Ion exchange membrane with catalyst layer, ion exchange membrane and electrolytic hydrogenation device

By using an ion exchange membrane with a catalyst layer in an aromatic compound electrolytic hydrogenation device, using a fluoropolymer layer with low ion exchange capacity and a hierarchical configuration with high ion exchange capacity, the high electrolysis voltage and low current efficiency in electrolytic hydrogenation are solved. problem, achieving an improvement in electrolytic hydrogenation efficiency.

CN115066515BActive Publication Date: 2024-10-18AGC INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202180012939.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-02-04
Publication Date
2024-10-18
Estimated Expiration
2041-02-04

AI Technical Summary

Technical Problem

During the electrolytic hydrogenation process of existing aromatic compound electrolytic hydrogenation devices, the electrolysis voltage is high and the current efficiency is low, making it difficult to meet the demand for improving production efficiency.

Method used

An ion exchange membrane with a catalyst layer is used, which is composed of an inorganic particle layer, a fluoropolymer layer with a sulfonic acid functional group, and a catalyst layer, and the ion exchange capacity of the first fluoropolymer is lower than that of the second fluoropolymer. It is an electrolytic hydrogenation device with an inorganic particle layer on the anode side and a catalyst layer on the cathode side.

Benefits of technology

It effectively reduces the electrolysis voltage and improves the current efficiency. By optimizing the membrane structure and hierarchical configuration, it inhibits the swelling of moisture and aromatic compounds, reducing the problems of rising electrolysis voltage and reducing current efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003783304770000131
    Figure BDA0003783304770000131
  • Figure BDA0003783304770000141
    Figure BDA0003783304770000141
  • Figure BDA0003783304770000151
    Figure BDA0003783304770000151
Patent Text Reader

Abstract

An ion exchange membrane with a catalyst layer, an ion exchange membrane, and an electrolytic hydrogenation device are provided, which can reduce the electrolysis voltage and improve the current efficiency during the electrolytic hydrogenation of aromatic compounds. The ion exchange membrane with a catalyst layer of the present invention sequentially comprises: an inorganic particle layer, which contains inorganic particles and a binder; a layer (Sa), which contains a first fluoropolymer having a sulfonic acid functional group; a layer (Sb), which contains a second fluoropolymer having a sulfonic acid functional group; and a catalyst layer, wherein the ion exchange capacity of the first fluoropolymer is lower than the ion exchange capacity of the second fluoropolymer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an ion exchange membrane with a catalyst layer, an ion exchange membrane and an electrolytic hydrogenation device. Background Art

[0002] As a method for producing a hydrogenated organic substance (for example, cyclohexane, methylcyclohexane, decalin, etc.), there is known a method of adding hydrogen to an aromatic compound (for example, benzene, toluene, naphthalene, etc.) using a hydrogenation reactor.

[0003] In recent years, electrolytic hydrogenation of aromatic compounds has been studied instead of the above methods because the production of hydrogenated organic matter can be simplified. The electrolytic hydrogenation of aromatic compounds is carried out using, for example, an electrolytic hydrogenation device having a structure in which a cathode and an anode are separated by an ion exchange membrane.

[0004] In Patent Document 1, as an ion exchange membrane in an electrolytic hydrogenation device, a cathode catalyst layer-electrolyte membrane assembly is disclosed, which comprises: an electrolyte membrane (product name "NRE-212CS", manufactured by DuPont, a membrane composed of a fluorinated polymer having a sulfonic acid group), a zirconium oxide layer disposed on the surface of the anode side of the electrolyte membrane, and a catalyst layer disposed on the surface of the cathode side of the electrolyte membrane.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent No. 6400410 Summary of the invention

[0008] Problem that the invention aims to solve

[0009] In recent years, in the electrolytic hydrogenation of aromatic compounds using an electrolytic hydrogenation device, there has been a demand for a further reduction in electrolysis voltage and a further improvement in current efficiency in order to further improve the production efficiency of hydrogenated organic matter.

[0010] The present inventors referred to Patent Document 1 and applied an ion exchange membrane with a catalyst layer, which sequentially comprises an inorganic particle layer, a layer comprising a fluorinated polymer having a sulfonic acid functional group, and a catalyst layer, to an electrolytic hydrogenation apparatus. As a result, it was found that there was room for improvement in at least one of the electrolysis voltage and the current efficiency during the electrolytic hydrogenation of aromatic compounds.

[0011] The present invention has been made in view of the above-mentioned actual situation, and an object of the present invention is to provide an ion exchange membrane with a catalyst layer, an ion exchange membrane, and an electrolytic hydrogenation device which can reduce the electrolysis voltage and improve the current efficiency during the electrolytic hydrogenation of aromatic compounds.

[0012] Solutions for solving problems

[0013] The present inventors have conducted in-depth research on the above-mentioned subject and found that, in the case of an ion exchange membrane with a catalyst layer which sequentially comprises an inorganic particle layer, a layer (Sa) comprising a first fluoropolymer, a layer (Sb) comprising a second fluoropolymer, and a catalyst layer, and the ion exchange capacity of the first fluoropolymer is lower than the ion exchange capacity of the second fluoropolymer, if an electrolytic hydrogenation device is used in which the inorganic particle layer of the ion exchange membrane with the catalyst layer is arranged on the anode side and the catalyst layer of the ion exchange membrane with the catalyst layer is arranged on the cathode side, the desired effect can be obtained, thereby completing the present invention.

[0014] That is, the inventors have found that the above-mentioned problems can be solved by the following configuration.

[0015] [1] An ion exchange membrane with a catalyst layer, which comprises:

[0016] an inorganic particle layer comprising inorganic particles and a binder;

[0017] A layer (Sa) comprising a first fluorinated polymer having a sulfonic acid type functional group;

[0018] a layer (Sb) comprising a second fluorine-containing polymer having a sulfonic acid type functional group; and

[0019] Catalyst layer,

[0020] The ion exchange capacity of the first fluorinated polymer is lower than the ion exchange capacity of the second fluorinated polymer.

[0021] [2] The ion exchange membrane with a catalyst layer according to [1], wherein the interface of the layer (Sa) on the inorganic particle layer side has a concavo-convex structure.

[0022] [3] The ion exchange membrane with a catalyst layer according to [1] or [2], further comprising a reinforcing material including reinforcing fibers.

[0023] [4] The ion exchange membrane with a catalyst layer according to any one of [1] to [3], wherein the ion exchange capacity of the first fluorinated polymer is 0.5 to 1.1 milliequivalents / g of dry resin.

[0024] [5] The ion exchange membrane with a catalyst layer according to any one of [1] to [4], wherein the ion exchange capacity of the second fluorinated polymer is 0.7 to 2.0 milliequivalents / g of dry resin.

[0025] [6] The ion exchange membrane with a catalyst layer according to any one of [1] to [5], wherein the first fluorinated polymer having a sulfonic acid functional group comprises a unit based on a fluorinated olefin and a unit having a sulfonic acid functional group and a fluorine atom.

[0026] [7] The ion exchange membrane with a catalyst layer according to [6], wherein the fluorine-containing olefin is tetrafluoroethylene, chlorotrifluoroethylene, vinylidene fluoride, vinyl fluoride or hexafluoropropylene.

[0027] [8] The ion exchange membrane with a catalyst layer according to [6] or [7], wherein the unit having a sulfonic acid type functional group and a fluorine atom is a unit represented by formula (1).

[0028] Formula (1) -[CF2-CF(-L-(SO3M) n )]-

[0029] In the formula, L is an n+1-valent perfluorocarbon group which may contain an ethereal oxygen atom, M is a hydrogen atom, an alkali metal or a quaternary ammonium cation, and n is 1 or 2.

[0030] [9] An ion exchange membrane comprising:

[0031] an inorganic particle layer comprising inorganic particles and a binder;

[0032] a layer (Sa) comprising a first fluorinated polymer having a sulfonic acid type functional group; and

[0033] a layer (Sb) comprising a second fluorinated polymer having a sulfonic acid type functional group,

[0034] The ion exchange capacity of the first fluorinated polymer is lower than the ion exchange capacity of the second fluorinated polymer.

[0035]

[10] The ion exchange membrane according to [9], wherein the interface of the layer (Sa) on the inorganic particle layer side has a concavo-convex structure.

[0036]

[11] The ion exchange membrane according to [9] or

[10] , further comprising a reinforcing material comprising reinforcing filaments.

[0037]

[12] The ion exchange membrane according to any one of [9] to

[11] , wherein the ion exchange capacity of the first fluorinated polymer is 0.5 to 1.1 milliequivalents / g of dry resin.

[0038]

[13] The ion exchange membrane according to any one of [9] to

[12] , wherein the ion exchange capacity of the second fluorinated polymer is 0.7 to 2.0 milliequivalents / g dry resin.

[0039]

[14] A method for producing an ion exchange membrane with a catalyst layer, which is the method for producing an ion exchange membrane with a catalyst layer according to any one of [1] to [8], wherein:

[0040] The ion exchange membrane described in [9] is obtained, and a catalyst layer is provided on the above-mentioned layer (Sb).

[0041]

[15] An electrolytic hydrogenation device comprising: an electrolytic cell having an anode and a cathode; and an ion exchange membrane having a catalyst layer according to any one of [1] to [8],

[0042] The ion exchange membrane with the catalyst layer is arranged in the electrolytic cell so as to separate the anode and the cathode.

[0043] The inorganic particle layer of the ion exchange membrane with a catalyst layer is arranged on the anode side, and the catalyst layer of the ion exchange membrane with a catalyst layer is arranged on the cathode side.

[0044]

[16] The electrolytic hydrogenation device according to

[15] , wherein an aqueous electrolyte solution is supplied to an anode chamber in which the anode is arranged, and an aromatic compound is supplied to a cathode chamber in which the cathode is arranged.

[0045] Effects of the Invention

[0046] According to the present invention, an ion exchange membrane with a catalyst layer, an ion exchange membrane, and an electrolytic hydrogenation apparatus can be provided, which can reduce the electrolysis voltage and improve the current efficiency during the electrolytic hydrogenation of aromatic compounds. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 It is a schematic cross-sectional view showing an example of the ion exchange membrane with a catalyst layer of the present invention.

[0048] Figure 2 This is a partially enlarged schematic cross-sectional view showing an example of the ion exchange membrane with a catalyst layer of the present invention.

[0049] Figure 3 It is a schematic cross-sectional view showing an example of the ion exchange membrane of the present invention.

