Components for semiconductor manufacturing equipment and semiconductor manufacturing equipment
By employing composite structures and polycrystalline ceramic layers in components used in semiconductor manufacturing equipment, the problem of particle generation has been solved, yield and production efficiency have been improved, and damage caused by physical contact and maintenance has been reduced.
Patent Information
- Application Number
- CN202210355991.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-04-21
- Filing Date
- 2022-04-06
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-04-06
AI Technical Summary
In the semiconductor manufacturing process, particle generation from components used in semiconductor manufacturing equipment leads to a decrease in yield, and existing technologies are unable to effectively reduce particle generation or its impact.
The composite structure, consisting of a substrate and a ceramic layer, with through-holes designed as a combination of inclined and vertical surfaces, combined with the use of a polycrystalline ceramic layer, improves resistance to plasma corrosion and hardness, and reduces particle generation.
It effectively suppresses the generation and impact of particles, improves the yield and production efficiency of semiconductor manufacturing equipment, and reduces damage caused by physical contact and maintenance.
Smart Images

Figure CN115223837B_ABST
Abstract
Description
Technical Field
[0001] The present invention generally relates to a component for a semiconductor manufacturing apparatus and a semiconductor manufacturing apparatus. Background Technology
[0002] In the manufacturing process of semiconductor equipment, semiconductor manufacturing apparatuses are used to process workpieces such as semiconductor wafers using plasma. Within such an apparatus, a component for semiconductor manufacturing is configured with at least one aperture that comes into contact with the plasma. Particles sometimes arise from this component. Since particles are a major cause of reduced yield in the manufactured semiconductor equipment, it is necessary to reduce the generation or impact of particles.
[0003] Patent documents Patent Document 1: Japanese Patent Application Publication No. 2012-057251 Patent Document 2: Japanese Patent Application Publication No. 2016-028379 Summary of the Invention
[0004] The present invention was made based on the understanding of the problems in the prior art described above. The technical problem to be solved is to provide a component for a semiconductor manufacturing apparatus and a semiconductor manufacturing apparatus that can reduce the generation or impact of particles.
[0005] The first invention is a component for a semiconductor manufacturing apparatus, used within a cavity of the semiconductor manufacturing apparatus, characterized by comprising a composite structure including: a substrate having a first surface and a second surface opposite to the first surface; and a ceramic layer having a first portion exposed on the first surface of the substrate. The composite structure has a through-hole extending in a first direction from the first surface toward the second surface and penetrating the substrate and the ceramic layer. The through-hole has: a first hole region continuous with the surface of the first portion and inclined relative to the first direction; a second hole region located between the second surface and the first hole region in the first direction and extending along the first direction; and a third hole region located between the first hole region and the second hole region in the first direction and inclined relative to the first direction. The hardness of the third hole region is higher than that of the first hole region.
[0006] According to this component for a semiconductor manufacturing apparatus, since the third hole region has relatively high hardness, damage to the third hole region caused by physical contact during maintenance or handling of the component for the semiconductor manufacturing apparatus can be suppressed. Therefore, particle generation can be suppressed.
[0007] The second invention is a component for a semiconductor manufacturing apparatus, characterized in that, in the first invention, the substrate includes at least one hole penetrating the first surface and the second surface, a portion of the through-hole of the composite structure is at least a portion of the hole of the substrate, the hole of the substrate having: an inclined surface continuous with the first surface and inclined relative to the first direction; and a vertical surface located between the second surface and the inclined surface in the first direction and extending along the first direction, the inclined surface being straight in a cross-section parallel to the first direction.
[0008] According to the component for this semiconductor manufacturing apparatus, it is possible to alleviate electric field concentration in a tilted surface or a ceramic layer on a tilted surface.
[0009] The third invention is a component for a semiconductor manufacturing apparatus, characterized in that, in the first invention, the substrate includes at least one hole penetrating the first surface and the second surface, a portion of the through-hole of the composite structure is at least a portion of the hole of the substrate, the hole of the substrate having: an inclined surface continuous with the first surface and inclined relative to the first direction; and a vertical surface located between the second surface and the inclined surface in the first direction and extending along the first direction, the angle formed by the first surface and the inclined surface being larger than the angle formed by the vertical surface and the inclined surface.
[0010] For example, during surface cleaning and other maintenance of components for semiconductor manufacturing equipment, if the angle formed by the first surface and the inclined surface is greater than the angle formed by the vertical surface and the inclined surface, the third hole region will be more prone to wear than the first hole region. In contrast, according to this semiconductor manufacturing equipment component, because the third hole region has high hardness, damage to the third hole region due to physical contact during maintenance of the semiconductor manufacturing equipment component can be suppressed. Therefore, particle generation can be suppressed.
[0011] The fourth invention is a component for a semiconductor manufacturing apparatus, characterized in that, in the first invention, the substrate includes at least one hole penetrating the first surface and the second surface, a portion of the through-hole of the composite structure is at least a portion of the hole of the substrate, the hole of the substrate having: a first hole portion continuous with the first surface and inclined relative to the first direction; a second hole portion located between the second surface and the first hole portion in the first direction and extending along the first direction; a third hole portion located between the first hole portion and the second hole portion in the first direction and inclined relative to the first direction, the ceramic layer having higher plasma corrosion resistance than the substrate, the ceramic layer further including a second portion disposed on the first hole portion, the first hole region being the surface of the second portion.
[0012] According to the component for this semiconductor manufacturing apparatus, a ceramic layer is provided on the first surface of a substrate. Furthermore, a ceramic layer with high resistance to plasma corrosion is provided at the first aperture of a hole in the substrate. This further suppresses the generation of particles from the substrate.
[0013] The fifth invention is a component for a semiconductor manufacturing apparatus, characterized in that, in the fourth invention, the third hole is exposed, and the third hole region is the third hole.
[0014] According to the component for the semiconductor manufacturing apparatus, it is possible to effectively suppress the generation of particles from the ceramic layer due to the formation of a poorly shaped ceramic layer at the third hole.
[0015] The sixth invention is a component for a semiconductor manufacturing apparatus, characterized in that, in the fourth invention, the ceramic layer further includes a third portion disposed on the third hole, the third hole region being the surface of the third portion.
[0016] According to the component for this semiconductor manufacturing apparatus, a ceramic layer is provided on the third hole portion. This allows for the suppression of particle generation from the holes in the substrate at the third hole portion.
[0017] The seventh invention is a component for a semiconductor manufacturing apparatus, characterized in that, in the sixth invention, the material of the third part is different from the material of the second part, and the hardness of the material of the third part is higher than the hardness of the material of the second part.
[0018] According to the component for the semiconductor manufacturing apparatus, since the hardness of the third part of the material is higher than that of the second part of the material, the hardness of the third hole region can be made higher than that of the first hole region.
[0019] The eighth invention is a component for a semiconductor manufacturing apparatus, characterized in that, in the seventh invention, the density of the third part is higher than the density of the second part.
[0020] According to the component for the semiconductor manufacturing apparatus, since the density of the third part of the material is higher than that of the second part of the material, the hardness of the third hole region is higher than that of the first hole region.
[0021] The ninth invention is a component for a semiconductor manufacturing apparatus, characterized in that, in any one of the inventions described in the first to eighth claims, the ceramic layer comprises polycrystalline ceramic.
[0022] According to the components used in this semiconductor manufacturing apparatus, the generation or impact of particles can be reduced more reliably.
[0023] The 10th invention is a component for a semiconductor manufacturing apparatus, characterized in that, in the 9th invention, the average crystallite size of the polycrystalline ceramic calculated from a TEM image at a magnification of 400,000 to 2,000,000 times is 3 nanometers or more and 50 nanometers or less.
[0024] According to the components used in this semiconductor manufacturing apparatus, the generation or impact of particles can be reduced more reliably.
[0025] The 11th invention is a component for a semiconductor manufacturing apparatus, characterized in that, in any one of the inventions described in the 1st to 10th inventions, the ceramic layer comprises at least one selected from oxides of rare earth elements, fluorides of rare earth elements, and fluorides of rare earth elements.
[0026] According to the components used in this semiconductor manufacturing apparatus, the generation or impact of particles can be reduced more reliably.
[0027] The 12th invention is a component for a semiconductor manufacturing apparatus, characterized in that, in the 11th invention, the rare earth element is at least one selected from Y, Sc, Yb, Ce, Pr, Eu, La, Nd, Pm, Sm, Gd, Tb, Dy, Ho, Er, Tm and Lu.
[0028] According to the components used in this semiconductor manufacturing apparatus, the generation or impact of particles can be reduced more reliably.
[0029] The 13th invention is a component for a semiconductor manufacturing apparatus, characterized in that, in any one of the inventions described in the 1st to 12th claims, the substrate comprises ceramic.
[0030] According to the components used in this semiconductor manufacturing apparatus, the generation or impact of particles can be reduced more reliably.
[0031] The 14th invention is a component for a semiconductor manufacturing apparatus, characterized in that, in the 13th invention, the substrate comprises aluminum oxide.
[0032] According to the components used in this semiconductor manufacturing apparatus, the generation or impact of particles can be reduced more reliably.
[0033] The 15th invention is a semiconductor manufacturing apparatus comprising: a chamber; and a semiconductor manufacturing apparatus component as described in any one of the 1 to 14, the chamber having an inner wall forming a space for generating plasma, the semiconductor manufacturing apparatus component constituting at least a portion of the inner wall.
[0034] According to this semiconductor manufacturing apparatus, it is possible to reduce the generation or impact of particles.
[0035] According to the present invention, a component for a semiconductor manufacturing apparatus and a semiconductor manufacturing apparatus can be provided, which can reduce the generation or influence of particles. Attached Figure Description
[0036] Figure 1 This is a cross-sectional view illustrating a semiconductor manufacturing apparatus having components for a semiconductor manufacturing apparatus according to the first embodiment. Figure 2 This is a cross-sectional view illustrating a portion of a component of a semiconductor manufacturing apparatus according to the first embodiment. Figure 3 (a)~ Figure 3 (c) is a cross-sectional view illustrating a portion of a component of another semiconductor manufacturing apparatus according to the first embodiment. Figure 4 (a)~ Figure 4 (c) is a cross-sectional view illustrating a portion of the substrate according to the first embodiment. Figure 5 (a) and 5(b) are cross-sectional views illustrating a portion of a component of a semiconductor manufacturing apparatus according to the second embodiment. Figure 6 (a) and Figure 6 (b) is a cross-sectional view illustrating a portion of a component used in a semiconductor manufacturing apparatus. Figure 7 It is a graph illustrating the stress of components used in semiconductor manufacturing equipment. Figure 8 This is a table illustrating the evaluation of particle resistance in components used in semiconductor manufacturing equipment. Symbol Explanation 10, 10a~10c - Substrate; 11 - First surface; 12 - Second surface; 13 - Hole; 13a - First hole portion; 13ac - Inclined surface; 13b - Second hole portion; 13c - Third hole portion; 13s - Inner peripheral surface; 14, 15 - Boundary; 16a - First region; 16b - Second region; 16c - Boundary; 17 - Boundary; 20 - Ceramic layer; 21 - First part; 21s - Surface; 22 - Second part; 22s - Surface; 23 - Third part; 23s - Surface; 30 - Composite structure; θα, θβ, θ1~θ4 - Angle; 100 - Semiconductor Semiconductor manufacturing apparatus; 110-Cavity; 111-Inner wall; 111b-Lower inner wall; 111u-Upper inner wall; 120, 120a~120e-Components for semiconductor manufacturing apparatus; 160-Electrostatic chuck; 191-Region; 210-Wafer; 221-Particle; 311-First main surface; 312-Second main surface; 313-Through hole; 313a-First hole region; 313b-Second hole region; 313c-Third hole region; 313s-Inner peripheral surface; L1~L3-Line segment; T21, T22-Thickness; e1~e4-End; P1~P3-Part. Detailed Implementation
[0037] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. Furthermore, in the drawings, the same reference numerals are used to denote the same constituent elements, and detailed descriptions are omitted where appropriate. The accompanying drawings are schematic or conceptual, and the relationship between the thickness and width of each part, the ratio of the size between parts, etc., may not be the same as the actual object. Even when representing the same part, different dimensions and proportions may be shown depending on the drawing.
