A superparamagnetic nano-iron material and its composite materials, preparation method and application
By using iron salts and reducing agents to prepare superparamagnetic nano-iron materials under a nitrogen atmosphere, combined with surface modification and doping technology, the problem of agglomeration of nano-iron materials was solved and its efficient decontamination ability and stability in soil and water were achieved. properties and suitable for environmental remediation applications.
Patent Information
- Application Number
- CN202210644231.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-09
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-06-09
AI Technical Summary
Nano-iron materials are prone to agglomeration due to the magnetic interaction between particles, resulting in a reduction in specific surface area and poor transmission performance, which affects its treatment effect in soil and groundwater.
Superparamagnetic nano-iron materials are prepared using high-speed mechanical stirring of iron salts and reducing agents in a nitrogen atmosphere. Their stability and dispersion are improved through surface modification materials and doped composite materials to avoid agglomeration caused by magnetic interactions.
It achieves long-term stability and efficient processing performance of nano-iron materials in the water phase, can effectively remove heavy metals and organic pollutants in soil and water, reduces production costs, and is suitable for industrial production.
Smart Images

Figure CN115106519B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nano material preparation and environmental restoration, and in particular to a superparamagnetic nano iron material and a composite material thereof, a preparation method and application thereof. Background Art
[0002] Nano-iron materials have strong reduction and catalytic effects and high reaction activity. They are widely used to remove organic pollutants and heavy metal ions in soil, groundwater, rivers, lakes and industrial wastewater, such as reducing and repairing groundwater contaminated by chlorinated hydrocarbons, catalyzing Fenton oxidation of soil contaminated by petroleum hydrocarbons, and treating salt-containing organic wastewater that is difficult to degrade by self-catalytic Fenton oxidation. Nano-iron materials include nano-zero-valent iron and its oxides, nano-iron materials doped with heterometallic materials, and nano-iron materials composited with biochar, graphene, and natural minerals.
[0003] However, due to the inherent magnetic interaction between particles, nano-iron materials are very easy to agglomerate into micron or even millimeter-sized particles, resulting in a decrease in their specific surface area and thus a decrease in their activity. Their transmission performance in soil and groundwater media is very poor, affecting their treatment effect. At present, the main method is surface modification, such as using high molecular polymers such as carboxymethyl cellulose, PVP and PVA to coat the surface of nano-iron to enhance the double-layer repulsion between nano-iron particles and prevent nano-iron from agglomerating to enhance the migration performance and reaction activity of nano-iron materials. However, when nano-iron materials are dispersed in the aqueous phase, due to the micro-convection phenomenon caused by Brownian motion, there is always relative motion between the nano-iron materials, which in turn generates induced current under electromagnetic induction, destroying the double-layer of the nano-iron material and causing the material to agglomerate. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a superparamagnetic nano iron material and its composite material, a preparation method and application.
[0005] In a first aspect, the present invention provides a superparamagnetic nano-iron material, which is realized by adopting the following technical solution.
[0006] A superparamagnetic nano iron material is a nano zero-valent iron material with superparamagnetic properties which is mainly prepared from iron salt and a reducing agent.
[0007] In a second aspect, the present invention provides an application of a superparamagnetic nano-iron material, which is achieved by adopting the following technical solution.
[0008] An application of the superparamagnetic nano-iron material in environmental remediation is specifically used for remediating contaminated sites such as soil and groundwater contaminated by heavy metals and organochlorine compounds, as well as for the degradation and removal of heavy metals and organic pollutants in sewage and drinking water.
[0009] In a third aspect, the present invention provides a method for preparing a superparamagnetic nano-iron material, which is achieved by adopting the following technical solution.
[0010] A method for preparing a superparamagnetic nano-iron material comprises the following steps:
[0011] S1. According to a molar ratio of 1:0.5~20, the iron salt and the surface modification material are dissolved in deoxygenated ethanol to prepare a mixed solution of 5~400 g / L of the iron salt and the surface modification material;
[0012] S2. Weigh the reducing agent and dissolve it in the deoxygenated ethanol, and add ethylenediamine to the reducing agent in a molar ratio of 1:0.01 to 1 to prepare a mixed solution;
[0013] S3. According to the molar ratio of iron salt to reducing agent of 1:1~50, under the protection of nitrogen atmosphere and high-speed mechanical stirring, the mixed solution of step S2 is added dropwise to the mixed solution of step S1. After the addition is completed, the reaction is continued with stirring for 10~30 minutes to obtain a superparamagnetic nano iron material.