[0050] Figure 4 This is a schematic diagram showing an example of the electrolytic hydrogenation device of the present invention. DETAILED DESCRIPTION

[0051] The following definitions of terms apply throughout this specification and claims.

[0052] An "ion exchange membrane" is a membrane comprising a polymer having ion exchange groups.

[0053] The "ion exchange group" is a group that can convert at least a part of the ions contained in the group into other ions, and examples thereof include the carboxylic acid type functional group and the sulfonic acid type functional group described below.

[0054] "Carboxylic acid-type functional group" refers to a carboxylic acid group (-COOH) or a carboxylate group (-COOM 1 Among them, M 1 is an alkali metal or quaternary ammonium salt base. ).

[0055] "Sulfonic acid functional group" refers to a sulfonic acid group (-SO3H) or a sulfonate group (-SO3M 2 Among them, M 2 is an alkali metal or quaternary ammonium salt base. ).

[0056] A "precursor layer" is a layer (membrane) comprising a polymer having groups that can be converted into ion exchange groups.

[0057] The "group convertible into an ion exchange group" means a group convertible into an ion exchange group by a known treatment such as a hydrolysis treatment or an acidification treatment.

[0058] The "group convertible into a sulfonic acid type functional group" refers to a group convertible into a sulfonic acid type functional group by a known treatment such as a hydrolysis treatment or an acidification treatment.

[0059] The "fluorine-containing polymer" refers to a high molecular weight compound having fluorine atoms in the molecule.

[0060] “Perfluorocarbon polymer” refers to a polymer in which all hydrogen atoms bonded to carbon atoms in the polymer are replaced by fluorine atoms. A portion of the fluorine atoms in the perfluorocarbon polymer may be replaced by one or both of chlorine atoms and bromine atoms.

[0061] The term "monomer" refers to a compound having a polymerizable carbon-carbon unsaturated double bond.

[0062] The "fluorine-containing monomer" refers to a monomer having a fluorine atom in the molecule.

[0063] "Structural unit" refers to a part derived from a monomer that exists in a polymer and constitutes the polymer. For example, when a structural unit is produced by addition polymerization of a monomer having a carbon-carbon unsaturated double bond, the structural unit derived from the monomer is a divalent structural unit produced by the rupture of the unsaturated double bond. In addition, the structural unit can be a structural unit obtained by chemically converting the structural unit, such as hydrolyzing the structural unit, after forming a polymer having a structure of a certain structural unit. It should be noted that, hereinafter, depending on the circumstances, the structural unit derived from each monomer is sometimes recorded by adding the name of "unit" to the monomer name.

[0064] The "reinforcement material" refers to a material for improving the strength of the ion exchange membrane. The reinforcement material is a material derived from a reinforcing cloth.

[0065] The “reinforcement cloth” refers to a cloth used as a raw material of a reinforcing material for improving the strength of an ion exchange membrane.

[0066] The “reinforcement yarn” is a yarn constituting the reinforcing cloth, and is made of a material that does not dissolve even when the reinforcing cloth is immersed in an alkaline aqueous solution (for example, a sodium hydroxide aqueous solution having a concentration of 32% by mass).

[0067] The “sacrificial yarn” is a yarn constituting the reinforcing cloth and is a yarn containing a material that is eluted by the alkaline aqueous solution and / or the process liquid (for example, the electrolyte solution or the aromatic compound used in the electrolytic hydrogenation of the aromatic compound).

[0068] The "dissolution pores" are pores formed as a result of the sacrificial silk being dissolved in an alkaline aqueous solution.

[0069] The "reinforced precursor film" refers to a film in which a reinforcing cloth is arranged in a precursor layer.

[0070] The numerical range expressed with "to" means a range including the numerical values ​​described before and after "to" as the lower limit and the upper limit.

[0071] The thickness of each layer of the ion exchange membrane with a catalyst layer when dried was obtained by observing the cross section of the ion exchange membrane with a catalyst layer using an optical microscope after drying the ion exchange membrane with a catalyst layer at 90° C. for 2 hours, and using image software. It should be noted that when there are concave and convex portions on the surface of the layer, the thickness of the concave portion at 10 points in the layer and the thickness of the convex portion at 10 points in the layer were measured, and the arithmetic mean of the thickness of the total 20 points was taken as the thickness of the layer.

[0072] "TQ value" is a value related to the molecular weight of the polymer, indicating the capacity flow rate: 100mm 3 The volume flow rate is: the polymer is melted and flows out from a throttle hole (diameter: 1mm, length: 1mm) at a certain temperature under a pressure of 3MPa. 3 The unit of / second represents the value of the amount of polymer flowing out. The higher the TQ value, the higher the molecular weight.

[0073] The "ion exchange capacity" is a value calculated as follows. First, the fluoropolymer is placed in a glove box with dry nitrogen flowing for 24 hours, and the dry mass of the fluoropolymer is measured. Thereafter, the fluoropolymer is immersed in a 2 mol / L sodium chloride aqueous solution at 60°C for 1 hour. The fluoropolymer is washed with ultrapure water and taken out, and the liquid immersed in the fluoropolymer is titrated with a 0.1 mol / L sodium hydroxide aqueous solution to determine the ion exchange capacity of the fluoropolymer.

[0074] [Ion exchange membrane with catalyst layer]

[0075] The ion exchange membrane with a catalyst layer of the present invention comprises, in sequence: an inorganic particle layer, which contains inorganic particles and a binder; a layer (Sa), which contains a first fluorinated polymer having a sulfonic acid functional group (hereinafter also referred to as "fluorinated polymer (S1)"); a layer (Sb), which contains a second fluorinated polymer having a sulfonic acid functional group (hereinafter also referred to as "fluorinated polymer (S2)"); and a catalyst layer.

[0076] Furthermore, the ion exchange capacity of the fluorinated polymer (S1) is lower than the ion exchange capacity of the fluorinated polymer (S2).

[0077] The ion exchange membrane with a catalyst layer of the present invention is preferably used for electrolytic hydrogenation of aromatic compounds. When the ion exchange membrane with a catalyst layer of the present invention is applied to an electrolytic hydrogenation device, if the inorganic particle layer is arranged on the anode side and the catalyst layer is arranged on the cathode side, the electrolytic voltage can be reduced during the electrolytic hydrogenation of aromatic compounds, and the current efficiency can be improved.

[0078] The details of the reason are not clear, but it is presumed to be due to the following reasons.

[0079] In the electrolytic hydrogenation device, an ion exchange membrane with a catalyst layer is arranged in an electrolytic cell in a manner that separates an anode chamber in which an anode is arranged and a cathode chamber in which a cathode is arranged, and an aqueous electrolyte solution is supplied to the anode chamber, and an aromatic compound is supplied to the cathode chamber. It is believed that when such an electrolytic hydrogenation device is driven, protons (H + ) moves to the cathode side via the ion exchange membrane with the catalyst layer, thereby causing hydrogenation of the aromatic compound based on proton addition near the surface of the catalyst layer.

[0080] Here, the hydrogenation reaction of the aromatic compound on the cathode side occurs on the catalyst layer. Specifically, it is considered that hydrogen activated on the catalyst included in the catalyst layer contacts the aromatic compound, electrons flow therein, and hydrogenation of the aromatic compound occurs.

[0081] However, when moisture exists around the catalyst, aromatic compounds are less likely to approach the reaction field around the catalyst. As a result, activated hydrogen reacts with electrons to generate hydrogen in the cathode chamber, which causes a problem of reduced current efficiency.

[0082] On the other hand, an electrolyte membrane with a low ion exchange capacity is less likely to allow water to pass through than an electrolyte membrane with a high ion exchange capacity, and can improve current efficiency, but will increase the electrolysis voltage.

[0083] In addition, an electrolyte membrane having a high ion exchange capacity allows water to pass more easily than an electrolyte membrane having a low ion exchange capacity, thereby reducing current efficiency, but can reduce the electrolysis voltage.

[0084] The inventors of the present invention considered the above matters and found that when the electrolyte membrane is a multilayer structure, the layer (Sa) containing the fluorinated polymer (S1) with low ion exchange capacity is arranged on the anode side, and the layer (Sb) containing the fluorinated polymer (S2) with high ion exchange capacity is arranged on the cathode side, the movement of water from the anode chamber to the cathode chamber can be suppressed, and the current efficiency can be improved. In addition, it was found that by using such an electrolyte membrane, electrolysis at a low voltage can be achieved.

[0085] Here, in the electrolytic hydrogenation of aromatic compounds using an electrolytic hydrogenation device, an aqueous electrolyte solution is supplied to the anode chamber and an aromatic compound is supplied to the cathode chamber. In this case, when an ion exchange membrane with a catalyst layer having a single-layer electrolyte membrane is used, the surface of the electrolyte membrane on the anode chamber side is in contact with the aqueous electrolyte solution, and the surface of the electrolyte membrane on the cathode chamber side is in contact with the aromatic compound. In this way, due to the difference in the degree of swelling between the relative surfaces of the ion exchange membrane with the catalyst layer, wrinkles may sometimes be generated in the ion exchange membrane with the catalyst layer. As a result, an increase in electrolysis voltage and a decrease in current efficiency may sometimes be caused.

[0086] In view of this problem, the present inventors have found that if the layer (Sa) containing the fluorinated polymer (S1) is arranged on the anode side and the layer (Sb) containing the fluorinated polymer (S2) is arranged on the cathode side, the generation of wrinkles in the ion exchange membrane with the catalyst layer can be suppressed. This is presumably due to the following reasons.

[0087] The fluorinated polymer (S1) has a lower ion exchange capacity than the fluorinated polymer (S2), and is therefore less susceptible to swelling due to water. On the other hand, since the fluorinated polymer (S2) has a higher ion exchange capacity than the fluorinated polymer (S1), it is less susceptible to swelling due to an organic solvent (aromatic compound). Therefore, it is believed that the degree of swelling of the fluorinated polymer (S1) due to water and the degree of swelling of the fluorinated polymer (S2) due to aromatic compounds are balanced, and the generation of wrinkles on the surface of the ion exchange membrane with the catalyst layer can be suppressed.

[0088] The following is based on Figure 1 The ion exchange membrane with a catalyst layer of the present invention will be described, but the present invention is not limited to Figure 1 content.

