Chloroprene block copolymer latex

By introducing a polymer block with a high glass transition temperature and a chloroprene polymer block into the polychloroprene block copolymer latex, the problem of vulcanizing agent in the polychloroprene rubber composition is solved It achieves high mechanical stability and heat aging resistance without causing skin allergies and cost increase issues.

CN115335422BActive Publication Date: 2024-10-08DENKA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180024128.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-26
Filing Date
2021-03-22
Publication Date
2024-10-08
Estimated Expiration
2041-03-22

AI Technical Summary

Technical Problem

Existing polychloroprene rubber compositions require the use of vulcanizing agents to obtain mechanical strength, resulting in skin allergies and increased costs. Moreover, styrene·isoprene·styrene triblock copolymer latex does not use vulcanization accelerators. Poor mechanical stability when dosed.

Method used

Develop a chloroprene-based block copolymer latex containing a polymer block with a glass transition temperature of 80°C or higher and a chloroprene-based polymer block, and obtain high tensile strength at break through dip molding and heat treatment and heat aging resistance without the use of vulcanizing agents or vulcanizing accelerators.

Benefits of technology

It is possible to obtain a dip-molded film with excellent mechanical stability, softness, tensile properties and heat aging resistance without using vulcanizing agents or vulcanizing accelerators, reducing the risk of allergies and production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003861600200000061
    Figure BDA0003861600200000061
  • Figure BDA0003861600200000111
    Figure BDA0003861600200000111
  • Figure BDA0003861600200000112
    Figure BDA0003861600200000112
Patent Text Reader

Abstract

A chloroprene block copolymer latex is provided, which has excellent mechanical stability and can obtain a dip-molded film having excellent softness, tensile properties and heat aging resistance even without using a vulcanizing agent and a vulcanization accelerator. According to the present invention, a chloroprene block copolymer latex is provided, which contains a chloroprene block copolymer, wherein the chloroprene block copolymer contains: 5 to 30% by weight of a polymer block (A) derived from a monomer which gives a polymer having a glass transition temperature of 80°C or higher when homopolymerized; and 70 to 95% by weight of a chloroprene polymer block (B) mainly composed of chloroprene monomer units, wherein a film obtained by dip-molding the chloroprene block copolymer latex has a tensile strength at break measured according to JIS K 6251 of 17 MPa or higher after heat treatment at 130°C for 30 minutes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a chloroprene block copolymer latex. Background Art

[0002] Polychloroprene latex is known to be used as a material for dip-molded products such as medical surgical gloves, examination gloves, industrial gloves, balloons, catheters, rubber boots, etc. In addition, it is used as a coating, adhesive, and bonding agent by mixing various additives.

[0003] Various technologies related to polychloroprene for dip-molded products have been proposed. As prior art documents, there are known copolymer latex of chloroprene and 2,3-dichloro-1,3-butadiene (for example, see Patent Document 1), modified polychloroprene latex obtained by copolymerizing chloroprene and methacrylic acid (for example, see Patent Document 2), chloroprene polymer latex not containing a vulcanization accelerator (for example, see Patent Document 3), and polychloroprene latex containing composite zinc oxide containing an inorganic salt and zinc oxide (for example, see Patent Document 4).

[0004] In addition, as technologies related to chloroprene block copolymers, there are copolymers obtained by polymerizing chloroprene using azo group-containing polystyrene as an initiator (for example, see Patent Document 5); copolymers obtained by polymerizing dithiocarbamate-esterified polychloroprene and aromatic vinyl monomers (for example, see Patent Document 6); copolymers obtained by linking chloroprene polymers with hydrophilic oligomers or hydrophilic polymers (for example, see Patent Document 7); copolymers having blocks of aromatic vinyl compound polymers and blocks of chloroprene polymers and having determined overall number average molecular weights and number average molecular weights of the blocks of chloroprene polymers (for example, see Patent Document 8); copolymers having blocks of acrylate polymers and blocks of chloroprene polymers (for example, see Patent Document 9); and as a method for chemically bonding molecules without using vulcanization, there is the technology described in Patent Document 10.

