High-entropy oxide and preparation method and application thereof
Through PVP templateization and freeze-drying technology, the high-entropy oxide FeCoMnCuCrOx catalyst is prepared at low temperature, which solves the problem of high-temperature preparation limitations in the existing technology, achieves high stability and high catalytic activity, has high selectivity for hydrogen sulfide, and improves the Economic benefits.
Patent Information
- Application Number
- CN202410926846.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-22
AI Technical Summary
The existing synthesis methods of high-entropy oxide materials are limited by high temperature and professional equipment, and it is difficult to prepare at low temperature and efficiently, resulting in a decrease in stability of the catalyst and the occurrence of secondary pollution during the hydrogen sulfide purification process.
Using PVP template method and freeze-drying technology, a high-entropy oxide FeCoMnCuCrOx catalyst was prepared by lyophilizing liquid nitrogen and calcining at 400-500°C to form a two-dimensional stable structure, with high catalytic oxidation activity and high selectivity.
It realizes the efficient preparation of high-entropy oxide catalysts at low temperatures, maintains high stability and high catalytic activity, has high selectivity for hydrogen sulfide, avoids the decline in stability caused by long-term use, and improves economic benefits.
Smart Images

Figure CN118988338A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of high entropy oxide material preparation, and in particular relates to a high entropy oxide and a preparation method and application thereof. Background Art
[0002] Metal oxide catalysts have excellent catalytic oxidation activity in the field of sulfur-containing pollutants, especially hydrogen sulfide purification. However, high temperature conditions during the catalytic oxidation of hydrogen sulfide will lead to the generation of secondary pollution. At the same time, the interaction between sulfur and metal often leads to catalyst poisoning and deactivation, resulting in a trend of decreased stability.
[0003] In recent years, as technology continues to advance and applications become more specialized, the demand for materials with new functionalities and properties that meet specific requirements has increased. To meet this demand, a strategy has been proposed to increase the chemical complexity of materials beyond the current state of the art, resulting in a new class of materials known as high-entropy materials. High-entropy materials consist of many different elements in a single-phase crystal structure, opening up a huge chemical parameter space with an almost infinite number of element combinations. This versatility allows compounds to meet specific needs and be tailored to the desired properties and applications, improving the quality and functionality of materials in a sustainable way.
[0004] At present, high entropy materials, especially high entropy oxide materials, have been gradually applied in the fields of energy, electronics, catalysis, etc. However, existing methods for synthesizing high entropy oxide materials, such as carbon thermal shock technology and rapid moving bed pyrolysis technology, are limited by high temperature (usually >1000°C), professional equipment and cumbersome procedures. Therefore, it is urgent to develop a low-temperature and simple method for preparing high entropy oxide catalysts for low-temperature, high-selectivity and high-stability removal of hydrogen sulfide (H2S). Summary of the invention
[0005] In order to solve the above technical problems, the present invention proposes a high entropy oxide and a preparation method and application thereof.
[0006] To achieve the above object, the present invention provides a high entropy oxide (FeCoMnCuCrO x A method for preparing a high entropy oxide (HEO) comprises the following steps:
[0007] Dissolving PVP in water to obtain a PVP solution, adding a soluble metal salt to the PVP solution and stirring evenly to obtain a mixed solution, dropping the mixed solution into liquid nitrogen for freeze drying, and then calcining to obtain the high entropy oxide;
[0008] The soluble metal salts include soluble iron salts, cobalt salts, manganese salts, copper salts and chromium salts.
[0009] Furthermore, the molar ratio of the soluble iron salt, cobalt salt, manganese salt, copper salt and chromium salt is 1:1:1:1:1.
[0010] Furthermore, the soluble iron salt is ferric nitrate, the soluble cobalt salt is cobalt nitrate, the soluble manganese salt is manganese nitrate, the soluble copper salt is one or more of copper nitrate, copper sulfate and copper acetate, and the soluble chromium salt is chromium nitrate.
[0011] Furthermore, the soluble iron salt is ferric nitrate nonahydrate, the soluble cobalt salt is cobalt nitrate hexahydrate, the soluble manganese salt is manganese nitrate tetrahydrate, the soluble copper salt is one or more of copper nitrate trihydrate, copper sulfate pentahydrate and copper acetate monohydrate, and the soluble chromium salt is chromium nitrate nonahydrate.