[0089] Figure 1 FIG. 2 is a schematic cross-sectional view showing an example of an ion exchange membrane with a catalyst layer according to the present invention. Figure 1As shown, the ion exchange membrane 1 with a catalyst layer comprises: an electrolyte 12 formed by a layer 12A as a layer (Sa) and a layer 12B as a layer (Sb), an inorganic particle layer 14 arranged on the surface of the layer 12A, and a catalyst layer 16 arranged on the surface of the layer 12B, and a reinforcing material 20 is arranged in the electrolyte membrane 12.

[0090] <Layer(Sa)>

[0091] The layer 12A as the layer (Sa) may be a layer containing the fluorinated polymer (S1), and is preferably a layer consisting only of the fluorinated polymer (S1) without containing any material other than the fluorinated polymer (S1). That is, the layer (Sa) is preferably a layer consisting of the fluorinated polymer (S1).

[0092] When the ion exchange membrane 1 with a catalyst layer is applied to an electrolytic hydrogenation device described later, the layer 12A is arranged on the anode side relative to the layer 12B.

[0093] The thickness of the layer 12A when dried is preferably 5 to 60 μm, more preferably 10 to 40 μm, and particularly preferably 10 to 30 μm. If the thickness of the layer 12A when dried is above the lower limit, the mechanical strength of the ion exchange membrane 1 with the catalyst layer is improved, and the current efficiency is more excellent. If the thickness of the layer 12A when dried is below the upper limit, the resistance of the ion exchange membrane 1 with the catalyst layer can be suppressed to be relatively low.

[0094] like Figure 1 As shown, the layer 12A preferably has a concavo-convex structure at the interface on the inorganic particle layer 14 side. When the interface on the inorganic particle layer 14 side has a concavo-convex structure, the electrolyte aqueous solution is easily supplied to the anode and the anode side of the ion exchange membrane 1 with the catalyst layer (i.e., the inorganic particle layer 14 side of the layer 12A), and the electrolyte aqueous solution easily passes through. Thus, the reduction of the effective electrolysis area can be suppressed, and thus the increase of the electrolysis voltage can be suppressed.

[0095] In the present invention, the concave-convex structure at the interface on the inorganic particle layer side of layer (Sa) refers to a structure having multiple protrusions from layer (Sb) toward the inorganic particle layer in the in-plane direction (hereinafter also referred to as "convexities"), and the shortest distance from the top of the convexity to the lowest position of the convexity (hereinafter also referred to as "the height of the convexity") is greater than 2μm.

[0096] Figure 2 This is a partially enlarged view of a cross section of the ion exchange membrane with a catalyst layer of the present invention. Figure 2In the example, layer 12A has a plurality of continuously formed convex portions B at the interface on the inorganic particle layer 14 side. The height of convex portion B corresponds to the shortest distance D1 from position P1 corresponding to the vertex of convex portion B (convex portion B2) to the lowest position P2 of convex portion B (convex portion B2).

[0097] The height of the convex portion is measured as follows.

[0098] First, the ion exchange membrane with the catalyst layer is cut along the thickness direction, and an enlarged image (e.g., 100 times) of the cross section of the ion exchange membrane with the catalyst layer is taken using an optical microscope (product name "BX-51", manufactured by Olympus Corporation). Next, based on the taken enlarged image, the height ( Figure 2 The shortest distance D1).

[0099] The height of the convex portion is 2 μm or more, preferably 2 to 80 μm, and particularly preferably 10 to 50 μm from the viewpoint of better current efficiency.

[0100] The convex portions are preferably formed continuously in the in-plane direction of the layer (Sa), and are preferably formed at a periodic pitch.

[0101] When the surface of the inorganic particle layer side of layer (Sa) has a concavoconvex structure, the average distance between the apexes of the convex parts is preferably 20 to 500 μm, more preferably 50 to 400 μm, and particularly preferably 100 to 300 μm from the viewpoint of further improving the current efficiency.

[0102] In the present invention, the average distance between vertices of the convex portions is the shortest distance between vertices of adjacent convex portions, and refers to the arithmetic mean value between vertices at 10 different points.

[0103] Figure 2 In the example, the shortest distance between the vertices of adjacent convex portions corresponds to the shortest distance D2 from the position T1 corresponding to the vertex of convex portion B1 to the position T2 corresponding to the vertex of convex portion B2 adjacent to convex portion B1.

[0104] The shortest distance between the vertices of adjacent convex portions is measured using the enlarged image described in the measurement of the height of the convex portion described above.

[0105] Specific examples of methods for forming a concave-convex structure at the interface on the inorganic particle layer side of layer (Sa) include: a method of sandblasting the layer (Sa); a method of hot pressing the layer (Sa) and a film or metal mold having a concave-convex structure; a method of hot pressing the layer (Sa) and solid particles and then removing the particles; a method of using a film or metal mold having a concave-convex structure when forming the layer (Sa); and a method of forming the layer (Sa) on a film having a concave-convex structure.

[0106] Alternatively, a method of laminating the layer (Sa), the reinforcing material, and the layer (Sb) in sequence and performing vacuum suction may be used, thereby forming a concavo-convex structure on the surface of the layer (Sa) corresponding to the surface shape of the reinforcing material.

[0107] The method of using a thin film having a concavo-convex structure when forming the layer (Sa) is relatively simple and has little impurity mixing due to treatment, so a film with stable performance can be obtained, which is preferred.

[0108] From the viewpoint of moldability and chemical resistance, the film having a concavo-convex structure is preferably made of polyethylene or polypropylene.

[0109] It should be noted that Figure 1 In the example shown, the interface of the layer 12A on the inorganic particle layer 14 side has a concavo-convex structure, but the invention is not limited thereto, and the interface of the layer 12A on the inorganic particle layer 14 side may not have a concavo-convex structure.

[0110] (Fluoropolymer (S1))

[0111] The layer (Sa) may contain one kind of the fluorinated polymer (S1) alone, or may contain two or more kinds of the fluorinated polymers (S1).

[0112] Layer (Sa) may contain polymers other than fluoropolymer (S1) (hereinafter also referred to as other polymers), preferably substantially composed of fluoropolymer (S1). Substantially composed of fluoropolymer (S1) means that the content of fluoropolymer (S1) is 90% by mass or more relative to the total mass of the polymer in layer (Sa). The upper limit of the content of fluoropolymer (S1) is 100% by mass relative to the total mass of the polymer in layer (Sa).

[0113] Specific examples of other polymers include one or more polyazole compounds selected from the group consisting of polymers of heterocyclic compounds containing one or more nitrogen atoms in the ring and polymers of heterocyclic compounds containing one or more nitrogen atoms in the ring and containing oxygen atoms and / or sulfur atoms.

[0114] Specific examples of the polyazole compound include polyimidazole compounds, polybenzimidazole compounds, polybenzbisimidazole compounds, polybenzoxazole compounds, polyoxazole compounds, polythiazole compounds, and polybenzothiazole compounds.

[0115] In addition, from the viewpoint of oxidation resistance of the ion exchange membrane with a catalyst layer, other polymers include polyphenylene sulfide resin and polyphenylene ether resin.

[0116] The fluorinated polymer (S1) preferably comprises a unit based on a fluorinated olefin and a unit having a sulfonic acid type functional group and a fluorine atom.

[0117] As the fluorinated olefin, for example, there can be mentioned fluorinated olefins having one or more fluorine atoms in the molecule and having 2 to 3 carbon atoms. Specific examples of fluorinated olefins include tetrafluoroethylene (hereinafter also referred to as "TFE"), chlorotrifluoroethylene, vinylidene fluoride, vinyl fluoride, and hexafluoropropylene. Among them, TFE is preferred from the perspectives of the production cost of the monomer, the reactivity with other monomers, and the excellent properties of the obtained fluorinated polymer (S1).

[0118] The fluorinated olefins may be used alone or in combination of two or more.

[0119] As the unit having a sulfonic acid type functional group and a fluorine atom, a unit represented by formula (1) is preferred.

[0120] Formula (1) -[CF2-CF(-L-(SO3M) n )]-

[0121] In the formula (1), L is an n+1-valent perfluorocarbon group which may contain an etheric oxygen atom.

[0122] The etheric oxygen atom may be located at the terminal of the perfluorocarbon group or between carbon atoms.

[0123] The number of carbon atoms in the n+1-valent perfluorocarbon group is preferably 1 or more, particularly preferably 2 or more, and is preferably 20 or less, particularly preferably 10 or less.

[0124] L is an n+1-valent perfluoroaliphatic hydrocarbon group optionally containing an etheric oxygen atom, and particularly preferably n=1, i.e. a divalent perfluoroalkylene group optionally containing an etheric oxygen atom, or n=2, i.e. a trivalent perfluoroaliphatic hydrocarbon group optionally containing an etheric oxygen atom.

[0125] The divalent perfluoroalkylene group may be linear or branched.

[0126] M is a hydrogen atom, an alkali metal or a quaternary ammonium cation.

[0127] n is 1 or 2.

[0128] The unit represented by formula (1) is preferably a unit represented by formula (1-1), a unit represented by formula (1-2), a unit represented by formula (1-3), or a unit represented by formula (1-4).

[0129] Formula (1-1) -[CF2-CF(-OR f1 -SO3M)]-

[0130] Formula (1-2) -[CF2-CF(-R f1 -SO3M)]-

[0131]

[0132] R f1 The perfluoroalkylene group is a perfluoroalkylene group which may contain an oxygen atom between carbon atoms. The number of carbon atoms in the perfluoroalkylene group is preferably 1 or more, particularly preferably 2 or more, and is preferably 20 or less, particularly preferably 10 or less.

[0133] R f2 The perfluoroalkylene group is a single bond or may contain an oxygen atom between carbon atoms. The number of carbon atoms in the perfluoroalkylene group is preferably 1 or more, particularly preferably 2 or more, and is preferably 20 or less, particularly preferably 10 or less.

[0134] R f3 The perfluoroalkylene group is a single bond or may contain an oxygen atom between carbon atoms. The number of carbon atoms in the perfluoroalkylene group is preferably 1 or more, particularly preferably 2 or more, and is preferably 20 or less, particularly preferably 10 or less.

[0135] r is 0 or 1.

[0136] m is 0 or 1.

[0137] M is a hydrogen atom, an alkali metal or a quaternary ammonium cation.

[0138] As the unit represented by the formula (1-1) and the unit represented by the formula (1-2), the unit represented by the formula (1-5) is more preferable.

[0139] Formula (1-5) -[CF2-CF(-(CF2) x -(OCF2CFY) y -O-(CF2) z -SO3M)]-

[0140] x is 0 or 1, y is an integer of 0 to 2, z is an integer of 1 to 4, Y is F or CF3, and M is as described above.

