A silicon carbide epitaxial structure and preparation method thereof

By treating the substrate with wet cleaning and in-situ etching, and adjusting the doping concentration in the SiC buffer layer, the problem of unstable performance caused by differences in doping concentration in the epitaxial growth of silicon carbide is solved, and the quality of the epitaxial layer and devices are improved. performance.

CN115247278BActive Publication Date: 2024-10-11CEC COMPOUND SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210719055.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-23
Publication Date
2024-10-11
Estimated Expiration
2042-06-23

AI Technical Summary

Technical Problem

In the epitaxial growth of silicon carbide, the difference in doping concentration between the substrate and the buffer layer and the buffer layer and the epitaxial layer leads to unstable resistivity and capacitance performance, and defects, which affect device performance.

Method used

The substrate is processed by wet cleaning and in-situ etching, and the growth source and doping source are used to adjust the doping concentration of the SiC buffer layer so that it changes in a step-like, slope-like or cyclic manner between the substrate and the epitaxial layer. Slowly transition the doping concentration, thereby improving the interface quality.

Benefits of technology

It effectively reduces defects in the silicon carbide epitaxial layer, improves the stability of resistivity and capacitance performance, and improves the overall performance of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115247278B_ABST
    Figure CN115247278B_ABST
Patent Text Reader

Abstract

The present invention provides a silicon carbide epitaxial structure and a preparation method thereof, and specifically relates to the technical field of silicon carbide epitaxial growth. The preparation method of the present invention comprises the following steps: selecting a silicon carbide substrate and wet-cleaning it; placing the wet-cleaned silicon carbide substrate in a reaction chamber, and evacuating the reaction chamber to a vacuum; introducing hydrogen and hydrogen chloride into the reaction chamber to in-situ etch the silicon carbide substrate; introducing a growth source and a doping source into the reaction chamber to grow a silicon carbide buffer layer, wherein the doping concentration of the silicon carbide buffer layer varies between the doping concentration of the silicon carbide substrate and the doping concentration of the silicon carbide epitaxial layer; and growing the silicon carbide epitaxial layer on the silicon carbide buffer layer. The preparation method of the present invention can improve the quality of the silicon carbide epitaxial layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicon carbide epitaxial growth, and in particular to a silicon carbide epitaxial structure and a preparation method thereof. Background Art

[0002] As a third-generation semiconductor material, silicon carbide (SiC) is widely used in high-temperature, high-frequency, high-power and strong radiation power electronic devices due to its excellent properties such as large bandgap, excellent stability, high thermal conductivity, high critical breakdown field strength, and high saturated electron drift velocity. However, the yield of silicon carbide devices is limited by the development of silicon carbide epitaxial technology.

[0003] At present, silicon carbide epitaxial growth adopts CVD (chemical vapor deposition) method for homoepitaxial growth. Since the substrate is doped with ultra-high concentration and the epitaxial layer is low-doped, a buffer (Bffer) layer with a doping concentration between the substrate and the epitaxial layer is usually grown between the substrate and the epitaxial layer to improve the quality of the epitaxial layer. However, in the above process, the interface between the substrate and the buffer is very steep because the doping is reduced by two orders of magnitude from ultra-high doping. The interface between the buffer layer and the epitaxial layer also has a doping jump of more than 2 orders of magnitude, or even 3 orders of magnitude, and the interface is even steeper. The steep doping concentration at the interface and the uncontrollable variables lead to differences in the resistivity, capacitance and other properties of the epitaxial growth, and even damage to the device. Summary of the invention

[0004] In view of the above shortcomings of the prior art, the present invention provides a silicon carbide epitaxial structure and a preparation method thereof, so as to improve the problem of differences in resistivity, capacitance and other properties caused by a sudden change in doping concentration at the interface of the silicon carbide epitaxial structure.

[0005] To achieve the above-mentioned purpose and other related purposes, the present invention provides a method for preparing a silicon carbide epitaxial structure, comprising the following steps: selecting a silicon carbide (SiC) substrate and wet-cleaning it; placing the wet-cleaned SiC substrate in a reaction chamber, and evacuating the reaction chamber to a vacuum; introducing hydrogen (H2) and hydrogen chloride (HCl) into the reaction chamber to in-situ etch the SiC substrate; introducing a growth source and a doping source into the reaction chamber to grow a SiC buffer layer, wherein the doping concentration of the SiC buffer layer varies between the doping concentration of the SiC substrate and the doping concentration of the SiC epitaxial layer; and growing the SiC epitaxial layer on the SiC buffer layer.

