A beer cap with good sealing effect and preparation method thereof

By using beer caps made of materials such as polypropylene and styrene-ethylene-butylene-styrene front-end copolymer, combined with specific fillers and additives, the problems of beer cap sealing and deformation under high temperature and pressure are solved, achieving excellent results. Excellent impact resistance and sealing effect to ensure the preservation quality of beer.

CN115160684BActive Publication Date: 2024-10-01CHUNTING FOOD TECH (ANHUI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111018703.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-01
Publication Date
2024-10-01
Estimated Expiration
2041-09-01

AI Technical Summary

Technical Problem

The sealing effect of beer caps on the market is not ideal, which can easily lead to air leakage and liquid leakage, and are easily deformed under high temperature and pressure, posing safety hazards and poor taste.

Method used

The seal is made of a tapered cover made of polypropylene as the main material and a styrene-ethylene-butylene-styrene front-end copolymer, combined with a specific melt flow rate and lubricants, antioxidants, fillers and filling oils. Forming excellent impact resistance and sealing effect, the integrated beer cap is prepared through a two-color injection molding machine.

Benefits of technology

It has excellent impact resistance and sealing performance at low temperatures, can withstand high pressure, and does not cause the taste of beer to deteriorate after high-temperature sterilization. The color of the seal is uniform and not easy to change color.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a beer cap with good sealing effect and a preparation method thereof, comprising a cap body and a sealing member, wherein the cap body is in a conical structure, the sealing member is fixedly connected around the conical structure, and the cap body comprises the following raw materials in parts by weight: 99-99.4 parts of polypropylene, 0.1-0.2 parts of lubricant, 0.2-0.033 parts of antioxidant, and 0.3-0.5 parts of whitening agent. The present application uses a special composition ratio of the cap body and the sealing member to obtain a beer cap with good sealing performance during actual use, and has excellent impact resistance, and can withstand greater pressure without deformation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bottle caps, in particular to IPC classification number B65D41 / 32, and more particularly to a beer cap with good sealing effect and a preparation method thereof. Background Art

[0002] Conventional beer caps on the market are generally made of iron sheets. When opening the cap, it is necessary to use a matching opener, and sometimes other tools such as chopsticks, lighters, etc. are used to open the bottle cap. In this process, the glass bottle mouth is easily damaged, which poses certain safety risks. For this reason, a new type of beer bottle cap-swing cap has been developed on the market, which can be more convenient for people to operate and increase the safety of operation. However, the sealing effect of some swing caps on the market is not ideal, which easily leads to problems such as air leakage and liquid leakage, and beer is usually sterilized at high temperature after canning, and the cover body is prone to deformation under high temperature and high pressure. Chinese patent CN204606527U discloses a snap-on beer bottle cap, which does not need to use a bottle opener and is made of food-grade plastic, thereby avoiding damage to the bottle mouth and reducing safety hazards, but the patent does not solve the problem of easy deformation under high temperature and high pressure. Summary of the invention

[0003] In response to the above-mentioned technical problems, on the one hand, the present invention provides a beer cap with good sealing effect, including a cap body and a sealing member, wherein the cap body is a conical structure, and the sealing member is fixedly connected around the conical structure, and the cap body includes the following raw materials in parts by weight: 99-99.4 parts of polypropylene, 0.1-0.2 parts of lubricant, 0.2-0.033 parts of antioxidant, and 0.3-0.5 parts of whitening agent.

[0004] In some embodiments, the polypropylene has a melt index of 18-22 g / 10 min and a Vicat softening point of 150-160°C.

[0005] Preferably, the polypropylene has a melt index of 20 g / 10 min and a Vicat softening point of 156°C.

[0006] The melt index is tested according to ASTM D-1238 standard, and the Vicat softening point is tested according to ASTM D-1525 standard.

[0007] More preferably, the polypropylene is purchased from LG Chemical (Guangzhou) Engineering Plastics Co., Ltd., and the model is LG H1615 food grade.

[0008] In some embodiments, the lubricant includes at least one of ethylene bisstearamide, oleamide, fatty acid amide, stearic acid, and stearate.

[0009] Preferably, the lubricant is oleamide.

[0010] In some embodiments, the antioxidant includes a phosphite antioxidant and / or a tert-butylphenol antioxidant.