[0141] Specific examples of the unit represented by formula (1-1) include the following units: w in the formula is an integer of 1 to 8, and x is an integer of 1 to 5. M in the formula has the same meaning as described above.

[0142] -[CF2-CF(-O-(CF2) w -SO3M)]-

[0143] -[CF2-CF(-O-CF2CF(CF3)-O-(CF2) w -SO3M)]-

[0144] -[CF2-CF(-(O-CF2CF(CF3)) x -SO3M)]-

[0145] Specific examples of the unit represented by formula (1-2) include the following units: w in the formula is an integer of 1 to 8. M in the formula has the same meaning as described above.

[0146] -[CF2-CF(-(CF2) w -SO3M)]-

[0147] -[CF2-CF(-CF2-O-(CF2) w -SO3M)]-

[0148] As the unit represented by the formula (1-3), the unit represented by the formula (1-3-1) is preferred. M in the formula has the same meaning as described above.

[0149]

[0150] R f4 is a linear perfluoroalkylene group having 1 to 6 carbon atoms, R f5 It is a single bond or a linear perfluoroalkylene group having 1 to 6 carbon atoms which may contain an oxygen atom between carbon atoms. r and M are as defined above.

[0151] Specific examples of the unit represented by formula (1-3-1) include the following.

[0152]

[0153] As the unit represented by formula (1-4), the unit represented by formula (1-4-1) is preferred. f1 , R f2 and M are defined as above.

[0154]

[0155] Specific examples of the unit represented by formula (1-4-1) include the following.

[0156]

[0157] The unit having a sulfonic acid type functional group and a fluorine atom may be used alone or in combination of two or more.

[0158] The fluorinated polymer (S1) may contain units based on a fluorinated olefin and units based on a monomer other than the unit having a sulfonic acid type functional group and a fluorine atom (hereinafter also referred to as other monomer).

[0159] Specific examples of other monomers include CF2=CFR f6 (Among them, R f6 It is a perfluoroalkyl group having 2 to 10 carbon atoms. )CF2=CF-OR f7 (Among them, Rf7 It is a perfluoroalkyl group having 1 to 10 carbon atoms. )CF2=CFO(CF2) v CF=CF2 (wherein v is an integer from 1 to 3).

[0160] From the viewpoint of maintaining the ion exchange performance, the content of the units based on other monomers is preferably at most 30 mass % based on all the units in the fluorinated polymer (S1).

[0161] The ion exchange capacity of the fluorinated polymer (S1) is preferably 0.5 to 1.1 milliequivalents / g of dry resin, more preferably 0.6 to 1.1 milliequivalents / g of dry resin, particularly preferably 0.6 to 1.0 milliequivalents / g of dry resin.

[0162] When the ion exchange capacity of the fluorinated polymer (S1) is at least the above lower limit, the resistance of the ion exchange membrane 1 with a catalyst layer is low and the electrolysis voltage can be further reduced. On the other hand, when the ion exchange capacity of the fluorinated polymer (S1) is at most the above upper limit, the current efficiency is further improved.

[0163] <Layer (Sb)>

[0164] The layer 12B as the layer (Sb) may be a layer containing the fluorinated polymer (S2), and is preferably a layer consisting only of the fluorinated polymer (S2) without containing any material other than the fluorinated polymer (S2). That is, the layer (Sb) is preferably a layer consisting of the fluorinated polymer (S2).

[0165] When the ion exchange membrane 1 with a catalyst layer is applied to an electrolytic hydrogenation device described later, the layer 12B is arranged on the cathode side relative to the layer 12A.

[0166] Figure 1 In the figure, layer 12B is shown as a single layer, but it can also be a layer formed by multiple layers. When layer 12B is formed by multiple layers, each layer can have a different type of structural unit constituting the fluorinated polymer (S2) and a different ratio of structural units having sulfonic acid type functional groups.

[0167] In addition, when the layer 12B is formed of a plurality of layers, the ion exchange capacity of the fluorinated polymer (S2) contained in each layer is higher than the ion exchange capacity of the fluorinated polymer (S1) contained in the layer 12A.

[0168] When layer 12B is formed of a plurality of layers, each layer 12B is preferably arranged so that the ion exchange capacity increases from inorganic particle layer 14 toward catalyst layer 16. This can suppress delamination of each layer constituting layer 12B.

[0169] The thickness of the layer 12B when dried (the total when the layer 12B is formed by a plurality of layers) is preferably 50 to 500 μm, more preferably 50 to 200 μm, and particularly preferably 50 to 150 μm. If the thickness of the layer 12B when dried is above the lower limit, the mechanical strength of the ion exchange membrane 1 with the catalyst layer is improved, and the current efficiency is more excellent. If the thickness of the layer (Sb) 12B when dried is below the upper limit, the resistance of the ion exchange membrane 1 with the catalyst layer can be suppressed to a lower level.

[0170] (Fluoropolymer (S2))

[0171] The layer (Sb) may contain one kind of fluorinated polymer (S2) alone, or may contain two or more kinds of fluorinated polymers (S2).

[0172] Layer (Sb) may include polymers other than fluoropolymer (S2), preferably substantially composed of fluoropolymer (S2). Substantially composed of fluoropolymer (S2) means that, relative to the total mass of the polymer in the layer (Sb), the content of fluoropolymer (S2) is 90% by mass or more. The upper limit of the content of fluoropolymer (S2) is 100% by mass relative to the total mass of the polymer in the layer (Sb).

[0173] Specific examples of the polymer other than the fluorinated polymer (S2) are the same as those of the polymer other than the fluorinated polymer (S1) (other polymer) described above.

[0174] It is preferred to use the fluorinated polymer (S2) which is the same as the fluorinated polymer (S1) except that the ion exchange capacity is different.

[0175] The ion exchange capacity of the fluorinated polymer (S1) and the fluorinated polymer (S2) can be adjusted by changing the content of the ion exchange group in the fluorinated polymer (S1) or the fluorinated polymer (S2).

[0176] The ion exchange capacity of the fluorinated polymer (S2) is preferably 0.7 to 2.0 milliequivalents / g dry resin, more preferably 0.7 to 1.5 milliequivalents / g dry resin, further preferably 0.7 to 1.4 milliequivalents / g dry resin, particularly preferably 0.8 to 1.4 milliequivalents / g dry resin.

[0177] When the ion exchange capacity of the fluorinated polymer (S2) is at least the above lower limit, the resistance of the ion exchange membrane with the catalyst layer is low, and the electrolysis voltage can be further reduced. In addition, when the ion exchange capacity of the fluorinated polymer (S2) is at most the above upper limit, the current efficiency is more excellent.

[0178] When layer (Sb) is a single layer, from the perspective of further exerting the effect of the present invention, the absolute value of the difference between the ion exchange capacity of the fluorinated polymer (S1) and the ion exchange capacity of the fluorinated polymer (S2) is preferably 0.1 to 1.4 milliequivalents / g of dry resin, more preferably 0.1 to 0.65 milliequivalents / g of dry resin, further preferably 0.1 to 0.6 milliequivalents / g of dry resin, and particularly preferably 0.1 to 0.5 milliequivalents / g of dry resin.

[0179] When layer (Sb) is formed of a plurality of layers, from the perspective of further exerting the effect of the present invention, the absolute value of the difference between the ion exchange capacity of the fluorinated polymer (S1) and the ion exchange capacity of the fluorinated polymer (S2) contained in the layer disposed closest to the layer (Sa) among the layers constituting layer (Sb) is preferably 0.1 to 1.4 milliequivalents / g of dry resin, more preferably 0.1 to 0.65 milliequivalents / g of dry resin, and particularly preferably 0.1 to 0.5 milliequivalents / g of dry resin.

[0180] When the layer (Sb) is formed by a plurality of layers, from the perspective of further exerting the effect of the present invention, the absolute value of the difference in ion exchange capacity of the fluoropolymer (S2) contained in each layer constituting the layer (Sb) is preferably 0.1 to 0.65 milliequivalents / g of dry resin, more preferably 0.1 to 0.5 milliequivalents / g of dry resin, and particularly preferably 0.1 to 0.3 milliequivalents / g of dry resin.

[0181] <Inorganic particle layer>

[0182] The inorganic particle layer 14 is a layer containing inorganic particles and a binder, and is arranged on the surface of the layer 12A opposite to the surface on which the layer 12B is arranged.

[0183] When oxygen generated by electrolysis of the aqueous electrolyte solution adheres to the surface of the layer (Sa), the electrolysis voltage increases during electrolytic hydrogenation of the aromatic compound. The inorganic particle layer is provided to inhibit the adhesion of oxygen generated by electrolysis of the aqueous electrolyte solution to the surface of the layer (Sa) and to inhibit the increase in the electrolysis voltage.

[0184] From the viewpoint of being able to further reduce the electrolysis voltage, the thickness of the inorganic particle layer 14 is preferably 1 to 50 μm, more preferably 1 to 30 μm, and particularly preferably 1 to 20 μm.

[0185] The inorganic particles are preferably hydrophilic and are specifically preferably at least one selected from the group consisting of oxides, nitrides and carbides of Group 4 or Group 14 elements, more preferably SiO2, SiC, ZrO2, ZrC, and particularly preferably ZrO2.

[0186] The average particle size of the inorganic particles is preferably 0.01 to 10 μm, more preferably 0.01 to 5 μm, and further preferably 0.5 to 3 μm. If the average particle size of the inorganic particles is above the lower limit, a high gas adhesion inhibition effect can be obtained. If the average particle size of the inorganic particles is below the upper limit, the inorganic particles have excellent resistance to shedding.

[0187] The average particle size of the inorganic particles is a value obtained by calculating the volume average of the 50% particle size (D ) obtained by measuring a dispersion in which the inorganic particles are dispersed in a solvent using a known particle size distribution measuring device based on the laser diffraction / scattering method (a laser diffraction / scattering particle size distribution measuring device manufactured by Microtrac BEL Corp. or a device based thereon) according to the particle size distribution measuring device. 50 ).

[0188] As the binder, preferably a hydrophilic fluorinated polymer having a carboxylic acid group or a sulfonic acid group is preferred, and more preferably a fluorinated polymer having a sulfonic acid group. The fluorinated polymer may be a homopolymer of a monomer having a carboxylic acid group or a sulfonic acid group, or a copolymer of a monomer having a carboxylic acid group or a sulfonic acid group and a monomer copolymerizable with the monomer.