[0005] In addition, various thermoplastic elastomers have been developed as elastomers that can obtain high strength without vulcanization. As a thermoplastic elastomer for dip-molded products, a styrene-isoprene-styrene triblock copolymer latex emulsified by a forced emulsification method has been developed (see, for example, Patent Document 11).

[0006] [Prior art literature]

[0007] [Patent Literature]

[0008] Patent Document 1: International Publication No. 2019 / 009038

[0009] Patent Document 2: Japanese Patent Application Publication No. 2014-114342

[0010] Patent Document 3: International Publication No. 2016 / 166998

[0011] Patent Document 4: International Publication No. 2013 / 015043

[0012] Patent Document 5: Japanese Patent Application Laid-Open No. 3-207710

[0013] Patent Document 6: Japanese Patent Application Laid-Open No. 3-212414

[0014] Patent Document 7: Japanese Patent Application Publication No. 2007-297502

[0015] Patent Document 8: International Publication No. 2018 / 181801

[0016] Patent Document 9: International Publication No. 2019 / 026914

[0017] Patent Document 10: Japanese Patent Application Publication No. 2014-221901

[0018] Patent Document 11: U.S. Patent No. 3238173 Summary of the invention

[0019] Problem that the invention aims to solve

[0020] In the past, in order to obtain the required mechanical strength, polychloroprene rubber compositions inevitably used vulcanizing agents such as sulfur, zinc oxide, and magnesium oxide; as well as vulcanization accelerators such as thiuram, dithiocarbamate, thiourea, guanidine, xanthate, and thiazole. Vulcanization accelerators are type IV allergens that cause skin diseases such as dermatitis, so reducing or eliminating the use of vulcanization accelerators has become an important issue. In addition, not using vulcanization accelerators can not only reduce allergies, but also reduce costs, so it is expected to develop a rubber composition that exhibits sufficient mechanical strength without using vulcanization accelerators.

[0021] On the other hand, styrene-isoprene-styrene triblock copolymer latex and styrene-butadiene-styrene triblock copolymer latex can show sufficient mechanical strength without using a vulcanization accelerator, but since they are produced by a forced emulsification method, the latex particle size cannot be reduced, and there is a problem of poor mechanical stability of the latex.

[0022] Therefore, an object of the present invention is to provide a chloroprene block copolymer latex which has excellent mechanical stability and can provide a dip molding film having excellent flexibility, tensile properties and heat aging resistance without using a vulcanizing agent or a vulcanization accelerator.

[0023] Solutions for solving problems

[0024] The gist of the present invention is as follows.

[0025] (1) A chloroprene block copolymer latex comprising a chloroprene block copolymer, wherein the chloroprene block copolymer comprises 5 to 30% by mass of a polymer block (A) derived from a monomer which, when homopolymerized, can give a polymer having a glass transition temperature of 80° C. or higher; and 70 to 95% by mass of a chloroprene polymer block (B) containing a chloroprene monomer unit.

[0026] The tensile strength at break measured according to JIS K 6251 after heat treatment at 130° C. for 30 minutes obtained by dip-molding the chloroprene block copolymer latex is 17 MPa or more.

[0027] (2) The chloroprene block copolymer latex according to (1), wherein 5 to 15% by mass of the polymer block (A) and 85 to 95% by mass of the chloroprene polymer block (B) are contained in 100% by mass of the chloroprene block copolymer.

[0028] (3) The chloroprene block copolymer latex according to (1) or (2), wherein the average particle size of the chloroprene block copolymer latex measured by a dynamic light scattering method is 300 nm or less.

[0029] (4) The chloroprene block copolymer latex according to any one of (1) to (3), wherein the chloroprene polymer block (B) comprises a chloroprene monomer unit and a polyfunctional monomer unit.

[0030] (5) The chloroprene block copolymer latex according to any one of (1) to (4), which is used for impregnation of a molded article.