[0012] Furthermore, the usage ratio of the PVP to the soluble iron salt is 4g:2.02g.
[0013] Furthermore, the mass ratio of the PVP to water is (0.1-0.2):1.
[0014] Furthermore, the freeze-drying time is 36-72 hours.
[0015] Furthermore, the calcination temperature is 400-500°C, the calcination time is 5-8h, and the heating rate is 1-5°C / min.
[0016] Furthermore, the stirring speed is 40-80 rpm, and the stirring time is 30-90 min.
[0017] The present invention also proposes a high entropy oxide prepared by the preparation method, which has a two-dimensional stable structure.
[0018] The present invention also proposes the application of the high entropy oxide in the selective catalytic oxidation of H2S.
[0019] Furthermore, the temperature at which the high entropy oxide selectively catalyzes the oxidation of H2S is room temperature.
[0020] Compared with the prior art, the present invention has the following advantages and technical effects:
[0021] Existing high entropy oxide material synthesis methods, such as carbon thermal shock technology and fast moving bed pyrolysis technology, are limited by high temperature (usually >1000°C), professional equipment and cumbersome procedures. The present invention realizes the preparation of low-temperature and efficient high entropy oxide catalysts by combining a simple PVP template method with freeze-drying technology. In addition, by calcining at 400-500°C, the formation of a high-stability structure of the high entropy oxide catalyst can be achieved. The prepared high entropy oxide catalyst has high catalytic oxidation activity and high S (elemental sulfur) selectivity for hydrogen sulfide gas, and will not cause a decrease in stability due to long-term testing, thereby improving the economic benefits of the high entropy oxide catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0023] Figure 1 The FeCoMnCuCrO prepared in Example 1 x Scanning electron microscopy (SEM) image (a) and element distribution map (b) of the high entropy oxide catalyst;
[0024] Figure 2 The FeCoMnCuCrO prepared in Example 1 x X-ray diffraction (XRD) spectrum of high entropy oxide catalyst;
[0025] Figure 3 It is a comparison chart of the activities of high entropy oxide catalysts prepared by the empty tube group, Example 1, Example 2, Example 3 and Comparative Examples 1-8;
[0026] Figure 4 FeCoMnCuCrO prepared in Example 1, Example 2 and Example 3 x Stability test results of high entropy oxide catalysts. DETAILED DESCRIPTION
[0027] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0028] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0029] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0030] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0031] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0032] The embodiment of the present invention provides a high entropy oxide (FeCoMnCuCrO x A method for preparing a high entropy oxide (HEO) comprises the following steps:
[0033] Dissolving PVP (polyvinyl pyrrolidone) in water to obtain a PVP solution, adding a soluble metal salt to the PVP solution and stirring evenly to obtain a mixed solution, dropping the mixed solution into liquid nitrogen for freeze drying, and then calcining to obtain the high entropy oxide;
[0034] The soluble metal salts include soluble iron salts, cobalt salts, manganese salts, copper salts and chromium salts. The high entropy oxides formed by the five metals are spinel structures. The stable spinel structures have good catalytic oxidation activity and stability of H2S. Replacing or reducing the metal salts will result in the inability to form a catalyst with a stable spinel structure, which is not conducive to the catalytic oxidation removal of H2S.
[0035] In a preferred embodiment of the present invention, the molar ratio of the soluble iron salt, cobalt salt, manganese salt, copper salt and chromium salt is 1:1:1:1:1. This ratio is selected because statistical thermodynamics shows that the more microscopic states and microscopic components there are in the system, the higher the entropy value, and for high entropy oxides, when the atomic percentages of all components in the system are equal, the entire system reaches the maximum configuration entropy. At this time, the prepared high entropy oxide catalyst is an entropy-stabilized oxide, which is conducive to the catalytic oxidation removal of H2S.