[0038] (First Embodiment) Figure 1 This is a cross-sectional view illustrating a semiconductor manufacturing apparatus having components for a semiconductor manufacturing apparatus according to the first embodiment. Figure 1 The semiconductor manufacturing apparatus 100 shown includes a chamber 110, a semiconductor manufacturing apparatus component 120, and an electrostatic chuck 160. The electrostatic chuck 160 is disposed in the lower part of the chamber 110. A wafer 210 or similar object to be attracted is placed on the electrostatic chuck 160. In this example, the semiconductor manufacturing apparatus component 120 is disposed in the upper part of the chamber 110. For example, the semiconductor manufacturing apparatus component 120 is a top plate component of the chamber 110 located directly above the electrostatic chuck 160 and the wafer 210 within the chamber 110.
[0039] The chamber 110 has an inner wall 111 that forms a space (region 191) for generating plasma. The ceramic layer 20 on the surface of the component 120 for the semiconductor manufacturing apparatus (see reference) Figure 2 This constitutes at least a portion of the inner wall 111. In this example, the inner wall 111 has a lower inner wall 111b on which an electrostatic chuck 160 is disposed, and an upper inner wall 111u disposed above the lower inner wall 111b. A ceramic layer 20 of a semiconductor manufacturing apparatus component 120 is disposed in at least a portion of the upper inner wall 111u.
[0040] High-frequency power is supplied to the semiconductor manufacturing apparatus 100, and as... Figure 1 As indicated by arrow A1, a raw material gas, such as a halogen gas, is introduced into the chamber 110. Thus, the raw material gas introduced into the chamber 110 is plasma-ionized in the region 191 between the electrostatic chuck 160 and the semiconductor manufacturing apparatus component 120.
[0041] Here, if the inner wall of chamber 110 is corroded by plasma, particles 221 may be generated. When these particles 221 adhere to wafer 210, the manufactured semiconductor equipment will malfunction. This will reduce the yield and production efficiency of semiconductor devices. Therefore, the components 120 for semiconductor manufacturing apparatus need to be plasma resistant.
[0042] Furthermore, the semiconductor manufacturing apparatus component described in the embodiments may also be a component disposed in a location other than the upper part of the cavity. Additionally, the semiconductor manufacturing apparatus using the semiconductor manufacturing apparatus component is not limited to... Figure 1 The examples are not limited to semiconductor manufacturing apparatuses (semiconductor processing apparatuses) that perform processes such as annealing, etching, sputtering, and CVD (Chemical Vapor Deposition).
[0043] The components for semiconductor manufacturing apparatus according to the present invention can be used as various components within a semiconductor manufacturing apparatus, and are particularly suitable for use as components in environments exposed to corrosive, high-density plasma atmospheres. Specifically, examples include chamber walls, spray plates, bushings, seals, windows, edge rings, focusing rings, etc.
[0044] Figure 2 This is a cross-sectional view illustrating a portion of a component of a semiconductor manufacturing apparatus according to the first embodiment. Figure 2 Magnification Figure 1 The area near region R shown. The component 120 for a semiconductor manufacturing apparatus includes a substrate 10 and a ceramic layer 20. The substrate 10 has a first surface 11 and a second surface 12 opposite to the first surface 11. The first surface 11 faces... Figure 1 The inner surface of the cavity 110 shown has a second surface 12 facing the outer surface of the cavity 110. At least one hole 13 is provided in the substrate 10. The hole 13 penetrates the substrate 10 from the first surface 11 to the second surface 12.
[0045] In this example, the substrate 10 is, for example, plate-shaped (circular plate-shaped). The first surface 11 and the second surface 12 are, for example, planar. However, the first surface 11 and the second surface 12 may also be curved surfaces. In addition, a hole 13 is provided in the center of the substrate 10. For example, a component such as an ejector for injecting plasma feed gas is disposed in the hole 13. The plasma feed gas is introduced into the cavity 110 through the hole 13. However, the hole 13 may not be a hole for supplying plasma generation feed gas into the cavity 110, but may be any hole penetrating the substrate 10. In addition, the hole 13 may not be in the center of the substrate 10, and multiple holes may be provided.
[0046] The direction from face 11 toward face 12 is defined as the Z direction (first direction). A direction perpendicular to the Z direction is defined as the X direction, and a direction perpendicular to both the Z and X directions is defined as the Y direction. For example, face 11 and face 12 are perpendicular to the Z direction and extend along the XY plane.
[0047] Hole 13 (inner peripheral surface 13s) has a first hole portion 13a, a second hole portion 13b, and a third hole portion 13c. When viewed along the Z direction, hole 13 is, for example, circular. The inner peripheral surface 13s is the inner peripheral surface of the substrate 10 that defines hole 13. The inner peripheral surface 13s faces inward toward the hole 13 and intersects the XY plane.
[0048] The first hole portion 13a is located near the first surface 11 in the inner circumferential surface 13s, and is the region adjacent to the first surface 11. The first hole portion 13a is continuous with the first surface 11. The first hole portion 13a is located between the first surface 11 and the second surface 12 in the Z direction. The first hole portion 13a is not parallel to the first surface 11, but is an inclined surface that intersects the first surface 11 and the Z direction. The first hole portion 13a can also be a surface extending parallel to the Z direction. In this example, in such... Figure 2 In the cross-section shown parallel to the Z direction, the first hole 13a is straight. However, in the cross-section parallel to the Z direction, the first hole 13a may not be straight; for example, it may be curved. When viewed along the Z direction (i.e., when projected onto the XY plane), the first hole 13a is, for example, an annular shape surrounded by the first surface 11.
[0049] In this example, in a cross-section parallel to the Z direction, the boundary 14 where the first surface 11 contacts the first hole 13a is an angle. However, the first surface 11 and the first hole 13a can also be connected smoothly. In other words, in Figure 2 In the cross-section, boundary 14 can also be rounded and curved, having curvature.
[0050] The second hole 13b is located in the Z direction between the first hole 13a and the second surface 12. In other words, the position of the second hole 13b in the Z direction is between the position of the first hole 13a in the Z direction and the position of the second surface 12 in the Z direction. For example, the second hole 13b is located near the second surface 12 in the inner circumferential surface 13s, and is the region adjacent to the second surface 12. The second hole 13b may be continuous with the second surface 12. The second hole 13b extends along the Z direction, for example, parallel to the Z direction. The second hole 13b forms a vertical plane, for example, substantially perpendicular to the second surface 12. When viewed along the Z direction, the second hole 13b is, for example, an annular shape located inside the first hole 13a.
[0051] The third hole 13c is located between the first hole 13a and the second hole 13b in the Z direction. In other words, the position of the third hole 13c in the Z direction is between the positions of the first hole 13a and the second hole 13b in the Z direction. The third hole 13c is a region in the inner circumferential surface 13s that is continuous with the first hole 13a. The third hole 13c is not parallel to the first surface 11, but is an inclined surface that intersects the first surface 11 and the Z direction. The third hole 13c can also be a surface extending along the Z direction. In this example, in a cross-section parallel to the Z direction, the third hole 13c is straight. However, in a cross-section parallel to the Z direction, the third hole 13c may not be straight; for example, it may be curved. When viewed along the Z direction, the third hole 13c is, for example, an annular shape surrounded by and in contact with the first hole 13a, and the second hole 13b is located inside the third hole 13c. The third hole 13c and the second hole 13b can be continuous.
[0052] In this example, in a cross-section parallel to the Z direction, the direction in which the first hole 13a extends is the same as the direction in which the third hole 13c extends. In other words, the angle θ1 formed by the third hole 13c and the Z direction is the same as the angle θ2 formed by the first hole 13a and the Z direction. However, angles θ1 and θ2 can also be different.
[0053] Furthermore, in this example, in a cross-section parallel to the Z direction, the boundary 17 where the second hole 13b and the third hole 13c meet is at an angle. However, the second hole 13b and the third hole 13c can also be connected smoothly. In other words, in Figure 2 In the cross-section, boundary 17 can also be rounded and curved, having curvature.
[0054] Additionally, the hole 13 (the inner circumferential surface 13s of the hole) has an inclined surface 13ac. The inclined surface 13ac is, for example, a surface including a first hole portion 13a and a third hole portion 13c. The inclined surface 13ac is continuous with the first surface 11 and inclined relative to the first surface 11 and the Z direction. The inclined surface 13ac is continuous with the vertical surface (the second hole portion 13b) and connects the first surface 11 and the second hole portion 13b. In this example, the inclined surface 13ac formed by the first hole portion 13a and the third hole portion 13c is straight in a cross-section parallel to the Z direction. However, the inclined surface 13ac can also be curved.
[0055] The angle θα formed by the first surface 11 and the inclined surface 13ac is larger than the angle θβ formed by the second hole 13b (vertical surface) and the inclined surface 13ac. For example, angle θα is the angle formed by the first surface 11 and the first hole 13a, and angle θβ is the angle formed by the second hole 13b and the third hole 13c.
[0056] The ceramic layer 20 has higher resistance to plasma corrosion than the substrate 10. The ceramic layer 20 is disposed on the substrate 10. More specifically, such as... Figure 2 As shown, the ceramic layer 20 includes a first portion 21 and a second portion 22. The first portion 21 is disposed on and in contact with the first surface 11. The first portion 21 is disposed on the entire first surface 11. The second portion 22 is disposed on and in contact with the first hole 13a. The surfaces 21s of the first portion 21 and 22s of the second portion 22 are in direct contact with the plasma in the chamber 110. That is, surface 21s is the side of the first portion 21 opposite to the side that contacts the first surface 11, and is configured to be exposed into the chamber 110. Surface 22s is the side of the second portion 22 opposite to the side that contacts the first hole 13a, and is configured to be exposed into the chamber 110. The first surface 11 is covered by the first portion 21, so it is not in direct contact with the plasma. In addition, the first hole 13a is covered by the second portion 22, so it is not in direct contact with the plasma. That is, the first surface 11 and the first hole 13a are covered by a ceramic layer 20, which is configured to be exposed to plasma. Surface 21s is, for example, a plane parallel to the XY plane. Surface 21s can also be a curved surface. Surface 22s is an inclined surface that intersects surface 21s and the Z direction. Surface 21s can also be a surface extending along the Z direction.
[0057] No ceramic layer 20 is provided on the second surface 12, the second hole portion 13b, and the third hole portion 13c. In other words, in this example, the area on the inner peripheral surface 13s of the hole 13 where the ceramic layer 20 is provided is the first hole portion 13a, while the areas where the ceramic layer 20 is not provided are the second hole portion 13b and the third hole portion 13c. The third hole portion 13c is connected to the end of the second portion 22. The second hole portion 13b and the third hole portion 13c are exposed to the plasma in the chamber 110 and are in direct contact with the plasma. The second hole portion 13b and the third hole portion 13c are not covered by the ceramic layer 20.
