A 3D printed high-load zinc ion battery electrode and preparation method thereof

The three-dimensional structural electrodes of NHCFs and PVO materials were prepared through extruded 3D printing technology, which solved the problem of low load of traditional electrodes, achieved high load and high specific capacity, and improved the performance of zinc ion batteries.

CN115148965BActive Publication Date: 2024-11-01HUNAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210542770.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-18
Publication Date
2024-11-01
Estimated Expiration
2042-05-18

AI Technical Summary

Technical Problem

Traditional zinc ion batteries have low electrode loads, making it difficult to meet the demand for high performance of new energy storage batteries.

Method used

Extruded 3D printing technology is used to prepare three-dimensional structural electrodes of NHCFs and PVO materials, and through specific chemical reactions and treatment steps, electrodes with high load and high specific capacity are formed.

Benefits of technology

The high load capacity and high specific capacity of zinc ion battery electrodes are achieved, which improves the transmission efficiency of ions and electrons and improves the performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115148965B_ABST
    Figure CN115148965B_ABST
Patent Text Reader

Abstract

The present invention provides a 3D printed high-load zinc ion battery electrode and a preparation method thereof, the method comprising the following steps: preparing polypyrrole, annealing in a nitrogen atmosphere to obtain nitrogen-doped hollow carbon nanotubes NHCFs; adding V2O5 and aniline, adjusting the pH value with hydrochloric acid, and obtaining NHCFs / PVO material through hydrothermal reaction; mixing with a conductive additive, an adhesive, and a solvent to obtain NHCFs / PVO ink; transferring the ink to a syringe, installing it on a 3D printing device, designing a three-dimensional structure and importing it into the printing device, setting relevant parameters and printing to obtain an NHCFs / PVO electrode. The electrode obtained by the present invention is a three-dimensional structure with a large porosity, which is conducive to the transmission and transportation of ions and electrons. Compared with the zinc ion battery positive electrode obtained by the prior art, the NHCFs / PVO electrode has the advantages of high load and high specific capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of zinc ion batteries, and in particular to a 3D printed high-load zinc ion battery electrode and a preparation method thereof. Background Art

[0002] In today's society, electronic devices such as wearable devices and electric vehicles are developing rapidly. In order to ensure the stable operation and long-term operation of these electronic devices, people's demand for new energy storage batteries is becoming more and more significant. Different from the previous lithium-ion batteries with long manufacturing cycles, high production costs and many safety issues, zinc-ion batteries have a safe preparation process, high discharge capacity and are environmentally friendly, becoming an important direction for new energy storage batteries.

[0003] The performance of zinc-ion batteries is closely related to the electrodes they use. In order to improve the performance of electrodes, in addition to innovations in electrode materials, advanced manufacturing technologies can also be used. Electrodes made using traditional electrode preparation technologies often have very low loading capacity. 3D printing technology, as an emerging technology, can be used to manufacture energy storage batteries with excellent loading capacity and discharge specific capacity because it can construct three-dimensional structures that are conducive to carrier transport. Summary of the invention

[0004] In view of this, the purpose of the present invention is to use extrusion 3D printing to prepare a three-dimensional structure electrode with high loading and high specific capacity for application in zinc ion batteries.

[0005] In order to achieve the above object, the technical solution of the present invention is as follows:

[0006] A 3D printed high-load zinc ion battery electrode, characterized in that the main components of the electrode are NHCFs and PVO, and the ratio of NHCFs to PVO is 1:3 or 2:3.

[0007] A method for preparing a 3D printed high-load zinc ion battery electrode, characterized in that it comprises the following steps:

[0008] 1) adding pyrrole monomer to a mixed solution of methyl orange and ferric chloride and stirring to obtain polypyrrole, and annealing in a nitrogen atmosphere to obtain nitrogen-doped hollow carbon nanotubes NHCFs;

[0009] 2) dissolving the NHCFs obtained in step 1) and V2O5 into a mixed solution, then adding aniline and hydrochloric acid in sequence, transferring to an autoclave for heat preservation, then placing in an oven for heating, and finally washing and drying to obtain NHCFs / PVO material;

[0010] 3) mixing the material obtained in step 2) with a conductive additive, a binder, and a solvent to obtain NHCFs / PVO ink;

[0011] 4) The ink obtained in step 3) is transferred into a syringe, installed on a 3D printing device, a three-dimensional structure is designed and imported into the printing device, relevant parameters are set and printing is performed to obtain a NHCFs / PVO electrode.

[0012] Furthermore, in the above step 1), in the mixed solution of methyl orange and ferric chloride, the mass ratio of methyl orange to ferric chloride is 1:5; the stirring time is 24-36h, and the temperature is 20-30°C.