[0031] Effects of the Invention

[0032] According to the present invention, there is provided a chloroprene block copolymer latex which has excellent mechanical stability and can provide a dip molding film having excellent flexibility, tensile properties and heat aging resistance without using a vulcanizing agent or a vulcanization accelerator. DETAILED DESCRIPTION

[0033] Hereinafter, embodiments of the present invention will be described in detail. It should be noted that in this specification and claims, "A to B" means A or more and B or less.

[0034] <Chloroprene-based block copolymer latex>

[0035] The chloroprene block copolymer latex contains a chloroprene block copolymer containing 5 to 30% by mass of a polymer block (A) and 70 to 95% by mass of a chloroprene polymer block (B) containing a chloroprene monomer unit.

[0036] [Polymer block (A)]

[0037] The polymer block (A) is a polymer block derived from a monomer that can obtain a polymer with a glass transition temperature of 80°C or more when homopolymerized. By using such a monomer, the tensile strength at break and heat aging resistance of the obtained dip-molded film can be improved. It is preferred to use a monomer that can obtain a polymer with a glass transition temperature of 85°C or more. From the viewpoint of moldability, it is preferred to obtain a monomer with a glass transition temperature of 150°C or less, and it is particularly preferred to obtain a polymer with a glass transition temperature of 120°C or less. The glass transition temperature is, for example, 80, 85, 90, 95, 100, 105, 110, 120, 130, 140, 150°C, and may also be within the range between any two of the values ​​exemplified here. It should be noted that in this specification, the glass transition temperature is the extrapolated glass transition temperature (Teg) measured according to JIS K 7121. When the polymer block (A) is a polymer block obtained by polymerizing a monomer (A), when the monomer A is homopolymerized to form a homopolymer (A) having a number average molecular weight of 10,000 to 30,000, the homopolymer (A) is preferably a monomer having the above-mentioned glass transition temperature.

[0038] As monomer units constituting the polymer block (A), there can be mentioned aromatic vinyl monomer units, methyl methacrylate monomer units, and acrylonitrile monomer units. Preferably, units derived from aromatic vinyl monomers are used, and styrene units are preferably used. Within the scope of not impairing the purpose of the present invention, the polymer block (A) may also be a polymer block obtained by copolymerizing these monomers with each other or a polymer block composed of units derived from these monomers and copolymerizable monomer units.

[0039] The number average molecular weight of the polymer block (A) is preferably 10,000 or more from the viewpoint of the tensile properties, heat aging resistance, and moldability of the obtained dip-molded film. The number average molecular weight of the polymer block (A) can be, for example, 10000, 15000, 20000, 25000, 30000, or within the range between any two values ​​exemplified here. In addition, the molecular weight distribution of the polymer block (A) is preferably 2.0 or less from the viewpoint of moldability. The molecular weight distribution of the polymer block (A) can be, for example, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, or within the range between any two values ​​exemplified here.

[0040] In addition, in this specification, the number average molecular weight and the weight average molecular weight are values ​​measured by gel permeation chromatography (GPC) in terms of polystyrene, and are measured under the following measurement conditions.

[0041] Device name: HLC-8320 (manufactured by Tosoh Corporation)

[0042] Column: 3 TSKgel GMHHR-H connected in series

[0043] Temperature: 40℃

[0044] Detection: Differential refractive index

[0045] Solvent: Tetrahydrofuran

[0046] Standard curve: drawn using standard polystyrene (PS).

[0047] [Chloroprene-based polymer block (B)]

[0048] The chloroprene polymer block (B) contains chloroprene monomer (2-chloro-1,3-butadiene) units and is mainly composed of chloroprene monomer units. The chloroprene polymer block (B) may also contain polyfunctional monomer units. It should be noted that, within the scope of not impairing the purpose of the present invention, the chloroprene polymer block (B) may also be a polymer block composed of chloroprene monomer units, polyfunctional monomer units and units derived from monomers copolymerizable with them. When the chloroprene polymer block (B) is 100% by mass, the chloroprene polymer block (B) preferably contains 90% by mass or more of structural units derived from chloroprene monomers.