[0006] In one example of the present invention, the wet cleaning includes: placing the SiC substrate in a mixed solution of concentrated sulfuric acid (H2SO4) and hydrogen peroxide (H2O2), soaking it at 100-150°C for 80-100 minutes, and performing a primary oxidation on the SiC substrate; repeatedly cleaning the SiC substrate after the primary oxidation in ultrapure water at 40-60°C to remove the residual concentrated H2SO4 and H2O2 mixed solution; soaking the cleaned SiC substrate in a hydrofluoric acid (HF) solution with a concentration of 5-15% for 50-70 minutes to wash away the oxide layer on the surface of the substrate; The SiC substrate is repeatedly cleaned in ultrapure water at 40 to 60° C. to remove residual HF; the cleaned SiC substrate is immersed in a mixed solution of ammonia (NH3·H2O), H2O2 and water for 50 to 70 minutes to perform secondary oxidation on the SiC substrate; the secondary oxidized SiC substrate is repeatedly cleaned in ultrapure water at 40 to 60° C. to remove residual ammonia and hydrogen peroxide; the cleaned SiC substrate is immersed in a hydrochloric acid (HCl) solution with a concentration of 5 to 15% for 50 to 70 minutes to clean the surface oxide layer; and the SiC substrate is ultrasonically cleaned in ultrapure water to remove residual HCl on the surface of the substrate.

[0007] In an example of the present invention, in the mixture and solution of H2SO4 and H2O2, the concentration of H2SO4 is 80-90%, and the concentration of H2O2 is 10-20%.

[0008] In an example of the present invention, the SiC substrate is a silicon-surface SiC substrate with an angle of 4° toward the <11-20> direction.

[0009] In an example of the present invention, the in-situ etching includes: introducing H2 into the reaction chamber, maintaining the H2 flow rate at 80-100 L / min, the reaction chamber pressure at 100-200 mbar, and raising the temperature of the reaction chamber from room temperature to 1630-1650°C at a heating rate of 45-60°C / min; then introducing hydrogen chloride (HCl) gas into the reaction chamber, etching for 500-700 seconds while maintaining the pressure and temperature in the chamber unchanged, and the flow rate of the HCl gas gradually increases from the initial 20-50 sccm to 500-600 sccm during the etching time.

[0010] In one example of the present invention, growing a silicon carbide buffer layer includes: adjusting the temperature of the reaction chamber to 1630-1650°C and the pressure to 100-200 mbar, introducing a carbon source, a silicon source and an N-type doping source into the reaction chamber to grow a SiC buffer layer, wherein the flow rate of the silicon source is 500-1000 sccm, the carbon-silicon ratio of the carbon source to the silicon source is 0.5-1.2, and the flow rate of the N-type doping source changes continuously with the doping concentration of the silicon carbide buffer layer during the growth process.

[0011] In an example of the present invention, the doping concentration of the SiC buffer layer decreases in a step-by-step manner between the doping concentration of the SiC substrate and the doping concentration of the SiC epitaxial layer, and the decrease pattern follows the following model: first stage: y(x2-x1)=-4E18*x; second stage: y(x3-x2)=1E18; third stage: y(x4-x3)=-1E18*x; wherein y represents the doping concentration of the silicon carbide buffer layer, x represents the growth position of the buffer layer, x1 represents the interface position at the beginning of the first stage, x2 represents the interface position at the end of the first stage, x3 represents the interface position at the end of the second stage, and x4 represents the interface position at the end of the third stage.

[0012] In an example of the present invention, the doping concentration of the SiC buffer layer slowly decreases between the doping concentration of the SiC substrate and the doping concentration of the SiC epitaxial layer; the decreasing pattern follows the following pattern: First stage: y(x2-x1)=-x 2 +5E18; second stage: y(x3-x2)=1E18; third stage: y(x4-x3)=-x 2 +1E18; wherein y represents the doping concentration of the silicon carbide buffer layer, x represents the growth position of the silicon carbide buffer layer, x1 represents the interface position at the beginning of the first stage, x2 represents the interface position at the end of the first stage, x3 represents the interface position at the end of the second stage, and x4 represents the interface position at the end of the third stage.

[0013] In one example of the present invention, the doping concentration of the SiC buffer layer varies in a straight-down manner between the doping concentration of the SiC substrate and the doping concentration of the SiC epitaxial layer, and the variation pattern follows the following model: y(x2-x1)=-5E18*x; wherein y represents the doping concentration of the silicon carbide buffer layer, x represents the growth position of the silicon carbide buffer layer, x1 represents the interface position where the buffer layer starts, and x2 represents the interface position where the buffer layer ends.

[0014] In an example of the present invention, the doping concentration of the SiC buffer layer changes cyclically between the doping concentration of the SiC substrate and the doping concentration of the SiC epitaxial layer, and the change pattern follows the following model: y(x n -x n-1 )=1E16 and y(x n+1 -x n )=5E18 alternately; wherein y represents the doping concentration of the silicon carbide buffer layer, x represents the growth position of the silicon carbide buffer layer, and x n represents the interface position where the nth buffer layer starts, x n+1 Indicates the interface position where the nth buffer layer ends, where n is an integer greater than 1.

[0015] In an example of the present invention, the doping concentration of the SiC buffer layer changes cyclically between the doping concentration of the SiC substrate and the doping concentration of the SiC epitaxial layer, and the change pattern follows the following model: y(x n -x n-1 )=1E16 and y(x n+1 -x n )=1E18; alternately, wherein y represents the doping concentration of the silicon carbide buffer layer, x represents the growth position of the silicon carbide buffer layer, and x n represents the interface position where the nth buffer layer starts, x n+1 Indicates the interface position where the nth buffer layer ends, where n is an integer greater than 1.