[0013] Furthermore, in the above step 1), after obtaining the polypyrrole, it is necessary to wash with deionized water, filter 5-8 times, and then dry. The drying time is 72-84 hours and the drying temperature is 60-70°C.

[0014] Furthermore, in the above step 1), the annealing temperature in a nitrogen atmosphere is 700-900° C., and the annealing time is 2-3 hours.

[0015] Furthermore, in the above step 2), the mass ratio of NHCFs to V2O5 is 3:1, the aniline is added in an appropriate amount, and the hydrochloric acid is added to adjust the pH to 2.5.

[0016] Furthermore, in the above step 2), the aniline and hydrochloric acid are added successively and then stirred vigorously for 20-30 minutes.

[0017] Furthermore, in the above step 2), the temperature of the oven heating is 100-120°C, and the heating time is 24-36h; the specific step of washing is washing with anhydrous ethanol and deionized water until the supernatant is clear, the drying temperature is 50-70°C, and the drying time is 48-72h.

[0018] Furthermore, in the above step 3), the mass ratio of the material to the conductive aid and the adhesive is 8:1:1, the conductive aid is a conductive carbon material such as carbon nanotubes, graphene or carbon black, the adhesive is one of polyvinylidene fluoride or sodium carboxymethyl cellulose, and the solvent is N-methylpyrrolidone.

[0019] Furthermore, in the above step 4), the three-dimensional structure is a woodpile-like structure, and the relevant parameters include a printing height of 0.3-0.4 mm and a moving speed of 4-8 mm·s -1 .

[0020] Compared with the prior art, the present invention has the following advantages:

[0021] 1. The 3D printed high-load zinc-ion battery electrode obtained by this method has a large porosity, which is conducive to the transmission and transportation of ions and electrons.

[0022] 2. The 3D printed high-load zinc-ion battery electrode obtained by this method has the advantages of high loading capacity and high specific capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to make the content of the present invention clearer, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which:

[0024] Figure 1 This is an implementation roadmap for a 3D printed high-load zinc ion battery electrode and a preparation method thereof provided by the present invention; wherein 1 is nitrogen-doped hollow carbon nanotube NHCFs, 2 is NHCFs / PVO material, 3 is NHCFs / PVO ink, and 4 is NHCFs / PVO electrode.

[0025] Figure 2 This is a physical photo of the 3D printed high-load zinc ion battery electrode prepared in Example 1 of the present invention.

[0026] Figure 3 This is a scanning electron microscope photograph of the 3D printed high-load zinc ion battery electrode prepared in Example 1 of the present invention.

[0027] Figure 4 The 3D printed high-load zinc ion battery electrode prepared in Example 1 of the present invention is -1 Cyclic performance test diagram at current density. DETAILED DESCRIPTION

[0028] The technical scheme in the embodiment of the present invention will be described in detail below in conjunction with the accompanying drawings in the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. Based on the embodiment of the present invention, all other embodiments implemented by those skilled in the art without creative work are within the protection scope of the present invention.

[0029] Example 1

[0030] The embodiment of the present invention provides a 3D printed high-load zinc ion battery electrode and a preparation method thereof, Figure 1 As shown, the following steps are included:

[0031] 1. Using polypyrrole as a precursor, nitrogen-doped hollow carbon nanotubes were synthesized by chemical reaction. 0.78g of methyl orange and 3.89g of ferric chloride were dispersed in 482mL and 20mL of deionized water, respectively, and stirred continuously. The two solutions were then mixed and vigorously stirred at room temperature for 30 minutes, and then 0.84mL of pyrrole monomer was slowly added to the above mixture. After continuous stirring at 25°C for 24h, the obtained polypyrrole was washed with deionized water, filtered 5 times, and then dried at 60°C for 72h. Finally, the polypyrrole sample was annealed at 800°C for 2h in a nitrogen atmosphere to obtain a NHCFs sample.

[0032] 2. Preparation of NHCFs / PVO by hydrothermal reaction. First, 0.18g V2O5 and 0.06g NHCFs were dissolved in 30mL deionized water to prepare a mixed solution. After being stirred vigorously in a water bath at room temperature for 10 minutes, 60μL of aniline was added to the mixed solution and stirred vigorously for 20 minutes. Then, in order to make the pH value reach 2.5, 0.28mL of 3M hydrochloric acid was added to the lead solution and stirred vigorously for 30 minutes. The above solution was then poured into a 50mL Teflon-lined stainless steel autoclave and heated continuously at 120°C in an oven for 24h. Finally, the obtained NHCFs / PVO was washed with anhydrous ethanol and deionized water until the supernatant was clear, and dried in an oven at 60°C for 48h.