[0011] Preferably, the antioxidant includes a phosphite antioxidant and a tert-butylphenol antioxidant.

[0012] More preferably, the antioxidant comprises antioxidant 168 and tert-butylphenol antioxidant, wherein the tert-butylphenol antioxidant accounts for 3.3-15 wt % of antioxidant 168.

[0013] Further preferably, the tert-butylphenol antioxidant includes 2-tert-butyl-p-ethylphenol.

[0014] During actual use, the applicant discovered that the cap body of the beer cap prepared by the present invention would turn yellow, thus affecting the appearance quality of the product and further affecting the sales situation. After extensive research, the applicant discovered that adding certain antioxidants to the system, especially antioxidants including antioxidant 168 and tert-butyl phenol antioxidants, wherein the tert-butyl classified antioxidant is 3.3-15wt% of antioxidant 168, can prevent the prepared cap body from changing color or fading for a long time. The applicant believes that the specific antioxidant may prevent the polypropylene molecular segments from combining with free radicals in the air and being oxidized, and can be unaffected during the long-term storage of beer.

[0015] In some embodiments, the whitening agent includes titanium dioxide.

[0016] At present, the plastic beer caps on the market are mainly made of polyolefins, and the applicant has found that the beer cap body made of a single polypropylene has poor impact resistance, especially when transporting beer in an environment with low temperature. Due to the violent shaking, the pressure inside the beer bottle is relatively high, and the cap body is prone to deformation or falling off. After a lot of research, the applicant found that the swing cap structure made of a specific material can have excellent impact resistance and sealing performance at low temperatures, and can well withstand the high pressure generated during low-temperature transportation. The applicant believes that the possible reason is that on the one hand, the polypropylene with a specific melt flow rate and softening point cooperates with the lubricant and antioxidant to form a system The fluidity during the processing is good, and at the same time, the dispersion effect of the whitening agent in the system is promoted, and the elasticity of the prepared cover is increased; on the other hand, the sealing material prepared by the special resin material improves the sealing effect between the seal and the bottle mouth, so that it has excellent impact resistance under the condition of high pressure in the bottle. The applicant believes that the possible reason is that the polypropylene with a specific melt flow rate and the styrene-ethylene-butylene-styrene front-stage copolymer are compounded in a weight ratio of (0.9-1): 1, which can form a unique sea-island structure, so that the two-phase interface forms a shear band when impacted and consumes a certain amount of energy, thereby ensuring excellent sealing and impact resistance at low temperatures.

[0017] In some embodiments, the seal comprises the following raw materials in parts by weight: 68-72 parts of resin material, 0.5-1 parts of filler, 26-30 parts of filler oil, and 0.3-1 parts of additive.

[0018] Preferably, the sealing component comprises the following raw materials in parts by weight: 70-72 parts of resin material, 0.6-0.8 parts of filler, 28-29 parts of filling oil, and 0.4-0.8 parts of additive.

[0019] In some embodiments, the raw material of the seal further includes a pigment.

[0020] In some embodiments, the resin material includes polypropylene and / or styrene-ethylene-butylene-styrene front-stage copolymer.

[0021] Preferably, the resin material includes polypropylene and styrene-ethylene-butylene-styrene front-end copolymer, and the weight ratio of the two is (0.9-1):1.

[0022] More preferably, the resin material includes polypropylene and styrene-ethylene-butylene-styrene front-end copolymer, and the weight ratio of the two is (0.91-0.97):1.

[0023] In some embodiments, the melt flow rate of the styrene-ethylene-butylene-styrene front-stage copolymer is 10-15 g / 10 min, and the specific gravity is 0.8-0.95 g / cm 3 .

[0024] Preferably, the melt flow rate of the styrene-ethylene-butylene-styrene front-stage copolymer is 12 g / 10 min, and the specific gravity is 0.86-0.9 g / cm 3 .

[0025] The melt index is tested according to ASTM D-1238 standard, and the specific gravity is tested according to ASTM D792 standard.

[0026] More preferably, the styrene-ethylene-butylene-styrene front-stage copolymer is purchased from Shanghai Yiding Plastic Co., Ltd., and the model is P3080-2 food grade.

[0027] In some embodiments, the filler includes at least one of hydrated magnesium silicate, mica powder, calcium carbonate, and white carbon black.

[0028] Preferably, the filler is hydrated magnesium silicate.