[0058] The arithmetic mean height Sa of surface 21s in part 1 21 is less than the arithmetic mean height Sa of surface 22s in part 22. The arithmetic mean height Sa (surface roughness) can be evaluated by the method described later. For example, the surface roughness of part 1 21 (the roughness of surface 21s) is less than the surface roughness of part 22 (the roughness of surface 22s).
[0059] As described above, to reduce particles, components of semiconductor manufacturing apparatuses that come into contact with plasma are required to have plasma resistance. To this end, conventionally, methods have employed coatings with plasma-resistant films (layers) to coat the surfaces of semiconductor manufacturing apparatus components. However, even when coating the non-hole portions of a semiconductor manufacturing apparatus component (e.g., a top plate component) with a highly plasma-resistant film (e.g., Y₂O₃), it has recently become possible that the requirement for particle reduction is not sufficiently met. Therefore, for example, it is also necessary to control particles from holes. Particles from holes include, for example, particles generated due to the detachment of a portion of the coating disposed in the hole, and particles from components (e.g., ejectors) disposed in the hole.
[0060] In contrast, in this embodiment, a ceramic layer 20 is provided on the first surface 11 and the first hole 13a of the substrate 10, and the arithmetic mean height Sa of the surface 21s of the first portion 21 on the first surface 11 is less than the arithmetic mean height Sa of the surface 22s of the second portion 22 on the first hole 13a. This reduces the generation or impact of particles.
[0061] For example, since the arithmetic mean height Sa (surface roughness) of the surface 21s of the first portion 21 in contact with the corrosive plasma is relatively small, the generation of particles from the first portion 21 can be effectively suppressed. That is, for example, the first portion has a smooth structure, which can suppress the generation of cracks or particles based on the unevenness in the first portion 21. For example, it can suppress the first portion 21 from being corroded by the plasma and causing a portion of it to detach from the ceramic layer 20 and become particles.
[0062] Furthermore, since the arithmetic mean height Sa (surface roughness) of the surface 22s of the second portion 22 on the first aperture 13a is relatively large, the generation or influence of particles from the aperture 13 can be suppressed. For example, since the second portion 22 is provided on the first aperture 13a, it is assumed that the influence of the electric field in the second portion 22 may be greater than that in the first portion 21. That is, when the first portion 21 provided on the first surface 11 is exposed to plasma, since the second portion 22 on the first aperture 13a is near the edge of the aperture 13, the electric field may be more easily concentrated than in the first portion 21. In the part where the electric field is concentrated, the electric field strength is large, and the damage caused by the plasma concentration is greater. The damaged part may detach from the ceramic layer 20 and generate particles. In contrast, in this embodiment, since the arithmetic mean height Sa of the surface 22s of the second portion 22 is relatively large, the surface area of the second portion 22 is larger, thereby mitigating the concentration of the electric field.
[0063] In addition, since the arithmetic mean height Sa of the surface 22s of the second part 22 located near the edge of the hole 13 (near the outlet) is relatively large, the particles generated from the hole 13 can be captured by the second part 22, thereby more effectively suppressing the influence of the particles.
[0064] Furthermore, when the plasma-generating gas passes through the hole 13, the temperature around the hole changes due to the gas ejection. Therefore, the thermal stress in the second part 22 may be higher than that in the first part 21. Cracks or particles may form in the second part 22 due to this thermal stress. Conversely, since the arithmetic mean height Sa of the surface 22s of the second part 22 is relatively large, the surface area of the second part 22 becomes larger, thereby improving the heat dissipation (heat dissipation) effect of the second part 22. This helps to suppress the generation of cracks or particles in the second part 22.
[0065] For example, the surface roughness of the second part 22 is preferably more than 2 times and less than 10 times the surface roughness of the first part, more preferably less than 5 times. The arithmetic mean height Sa of the surface 22s of the second part 22 is preferably more than 2 times and less than 10 times the arithmetic mean height Sa of the surface 21s of the first part 21, more preferably less than 5 times. The arithmetic mean height Sa of the surface 22s of the second part 22 is, for example, less than 0.5 micrometers (μm), or, for example, more than 0.005 μm. The arithmetic mean height Sa of the surface 21s of the first part 21 is, for example, less than 0.1 μm, and also, for example, more than 0.001 μm. With such a configuration, the generation or influence of particles can be reduced more reliably.
[0066] For example, the surface roughness of the third hole portion 13c is greater than the surface roughness of the first portion 21 and greater than the surface roughness of the second portion 22. For example, the arithmetic mean height Sa of the third hole portion 13c is greater than the arithmetic mean height Sa of the surface 21s of the first portion 21 and greater than the arithmetic mean height Sa of the surface 22s of the second portion 22.
[0067] As previously stated, in this example, no ceramic layer 20 is provided on the third hole portion 13c, and the inner wall of the hole 13 is exposed. That is, the third hole portion 13c is the boundary portion between the ceramic layer 20 and the inner wall of the hole 13, and is the end of the substrate that comes into contact with the plasma. By setting the arithmetic mean height Sa (surface roughness) of such a substrate end portion (the third hole portion 13c) to be relatively large, the surface area of the substrate end portion is increased, thereby mitigating the electric field concentration at the substrate end portion. Thus, for example, it is possible to suppress plasma damage caused by electric field concentration at the substrate end portion, thereby suppressing the generation of particles from the substrate end portion.
[0068] For example, preferably, the surface roughness of the third hole 13c is greater than twice the surface roughness of the first part 21. It is also preferably that the surface roughness of the third hole 13c is less than ten times the surface roughness of the first part 21. Preferably, the arithmetic mean height Sa of the third hole 13c is greater than twice the arithmetic mean height Sa of the surface 21s of the first part 21. It is also preferably that the arithmetic mean height Sa of the third hole 13c is less than ten times the arithmetic mean height Sa of the surface 21s of the first part 21. With this configuration, the generation or influence of particles can be reduced more reliably.
[0069] Furthermore, the surface roughness of the third hole portion 13c may be greater than the surface roughness of the first portion 21 and less than the surface roughness of the second portion 22. For example, the arithmetic mean height Sa of the third hole portion 13c may be greater than the arithmetic mean height Sa of the surface 21s of the first portion 21 and less than the arithmetic mean height Sa of the surface 22s of the second portion 22.
[0070] In the third hole portion 13c, since the plasma is in direct contact with the substrate 10, particles from the substrate 10 are easily generated. In contrast, in this embodiment, the third hole portion 13c is positioned away from the first surface 11 and the second surface 12, compared to the first hole portion 13a and the second hole portion 13b. Furthermore, when the arithmetic mean height Sa of the third hole portion 13c is less than the arithmetic mean height Sa of the surface of the second portion 22, the generation of particles from the third hole portion 13c can be further reduced. That is, for example, the generation of cracks or particles based on the unevenness in the third hole portion 13c can be suppressed. It is also possible to prevent a portion of the third hole portion 13c from detaching from the substrate 10 and becoming particles.
[0071] As described above, if the substrate 10 is corroded due to contact with plasma, tiny particles will be generated from the substrate 10, potentially leading to a decrease in the yield of the manufactured semiconductor device. Therefore, the surfaces of the substrate 10 in contact with plasma are covered with a ceramic layer having higher resistance to plasma corrosion than the substrate 10. Although the holes 13 provided on the substrate 10 have, for example, vertical surfaces perpendicular to the first and second surfaces of the substrate 10, some plasma can seep into the holes 13 and corrode the inner walls of the holes 13, thereby generating particles from the holes 13. Therefore, it is possible to consider providing a ceramic layer with high resistance to plasma corrosion on the inner walls (e.g., the vertical surfaces) of the holes 13. However, for example, the ceramic layer inside the holes 13 may be relatively fragile, and particles can be generated when the fragile ceramic layer is corroded by plasma. Furthermore, plasma concentration is easily caused on the inclined surfaces (first hole 13a and third hole 13c) between the first surface 11 and the second hole 13b.
[0072] In contrast, in this embodiment, in the inclined surface 13ac formed by the first hole 13a and the third hole 13c, a second portion 22 of the ceramic layer 20 is provided on the first hole 13a, which is relatively close to the first portion 21 that is in contact with the plasma. This effectively suppresses the generation of particles from the first hole 13a. On the other hand, in the inclined surface 13ac, the third hole 13c, which is relatively far from the first portion 21, is in contact with the plasma. That is, compared to the first hole 13a, the third hole 13c, which is farther from the first portion 21 and has a lower risk of plasma corrosion, is not covered by the ceramic layer 20, and the substrate 10 is in direct contact with the plasma on the third hole 13c. This effectively suppresses the generation of particles from the ceramic layer due to the formation of a poorly structured ceramic layer on the third hole 13c.
[0073] Furthermore, if the inclined surface 13ac is curved in a cross-section parallel to the Z direction, the electric field will concentrate on the inclined surface 13ac or the ceramic layer 20 on the inclined surface 13ac, thereby generating particles. In contrast, if the inclined surface 13ac is straight in a cross-section parallel to the Z direction, the concentration of the electric field in the inclined surface 13ac or the ceramic layer 20 on the inclined surface 13ac can be more mitigated.
[0074] Furthermore, for example, in the ceramic layer 20, the second portion 22 is thinner than the first portion 21. That is, the thickness T22 of the second portion 22 is less than the thickness T21 of the first portion 21. Since the first portion 21, which is more easily exposed to plasma, is thicker than the second portion 22, the generation of particles from the first surface 11 can be further suppressed. On the other hand, since the second portion 22, which is less easily exposed to plasma than the first portion 21, is relatively thin, for example, the collapse of the ceramic layer 20 in the second portion 22 can be suppressed, thereby further suppressing the generation of particles. For example, by thinning the film thickness of the second portion, deformation or internal stress in the film can be mitigated, thereby suppressing film collapse.
[0075] The thickness of ceramic layer 20 is the distance from the surface of substrate 10 to the surface of ceramic layer 20. Specifically, the thickness of ceramic layer 20 (thicknesses T11 and T22) is calculated as follows. Figure 2As shown, the semiconductor manufacturing apparatus component 120 is cut parallel to the Z-direction, and the cut surface is observed using a scanning electron microscope (SEM) to determine the thickness of the ceramic layer 20. For example, the thickness T21 of the first portion 21 is the length from the first surface 11 to the first surface 21s along the direction perpendicular to the first surface 11. For example, the thickness T22 of the second portion 22 is the length from the first hole 13a to the surface 22s along the direction perpendicular to the first hole 13a. For example, a HITACHI S-5500 SEM can be used, and the SEM observation conditions can be 5000x magnification and 15kV accelerating voltage. When the thickness is uneven in the cut surface image, measurements are taken at multiple locations, and the average value is calculated. The method of making the thickness T22 of the second part 22 less than the thickness T21 of the first part 21 can be achieved by using known methods such as different film-forming times (making the film-forming time of the second part shorter than that of the first part) or different grinding amounts (making the grinding amount of the second part greater than that of the first part).