[0189] The mass ratio of the binder (hereinafter also referred to as "binder ratio") relative to the total mass of the inorganic particles and the binder in the inorganic particle layer is preferably 0.1 to 0.5. If the binder ratio in the inorganic particle layer is above the above lower limit, the inorganic particles have excellent resistance to falling off. If the binder ratio in the inorganic particle layer is below the above upper limit, a high gas adhesion inhibition effect can be obtained.

[0190] When the surface of the inorganic particle layer side of the layer (Sa) has a concavo-convex structure, the inorganic particle layer preferably has a surface shape of the concavo-convex structure following the concavo-convex structure of the layer (Sa) (see Figure 1 ).

[0191] <Catalyst layer>

[0192] The catalyst layer 16 is a layer containing a catalyst, and is arranged on the surface of the layer 12B which is opposite to the surface on which the layer 12A is arranged.

[0193] Specific examples of the catalyst include: a supported catalyst in which platinum, a platinum alloy or a catalyst containing platinum having a core-shell structure is supported on a carbon support, an iridium oxide catalyst, an alloy containing iridium oxide, and a catalyst containing iridium oxide having a core-shell structure. As a carbon support, carbon black powder can be mentioned.

[0194] From the viewpoint of suppressing the falling of the catalyst, the catalyst layer 16 may further contain a polymer having an ion exchange group. Examples of the polymer having an ion exchange group include a fluorine-containing polymer having an ion exchange group.

[0195] Figure 1 In the example of FIG. 1 , the catalyst layer 16 is formed on the surface of the layer 12B, which is a so-called zero gap structure. However, the present invention is not limited thereto, and the catalyst layer 16 may be formed on the layer 12B via other layers. In other words, other layers may be formed between the catalyst layer 16 and the layer 12B.

[0196] For example, a carbon felt that functions as a cathode and a gas diffusion layer may be provided on the surface of the layer (Sb), and a catalyst layer may be formed on the surface of the carbon felt.

[0197] <Reinforcement Materials>

[0198] The reinforcing material 20 is disposed in the electrolyte 12 .

[0199] The reinforcing material 20 is a material for reinforcing the electrolyte membrane 12 and is derived from a reinforcing cloth. The reinforcing cloth is formed by warp and weft, and preferably the warp and weft are orthogonal. Figure 1 As shown, the reinforcing cloth may have reinforcing wires 22 and sacrificial wires 24 , but may also not have sacrificial wires 24 .

[0200] As the reinforcing yarn 22, yarns made of a perfluorocarbon polymer are preferred, yarns made of polytetrafluoroethylene (hereinafter also referred to as "PTFE") are more preferred, and PTFE yarns made of only PTFE are still more preferred.

[0201] The sacrificial wire 24 is a wire at least partly dissolved by pretreatment (for example, a treatment of immersing the reinforcement precursor film in an alkaline aqueous solution) or process liquid (ie, the electrolyte solution or aromatic compound used in the electrolytic hydrogenation of the aromatic compound).

[0202] The sacrificial wire 24 is preferably a wire dissolved by the process liquid. Thus, the ion exchange membrane 1 with the catalyst layer has excellent handling properties from the manufacture of the ion exchange membrane 1 with the catalyst layer to the adjustment operation of the electrolytic hydrogenation of aromatic compounds. In addition, the sacrificial wire 1 dissolves during the operation of the electrolytic hydrogenation device, thereby further reducing the electrolysis voltage.

[0203] One sacrificial yarn 24 may be a monofilament composed of one filament, or may be a multifilament composed of two or more filaments.

[0204] As the sacrificial yarn 24, preferably, a PET yarn formed only of PET, a PET / PBT yarn formed of a mixture of PET and polyethylene terephthalate (hereinafter also referred to as "PBT"), a PBT yarn formed only of PBT, or a PTT yarn formed only of polytrimethylene terephthalate (hereinafter also referred to as "PTT"), and a PET yarn is more preferred.

[0205] Figure 1In the example, a portion of the sacrificial wire 24 remains, and dissolution holes 28 are formed around the dissolved residues of the filaments 26 of the sacrificial wire 24. Therefore, the ion exchange membrane 1 with the catalyst layer is not easily damaged by cracks, etc., during the processing of the ion exchange membrane 1 with the catalyst layer after the manufacture of the ion exchange membrane 1 with the catalyst layer before the regulated operation of the electrolytic hydrogenation of aromatic compounds and the installation of the ion exchange membrane 1 with the catalyst layer in the electrolytic cell during the regulated operation.

[0206] Figure 1 In the example of FIG. 1 , the reinforcing material 20 is provided, but the invention is not limited thereto. The ion exchange membrane with a catalyst layer of the present invention may not have a reinforcing material.

[0207] in addition, Figure 1 In the example shown in FIG. 1 , the reinforcing material 20 is disposed between the layer 12A and the layer 12B, but the position of the reinforcing material is not limited thereto, and for example, the reinforcing material may be disposed in the layer 12A or in the layer 12B.

[0208] <Method for producing an ion exchange membrane with a catalyst layer>

[0209] An example of a method for producing an ion exchange membrane with a catalyst layer of the present invention is shown below. The method for producing an ion exchange membrane with a catalyst layer of the present invention preferably includes the following steps (i) to (iv). Thus, the ion exchange membrane with a catalyst layer of the present invention is obtained.

[0210] Step (i): a step of obtaining a precursor film, wherein the precursor film is sequentially laminated with: a layer (Sa') comprising a fluorinated polymer (S1') having a group that can be converted into a sulfonic acid type functional group, and a layer (Sb') comprising a fluorinated polymer (S2') having a group that can be converted into a sulfonic acid type functional group.

[0211] Step (ii): Step of forming an inorganic particle layer on the surface of layer (Sa')

[0212] Step (iii): a step of converting the groups in the precursor film that can be converted into sulfonic acid type functional groups into sulfonic acid type functional groups

[0213] Step (iv): Step of forming a catalyst layer on the surface of layer (Sb')

[0214] Here, the order of carrying out steps (i) to (iv) is not particularly limited, and it is preferably carried out in the order of step (i), step (ii), step (iii) and step (iv). Alternatively, it may be carried out in the order of step (ii), step (i), step (iii) and step (iv).

[0215] Hereinafter, an example of the method for producing the ion exchange membrane with a catalyst layer of the present invention will be described for each step.

[0216] (Process (i))

[0217] The precursor film may be produced by sequentially arranging a layer (Sa') containing a fluorinated polymer (S1') and a layer (Sb') containing a fluorinated polymer (S2'), and laminating them using a laminating roll or a vacuum laminating apparatus.

[0218] The precursor film may be a reinforced precursor film having a reinforcing material including reinforcing filaments. In this case, for example, the layer (Sa'), the reinforcing material, and the layer (Sb') are sequentially arranged to obtain the reinforced precursor film according to the above method.

[0219] The surface of the layer (Sa') opposite to the surface on which the layer (Sb') is disposed may be treated to have a concavo-convex structure using any of the above methods.

[0220] By the step (iii) described later, the layer (Sa') containing the fluorinated polymer (S1') is converted into the layer (Sa) containing the fluorinated polymer (S1), and the layer (Sb') containing the fluorinated polymer (S2') is converted into the layer (Sb) containing the fluorinated polymer (S2).

[0221] The fluorinated polymer (S1') is preferably a copolymer of a fluorinated olefin and a monomer having a group convertible into a sulfonic acid type functional group and a fluorine atom (hereinafter also referred to as "fluorinated monomer (S1')").

[0222] As the method for copolymerizing the fluorinated polymer (S1'), a known method such as solution polymerization, suspension polymerization, emulsion polymerization, etc. may be employed.

[0223] The fluorinated olefins include those exemplified above, and TFE is preferred from the viewpoints of the production cost of the monomer, the reactivity with other monomers, and the excellent properties of the obtained fluorinated polymer (S1).

[0224] The fluorinated olefins may be used alone or in combination of two or more.

[0225] Examples of the fluorine-containing monomer (S1′) include compounds having one or more fluorine atoms in the molecule, having an ethylenic double bond, and having a group that can be converted into a sulfonic acid type functional group.

[0226] As the fluorinated monomer (S1'), a compound represented by the formula (2) is preferred from the viewpoints of the production cost of the monomer, the reactivity with other monomers, and the excellent properties of the obtained fluorinated polymer (S1).

[0227] Formula (2) CF2 = CF-L-(A) n

[0228] In formula (2), L and n are as defined above.

[0229] A is a group that can be converted into a sulfonic acid type functional group. The group that can be converted into a sulfonic acid type functional group is preferably a functional group that can be converted into a sulfonic acid type functional group by hydrolysis. As specific examples of the group that can be converted into a sulfonic acid type functional group, -SO2F, -SO2Cl, -SO2Br can be cited. When there are two A in formula (2), A can be the same as or different from each other.

[0230] As the compound represented by formula (2), the compound represented by formula (2-1), the compound represented by formula (2-2), the compound represented by formula (2-3), the compound represented by formula (2-4) and the compound represented by formula (2-3) are preferred.

[0231] Formula (2-1) CF2=CF-OR f1 -A

[0232] Formula (2-2) CF2=CF-R f1 -A

[0233]

[0234] R in the formula f1 , R f2 , r and A are defined as above.

[0235]

[0236] R in the formula f1 , R f2 , R f3 , r, m and A are defined as above.

[0237] Formula (2-5) CF2 = CF-(CF2) x -(OCF2CFY) y -O-(CF2) z -SO3M

[0238] In the formula, M, x, y, z and Y are as defined above.

[0239] Specific examples of the compound represented by formula (2-1) include the following compounds: wherein w is an integer of 1 to 8, and x is an integer of 1 to 5.

[0240] CF2=CF-O-(CF2) w -SO2F

[0241] CF2=CF-O-CF2CF(CF3)-O-(CF2) w -SO2F

[0242] CF2=CF-[O-CF2CF(CF3)] x -SO2F

[0243] Specific examples of the compound represented by formula (2-2) include the following compounds: wherein w in the formula is an integer of 1 to 8.

[0244] CF2=CF-(CF2) w -SO2F

[0245] CF2=CF-CF2-O-(CF2) w -SO2F

[0246] As the compound represented by the formula (2-3), the compound represented by the formula (2-3-1) is preferred.

[0247]

[0248] R in the formula f4 , R f5 , r and A are defined as above.

