics, heat resistance, hydrolysis resistance, abrasion resistance, and adhesiveness can be provided, and can be suitably used as a polyol for synthetic leather production. According to the present invention, a method for producing such a polyester polycarbonate polyol can also be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a cross-sectional view of an example of synthetic leather obtained using the polyester polycarbonate polyol of the present invention.

[0044] Figure 2This is a diagram showing an example of a production process diagram of a synthetic leather obtained by using the polyester polycarbonate polyol of the present invention.

[0045] Description of Reference Numerals

[0046] 1 Release paper

[0047] 2 Epidermis

[0048] 3 Adhesive layer

[0049] 4. Base material (non-woven fabric)

[0050] 5 Mixing tube (epidermis)

[0051] 6 Mixing tube (adhesive layer)

[0052] 7-piece structure (dry synthetic leather)

[0053] 8 Coating roller

[0054] 9 Crimping roller

[0055] 10 Take-up roller

[0056] 11 Dryer DETAILED DESCRIPTION

[0057] Hereinafter, this specific embodiment (hereinafter abbreviated as "this embodiment") will be described in detail. It should be noted that the present invention is not limited to the following embodiment, and various modifications can be made within the scope of the gist thereof.

[0058] The polyester polycarbonate polyol of the present embodiment has a repeating unit represented by the following formula (1) and a repeating unit represented by the following formula (2), has a hydroxyl group at the molecular end, a hydroxyl value of 37 to 86 mgKOH / g, and a carbonate group content of 15 to 40% by mass.

[0059]

[0060] (In formula (1), R1 is a divalent straight-chain aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.)

[0061]

[0062] (In formula (2), R2 is a divalent hydrocarbon having 2 to 15 carbon atoms; R3 is a divalent straight-chain aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.)

[0063] The polyester polycarbonate polyol of the present embodiment can be generally cured using a curing agent such as polyisocyanate, and used as a polyurethane in various molded products, adhesives, coating agents, and the like.

[0064] <Polyester polycarbonate polyol>

[0065] The polyester polycarbonate polyol of the present embodiment has a hydroxyl value of 37 to 86 mgKOH / g, preferably 45 to 75 mgKOH / g, and more preferably 50 to 65 mgKOH / g.

[0066] When the hydroxyl value of component (a) is 37 mgKOH / g or more, the strength and chemical resistance of the obtained polyurethane tend to be excellent. In addition, when the hydroxyl value of the polyester polycarbonate polyol is 86 mgKOH / g or less, the softness (touch) and low-temperature properties of the obtained synthetic leather tend to be high.

[0067] The melt viscosity of the polyester polycarbonate polyol at 50°C is preferably 1000 to 9000 mPa·s, more preferably 1500 to 8500 mPa·s, and further preferably 2000 to 7000 mPa·s. By setting the melt viscosity of the polyester polycarbonate polyol at 50°C to 1000 mPa·s or more, there is a tendency for the softness and low-temperature properties of the obtained polyurethane to be improved. In addition, by setting the melt viscosity of the polyester polycarbonate polyol at 50°C to 6000 mPa·s or less, there is a tendency for not only a polyurethane having excellent strength and chemical resistance to be obtained, but also the amount of solvent can be reduced when a solvent is used in the manufacture of the polyurethane.

[0068] The hydroxyl value in one molecule of the polyester polycarbonate polyol is preferably 1.7 to 3.5, more preferably 1.8 to 3.0, and still more preferably 2.0 to 2.5. By setting the hydroxyl value to 1.7 or more, there is a tendency that the strength, chemical resistance, heat resistance, and hydrolysis resistance of the obtained polyurethane are improved. In addition, by setting the hydroxyl value to 3.0 or less, not only a moderate curing time can be obtained when the polyurethane is manufactured, but also the softness of the obtained polyurethane can be obtained.

[0069] The carbonate group content contained in one molecule of the polyester polycarbonate diol of the present embodiment is 15 to 40% by mass, more preferably 21 to 40% by mass, further preferably 25 to 35% by mass, and particularly preferably 25 to 30% by mass. By making the carbonate group content 15% or more by mass, there is a tendency that the strength, chemical resistance, abrasion resistance, and hydrolysis resistance of the obtained polyurethane can be obtained. In addition, by making the carbonate group content 40% or less by mass, there is not only a tendency that the low temperature characteristics and flexibility of the obtained polyurethane are excellent, but also a tendency that the product appearance of the polyurethane is excellent because the viscosity of the obtained polyurethane is suppressed to be relatively low.

[0070] The carbonate group content is the amount of carbonate groups contained in one molecule of the polyester polycarbonate diol, and is specifically determined by the following formula (6).

[0071] Carbonate group content (%)

[0072] = (molecular weight of carbonate group) × (number of carbonate groups in one molecule) / (number average molecular weight of polyester polycarbonate polyol) × 100 (6)

[0073] (Here, the molecular weight of the carbonate group (-OC=OO-) is 60.01.)

[0074] The polyester polycarbonate polyol of the present embodiment has a repeating unit represented by the following formula (1) and a repeating unit represented by the following formula (2), and the molecular terminal is a hydroxyl group. The method for producing the polyester polycarbonate polyol of the present embodiment is not particularly limited, and can be synthesized by, for example, using a difunctional diol compound (if necessary, further using a trifunctional or higher polyol), a dibasic acid, and a carbonate as raw materials, and by, for example, an ester exchange reaction described in "Polymer Reviews, Vol. 9, pp. 9-20".

[0075]

[0076] (In formula (1), R1 is a divalent straight-chain aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.)

[0077]

[0078] (In formula (2), R2 is a divalent hydrocarbon having 2 to 15 carbon atoms; R3 is a divalent straight-chain aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.)

[0079] The difunctional diol compound used in the transesterification reaction is not particularly limited, and examples thereof include diols having a divalent straight-chain aliphatic or alicyclic hydrocarbon skeleton having 2 to 15 carbon atoms. Specific examples of the difunctional diol compound include ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,15-pentadecanediol, 1,3-cyclohexanediol, 1,4-cyclohexanedimethanol, and the like.

[0080] These bifunctional diol compounds may be used alone or in combination of two or more.

[0081] Among these, from the viewpoint of obtaining polyurethane having excellent softness (touch), chemical resistance, low temperature characteristics, and heat resistance, linear alkylene glycols having 3 to 9 carbon atoms are preferred, and linear alkylene glycols having 4 to 6 carbon atoms are more preferred. In addition, it is preferred to use two or more linear alkylene glycols in combination.

[0082] When the carbon number of the bifunctional diol compound is 2 or more, the viscosity of the polyester polycarbonate polyol can be suppressed to a low level, the amount of organic solvent used can be reduced, and on this basis, the flexibility and low-temperature properties of the obtained polyurethane tend to be improved. When the carbon number of the bifunctional diol compound is 15 or less, the chemical resistance of the obtained polyurethane tends to be excellent.

[0083] By using two or more difunctional diol compounds in combination, not only the regularity of the structural unit of the obtained polyester polycarbonate polyol is reduced, but also a liquid polyester polycarbonate polyol can be obtained at room temperature (25° C.) due to reduced crystallinity, and there is a tendency that the flexibility of the polyurethane is improved. In addition, when an organic solvent is used in the production of polyurethane, there is a tendency that the amount of the organic solvent used can be suppressed.

[0084] In the present embodiment, as a raw material of the polyester polycarbonate polyol, in addition to the difunctional diol, a trifunctional or higher-functional polyol compound may be used as necessary.

[0085] The polyol compound is not particularly limited, and examples thereof include trimethylolethane, trimethylolpropane, hexanetriol, pentaerythritol, glycerol, etc. By using a polyol, the hydroxyl value in one molecule can be easily adjusted to the range of 1.7 to 3.5.

[0086] In this embodiment, preferably, 50 mol% or more of the repeating units represented by formula (1) include at least two repeating units selected from the group consisting of formula (3), formula (4) and formula (5). The content of the above repeating units is preferably 70 mol% or more, more preferably 80 mol% or more.

[0087]

[0088] By making at least two repeating units selected from the group consisting of formula (3), formula (4) and formula (5) among the repeating units shown in formula (1) account for 50 mol% or more, the obtained polyurethane has excellent softness (touch), chemical resistance, low temperature characteristics and heat resistance. On this basis, when a solvent is used in the manufacture of polyurethane, there is a tendency to reduce the amount of solvent used. From the same point of view, it is preferred that 50 mol% or more of the repeating units shown in formula (1) contain repeating units of formula (4) and formula (5), and it is preferred that 50 mol% or more of the repeating units shown in formula (1) contain repeating units of formula (3) and formula (5), and the carbonate group content is 21 to 40 mass%.

[0089] In this embodiment, when two repeating units are selected from formula (3), formula (4) and formula (5), the ratio of the two repeating units is 90:10 to 10:90, preferably 70:30 to 30:70 in terms of molar ratio. By making the copolymerization ratio within the above range, there is a tendency that the crystallinity of the polyester polycarbonate polyol is reduced, and a polyurethane having high flexibility, good low temperature properties and touch can be obtained. Furthermore, if the copolymerization ratio is within this range, when a solvent is used in the manufacture of the polyurethane, there is a tendency that the amount of the solvent used can be reduced.