[0016] In an example of the present invention, the doping concentration of the SiC buffer layer changes cyclically between the doping concentration of the SiC substrate and the doping concentration of the SiC epitaxial layer, and the change pattern follows the following model: y(x n -x n-1 )=1E18 and y(x n+1 -x n )=5E18 alternately; wherein y represents the doping concentration of the silicon carbide buffer layer, x represents the growth position of the silicon carbide buffer layer, and x n represents the interface position where the nth buffer layer starts, x n+1 Indicates the interface position where the nth buffer layer ends, where n is an integer greater than 1.

[0017] In an example of the present invention, growing the SiC epitaxial layer includes: adjusting the temperature of the reaction chamber to 1600-1630° C., adjusting the growth source and the doping source to required values, and growing the epitaxial layer according to a process procedure.

[0018] Another aspect of the present invention provides a SiC epitaxial structure, which is prepared by the preparation method of the present invention.

[0019] The present invention provides a method for preparing a SiC epitaxial structure. The method controls the doping concentration of the buffer layer by controlling the flow rate of the doping gas during the growth of the buffer layer, thereby realizing that the doping concentration of the buffer layer changes slowly between the doping concentration of the SiC substrate and the doping concentration of the SiC epitaxial layer, so that the doping concentration at the interface between the SiC substrate and the SiC buffer layer and the interface between the SiC buffer layer and the SiC epitaxial layer slowly transitions, thereby improving the quality of the epitaxial layer. In the process of cleaning the substrate, a wet cleaning process is adopted, and the surface of the substrate after mechanical treatment can be improved by multiple oxidations and reductions, and excess impurities can be removed; in addition, when etching the substrate, the combination of H2 and HCl can be used to enhance the etching effect, reduce the time required for etching, and effectively reduce the defects of the silicon carbide epitaxial layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 This is a flow chart of the method for preparing the silicon carbide epitaxial structure of the present invention;

[0022] Figure 2 for Figure 1 Flow chart of wet cleaning;

[0023] Figure 3 A schematic diagram of the variation of doping concentration of a buffer layer using a first doping model in an embodiment of a method for preparing a silicon carbide epitaxial structure of the present invention;

[0024] Figure 4 A schematic diagram of the variation of doping concentration of a buffer layer using a second doping model in an embodiment of a method for preparing a silicon carbide epitaxial structure of the present invention;

[0025] Figure 5 A schematic diagram of the variation of doping concentration of a buffer layer using a third doping model in an embodiment of a method for preparing a silicon carbide epitaxial structure of the present invention;

[0026] Figure 6 A schematic diagram of the variation of doping concentration of a buffer layer using a fourth doping model in an embodiment of a method for preparing a silicon carbide epitaxial structure of the present invention;

[0027] Figure 7 A schematic diagram of the variation of doping concentration of a buffer layer using the fifth doping model in an embodiment of the method for preparing a silicon carbide epitaxial structure of the present invention;

[0028] Figure 8 A schematic diagram of the variation of doping concentration of a buffer layer using a sixth doping model in an embodiment of a method for preparing a silicon carbide epitaxial structure of the present invention;

[0029] Fig. 9 It is a structural schematic diagram of the silicon carbide epitaxial structure of the present invention;

[0030] Fig.10 is a topographical diagram of an epitaxial layer of a silicon carbide epitaxial structure of the present invention;

[0031] Fig.11 This is a morphology diagram of the epitaxial layer of the silicon carbide epitaxial structure of the present invention without the introduction of HCl during the etching process.

[0032] Component number description

[0033] 1. SiC substrate; 2. SiC buffer layer; 3. SiC epitaxial layer. DETAILED DESCRIPTION

[0034] The following is an explanation of the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the features in the following embodiments and the embodiments can be combined with each other without conflict. It should also be understood that the terms used in the embodiments of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods for which specific conditions are not specified in the following examples are usually carried out under conventional conditions or according to the conditions recommended by the manufacturers.

[0035] It should be noted that the terms such as "upper", "lower", "left", "right", "middle" and "one" etc. used in this specification are only for the convenience of description and are not intended to limit the scope of implementation of the present invention. Changes or adjustments to their relative relationships, without substantially changing the technical content, should also be regarded as the scope of implementation of the present invention.

[0036] See also Figure 1 and Fig. 9 The present invention provides a method for preparing a SiC epitaxial structure, comprising the following steps:

[0037] S1, selecting a SiC substrate 1 and performing wet cleaning on it;

[0038] S2, placing the wet-cleaned SiC substrate 1 in a reaction chamber, and evacuating the reaction chamber to a vacuum;

[0039] S3, introducing H2 and HCl into the reaction chamber to perform in-situ etching on the SiC substrate 1;

[0040] S4, introducing a growth source and a doping source into the reaction chamber to grow a SiC buffer layer 2, wherein the doping concentration of the SiC buffer layer 2 varies between the doping concentration of the SiC substrate 1 and the doping concentration of the SiC epitaxial layer 3;

[0041] S5 . Growing a SiC epitaxial layer 3 on the SiC buffer layer 2 .