[0249] Specific examples of the compound represented by formula (2-3-1) include the following.

[0250]

[0251] As the compound represented by the formula (2-4), the compound represented by the formula (2-4-1) is preferred.

[0252]

[0253] R in the formula f1 , R f2 and A are defined as above.

[0254] Specific examples of the compound represented by formula (2-4-1) include the following.

[0255]

[0256] The fluorinated monomer (S1') may be used alone or in combination of two or more.

[0257] In the production of the fluorinated polymer (S1'), other monomers may be used in addition to the fluorinated olefin and the fluorinated monomer (S1'). Examples of the other monomers include those exemplified above.

[0258] The TQ value of the fluoropolymer (S1') is preferably in the range of 150 to 350°C, more preferably 170 to 300°C, further preferably 200 to 250°C, from the viewpoint of mechanical strength and membrane production properties as an ion exchange membrane with a catalyst layer.

[0259] When the fluorinated polymer (S2') is converted into the fluorinated polymer (S2), it is preferred to use the same polymer as the fluorinated polymer (S1') except that the ion exchange capacity of the fluorinated polymer (S1) is different.

[0260] (Step (ii))

[0261] The method for forming the inorganic particle layer is not particularly limited. For example, there may be mentioned a method of applying an inorganic particle dispersion containing inorganic particles, a binder and a solvent on the surface of the layer (Sa') and drying the applied layer of the inorganic particle dispersion.

[0262] The coating conditions and drying conditions are not particularly limited, and known conditions can be adopted.

[0263] The inorganic particles and the binder contained in the inorganic particle dispersion are as described above. The solvent contained in the inorganic particle dispersion is not particularly limited, and water or an organic solvent can be used.

[0264] (Process (iii))

[0265] Specific examples of the method for converting the group in the precursor film that can be converted into a sulfonic acid type functional group into a sulfonic acid type functional group include a method of subjecting the precursor film to a treatment such as a hydrolysis treatment or an acidification treatment.

[0266] Among them, a method of bringing the precursor film into contact with an alkaline aqueous solution is preferred.

[0267] When the above-mentioned reinforcement precursor film is used as the precursor film, at least a part of the sacrificial filaments included in the reinforcement precursor film is hydrolyzed and dissolved by the action of the alkaline aqueous solution.

[0268] Specific examples of the method of bringing the precursor film into contact with the alkaline aqueous solution include a method of immersing the precursor film in the alkaline aqueous solution and a method of spraying and applying the alkaline aqueous solution to the surface of the precursor film.

[0269] The temperature of the alkaline aqueous solution is preferably 30 to 100° C., particularly preferably 40 to 100° C. The contact time between the precursor film and the alkaline aqueous solution is preferably 3 to 150 minutes, particularly preferably 5 to 50 minutes.

[0270] The alkaline aqueous solution preferably contains an alkali metal hydroxide, a water-soluble organic solvent and water.

[0271] Examples of the alkali metal hydroxide include sodium hydroxide and potassium hydroxide.

[0272] In this specification, the water-soluble organic solvent is an organic solvent that is easily soluble in water, and specifically, an organic solvent having a solubility of 0.1 g or more in 1000 ml (20° C.) of water is preferred, and an organic solvent having a solubility of 0.5 g or more is particularly preferred. The water-soluble organic solvent preferably includes at least one selected from the group consisting of aprotic organic solvents, alcohols, and amino alcohols, and particularly preferably includes an aprotic organic solvent.

[0273] The water-soluble organic solvent may be used alone or in combination of two or more.

[0274] Specific examples of the aprotic organic solvent include dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, and N-ethyl-2-pyrrolidone, and dimethyl sulfoxide is preferred.

[0275] Specific examples of the alcohols include methanol, ethanol, isopropanol, butanol, methoxyethoxyethanol, butoxyethanol, butyl carbitol, hexyloxyethanol, octanol, 1-methoxy-2-propanol, and ethylene glycol.

[0276] Specific examples of amino alcohols include ethanolamine, N-methylethanolamine, N-ethylethanolamine, 1-amino-2-propanol, 1-amino-3-propanol, 2-aminoethoxyethanol, 2-aminothioethoxyethanol, and 2-amino-2-methyl-1-propanol.

[0277] The concentration of the alkali metal hydroxide in the alkaline aqueous solution is preferably 1 to 60% by mass, particularly preferably 3 to 55% by mass.

[0278] The content of the water-soluble organic solvent in the alkaline aqueous solution is preferably 1 to 60% by mass, particularly preferably 3 to 55% by mass.

[0279] The concentration of water in the alkaline aqueous solution is preferably 39 to 80% by mass.

[0280] After the precursor film is brought into contact with the alkaline aqueous solution, a treatment to remove the alkaline aqueous solution may be performed. As a method of removing the alkaline aqueous solution, for example, a method of washing the precursor film brought into contact with the alkaline aqueous solution with water is exemplified.

[0281] The ion exchange groups may be converted to the acidic form by contacting the precursor film with the alkaline aqueous solution and then contacting the resulting film with an acidic aqueous solution.

[0282] Specific examples of the method of bringing the precursor film into contact with the acidic aqueous solution include a method of immersing the precursor film in the acidic aqueous solution and a method of spraying and applying the acidic aqueous solution to the surface of the precursor film.

[0283] The acidic aqueous solution preferably contains an acid component and water.

[0284] Specific examples of the acid component include hydrochloric acid and sulfuric acid.

[0285] (Process (iv))

[0286] The method for forming the catalyst layer is not particularly limited. For example, a method of applying a catalyst dispersion containing a catalyst, a polymer having an ion exchange group and a solvent to the surface of the layer (Sb') and drying the applied layer of the catalyst dispersion is mentioned.

[0287] The coating conditions and drying conditions are not particularly limited, and known conditions can be adopted.

[0288] The catalyst and the polymer having an ion exchange group contained in the catalyst dispersion are as described above. The solvent contained in the catalyst dispersion is not particularly limited, and water or an organic solvent can be used.

[0289] [Ion exchange membrane]

[0290] The ion exchange membrane of the present invention comprises an inorganic particle layer containing inorganic particles and a binder, a layer (Sa) containing a first fluorinated polymer having a sulfonic acid functional group, and a layer (Sb) containing a second fluorinated polymer having a sulfonic acid functional group in this order.

[0291] Furthermore, the ion exchange capacity of the first fluorinated polymer is lower than the ion exchange capacity of the second fluorinated polymer.

[0292] Figure 3 FIG. 2 is a cross-sectional view showing an example of an ion exchange membrane of the present invention. Figure 3 As shown, the ion exchange membrane 10 includes an electrolyte 12 formed of a layer 12A as a layer (Sa) and a layer 12B as a layer (Sb), and an inorganic particle layer 14 disposed on the surface of the layer 12A, and a reinforcing material 20 is disposed in the electrolyte membrane 12. Figure 3 As shown, the surface of the layer 12A on the inorganic particle layer 14 side has a concavo-convex structure.

[0293] The ion exchange membrane of the present invention has the same configuration as the ion exchange membrane with a catalyst layer of the present invention, except that it does not have the catalyst layer that the ion exchange membrane with a catalyst layer of the present invention has, and the preferred embodiments are also the same.

[0294] The details of each layer of the ion exchange membrane of the present invention are the same as those of the ion exchange membrane with a catalyst layer of the present invention, and therefore the description thereof will be omitted.

[0295] The method for producing the ion exchange membrane of the present invention is not particularly limited, and the ion exchange membrane can be obtained by, for example, carrying out the steps (i) to (iv) described above as an example of the method for producing the ion exchange membrane with a catalyst layer of the present invention except for step (iv).

[0296] The ion exchange membrane of the present invention is suitably used for production of the ion exchange membrane with a catalyst layer of the present invention.

[0297] [Electrolytic hydrogenation device]

[0298] The electrolytic hydrogenation device of the present invention comprises: an electrolytic cell having an anode and a cathode, and an ion exchange membrane with a catalyst layer of the present invention, wherein the ion exchange membrane with a catalyst layer is arranged in the electrolytic cell in a manner to separate the anode and the cathode, the inorganic particle layer of the ion exchange membrane with a catalyst layer is arranged on the anode side, and the catalyst layer of the ion exchange membrane with a catalyst layer is arranged on the cathode side.

[0299] The electrolytic hydrogenation device of the present invention includes the above-mentioned ion exchange membrane with a catalyst layer, and therefore can reduce the electrolysis voltage and improve the current efficiency during the electrolytic hydrogenation of aromatic compounds.

[0300] One embodiment of the electrolytic hydrogenation device of the present invention is Figure 4 Take this as an example to illustrate. Figure 4 This is a schematic diagram showing an example of the electrolytic hydrogenation device of the present invention.

[0301] like Figure 4 As shown, the electrolytic hydrogenation device 100 comprises: an electrolytic cell 110 having a cathode 112 and an anode 114, and an ion exchange membrane 1 with a catalyst layer, wherein the ion exchange membrane 1 with the catalyst layer is installed in the electrolytic cell 110 in a manner that divides the electrolytic cell 110 into a cathode chamber 116 on the cathode 112 side and an anode chamber 118 on the anode 114 side.

[0302] like Figure 4 As shown, the ion exchange membrane 1 with a catalyst layer is installed in the electrolytic cell 110 in such a manner that the inorganic particle layer 14 is on the anode 114 side and the catalyst layer 16 is on the cathode 112 side.

[0303] The cathode 112 may be disposed in contact with the ion exchange membrane 1 with a catalyst layer, or may be disposed with a gap therebetween.

[0304] As a material constituting the cathode 112 and the cathode chamber 116, stainless steel, nickel, etc. are preferable.

[0305] Examples of materials constituting the anode 114 and the anode chamber 118 include stainless steel and nickel.

[0306] The surfaces of the cathode 112 and the anode 114 as electrode substrates are preferably coated with, for example, ruthenium oxide, iridium oxide, or the like.

[0307] When electrolytic hydrogenation of aromatic compounds is performed using the electrolytic hydrogenation device 100 , an electrolytic aqueous solution is supplied to an anode chamber 118 in which an anode 114 is arranged, and an aromatic compound is supplied to a cathode chamber 116 in which a cathode 112 is arranged.

[0308] Specific examples of the aromatic compound include benzene, toluene, and naphthalene.

[0309] The electrolyte aqueous solution is a solution in which an electrolyte is dissolved in water. Examples of the electrolyte include sulfuric acid and nitric acid. The electrolyte concentration is not particularly limited.