[0090] In the present embodiment, when the three repeating units of formula (3), formula (4) and formula (5) are selected, when the total of the three repeating units of formula (3), formula (4) and formula (5) is set to 100 mol%, the proportion of the structural units of formula (3), formula (4) and formula (5) is preferably 5 mol% or more, more preferably 10 mol% or more, and further preferably 20 mol% or more. By making the proportion of each of the three repeating units of formula (3), formula (4) and formula (5) in the total of the three repeating units of formula (3), formula (4) and formula (5) within the above range, there is a tendency that the crystallinity of the polycarbonate diol is reduced, and a polyurethane having high flexibility, good low temperature characteristics and touch can be obtained. Furthermore, by making the proportion of each of the three repeating units of formula (3), formula (4) and formula (5) within the above range, there is a tendency that the amount of the solvent used can be reduced when a solvent is used in the manufacture of the polyurethane.

[0091] As the dibasic acid that can be used in the synthesis of the polyester polycarbonate polyol of the present embodiment, aliphatic and / or aromatic dicarboxylic acids can be listed. As aliphatic dicarboxylic acids, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, etc. can be listed. As aromatic dicarboxylic acids, phthalic acid, isophthalic acid, terephthalic acid, etc. can be listed. In order to obtain polyurethane with excellent flexibility, aliphatic dicarboxylic acids are particularly preferably used, wherein, succinic acid, glutaric acid, adipic acid are preferably used. In addition, these dicarboxylic acids can also be used in the form of esters of alcohol, for example, can be used in the form of methyl esters such as dimethyl succinate, dimethyl glutarate, dimethyl adipate. These dicarboxylic acids can be used alone or in combination with a variety of them.

[0092] The molar ratio of the polycarbonate structural unit represented by formula (1) to the polyester structural unit represented by formula (2) in the polyester polycarbonate polyol of the present embodiment is preferably 50 / 50 to 95 / 5, more preferably 60 / 40 to 90 / 10, and even more preferably 70 / 30 to 80 / 20.

[0093] When the molar ratio of the polycarbonate structural unit represented by formula (1) to the polyester structural unit represented by formula (2) is within the above range, a polyurethane having excellent flexibility, chemical resistance, adhesiveness and hydrolysis resistance can be obtained.

[0094] As carbonates that can be used in the synthesis of the polyester polycarbonate polyol of the present embodiment, for example, dialkyl carbonates such as dimethyl carbonate, diethyl carbonate, dipropyl carbonate, and dibutyl carbonate; diaryl carbonates such as diphenyl carbonate; alkylene carbonates such as ethylene carbonate, 1,3-propylene carbonate, 1,2-propylene carbonate, 1,2-butylene carbonate, 1,3-butylene carbonate, and 1,2-pentylene carbonate, etc. From the viewpoint of ease of acquisition and ease of setting conditions for the polymerization reaction, dimethyl carbonate, diethyl carbonate, diphenyl carbonate, and ethylene carbonate are preferably used as carbonates.

[0095] When manufacturing the polyester polycarbonate polyol of the present embodiment, a catalyst may be added or not. When adding a catalyst, it can be freely selected from the catalysts used in the usual transesterification reaction. As a catalyst, metals such as lithium, sodium, potassium, rubidium, cesium, magnesium, calcium, strontium, barium, zinc, aluminum, titanium, zirconium, hafnium, cobalt, germanium, tin, lead, antimony, arsenic, cerium and their metal salts, their metal alkoxides, and organic compounds containing the metals can be used. Among the above-mentioned catalysts, metal alkoxides are preferred. Alkoxides of metals selected from titanium, zirconium and hafnium as metals of Group 4 of the periodic table are not easily affected by the generated water and can maintain high activity, so they are particularly preferred. In addition, the amount of the catalyst is usually 0.00001 to 0.1% by mass of the mass of the difunctional diol compound as a raw material and the trifunctional or higher polyol that can be included as needed, preferably 0.001 to 0.05% by mass, and more preferably 0.01 to 0.03% by mass. When the amount of the catalyst is 0.0001% by mass or more, the reaction rate can be shortened and the productivity can be improved. When the amount of the catalyst is 0.1% by mass or less, the hue of the obtained polyester carbonate polyol is excellent.

[0096] The method for producing the polyester polycarbonate polyol in the present embodiment is as described above, and can be synthesized by using a bifunctional diol compound (if necessary, a trifunctional or higher-functional polyol), a dibasic acid, and a carbonate as raw materials and performing an ester exchange reaction.

[0097] More specifically, the transesterification reaction is carried out according to the following steps.

[0098] First, one or more difunctional diol compounds at a prescribed ratio (if necessary, one or more trifunctional or higher polyols at a prescribed ratio) are mixed with a dibasic acid at a prescribed ratio and one or more carbonates at a prescribed ratio, and an ester exchange reaction is carried out at a temperature of 100 to 200° C., preferably 140 to 180° C., under normal pressure or reduced pressure and in the presence or absence of an ester exchange catalyst.

[0099] Next, alcohol derived from carbonate and water derived from dibasic acid (monohydric alcohol derived from dibasic acid when dibasic acid ester is used) generated during the reaction are removed by distillation to obtain a polyester polycarbonate polyol having a molecular weight of about 300 to 500 g / mol.

[0100] Next, the unreacted carbonate and difunctional diol (and any trifunctional or higher polyol included) and water generated by the condensation reaction of the dibasic acid (monohydric alcohol derived from the dibasic acid ester when the dibasic acid ester is used) can be distilled off under reduced pressure at 130 to 230° C., preferably at 150 to 200° C., and a polyester polycarbonate polyol having a desired hydroxyl value can be obtained through a condensation reaction.

[0101] The hydroxyl value of the polyester polycarbonate polyol can be adjusted by controlling the initial charging ratio of each component, the amount of each raw material distilled off during production, and the amount of the reaction product.

[0102] The polyester polycarbonate polyol of the present embodiment may be produced by preliminarily producing a polycarbonate polyol and a polyester polyol, mixing the polycarbonate polyol and the polyester polyol, and subjecting the mixture to an ester exchange reaction at a temperature of 100 to 200° C. under stirring in the presence or absence of the ester exchange catalyst.

[0103] In one embodiment, the present embodiment relates to a method for producing a polyester polycarbonate polyol, characterized in that it is a method for producing the polyester polycarbonate polyol of the present embodiment described above, using a metal alkoxide as a catalyst. The catalyst is a catalyst for transesterification, preferably an alkoxide of a metal of Group 4 of the periodic table.

[0104] In one embodiment, the production method includes a step of subjecting a difunctional diol compound (and, if necessary, a trifunctional or higher-functional polyol), a dibasic acid, and a carbonate to an ester exchange reaction using a metal alkoxide as a catalyst.

[0105] In one embodiment, the above-mentioned production method includes the following steps: a step of reacting a difunctional diol compound (and further a trifunctional or higher polyol as needed) with a dibasic acid to obtain a polycarbonate polyol; a step of reacting a dibasic acid with a carbonate to obtain a polyester polyol; and a step of using a metal alkoxide as a catalyst to cause an ester exchange reaction between the polycarbonate polyol and the polyester polyol.

[0106] In the method of producing polyurethane using the polyester polycarbonate polyol (hereinafter referred to as component (a)) of the present embodiment, a curing agent such as polyisocyanate (hereinafter referred to as component (b)) and, if necessary, a chain extender (hereinafter referred to as component (c)) are generally used.

[0107] In the method for producing polyurethane using the polyester polycarbonate polyol of the present embodiment, a mixture obtained by mixing the constituent components (a), (b) and (c) at once can be used as a curable composition (one-step method). Alternatively, an isocyanate-terminated prepolymer composition obtained by reacting the component (a) with the component (b) in advance can be prepared, and a mixture obtained by mixing the isocyanate-terminated prepolymer composition and the component (c) can be used as a curable composition (prepolymer method).

[0108] As the polyisocyanate used when producing polyurethane using the polyester polycarbonate polyol of the present embodiment, generally, a polyisocyanate having an average number of functional groups of 2 to 6 per molecule (component (b)) can be used.

[0109] Examples of the polyisocyanate of component (b) include aromatic diisocyanates such as 2,4-toluene diisocyanate, 2,6-toluene diisocyanate and mixtures thereof, diphenylmethane-4,4′-diisocyanate (MDI), naphthalene-1,5-diisocyanate (NDI), 3,3′-dimethyl-4,4′-biphenylene diisocyanate (TODI), and polymethylene polyphenylene polyisocyanate (PMDI); aromatic aliphatic diisocyanates such as xylylene diisocyanate (XDI) and phenylene diisocyanate; and aliphatic diisocyanates such as 4,4′-methylenebiscyclohexyl diisocyanate (hydrogenated (also referred to as hydrogenated) MDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), and cyclohexane diisocyanate (hydrogenated XDI).