[0049] The content of each structural unit in the chloroprene polymer block (B) is not particularly limited, but preferably 90 to 99.95% by mass of the chloroprene monomer unit and 0.05 to 10% by mass of the polyfunctional monomer unit. The content of the polyfunctional monomer unit in the chloroprene polymer block (B) is, for example, 0.05, 0.50, 1.00, 2.00, 3.00, 4.00, 5.00, 6.00, 7.00, 8.00, 9.00, 10.00% by mass, and may be within the range between any two of the values ​​exemplified here.

[0050] [Multifunctional monomer]

[0051] The multifunctional monomer is used to improve the tensile properties and heat aging resistance of the obtained dip molding film. The multifunctional monomer is a compound having two or more free radical polymerizable groups in the molecule. From the viewpoint of the softness, tensile strength at break and moldability of the obtained dip molding film, it is suitable to use the monomer represented by chemical formula (1) and the aromatic polyene monomer. As the monomer represented by chemical formula (1), it is particularly suitable to use 1,9-nonanediol dimethacrylate, 1,9-nonanediol diacrylate, neopentyl glycol dimethacrylate, neopentyl glycol diacrylate, 1,6-hexanediol dimethacrylate, 1,6-hexanediol diacrylate, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, triethylene glycol diacrylate, polyethylene glycol dimethacrylate, polyethylene glycol diacrylate. The aromatic polyene monomer is an aromatic polyene having 10 to 30 carbon atoms and having a plurality of double bonds (vinyl groups) and a single or multiple aromatic groups. Examples thereof include units derived from aromatic polyene monomers such as o-divinylbenzene, p-divinylbenzene, m-divinylbenzene, 1,4-divinylnaphthalene, 3,4-divinylnaphthalene, 2,6-divinylnaphthalene, 1,2-divinyl-3,4-dimethylbenzene, and 1,3-divinyl-4,5,8-tributylnaphthalene. It is preferred to use any one of o-divinylbenzene units, p-divinylbenzene units, and m-vinylbenzene units, or a mixture of two or more thereof.

[0052]

Chemistry 1

[0053]

[0054] (In the formula, R1 and R2 represent hydrogen, chlorine, substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted aryl, substituted or unsubstituted mercapto, or substituted or unsubstituted heterocyclic group. W1 represents a structure containing one or more saturated or unsaturated hydrocarbon groups, saturated or unsaturated cyclic hydrocarbon groups, saturated or unsaturated hydrocarbon groups containing heteroatoms, or saturated or unsaturated cyclic hydrocarbon groups containing heteroatoms. Z1 represents oxygen, nitrogen, or sulfur.)

[0055] The content of each structural unit of the chloroprene block copolymer is 5-30 mass% of polymer block (A) and 70-95 mass% of chloroprene polymer block (B), preferably 5-15 mass% of polymer block (A) and 85-95 mass% of chloroprene polymer block (B). When the polymer block (A) is 5 mass% or more, the tensile strength at break and heat aging resistance of the obtained dip molding film are improved. When the polymer block (A) is 30 mass% or less, the softness of the obtained dip molding film is improved. The polymer block (A) is preferably 15 mass% or less. When the chloroprene polymer block (B) is 70 mass% or more, the softness of the obtained dip molding film is improved. The chloroprene polymer block (B) is preferably 85 mass% or more. When the chloroprene polymer block (B) is 95 mass% or less, the tensile strength at break of the obtained dip molding film is improved. When the chloroprene block copolymer is taken as 100 mass %, the content of the polymer block (A) contained in the chloroprene block copolymer is, for example, 5, 10, 15, 20, 25, or 30 mass %, and may be within the range between any two of the values ​​exemplified here.

[0056] The chloroprene block copolymer according to one embodiment of the present invention may be composed of a polymer block (A) and a polymer block (B), and may not contain other polymer blocks. The chloroprene block copolymer may be a diblock copolymer of a polymer block (A) and a polymer block (B).