[0310] When the electrolytic hydrogenation device 100 is driven, protons (H + ) moves to the cathode chamber 116 side via the ion exchange membrane with a catalyst layer 1. Then, hydrogenation of the aromatic compound by proton addition occurs near the surface of the catalyst layer 16, and a hydrogenated organic substance is obtained in the cathode chamber 116.

[0311] Specific examples of the hydrogenated organic substance include cyclohexane, methylcyclohexane, and decahydronaphthalene.

[0312] Example

[0313] Hereinafter, the present invention will be described in detail with reference to examples. Examples 1 to 8 are examples, and Examples 9 to 12 are comparative examples. However, the present invention is not limited to these examples.

[0314] [Thickness of each layer of the ion exchange membrane with catalyst layer, ion exchange capacity of the fluorinated polymer]

[0315] The measurement was performed according to the above method.

[0316] [Evaluation test of electrolysis voltage and current efficiency]

[0317] The effective power-carrying area is 1.5dm 2 In a test electrolytic cell (electrolysis surface size is 150 mm vertical × 100 mm horizontal), an ion exchange membrane with a catalyst layer-anode assembly is arranged in a manner that the side without a catalyst layer faces the anode. It should be noted that as the anode, an electrode with ruthenium-containing Raney nickel electrodeposited on a SUS304 stamping metal (short diameter 5 mm, long diameter 10 mm) is used. In addition, the anode and the ion exchange membrane with a catalyst layer are directly in contact, and no gap is generated.

[0318] The flow rate of toluene supplied to the cathode chamber was adjusted to 5 mL / min, and the flow rate of 1 M sulfuric acid aqueous solution supplied to the anode chamber was adjusted to 10 mL / min. At a temperature of 65°C and a current density of 400 mA / cm 2The electrolytic hydrogenation of toluene was carried out under the conditions of , and the electrolytic voltage (V) and current efficiency (%) were measured one day after the start of the operation, and evaluated according to the following criteria.

[0319] (Electrolysis voltage)

[0320] ◎:2.3V or less

[0321] ○: More than 2.3V and less than 2.4V

[0322] ×: more than 2.4V

[0323] (Current efficiency)

[0324] ◎:More than 98%

[0325] ○: 96% or more and less than 98%

[0326] ×: Less than 96%

[0327] [Production of fluorinated polymer (S1')]

[0328] CF2=CF2 and a monomer (X) represented by the following formula (X) were copolymerized to obtain a fluorinated polymer (S1') (ion exchange capacity: 0.65 meq / g dry resin).

[0329] CF2=CF-O-CF2CF(CF3)-O-CF2CF2-SO2F···(X)

[0330] [Production of fluorinated polymer (S2')]

[0331] CF2=CF2 and monomer (X) are copolymerized to obtain a fluorine-containing polymer (S2') (ion exchange capacity: 0.80 meq / g dry resin).

[0332] [Production of fluorinated polymer (S3')]

[0333] CF2=CF2 and monomer (X) are copolymerized to obtain a fluorine-containing polymer (S3') (ion exchange capacity: 1.00 meq / g dry resin).

[0334] [Production of fluorinated polymer (S4')]

[0335] CF2=CF2 and monomer (X) are copolymerized to obtain a fluorine-containing polymer (S4') (ion exchange capacity: 1.10 meq / g dry resin).

[0336] [Production of fluorinated polymer (S5')]

[0337] CF2=CF2 and monomer (X) are copolymerized to obtain a fluorine-containing polymer (S5') (ion exchange capacity: 1.25 meq / g dry resin).

[0338] The ion exchange capacity described in the above [Production of fluorinated polymer (S1′)] to [Production of fluorinated polymer (S5′)] indicates the ion exchange capacity of the fluorinated polymer obtained when the fluorinated polymers (S1′) to (S5′) are hydrolyzed in the steps described later.

[0339] [Manufacturing of Film A]

[0340] The fluorinated polymer (S1') was molded by a melt extrusion method to obtain a film A (film thickness: 20 μm) composed of the fluorinated polymer (S1').

[0341] [Manufacturing of Film B]

[0342] The fluorinated polymer (S2') was molded by a melt extrusion method to obtain a film B (film thickness: 20 μm) composed of the fluorinated polymer (S2').

[0343] [Manufacturing of Film C]

[0344] The fluorinated polymer (S3') was molded by a melt extrusion method to obtain a thin film C (film thickness: 20 μm) composed of the fluorinated polymer (S3').

[0345] [Manufacturing of Film D]

[0346] The fluorinated polymer (S3') was molded by a melt extrusion method to obtain a thin film D (film thickness: 40 μm) composed of the fluorinated polymer (S3').

[0347] [Manufacturing of Film E]

[0348] The fluorinated polymer (S3') was molded by a melt extrusion method to obtain a thin film E (film thickness: 80 μm) composed of the fluorinated polymer (S3').

[0349] [Manufacturing of Film F]

[0350] The fluorinated polymer (S4') was molded by a melt extrusion method to obtain a thin film F (film thickness: 20 μm) composed of the fluorinated polymer (S4').

[0351] [Manufacturing of Film G]

[0352] The fluorinated polymer (S4') was molded by a melt extrusion method to obtain a thin film G (film thickness: 80 μm) composed of the fluorinated polymer (S4').

[0353] [Manufacturing of Film H]

[0354] The fluorinated polymer (S5') was molded by a melt extrusion method to obtain a thin film H (film thickness: 80 μm) composed of the fluorinated polymer (S5').

[0355] [Manufacturing of Film I]

[0356] The fluorinated polymer (S5') was molded by a melt extrusion method to obtain a thin film I (film thickness: 100 μm) composed of the fluorinated polymer (S5').

[0357] [Manufacture of reinforcing cloth]

[0358] The warp and weft yarns were made of 50 denier PTFE yarns, and the PTFE yarns were woven in a plain manner so that the density of the PTFE yarns was 80 yarns / inch to obtain a woven fabric 1. The weight per unit area of ​​the woven fabric 1 was 38 g / m 2 It should be noted that the warp and weft threads are composed of slit film threads.

[0359] [Preparation of Inorganic Particle Paste]

[0360] 29.0 mass % of zirconium oxide (average particle size: 1 μm), 1.3 mass % of methylcellulose, 4.6 mass % of cyclohexanol, 1.5 mass % of cyclohexane, and 63.6 mass % of water were mixed to obtain an inorganic particle paste (inorganic particle dispersion).

[0361] [Example 1]

[0362] Film A, reinforcing cloth, film I, and demolding PET film (thickness: 100 μm) are overlapped in order with the demolding PET film at the bottom. In a constant temperature bath set at 220°C, the air between film A and film I is vacuum-sucked while heating to integrate the layers. Then, the peeling PET film is peeled off to obtain a reinforced precursor film 1-1.

[0363] Next, the inorganic particle paste was transferred to the surface of the electrolyte membrane film A by roll pressing, thereby obtaining a reinforced precursor film 1-2 having an inorganic particle layer disposed on the surface of the film A. The adhesion amount of zirconium oxide was set to 20 g / m 2 .

[0364] The reinforced precursor membrane 1-2 was immersed in a solution of dimethyl sulfoxide / potassium hydroxide / water = 30 / 5.5 / 64.5 (mass ratio) at 95°C for 30 minutes to hydrolyze the groups in the reinforced precursor membrane 1-2 that can be converted into sulfonic acid type functional groups and convert them into K-type sulfonic acid type functional groups, and then washed with water. Thereafter, the obtained membrane was immersed in 1M sulfuric acid to convert the terminal groups from K-type to H-type, and then dried to obtain an ion exchange membrane 1.

[0365] The following dispersion is obtained: a dispersion in which a polymer (ion exchange capacity: 1.10 milliequivalents / g of dry resin) prepared by copolymerizing TFE and the above-mentioned monomer (X) and then hydrolyzing and acid-treating is dispersed in a solvent of water / ethanol = 40 / 60 (mass %) at a solid content concentration of 25.8% (hereinafter also referred to as "dispersion X").

[0366] Water (59.4 g) and ethanol (39.6 g) were added to 11 g of a supported catalyst having 46% by mass of platinum supported on carbon powder ("TEC10E50E" manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.), and mixed and pulverized using an ultrasonic homogenizer to obtain a catalyst dispersion.

[0367] A mixed solution (29.2 g) obtained by mixing and kneading the dispersion X (20.1 g), ethanol (11 g) and ZEORORA-H (manufactured by Zeon Corporation) (6.3 g) in advance was added to the catalyst dispersion. Water (3.66 g) and ethanol (7.63 g) were then added to the obtained dispersion, and the mixture was mixed for 60 minutes using a paint mixer to obtain a solid content concentration of 10.0% by mass to obtain a cathode catalyst ink (catalyst dispersion).

[0368] The cathode catalyst ink was applied to an ETFE sheet using a die coater, dried at 80°C, and then heat treated at 150°C for 15 minutes to obtain a platinum content of 0.4 mg / cm 2 The cathode catalyst layer is printed (decal).

[0369] The surface of the ion exchange membrane 1 where the inorganic particle layer is not formed is opposite to the surface where the cathode catalyst layer is printed, and hot pressing is performed under the conditions of a pressing temperature of 150°C, a pressing time of 2 minutes, and a pressure of 3MPa, so that the ion exchange membrane 1 and the cathode catalyst layer are joined, and the pressure is released and taken out after the temperature is lowered to 70°C, and the ETFE sheet printed with the cathode catalyst layer is peeled off to obtain an ion exchange membrane with a catalyst layer of Example 1. A carbon felt as a cathode is joined to the surface of the catalyst layer of the obtained ion exchange membrane to obtain an ion exchange membrane-cathode joint body with a catalyst layer.

[0370] It should be noted that the cathode area of ​​the ion exchange membrane-cathode assembly with a catalyst layer is 25 cm 2 .

[0371] [Example 2]

[0372] Film F and film H are heat-pressed to obtain a multilayer film FH.

[0373] Film A, reinforcing cloth, multilayer film FH, and demolding PET film (thickness: 100 μm) are overlapped in order with the demolding PET film at the bottom. In a constant temperature bath set at 220°C, the air between film A and the multilayer film FH is vacuum-sucked while heating to integrate the layers. The peeling PET film is then peeled off to obtain a reinforced precursor film 2-1.

[0374] In addition, the multilayer film FH is arranged so that the film F side becomes the reinforcing fabric side.