[0076] Furthermore, the edge (boundary 14) formed by the first surface 11 and the inclined surface 13ac is located near the plasma irradiation surface (surface 21s). Therefore, plasma sometimes tends to concentrate near this edge (the ceramic layer 20 on the edge). In contrast, in this embodiment, the angle θα formed by the first surface 11 and the inclined surface 13ac is larger than the angle θβ between the inclined surface 13ac and the vertical surface (the second hole 13b). Because the angle θα is relatively large, it is possible to mitigate the concentration of plasma near the edge formed by the first surface 11 and the inclined surface 13ac, thereby suppressing particle generation. On the other hand, when the angle θβ is large, plasma is more likely to penetrate into the interior of the hole 13. In contrast, by making the angle θβ relatively small, it is possible to effectively suppress plasma penetration into the interior of the hole 13.
[0077] Furthermore, when angle θα is greater than angle θβ, the length of the second hole portion 13b in the Z direction is more likely to increase. For example, as described later... Figure 6 (a) shows the length Ln ratio Figure 6 (b) shows a longer length Ln. Furthermore, for example, in Figure 2If the thickness of the substrate 10 (positions of the first surface 11 and the second surface 12 in the Z direction) and the diameter of the hole 13 (positions of the boundary 14 and the boundary 17 in the X direction) are not changed, and the inclined surface 13ac remains straight while θα is further increased, the position of the boundary 17 decreases, and the second hole portion 13b becomes longer in the Z direction. Since the flow (directionality) of the feed gas of the plasma flowing into the chamber from the hole 13 is restricted, for example, by the second hole portion 13b, the longer the second hole portion 13b, the easier it is to stabilize the flow of the feed gas. In addition, when components such as ejectors are fixed in the second hole portion 13b, the longer second hole portion 13b makes it easier to install the components and suppresses the exposure of the components to the plasma.
[0078] Boundaries 14 and 17 are preferably chamfered. This can further mitigate the concentration of plasma in the ceramic layer 20 on boundary 14 or on boundary 17.
[0079] The angle θα is, for example, 150° to 180°, preferably 160° to 180°. This further mitigates plasma concentration near the edges formed by the first surface 11 and the inclined surface 13ac, and further suppresses particle generation.
[0080] The angle θβ is, for example, greater than 90° and less than 120°, preferably greater than 90° and less than 105°. This allows for more effective suppression of plasma intrusion into the hole.
[0081] For example, the density of part 22 is higher than that of part 1 21. Additionally, for example, the hardness of part 22 is higher than that of part 1 21.
[0082] During the maintenance or handling of components for semiconductor manufacturing apparatuses, the vicinity of hole 13 (and via 313 described later) may come into physical contact with other components (e.g., clamps such as pins, sponge-like cleaning pads). Due to this physical contact, wear, damage, or peeling may occur near hole 13 (and via 313), and particles may be generated. For example, when handling components for semiconductor manufacturing apparatuses, clamps such as positioning pins are sometimes inserted into hole 13. Compared to the first part 21, the second part 22 disposed in hole 13 is more likely to come into physical contact with such clamps. Furthermore, for example, during the maintenance of components for semiconductor manufacturing apparatuses, surface cleaning is performed on the side with the first surface 11, and the first part 21 and the second part 22 come into contact with components such as cleaning pads. At this time, due to the shape of hole 13, the force applied from the cleaning pad to the second part 22 disposed on hole 13 may be greater than the force applied from the cleaning pad to the first part 21 on the first surface 11. The contact area between the cleaning pad and the components of the semiconductor manufacturing apparatus is generally smaller in the second portion 22 located on the inclined surface than in the first portion 21 located on the flat surface. Therefore, when the force applied to the cleaning pad is constant, the force per unit area is greater in the second portion 22 due to the smaller contact area.
[0083] In this regard, since the second part 22 has a relatively high density, damage or peeling in the second part 22 due to physical contact during maintenance or handling of components for semiconductor manufacturing apparatus can be suppressed. Therefore, particle generation can be further suppressed. Furthermore, since the second part 22 has a relatively high hardness, damage or peeling in the second part 22 due to physical contact during maintenance or handling of components for semiconductor manufacturing apparatus can be suppressed. Therefore, particle generation can be further suppressed.
[0084] Figure 3 (a)~ Figure 3 (c) is a cross-sectional view illustrating a portion of a component of another semiconductor manufacturing apparatus according to the first embodiment. Figure 3 (a)~ Figure 3 (c) The semiconductor manufacturing apparatus components 120a-120c shown in the diagram differ in the shape of the hole 13 from those shown in the diagram. Figure 1 and Figure 2 The semiconductor manufacturing apparatus component 120 is described. Apart from this, the semiconductor manufacturing apparatus components 120a to 120c are the same as the semiconductor manufacturing apparatus component 120. exist Figure 3 In the semiconductor manufacturing apparatus component 120a shown in (a), the first hole portion 13a and the third hole portion 13c are both straight in a cross-section parallel to the Z direction. Figure 3In (a), on a cross section parallel to the Z direction, the direction in which the first hole 13a extends is not on the same straight line as the direction in which the third hole 13c extends, and they are not parallel. For example, the angle θ1 formed by the third hole 13c and the Z direction is smaller than the angle θ2 formed by the first hole 13a and the Z direction.
[0085] In the component 120a for a semiconductor manufacturing apparatus, on a cross-section parallel to the Z direction, the boundary 15 where the first hole 13a and the third hole 13c meet is an angle. However, in Figure 3 In the cross section (a), the boundary 15 can also be rounded and curved, having curvature.
[0086] exist Figure 3 In the semiconductor manufacturing apparatus component 120b shown in (b), the third hole portion 13c is straight in a cross-section parallel to the Z direction, while the first hole portion 13a is bent. For example, the first hole portion 13a has a first region 16a that contacts the first surface 11 and a second region 16b that contacts the third hole portion 13c. Figure 3 In the cross section (b), region 16a and region 16b are both straight. Region 16a and region 16b can also be curved.
[0087] exist Figure 3 In example (b), the directions of extension of region 16a and region 16b are not on the same straight line and are not parallel. For example, the angle θ3 formed by region 16b and the Z direction is smaller than the angle θ4 formed by region 16a and the Z direction. Figure 3 In example (b), the direction in which the second region 16b extends is on the same straight line as the direction in which the third hole 13c extends.
[0088] In the component 120b of the semiconductor manufacturing apparatus, on a cross-section parallel to the Z direction, the boundary 16c where the first region 16a and the second region 16b meet is an angle. However, in Figure 3 In the cross section (b), the boundary 16c can also be rounded and curved, having curvature.
[0089] exist Figure 3 In the semiconductor manufacturing apparatus component 120c shown in (c), the first hole portion 13a has a first region 16a and a second region 16b, and its boundary 16c is an angle. Additionally, the boundary 15 between the first hole portion 13a and the third hole portion 13c is an angle. Boundaries 15 and 16c may also be rounded and curved, having curvature. As described above, the cross-sectional shape of the hole 13 can be appropriately bent or curved.
[0090] When evaluating the arithmetic mean height Sa, a laser microscope is used to examine the arithmetic mean height Sa of the surface being evaluated. This arithmetic mean height Sa is specified in the international standard ISO 025178 (JIS B 0681) concerning three-dimensional surface properties.
[0091] As a laser microscope, a "VK-X1000 / KEYENCE" is used. The objective lens magnification is set to 1000x. The S-filter is set to 2.5μm or 0.8μm, and the L-filter is set to 0.5mm.
[0092] The arithmetic mean height is a three-dimensional roughness parameter (three-dimensional height direction parameter) that extends the two-dimensional arithmetic mean roughness Ra to three dimensions. Specifically, the arithmetic mean height Sa is the volume of the portion enclosed by the surface shape curve and the mean surface divided by the measured area. Let the mean surface be the xy plane, the longitudinal direction be the z-axis, and the measured surface shape curve be z(x, y), then the arithmetic mean height Sa is defined by the following formula. Here, “A” in formula (1) is the measured area. [Formula 1]
[0093] The density of the ceramic layer 20 represents the size of the (nanoscale) gaps between the particles constituting the film. The density of the ceramic layer 20 (the density of part 1 21, part 22, and part 3 23, etc., described later) can be evaluated using, for example, the brightness Sa calculated according to the method described in Patent No. 6597922. In an embodiment, high density corresponds to low brightness Sa.
[0094] Furthermore, in this embodiment, the surface hardness of the ceramic layer 20 and the substrate 10 (the hardness of Part 1 21, Part 2 22, and the first hole region 313a and the third hole region 313c, described later) can be evaluated using the method specified in ISO 14577. Specifically, the surface of the evaluation object is subjected to hardness measurement based on a micro-indentation hardness test (nano-indentation). A Glasswell indenter is used, and the indentation depth is set to a fixed value of 200 nm. The indentation hardness (HIT) is measured. Surfaces other than damaged or dented surfaces are selected as the measurement locations for the HIT of the evaluation object's surface. More preferably, the surface of the evaluation object is a smooth surface after grinding. The number of measurement points is set to at least 25 points. The average value of the measured HIT of 25 or more points is taken as the hardness in this embodiment. Other test methods and analytical methods, performance verification procedures for test apparatus, and conditions required by standard reference samples comply with ISO 14577.
[0095] In this implementation, high plasma corrosion resistance corresponds to a small arithmetic mean height Sa of the surface after the baseline plasma resistance test. The baseline plasma resistance test is performed as follows: Plasma is irradiated onto the surface of the evaluation object, such as a ceramic layer or substrate. An inductively coupled plasma reactive ion etching apparatus (Muc-21Rv-Aps-Se / Sumitomo Precision Industries) is used as the plasma etching apparatus. The plasma etching conditions are as follows: the ICP output is set to 1500W, the bias output to 750W, a mixture of 100ccm CHF3 and 10ccm O2 gas is used as the process gas, the pressure is set to 0.5Pa, and the plasma etching time is set to 1 hour. The surface condition of the evaluation object after plasma irradiation is photographed using a laser microscope. Specifically, an OLS4500 / Olympus laser microscope was used with an MPLAPON 100xLEXT objective lens (0.95 apertures, 0.35 mm working distance, 0.52 μm focal spot diameter, 128 × 128 μm measurement area), and the magnification was set to 100x. A λc filter to remove fluctuation components was set to 25 μm. Measurements were performed at any three locations, and the average value was taken as the arithmetic mean height Sa. Other appropriate references were made to the international standard ISO 25178 for three-dimensional surface properties. As one embodiment of the invention, the arithmetic mean height Sa of the ceramic layer or substrate surface after the "reference plasma resistance test" is preferably 0.060 or less, more preferably 0.030 or less.
[0096] Reference Figure 4 (a)~ Figure 4 (c) The calculation methods for angles θα and θβ in this application specification are explained. Figure 4 (a)~ Figure 4 (c) is a cross-sectional view illustrating a portion of the substrate according to the first embodiment.
[0097] Figure 4 (a) The substrate 10a shown is related to Figure 2 The substrate 10 described is the same. The first surface 11 extends along the XY plane. The second hole 13b extends along the Z direction. In this example, the inclined surface 13ac connecting the first surface 11 and the second hole 13b is straight in a cross-section parallel to the Z direction. In the cross-section parallel to the Z direction, the inclined surface 13ac extends straight from end e1 of the first surface 11 to end e2 of the second hole 13b. End e1 is the point where the first surface 11 contacts the inclined surface 13ac, and end e2 is the point where the second hole 13b contacts the inclined surface 13ac.