[0014] After the reaction is completed, the obtained superparamagnetic nano-iron material is stored in a sealed bottle; or dried under a nitrogen atmosphere for long-term storage.
[0015] Furthermore, the iron salt is selected from one or more of ferric chloride, ferrous chloride, ferrous sulfate, ferrous carbonate, ferrous acetate, ferric citrate, ammonium ferrous sulfate, ferrous oxalate, ferrous hydroxide, ferric oxide, rust, and iron sulfide, preferably ferrous chloride, ferrous citrate, ferrous oxalate, and iron oxide, and more preferably ferric hydroxide, ferric oxide, and rust.
[0016] Furthermore, the molar ratio of the iron salt to the surface modification material is preferably 1:5.
[0017] Furthermore, the surface modification material is selected from one or more of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, hexadecyl ammonium bromide, carboxymethyl cellulose, polyvinyl pyrrolidone, polyvinyl alcohol, polyacrylic acid, polyacrylamide, polylysine, guar gum, and rhamnolipid, preferably carboxymethyl cellulose.
[0018] Furthermore, the reducing agent is selected from one or more of sodium dithionite, thiourea dioxide, hydrazine hydrate, sodium borohydride, and potassium borohydride, preferably thiourea dioxide.
[0019] In a fourth aspect, the present invention provides a superparamagnetic nano-iron composite material, which is realized by adopting the following technical solution.
[0020] A superparamagnetic nano-iron composite material is a nano-zero-valent iron composite material with superparamagnetic properties, which is mainly prepared from iron salt, a reducing agent and a doped composite material.
[0021] In a fifth aspect, the present application provides an application of a superparamagnetic nano-iron composite material, which is achieved by adopting the following technical solution.
[0022] An application of the superparamagnetic nano-iron composite material in environmental remediation is specifically used for remediating contaminated sites such as soil and groundwater contaminated by heavy metals and organic chlorine compounds, as well as for degrading and removing heavy metals and organic pollutants in sewage and drinking water.
[0023] In a sixth aspect, the present invention provides a method for preparing a superparamagnetic nano-iron composite material, which is achieved by adopting the following technical solution.
[0024] A method for preparing a superparamagnetic nano-iron composite material comprises adding a doped composite material to the mixed solution of the iron salt and the surface modification material in step S1 according to a mass ratio of iron to the doped composite material of 1:0.001-100.
[0025] Furthermore, the mass ratio of the iron to the doped composite material is preferably 1:5.
[0026] Furthermore, the doped composite material is selected from one or more of metal salts, carbon materials, sulfur materials, metal oxides, metal hydroxides, natural fibers and natural mineral materials.
[0027] Furthermore, the sulfur material is selected from one or more of sublimated sulfur, sodium sulfide, potassium sulfide, and iron sulfide, preferably sodium sulfide.
[0028] Furthermore, the metal salt is selected from one or more of calcium, magnesium, aluminum, manganese, cobalt, nickel, copper, zinc, and palladium, preferably copper salt.
[0029] Furthermore, the carbon material is selected from one or more of biochar, activated carbon, graphene, carbon nanotubes, carbon quantum dots, carbon fibers, graphyne, and silicon carbide, preferably biochar.
[0030] Furthermore, the metal oxide is selected from one or more of MgO, Al2O3, Fe2O3, CaO, CeO2, TiO2, MnO2, SiO2, ZnO, MgAl2O4, MnFe2O4, MgAl2O4, MgFe2O4, ZnFe2O4, and ZnAl2O4, and is preferably metal oxides with little impact on the environment, such as Al2O3, Fe2O3, CaO, TiO2, MgAl2O4, and MgFe2O4.
