Method for recovering silver from silver-containing waste liquid
By using ammonia water and sodium hydroxide solution in silver-containing waste liquid to form silver oxide precipitation, the complex and time-consuming problems in the existing technology are solved, efficient and simple silver recovery is achieved, the recovery rate and purity are improved, and it is suitable for large-scale production. Batch processing.
Patent Information
- Application Number
- CN202210991088.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-17
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-08-17
AI Technical Summary
The existing methods for recovering silver from silver-containing waste liquids are complicated, involve many chemicals, and have long cycles, making it difficult to achieve efficient and simple mass processing.
By adding ammonia water and sodium hydroxide solution to the silver-containing wastewater, controlling the stirring and dripping rate to form silver oxide precipitate, followed by press filtration and washing to ensure that the silver ion concentration reaches the sewage discharge standard and improve the recovery rate and purity.
It achieves efficient recovery of silver, simplifies the process flow, improves the recovery rate and production line revenue, and ensures that the concentration of silver ions in the waste liquid meets the pollution discharge standards. The purity of silver is high and suitable for large-scale processing.
Abstract
Description
Technical Field
[0001] The invention relates to the field of hydrometallurgical recovery, and in particular to a method for recovering silver from silver-containing waste liquid. Background Art
[0002] In the production process of silver nitrate, there are many heating processes involved, especially the evaporation and concentration process, which will produce a large amount of silver-containing distillate. The silver content of these distillates is 500-800 mg / L. Although some clean silver-containing distillate can be used to replace pure water as feed water, the amount of silver-containing distillate produced is much greater than the feed consumption. In the industrial production of silver nitrate, the cleaning of equipment will also produce a lot of silver-containing wash water, in which silver mainly exists in the form of silver ions. As a precious metal, silver is very important to recover silver from silver-containing solutions. The methods for recovering silver from silver-containing waste liquid mainly include precipitation method, electrolysis method, reduction substitution method, ion exchange method and adsorption method. Among them, the precipitation method recovers silver from silver-containing waste liquid, which is to add appropriate anions to the silver-containing solution to enrich the silver in the waste liquid in the form of precipitation. After filtering, washing and drying, a silver precipitate is obtained, and then the precipitate is mixed with a certain amount of sodium carbonate and roasted at about 1100°C to obtain elemental silver. The precipitation method includes silver sulfide precipitation method and silver chloride precipitation method. However, whether it is the silver sulfide precipitation method or the silver chloride precipitation method, both have disadvantages such as complex operation methods, large number of chemicals used in the process, and long cycle. Summary of the invention
[0003] In view of the problems existing in the prior art, the purpose of the present disclosure is to provide a method for recovering silver from silver-containing waste liquid.
[0004] In order to achieve the above-mentioned purpose, the present disclosure provides a method for recovering silver from silver-containing waste liquid, which comprises the following steps: step 1, preparing ammonia for silver-containing waste water: after adding silver-containing waste water to a precipitation kettle to a high liquid level, stirring is started, and then ammonia water is added dropwise, a brown precipitate first appears in the solution, and as the ammonia water is added dropwise, the precipitate dissolves, and the solution becomes a colorless and transparent solution again, and stirring is continued for 10 to 30 minutes; step 2, synthesizing silver oxide reaction: keeping stirring, adding sodium hydroxide solution to the precipitation kettle, and then standing, stirring is started again and the solution is heated to 60 to 80° C., and the pH value is controlled to be 11.5 to 12.5; step 3, filter pressing: filter the slurry in the precipitation kettle, and the filter press liquid is sent to a washing tank, and then the filter press liquid is circulated between the washing tank and the filter press until the filtrate is clear and then discharged to the sewage workshop through two-stage precision filters in sequence; step 4, washing: unloading the filter cake into the washing tank and repeatedly washing it with pure water until the conductivity of the supernatant of the washing liquid is less than 50us / cm.
[0005] In some embodiments, in step 1, the rate of adding aqueous ammonia is 1 L / h to 5 L / h.
[0006] In some embodiments, in step 1, the concentration of the added ammonia water is 5-10 mol / L.
[0007] In some embodiments, in step 2, the rate of adding the sodium hydroxide solution is 1 to 5 L / h.
[0008] In some embodiments, in step 2, the concentration of the added sodium hydroxide solution is 3-5 mol / L.
[0009] In some embodiments, in step 2, the mass ratio of Ag to NaOH is 1.15:1.
[0010] In some embodiments, in step 2, the stirring time is restarted for 10-20 minutes.
[0011] The beneficial effects of the present disclosure are as follows:
[0012] The method disclosed in the present invention improves the recovery rate of precious metals and thus increases the revenue of the production line, while at the same time allowing the concentration of silver ions in the waste liquid to reach relevant pollution discharge standards. In addition, the process flow of the present invention is short, the operation is simple and convenient, and silver-containing wastewater can be treated in large quantities. DETAILED DESCRIPTION
[0013] The method for recovering silver from silver-containing waste liquid according to the present disclosure is described in detail below.