[0110] As the polyisocyanate of component (b), a polyisocyanate having an average of 2.1 or more isocyanate groups in one molecule may be used. As the polyisocyanate having an average of 2.1 or more isocyanate groups in one molecule, aromatic polyisocyanates such as crude MDI and crude TDI may be used; derivatives of aliphatic isocyanates such as HDI and IPDI, specifically diisocyanate derivatives such as biuret, allophanate, uretdione, and isocyanurate; and polyol adducts may be used.

[0111] The polyisocyanate having 2.1 or more isocyanate groups in one molecule is not particularly limited, and examples thereof include Sumidur 44S and 44V70 (both manufactured by Sumika Bayer Urethanes), Desmodur HL (manufactured by Sumika Bayer Urethanes) which is a copolymer of TDI and HDI, and various DURANATEs manufactured by Asahi Kasei Corporation, namely, DURANATE 24A-100, DURANATE 22A-75PX, DURANATE 18H-70B, DURANATE 21S-75E, DURANATE THA-100, DURANATE TPA-100, DURANATE TKA100, DURANATE MFA-75X, DURANATE TSA-100, DURANATE TSS-100, DURANATE TSE-100, DURANATE D-101, DURANATE D-201, DURANATE P-301-75E, DURANATE DURANATE Available in the form of WB40-100, DURANATE WB40-80D, DURANATE WT20-100, DURANATE WT30-100, etc.

[0112] As the polyisocyanate of component (b), aromatic polyisocyanates such as MDI are preferably used. By using aromatic polyisocyanates, there is a tendency to obtain polyurethane with excellent mechanical properties. When aromatic polyisocyanates such as MDI as component (b) are used in curable composition, the curable composition can be suitably used as an adhesive for the base fabric and the epidermis of synthetic leather.

[0113] When an aliphatic polyisocyanate such as hydrogenated MDI as component (b) is used in the curable composition, synthetic leather having excellent weather resistance can be obtained using the curable composition. Therefore, the curable composition can be suitably used as a curable composition for synthetic leather for a surface layer.

[0114] As the component (b), a so-called blocked isocyanate obtained by blocking a polyisocyanate with a known blocking agent such as butanol, 2-ethylhexanol and other lower alcohols, methyl ethyl ketone oxime, lactams, phenols, imidazoles, active methylene compounds and the like may be used.

[0115] When the polyester polycarbonate polyol of the present embodiment is used to manufacture polyurethane, a chain extender (component (c)) can be used as needed. The chain extender is used to improve the abrasion resistance and strength of the obtained polyurethane. On the other hand, it sometimes reduces the softness of the obtained polyurethane, so it can be used appropriately and as needed. As a chain extender, it is not particularly limited, and short-chain glycols such as ethylene glycol and 1,4-butanediol can be listed, and polyols such as trimethylolethane, trimethylolpropane, hexanetriol, pentaerythritol, and glycerol can be listed. In addition, as a chain extender, it is not particularly limited, and diamines such as ethylenediamine, propylenediamine, hexamethylenediamine, toluenediamine, benzyl diamine, diphenyl diamine, diaminodiphenylmethane, diaminocyclohexylmethane, piperazine, 2-methylpiperazine, isophorone diamine, 3,3'-dichloro-4,4'-diaminodiphenylmethane (MOCA) and water can be listed.

[0116] The amount of the chain extender added is preferably 30% by mass or less, more preferably 3% by mass or more and 20% by mass or less, and further preferably 5% by mass or more and 15% by mass or less, relative to the total of the components (a) and (b). In addition, by using a polyol as a chain extender, the crosslinking density of the obtained polyurethane can be increased, and the strength, abrasion resistance, and chemical resistance can be improved.

[0117] When expressed as [isocyanate equivalent of component (b)] / [the total of hydroxyl equivalents of component (a) and component (c)], the amount of polyester polycarbonate polyol of component (a), polyisocyanate of component (b) and chain extender of component (c) is adjusted to preferably 0.7 to 1.3, more preferably 0.8 to 1.2, and even more preferably 0.9 to 1.1. By adjusting [isocyanate equivalent of component (b)] / [the total of hydroxyl equivalents of component (a) and component (c)] to 0.7 or more and 1.3 or less, the molecular weight of the obtained polyurethane can be appropriately controlled, and there is a tendency for excellent mechanical properties such as strength, elongation, and abrasion resistance.

[0118] When the polyester polycarbonate polyol of the present embodiment is used to manufacture polyurethane, an inactive organic solvent may be included as needed to adjust the workability when manufacturing carbamate. The content of the inactive organic solvent is preferably 80% by mass or less, more preferably 70% by mass or less, and further preferably 60% by mass or less relative to the polyurethane. In order to reduce the viscosity of the curable composition, improve its workability, and further improve the appearance of the obtained polyurethane, it is effective to add an inactive organic solvent.

[0119] As long as the inactive organic solvent is substantially inactive with respect to the polyisocyanate, there is no particular limitation, and it is preferred that it does not have active hydrogen. As the inactive organic solvent, there is no particular limitation, for example, hydrocarbons such as pentane, hexane, heptane, octane, decane, petroleum ether, petroleum benzine, volatile oil, petroleum spirit, cyclohexane, methylcyclohexane, etc.; fluorine-based inactive liquids such as fluorinated oils such as trichlorofluoroethane, tetrachlorodifluoroethane, and perfluoroether; perfluorocyclohexane, perfluorobutyltetrahydrofuran, perfluorodecahydronaphthalene, perfluoro-n-butylamine, perfluoropolyether, dimethylpolysiloxane, etc. They can be used alone or in the form of a mixture. As the inactive organic solvent, single solvents or mixed solvents such as methyl ethyl ketone (also referred to as MEK), acetone, N,N-dimethylformamide (DMF), ethyl acetate, butyl acetate, toluene, and xylene can also be listed.

[0120] When the polyester polycarbonate polyol of the present embodiment is used to manufacture polyurethane, polyols other than the polyester polycarbonate polyol may be used in combination as needed. The polyols other than the polyester polycarbonate polyol are not particularly limited, and polyether polyols, polyester polyols, polycarbonate polyols, polyolefin polyols, polybutadiene polyols, polyacrylic polyols, oil-modified polyols, etc. may be cited.

[0121] The amount of the polyol other than the polyester polycarbonate polyol added is preferably 50% by mass or less, more preferably 30% by mass or less, and further preferably 20% by mass or less, based on the total mass of the polyester polycarbonate polyol and the polyol other than the polyester polycarbonate polyol.

[0122] <Other additives>

[0123] When the polyester polycarbonate polyol of this embodiment is used to manufacture polyurethane, a curing accelerator (catalyst), a filler, a flame retardant, a dye, an organic or inorganic pigment, a release agent, a fluidity regulator, a plasticizer, an antioxidant, an ultraviolet absorber, a light stabilizer, a defoamer, a leveling agent, a colorant, a foaming agent, etc. may be added according to various uses.

[0124] The curing accelerator is not particularly limited, and examples thereof include amines and metal catalysts.

[0125] The amine-based effect accelerator is not particularly limited, and examples thereof include triethylamine and N,N-dimethylcyclohexylamine as monoamines; tetramethylethylenediamine, other triamines, cyclic amines, alcoholamines such as dimethylethanolamine, and etheramines as diamines.

[0126] The metal catalyst is not particularly limited, and examples thereof include potassium acetate, potassium 2-ethylhexanoate, calcium acetate, lead octylate, dibutyltin dilaurate, tin octylate, bismuth neodecanoate, bismuth oxycarbonate, bismuth 2-ethylhexanoate, zinc octylate, zinc neodecanoate, phosphine, and diethoxyphosphorylthiocholine.

[0127] The filler and pigment are not particularly limited, and examples thereof include woven fabrics, glass fibers, carbon fibers, polyamide fibers, mica, kaolin, bentonite, metal powder, azo pigments, carbon black, clay, silica, talc, gypsum, alumina white, and barium carbonate.

[0128] The release agent, the fluidity adjuster, and the leveling agent are not particularly limited, and examples thereof include silicone, AEROSIL, wax, stearate, polysiloxane such as BYK-331 (manufactured by BYK Chemicals Co., Ltd.), and the like.

[0129] When polyurethane is produced using the polyester polycarbonate polyol of the present embodiment, an antioxidant, a light stabilizer, and a heat stabilizer are preferably used as additives.

[0130] As the antioxidant, there is no particular limitation, and for example, phosphorus compounds such as aliphatic, aromatic or alkyl-substituted aromatic esters of phosphoric acid or phosphorous acid, hypophosphorous acid derivatives, phenylphosphonic acid, phenylphosphinic acid, diphenylphosphonic acid, polyphosphonates, dialkyl pentaerythritol diphosphites, dialkyl bisphenol A diphosphites, phenol derivatives, especially hindered phenol compounds, thioethers, disulfide carboxylates, mercaptobenzimidazoles, thiocarbanilides, thiodipropionates, and tin compounds such as tin maleate and dibutyltin oxide can be used. These can be used alone or in combination of two or more.