[0029] In some embodiments, the extender oil comprises white oil.

[0030] After the beer is canned, it is usually necessary to carry out high-temperature sterilization at a temperature greater than 80°C. The applicant found that although the beer cap prepared in the present application has excellent impact resistance and sealing performance at low temperatures, it will cause the taste of beer to deteriorate during the high-temperature sterilization process. The applicant speculates that the possible reason is that the stability of the polypropylene in the seal is weak under high temperature conditions, and it is easy to loosen slightly with the beer bottle, causing part of the carbon dioxide in the beer to diffuse away, and part of the oxygen in the air penetrates into the beer, which will change the state of the beer, thereby making the taste of the beer worse. After a large number of experiments, the applicant found that adding a certain proportion of filler and filler oil to this system, especially when the filler is hydrated magnesium silicate and the filler oil is white oil, can increase the sealing effect between the prepared seal and the beer bottle. The applicant speculates that the possible reason is that on the one hand, the filler oil can promote the compatibility between polypropylene and the styrene-ethylene-butylene-styrene front-stage copolymer, increase the fit between the seal and the glass wall, and at the same time, the added hydrated magnesium silicate can produce relative slip between layers under high temperature and high pressure due to its layered structure, thereby increasing the adhesion and further promoting the sealing effect at high temperature.

[0031] In some embodiments, the auxiliary agent includes one or more of a UV absorber, an antioxidant, and a lubricant.

[0032] Preferably, the auxiliary agent is a mixture of an ultraviolet absorber, an antioxidant, and a lubricant, and the weight ratio is (2-6): (1.5-5): 1.

[0033] In some embodiments, the ultraviolet absorber includes at least one of UV326, UV234, and UV531.

[0034] Preferably, the ultraviolet absorber is UV326.

[0035] In some embodiments, the antioxidant includes antioxidant 1010 and antioxidant 168 in a weight ratio of 1:(1-3).

[0036] Preferably, the antioxidant includes antioxidant 1010 and antioxidant 168 in a weight ratio of 1:2.

[0037] In some embodiments, the lubricant includes one of erucamide and oleamide.

[0038] Preferably, the lubricant is erucamide.

[0039] In order to give the seal a certain color, it is usually necessary to add certain pigments during the preparation process. However, the applicant found that there would be color unevenness in this system, and found that the seal would fade and yellow during the long-term storage of beer. The applicant found that adding specific additives to the raw materials of the seal, especially the additives being a mixture of ultraviolet absorbers, antioxidants, and lubricants in a weight ratio of (2-6): (1.5-5): 1, can make the prepared seals uniform in color and less prone to discoloration and fading. The applicant speculates that the possible reasons are that on the one hand, the addition of lubricant erucamide enhances the interaction with the resin material, drives the dispersion of the pigment, and avoids the problems of agglomeration and agglomeration. At the same time, the addition of ultraviolet absorbers and antioxidants reduces the invasion of free radicals in the environment and increases its shielding protection performance.

[0040] Another aspect of the present invention provides a method for preparing a beer cap with good sealing effect, which comprises at least the following steps: firstly, the raw material of the cap body is put into an injection molding barrel of a two-color injection molding machine for injection molding into a product, and then the mold is flipped on the two-color machine so that it jumps to the mold cavity corresponding to the other injection molding barrel for injection molding of the sealing material, thereby forming an integrated beer cap.

[0041] In some embodiments, the injection molding temperature of the cover is 180-200°C, preferably 190°C.

[0042] In some embodiments, the injection molding temperature of the seal is 130-150°C, preferably 140°C.

[0043] In some embodiments, the injection molding machine has an attack time of 20-40 seconds, a holding time of 20-30 seconds, and a cooling time of 15-25 seconds.

[0044] Preferably, the injection molding machine has an attack time of 30 seconds, a holding time of 25 seconds, and a cooling time of 20 seconds.