[0031] Furthermore, the metal hydroxide is selected from one or more of Mg(OH)2, Al(OH)3, AlOOH, Fe(OH)3, CeOOH, MnOOH, MgAl two-dimensional layered double metal hydroxide, ZnAl two-dimensional layered double metal hydroxide, MgZnAl two-dimensional layered double metal hydroxide, MgFe two-dimensional layered double metal hydroxide, and MgFeAl two-dimensional layered double metal hydroxide, preferably Al(OH)3, AlOOH, Fe(OH)3 and MgAl two-dimensional layered double metal hydroxide.
[0032] Furthermore, the natural fiber material is selected from one or more of cellulose, chitosan, silk, bamboo fiber, flax fiber, and cotton fiber, preferably cellulose and cotton fiber.
[0033] Furthermore, the natural mineral material is selected from one or more of vermiculite, montmorillonite, kaolin, attapulgite, basalt, rectorite, sepiolite, zeolite, diatomaceous earth, wollastonite, volcanic ash and tourmaline, preferably montmorillonite and attapulgite.
[0034] The superparamagnetic nano zero-valent iron and its composite materials prepared in the present application include superparamagnetic sulfide nano zero-valent iron, superparamagnetic carbonized nano zero-valent iron, bimetallic doped superparamagnetic nano zero-valent iron, bimetallic doped carbonized nano zero-valent iron, bimetallic doped superparamagnetic sulfide nano zero-valent iron, carbon material-supported superparamagnetic nano zero-valent iron, carbon material-supported superparamagnetic carbonized nano zero-valent iron, carbon material-supported superparamagnetic sulfide nano zero-valent iron, metal oxide-supported superparamagnetic nano zero-valent iron, metal oxide-supported superparamagnetic carbonized nano zero-valent iron, metal oxide-supported superparamagnetic sulfide nano zero-valent iron. Iron, superparamagnetic nano-zero-valent iron supported by metal hydroxide, superparamagnetic carbonized nano-zero-valent iron supported by metal hydroxide, superparamagnetic sulfide nano-zero-valent iron supported by metal hydroxide, superparamagnetic nano-zero-valent iron supported by natural fiber materials, superparamagnetic carbonized nano-zero-valent iron supported by natural fiber materials, superparamagnetic sulfide nano-zero-valent iron supported by natural fiber materials, superparamagnetic nano-zero-valent iron supported by natural minerals, superparamagnetic carbonized nano-zero-valent iron supported by natural minerals, sulfide nano-zero-valent iron supported by natural minerals, and other materials that exhibit superparamagnetic properties and have zero-valent iron as the main component.
[0035] This application has the following beneficial effects.
[0036] 1. The superparamagnetic nano-iron material and the composite material thereof of the present invention have no magnetic interaction between the particles, and when dispersed in the aqueous phase, they have good long-term stability, will not agglomerate and settle, and can give full play to the efficient processing performance of the nano-iron material;
[0037] 2. The superparamagnetic nano-iron material and the composite material thereof of the present invention have simple preparation methods and low production costs, and can effectively remove various organic pollutants and heavy metal ions in soil and water environments, and have better effects when used for environmental remediation, and have low comprehensive costs;
[0038] 3. The preparation method of the superparamagnetic nano-iron material and the composite material thereof provided by the present invention is easy to scale up and can be directly used for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a TEM photo of the superparamagnetic nano-iron material synthesized in Example 1 of the present invention;
[0040] Figure 2 is a hysteresis loop diagram of the superparamagnetic nano-iron material synthesized in Example 1 of the present invention;
[0041] Figure 3 This is a photograph of the aqueous dispersion of the superparamagnetic nano-iron material synthesized in Example 1 of the present invention;
[0042] Figure 4 This is the kinetic curve of TCE degradation by the superparamagnetic nano-iron material synthesized in Example 1 of the present invention;
[0043] Figure 5 The hydrogen evolution performance of the superparamagnetic nano-iron material synthesized in Example 1 of the present invention under shaking table conditions;
[0044] Figure 6 is a hysteresis loop diagram of the superparamagnetic nano-iron material synthesized in Example 2 of the present invention;
[0045] Figure 7 is a hysteresis loop diagram of the superparamagnetic nano-iron material synthesized in Example 3 of the present invention;
[0046] Figure 8 It is the hysteresis loop diagram of the superparamagnetic nano-iron material synthesized in Example 4 of the present invention. DETAILED DESCRIPTION
[0047] The present patent application is further described below in conjunction with the accompanying drawings and embodiments.