[0131] <Method for producing synthetic leather>

[0132] The method for producing polyurethane using the polyester polycarbonate polyol of the present embodiment can be applied to produce synthetic leather. Examples of the method for producing synthetic leather using the polyester polycarbonate polyol of the present embodiment include a wet method in which the polyurethane produced using the polyester polycarbonate polyol of the present embodiment is applied or impregnated onto a substrate (base fabric) and wet-coagulated; a dry method in which the polyurethane produced using the polyester polycarbonate polyol of the present embodiment is applied onto release paper or a substrate (base fabric) and dried.

[0133] Furthermore, as a method for manufacturing synthetic leather, the following transfer coating method (a type of dry method) can also be used: polyurethane manufactured using the polyester polycarbonate polyol of this embodiment is coated on release paper to form a surface material, and then the polyurethane manufactured using the polyester polycarbonate polyol of this embodiment is used as an adhesive layer, and after laminating the surface material to a substrate (base cloth), the release paper is removed.

[0134] The following describes a method for producing synthetic leather by taking a dry process as an example.

[0135] As the substrate (base fabric), various substrates (base fabrics) can be used, for example, fibrous substrates can be listed. As the fibrous substrate, fiber assemblies obtained by forming fibers into non-woven fabrics, woven fabrics, meshes, etc.; or substrates obtained by bonding the fibers of the fiber assembly with elastic polymers, etc. can be listed. As the fibers used in the fiber assembly, natural fibers such as kapok, hemp, and wool; regenerated or semi-synthetic fibers such as rayon and acetate; synthetic fibers such as polyamide, polyester, polyacrylonitrile, polyvinyl alcohol, and polyolefins can be listed. These fibers can be single-spun fibers or mixed-spun fibers. As other substrates, paper, release paper, polyester, polyolefin plastic films, metal plates such as aluminum, glass plates, etc. can be listed.

[0136] The polyurethane produced using the polyester polycarbonate polyol of the present embodiment can be coated by a generally used method, such as a floating knife coater, a roll blade coater, a reverse roll coater, a roll blade coater, a gravure roll coater, a kiss roll coater, etc.

[0137] The obtained synthetic leather can be used directly. Alternatively, for the purpose of further imparting various characteristics, the synthetic leather can also be obtained by coating a polymer solution or emulsion of a polyurethane resin, vinyl chloride, a cellulose resin, etc. In addition, the synthetic leather can also be obtained by laminating with a coating film and then peeling off a release paper to obtain a laminated body, wherein the coating film is obtained by drying the above-mentioned polymer solution or emulsion separately coated on the release paper.

[0138] Hereinafter, the present embodiment will be described with reference to the drawings. The drawings and manufacturing conditions described below are one form of the present embodiment, and the present embodiment is not limited thereto.

[0139] Figure 1 is through Figure 2 Schematic cross-sectional view of a synthetic leather laminate produced by a dry process as shown. The laminate has a structure in which an adhesive layer 3 is sandwiched between a substrate (nonwoven fabric) 4 and a skin layer 2. A release paper 1 used during production is attached to the outermost layer, but it is peeled off and reused when used.

[0140] Figure 21 is a schematic diagram showing one method for producing a dry synthetic leather laminate sheet using a polyurethane produced using the polyester polycarbonate polyol of the present embodiment. In the production method, first, a curable composition is cast on a release paper 1 (usually having a leather-like pattern), wherein the curable composition is obtained by mixing various raw materials adjusted to a predetermined temperature in a mixing tube 5.

[0141] When the one-step method is used, component (a), component (b) and component (c) as required, as well as an inactive organic solvent and additives as required are continuously fed into a mixing tube 5, respectively, or component (b) and other raw materials (a mixture of component (a), component (c), an inactive organic solvent and additives as required) are continuously fed into a mixing tube 5, mixed, and cast on a release paper 1.

[0142] When the prepolymer method is used, a mixture of a prepolymer composition, a polycarbonate polyol that has not been prepolymerized (component (a)) and / or a chain extender (component (c)), an inactive organic solvent as required, and additives is continuously fed into a mixing tube 5, mixed, and cast on a release paper 1.

[0143] The temperature of each component before mixing is usually adjusted to 20 to 80°C, preferably 30 to 70°C, and more preferably 40 to 60°C. In addition, the temperature of the mixing tube 5 is also usually adjusted to a temperature of 20 to 80°C, preferably 30 to 70°C, and more preferably 40 to 60°C. By making the temperature of each component before mixing and the temperature of the mixing tube 5 above 20°C, there is a tendency that the viscosity of the raw materials used, especially the polycarbonate polyol, is suppressed and the flow rate is stabilized. In addition, by making the temperature of each component before mixing and the temperature of the mixing tube 5 below 80°C, the curing speed of the curable polyurethane manufactured by the polyester polycarbonate polyol of this embodiment can be appropriately controlled, and there is a tendency to suppress a sharp increase in viscosity and obtain synthetic leather of uniform thickness.

[0144] After that, after being formed into a sheet of a certain thickness by a coating roller 8, it is passed through a dryer 11 for curing and drying of the inert organic solvent to form the surface skin layer 2 of the synthetic leather. The temperature of the dryer is usually set to 60 to 150° C., preferably 70 to 130° C., and more preferably 80 to 120° C. The drying time is usually 2 to 15 minutes, preferably 3 to 10 minutes, and more preferably 4 to 7 minutes.

[0145] Next, the respective raw materials of the curable polyurethane composition adjusted to a predetermined temperature in advance are mixed in a mixing tube 6 , and the curable composition thus obtained is cast to form the adhesive layer 3 .

[0146] When a one-step method is applied in the manufacture of the adhesive layer, components (a), (b) and (c), as well as an inactive organic solvent and an additive as required, are respectively and continuously fed into a mixing tube 6, or component (b) and other raw materials (a mixture of components (a), (c) and an inactive organic solvent and an additive as required) are both continuously fed into a mixing tube 6, mixed, and cast on the epidermis layer.

[0147] When the prepolymer method is applied to the manufacture of the adhesive layer, the prepolymer composition and the unprepolymerized polyol (component (a)), as well as the inactive organic solvent and additives as required, are respectively continuously fed into the mixing tube 6, or the prepolymer composition and a mixture of other raw materials (unprepolymerized polyol (component (a) and / or chain extender (component (c)), as required, inactive organic solvent, additives) are continuously fed into the mixing tube 6, mixed, and cast on the skin layer.

[0148] The temperature of each component before mixing is usually adjusted to 20 to 60°C, preferably 30 to 50°C, and more preferably 35 to 45°C. In addition, the temperature of the mixing tube 6 is also usually adjusted to 20 to 60°C, preferably 30 to 50°C, and more preferably 35 to 45°C. By making the temperature of each component before mixing and the temperature of the mixing tube 6 above 20°C, the viscosity of the raw materials used, especially polyester polycarbonate polyol, can be suppressed, and there is a tendency for the flow rate to be stable. In addition, by making the temperature of each component before mixing and the temperature of the mixing tube 6 below 60°C, the curing speed of the curable composition can be appropriately controlled, and there is a tendency to suppress the rapid viscosity increase of the curable composition and obtain a uniform thickness of the synthetic leather.

[0149] After that, after being formed into a sheet of a certain thickness by a coating roller 8, it is passed through a dryer 11 for curing and drying of the inactive organic solvent to form an adhesive layer 3 of synthetic leather. Next, the substrate 4 and the adhesive layer 3 are overlapped and pressed by a pressing roller 9 to obtain a sheet structure 7, which is wound up by a winding roller 10 to obtain a desired synthetic leather laminate. The temperature of the dryer 11 is usually set to 60 to 150° C., preferably 70 to 130° C., and more preferably 80 to 120° C. The drying time is usually 2 to 15 minutes, preferably 3 to 10 minutes, and more preferably 4 to 7 minutes.

[0150] Figure 2The manufacturing example of synthetic leather including three layers of epidermis layer / adhesive layer / substrate is shown in, but the synthetic leather laminate including two layers of epidermis layer / substrate with the adhesive layer omitted can also be manufactured using the same equipment. The adhesion between the epidermis layer and the substrate is controlled by adjusting the curing state of the curable composition. Specifically, it can be obtained by pressing the curable composition with the substrate in an incompletely cured state. Therefore, the curing temperature of the dryer 11 is set to 60 to 150°C, preferably 70 to 130°C, and more preferably 80 to 120°C. The drying time is usually set to 2 minutes to 15 minutes, preferably 3 minutes to 10 minutes, and more preferably 4 minutes to 7 minutes.

[0151] <Purpose>

[0152] The synthetic leather obtained by using the polyurethane produced by using the polyester polycarbonate polyol of the present embodiment can be used for automotive interior materials such as automotive sheets, furniture such as sofas, clothing, shoes, bags, other general merchandise, etc. In addition, it can also be used for laminating adhesives and surface protective agents for various films.