[0098] In a cross-section parallel to the Z direction, when the portion P1 of the inclined surface 13ac, continuous with the first surface 11, is a straight line, θα is the angle between the first surface 11 and portion P1. In a cross-section parallel to the Z direction, when the portion P2 of the inclined surface 13ac, continuous with the second hole portion 13b, is a straight line, θβ is the angle between the second hole portion 13b and portion P2. Figure 4 In example (a), angle θα is the angle formed by the line segment connecting the first surface 11 and the connecting end e1 and end e2, and angle θβ is the angle formed by the second hole 13b and the line segment connecting the connecting end e1 and end e2. In addition, angles θα and θβ are angles inside the substrate 10, which are 180° or less.
[0099] like Figure 4 (b) and Figure 4 As shown in (c), when parts P1 and P2 bend on the cross section parallel to the Z direction, the angles θα and θβ are calculated as follows. Figure 4 (b) The substrate 10b shown differs from substrate 10a in the shape of the inclined surface 13ac. In substrate 10b, on a cross-section parallel to the Z direction, the portion P1 of the inclined surface 13ac that is continuous with the first surface 11 is curved, while the portion continuous with part P1 is straight. At this time, the angle θα is as follows... Figure 4 (b) shows the angle formed by the first surface 11 and line segment L1. Line segment L1 is the line segment connecting end e1 and end e4, and end e4 is the endpoint of the straight section in the inclined surface 13ac that is continuous with part P1. Furthermore, in the substrate 10b, on a cross-section parallel to the Z direction, the portion P2 in the inclined surface 13ac that is continuous with the second hole 13b is curved, and the portion continuous with part P2 is straight. At this time, the angle θβ is as follows: Figure 4 (b) shows the angle formed by the second hole portion 13b and line segment L2. Line segment L2 is the line segment connecting end e2 and end e3, and end e3 is the endpoint of the straight section in the inclined surface 13ac that is continuous with portion P2. In this example, in the inclined surface 13ac, there is a straight section P3 between portion P1 and portion P2, and end e3 of portion P3 is the point where portion P3 contacts portion P1, and end e4 of portion P3 is the point where portion P3 contacts portion P2.
[0100] Figure 4 (c) shows a substrate 10c that differs from substrate 10a in the shape of its inclined surface 13ac. In substrate 10c, the inclined surface 13ac is curved on a cross-section parallel to the Z direction. In this case, the angle θα is as follows... Figure 4 (c) shows the angle formed by the first surface 11 and the line segment L3 connecting end e1 and end e2. Furthermore, at this time, angle θβ is as follows: Figure 4(c) shows the angle formed by the second hole 13b and line segment L3.
[0101] The substrate 10 can also be any one of metal, ceramic, glass, plastic, or a combination thereof. Preferably, the substrate 10 is metal or ceramic. Metals can be aluminum or aluminum alloys with anodized surfaces (aluminum anodizing). Ceramic materials can be alumina, aluminum nitride, etc.
[0102] The ceramic layer 20 includes, for example, polycrystalline ceramic. The ceramic layer 20 is a layer primarily composed of ceramic. The ceramic layer 20 includes at least one selected from, for example, oxides of rare earth elements, fluorides of rare earth elements, and fluoride oxides of rare earth elements. For example, as rare earth elements, at least one selected from Y, Sc, Yb, Ce, Pr, Eu, La, Nd, Pm, Sm, Gd, Tb, Dy, Ho, Er, Tm, and Lu can be listed. More specifically, the ceramic layer 20 includes oxides selected from yttrium (Y₂O₃, Y ... α O β (Non-stoichiometric composition), yttrium fluoride oxides (YOF, Y5O4F7, Y6O5F8, Y7O6F9 and Y... 17 O 14 F 23 ), (YO 0.826 F 0.17 )F 1.174 , YF3, Er2O3, Gd2O3, Nd2O3, Y3Al5O 12 , Y4Al2O9, Y2O3-ZrO2, Er3Al5O 12 Gd3Al5O 12 , Er4Al2O9, ErAlO3, Gd4Al2O9, GdAlO3, Nd3Al5O 12 The ceramic layer 20 may contain at least one selected from Fe, Cr, Zn, and Cu. For example, the ceramic layer 20 contains at least one of fluorine and oxygen, and yttrium. The ceramic layer 20 is, for example, composed primarily of yttrium oxide (Y2O3), yttrium fluoride (YF3), or yttrium oxyfluoride (YOF). In this application specification, "main component" means that the component contains more than 50%, preferably more than 70%, more preferably more than 90%, even more preferably more than 95%, and most preferably 100%. The "%" used here refers to, for example, mass.
[0103] Alternatively, the ceramic layer 20 can be a substance other than oxides, fluorides, or fluorine oxides. Specifically, examples include compounds containing Cl and Br elements (chlorides, bromides).
[0104] In the component 120 of the semiconductor manufacturing apparatus, the ceramic layer 20 may be composed of only polycrystalline ceramic, or it may include polycrystalline ceramic and amorphous ceramic.
[0105] In the ceramic layer 20, the average crystallite size of the polycrystalline ceramic is between 3 nm and 50 nm. Preferably, the upper limit is 30 nm, more preferably 20 nm, and even more preferably 15 nm. In addition, the lower limit is preferably 5 nm.
[0106] The "average crystallite size" can be obtained by the following method. First, a transmission electron microscope (TEM) image is captured at a magnification of 400,000x or higher. In this image, the average crystallite size is calculated based on the average diameter of 15 approximately circular crystallites. If the sample thickness during FIB processing is sufficiently thin (around 30 nm), the crystallites can be more clearly identified. The magnification can be appropriately selected, for example, within the range of 400,000x to 2,000,000x.
[0107] In the manufacturing steps of the semiconductor manufacturing apparatus component according to the embodiment, a substrate 10 having holes 13 is first prepared. Then, the shape of the substrate 10 is adjusted by appropriate means. For example, the substrate 10 is subjected to at least one of the following treatments: sandblasting, physical polishing, chemical mechanical polishing, polishing, and chemical polishing. As a result, the arithmetic mean height Sa (surface roughness) and shape of the first surface 11 and the holes 13 (first hole portion 13a, second hole portion 13b, and third hole portion 13c) can be controlled.
[0108] Next, a ceramic layer 20 is formed on the substrate 10. After the ceramic layer 20 is formed, fine grinding is performed. Grinding can be performed using at least one of sandblasting, physical grinding, chemical mechanical polishing, polishing (lapping), and chemical grinding. Thus, for example, the arithmetic mean height Sa and shape of the ceramic layer 20 (surface 21s of the first part 21 and surface 22s of the second part 22), the second hole 13b, and the third hole 13c can be controlled.
[0109] Alternatively, the method for forming the ceramic layer 20 on the substrate 10 can be, for example, spraying, CVD, ALD (Atomic Layer Deposition), PVD (Physical Vaper Deposition), or aerosol deposition.
[0110] When forming a ceramic layer 20 on the substrate 10, for example using aerosol deposition, spraying, CVD, or PVD, a mask such as tape can be applied to the portion that becomes the third hole 13c before forming the film that becomes the ceramic layer 20. By removing the mask after film formation, the second hole 13b and the third hole 13c, which are exposed without the ceramic layer 20, are formed. Alternatively, the second hole 13b and the third hole 13c can be exposed by removing a portion of the film after film formation, such as by grinding, without applying a mask.
[0111] According to the method of forming ceramic layer 20, the ceramic layer 20 may be difficult to form on the inner peripheral surface 13s, i.e., the third hole portion 13c, compared to the first surface 11. That is, in methods such as PVD, spraying, and aerosol deposition, where raw material particles are supplied (e.g., collided with) to the substrate 10 from the first surface 11 side to form a ceramic layer, since the third hole portion 13c is separated from the first surface 11 and tilted relative to it, the raw material particles may reach the third hole portion 13c in a state different from the plane, such as being difficult to reach. In this case, if it is assumed that the ceramic layer 20 is formed on the third hole portion 13c, the quality (e.g., density, hardness, etc.) of the ceramic layer 20 formed on the third hole portion 13c may be lower than the quality of the ceramic layer 20 formed on the first surface 11. A portion of the low-quality and fragile ceramic layer 20 is more likely to detach from the substrate and may become a source of particle generation. By not providing a ceramic layer 20 in the third hole 13c, the generation of particles can be reduced.
[0112] For example, in the third hole 13c, it is sometimes difficult to form a ceramic layer on the inner wall (vertical surface) of the hole 13. When a ceramic layer is provided inside the hole 13, the properties (e.g., density and film thickness) of the ceramic layer inside the hole 13 may be worse than those of the ceramic layer provided on the first surface of the substrate. When the fragile ceramic layer inside the hole 13 is corroded by plasma, particles may be generated. Furthermore, for example, the mechanical properties (e.g., strength, hardness, or toughness relative to external forces) of the poorly shaped ceramic layer may be worse than those of the substrate. Therefore, particles may be generated due to physical impacts or contact during the handling or maintenance of components for semiconductor manufacturing equipment.
[0113] For example, when the ceramic layer 20 is formed by PVD, spraying or aerosol deposition, it is not easy to form a film on the vertical second pore portion 13b. Since the second pore portion 13b is relatively long, film formation inside the pore can be suppressed.
[0114] Furthermore, in aerosol deposition, microparticles, serving as the material, collide with a substrate, and the impact of these collisions causes the microparticles to bond together on the substrate, forming a layered structure. On the other hand, in aerosol deposition, if the substrate surface where the microparticles collide is rough, the microparticles are difficult to bond and aggregate on the substrate, making it difficult to form a layered structure. In this embodiment, since the arithmetic mean height Sa of the third pore 13c is relatively large, the formation of a fragile ceramic layer on the third pore 13c by aerosol deposition can be more reliably suppressed. Therefore, particle generation can be suppressed.
[0115] Thus, when using aerosol deposition, for example, by controlling the arithmetic mean height Sa of the third hole 13c, the formation of a ceramic layer on the third hole 13c can be suppressed. When using aerosol deposition, since processes such as masking before film formation can be omitted, it is easier to manufacture components for semiconductor manufacturing devices.
[0116] The "aerosol deposition method" is as follows: an "aerosol" containing brittle material particles dispersed in a gas is sprayed from a nozzle onto a substrate, causing the particles to collide with the substrate such as metal, glass, ceramic, or plastic. The impact of the collision causes the brittle material particles to deform or break, and these particles are bonded together, thereby directly forming a layered structure (also known as a film structure) composed of the constituent materials of the particles on the substrate.
[0117] In this example, an aerosol, consisting of a mixture of particles and gaseous materials of ceramic materials with excellent particle resistance, such as yttrium, is sprayed onto the substrate 10 to form a layered structure (ceramic layer 20).
[0118] According to the aerosol deposition method, layered structures can be formed at room temperature without the need for heating and cooling devices, and layered structures with mechanical strength equal to or greater than that of sintered bodies can be obtained. In addition, by controlling the conditions of particle collision, the shape and composition of particles, the density, microstructure, mechanical strength, and electrical properties of the layered structures can be varied.
[0119] Furthermore, in this article, "polycrystalline" refers to a structure formed by the aggregation and condensation of grains. A grain is essentially composed of a single crystal. The diameter of the grain is typically greater than 5 nanometers (nm). However, when particles are not broken up and enter the structure, the grain is considered polycrystalline.
[0120] Furthermore, in this application specification, "microparticle" refers to particles with an average particle size of 5 micrometers (μm) or less, as determined by particle size distribution measurement or scanning electron microscopy, when the primary particles are dense particles. When the primary particles are porous particles that are easily broken by impact, it refers to particles with an average particle size of 50 μm or less.