[0057] [Average particle size of latex]

[0058] The average particle size measured by dynamic light scattering method for the chloroprene block copolymer latex is preferably 300 nm or less, more preferably 250 nm or less, and further preferably 200 nm or less from the viewpoint of mechanical stability of the latex. The lower limit may be, for example, 100 nm or more. The average particle size may be, for example, 100, 120, 140, 150, 160, 170, 180, 190, 200, 220, 240, 260, 280, 300 nm, or may be within the range between any two values ​​exemplified here.

[0059] It should be noted that in this specification, the average particle size refers to the average particle size measured by dynamic light scattering method and calculated by photon correlation method. The average particle size can be adjusted by controlling the mixing type or amount of the chloroprene block copolymer latex and the production conditions.

[0060] The weight average molecular weight of the chloroprene block copolymer is not particularly limited, but is preferably 50,000 to 600,000, and particularly preferably 100,000 to 500,000, from the viewpoint of molding processability.

[0061] The mechanical stability of the chloroprene block copolymer latex involved in one embodiment of the present invention is preferably 1% by mass or less, more preferably 0.2% by mass or less, and further preferably 0.1% by mass or less. It should be noted that the mechanical stability of the chloroprene block copolymer latex can be evaluated by the determination method described in the embodiment. The mechanical stability can be adjusted by controlling the mixing type or amount of the chloroprene block copolymer latex and the manufacturing conditions, for example, by controlling the average particle size of the chloroprene block copolymer latex.

[0062] [Dip molding film]

[0063] For the chloroprene block copolymer latex of the present embodiment, the tensile strength at break measured according to JIS K 6251 after the chloroprene block copolymer latex is dip-molded to obtain the dip-molded film is 17 MPa or more after heat treatment at 130°C for 30 minutes, and an unvulcanized dip-molded film without a vulcanizing agent and a vulcanization accelerator can be provided. The unvulcanized dip-molded film has flexibility and can exert sufficient mechanical strength even without a vulcanizing agent and a vulcanization accelerator. The tensile strength at break is more preferably 18 MPa or more, more preferably 19 MPa or more, and more preferably 20 MPa or more. The upper limit is not particularly limited, for example, 30 MPa or less.

[0064] For the chloroprene block copolymer latex involved in one embodiment of the present invention, after the above-mentioned dip-molded film is heat-treated at 30°C for 30 minutes and then subjected to a heat aging test at 100°C for 22 hours, the tensile strength at break measured according to JIS K6251 is preferably 17 MPa or more, more preferably 18 MPa or more, further preferably 19 MPa or more, and further preferably 20 MPa or more. The upper limit is not particularly limited, for example, it is 30 MPa or less.

[0065] In addition, for the chloroprene block copolymer latex of the present embodiment, the elongation at break measured according to JIS K 6251 after the dip-molded film obtained by dip-molding the chloroprene block copolymer latex is heat-treated at 130° C. for 30 minutes is preferably 900% or more, more preferably 905% or more, and further preferably 910% or more. The upper limit is not particularly limited, and is, for example, 1300% or less.

[0066] For the chloroprene block copolymer latex involved in one embodiment of the present invention, after the above-mentioned dip-molded film is heat-treated at 30°C for 30 minutes and then subjected to a heat aging test at 100°C for 22 hours, the elongation at break measured according to JIS K6251 is preferably 900% or more, more preferably 905% or more, and further preferably 910% or more. The upper limit is not particularly limited, and is, for example, 1300% or less.

[0067] The chloroprene block copolymer latex of the present embodiment preferably has a 500% elongation modulus of 3.0 MPa or less, more preferably 2.9 MPa or less, and further preferably 2.8 MPa or less, measured according to JIS K 6251 after heat treatment at 130° C. for 30 minutes for a dip-molded film obtained by dip-molding the chloroprene block copolymer latex. The lower limit is not particularly limited, and is, for example, 1.0 MPa or more.

[0068] For the chloroprene block copolymer latex involved in one embodiment of the present invention, after the above-mentioned dip-molded film is heat-treated at 30°C for 30 minutes and then subjected to a heat aging test at 100°C for 22 hours, the 500% elongation modulus measured according to JIS K6251 is preferably 3.0 MPa or less, more preferably 2.9 MPa or less, and further preferably 2.8 MPa or less. The lower limit is not particularly limited, and is, for example, 1.0 MPa or more.