[0042] See also Figure 1 , Figure 2 and Fig. 9In step S1, the SiC substrate 1 is a silicon carbide substrate with a silicon surface that is 4° in the <11-20> direction. For example, a 6-inch silicon carbide substrate with a silicon surface that is 4° in the <11-20> direction or a 4-inch silicon carbide substrate with a silicon surface that is 4° in the <11-20> direction can be selected. The specific size can be selected according to needs and is not limited here. The SiC substrate 1 is wet cleaned, that is, the substrate surface is improved by multiple oxidation and reduction methods to remove excess impurities. The wet cleaning steps specifically include:

[0043] S11, placing the SiC substrate 1 in a mixed solution of concentrated H2SO4 and H2O2, soaking it at 100-150°C for 80-100 minutes, and performing primary oxidation on the SiC substrate 1;

[0044] S12, repeatedly washing the SiC substrate 1 after the primary oxidation in pure water at 40-60° C. to remove the residual H2SO4 and H2O2 mixed solution;

[0045] S13, soaking the cleaned SiC substrate 1 in a HF solution with a concentration of 5 to 15% for 50 to 70 minutes to wash away the oxide layer on the surface of the substrate;

[0046] S14, repeatedly washing the SiC substrate 1 in pure water at 40-60° C. to remove residual HF solution;

[0047] S15, placing the cleaned SiC substrate 1 in a mixed solution of NH3·H2O, H2O2 and H2O to perform secondary oxidation on the SiC substrate 1;

[0048] S16. The SiC substrate 1 after secondary oxidation is repeatedly cleaned in ultrapure water at 40 to 60° C. to remove residual NH 3 ·H 2 O and H 2 O 2 .

[0049] S17, soaking the cleaned SiC substrate 1 in a 5-15% HCl solution for 50-70 minutes to clean the oxide layer on the surface;

[0050] S18. Perform ultrasonic cleaning in pure water to remove residual HCl solution on the surface of the substrate.

[0051] Wherein, in step S11, the concentration of concentrated H2SO4 in the mixed solution of concentrated H2SO4 and H2O2 is 80-90%, and the concentration of H2O2 is 10-20%, for example, the concentration of H2SO4 is 80%, and the concentration of H2O2 is 20%; or the concentration of concentrated H2SO4 is 85%, and the concentration of H2O2 is 15%; or the concentration of concentrated H2SO4 is 90%, and the concentration of H2O2 is 10%. The immersion time of SiC substrate 1 in the mixed solution of concentrated H2SO4 and H2O2 is 80-100 minutes, so that the surface of the substrate is oxidized. The immersion time can be selected as any value within the above numerical range, such as 80 minutes, 90 minutes or 100 minutes.

[0052] Step S12 is to take out the SiC substrate 1 processed in step S11 from the mixed solution of concentrated H2SO4 and H2O2, and put it into ultrapure water at 40-60°C for repeated cleaning to remove the concentrated H2SO4 and H2O2 remaining on the surface of the substrate. The temperature of the ultrapure water can be 40°C, 50°C or 60°C, etc. The repeated cleaning can be selected to be repeated 5-6 times in an ultrasonic cleaning machine with ultrapure water until the residual concentrated H2SO4 and H2O2 are completely removed.

[0053] Step S13 is to take the SiC substrate 1 out of the ultrapure water in step S12, put it into a HF solution with a concentration of 5-15% and clean it at room temperature to remove the oxide layer on the surface of the substrate. The concentration of HF can be selected as 5%, 8%, 11% or 15%, etc. The cleaning time of the SiC substrate 1 in HF is 50-70 minutes, for example, the cleaning time can be any value within the above numerical range such as 50 minutes, 60 minutes or 70 minutes, and can be selected according to the thickness of the oxide layer on the surface of the substrate.

[0054] Step S14 is to take out the SiC substrate 1 processed in step S13 and repeatedly clean it in ultrapure water at 40-60° C. until the HF solution remaining on the surface of the substrate is cleaned. The specific cleaning conditions can refer to step S12.

[0055] Step S15 is to immerse the SiC substrate 1 processed in step S14 in a mixed solution of NH3H2O, H2O2 and H2O for 50 to 70 minutes to perform secondary oxidation on the substrate surface; in the mixed solution, the concentration of NH3H2O ​​is 5 to 10%, and the concentration of H2O2 is 5 to 10%. For example, the concentration of NH3H2O ​​can be selected to be 5%, 8% or 10%, and the concentration of H2O2 can be 5%, 7% or 10%, etc.

[0056] Step S16 is to take out the SiC substrate 1 processed in step S15 and repeatedly wash it in ultrapure water at 40-60° C. until the NH 3 H 2 O and H 2 O 2 remaining on the surface of the substrate are cleaned. The specific cleaning conditions can refer to step S14.

[0057] Step S17 is to place the SiC substrate 1 cleaned in step S16 in a 5-15% HCl solution for cleaning to remove the oxide layer on the surface of the substrate. The concentration of the HCl solution is, for example, 5%, 10% or 15%. The cleaning time of the SiC substrate 1 in HCl is 50-70 minutes, which can be selected according to the thickness of the oxide layer on the surface of the substrate.

[0058] Step S18 is to place the SiC substrate 1 processed in step S16 in ultrapure water for ultrasonic cleaning.