[0153] Example

[0154] The present invention is described in more detail below by way of examples and comparative examples, but the present invention is not limited to these examples unless the gist of the invention is exceeded. In the following examples and comparative examples, the analysis and evaluation methods of the physical properties of each component are as follows.

[0155] [Analysis and evaluation of polyester polycarbonate polyols]

[0156] <Hydroxy Value of Polyester Polycarbonate Polyol>

[0157] The measurement was conducted in accordance with JIS K1557-1.

[0158] <Composition of polyester polycarbonate polyol (copolymerization ratio)>

[0159] 1g of polyester polycarbonate polyol sample was weighed into a 100mL eggplant flask, and 30g of methanol and 8g of 28% sodium methoxide methanol solution were added, and the mixture was reacted at 100°C for 1 hour. After the reaction solution was cooled to room temperature, 2 to 3 drops of phenolphthalein were added as an indicator and neutralized with hydrochloric acid. After cooling in a refrigerator for 1 hour, the mixture was filtered and analyzed using a gas chromatograph (GC). In the GC analysis, a gas chromatograph GC-14B (manufactured by Shimadzu Corporation, Japan) with a DB-WAX (manufactured by J&W Company, USA) as a column was used, diethylene glycol diethyl ester was used as an internal standard, and a hydrogen flame ionization detector (FID) was used as a detector to perform quantitative analysis of each component. It should be noted that the temperature rise curve of the column is as follows: after maintaining at 60°C for 5 minutes, the temperature was raised to 250°C at 10°C / min.

[0160] The composition (copolymerization ratio) of the polyester polycarbonate polyol was determined from the alcohol components detected from the above analysis results and the methyl ester component derived from the dibasic acid.

[0161] For the composition of the polyester polycarbonate polyol containing a dibasic acid, the molar number of the diols constituting the carbonate skeleton can be calculated by using the value after deducting the diol having the same molar number as the molar number of the methyl ester derived from the dibasic acid (when multiple diols are used, the calculation is performed based on the ratio of the diols obtained by gas chromatography, assuming that the composition of the diols in the carbonate skeleton is the same as the composition of the diols in the ester skeleton).

[0162] <Measurement of Melt Viscosity>

[0163] The polyester polycarbonate polyol was preheated to 50°C, and then the melt viscosity was measured at 50°C using an E-type viscometer (TVE-22HT, cone No. 6, manufactured by Toki Sangyo Co., Ltd.).

[0164] <Carbonate Group Content of Polyester Polycarbonate Polyol>

[0165] The carbonate group content is the amount of carbonate groups contained in one molecule of polyester polycarbonate diol, and is specifically determined by the following formula (6).

[0166] Carbonate group content (%)

[0167] = (molecular weight of carbonate group) × (number of carbonate groups in one molecule) / (number average molecular weight of polyester polycarbonate polyol) × 100 (6)

[0168] (Here, the molecular weight of the carbonate group (-OC=OO-) is 60.01.)

[0169] The number of carbonate groups in one molecule can be determined from the number of repeating units (x) of the carbonate structure using the following formula (8) based on the structure of the following formula (7).

[0170]

[0171] (Here, m represents the average number of methylene groups in the diol, x represents the number of repeating units of the carbonate structural skeleton in one molecule, y represents the number of repeating units of the ester structural skeleton, and the underlined portion represents the terminal group. R2 represents a hydrocarbon derived from the dibasic acid used.)

[0172] The structure of each segment constituting the polycarbonate is determined from the composition of the polyester polycarbonate polyol determined in the above <Composition (copolymerization ratio) of polyester polycarbonate polyol> The number of methylene groups in each constituting segment is determined from this, and the average number of methylene groups (m) is calculated from the ratio.

[0173] Carbonate group repeating unit number (x)

[0174] = [(number average molecular weight (Mn) - (molecular weight of ester backbone) - (molecular weight of terminal group)) / (molecular weight of carbonate backbone repeating unit) (8)

[0175] In formula (8), the molecular weight of the ester skeleton is calculated by the composition of the carbonate skeleton obtained by the gas chromatography and the composition of the ester skeleton. Specifically, the following number is the molecular weight of the ester skeleton: the molecular weight obtained by deducting the average molecular weight of the average terminal diol group from the average molecular weight of the polyester polycarbonate polyol is multiplied by the number obtained by converting the molar composition of the ester skeleton obtained by gas chromatography into the mass ratio obtained by mass composition.

[0176] [Analysis and evaluation of polyurethane films]

[0177] <Production of polyurethane film>

[0178] The components of the curable composition of the present invention preheated to 40°C were added to a 200 mL separable four-necked flask with a stirring blade (45 degrees tilted, 4 blades paddle type) under a nitrogen atmosphere in an amount of 80 g in terms of the curable composition. After stirring at 40°C for 5 minutes, the mixture was applied to a polypropylene resin sheet (100 mm in width, 1200 mm in length, and 1 mm in thickness) using an applicator with a width of 80 mm, a length of 100 mm, and a thickness of 0.6 mm. The mixture was dried on a heating plate at a surface temperature of 60°C for 2 hours, and then dried in an oven at 100°C for 12 hours. Furthermore, the mixture was allowed to stand at a constant temperature and humidity of 23°C and 55% RH for more than 12 hours to obtain a polyurethane film. The obtained polyurethane film was subjected to the evaluation of various physical properties.

[0179] <Softness of polyurethane film>

[0180] The softness of the polyurethane film was evaluated by five inspectors, who evaluated the touch of the film by hand. The evaluation criteria were as follows.

[0181] ○ indicates softness, and the evaluation results of the five inspectors were consistent.

[0182] △ means slightly hard, and the evaluation results of the five inspectors were consistent.

[0183] × indicates hard, and the evaluation results of the five inspectors are consistent.

[0184] <Appearance of polyurethane film>

[0185] The surface appearance of the polyurethane film produced as described above was visually evaluated according to the following criteria.

[0186] ○ indicates a smooth surface.

[0187] △ indicates that streaks are slightly observed on the surface along the applicator moving direction.

[0188] × indicates that a large number of streaks were observed on the surface along the direction of applicator movement.

[0189] <Determination of Molecular Weight>

[0190] A portion of the polyurethane film was cut out and an N,N-dimethylacetamide solution was prepared so that the polyurethane concentration became 0.1 mass %, and the number average molecular weight (Mn) converted to standard polystyrene was measured using a GPC apparatus [manufactured by Tosoh Corporation, product name "HLC-8320" (column: Tskgel SuperHM-H·4 columns), an eluent was a solution obtained by dissolving 2.6 g of lithium bromide in 1 L of dimethylacetamide].

[0191] <Evaluation of Oleic Acid Resistance>

[0192] Cut out a 3cm×3cm test piece from the polyurethane film. After measuring the weight of the test piece with a precision balance, put it into a 250mL glass bottle containing 50mL of oleic acid as the test solvent, and let it stand in a constant temperature bath under a nitrogen atmosphere at 80°C for 16 hours. After the test, take out the test piece, gently wipe the back with a paper handkerchief, measure the weight with a precision balance, and calculate the weight change rate (increase rate) compared with before the test. When the weight change rate is close to 0%, it means that the oleic acid resistance is good.

[0193] <Evaluation of ethanol resistance>

[0194] Using the same method as in the above-mentioned <Evaluation of Oleic Acid Resistance>, after making the urethane film, cut the test piece of the urethane film into 3cm×3cm. After measuring the weight of the test piece with a precision balance, put it into a glass culture dish with an inner diameter of 10cmφ filled with 50mL of ethanol as a test solvent, and immerse it at room temperature of about 23°C for 1 hour. After the test, take out the test piece, wipe it lightly with a paper handkerchief, and measure the weight with a precision balance to calculate the weight change rate (increase rate) compared with before the test. When the weight change rate is close to 0%, it means that the ethanol resistance is good.

[0195] <Measurement of glass transition temperature (Tg)>

[0196] A test piece with a width of 10 mm, a length of 40 mm, and a thickness of 0.4 mm was cut out from the polyurethane film. The test piece was set with a distance between the clamps of 20 mm using a viscoelasticity measuring device (manufactured by Hitachi High-Technologies Corporation, [TA7000 series, DMA7100]), and the viscoelasticity was measured while the temperature was raised from -100°C to 100°C at 5°C / min. The peak of tanδ was read to determine the glass transition temperature (Tg).

[0197] <Room temperature tensile test>

[0198] In accordance with JIS K6301 (2010), a tensile test was conducted on a polyurethane test piece in the form of a short strip having a width of 10 mm, a length of 100 mm, and a thickness of about 0.5 mm using a tensile testing machine (manufactured by ORIENTEC, product name "TENSILON, RTE-1210 model") at a distance between the clamps of 20 mm, a tensile speed of 100 mm / min, and a temperature of 23°C (relative humidity of 55%), and the stress, breaking point strength, and breaking point elongation of the test piece when the test piece was elongated by 100% were measured.