[0036] In a preferred embodiment of the present invention, the soluble iron salt is ferric nitrate, the soluble cobalt salt is cobalt nitrate, the soluble manganese salt is manganese nitrate, the soluble copper salt is one or more of copper nitrate, copper sulfate and copper acetate, and the soluble chromium salt is chromium nitrate. More preferably, the soluble iron salt is ferric nitrate nonahydrate, the soluble cobalt salt is cobalt nitrate hexahydrate, the soluble manganese salt is manganese nitrate tetrahydrate, the soluble copper salt is one or more of copper nitrate trihydrate, copper sulfate pentahydrate and copper acetate monohydrate, and the soluble chromium salt is chromium nitrate nonahydrate.
[0037] In a preferred embodiment of the present invention, the usage ratio of the PVP to the soluble iron salt is 4g:2.02g.
[0038] In a preferred embodiment of the present invention, the mass ratio of the PVP to water is (0.1-0.2):1, and the weight of 1 mL of deionized water is 1 g.
[0039] In a preferred embodiment of the present invention, the freeze drying time is 36-72 hours. The freeze drying process uses liquid nitrogen to synthesize high entropy oxide catalysts at low temperature, which can effectively prevent the aggregation of particles. At the same time, this method can maintain the original spatial structure of the oxide. Moreover, the product prepared by the freeze drying method generally has a higher specific surface area and catalytic activity. Another purpose of freeze drying is to remove the solvent water used to disperse the metal salts, thereby facilitating the subsequent calcination process.
[0040] In a preferred embodiment of the present invention, the calcination temperature is 400-500°C, the calcination time is 5-8h, and the heating rate is 1-5°C / min. The purpose of calcination is to remove nitrates in the mixed phase to form a uniformly dispersed high entropy metal oxide. This step is conducive to the formation of a spinel structure, thereby enhancing the activity and stability of the catalyst.
[0041] In a preferred embodiment of the present invention, the stirring speed is 40-80 rpm, and the stirring time is 30-90 min.
[0042] The embodiment of the present invention also provides a high entropy oxide prepared by the preparation method, which has a two-dimensional stable structure.
[0043] The embodiment of the present invention also proposes the application of the high entropy oxide in the selective catalytic oxidation of H2S.
[0044] In a preferred embodiment of the present invention, the temperature for the high entropy oxide to selectively catalyze the oxidation of H2S is room temperature.
[0045] In a preferred embodiment of the present invention, room temperature refers to "25±2°C".
[0046] The technical solution of the present invention is further illustrated by the following embodiments.
[0047] Example 1
[0048] (1) Take 4 g of PVP in a beaker, add 25 mL of deionized water and fully dissolve it under the action of a magnetic stirrer to obtain a PVP solution;
[0049] (2) Weigh equal moles of soluble metal nitrates: 2.02 g Fe(NO3)3·9H2O, 1.765 g Co(NO3)3·6H2O, 1.255 g Mn(NO3)2·4H2O, 1.208 g Cu(NO3)2·3H2O, 2 g Cr(NO3)3·9H2O, dissolve them in the above PVP solution and continue stirring at 60 rpm for 30 min to obtain a mixed solution;
[0050] (3) Take another beaker and wrap it with tin foil to keep it warm. Pour 50 mL of liquid nitrogen into it. Use a rubber-tipped dropper to draw the mixed solution prepared above and slowly add it dropwise into the liquid nitrogen. After it is fully solidified, freeze-dry it for 48 hours to remove water.
[0051] (4) The dried solid was placed in a muffle furnace and calcined at 450°C (heating rate 1°C / min) for 6 h to obtain FeCoMnCuCrO x The high entropy oxide catalyst is denoted as FeCoMnCuCr (FD-Example 1).
[0052] FeCoMnCuCrO prepared in Example 1 of the present invention x The scanning transmission electron microscopy (SEM) image (a) and element distribution map (b) of the high entropy oxide catalyst are shown in Figure 1 , X-ray diffraction spectrum (XRD) diagram is shown in Figure 2 ,Depend on Figure 1-2 It can be seen that FeCoMnCuCrO was successfully synthesized in Example 1 of the present invention. x High entropy oxide catalyst. SEM results show that the synthesized high entropy oxide catalyst has an obvious two-dimensional flake structure, and XRD results show that a high entropy oxide catalyst with a spinel configuration is synthesized.