[0059] See also Figure 1 and Fig. 9 Step S2 is to mount the SiC substrate 1 on a graphite base with the silicon surface of the SiC substrate 1 tilted 4° in the <11-20> direction facing upward, and then place the graphite base with the SiC substrate 1 mounted in a reaction chamber, replace the air in the reaction chamber with argon gas, and evacuate the reaction chamber to a vacuum.

[0060] See also Figure 1 and Fig. 9 In step S3, the SiC substrate 1 is etched in situ. After the reaction chamber is evacuated to vacuum, H2 is introduced into the reaction chamber, and the flow rate of H2 is maintained at 80-100 L / min, and the pressure is maintained at 100-200 mbar. At the same time, the temperature of the reaction chamber is increased to 1630-1650°C at a heating rate of 45-60°C / min. For example, the flow rate of H2 can be selected as 80 L / min, 90 L / min or 100 L / min, the pressure is 100 mbar, 150 mbar, 180 mbar, 200 mbar, etc., the heating rate can be selected as 45°C / min, 50°C / min, 60°C / min, etc., and the temperature of the reaction chamber can be selected as 1630°C, 1640°C or 1650°C; then, the temperature and pressure of the reaction chamber are kept unchanged, and HCl gas is introduced to etch the SiC substrate 1 with H2 and HCl for 500-700 seconds. The initial flow rate of HCl is 20-50 sccm, and gradually increases to 500-600 sccm during the etching time. For example, the initial flow rate of HCl can be selected as 20 sccm, 30 sccm, 40 sccm, 50 sccm, etc., and the etching time is 5 min, 8 min, 10 min, etc. During the etching time, the flow rate of HCl gradually increases to 500 sccm, 550 sccm, 600 sccm, etc. Introducing a small amount of HCl during the H2 etching process can enhance the etching effect, reduce the time required for etching, and effectively reduce defects in the silicon carbide epitaxy process, especially the inhibition or conversion of BPD (basal plane dislocation).

[0061] See also Figure 1 and Fig. 9, step S4 is to keep the temperature and pressure of the reaction chamber unchanged after etching, introduce carbon source, silicon source and doping source into the reaction chamber to grow SiC buffer layer 2 on SiC substrate 1, wherein the flow rate of silicon source is 500-1000sccm, the flow rate of carbon source is corrected according to carbon-silicon ratio, carbon-silicon ratio is 0.5-1.2, for example, the flow rate of silicon source can be selected as 500sccm, 700sccm, 900sccm, 1000sccm, carbon-silicon ratio can be 0.5, 0.8, 1, 1.2, etc. The flow rate of doping source is constantly changed during the growth of buffer layer so that the doping concentration of buffer layer changes between the doping concentration of SiC substrate 1 and the doping concentration of SiC epitaxial layer 3, and the flow rate of doping source is 10-110sccm. In the present invention, silicon source can be selected from silane, dichlorosilane, trichlorosilane or tetrachlorosilane, carbon source can be selected from methane, ethylene, acetylene or propane, etc.; doping source can be selected from N-type doping source N2. The doping concentration of the SiC substrate 1 is on the order of (5-10)E18, and the doping concentration of the SiC epitaxial layer is on the order of 1E16. The doping modes of the buffer layer are as follows:

[0062] See also Figure 1 , Figure 3 and Fig. 9 In the first doping method, the concentration of the buffer layer decreases in a step-by-step manner. In this mode, the buffer layer is divided into three growth stages. The doping method of the first stage is: y(x2-x1)=-4E18*x, and the value range of x is from x1 to x2; the doping method of the second stage is: y(x3-x2)=1E18, and the value range of x is from x2 to x3; the doping method of the third stage is: y(x4-x3)=-1E18*x, and the value range of x is from x3 to x4; wherein y represents the doping concentration of the buffer layer, x represents the growth position of the buffer layer, x1 represents the interface position at the beginning of the first stage, x2 represents the interface position at the end of the first stage (the beginning of the second stage), x3 represents the interface position at the end of the second stage (the end of the third stage), and x4 represents the interface position at the end of the third stage; (x2-x1) represents the thickness of the buffer layer grown in the first stage, (x3-x2) represents the thickness of the buffer layer grown in the second stage, and (x4-x3) represents the thickness of the buffer layer grown in the third stage. During specific growth, the above growth model can be input into the control program, and the flow controller can be controlled by the control program to adjust the flow of the doping source to achieve the adjustment of the doping concentration of the buffer layer. In this embodiment, the buffer layer adopts the mode of direct drop doping growth-constant doping growth-direct drop doping growth, which can reduce the difference in doping concentration at the interface between the substrate and the buffer layer, and the difference in doping concentration at the interface between the buffer layer and the epitaxial layer, thereby improving the growth quality of the epitaxial layer.