[0199] <Low Temperature Tensile Test>

[0200] According to JIS K6301 (2010), a polyurethane test piece having a width of 10 mm, a length of 100 mm, and a thickness of about 0.5 mm was placed in a tensile testing machine (TENSILON, RTE-1210, manufactured by ORIENTEC) with a thermostatic chamber (TLF-R3T-EW, manufactured by ORIENTEC) with a distance between the clamps of 20 mm. After standing at -20°C for 5 minutes, a tensile test was performed at a tensile speed of 100 mm / min, and the stress at which the test piece was elongated by 100% was measured.

[0201] <Evaluation of Heat Resistance>

[0202] The polyurethane film was prepared into a short strip with a width of 10 mm, a length of 100 mm, and a thickness of about 50 μm, and heated in a gear oven at 120° C. for 1000 hours. The breaking strength of the heated sample was measured in the same manner as in the <Room Temperature Tensile Test>, and the retention rate (%) was determined.

[0203] <Evaluation of hydrolysis resistance>

[0204] The polyurethane film was made into a short strip with a width of 10 mm, a length of 100 mm, and a thickness of about 50 μm, and heated in a constant temperature and humidity chamber at a temperature of 70°C and a relative humidity of 95% for 400 hours. The breaking strength of the heated sample was measured in the same manner as in the above <Room Temperature Tensile Test>, and its retention rate (%) was calculated.

[0205] [Analysis and evaluation of synthetic leather]

[0206] <Softness of synthetic leather>

[0207] The softness of the synthetic leather was evaluated by five inspectors, who evaluated the touch of the synthetic leather by hand. The evaluation criteria were as follows.

[0208] ○ indicates softness, and the evaluation results of the five inspectors were consistent.

[0209] △ means slightly hard, and the evaluation results of the five inspectors were consistent.

[0210] × indicates hard, and the evaluation results of the five inspectors are consistent.

[0211] <Abrasion resistance of synthetic leather>

[0212] A load of 9.8 N was applied to the friction piece covered with cotton cloth to abrade the surface of the synthetic leather. The friction piece was abraded 10,000 times at a speed of 60 back and forth / minute over a distance of 140 mm on the surface of the synthetic leather. The synthetic leather after abrasion was observed and judged according to the following criteria.

[0213] ○ indicates that the resin layer has no cracks or damage.

[0214] △ indicates that cracks occurred in the resin layer.

[0215] × indicates that the resin layer is damaged.

[0216] <Low-temperature storage stability of synthetic leather>

[0217] The synthetic leather was wound around a paper tube with a diameter of 10 cm and stored in a thermostatic chamber at -20°C for 1 month. The synthetic leather was removed from the paper tube and placed in a thermostatic chamber at 23°C and 50% humidity for 1 day, and the surface was visually observed.

[0218] The case where there were no cracks or wrinkles at all was evaluated as "○", the case where slight cracks or wrinkles of 1 mm or less were observed was evaluated as "△", and the case where cracks or wrinkles exceeding 1 mm were observed was evaluated as "×".

[0219] <Evaluation method of adhesiveness>

[0220] The interface between the polyester base fabric and the polyurethane resin layer of the synthetic leather was previously scratched, and the peeled urethane resin layer and the base fabric were fixed with clamps respectively. The peel strength between the polyurethane layer and the base fabric was measured at a temperature of 23°C and a speed of 200 mm / min in accordance with JIS K6854-2 using a tensile tester (manufactured by ORIENTEC, TENSILON RTE-1210 model) as an evaluation of the adhesion.

[0221] [Example 1]

[0222] [Polymerization Example 1 of Polyester Polycarbonate Polyol]

[0223] 221 g (2.51 mol) of ethylene carbonate, 148 g (1.64 mol) of 1,4-butanediol, 195 g (1.65 mol) of 1,6-hexanediol, and 202 g (1.38 mol) of adipic acid were added to a 2L glass flask equipped with a distillation column filled with regular packing and a stirring device. 0.10 g of titanium tetra-n-butoxide was added as a catalyst, the reaction temperature was set to 150-170°C, and the pressure was reduced from 10 kPa to 3 kPa while the generated mixture of water, ethylene glycol and ethylene carbonate was distilled off, and the reaction was carried out for 12 hours.

[0224] Thereafter, the reaction was switched to single distillation, and the monomer was distilled off at 170° C. for 5 hours while the pressure was gradually reduced to 0.1 kPa. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC1) are shown in Table 1.

[0225] [Example 2]

[0226] [Polymerization Example 2 of Polyester Polycarbonate Polyol]

[0227] The polymerization was carried out in the same manner as in Polymerization Example 1 except that the amount of adipic acid charged was 171 g (1.17 mol) using the same apparatus as in Polymerization Example 1. Table 1 shows the analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC2).

[0228] [Example 3]

[0229] [Polymerization Example 3 of Polyester Polycarbonate Polyol]

[0230] Using the same apparatus as in Polymerization Example 1, polymerization was carried out in the same manner as in Polymerization Example 1 except that the amount of adipic acid charged was 122 g (0.84 mol). Table 1 shows the analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC3).

[0231] [Example 4]

[0232] [Polymerization Example 4 of Polyester Polycarbonate Polyol]

[0233] The polymerization was carried out in the same manner as in Polymerization Example 1 except that the amount of adipic acid charged was 90 g (0.62 mol) using the same apparatus as in Polymerization Example 1. Table 1 shows the analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC4).

[0234] [Example 5]

[0235] [Polymerization Example 5 of Polyester Polycarbonate Polyol]

[0236] The polymerization was carried out in the same manner as in Polymerization Example 1 except that the amount of adipic acid charged was 49 g (0.33 mol) using the same apparatus as in Polymerization Example 1. Table 1 shows the analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC5).

[0237] [Example 6]

[0238] [Polymerization Example 6 of Polyester Polycarbonate Polyol]

[0239] The polymerization was carried out in the same manner as in Polymerization Example 1 except that the amount of adipic acid charged was changed to 28 g (0.19 mol) using the same apparatus as in Polymerization Example 1. Table 1 shows the analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC6).

[0240] [Example 7]

[0241] [Polymerization Example 7 of Polyester Polycarbonate Polyol]

[0242] The polymerization was carried out in the same manner as in Polymerization Example 1 except that the feed amounts were changed to 221 g (2.51 mol) of ethylene carbonate, 171 g (1.64 mol) of 1,5-pentanediol, 195 g (1.65 mol) of 1,6-hexanediol, and 122 g (0.84 mol) of adipic acid using the same apparatus as in Polymerization Example 1. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC7) are shown in Table 1.

[0243] [Example 8]

[0244] [Polymerization Example 8 of Polyester Polycarbonate Polyol]

[0245] The polymerization was carried out in the same manner as in Polymerization Example 1 except that the feed amounts were changed to 221 g (2.51 mol) of ethylene carbonate, 171 g (1.64 mol) of 1,5-pentanediol, 195 g (1.65 mol) of 1,6-hexanediol, and 90 g (0.62 mol) of adipic acid using the same apparatus as in Polymerization Example 1. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC8) are shown in Table 1.

[0246] [Example 9]

[0247] [Polyester polycarbonate polyol polymerization example 9]

[0248] The polymerization was carried out in the same manner as in Polymerization Example 1 except that the feed amounts were changed to 221 g (2.51 mol) of ethylene carbonate, 171 g (1.64 mol) of 1,5-pentanediol, 195 g (1.65 mol) of 1,6-hexanediol, and 90 g (0.62 mol) of adipic acid using the same apparatus as in Polymerization Example 1. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC9) are shown in Table 1.

[0249] [Example 10]

[0250] [Polymerization Example 10 of Polyester Polycarbonate Polyol]

[0251] The polymerization was carried out in the same manner as in Polymerization Example 1 except that the feed amounts were changed to 250 g (2.84 mol) of ethylene carbonate, 494 g (4.18 mol) of 1,6-hexanediol, and 122 g (0.84 mol) of adipic acid using the same apparatus as in Polymerization Example 1. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC10) are shown in Table 1.

[0252] [Example 11]

[0253] [Polymerization Example 11 of Polyester Polycarbonate Polyol]

[0254] The polymerization was carried out in the same manner as in Polymerization Example 1 except that the feed amounts were changed to 250 g (2.84 mol) of ethylene carbonate, 377 g (4.18 mol) of 1,4-butanediol, and 122 g (0.84 mol) of adipic acid using the same apparatus as in Polymerization Example 1. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC11) are shown in Table 1.

[0255] [Example 12]

[0256] [Polymerization Example 12 of Polyester Polycarbonate Polyol]

[0257] Polymerization was carried out in the same manner as in Polymerization Example 3 except that the polymerization time after switching to single distillation was 4 hours. Table 1 shows the analysis results of the obtained polycarbonate polyol (also referred to as PEC12).