[0053] Comparative Example 1
[0054] The same as Example 1, except that in step (2), the molar ratio of Fe(NO3)3·9H2O, Co(NO3)3·6H2O, Mn(NO3)2·4H2O, Cu(NO3)2·3H2O and Cr(NO3)3·9H2O is 0.5:1.125:1.125:1.125:1.125, specifically: weigh 1.01g Fe(NO3)3·9H2O, 1.99g Co(NO3)3·6H2O, 1.411g Mn(NO3)2·4H2O, 1.359g Cu(NO3)2·3H2O, and 2.25g Cr(NO3)3·9H2O, and the obtained high entropy oxide is recorded as FeCoMnCuCr (comparative sample 1).
[0055] Comparative Example 2
[0056] The same as Example 1, the only difference is that the type of soluble metal salt in step (2) is different, specifically: weigh 1.45g Ni(NO3)2·6H2O, 1.765g Co(NO3)3·6H2O, 1.255g Mn(NO3)2·4H2O, 1.208g Cu(NO3)2·3H2O, and 2g Cr(NO3)3·9H2O, and the obtained high entropy oxide is recorded as NiCoMnCuCr (comparative sample 2).
[0057] Comparative Example 3
[0058] The same as Example 1, except that in step (2), the molar ratio of Fe(NO3)3·9H2O, Co(NO3)3·6H2O, Mn(NO3)2·4H2O, Cu(NO3)2·3H2O and Cr(NO3)3·9H2O is 1.125:1.125:1.125:1.125:0.5, specifically: weigh 2.27g Fe(NO3)3·9H2O, 1.99g Co(NO3)3·6H2O, 1.411g Mn(NO3)2·4H2O, 1.359g Cu(NO3)2·3H2O, and 1g Cr(NO3)3·9H2O, and the obtained high entropy oxide is recorded as FeCoMnCuCr (comparative sample 3).
[0059] Example 2
[0060] (1) Take 4 g of PVP in a beaker, add 40 mL of deionized water and fully dissolve it under the action of a magnetic stirrer to obtain a PVP solution;
[0061] (2) Weigh equal moles of soluble metal nitrates: 2.02 g Fe(NO3)3·9H2O, 1.765 g Co(NO3)3·6H2O, 1.255 g Mn(NO3)2·4H2O, 1.208 g Cu(NO3)2·3H2O, 2 g Cr(NO3)3·9H2O, dissolve them in the above PVP solution and continue stirring at 80 rpm for 50 min to obtain a mixed solution;
[0062] (3) Take another beaker and wrap it with tin foil to keep it warm. Pour 50 mL of liquid nitrogen into it. Use a rubber-tipped dropper to draw the mixed solution prepared above and slowly add it dropwise into the liquid nitrogen. After it is fully solidified, freeze-dry it for 72 hours to remove water.
[0063] (4) The dried solid was placed in a muffle furnace and calcined at 400 °C (heating rate 3 °C / min) for 8 h to obtain FeCoMnCuCrO x High entropy oxide catalyst (FD-Example 2).
[0064] Example 3
[0065] (1) Take 4 g of PVP in a beaker, add 20 mL of deionized water and fully dissolve it under the action of a magnetic stirrer to obtain a PVP solution;
[0066] (2) Weigh equal moles of soluble metal nitrates: 2.02 g Fe(NO3)3·9H2O, 1.765 g Co(NO3)3·6H2O, 1.255 g Mn(NO3)2·4H2O, 1.208 g Cu(NO3)2·3H2O, 2 g Cr(NO3)3·9H2O, dissolve them in the above PVP solution and continue stirring at 40 rpm for 90 min to obtain a mixed solution;
[0067] (3) Take another beaker and wrap it with tin foil to keep it warm. Pour 50 mL of liquid nitrogen into it. Use a rubber-tipped dropper to draw the mixed solution prepared above and slowly add it dropwise into the liquid nitrogen. After it is fully solidified, freeze-dry it for 36 hours to remove water.
[0068] (4) The dried solid was placed in a muffle furnace and calcined at 500°C (heating rate 5°C / min) for 5 h to obtain FeCoMnCuCrO x High entropy oxide catalyst (FD-Example 3).