[0063] See also Figure 1 , Figure 4 and Fig. 9In the second doping method, the concentration of the buffer layer decreases in a slope. In this mode, the buffer layer is divided into three growth stages. The doping method of the first stage is: y(x2-x1)=-x 2 +5E18, the value range of x is from x1 to x2; the doping method of the second stage is: y(x3-x2)=1E18, the value range of x is from x2 to x3; the doping method of the third stage is: y(x4-x3)=-x 2 +1E18*x, the value range of x is from x3 to x4; wherein, y represents the doping concentration of the buffer layer, x represents the growth position of the buffer layer, x1 represents the interface position at the beginning of the first stage, x2 represents the interface position at the end of the first stage (the beginning of the second stage), x3 represents the interface position at the end of the second stage (the end of the third stage), and x4 represents the interface position at the end of the third stage; (x2-x1) represents the thickness of the buffer layer grown in the first stage, (x3-x2) represents the thickness of the buffer layer grown in the second stage, and (x4-x3) represents the thickness of the buffer layer grown in the third stage. During specific growth, the above growth model can be input into the control program, and the flow controller can be controlled by the control program to adjust the flow of the doping source to achieve the adjustment of the doping concentration of the buffer layer. In this embodiment, the buffer layer adopts the mode of exponentially declining doping growth-constant doping growth-exponentially declining doping growth, which can reduce the difference in doping concentration at the interface between the substrate and the buffer layer, and the difference in doping concentration at the interface between the buffer layer and the epitaxial layer, thereby improving the growth quality of the epitaxial layer.

[0064] See also Figure 1 , Figure 5 and Fig. 9 , the concentration of the buffer layer in the third doping method decreases linearly. In this mode, the doping method of the buffer layer is: y(x2-x1)=-5E18x, and the value range of x is from x1 to x2; wherein y represents the doping concentration of the buffer layer, x represents the growth position of the buffer layer, x1 represents the interface position where the growth of the buffer layer begins, x2 represents the interface position where the growth of the buffer layer ends, and (x2-x1) represents the thickness of the buffer layer. During specific growth, the above growth model can be input into the control program, and the flow controller can be controlled by the control program to adjust the flow of the doping source to achieve the adjustment of the doping concentration of the buffer layer. In this embodiment, the buffer layer adopts a linear decline doping growth mode, which can reduce the difference in doping concentration at the interface between the substrate and the buffer layer, and the difference in doping concentration at the interface between the buffer layer and the epitaxial layer, thereby improving the growth quality of the epitaxial layer.

[0065] See also Figure 1 and Figures 6 to 9, the doping concentration of the SiC buffer layer 2 can also be grown in a cyclic transformation mode, that is, the SiC buffer layer 2 is alternately and repeatedly grown n (n is a positive integer) layers according to several different doping concentrations until the buffer layer growth is completed, and there are multiple concentration changes between the first buffer layer and the nth buffer layer. The buffer layers with different doping concentrations slow down the doping concentration at the interface between the substrate and the buffer layer, and the interface between the buffer layer and the epitaxial layer, forming a slow transition layer, so that the resistance and capacitance in the epitaxial structure can achieve a controllable effect. The doping concentration fault can also cause a series of quantum wells to appear in the buffer layer, thereby extending the time that the carriers stay in the buffer layer and thus extending the carrier lifetime. During specific growth, the growth model of cyclic growth can be input into the control program, and the control program controls the flow controller to adjust the flow of the doping source to achieve the adjustment of the doping concentration of the buffer layer.

[0066] The cyclic growth model includes the following doping methods:

[0067] The fourth doping method (cycle mode 1): according to y(x n -x n-1 )=1E16 and y(x n+1 -x n )=5E18 (n is an integer greater than 1) and the buffer layers are grown in an alternating manner, that is, the first buffer layer is doped in a manner of y(x2-x1)=1E16; the second buffer layer is doped in a manner of y(x3-x2)=5E18; the third buffer layer is doped in a manner of y(x4-x3)=1E16; the fourth buffer layer is doped in a manner of y(x5-x4)=5E18; ...; (x n -x n-1 )=1E16,(x n+1 -x n )=5E18; repeat this cycle until the growth of the buffer layer is completed. Wherein, y represents the doping concentration of the silicon carbide buffer layer, x represents the growth position of the silicon carbide buffer layer, x1 represents the interface position where the first buffer layer starts, and x2 represents the interface position where the first buffer layer ends...x n represents the interface position where the nth buffer layer starts, x n+1 Indicates the interface position where the nth buffer layer ends, (x n -x n-1 ) represents the thickness of the (n-1)th buffer layer.

[0068] The fifth doping method (cycle mode 2): according to y(x n -x n-1 )=1E16 and y(x n+1 -x n)=1E18 (n is an integer greater than 1) and the buffer layers are grown in an alternating manner, that is, the first buffer layer is doped in a manner of y(x2-x1)=1E16; the second buffer layer is doped in a manner of y(x3-x2)=1E18; the third buffer layer is doped in a manner of y(x4-x3)=1E16; the fourth buffer layer is doped in a manner of y(x5-x4)=1E18; ...; (x n -x n-1 )=1E16,(x n+1 -x n )=1E18; repeat this cycle until the growth of the buffer layer is completed. Wherein, y represents the doping concentration of the silicon carbide buffer layer, x represents the growth position of the silicon carbide buffer layer, x1 represents the interface position where the first buffer layer starts, and x2 represents the interface position where the first buffer layer ends...x n represents the interface position where the nth buffer layer starts, x n+1 Indicates the interface position where the nth buffer layer ends, (x n -x n-1 ) represents the thickness of the (n-1)th buffer layer.