[0258] [Example 13]

[0259] [Polyester polycarbonate polyol polymerization example 13]

[0260] Polymerization was carried out in the same manner as in Polymerization Example 3 except that the polymerization time after switching to single distillation was 3 hours. Table 1 shows the analysis results of the obtained polycarbonate polyol (also referred to as PEC13).

[0261] [Example 14]

[0262] [Polymerization Example 14 of Polyester Polycarbonate Polyol]

[0263] Polymerization was carried out in the same manner as in Polymerization Example 3 except that the polymerization time after switching to single distillation was 7 hours. Table 1 shows the analysis results of the obtained polycarbonate polyol (also referred to as PEC14).

[0264] [Example 15]

[0265] [Polymerization Example 15 of Polyester Polycarbonate Polyol]

[0266] Polymerization was carried out in the same manner as in Polymerization Example 3 except that the polymerization time after switching to single distillation was 9 hours. Table 1 shows the analysis results of the obtained polycarbonate polyol (also referred to as PEC15).

[0267] [Example 16]

[0268] [Polymerization Example 16 of Polyester Polycarbonate Polyol]

[0269] The polymerization was carried out in the same manner as in Polymerization Example 1 except that the feed amounts were changed to 221 g (2.51 mol) of ethylene carbonate, 185 g (2.05 mol) of 1,4-butanediol, 195 g (1.65 mol) of 1,6-hexanediol, and 122 g (0.84 mol) of adipic acid using the same apparatus as in Polymerization Example 1. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC16) are shown in Table 1.

[0270] [Example 17]

[0271] [Polyester polycarbonate polyol polymerization example 17]

[0272] The polymerization was carried out in the same manner as in Polymerization Example 1 except that the feed amounts were changed to 221 g (2.51 mol) of ethylene carbonate, 92 g (1.02 mol) of 1,4-butanediol, 390 g (3.30 mol) of 1,6-hexanediol, and 122 g (0.84 mol) of adipic acid using the same apparatus as in Polymerization Example 1. The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC17) are shown in Table 1.

[0273] [Example 18]

[0274] [Polymerization Example 18 of Polyester Polycarbonate Polyol]

[0275] Using the same apparatus as in Polymerization Example 1, polymerization was carried out in the same manner as in Polymerization Example 3 except that terephthalic acid was used instead of adipic acid and the amount of terephthalic acid charged was 140 g (0.84 mol). The analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC18) are shown in Table 1.

[0276] [Comparative Example 1]

[0277] [Polymerization Example 19 of Polyester Polycarbonate Polyol]

[0278] Polymerization was carried out in the same manner as in Polymerization Example 3 except that the polymerization time after switching to single distillation was set to 2 hours. Table 1 shows the analysis results of the obtained polycarbonate polyol (also referred to as PEC19).

[0279] [Comparative Example 2]

[0280] [Polymerization Example 20 of Polyester Polycarbonate Polyol]

[0281] Polymerization was carried out in the same manner as in Polymerization Example 3 except that the polymerization time after switching to single distillation was 11 hours. Table 1 shows the analysis results of the obtained polycarbonate polyol (also referred to as PEC20).

[0282] [Comparative Example 3]

[0283] [Polymerization Example 21 of Polyester Polycarbonate Polyol]

[0284] Using the same apparatus as in Polymerization Example 1, polymerization was carried out in the same manner as in Polymerization Example 1 except that the amount of adipic acid charged was 280 g (1.92 mol). Table 1 shows the analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC21).

[0285] [Comparative Example 4]

[0286] [Polymerization Example 22 of Polyester Polycarbonate Polyol]

[0287] The polymerization was carried out in the same manner as in Polymerization Example 1 except that the amount of adipic acid charged was 20 g (0.14 mol) using the same apparatus as in Polymerization Example 1. Table 1 shows the analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC22).

[0288] [Comparative Example 5]

[0289] [Polymerization Example 23 of Polyester Polycarbonate Polyol]

[0290] 221 g (2.51 mol) of ethylene carbonate, 148 g (1.64 mol) of 1,4-butanediol, 195 g (1.65 mol) of 1,6-hexanediol, and 158 g (1.38 mol) of ε-caprolactone were added to a 2L glass flask equipped with a distillation column filled with regular packing and a stirring device. 0.10 g of titanium tetrabutoxide was added as a catalyst, the reaction temperature was set to 150-170°C, and the pressure was reduced from 10 kPa to 3 kPa while the generated mixture of water, ethylene glycol and ethylene carbonate was distilled off, and the reaction was carried out for 12 hours.

[0291] Thereafter, the reaction was switched to single distillation, and the pressure was gradually reduced to 0.1 kPa while reacting at 170° C. for 5 hours to distill off the monomer. Table 1 shows the analysis results of the obtained polyester polycarbonate polyol (also referred to as PEC23).

[0292] [Table 1]

[0293]

[0294] [Example 19]

[0295] 15.34 g (0.06 mol) of diphenylmethane-4,4'-diisocyanate (MDI, average number of isocyanate groups in one molecule: 2.0) and 80 g of N,N-dimethylformamide (DMF) were added to a 500 mL separable flask sealed with nitrogen and equipped with a stirrer, and heated to 40°C to obtain a solution. 40.0 g (0.02 mol) of polyester polycarbonate polyol PEC1 to which 60 g of N,N-dimethylformamide (DMF) and 0.0028 g of dibutyltin dilaurate as a catalyst were added dropwise to the flask over 30 minutes while stirring the solution. The reaction was carried out at 60°C under stirring for 2 hours to obtain a prepolymer of terminal isocyanate. Next, 3.6 g (0.04 mol) of 1,4-butanediol was added as a chain extender, and after reacting at 60°C for 1 hour, 0.5 g of ethanol was added as a reaction terminator to obtain a DMF solution of polyurethane (solid content was about 30% by mass). The obtained N,N-dimethylformamide (DMF) solution of polyurethane was applied to a glass plate and heated at 80°C for 2 hours to prepare a polyurethane film with a film thickness of 50 μm. After being left at room temperature for 24 hours, various physical properties were evaluated. The evaluation results are shown in Table 2.

[0296] [Examples 20 to 36]

[0297] A polyurethane film was obtained in the same manner as in Example 1 except that PEC2 to PEC18 were used as polyester polycarbonate polyols and the mass of the polyester polycarbonate used was set to the mass described in Table 2, and various physical properties were evaluated.

[0298] [Comparative Examples 6 to 10]

[0299] A polyurethane film was obtained in the same manner as in Example 1 except that PEC19 to PEC23 were used as polyester polycarbonate polyols and the mass of the polyester polycarbonate used was set to the mass described in Table 1, and various physical properties were evaluated.

[0300] [Table 2]

[0301]

[0302] [Example 37]

[0303] 15.74 g (0.06 mol) of 4,4'-methylenebiscyclohexyl diisocyanate (hydrogenated MDI, average number of isocyanate groups in one molecule: 2.0) and 80 g of N,N-dimethylformamide (DMF) were added to a 500 mL separable flask sealed with nitrogen and equipped with a stirrer, and heated to 50°C to obtain a solution. 40 g (0.02 mol) of polyester polycarbonate polyol PEC2 to which 60 g of N,N-dimethylformamide (DMF) and 0.0028 g of dibutyltin dilaurate as a catalyst were added dropwise to the flask over 30 minutes while stirring the solution. The reaction was carried out at 70°C under stirring for 2 hours to obtain a prepolymer of terminal isocyanate. Next, 6.8 g (0.04 mol) of isophorone diamine was added as a chain extender, and the reaction was carried out at 70°C for 2 hours. Then, 0.5 g of ethanol was added as a reaction terminator to obtain a DMF solution of polyurethane (solid content was about 30% by mass). The obtained N,N-dimethylformamide (DMF) solution of polyurethane was applied to a glass plate and heated at 80°C for 2 hours to prepare a polyurethane film with a film thickness of 50 μm. After being left at room temperature for 24 hours, various physical properties were evaluated. The evaluation results are shown in Table 3.

[0304] [Examples 38 to 46]

[0305] A polyurethane film was obtained in the same manner as in Example 37 except that PEC3, 4, 5, 8, 10, 11, 13, 14, and 18 were used as polyester polycarbonate polyols, and various physical properties were evaluated. The evaluation results are shown in Table 3.

[0306] [Comparative Examples 11 to 15]

[0307] A polyurethane film was obtained in the same manner as in Example 1 except that PC19 to PC23 were used as polyester polycarbonate polyols, and was subjected to evaluation of various physical properties. The evaluation results are shown in Table 3.

[0308] [Table 3]

[0309]

[0310] [Example 47]

[0311] Use with Figure 2 Using a release paper with a knotted pattern (R-8 manufactured by LINTEC), a composition having the same composition ratio as that of Example 38 (a prepolymer obtained by reacting an isocyanate with a polyester polycarbonate polyol and a chain extender were continuously mixed in a mixing tube at a temperature of 70°C just before use) was continuously cast onto the release paper, and the thickness was adjusted to 50 μm with a coating roll. The composition was passed through a dryer at 120°C to form a urethane layer serving as a skin layer.