[0033] 3. Preparation of NHCFs / PVO ink. Dissolve 40 mg of polyvinylidene fluoride binder in 1000 mL of N-methylpyrrolidone solvent and stir until there are no particles and bubbles. Mix 40 mg of carbon nanotube conductive additive and 320 mg of NHCFs / PVO active material evenly, and then pour them into the above solution in batches. After vigorous stirring for 12 hours, transfer the prepared ink to a 3 ml syringe for 3D printing.

[0034] 4. 3D printing of NHCFs / PVO electrodes. Install the syringe and 0.41 mm inner diameter metal needle on a dispensing machine with a three-axis extrusion system. Use software to draw a woodpile-like structure and import it into the 3D printing device. The dispensing machine prints a woodpile-like structure on the glass substrate based on the rheological properties of the ink. The printing height is 0.34 mm and the moving speed is 5 mm·s. -1 The printed pyre-like structure was solidified and separated from the glass after being soaked in deionized water, and then freeze-dried for 8 h to obtain a self-supporting 3D printed structure.

[0035] The NHCFs / PVO electrode obtained in this embodiment has a three-dimensional structure and a large porosity, which is conducive to the transmission and transportation of ions and electrons. Compared with the zinc ion battery positive electrode obtained by the prior art, the NHCFs / PVO electrode has the advantages of high loading capacity and high specific capacity.

[0036] The above embodiments are only examples for clearly describing the present invention, and are not intended to limit specific implementation methods, and those skilled in the art should understand that the scope of the present invention includes but is not limited to the above embodiments. Various changes made to the above embodiments in other forms without departing from the spirit or basic features of the present invention are all within the scope of protection of the present invention.

Claims

1. A 3D printed high-load zinc ion battery electrode, characterized in that: The main components of the electrode are NHCFs and PVO, and the ratio of NHCFs to PVO is 1:3 or 2:3; The method for preparing the electrode comprises the following steps: 1) adding pyrrole monomer to a mixed solution of methyl orange and ferric chloride and stirring to obtain polypyrrole, and annealing in a nitrogen atmosphere to obtain nitrogen-doped hollow carbon nanotubes NHCFs; 2) dissolving the NHCFs obtained in step 1) and V2O5 into a mixed solution, then adding aniline and hydrochloric acid in sequence, transferring to an autoclave for heat preservation, then placing in an oven for heating, and finally washing and drying to obtain NHCFs / PVO material; 3) mixing the material obtained in step 2) with a conductive additive, a binder, and a solvent to obtain NHCFs / PVO ink; 4) Transfer the ink obtained in step 3) into a syringe, install it on a 3D printing device, design the three-dimensional structure into a woodpile-like structure, and import it into the printing device, set the printing height to 0.3-0.4mm, and the moving speed to 4-8mm·s -1 , and printed to obtain NHCFs / PVO electrode.

2. The method for preparing a 3D printed high-load zinc ion battery electrode according to claim 1, wherein: In the step 1), in the mixed solution of methyl orange and ferric chloride, the mass ratio of methyl orange to ferric chloride is 1:5; the stirring time is 24-36 hours, and the temperature is 20-30°C.

3. The method for preparing a 3D printed high-load zinc ion battery electrode according to claim 1, wherein: In the step 1), after obtaining the polypyrrole, it is necessary to wash with deionized water, filter 5-8 times, and then dry. The drying time is 72-84 hours and the drying temperature is 60-70°C.

4. The method for preparing a 3D printed high-load zinc ion battery electrode according to claim 1, wherein: In the step 1), the annealing temperature in the nitrogen atmosphere is 700-900° C., and the annealing time is 2-3 hours.

5. The method for preparing a 3D printed high-load zinc ion battery electrode according to claim 1, characterized in that: In the step 2), the mass ratio of NHCFs to V2O5 is 3:1, the amount of aniline added is appropriate, and the hydrochloric acid is added to adjust the pH to 2.

5.

6. The method for preparing a 3D printed high-load zinc ion battery electrode according to claim 1, characterized in that: In the step 2), the aniline and the hydrochloric acid are added successively and then stirred vigorously for 20-30 minutes.

7. The method for preparing a 3D printed high-load zinc ion battery electrode according to claim 1, characterized in that: In the step 2), the temperature of the oven heating is 100-120° C., and the heating time is 24-36 hours; the specific step of washing is washing with anhydrous ethanol and deionized water until the supernatant is clear, and the drying temperature is 50-70° C., and the drying time is 48-72 hours.

8. The method for preparing a 3D printed high-load zinc ion battery electrode according to claim 1, characterized in that: In the step 3), the mass ratio of the material to the conductive aid and the adhesive is 8:1:1, the conductive aid is a conductive carbon material such as carbon nanotubes, graphene or carbon black, the adhesive is one of polyvinylidene fluoride or sodium carboxymethyl cellulose, and the solvent is N-methylpyrrolidone.