[0048] Example 1
[0049] In this embodiment, potassium borohydride is used to reduce ferrous chloride to prepare superparamagnetic nano iron material, and the specific preparation steps are as follows:
[0050] 1) According to the molar ratio of Fe: carboxymethyl cellulose = 1:2, weigh ferrous chloride and sodium carboxymethyl cellulose and add them to deoxyethanol, stir to dissolve, and adjust the volume to obtain a Fe solution with a mass concentration of 20 g / L. 2+ Solution;
[0051] 2) Weigh a certain amount of potassium borohydride and add it to deoxyethanol, stir to dissolve, and adjust the volume to obtain a potassium borohydride solution with a mass concentration of 40 g / L; add ethylenediamine to the potassium borohydride solution at a molar ratio of potassium borohydride to ethylenediamine of 10:1;
[0052] 3) Under vigorous mechanical stirring and nitrogen protection, the solution of step 2 was added dropwise to the solution of step 1 at a molar ratio of Fe: potassium borohydride = 1:3. After the addition was completed, the reaction was continued with stirring for 20 min;
[0053] 4) The nano-iron material prepared in step 3 is washed with anhydrous ethanol to remove soluble salt ions and impurities, and dried under a nitrogen atmosphere to obtain a superparamagnetic nano-iron material.
[0054] The experimental results are shown in the attached Figure 1 and 2 ,from Figure 1 It can be seen that the synthesized superparamagnetic nanoiron material is a cluster composed of nanoiron particles. Figure 2 The hysteresis loop shows that it has no obvious hysteresis loop, and the room temperature remanence and coercive force are 0.86 emug -1 and 2.63 Oe, showing obvious superparamagnetic characteristics.
[0055] Figure 3 The aqueous dispersion of the synthetic material of this embodiment shows strong stability. After standing for 6.5 days, no obvious agglomeration and sedimentation occurs, showing good long-term stability. From the partial enlarged image in the figure (red box), it can be seen that very little hydrogen is generated after standing for 6.5 days, indicating that the tendency of superparamagnetic nano-iron clusters to corrode and precipitate hydrogen is weak.
[0056] Figure 4 The material synthesized in this example is used to reduce and degrade the pollutant trichloroethylene. The degradation performance of superparamagnetic nano-iron clusters on trichloroethylene is tested by a shaking table experiment. The concentration of TCE is 10 mg / L and the dosage of superparamagnetic nano-iron clusters is 2 g / L. The figure shows that superparamagnetic nano-iron exhibits a faster degradation kinetics for TCE, and TCE can be completely reduced, degraded and dechlorinated within 24 hours. Its corrosion and hydrogen evolution performance is much weaker than that of ordinary nZVI ( Figure 5 ), the hydrogen production data was fitted by the first-order reaction kinetic equation, and the rate constant of the corrosion hydrogen evolution reaction was calculated to be 0.019d -1 , based on which its life span is estimated to be 53 days, which is much longer than that of ordinary nZVI.
[0057] Example 2
[0058] In this embodiment, potassium borohydride is used to reduce a mixed solution of ferrous chloride and nickel chloride to prepare a superparamagnetic nano-iron-nickel composite material. The specific preparation steps are as follows:
[0059] 1) According to the molar ratio of Fe:Ni:carboxymethyl cellulose = 1:0.05:5, weigh ferrous chloride, nickel chloride and carboxymethyl cellulose and add them to deoxyethanol, stir to dissolve, and adjust the volume to obtain a Fe solution with a mass concentration of 20 g / L. 2+ Mixing solutions;
[0060] 2) Weigh a certain amount of potassium borohydride and add it to deoxyethanol, stir to dissolve, and adjust the volume to obtain a potassium borohydride solution with a mass concentration of 40 g / L; add ethylenediamine to the potassium borohydride solution at a molar ratio of potassium borohydride to ethylenediamine of 10:1;
[0061] 3) Under vigorous mechanical stirring and nitrogen protection, the solution of step 2 was added dropwise to the solution of step 1 at a molar ratio of Fe: potassium borohydride = 1:3. After the addition was completed, the reaction was continued with stirring for 20 min;
[0062] 4) The nano-iron material prepared in step 3 is washed with anhydrous ethanol to remove soluble salt ions and impurities, and dried under a nitrogen atmosphere to obtain a superparamagnetic nano-iron-nickel composite material.