[0014] The present application discloses a method for recovering silver from silver-containing waste liquid, which comprises the following steps: step 1, preparing ammonia for the silver-containing waste water: after adding the silver-containing waste water to the precipitation kettle to the highest liquid level, stirring is started, and then ammonia water is added dropwise, a brown precipitate first appears in the solution, and as the ammonia water is added dropwise, the precipitate dissolves, and the solution becomes a colorless and transparent solution again, and stirring is continued for 10 to 30 minutes; step 2, synthesizing silver oxide reaction: keeping stirring, adding sodium hydroxide solution to the precipitation kettle, and then standing, stirring is started again and the solution is heated to 60 to 80° C., and the pH value is controlled to be 11.5 to 12.5; step 3, filter pressing: filtering the slurry in the precipitation kettle, and the filter press liquid is sent to a washing tank, and then the filter press liquid is circulated between the washing tank and the filter press until the filtrate is clear and then discharged to the sewage workshop through two-stage precision filters in sequence; step 4, washing: unloading the filter cake to the washing tank and repeatedly washing with pure water until the conductivity of the supernatant of the washing liquid is less than 50us / cm.
[0015] The present application adds ammonia to the silver ions in the wastewater and then controls the stirring speed and the dripping rate of the sodium hydroxide solution, so that the size of the precipitate can be effectively increased to facilitate filtration, and the silver precipitation in the waste liquid can be more thorough, thereby improving the recovery rate of silver, and ensuring that the silver ion content in the synthetic waste liquid is less than 0.5ppm. The silver recovered in the form of silver oxide has high purity.
[0016] In step 1, ammonia water is added dropwise to the silver-containing wastewater, and a brown precipitate first appears in the solution. As the ammonia water is added dropwise, the precipitate dissolves and the solution turns back into a colorless and transparent solution.
[0017] In some embodiments, in step 1, the rate of adding ammonia water is 1 L / h to 5 L / h. If the adding is too slow or the time is too long, the recovery efficiency will be affected, and if the adding is insufficient, the conversion of silver ions will be affected, thereby affecting the recovery rate; if the adding is too fast, the ammonia water will be excessive, which will inhibit the release of silver ions and also affect the yield of silver oxide.
[0018] In some embodiments, in step 1, the concentration of ammonia water added is 5-10 mol / L. If the concentration is too low, the size of the silver oxide produced will be too small, making it difficult to completely recycle, and the amount of wastewater will increase significantly; if the concentration is too high, the local NH 3 It is easy to overdose, over-complex the silver ions, and affect the release of silver ions.
[0019] In some embodiments, in step 2, the rate of adding sodium hydroxide solution is 1 to 5 L / h. If the dripping is too slow and the time is too long, the recovery efficiency will be affected, and if the dripping is insufficient, the conversion of silver ions will be affected, thereby affecting the recovery rate; if the dripping is too fast, the sodium hydroxide is easily excessive, the pH is too high, and the remaining impurities in the solution will be precipitated together, affecting the purity of silver oxide.
[0020] In some embodiments, in step 2, the concentration of the sodium hydroxide solution added is 3-5 mol / L. If the concentration is too low, the size of the silver oxide produced will be too small, making it difficult to completely recycle, and the amount of wastewater will increase significantly; if the concentration is too high, the local OH - It is easy to overdo it, causing local impurity ions to precipitate together with silver oxide, affecting the purity of silver oxide.
[0021] In some embodiments, in step 2, the mass ratio of Ag to NaOH is 1.15: 1. This ratio can make sodium hydroxide react with silver ammonium ions in wastewater to generate silver oxide.
[0022] In some embodiments, in step 2, the stirring time is restarted for 10-20 minutes.
[0023] [test]
[0024] Example 1
[0025] Step 1, adding ammonia to silver-containing wastewater: After adding silver-containing wastewater to the precipitation kettle to the highest liquid level, the silver content of the wastewater is 516.57 mg / l, stirring is started, and then ammonia water is added dropwise at a concentration of 8 mol / L. A brown precipitate first appears in the solution. With the addition of ammonia water, the precipitate dissolves, and the solution becomes a colorless and transparent solution again. Stirring is continued for 10 minutes;
[0026] Step 2, synthetic silver oxide reaction: keep stirring, add sodium hydroxide solution to the precipitation kettle, the concentration of which is 4 mol / L, silver oxide begins to be produced in the wastewater, continue to add sodium hydroxide solution until the pH of the solution is 11.87, then let it stand for 1 hour, start stirring again and heat the solution to 80°C;
[0027] Step 3, filter press: filter the slurry in the precipitation kettle, and press the filtrate into the washing tank. Then the filtrate circulates between the washing tank and the filter press until the filtrate is clear and then discharged to the sewage workshop through two-stage precision filters in turn;
[0028] Step 4, washing: unload the filter cake into a washing tank and repeatedly wash it with pure water until the conductivity of the supernatant of the washing liquid is less than 50us / cm, to obtain silver oxide. The silver concentration of the silver oxide synthesis waste liquid is 0.43mg / l, and the silver recovery rate is 99.91%.