[0121] Furthermore, in this application specification, "aerosol" refers to a solid-gas mixture in which the aforementioned particles are dispersed in a gas such as helium, nitrogen, argon, oxygen, dry air, or a mixture of these. Although it may sometimes contain some "agglomerates," it essentially refers to the state in which the particles are individually dispersed. The gas pressure and temperature of the aerosol are arbitrary, but it is preferable that, when the gas pressure is converted to 1 atmosphere and the temperature to 20 degrees Celsius, the concentration of particles in the gas is in the range of 0.0003 mL / L to 5 mL / L when ejected from the outlet, so as to facilitate the formation of layered structures.
[0122] Aerosol deposition is typically carried out at room temperature, and one of its characteristics is that it can form layered structures at temperatures sufficiently below the melting point of the microparticle material, i.e. below 100 degrees Celsius. In addition, in this application specification, "room temperature" refers to a temperature significantly lower than the sintering temperature of ceramics, which in fact refers to an environment of 0 to 100°C, and more generally refers to room temperature around 20°C ± 10°C.
[0123] The powder particles constituting the layered structure are mainly brittle materials such as ceramics and semiconductors. Besides using particles of the same material alone or mixing particles of different sizes, different types of brittle material particles can also be mixed or combined. Additionally, particles such as metallic and organic materials can be mixed into the brittle material particles or coated onto the surface of the brittle material particles. Even in these cases, the main material forming the layered structure is still a brittle material.
[0124] In the composite structure formed by this method, when crystalline brittle material particles are used as raw materials, the layered structure portion of the composite structure is a polycrystalline material with a grain size smaller than that of the raw material particles, and its crystals are substantially devoid of crystalline orientation. Furthermore, at the interfaces between the brittle material crystals, there is substantially no grain boundary layer composed of glass layers. Moreover, in most cases, the layered structure portion of the composite structure forms an "anchoring layer" that penetrates deep into the surface of the substrate (substrate 10 in this example). The layered structure with this anchoring layer is firmly attached to and formed on the substrate with extremely high strength.
[0125] The layered structures formed by aerosol deposition are significantly different from so-called "pressed powders," which are formed by pressing particles together under pressure and maintaining their shape through physical adhesion. They possess sufficient strength.
[0126] In aerosol deposition, the size of the brittle material particles used as raw materials and the crystallites (grains) of the resulting brittle material structures can be measured using methods such as X-ray diffraction to confirm the breakage and deformation of the incoming brittle material particles on the substrate. That is, the crystallite size of the layered structures formed by aerosol deposition is smaller than the crystallite size of the raw material particles. On the "dislocation surfaces" or "fracture surfaces" formed by particle crushing or deformation, "newly formed surfaces" are created, where atoms that were originally present inside the particles and bonded with other atoms become exposed. It is believed that these newly formed surfaces, with their high surface energy and high activity, combine with the surfaces of adjacent brittle material particles, or the newly formed surfaces of other adjacent brittle materials, or the surface of the substrate to form layered structures.
[0127] Alternatively, it can be argued that when hydroxyl groups are appropriately present on the surface of particles in aerosols, local shear stress generated between particles or between particles and structures during particle collisions leads to mechanochemical acid-base dehydration reactions, causing them to bond together. It can also be argued that continuous external mechanical impact forces cause these phenomena to persist, and through repeated deformation and breakage of particles, bonding develops and densifies, resulting in the growth of layered structures composed of brittle materials.
[0128] For example, when the ceramic layer 20 is formed by aerosol deposition, compared to sintered ceramic bodies or sprayed films, the ceramic layer 20 has a microstructure with small and dense crystallite sizes. Therefore, the particle resistance of the semiconductor manufacturing apparatus component 120 according to the embodiment is higher than that of sintered bodies or sprayed films. Furthermore, the probability of the semiconductor manufacturing apparatus component 120 of the embodiment becoming a particle generation source is lower than that of sintered bodies or sprayed films.
[0129] An example of an apparatus used when manufacturing the semiconductor manufacturing apparatus component 120 of the present invention using aerosol deposition will be described. The apparatus for aerosol deposition comprises a chamber, an aerosol supply unit, a gas supply unit, an exhaust unit, and piping. Inside the chamber, for example, a stage for mounting the substrate 10, a drive unit, and a nozzle are arranged. The drive unit allows the relative positions of the substrate 10 and the nozzle mounted on the stage to be changed. The distance between the nozzle and the substrate 10 can be constant or variable. In this example, the drive unit drives the stage, but the drive unit can also drive the nozzle. The driving direction is, for example, the XYZθ direction.
[0130] The aerosol supply unit is connected to the gas supply unit via piping. In the aerosol supply unit, an aerosol mixture of raw material particles and gas is supplied to the nozzle via piping. The apparatus also includes a powder supply unit for supplying the raw material particles. The powder supply unit can be located within the aerosol supply unit or separately from it. Additionally, an aerosol forming unit for mixing the raw material particles and gas can be provided outside the aerosol supply unit. By controlling the supply rate from the aerosol supply unit to maintain a constant amount of particles ejected from the nozzle, a homogeneous structure can be obtained.
[0131] The gas supply unit supplies nitrogen, helium, argon, air, etc. When the supplied gas is air, it is preferable to use compressed air with fewer impurities such as moisture and oil, or an air treatment unit is provided to remove impurities from the air.
[0132] Next, an example of the operation of the apparatus used in the aerosol deposition method will be described. With the substrate 10 placed on the stage in the chamber, the pressure inside the chamber is reduced to below atmospheric pressure by an exhaust unit such as a vacuum pump, specifically to about several hundred Pa. On the other hand, the internal pressure of the aerosol supply unit is set to be higher than the internal pressure of the chamber. The internal pressure of the aerosol supply unit is, for example, several hundred to tens of thousands of Pa. The powder supply unit can also be set to atmospheric pressure. By the pressure difference between the chamber and the aerosol supply unit, the particles in the aerosol are accelerated so that the ejection velocity of the raw material particles from the nozzle is in the subsonic to supersonic (50 to 500 m / s) range. The ejection velocity is controlled by the flow rate of the gas supplied from the gas supply unit, the type of gas, the shape of the nozzle, the length and inner diameter of the piping, the exhaust volume of the exhaust unit, etc. For example, a supersonic nozzle such as a Laval nozzle can also be used as the nozzle. The particles in the aerosol ejected at high speed from the nozzle collide with the substrate 10, and are crushed or deformed, thus accumulating on the substrate 10 as a structure (ceramic layer 20). By changing the relative position of the substrate 10 and the nozzle, a composite structure (semiconductor manufacturing device component 120) is formed on the substrate 10 having a structure (ceramic layer 20) with a specified area.
[0133] Alternatively, a fragmentation section can be installed before the nozzle to break up the agglomeration of particles. The fragmentation method in the fragmentation section can be any method. Examples include mechanical fragmentation such as vibration and impact, as well as well-known methods such as electrostatic discharge, plasma irradiation, and classification.
[0134] (Second Implementation) Figure 5 (a) and 5(b) are cross-sectional views illustrating a portion of a component of a semiconductor manufacturing apparatus according to the second embodiment.
[0135] The same description as that for component 120 in a semiconductor manufacturing apparatus can be applied to... Figure 5(a) shows the component 120d for a semiconductor manufacturing apparatus. However, the arithmetic mean height Sa of the surface of the first part 21 may not be less than the arithmetic mean height Sa of the surface of the second part 22, or it may be the same as that of the component 120 for a semiconductor manufacturing apparatus. In addition, the arithmetic mean height Sa of the third hole 13c may not be greater than the arithmetic mean height Sa of the surfaces of the first part 21 and the second part 22, or it may be the same as that of the component 120 for a semiconductor manufacturing apparatus.
[0136] like Figure 5 As shown in (a), the component 120d for a semiconductor manufacturing apparatus has a composite structure 30. A composite structure refers to a structure having a substrate and a structure (e.g., a layer or film) disposed on the surface of the substrate. The composite structure 30 includes a substrate 10 and a ceramic layer 20. In this example, the composite structure 30 is a stack of the substrate 10 and the ceramic layer 20. Alternatively, in an embodiment, the substrate 10 and the ceramic layer 20 may each have a stacked structure comprising multiple layers.
[0137] like Figure 5 As shown in (a), the composite structure 30 has a first main surface 311 and a second main surface 312 opposite to the first main surface 311. For example, the first main surface 311 is the surface 21s of the first portion of the ceramic layer 20, and the second main surface 312 is the second surface 12 of the substrate 10. In addition, at least one through-hole 313 is provided in the composite structure 30. The through-hole 313 extends along the Z direction and penetrates the substrate 10 and the ceramic layer 20. For example, a through-hole 313 is provided in the center of the composite structure 30. However, the through-hole 313 may not be in the center of the composite structure 30, or multiple through-holes may be provided.
[0138] When viewed along the Z-direction, the through-hole 313 is, for example, circular. The through-hole 313 (the inner circumferential surface 313s of the through-hole) has a first hole region 313a, a second hole region 313b, and a third hole region 313c. The first hole region 313a, the second hole region 313b, and the third hole region 313c are respectively arranged to be exposed to contact with plasma. The inner circumferential surface 313s is the inner circumferential surface of the composite structure 30 defining the through-hole 313. The inner circumferential surface 313s faces inwards towards the through-hole 313 and intersects the XY plane.
[0139] The first hole region 313a is located near the first principal surface 311 in the inner peripheral surface 313s, and is the region adjacent to the first principal surface 311. The first hole region 313a is continuous with the first principal surface 311. The first hole region 313a is located between the first principal surface 311 and the second principal surface 312 in the Z direction. The first hole region 313a is an inclined surface that is not parallel to the first principal surface 311 and intersects the first principal surface 311 and the Z direction. The first hole region 313a can also be a surface extending parallel to the Z direction. In a cross-section parallel to the Z direction, the first hole region 313a can be straight or curved. When viewed along the Z direction (i.e., when projected onto the XY plane), the first hole region 313a is, for example, an annular shape surrounded by the first principal surface 311.
[0140] The second hole region 313b is located in the Z direction between the first hole region 313a and the second main surface 312. In other words, the position of the second hole region 313b in the Z direction is between the position of the first hole region 313a in the Z direction and the position of the second main surface 312 in the Z direction. For example, the second hole region 313b is located near the second main surface 312 in the inner peripheral surface 313s, and is the region adjacent to the second main surface 312. The second hole region 313b may be continuous with the second main surface 312. The second hole region 313b extends along the Z direction, for example, parallel to the Z direction. The second hole region 313b is, for example, a vertical plane that is approximately perpendicular to the second main surface 312. When viewed along the Z direction, the second hole region 313b is, for example, an annular shape located inside the first hole region 313a.
[0141] The third hole region 313c is located in the Z direction between the first hole region 313a and the second hole region 313b. In other words, the position of the third hole region 313c in the Z direction is between the position of the first hole region 313a in the Z direction and the position of the second hole region 313b in the Z direction. The third hole region 313c is a region in the inner circumferential surface 313s that is continuous with the first hole region 313a. The third hole region 313c is an inclined surface that is not parallel to the first surface 11 and intersects the first surface 11 and the Z direction. The third hole region 313c can also be a surface extending along the Z direction. In a cross-section parallel to the Z direction, the third hole region 313c can be straight or curved. When viewed along the Z direction, the third hole region 313c is, for example, an annular shape that is surrounded and in contact with the first hole region 313a, and the second hole region 313b is located inside the third hole region 313c. Region 313c of the third borehole can be continuous with region 313b of the second borehole.