[0063] Figure 6 This is the hysteresis loop of the superparamagnetic nano-iron-nickel composite material synthesized in this example. It can be seen from the figure that the material exhibits obvious superparamagnetic properties.
[0064] Example 3
[0065] In this embodiment, potassium borohydride is used to reduce ferrous chloride to prepare a superparamagnetic nano-iron composite material loaded with attapulgite, and the specific preparation steps are as follows:
[0066] 1) According to the molar ratio of Fe: carboxymethyl cellulose = 1:2, weigh ferrous chloride and carboxymethyl cellulose, add them to deoxyethanol, stir to dissolve, and adjust the volume to obtain a Fe solution with a mass concentration of 20 g / L. 2+ Mixed solution. Weigh the attapulgite in a mass ratio of Fe:attapulgite = 1:5, add it to the above mixed solution, and stir evenly;
[0067] 2) Weigh a certain amount of potassium borohydride and add it to deoxyethanol, stir to dissolve, and adjust the volume to obtain a potassium borohydride solution with a mass concentration of 40 g / L; add ethylenediamine to the potassium borohydride solution at a molar ratio of potassium borohydride to ethylenediamine of 10:1;
[0068] 3) Under vigorous mechanical stirring and nitrogen protection, the solution of step 2 was added dropwise to the solution of step 1 at a molar ratio of Fe: potassium borohydride = 1:2. After the addition was completed, the reaction was continued with stirring for 20 min;
[0069] 4) The nano-iron material prepared in step 3 is washed with anhydrous ethanol to remove soluble salt ions and impurities, and dried under a nitrogen atmosphere to obtain a superparamagnetic nano-iron composite material loaded with attapulgite.
[0070] Figure 7 The hysteresis loop of the superparamagnetic nano-iron composite material loaded with attapulgite synthesized in this embodiment shows obvious superparamagnetic characteristics.
[0071] Example 4
[0072] In this embodiment, potassium borohydride is used as a reducing agent to prepare a superparamagnetic nano-iron composite material supported by magnesium aluminum double hydroxide, and the specific preparation steps are as follows:
[0073] 1) According to the molar ratio of Fe: carboxymethyl cellulose = 1:1, weigh ferrous chloride and carboxymethyl cellulose, add them to deoxyethanol, stir to dissolve, and adjust the volume to obtain a Fe solution with a mass concentration of 20 g / L. 2+ Mixed solution. Weigh magnesium aluminum double hydroxide according to the mass ratio of Fe: magnesium aluminum double hydroxide = 1:3, add it to the above mixed solution, and stir evenly;
[0074] 2) Weigh a certain amount of potassium borohydride and add it to deoxyethanol, stir to dissolve, and adjust the volume to obtain a potassium borohydride solution with a mass concentration of 40 g / L; add ethylenediamine to the potassium borohydride solution at a molar ratio of potassium borohydride to ethylenediamine of 20:1;
[0075] 3) Under vigorous mechanical stirring and nitrogen protection, the solution of step 2 was added dropwise to the solution of step 1 in a mass ratio of Fe: potassium borohydride = 1:2.5. After the addition was completed, the reaction was continued with stirring for 20 min;
[0076] 4) The nano-iron material prepared in step 3 is washed with anhydrous ethanol to remove soluble salt ions and impurities, and dried under a nitrogen atmosphere to obtain a superparamagnetic nano-iron composite material supported by magnesium aluminum double hydroxide.