[0029] Example 2
[0030] Step 1, adding ammonia to silver-containing wastewater: After adding silver-containing wastewater to the precipitation kettle to the highest liquid level, the silver content of the wastewater is 624.39 mg / l, stirring is started, and then ammonia water is added dropwise at a concentration of 10 mol / L. A brown precipitate first appears in the solution. With the addition of ammonia water, the precipitate dissolves, and the solution becomes a colorless and transparent solution again. Stirring is continued for 10 minutes;
[0031] Step 2, synthetic silver oxide reaction: keep stirring, add sodium hydroxide solution to the precipitation kettle, the concentration of which is 5 mol / L, silver oxide begins to be produced in the wastewater, continue to add sodium hydroxide solution dropwise until the pH of the solution is 11.91, then let it stand for 1 hour, start stirring again and heat the solution to 80°C;
[0032] Step 3, filter press: filter the slurry in the precipitation kettle, and press the filtrate into the washing tank. Then the filtrate circulates between the washing tank and the filter press until the filtrate is clear and then discharged to the sewage workshop through two-stage precision filters in turn;
[0033] Step 4, washing: unload the filter cake into a washing tank and repeatedly wash it with pure water until the conductivity of the supernatant of the washing liquid is less than 50us / cm, to obtain silver oxide. The silver concentration of the silver oxide synthetic waste liquid is 0.38mg / l, and the silver recovery rate is 99.94%.
[0034] Example 3
[0035] Step 1, adding ammonia to silver-containing wastewater: After adding silver-containing wastewater to the precipitation kettle to the highest liquid level, the silver content of the wastewater is 672.25 mg / 1, stirring is started, and then ammonia water is added dropwise at a concentration of 7 mol / L. A brown precipitate first appears in the solution. With the addition of ammonia water, the precipitate dissolves, and the solution becomes a colorless and transparent solution again. Stirring is continued for 10 minutes;
[0036] Step 2, synthetic silver oxide reaction: keep stirring, add sodium hydroxide solution to the precipitation kettle, the concentration of which is 3 mol / L, silver oxide begins to be produced in the wastewater, continue to add sodium hydroxide solution dropwise until the pH of the solution is 11.83, then let it stand for 1 hour, start stirring again and heat the solution to 80°C;
[0037] Step 3, filter press: filter the slurry in the precipitation kettle, and press the filtrate into the washing tank. Then the filtrate circulates between the washing tank and the filter press until the filtrate is clear and then discharged to the sewage workshop through two-stage precision filters in turn;
[0038] Step 4, washing: unload the filter cake into a washing tank and wash it repeatedly with pure water until the conductivity of the supernatant of the washing liquid is less than 50us / cm, to obtain silver oxide. The silver concentration of the silver oxide synthesis waste liquid is 0.40mg / l, and the silver recovery rate is 99.94%.
[0039] It can be seen from the above examples that the silver recovered in the form of silver oxide by the recovery method of the present application has high purity and high recovery rate.
[0040] The above disclosed features are not intended to limit the scope of implementation of the present disclosure. Therefore, all equivalent changes made to the contents described in the claims of the present disclosure should be included in the scope of the claims of the present disclosure.
Claims
1. A method for recovering silver from silver-containing waste liquid, comprising the following steps: Step 1, adding ammonia to the silver-containing wastewater: After adding the silver-containing wastewater to the precipitation kettle to the highest liquid level, start stirring, and then add ammonia water dropwise. A brown precipitate first appears in the solution. As the ammonia water is added dropwise, the precipitate dissolves, and the solution becomes a colorless and transparent solution again. Continue stirring for 10 to 30 minutes; Step 2, synthesizing silver oxide reaction: keep stirring, add sodium hydroxide solution to the precipitation kettle, then let it stand, start stirring again and heat the solution to 60-80° C., and control the pH value to 11.5-12.5; Step 3, filter press: filter the slurry in the precipitation kettle, and press the filtrate into the washing tank. Then the filtrate circulates between the washing tank and the filter press until the filtrate is clear and then discharged to the sewage workshop through two-stage precision filters in turn; Step 4, washing: unloading the filter cake into a washing tank and repeatedly washing with pure water until the conductivity of the washing liquid supernatant is less than 50us / cm, to obtain silver oxide, and the silver ion content in the silver oxide synthesis waste liquid is less than 0.5ppm; In step 1, the concentration of ammonia water added is 5 to 10 mol / L; In step 2, the concentration of the added sodium hydroxide solution is 3 to 5 mol / L; In step 1, the rate of adding ammonia water is: 1 L / h to 5 L / h; In step 2, the rate of adding sodium hydroxide solution is: 1-5 L / h; In step 2, the mass ratio of Ag to NaOH is 1.15:1; In step 2, the stirring time is restarted for 10-20 minutes.
Citation Information
Patent Citations
Shape and size controllable preparation method of micro-nano silver oxide
CN101054199A
Method for recovering sliver from silver-bearing waste liquor
CN104263948A
Production method for separating silver from silver waste liquid
CN107058757A
Silver-containing wastewater treatment device for industrial production
CN215559539U