[0069] The sixth doping method (cycle mode 3): according to y(x n -x n-1 )=1E18 and y(x n+1 -x n )=5E18 (n is an integer greater than 1) and the buffer layers are grown in an alternating manner, that is, the first buffer layer is doped in a manner of y(x2-x1)=1E18; the second buffer layer is doped in a manner of y(x3-x2)=5E18; the third buffer layer is doped in a manner of y(x4-x3)=1E18; the fourth buffer layer is doped in a manner of y(x5-x4)=5E18; ...; (x n -x n-1 )=1E18,(x n+1 -x n )=5E18; repeat this cycle until the growth of the buffer layer is completed. Wherein, y represents the doping concentration of the silicon carbide buffer layer, x represents the growth position of the silicon carbide buffer layer, x1 represents the interface position where the first buffer layer starts, and x2 represents the interface position where the first buffer layer ends...x n represents the interface position where the nth buffer layer starts, x n+1 Indicates the interface position where the nth buffer layer ends, (x n -x n-1 ) represents the thickness of the (n-1)th buffer layer.

[0070] See also Figure 1 and Fig.10After the growth of step S4 is completed, step S5 is performed to grow a SiC epitaxial layer 3 on the SiC buffer layer 2, specifically including: adjusting the temperature of the reaction chamber to the growth temperature of the SiC epitaxial layer 3 of 1600-1630°C, for example, the temperature is adjusted to 1600°C, 1620°C or 1630°C; at the same time, the flow rates of the silicon source, the carbon source and the doping source are adjusted to the set values ​​required for the growth of the SiC epitaxial layer 3 in a linear manner, and the epitaxial layer is grown until the epitaxial layer reaches the required thickness.

[0071] After the growth of the SiC epitaxial layer 3 is completed, the introduction of the growth source gas and the doping gas is cut off, the temperature of the reaction chamber is lowered to the standby temperature, the introduction of H2 into the reaction chamber is suspended, Ar is introduced into the reaction chamber to atmospheric pressure, the reaction chamber is opened, and the epitaxial structure is taken out of the reaction chamber.

[0072] See also Fig. 9 The present invention provides a silicon carbide epitaxial structure, which comprises a SiC substrate 1, a SiC buffer layer 2 and a SiC epitaxial layer 3 arranged in sequence from bottom to top. The epitaxial structure of the present invention is formed by the preparation method of the present invention, the SiC substrate 1 is selected from a silicon-surface silicon carbide substrate with a 4° deflection in the <11-20> direction, and the thickness and doping concentration of the SiC buffer layer 2 and the SiC epitaxial layer 3 can be prepared according to the preparation method of the present invention according to specific requirements.

[0073] See also Fig.10 and Fig.11 , Fig.10 The morphology of the SiC epitaxial structure prepared by the preparation method of the present invention is shown in FIG. Fig.11 The morphology of the SiC epitaxial structure prepared without HCl during the etching process is shown in Figure 2. Fig.10 and Fig.11 , it can be seen that Fig.10 The microstructure is clearer and has fewer defects, that is, introducing a small amount of HCl during the H2 etching process can enhance the etching effect and effectively reduce the defects in SiC epitaxy.

[0074] The present invention provides a method for preparing a silicon carbide epitaxial structure. The method controls the doping concentration of the buffer layer by controlling the flow rate of the doping gas during the growth of the buffer layer, thereby realizing that the doping concentration of the buffer layer changes slowly between the doping concentration of the silicon carbide substrate and the doping concentration of the silicon carbide epitaxial layer, so that the doping concentration at the interface between the silicon carbide substrate and the silicon carbide buffer layer and the interface between the silicon carbide buffer layer and the silicon carbide epitaxial layer slowly transitions, thereby improving the quality of the epitaxial layer. Therefore, the present invention effectively overcomes some practical problems in the prior art and thus has high utilization value and use significance.