[0077] Figure 8 The hysteresis loop of the superparamagnetic nano-iron composite material supported by the magnesium-aluminum double hydroxide synthesized in this embodiment shows obvious superparamagnetic characteristics.
[0078] The embodiments of this specific implementation method are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A superparamagnetic nano-iron material, characterized in that: The preparation method of the superparamagnetic nano-iron comprises the following steps: S1. According to a molar ratio of 1:1 to 5, the iron salt and the surface modification material are dissolved in deoxygenated ethanol to prepare a mixed solution of 20 g / L of the iron salt and the surface modification material; S2. Weigh the reducing agent and dissolve it in the deoxygenated ethanol, and add ethylenediamine to the reducing agent in a molar ratio of 10 to 20:1 to prepare a mixed solution; S3. According to the molar ratio of iron salt to reducing agent of 1:2~3, under the protection of nitrogen atmosphere and high-speed mechanical stirring, the mixed solution of step S2 is added dropwise to the mixed solution of step S1. After the addition is completed, the reaction is continued with stirring for 10~30 min to obtain a superparamagnetic nano iron material.
2. Use of the superparamagnetic nano-iron material according to claim 1 in environmental remediation.
3. A method for preparing superparamagnetic nano-iron according to claim 1, characterized in that: The following steps are involved: S1. According to a molar ratio of 1:1 to 5, the iron salt and the surface modification material are dissolved in deoxygenated ethanol to prepare a mixed solution of 20 g / L of the iron salt and the surface modification material; S2. Weigh the reducing agent and dissolve it in the deoxygenated ethanol, and add ethylenediamine to the reducing agent in a molar ratio of 10 to 20:1 to prepare a mixed solution; S3. According to the molar ratio of iron salt to reducing agent of 1:2~3, under the protection of nitrogen atmosphere and high-speed mechanical stirring, the mixed solution of step S2 is added dropwise to the mixed solution of step S1. After the addition is completed, the reaction is continued with stirring for 10~30 min to obtain a superparamagnetic nano iron material.
4. The method for preparing a superparamagnetic nano-iron material according to claim 3, characterized in that: The iron salt is selected from one or more of ferric chloride, ferrous chloride, ferrous sulfate, ferrous carbonate, ferrous acetate, ferrous citrate, ammonium ferrous sulfate, ferrous oxalate, and iron sulfide.
5. The method for preparing a superparamagnetic nano-iron material according to claim 3, characterized in that: The surface modification material is selected from one or more of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, hexadecyl ammonium bromide, carboxymethyl cellulose, polyvinyl pyrrolidone, polyvinyl alcohol, polyacrylic acid, polyacrylamide, polylysine, guar gum, and rhamnolipid.
6. The method for preparing a superparamagnetic nano-iron material according to claim 3, characterized in that: The reducing agent is selected from one or more of sodium dithionite, thiourea dioxide, hydrazine hydrate, sodium borohydride and potassium borohydride.
7. A method for preparing a superparamagnetic nano-iron composite material, characterized in that: To the mixed solution of the iron salt and the surface modification material in step S1 of any one of claims 3 to 6, the doped composite material is added in a ratio of 1:0.001 to 100 by mass of iron to the doped composite material.
8. The method for preparing a superparamagnetic nano-iron composite material according to claim 7, characterized in that: The doped composite material is selected from one or more of metal salts, carbon materials, sulfur materials, metal oxides, metal hydroxides, natural fibers and natural mineral materials.
9. A superparamagnetic nano-iron composite material prepared by the preparation method according to claim 7.
10. Use of the superparamagnetic nano-iron composite material according to claim 9 in environmental remediation.
Citation Information
Patent Citations
Synthetic method of hydrophilic monodisperse carboxyl superparamagnetic microsphere
CN101353181A
Silica micropowder loaded type nano zerovalent iron particle and preparation method thereof
CN101941068A
A nano-sized zero-valent iron stable in air and its preparation method
CN102284706A
Preparation method of attapulgite-loaded nanometre iron material
CN102755883A
Rapid preparation method of novel stable nano zero-valent iron particle
CN102861925A