[0375] An ion exchange membrane-cathode assembly with a catalyst layer of Example 2 was obtained in the same manner as in Example 1 except that the reinforced precursor film 2-1 was used instead of the reinforced precursor film 1-1.

[0376] [Example 3]

[0377] Film C and film H are heat-pressed to obtain a multilayer film CH.

[0378] The ion exchange membrane-cathode assembly with a catalyst layer of Example 3 was obtained in the same manner as in Example 2 except that the multilayer film CH was used instead of the multilayer film FH. The multilayer film CH was arranged so that the film C side became the reinforcing cloth side.

[0379] [Example 4]

[0380] Film C and film G are heat-pressed to obtain a multilayer film CG.

[0381] The ion exchange membrane-cathode assembly with a catalyst layer of Example 4 was obtained in the same manner as in Example 2 except that the multilayer film CG was used instead of the multilayer film FH. The multilayer film CG was arranged so that the film C side became the reinforcing cloth side.

[0382] [Example 5]

[0383] Film B and film E are heat-pressed to obtain a multilayer film BE.

[0384] The same procedure as in Example 2 was followed except that the multilayer film BE was used instead of the multilayer film FH to obtain an ion exchange membrane-cathode assembly with a catalyst layer of Example 5. The multilayer film BE was arranged so that the film B side became the reinforcing cloth side.

[0385] [Example 6]

[0386] Film C and film H are heat-pressed to obtain a multilayer film CH.

[0387] The same operation as in Example 2 was performed except that the multilayer film CH was used instead of the multilayer film FH and the film B was used instead of the film A to obtain the ion exchange membrane-cathode assembly with a catalyst layer of Example 6. It should be noted that the multilayer film CH was arranged so that the film C side became the reinforcing cloth side.

[0388] [Example 7]

[0389] The ion exchange membrane-cathode assembly with a catalyst layer of Example 7 was obtained in the same manner as in Example 1 except that the film D was used instead of the film A and the film H was used instead of the film I.

[0390] [Example 8]

[0391] An ion exchange membrane-cathode assembly with a catalyst layer of Example 8 was obtained in the same manner as in Example 3 except that the reinforcing cloth was not used.

[0392] [Example 9]

[0393] The ion exchange membrane-cathode assembly with a catalyst layer of Example 9 was obtained in the same manner as in Example 3 except that the inorganic particle layer was not provided on the surface of the thin film A.

[0394] [Example 10]

[0395] An ion exchange membrane-cathode assembly with a catalyst layer of Example 10 was obtained in the same manner as in Example 1 except that a membrane J (trade name “Nafion 115”, manufactured by Chemours) was used instead of the ion exchange membrane 1.

[0396] [Example 11]

[0397] An inorganic particle layer was formed on one surface of a film J (trade name "Nafion 115", manufactured by Chemours, a film made of a fluorinated polymer having a sulfonic acid group) by the same method as in Example 1 to obtain a film J with an inorganic particle layer.

[0398] The ion exchange membrane-cathode assembly with a catalyst layer of Example 11 was obtained in the same manner as in Example 1 except that the inorganic particle layer-bearing film J was used. The catalyst layer was formed on the surface of the film J opposite to the inorganic particle layer.

[0399] [Evaluation results]

[0400] The ion exchange membrane with a catalyst layer obtained as described above was used in various evaluation tests. The evaluation results are shown in Table 1.

[0401] Here, in Table 1, "IEC" means the ion exchange capacity of the fluorinated polymer.

[0402] In Table 1, “membrane thickness” refers to the film thickness of each layer in the ion exchange membrane with a catalyst layer, and is the same as the film thickness of each thin film used for preparing the ion exchange membrane with a catalyst layer.

[0403] In Table 1, "low IEC layer" refers to a layer formed of a fluorinated polymer having the lowest ion exchange capacity in the electrolyte membrane constituting the ion exchange membrane with a catalyst layer, i.e., layer (Sa). In addition, "high IEC layer" refers to a layer containing a fluorinated polymer having a higher ion exchange capacity than the "low IEC layer" in the electrolyte membrane constituting the ion exchange membrane with a catalyst layer, i.e., layer (Sb). Where one type of film is used as the electrolyte membrane, the type of the film used is recorded in the "low IEC layer" column.

[0404] [Table 1]

[0405]

[0406] As shown in Table 1, it is shown that: by making the electrolyte membrane into a multilayer structure, configuring a layer containing a fluorinated polymer with low ion exchange capacity (low IEC layer) on the anode side, and providing an inorganic particle layer on the surface of the low IEC layer, the electrolysis voltage can be reduced and the current efficiency can be improved during the electrolytic hydrogenation of aromatic compounds (Examples 1 to 8).

[0407] In addition, the ion exchange membrane with a catalyst layer of Example 1 was used, and the carbon felt as a cathode was bonded to the surface of the inorganic particle layer to obtain the ion exchange membrane-cathode assembly with a catalyst layer of Example 12. The formation surface of the inorganic particle layer of the ion exchange membrane-cathode assembly with a catalyst layer of Example 12 (i.e., the film A side) was arranged on the cathode side, and the formation surface of the catalyst layer (i.e., the film I side) was arranged on the anode side, and the same evaluation as Example 1 was performed. As a result, the voltage suddenly rose, and electrolytic hydrogenation could not be performed. As a reason for this, it is believed that it is because the film A and the film I are peeled off.

[0408] It should be noted that the entire contents of the specification, claims, drawings, and abstract of Japanese Patent Application No. 2020-018828 filed on February 6, 2020 are cited herein and incorporated as a disclosure of the present invention.

[0409] Description of Reference Numerals

[0410] 1 Ion exchange membrane with catalyst layer

[0411] 10 Ion exchange membrane

[0412] 12 Electrolyte membrane

[0413] 12A Floor(Sa)

[0414] 12B layer (Sb)

[0415] 14 Inorganic particle layer

[0416] 16 Catalyst layer

[0417] 20 Reinforcement Materials

[0418] 22 Reinforcement wire

[0419] 24 Sacrificial Silk

[0420] 26 Filament

[0421] 28 Dissolution hole

[0422] 100 Electrolytic hydrogenation device

[0423] 110 Electrolyzer

[0424] 112 cathode

[0425] 114 Anode

[0426] 116 Cathode Chamber

[0427] 118 Anode Chamber

[0428] B, B1, B2 convex part

[0429] D1, D2 shortest distance

[0430] P1, P2 positions

[0431] T1, T2 position

Claims

1. An ion exchange membrane with a catalyst layer, which comprises: an inorganic particle layer comprising inorganic particles and a binder; A layer Sa comprising a first fluorine-containing polymer having a sulfonic acid type functional group; a layer Sb comprising a second fluorine-containing polymer having a sulfonic acid type functional group; and Catalyst layer, The ion exchange capacity of the first fluorinated polymer is lower than the ion exchange capacity of the second fluorinated polymer, The ion exchange capacity of the first fluorinated polymer is 0.6 to 1.1 milliequivalents per gram of dry resin, The ion exchange capacity of the second fluorine-containing polymer is 0.8 to 2.0 milliequivalents per gram of dry resin.

2. The ion exchange membrane with a catalyst layer according to claim 1, in, The interface of the layer Sa on the inorganic particle layer side has a concavo-convex structure. 3 . The ion exchange membrane with a catalyst layer according to claim 1 , further comprising a reinforcing material including reinforcing fibers.

4. The ion exchange membrane with a catalyst layer according to claim 1 or 2, in, The first fluorine-containing polymer having a sulfonic acid functional group comprises a unit based on a fluorine-containing olefin and a unit having a sulfonic acid functional group and a fluorine atom.

5. The ion exchange membrane with a catalyst layer according to claim 4, in, The fluorine-containing olefin is tetrafluoroethylene, chlorotrifluoroethylene, vinylidene fluoride, vinyl fluoride or hexafluoropropylene.

6. The ion exchange membrane with a catalyst layer according to claim 4, in, The unit having a sulfonic acid type functional group and a fluorine atom is a unit represented by formula (1), Formula (1)-[CF 2 -CF(-L-(SO 3 M) n )]- In the formula, L is an n+1-valent perfluorocarbon group which may contain an ethereal oxygen atom, M is a hydrogen atom, an alkali metal or a quaternary ammonium cation, and n is 1 or 2.

7. A method for producing an ion exchange membrane with a catalyst layer, which is the method for producing an ion exchange membrane with a catalyst layer according to any one of claims 1 to 6, in, An ion exchange membrane is obtained, and a catalyst layer is provided on the layer Sb, The ion exchange membrane has in sequence: an inorganic particle layer comprising inorganic particles and a binder; a layer Sa comprising a first fluorine-containing polymer having a sulfonic acid type functional group; and a layer Sb comprising a second fluorine-containing polymer having a sulfonic acid type functional group, The ion exchange capacity of the first fluorinated polymer is lower than the ion exchange capacity of the second fluorinated polymer, The ion exchange capacity of the first fluorinated polymer is 0.6 to 1.1 milliequivalents per gram of dry resin, The ion exchange capacity of the second fluorine-containing polymer is 0.8 to 2.0 milliequivalents per gram of dry resin.

8. An electrolytic hydrogenation device comprising: an electrolytic cell having an anode and a cathode; and an ion exchange membrane with a catalyst layer according to any one of claims 1 to 6, The ion exchange membrane with the catalyst layer is arranged in the electrolytic cell in a manner to separate the anode and the cathode. The inorganic particle layer of the ion exchange membrane with a catalyst layer is arranged on the anode side, and the catalyst layer of the ion exchange membrane with a catalyst layer is arranged on the cathode side.

9. The electrolytic hydrogenation device according to claim 8, in, An aqueous electrolyte solution is supplied to an anode chamber in which the anode is arranged, and an aromatic compound is supplied to a cathode chamber in which the cathode is arranged.

Citation Information

Patent Citations

  • Copolymer containing peroxy bond in molecule

    JP1989000410B2

  • Adjustment mechanism

    JP2020018828A

  • Method for producing fluorine ion-containing permeable diaphragm, method for producing electrolytic device, method for producing gas, method for producing hydrogen gas and oxygen gas, and method for producing chlorine gas

    JP2018062647A

  • Method for producing a metal salt by electrolysis

    US4877498A

  • Perfluoro block polymer, liquid composition, solid polymer electrolyte membrane and membrane electrode assembly for solid polymer fuel cells

    WO2017170055A1