[0075] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for preparing a silicon carbide epitaxial structure, It is characterized in that The following steps are involved: Selecting a silicon carbide substrate and performing wet cleaning on it; Placing the wet-cleaned silicon carbide substrate in a reaction chamber, and evacuating the reaction chamber to a vacuum; Introducing hydrogen and hydrogen chloride into the reaction chamber to perform in-situ etching on the silicon carbide substrate, wherein the in-situ etching comprises: introducing hydrogen into the reaction chamber, maintaining the flow rate of hydrogen at 80-100 L / min, the pressure at 100-200 mbar, and raising the temperature of the reaction chamber to 1630-1650° C. at a heating rate of 45-60° C. / min; then maintaining the temperature and pressure of the reaction chamber unchanged, introducing hydrogen chloride gas, and etching the substrate for 500-700 seconds; wherein the initial flow rate of hydrogen chloride is 20-50 sccm, and gradually increases by 500-600 sccm during the etching time; A growth source and a doping source are introduced into the reaction chamber to grow a silicon carbide buffer layer, wherein the doping source is an N-type doping source N 2 , the doping concentration of the silicon carbide buffer layer varies between the doping concentration of the silicon carbide substrate and the doping concentration of the silicon carbide epitaxial layer; growing the silicon carbide epitaxial layer on the silicon carbide buffer layer; The doping concentration of the silicon carbide buffer layer decreases stepwise, slowly, linearly, or cyclically between the doping concentration of the silicon carbide substrate and the doping concentration of the silicon carbide epitaxial layer; the change follows any one of the following models: Step-down model: Stage 1: y(x 2 -x 1 )=-4E18*x; Second stage: y(x 3 -x 2 )=1E18; The third stage: y(x 4 -x 3 )=-1E18*x; where y represents the doping concentration of the silicon carbide buffer layer, x represents the growth position of the buffer layer, and x 1 represents the interface position where the first stage begins, x 2 Indicates the interface position at the end of the first stage, x 3 Indicates the interface position where the second stage ends, x 4 The interface position indicating the end of the third stage; Slow descent model: Phase 1: y(x 2 -x 1 )=-x 2 +5E18; Phase 2: y(x 3 -x 2 )=1E18; The third stage: y(x 4 -x 3 )=-x 2 +1E18; where y represents the doping concentration of the silicon carbide buffer layer, x represents the growth position of the silicon carbide buffer layer, and x 1 represents the interface position where the first stage begins, x 2 Indicates the interface position at the end of the first stage, x 3 Indicates the interface position where the second stage ends, x 4 The interface position indicating the end of the third stage; Straight-line decline model: y(x 2 -x 1 )=-5E18*x; wherein y represents the doping concentration of the silicon carbide buffer layer, x represents the growth position of the silicon carbide buffer layer, and x 1 represents the interface position where the buffer layer starts, x 2 The interface position indicating the end of the buffer layer; Cyclic Model 1: y(x n -x n-1 )=1E16 and y(x n+1 -x n )=5E18 alternately; wherein y represents the doping concentration of the silicon carbide buffer layer, x represents the growth position of the silicon carbide buffer layer, and x n represents the interface position where the nth buffer layer starts, x n+1 represents the interface position where the nth buffer layer ends, where n is an integer greater than 1; Cyclic Model 2: y(x n -x n-1 )=1E16 and y(x n+1 -x n )=1E18; alternately, wherein y represents the doping concentration of the silicon carbide buffer layer, x represents the growth position of the silicon carbide buffer layer, and x n represents the interface position where the nth buffer layer starts, x n+1 represents the interface position where the nth buffer layer ends, where n is an integer greater than 1; Cyclic Model 3: y(x n -x n-1 )=1E18 and y(x n+1 -x n )=5E18 alternately; wherein y represents the doping concentration of the silicon carbide buffer layer, x represents the growth position of the silicon carbide buffer layer, and x n represents the interface position where the nth buffer layer starts, x n+1 Indicates the interface position where the nth buffer layer ends, where n is an integer greater than 1.

2. The preparation method according to claim 1, It is characterized in that The wet cleaning comprises: placing the silicon carbide substrate in a mixed solution of concentrated sulfuric acid and hydrogen peroxide, and soaking it at 100 to 150° C. for 80 to 100 minutes to perform primary oxidation on the silicon carbide substrate; The silicon carbide substrate after the primary oxidation is repeatedly cleaned in ultrapure water at 40 to 60° C. to remove the residual mixed solution of concentrated sulfuric acid and hydrogen peroxide; The cleaned silicon carbide substrate is immersed in a hydrofluoric acid solution with a concentration of 5 to 15% for 50 to 70 minutes to wash away the oxide layer on the surface of the substrate; The silicon carbide substrate soaked in hydrofluoric acid is repeatedly cleaned in ultrapure water at 40 to 60° C. to remove residual hydrofluoric acid solution; The cleaned silicon carbide substrate is immersed in a mixed solution of ammonia water, hydrogen peroxide and water for 50 to 70 minutes to perform secondary oxidation on the silicon carbide substrate; The silicon carbide substrate after secondary oxidation is repeatedly cleaned in ultrapure water at 40 to 60° C. to remove residual ammonia and hydrogen peroxide; The cleaned silicon carbide substrate is immersed in a hydrochloric acid solution with a concentration of 5 to 15% for 50 to 70 minutes to clean the oxide layer on the surface; Ultrasonic cleaning was performed in pure water to remove the residual hydrochloric acid solution on the surface of the substrate.

3. The preparation method according to claim 1, It is characterized in that Growing a silicon carbide buffer layer includes: adjusting the temperature of the reaction chamber to 1630-1650°C and the pressure to 100-200 mbar, introducing a carbon source, a silicon source and an N-type doping source into the reaction chamber to grow the silicon carbide buffer layer, wherein the flow rate of the silicon source is 500-1000 sccm, the carbon-silicon ratio of the carbon source to the silicon source is 0.5-1.2, and the flow rate of the N-type doping source changes continuously with the doping concentration of the silicon carbide buffer layer during the growth process.

4. The preparation method according to claim 1, It is characterized in that Growing the silicon carbide epitaxial layer includes: adjusting the temperature of the reaction chamber to 1600-1630° C., adjusting the growth source and the doping source to the values ​​required by the silicon carbide epitaxial layer, and growing the silicon carbide epitaxial layer according to a process procedure.

5. A silicon carbide epitaxial structure, It is characterized in that The preparation is carried out by the preparation method described in any one of claims 1 to 4.