[0312] Next, a composition having the same composition ratio as that of Example 21 (the two components, a prepolymer obtained by reacting an isocyanate with a polyester polycarbonate polyol and a chain extender, were continuously mixed in a mixing tube at a temperature of 70° C. immediately before use) was continuously mixed in a mixing tube at a temperature of 40° C., and continuously cast on release paper, and adjusted to a thickness of 250 μm with a coating roller. The composition was passed through a 120° C. dryer to form a urethane layer serving as an adhesive layer.

[0313] Next, a base fabric (nonwoven fabric made of polyester fibers) having a thickness of 500 μm was bonded together using a pressure roller and wound up using a winding roller to obtain a synthetic leather made of a laminate of polyurethane. The obtained synthetic leather was evaluated. The results are shown in Table 4.

[0314] [Examples 48 to 54]

[0315] A synthetic leather composed of a laminate of polyurethane was obtained in the same manner as in Example 47 except that the polyurethane to be the surface layer and the polyurethane to be the adhesive layer were formed using the same composition ratio as in the examples shown in Table 4. The obtained synthetic leather was evaluated and the results are shown in Table 4.

[0316] [Comparative Examples 15 to 19]

[0317] A synthetic leather composed of a laminate of polyurethane was obtained in the same manner as in Example 47 except that the polyurethane to be the surface layer and the polyurethane to be the adhesive layer were formed using the same composition ratio as in the comparative example shown in Table 4. The obtained synthetic leather was evaluated and the results are shown in Table 4.

[0318] [Table 4]

[0319]

[0320] [Example 55]

[0321] [Polymerization Example 24 of Polyester Polycarbonate Polyol]

[0322] As a catalyst, 0.11 g of zirconium tetra-n-butoxide was added instead of titanium tetra-n-butoxide, and a polyester polycarbonate polyol was synthesized in the same manner as in Example 3. The obtained polyester polycarbonate polyol had an appearance of a viscous liquid, a hydroxyl value of 55.2 mgKOH / g, and a copolymerization ratio of 35.6 mol% of a carbonate structure derived from 1,4-butanediol, 35.9 mol% of a carbonate structure derived from 1,6-hexanediol, 28.5 mol% of an ester structure derived from adipic acid, and a carbonate group content of 26.6 mass %.

[0323] [Example 56]

[0324] [Polymerization Example 25 of Polyester Polycarbonate Polyol]

[0325] 221 g (2.51 mol) of ethylene carbonate, 148 g (1.64 mol) of 1,4-butanediol, 195 g (1.65 mol) of 1,6-hexanediol, and 122 g (0.84 mol) of adipic acid were added to a 2 L glass flask equipped with a distillation column filled with regular packing and a stirring device. 0.50 g of magnesium di-n-butoxide was added as a catalyst, the reaction temperature was set to 150-170°C, and the pressure was reduced from 10 kPa to 3 kPa while the generated mixture of water, ethylene glycol and ethylene carbonate was distilled off, and the reaction was carried out for 24 hours.

[0326] Thereafter, the reaction was switched to single distillation and the reaction was carried out at 170° C. for 20 hours while the pressure was gradually reduced to 0.1 kPa, thereby distilling off the monomer.

[0327] The obtained polyester polycarbonate polyol has the appearance of a viscous liquid, a hydroxyl value of 59.2 mgKOH / g, and a copolymerization ratio of 36.6 mol% of the carbonate structure derived from 1,4-butanediol, 34.1 mol% of the carbonate structure derived from 1,6-hexanediol, and 29.3 mol% of the ester structure derived from adipic acid, and a carbonate group content of 26.3 mass %.

[0328] [Comparative Example 20]

[0329] [Polymerization Example 26 of Polyester Polycarbonate Polyol]

[0330] A polyester polycarbonate polyol was synthesized in the same manner as in Example 3 except that 0.06 g of magnesium acetate tetrahydrate was added as a catalyst instead of titanium tetra-n-butoxide. The reaction was carried out at a reaction temperature of 150 to 170° C. and a pressure of 3 kPa, but no distillate was generated and the reaction was terminated without any reaction.

[0331] Industrial Applicability

[0332] The polyurethane obtained by using the polyester polycarbonate polyol of the present invention has excellent balance in flexibility, chemical resistance, low-temperature characteristics, heat resistance, adhesiveness, abrasion resistance, and touch, and therefore can be particularly suitably used for synthetic leather applications.

[0333] Furthermore, the polyester polycarbonate polyol of the present embodiment can also be used for lamination welding adhesives for various films, surface protective agents, and the like.

Claims

1. A polyester polycarbonate polyol having a repeating unit represented by the following formula (1) and a repeating unit represented by the following formula (2), The molecular ends of the polyester polycarbonate polyol are hydroxyl groups, the hydroxyl value is 37 to 86 mgKOH / g, and the carbonate group content is 15 to 40% by mass. In formula (1), R1 is a divalent straight-chain aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms; In formula (2), R2 is a divalent hydrocarbon having 2 to 15 carbon atoms, R3 is a divalent straight-chain aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms, The molar ratio of the structural unit represented by formula (1) to the structural unit represented by formula (2) is 60 / 40 to 90 / 10.

2. The polyester polycarbonate polyol according to claim 1, wherein The hydroxyl value is 45 to 75 mgKOH / g.

3. The polyester polycarbonate polyol according to claim 1, wherein The hydroxyl value is 50 to 65 mgKOH / g. 4 . The polyester polycarbonate polyol according to claim 1 , which has a melt viscosity at 50° C. of 1000 to 9000 mPa·s. 5 . The polyester polycarbonate polyol according to claim 1 , which has a melt viscosity at 50° C. of 1500 to 8500 mPa·s. 6 . The polyester polycarbonate polyol according to claim 1 , which has a melt viscosity at 50° C. of 2000 to 7000 mPa·s.

7. The polyester polycarbonate polyol according to claim 1, wherein The carbonate group content is 21 to 40% by mass.

8. The polyester polycarbonate polyol according to claim 1, wherein The carbonate group content is 25 to 35% by mass.

9. The polyester polycarbonate polyol according to claim 1, wherein The carbonate group content is 25 to 30% by mass.

10. The polyester polycarbonate polyol according to claim 1, wherein The molar ratio of the structural unit represented by formula (1) to the structural unit represented by formula (2) is 70 / 30 to 80 / 20.

11. The polyester polycarbonate polyol according to any one of claims 1 to 10, wherein 50 mol% or more of the repeating units represented by formula (1) contain at least two repeating units selected from the group consisting of formula (3), formula (4) and formula (5), 12. The polyester polycarbonate polyol according to claim 11, wherein 70 mol% or more of the repeating units represented by formula (1) contain at least two repeating units selected from the group consisting of formula (3), formula (4) and formula (5).

13. The polyester polycarbonate polyol according to claim 11, wherein 80 mol% or more of the repeating units represented by formula (1) contain at least two repeating units selected from the group consisting of formula (3), formula (4) and formula (5).

14. The polyester polycarbonate polyol according to claim 11, wherein 50 mol% or more of the repeating units represented by formula (1) include two repeating units selected from the group consisting of formula (3), formula (4) and formula (5), and the ratio of the two repeating units is 90:10 to 10:90 in terms of molar ratio.

15. The polyester polycarbonate polyol according to claim 11, wherein 50 mol% or more of the repeating units represented by formula (1) contain two repeating units selected from the group consisting of formula (3), formula (4) and formula (5), and the ratio of the two repeating units is 70:30 to 30:70 in terms of molar ratio.

16. The polyester polycarbonate polyol according to claim 11, wherein 50 mol% or more of the repeating units represented by formula (1) contain repeating units of formula (4) and formula (5).

17. The polyester polycarbonate polyol according to claim 11, wherein 50 mol% or more of the repeating units represented by formula (1) include repeating units of formula (3) and formula (5), and the carbonate group content is 21 to 40 mass%. 18 . Synthetic leather produced using the polyester polycarbonate polyol according to claim 1 .

19. A method for producing polyester polycarbonate polyol, characterized in that: This is a method for producing the polyester polycarbonate polyol according to any one of claims 1 to 10, using a metal alkoxide as a catalyst.

20. The method for producing a polyester polycarbonate polyol according to claim 19, wherein Metal alkoxides are alkoxides of metals of Group 4 of the Periodic Table.

Citation Information

Patent Citations

  • Porous sheet material and method for producing the same

    JP2003119314A

  • Polyurethane resin and surface film layer of synthetic leather obtained using the same

    JP2004346094A

  • Surface layer material-forming composition for fiber laminate, synthetic / artificial leather using the same, and method for producing synthetic / artificial leather

    JP2009185260A

  • Synthetic leather

    JP2013108196A

  • Urethane prepolymer composition, two liquid-type coating agent and synthetic imitation leather using the same

    JP2014105250A