[0045] Beneficial effects:

[0046] (1) The swing cap structure made of a specific material of the present invention can have excellent impact resistance and sealing performance at low temperatures, and can well withstand the high pressure generated during low-temperature transportation. On the one hand, the system formed by the cooperation of polypropylene with a specific melt flow rate and softening point, lubricant and antioxidant has good fluidity during the processing process, and at the same time promotes the dispersion effect of the whitening agent in the system, thereby increasing the elasticity of the prepared cap body; on the other hand, the sealing material made of a special resin material improves the sealing effect between the sealing member and the bottle mouth, so that it has excellent impact resistance under the condition of generating a large pressure in the bottle;

[0047] (2) The present invention can improve the sealing effect between the prepared sealing member and the beer bottle by adding a certain proportion of filler and filler oil into the system, especially when the filler is hydrated magnesium silicate and the filler oil is white oil;

[0048] (3) The present invention adds specific additives to the raw materials of the seal, especially the additive is a mixture of ultraviolet absorber, antioxidant and lubricant in a weight ratio of (2-6): (1.5-5): 1, which can make the prepared seal uniform in color and not prone to discoloration and fading. DETAILED DESCRIPTION

[0049] Example 1

[0050] On the one hand, this embodiment provides a beer cap with good sealing effect, including a cap body and a sealing member, wherein the cap body is a conical structure, and the sealing member is fixedly connected around the conical structure. The cap body includes the following raw materials in parts by weight: 99.2 parts of polypropylene, 0.15 parts of lubricant, 0.23 parts of antioxidant 168, 0.02 parts of tert-butylphenol antioxidant, and 0.4 parts of whitening agent.

[0051] The polypropylene was purchased from LG Chemical (Guangzhou) Engineering Plastics Co., Ltd., and the model was LG H1615 food grade. The melt index of the polypropylene was 20 g / 10 min, and the Vicat softening point was 156° C.

[0052] The lubricant is oleamide.

[0053] The tert-butylphenol antioxidant is 2-tert-butyl-p-ethylphenol.

[0054] The whitening agent is titanium dioxide.

[0055] The sealing element comprises the following raw materials in parts by weight: 34 parts of polypropylene, 36 parts of styrene-ethylene-butylene-styrene front-stage copolymer, 0.7 parts of filler, 28 parts of filling oil, 0.6 parts of auxiliary agent and 0.7 parts of pigment.

[0056] The polypropylene was purchased from LG Chemical (Guangzhou) Engineering Plastics Co., Ltd., model LG H1615 food grade, the melt index of polypropylene was 20g / 10min, and the Vicat softening point was 156°C; the styrene-ethylene-butylene-styrene front-stage copolymer was purchased from Shanghai Yiding Plastic Co., Ltd., model P3080-2 food grade, the melt flow rate was 12g / 10min, and the specific gravity was 0.86-0.9g / cm 3 .

[0057] The filler is hydrated magnesium silicate, purchased from Shanghai Shunshui Chemical Co., Ltd.

[0058] The filler oil is white oil purchased from Guangzhou Sijia Chemical Co., Ltd.

[0059] The auxiliary agent is a mixture of ultraviolet absorber, antioxidant and lubricant, and the weight ratio is 4:3:1. The ultraviolet absorber is UV-326; the antioxidant includes antioxidant 1010 and antioxidant 168, and the weight ratio is 1:2; the lubricant is erucamide.

[0060] The pigment was purchased from Yangzhou Yuhong Chemical Co., Ltd., and the model number was Pigment Red DPP.

[0061] Another aspect of this embodiment provides a method for preparing a beer cap with good sealing effect, including the following steps: first, the raw material of the cap body is put into an injection molding barrel of a two-color injection molding machine for injection molding into a product, and then the mold is flipped on the two-color machine to jump to the mold cavity corresponding to the other injection molding barrel for injection molding of the sealing material, thereby forming an integrated beer cap.

[0062] The injection molding temperature of the cover body is 190° C., the injection molding temperature of the seal is 140° C., the injection molding time of the injection molding machine is 30 seconds, the holding time is 25 seconds, and the cooling time is 20 seconds.

[0063] Example 2

[0064] On the one hand, this embodiment provides a beer cap with good sealing effect, including a cap body and a sealing member, wherein the cap body is a conical structure, and the sealing member is fixedly connected around the conical structure. The cap body includes the following raw materials in parts by weight: 99 parts of polypropylene, 0.2 parts of lubricant, 0.27 parts of antioxidant 168, 0.03 parts of tert-butylphenol antioxidant, and 0.5 parts of whitening agent.