[0069] Comparative Example 4
[0070] The same as Example 1, except that the calcination step in step (4) is omitted, specifically:
[0071] (1) Take 4 g of PVP in a beaker, add 25 mL of deionized water and fully dissolve it under the action of a magnetic stirrer to obtain a PVP solution;
[0072] (2) Weigh equal moles of soluble metal nitrates: 2.02 g Fe(NO3)3·9H2O, 1.765 g Co(NO3)3·6H2O, 1.255 g Mn(NO3)2·4H2O, 1.208 g Cu(NO3)2·3H2O, 2 g Cr(NO3)3·9H2O, dissolve them in the above PVP solution and continue stirring at 60 rpm for 30 min to obtain a mixed solution;
[0073] (3) Take another beaker, wrap it with tin foil to keep it warm, pour in 50 mL of liquid nitrogen, use a rubber-tipped dropper to draw the mixed solution prepared above, and slowly drop it into the liquid nitrogen. After it is fully solidified, freeze-dry it for 48 hours to remove water, and obtain FeCoMnCuCrO x High entropy oxide catalyst (Comparative Sample 4).
[0074] Comparative Example 5
[0075] The same as Example 1, except that the freeze-drying time was 24 h to obtain FeCoMnCuCrO x High entropy oxide catalyst (Comparative Sample 5).
[0076] Comparative Example 6
[0077] The same as Example 1, except that the dried solid was placed in a muffle furnace and calcined at 700°C to obtain FeCoMnCuCrO x High entropy oxide catalyst (Comparative Sample 6).
[0078] Comparative Example 7
[0079] The same as Example 1, the only difference is that the addition of Fe(NO3)3·9H2O is omitted, specifically:
[0080] (1) Take 4 g of PVP in a beaker, add 25 mL of deionized water and fully dissolve it under the action of a magnetic stirrer to obtain a PVP solution;
[0081] (2) Weigh equal moles of soluble metal nitrates: 1.765 g Co(NO3)3·6H2O, 1.255 g Mn(NO3)2·4H2O, 1.208 g Cu(NO3)2·3H2O, 2 g Cr(NO3)3·9H2O, dissolve in the above PVP solution and continue stirring at 60 rpm for 30 min to obtain a mixed solution;
[0082] (3) Take another beaker and wrap it with tin foil to keep it warm. Pour 50 mL of liquid nitrogen into it. Use a rubber-tipped dropper to draw the mixed solution prepared above and slowly add it dropwise into the liquid nitrogen. After it is fully solidified, freeze-dry it for 48 hours to remove water.
[0083] (4) The dried solid was placed in a muffle furnace and calcined at 450°C (heating rate 1°C / min) for 6 h to obtain CoMnCuCrO x High entropy oxide catalyst (Comparative Sample 7).
[0084] Comparative Example 8
[0085] The same as Example 1, the only difference is that the addition of Cr(NO3)3·9H2O is omitted, specifically:
[0086] (1) Take 4 g of PVP in a beaker, add 25 mL of deionized water and fully dissolve it under the action of a magnetic stirrer to obtain a PVP solution;
[0087] (2) Weigh equal moles of soluble metal nitrates: 2.02 g Fe(NO3)3·9H2O, 1.765 g Co(NO3)3·6H2O, 1.255 g Mn(NO3)2·4H2O, 1.208 g Cu(NO3)2·3H2O, dissolve them in the above PVP solution and continue stirring at 60 rpm for 30 min to obtain a mixed solution;
[0088] (3) Take another beaker and wrap it with tin foil to keep it warm. Pour 50 mL of liquid nitrogen into it. Use a rubber-tipped dropper to draw the mixed solution prepared above and slowly add it dropwise into the liquid nitrogen. After it is fully solidified, freeze-dry it for 48 hours to remove water.
[0089] (4) The dried solid was placed in a muffle furnace and calcined at 450°C (heating rate 1°C / min) for 6 h to obtain FeCoMnCuO x High entropy oxide catalyst (Comparative Sample 8).