[0142] exist Figure 5In example (a), the first hole region 313a of the through hole 313 is the surface 22s of the second portion 22 of the ceramic layer 20, the second hole region 313b is the second hole portion 13b of the hole 13 in the substrate 10, and the third hole region 313c is the third hole portion 13c of the hole 13 in the substrate 10. A portion of the through hole 313 of the composite structure 30 is at least a portion of the hole 13 in the substrate 10. Specifically, a portion of the through hole 313 is defined by the second hole portion 13b and the third hole portion 13c of the hole 13 in the substrate 10.
[0143] The hardness of the third hole region 313c is higher than that of the first hole region 313a. For example, the third hole region 313c is less prone to wear than the first hole region 313a. Figure 5 In example (a), the hardness of the third pore portion 13c of the substrate 10 is higher than the hardness of the surface 22s of the ceramic layer 20. For example, the hardness of the material of the substrate 10 is higher than the hardness of the material of the ceramic layer 20. As a result, the hardness of the third pore region 313c can be higher than the hardness of the first pore region 313a. Specifically, the materials of the first portion 21 and the second portion 22 of the ceramic layer 20 can be at least one of oxides of rare earth elements, fluorides of rare earth elements, and fluorides of rare earth elements. The rare earth element is at least one selected from the group consisting of Y, Sc, Yb, Ce, Pr, Eu, La, Nd, Pm, Sm, Gd, Tb, Dy, Ho, Er, Tm, and Lu. In addition, the material of the substrate 10 can be at least one of alumina (Al2O3), zirconium oxide (ZrO2), and aluminum nitride (AlN).
[0144] The third hole region 313c is located further inside the through hole 313 than the first hole region 313a. For example, during the handling of components for a semiconductor manufacturing apparatus, when a fixture such as a locating pin is inserted into the through hole 313, the third hole region 313c is more likely to come into physical contact with the fixture than the first hole region 313a. Furthermore, for example, during the maintenance of components for a semiconductor manufacturing apparatus, when both the first hole region 313a and the third hole region 313c come into contact with a cleaning pad, if the angle θβ is less than the angle θα, the third hole region 313c may be more prone to wear than the first hole region 313a. For example, when the angle θβ is less than the angle θα, the area near the corner of the boundary between the third hole region 313c and the second hole region 313b is more likely to experience force concentration than the area near the corner of the boundary between the first hole region 313a and the first main surface 311, thus leading to more wear.
[0145] In contrast, in this embodiment, since the third hole region 313c has relatively high hardness, damage to the third hole region 313c due to physical contact during maintenance or handling of components for semiconductor manufacturing apparatus can be suppressed. Therefore, particle generation can be suppressed.
[0146] Figure 5 (b) The semiconductor manufacturing apparatus component 120e differs from the semiconductor manufacturing apparatus component 120d in that the ceramic layer 20 has a third portion 23. In the semiconductor manufacturing apparatus component 120e, the third hole region 313c is the surface 23s of the third portion 23. Otherwise, the same description as that for the semiconductor manufacturing apparatus component 120d can be applied to the semiconductor manufacturing apparatus component 120e.
[0147] The third portion 23 of the ceramic layer 20 is disposed on and in contact with the third hole 13c. The third portion 23 is disposed continuously from the second portion 22. The surface 23s of the third portion 23 is in direct contact with the plasma. That is, the surface 23s is the side opposite to the surface of the third portion 23 that contacts the third hole 13c, and is configured to be exposed into the chamber 110. In this example, the first hole 13a and the third hole 13c are covered by the ceramic layer 20 and are not in direct contact with the plasma. As a result, the generation of particles from the first hole 13a and the third hole 13c of the substrate hole 13 can be suppressed. On the other hand, as Figure 5 As shown in (a), if the ceramic layer 20 is not provided on the third hole portion 13c, it is possible to suppress the formation of a ceramic layer 20 with poor properties on the third hole portion 13c, thereby suppressing the generation of particles from the ceramic layer 20.
[0148] exist Figure 5 In example (b), the first hole region 313a of the through hole 313 is the surface 22s of the second portion 22 of the ceramic layer 20, the second hole region 313b is the second hole portion 13b of the hole 13 in the substrate 10, and the third hole region 313c is the surface 23s of the third portion 23 of the ceramic layer 20. In this example, a portion of the through hole 313 of the composite structure 30 is also at least a portion of the hole 13 in the substrate 10. Specifically, a portion of the through hole 313 is defined by the second hole portion 13b of the hole 13 in the substrate 10.
[0149] In the component 120e for a semiconductor manufacturing apparatus, the hardness of the third hole region 313c is also higher than that of the first hole region 313a. That is, the hardness of the surface 23s of the third portion 23 of the ceramic layer 20 is higher than that of the surface 22s of the second portion 22 of the ceramic layer 20. As a result, damage to the third hole region 313c due to physical contact during maintenance or handling of the component for the semiconductor manufacturing apparatus can be suppressed. This also helps to suppress the generation of particles.
[0150] For example, the material of part 23 is different from the material of part 22, and the hardness of the material of part 23 is higher than that of the material of part 22. Therefore, the hardness of the third pore region 313c can be higher than that of the first pore region 313a. For example, the material of part 23 can be at least one of oxides of rare earth elements, fluorides of rare earth elements, and fluorides of rare earth elements. The rare earth element is at least one selected from the group consisting of Y, Sc, Yb, Ce, Pr, Eu, La, Nd, Pm, Sm, Gd, Tb, Dy, Ho, Er, Tm, and Lu. By making the composition of part 23 different from that of part 22, the hardness of part 23 can be different from that of part 22.
[0151] By using a masking material such as tape, the film that becomes part 22 and the film that becomes part 23 can be respectively set within desired ranges. For example, with a mask set on part 13a or part 22, the film of part 23 can be formed on part 3c. Alternatively, with a mask set on part 3c or part 23, the film of part 22 can be formed on part 13a. Thus, independent films can be formed on part 13a and part 13c, and the material of part 23 can be different from that of part 22. Therefore, the hardness of part 23 can be different from that of part 22. Alternatively, without using a masking material, independent films can be formed on part 13a and part 13c by removing a portion of the film after film formation through grinding or the like.
[0152] For example, the density of part 3 23 is higher than that of part 2 22. Therefore, the hardness of the third pore region 313c can be higher than that of the first pore region 313a. For example, parts 22 and 23 can be formed by performing a surface modification treatment on a portion of the film after forming a film that becomes parts 22 and 23. As an example of surface modification treatment, a method can be described as follows: after applying energy from the surface of the film to a predetermined depth range and melting it, cooling that range to form a molten solidified film. The molten solidified film formed by surface modification treatment is a dense film with fewer pores and a flattened surface compared to the area without surface modification treatment. Surface modification treatment can also employ methods that selectively thermally melt the surface. Specifically, examples of surface modification treatment include laser annealing or plasma jetting. For example, the area where surface modification treatment was performed becomes part 3 23, and the area where surface modification treatment was not performed becomes part 2 22.
[0153] The film-forming conditions of Part 3 23 can differ from those of Part 2 22. This can result in different densities or hardnesses between Part 3 23 and Part 2 22. When using aerosol deposition, these film-forming conditions can include, for example, the flow rate, velocity, or type of gas supplied from the gas supply unit. The film-forming conditions can also be determined by the angle at which the aerosol ejected from the nozzle impacts the substrate.
[0154] Alternatively, in this embodiment, the ceramic layer 20 may not necessarily be provided on the first hole portion 13a and the third hole portion 13c. The first hole region 313a may be the surface of the substrate 10. The hardness of a portion of the substrate surface may be appropriately adjusted by surface treatment (e.g., coating or modification treatment).
[0155] Figure 6 (a) and Figure 6 (b) is a cross-sectional view illustrating a portion of a component used in a semiconductor manufacturing apparatus. Figure 6 (a) Figure 6 (b) represents the substrate 10 of the components for a semiconductor manufacturing apparatus. Figure 6 (a) The composition and related aspects of the substrate 10 shown Figure 2 The substrate 10 is the same. Figure 6 In substrate 10 of (a), angle θα is 150°.
[0156] exist Figure 6 (b) shows that the angle θα in the substrate 10 is 120°. Figure 6 (b) The substrate 10 differs from the substrate 10 in the shape (length and angle) of the inclined surface 13ac and the length of the second hole 13b. Figure 6 (a) Substrate 10. In addition, Figure 6 (b) The composition of the substrate 10 and Figure 6 (a) is the same as the substrate 10.
[0157] exist Figure 6 In substrate 10 shown in (a), angle θα is greater than angle θβ. Figure 6 In substrate 10 shown in (b), angle θα is less than angle θβ. Figure 6 (a) The length Ln in the Z direction of the second hole 13b of the substrate 10 is greater than that of the substrate 10. Figure 6 (b) The length Ln in the Z direction of the second hole portion 13b of the substrate 10 is longer. Thus, when the thickness of the substrate 10 is fixed, if θα is greater than the angle θβ, it is easy to make the length of the second hole portion 13b in the Z direction longer.
[0158] Figure 6Figures (a) and (b) show the proximal circle PC. The proximal circle PC approaches the edge (boundary 14) formed by the first surface 11 and the inclined surface 13ac. The proximal circle PC is as follows: Figure 6 (a) and Figure 6 (b) The circle that contacts the first surface 11 and the inclined surface 13ac on the cross section parallel to the Z direction. Figure 6 The distance (distance t2) between the position of the center p of the proximal circle PC in the X direction and the position of the boundary 14 in the X direction in (a) is... Figure 6 In (b), the distance (distance t2) between the X-direction position of the center p of the proximal circle PC and the X-direction position of the boundary 14 is the same. That is, in Figure 6 (a) and Figure 6 In (b), if the positions of the boundaries 14 in the X direction are aligned, then the positions of the centers p in the X direction will also be aligned. At this point, Figure 6 (a) and Figure 6 (b) The slope width t shown is constant. That is, Figure 6 (a) width t and Figure 6 (b) The widths t are all equal. If we take Figure 6 Let the radius R of the proximal circle PC shown in (a) be r, then Figure 6 (b) shows that the radius R of the circumcircle PC is 0.47r.
[0159] Here, the width t of the inclination is the sum of the specified distances t1 and t2. Figure 6 In (a), the distance t1 is defined as the distance in the X direction from boundary 14 to the second hole 13b. The distance t1 is defined as constant. That is, Figure 6 The specified distance t1 in (a) and Figure 6 The specified distances t1 in (b) are equal. The width of the inclination t is the distance between the center p of the nearest circle PC and... Figure 6 The distance along the X direction between the second hole 13b in (a).
[0160] Figure 7 It is a graph illustrating the stress of components used in semiconductor manufacturing equipment. Figure 7 The calculation results illustrate the relationship between the radius R of the proximal circle PC and the stress S generated on a component used in a semiconductor manufacturing apparatus. That is, Figure 7 Indicates in relation to Figure 2 Among the same components used in semiconductor manufacturing equipment, and Figure 6 (a) and Figure 6(b) Similarly, the stress S changes when the radius R of the proximity circle PC of the substrate 10 is varied. More specifically, in the substrate 10, the distance t2 (the position of the center p of the proximity circle PC in the X direction, and the position of the boundary 14 in the X direction) and the thickness of the substrate 10 are kept constant, while θα is changed. Accordingly, the stress S generated on the ceramic layer 20 formed on the boundary 14 is calculated when the radius R, the length of the second hole 13b in the Z direction, and the shape (length and angle) of the inclined surface 13ac change. In addition, the angle θα is set to be greater than 90°, where the radius R > 0.27r.