[0065] The polypropylene was purchased from LG Chemical (Guangzhou) Engineering Plastics Co., Ltd., and the model was LG H1615 food grade. The melt index of the polypropylene was 20 g / 10 min, and the Vicat softening point was 156° C.

[0066] The lubricant is oleamide.

[0067] The tert-butylphenol antioxidant is 2-tert-butyl-p-ethylphenol.

[0068] The whitening agent is titanium dioxide.

[0069] The sealing element comprises the following raw materials in parts by weight: 35 parts of polypropylene, 37 parts of styrene-ethylene-butylene-styrene front-stage copolymer, 0.6 parts of filler, 26 parts of filling oil, 0.4 parts of auxiliary agent and 1 part of pigment.

[0070] The polypropylene was purchased from LG Chemical (Guangzhou) Engineering Plastics Co., Ltd., model LG H1615 food grade, the melt index of polypropylene was 20g / 10min, and the Vicat softening point was 156°C; the styrene-ethylene-butylene-styrene front-stage copolymer was purchased from Shanghai Yiding Plastic Co., Ltd., model P3080-2 food grade, the melt flow rate was 12g / 10min, and the specific gravity was 0.86-0.9g / cm 3 .

[0071] The filler is hydrated magnesium silicate, purchased from Shanghai Shunshui Chemical Co., Ltd.

[0072] The filler oil is white oil purchased from Guangzhou Sijia Chemical Co., Ltd.

[0073] The auxiliary agent is a mixture of an ultraviolet absorber, an antioxidant, and a lubricant, and the weight ratio is 2:1.5:1. The ultraviolet absorber is UV-326; the antioxidant includes antioxidant 1010 and antioxidant 168, and the weight ratio is 1:1; the lubricant is erucamide.

[0074] The pigment was purchased from Yangzhou Yuhong Chemical Co., Ltd., and the model number was Pigment Red DPP.

[0075] Another aspect of this embodiment provides a method for preparing a beer cap with good sealing effect, including the following steps: first, the raw material of the cap body is put into an injection molding barrel of a two-color injection molding machine for injection molding into a product, and then the mold is flipped on the two-color machine to jump to the mold cavity corresponding to the other injection molding barrel for injection molding of the sealing material, thereby forming an integrated beer cap.

[0076] The injection molding temperature of the cover body is 190° C., the injection molding temperature of the seal is 140° C., the injection molding time of the injection molding machine is 30 seconds, the holding time is 25 seconds, and the cooling time is 20 seconds.

[0077] Example 3

[0078] On the one hand, this embodiment provides a beer cap with good sealing effect, including a cap body and a sealing member, wherein the cap body is a conical structure, and the sealing member is fixedly connected around the conical structure. The cap body includes the following raw materials in parts by weight: 99.4 parts of polypropylene, 0.1 parts of lubricant, 0.19 parts of antioxidant 168, 0.01 parts of tert-butylphenol antioxidant, and 0.3 parts of whitening agent.

[0079] The polypropylene was purchased from LG Chemical (Guangzhou) Engineering Plastics Co., Ltd., and the model was LG H1615 food grade. The melt index of the polypropylene was 20 g / 10 min, and the Vicat softening point was 156° C.

[0080] The lubricant is oleamide.

[0081] The tert-butylphenol antioxidant is 2-tert-butyl-p-ethylphenol.

[0082] The whitening agent is titanium dioxide.

[0083] The sealing element comprises the following raw materials in parts by weight: 34 parts of polypropylene, 34 parts of styrene-ethylene-butylene-styrene front-stage copolymer, 0.8 parts of filler, 30 parts of filling oil, 0.4 parts of auxiliary agent and 0.8 parts of pigment.

[0084] The polypropylene was purchased from LG Chemical (Guangzhou) Engineering Plastics Co., Ltd., model LG H1615 food grade, the melt index of polypropylene was 20g / 10min, and the Vicat softening point was 156°C; the styrene-ethylene-butylene-styrene front-stage copolymer was purchased from Shanghai Yiding Plastic Co., Ltd., model P3080-2 food grade, the melt flow rate was 12g / 10min, and the specific gravity was 0.86-0.9g / cm 3 .

[0085] The filler is hydrated magnesium silicate, purchased from Shanghai Shunshui Chemical Co., Ltd.

[0086] The filler oil is white oil purchased from Guangzhou Sijia Chemical Co., Ltd.