[0090] Performance test of H2S selective catalytic combustion over high entropy oxide catalysts
[0091] Under atmospheric pressure, 100 mg of the high entropy oxide catalyst prepared in Examples 1-3 and Comparative Examples 1-8 were added to a tubular quartz reactor with a diameter of 5 mm, and a gas with a flow rate of 100 mL / min and a gas space velocity (SV) of 60,000 ml / g / h was introduced, and the gas consisted of 500 ppm H2S, 1% O2 and N2 in balance; heated from 25°C to 125°C (the heating rate was 5°C / min; the interval was 25°C / section), and each temperature section was kept warm for 30 minutes. The H2S stability test selected the temperature with the best elemental sulfur selectivity, i.e., 25°C, for testing, the test atmosphere was consistent with the activity test conditions, and the test time was 12 hours.
[0092] Another control group was set up, in which no high entropy oxide catalyst was added to the tubular quartz reactor, and other conditions were the same as the above conditions, and was recorded as the empty tube group.
[0093] The activity comparison diagram of the high entropy oxide catalysts prepared by the empty tube group, Examples 1-3 and Comparative Examples 1-8 is shown in Figure 3 ,from Figure 3 It can be seen that the high entropy oxide catalyst obtained when the molar ratio of the soluble metal salt in the embodiment is 1:1:1:1:1 shows excellent catalytic oxidation activity.
[0094] FeCoMnCuCrO prepared in Example 1-3 x The stability test results of high entropy oxide catalysts are shown in Figure 4 ,Depend on Figure 4 It can be seen that the FeCoMnCuCrO prepared in the embodiment of the present invention x The high entropy oxide catalyst can maintain a H2S conversion rate of more than 90% after 12 hours at 25°C, showing excellent stability.
[0095] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for preparing a high entropy oxide, It is characterized in that The following steps are involved: Dissolving PVP in water to obtain a PVP solution, adding a soluble metal salt to the PVP solution and stirring evenly to obtain a mixed solution, dropping the mixed solution into liquid nitrogen for freeze drying, and then calcining to obtain the high entropy oxide; The soluble metal salts include soluble iron salts, cobalt salts, manganese salts, copper salts and chromium salts.
2. The method for preparing a high entropy oxide according to claim 1, It is characterized in that The molar ratio of the soluble iron salt, cobalt salt, manganese salt, copper salt and chromium salt is 1:1:1:1:
1.
3. The method for preparing a high entropy oxide according to claim 2, It is characterized in that The soluble iron salt is ferric nitrate, the soluble cobalt salt is cobalt nitrate, the soluble manganese salt is manganese nitrate, the soluble copper salt is one or more of copper nitrate, copper sulfate and copper acetate, and the soluble chromium salt is chromium nitrate.
4. The method for preparing a high entropy oxide according to claim 1, It is characterized in that The usage ratio of the PVP to the soluble iron salt is 4g:2.02g.
5. The method for preparing a high entropy oxide according to claim 1, It is characterized in that The mass ratio of the PVP to water is (0.1-0.2):
1.
6. The method for preparing a high entropy oxide according to claim 1, It is characterized in that The freeze-drying time is 36-72h.
7. The method for preparing a high entropy oxide according to claim 1, It is characterized in that The calcination temperature is 400-500°C, the calcination time is 5-8h, and the heating rate is 1-5°C / min.
8. A high entropy oxide prepared by the preparation method according to any one of claims 1 to 7.
9. The high entropy oxide as claimed in claim 8 in H 2 Application in the selective catalytic oxidation of S.
10. According to claim 9, the high entropy oxide in H 2 Application in selective catalytic oxidation of S, It is characterized in that The high entropy oxide selectively catalyzes the oxidation of H 2 The temperature of S is room temperature.
Citation Information
Patent Citations
Preparation method of Fe-doped magnesium aluminate spinel catalyst and application of Fe-doped magnesium aluminate spinel catalyst in field of desulfurization
CN112517008A
Low-temperature preparation method and application of high-entropy two-dimensional catalyst
CN114950475A
Method for solvent-free synthesis of transition metal functionalized ordered mesoporous silica
CN118255359A
Process for selective oxidation of hydrogen sulfide to elemental sulfur
US5891415A
Method for the direct high-selectivity catalytic oxidative conversion of a low concentration of h2s in a gas into sulphur, and catalyst therefor
WO1994021358A1
Cited By
Preparation method of high-entropy material as well as product and application of high-entropy material
CN119819319A