[0161] The stress S is a calculated result of the stress (e.g., residual stress) generated in the connection portion of part 1 21 and part 22 (i.e., the ceramic layer 20 formed on boundary 14). For example, the magnitude of stress S corresponds to the electric field strength of the surface of the ceramic layer 20 on boundary 14.
[0162] As the angle θα increases, the radius R of the proximal circle PC also increases. For example... Figure 7 As shown, the stress S decreases as the radius R increases. For example, as... Figure 6 As shown in (a), let the radius R be r when the angle θα is 150°, and the stress S be approximately s. Figure 6 (b) shows that with an angle θα of 120° and a radius R of 0.47r, the calculated stress S is approximately 1.7s. That is, in Figure 6 In example (a), with Figure 6 Compared to example (b), stress concentration can be suppressed, and the stress is reduced by about 1.7 times. That is, by increasing the angle θα, stress concentration can be mitigated. The angle θα is, for example, 150° or more, and more preferably 160° or more.
[0163] For example, the inclined surface 13ac can be made straight in a cross-section parallel to the Z direction. If the inclined surface 13ac is curved in a cross-section parallel to the Z direction, the electric field will concentrate in the inclined surface 13ac or the ceramic layer 20 on the inclined surface 13ac, thereby generating particles. In contrast, when the inclined surface 13ac is straight in a cross-section parallel to the Z direction, the concentration of the electric field in the inclined surface 13ac or the ceramic layer 20 on the inclined surface 13ac can be further mitigated.
[0164] In addition, for example, when the radius R is 0.3r, the stress S is about 2.5s, and when the radius R is 0.7r, the stress S is about 1.2s.
[0165] Figure 8 This is a table illustrating the evaluation of particle resistance in components used in semiconductor manufacturing equipment. Samples 1-5 were respectively related to Figure 2 The component 120 described is the same as that used in the semiconductor manufacturing apparatus. For example... Figure 8 As shown, in samples 1 to 5, at least one of the arithmetic mean height Sa of the first part 21, the arithmetic mean height Sa of the second part 22, and the arithmetic mean height Sa of the third hole 13c was changed. In samples 1 to 5, except for the arithmetic mean height Sa, other parameters (e.g., angle θα, angle θβ, thickness of substrate 10, etc.) remained constant.
[0166] In sample 1, the arithmetic mean height Sa of part 1 21 is 0.03 μm, the arithmetic mean height Sa of part 2 22 is 0.06 μm, and the arithmetic mean height Sa of the third hole 13c is 0.2 μm. In sample 2, the arithmetic mean height Sa of part 1 21 is 0.03 μm, the arithmetic mean height Sa of part 2 22 is 0.12 μm, and the arithmetic mean height Sa of the third hole 13c is 0.5 μm. In sample 3, the arithmetic mean height Sa of part 1 21 is 0.06 μm, the arithmetic mean height Sa of part 2 22 is 0.35 μm, and the arithmetic mean height Sa of the third pore 13c is 0.3 μm. In sample 4, the arithmetic mean height Sa of part 1 21 is 0.08 μm, the arithmetic mean height Sa of part 2 22 is 0.81 μm, and the arithmetic mean height Sa of the third hole 13c is 0.85 μm. In sample 5, the arithmetic mean height Sa of part 1 21 is 0.15 μm, the arithmetic mean height Sa of part 2 22 is 0.41 μm, and the arithmetic mean height Sa of the third hole 13c is 0.2 μm.
[0167] in addition, Figure 8 This indicates the ratios R21 and R31 for each sample. R21 is the ratio of the arithmetic mean height Sa of part 22 to the arithmetic mean height Sa of part 11. R31 is the ratio of the arithmetic mean height Sa of the third hole 13c to the arithmetic mean height Sa of part 11.
[0168] in addition, Figure 8The particle resistance of each sample was indicated by “◎”, “○”, or “×”. In the evaluation of particle resistance, the samples were irradiated with plasma, and the difference between the arithmetic mean height Sa before and after plasma irradiation was evaluated. The plasma irradiation conditions were as follows. An inductively coupled plasma reactive ion etching apparatus (Muc-21Rv-Aps-Se / Sumitomo Precision Industries) was used as the plasma etching apparatus. The plasma etching conditions were as follows: the ICP (Inductively Coupled Plasma) output was set to 1500W, the bias output was set to 750W, a mixture of 100ccm CHF3 gas and 10ccm O2 gas was used as the process gas, the pressure was set to 0.5Pa, and the plasma etching time was set to 1 hour.
[0169] "◎" indicates that the change in the arithmetic mean height Sa due to plasma irradiation is small in all parts 1 (21), 2 (22), and 3 (13c). "○" indicates that the change in the arithmetic mean height Sa due to plasma irradiation is small in two or more locations in parts 1 (21), 2 (22), and 3 (13c). "×" indicates particle resistance other than "◎" and "○".
[0170] As previously stated, for example, the arithmetic mean height Sa of surface 22s of part 22 is more than 2 times and less than 10 times, more preferably less than 5 times, the arithmetic mean height Sa of surface 21s of part 1. In other words, the ratio R21 is more than 2.0 and less than 10, more preferably less than 5.0. Figure 8 As shown, sample 3, with an R21 ratio of 5.8, exhibits higher particle resistance than sample 4, which has an R21 ratio of 10.1. Samples 1, with an R21 ratio of 2.0, and 2, with an R21 ratio of 4.0, exhibit higher particle resistance than sample 3.
[0171] Furthermore, as previously stated, for example, the arithmetic mean height Sa of the third hole 13c is greater than twice the arithmetic mean height Sa of the surface 21s of the first part 21. In other words, it is greater than R31 by 2.0. Figure 8 As shown, the particle resistance of sample 2 with a ratio R31 of 16.7 and sample 3 with a ratio R31 of 5.0 is higher than that of sample 5 with a ratio R31 of 1.3.
[0172] In addition, regarding Figures 2-6 (b) The cross-sections of the components for the semiconductor manufacturing apparatus described may be cross-sections passing through the hole 13 at the center of the XY plane.
[0173] In this application specification, "perpendicular" and "parallel" include not only strict perpendicularity and strict parallelism, but also deviations such as those in the manufacturing process, as long as they are substantially perpendicular and substantially parallel.
[0174] The embodiments of the present invention have been described above. However, the present invention is not limited to the above description. Regarding the foregoing embodiments, any design modifications made by those skilled in the art that possess the features of the present invention are also included within the scope of the present invention. For example, the shape, size, material, configuration, and arrangement of various elements in a semiconductor manufacturing apparatus, such as components for a semiconductor manufacturing apparatus, are not limited to the illustrated components and can be appropriately modified. Furthermore, as long as it is technically feasible, the elements of the aforementioned embodiments can be combined, and such combined technologies are also included within the scope of the present invention as long as they contain the features of the present invention.
Claims
1. A component for a semiconductor manufacturing apparatus, used within a cavity of the semiconductor manufacturing apparatus, characterized in that, The composite structure comprises: a substrate including a first surface and a second surface opposite to the first surface; and a ceramic layer including a first portion exposed on the first surface of the substrate. The composite structure has a through-hole extending in a first direction from the first surface toward the second surface and penetrating the substrate and the ceramic layer. The through hole has: The first hole region is continuous with the surface of the first part and is inclined relative to the first direction; The second hole region is located between the second surface and the first hole region in the first direction, and extends along the first direction; And the third hole region, located between the first hole region and the second hole region in the first direction, and inclined relative to the first direction. The substrate includes at least one hole penetrating the first surface and the second surface. The holes in the substrate have: The first hole is continuous with the first surface and is inclined relative to the first direction; The second hole is located between the second surface and the first hole in the first direction, and extends along the first direction; and The third hole is located between the first hole and the second hole in the first direction, and is inclined relative to the first direction. The ceramic layer exhibits higher resistance to plasma corrosion than the substrate. The ceramic layer further includes a second portion disposed on the first hole. The first hole region is the surface of the second part. The third hole is set to be exposed, and the area of the third hole is the third hole portion. The hardness of the third hole region is higher than that of the first hole region.
2. The component for a semiconductor manufacturing apparatus according to claim 1, characterized in that, A portion of the through-hole in the composite structure is at least a portion of the hole in the substrate. The holes in the substrate have: An inclined surface, continuous with the first surface, and inclined relative to the first direction; And a vertical plane, located between the second plane and the inclined plane in the first direction, and extending along the first direction. The inclined surface is straight in a cross-section parallel to the first direction.
3. The component for a semiconductor manufacturing apparatus according to claim 1, characterized in that, A portion of the through-hole in the composite structure is at least a portion of the hole in the substrate. The pores of the substrate have: An inclined surface, continuous with the first surface, and inclined relative to the first direction; And a vertical plane, located between the second plane and the inclined plane in the first direction, and extending along the first direction. The angle formed by the first surface and the inclined surface is larger than the angle formed by the vertical surface and the inclined surface.
4. The component for a semiconductor manufacturing apparatus according to claim 1, characterized in that, The ceramic layer further includes a third portion disposed on the third hole. The third hole region is the surface of the third part.
5. The component for a semiconductor manufacturing apparatus according to claim 4, characterized in that, The material of the third part is different from the material of the second part. The material in the third part has a higher hardness than the material in the second part.
6. The component for a semiconductor manufacturing apparatus according to claim 5, characterized in that, The density of the third part is higher than that of the second part.
7. The component for a semiconductor manufacturing apparatus according to any one of claims 1 to 6, characterized in that, The ceramic layer comprises polycrystalline ceramic.
8. The component for a semiconductor manufacturing apparatus according to claim 7, characterized in that, The average crystallite size of the polycrystalline ceramic, calculated from TEM images at magnifications of 400,000 to 2,000,000 times, is greater than 3 nanometers and less than 50 nanometers.
9. A component for a semiconductor manufacturing apparatus according to any one of claims 1 to 6, characterized in that, The ceramic layer comprises at least one selected from oxides of rare earth elements, fluorides of rare earth elements, and fluorine oxides of rare earth elements.
10. The component for a semiconductor manufacturing apparatus according to claim 9, characterized in that, The rare earth element is selected from at least one of Y, Sc, Yb, Ce, Pr, Eu, La, Nd, Pm, Sm, Gd, Tb, Dy, Ho, Er, Tm and Lu.
11. The component for a semiconductor manufacturing apparatus according to any one of claims 1 to 6, characterized in that, The substrate comprises ceramic.
12. The component for a semiconductor manufacturing apparatus according to claim 11, characterized in that, The substrate comprises aluminum oxide.
13. A semiconductor manufacturing apparatus, comprising: a chamber; And a component for a semiconductor manufacturing apparatus according to any one of claims 1 to 12, characterized in that, The chamber has an inner wall that forms a space for generating plasma. The semiconductor manufacturing apparatus uses components that form at least a portion of the inner wall.
Citation Information
Patent Citations
Protective film, method for forming the same, apparatus for manufacturing semiconductor, and plasma treatment apparatus
JP2012057251A
Plasma processing device part, plasma processing device, and method for manufacturing part for plasma processing device
JP2016028379A
Plasma generating electrode and plasma processing device
CN102779715A