[0087] The auxiliary agent is a mixture of ultraviolet absorber, antioxidant and lubricant, and the weight ratio is 6:5:1. The ultraviolet absorber is UV-326; the antioxidant includes antioxidant 1010 and antioxidant 168, and the weight ratio is 1:3; the lubricant is erucamide.

[0088] The pigment was purchased from Yangzhou Yuhong Chemical Co., Ltd., and the model number was Pigment Red DPP.

[0089] Another aspect of this embodiment provides a method for preparing a beer cap with good sealing effect, including the following steps: first, the raw material of the cap body is put into an injection molding barrel of a two-color injection molding machine for injection molding into a product, and then the mold is flipped on the two-color machine to jump to the mold cavity corresponding to the other injection molding barrel for injection molding of the sealing material, thereby forming an integrated beer cap.

[0090] The injection molding temperature of the cover body is 190° C., the injection molding temperature of the seal is 140° C., the injection molding time of the injection molding machine is 30 seconds, the holding time is 25 seconds, and the cooling time is 20 seconds.

[0091] Example 4

[0092] This embodiment provides a beer cap with good sealing effect and a preparation method thereof. The specific implementation method is the same as that of Embodiment 1, except that the resin material does not include styrene-ethylene-butylene-styrene front segment copolymer.

[0093] Example 5

[0094] This embodiment provides a beer cap with good sealing effect and a preparation method thereof. The specific implementation method is the same as that of Embodiment 1, except that the raw material of the sealing component does not contain filler oil.

[0095] Performance Testing

[0096] 1. Sealing test

[0097] During the beer canning process, the pressure is increased to 7 Bar, and after high-temperature sterilization at 85°C, the bottles are stored at room temperature for one year. The pressure in the bottles is tested to determine whether there is leakage. A pressure between 6.5 and 7 Bar is recorded as no leakage, a pressure between 4 and 6.5 Bar is recorded as a slight leakage, and a pressure less than 4 Bar is recorded as a serious leakage. The results are shown in Table 1.

[0098] Table 1

[0099] serial number Sealing effect Example 1 No leakage Example 2 No leakage Example 3 No leakage Example 4 Serious air leakage Example 5 Slight air leakage

Claims

1. A beer cap with good sealing effect, characterized in that: The invention comprises a cover body and a sealing member, wherein the cover body is a conical structure, the sealing member is fixedly connected around the conical structure, and the cover body comprises the following raw materials in parts by weight: 99-99.4 parts of polypropylene, 0.1-0.2 parts of lubricant, 0.2-0.033 parts of antioxidant, and 0.3-0.5 parts of brightener; the melting index of the polypropylene in the cover body is 20g / 10min, and the Vicat softening point is 156°C; the lubricant in the cover body is oleic acid amide; the antioxidant in the cover body is antioxidant 168 and 2-tert-butyl-p-ethylphenol; the seal comprises the following raw materials in parts by weight: 68-75 parts of resin material, 0.5-1 parts of filler, 25-30 parts of filler oil, and 0.3-1 parts of additives; the resin material comprises polypropylene and styrene-ethylene-butylene-styrene block copolymer, and the weight ratio of the two is (0.9-1):1; the melt flow rate of the styrene-ethylene-butylene-styrene block copolymer is 12g / 10min, and the specific gravity is 0.86-0.9g / cm 3 ; The filler is hydrated magnesium silicate; the filling oil includes white oil; the auxiliary agent is a mixture of ultraviolet absorber, antioxidant and lubricant, and the weight ratio is (2-6): (1.5-5): 1, the ultraviolet absorber in the auxiliary agent is UV326, the antioxidant includes antioxidant 1010 and antioxidant 168, and the lubricant is erucamide.

2. A method for preparing a beer cap with good sealing effect according to claim 1, characterized in that: At least the following steps are included: First, the raw material of the cap body is put into one injection molding barrel of the two-color injection molding machine for injection molding into a product, and then the mold is flipped on the two-color machine to jump to the mold cavity corresponding to the other injection molding barrel for injection molding of the sealing material, thereby forming an integrated beer cap; The injection molding temperature of the cover body is 180-200°C; The injection molding temperature of the seal is 130-150°C; The injection molding machine has an attack time of 20-40 seconds, a holding time of 20-30 seconds, and a cooling time of 15-25 seconds.