[0069] It should be noted that the above-mentioned dip-molded film can be obtained by the method described in the Examples, and no vulcanizing agent and vulcanization accelerator are used during the molding of the dip-molded film.

[0070] In order to adjust the tensile strength at break, elongation at break and 500% elongation modulus of the dip-molded film obtained by dip-molding the chloroprene block copolymer latex, the amount of the polyfunctional monomer added may be adjusted, the content of the polyfunctional monomer unit contained in the chloroprene polymer block (B) or the content of the chloroprene polymer block (B) in the chloroprene block copolymer may be adjusted, or the type or amount of the functional group introduced by polymerization in the presence of a RAFT agent described below may be adjusted.

[0071] The dip-molded film obtained from the chloroprene block copolymer latex of the present embodiment may contain a vulcanizing agent or a vulcanization accelerator. When the dip-molded film contains a vulcanizing agent and a vulcanization accelerator, the total content can be 5% by mass or less, more preferably 1% by mass or less, and further preferably 0.1% by mass. However, even if the above-mentioned unvulcanized dip-molded film does not contain a vulcanizing agent and a vulcanization accelerator, it also has sufficient mechanical strength, so from the viewpoint of reducing allergic reactions and reducing costs, it is preferably free of a vulcanizing agent and a vulcanization accelerator.

[0072] [Method for producing chloroprene block copolymer latex]

[0073] The method for producing the chloroprene block copolymer latex involved in the present invention is described. The production method is not particularly limited as long as the desired chloroprene block copolymer latex can be obtained, and the chloroprene block copolymer latex can be obtained by the following production method: the chloroprene block copolymer latex is obtained through a secondary polymerization step consisting of an emulsion polymerization step 1 for synthesizing a polymer block (A) and an emulsion polymerization step 2 for synthesizing a chloroprene polymer block (B).

[0074] (Emulsion polymerization step 1)

[0075] The emulsion polymerization step 1 is described in detail. In the emulsion polymerization step 1, the monomers constituting the polymer block (A) are subjected to active free radical emulsion polymerization to synthesize the polymer block (A). As described above, the polymer block (A) obtained here preferably has the above-mentioned glass transition temperature. As the emulsifier used in the emulsion polymerization, there is no particular limitation, and from the viewpoint of emulsification stability, an anionic or nonionic emulsifier is preferred. In particular, for the reason that the dip molding film obtained from the obtained chloroprene block copolymer latex has appropriate strength and prevents excessive shrinkage and breakage, it is preferred to use an alkali metal salt of rosin acid. From the viewpoint of effectively carrying out the polymerization reaction, the concentration of the emulsifier is preferably 5 to 50% by mass relative to 100% by mass of the monomers constituting the polymer block (A). As a free radical polymerization initiator, a known free radical polymerization initiator can be used, for example, potassium persulfate, benzoyl peroxide, hydrogen peroxide, azo compounds, etc. The amount of pure water added is preferably 100 to 300% by mass relative to 100% by mass of the monomers constituting the polymer block (A). When the amount of pure water added is 300 mass % or less, the tensile strength at break of the obtained dip-molded film is improved. The polymerization temperature may be appropriately determined depending on the type of monomers, but is preferably 10 to 100°C, particularly preferably 20 to 80°C.

[0076] (Emulsion polymerization step 2)

[0077] In the emulsion polymerization step 2, pure water, an emulsifier, chloroprene monomers and multifunctional monomers are added to the latex containing the polymer block (A) obtained by the active free radical emulsion polymerization in the above-mentioned emulsion polymerization step 1 to carry out emulsion polymerization, thereby obtaining a chloroprene block copolymer latex. The chloroprene monomer can be added all at once or in batches. From the viewpoint of easy polymerization, the polymerization temperature of the emulsion polymerization step 2 is preferably 10 to 50°C. The polymerization reaction can be terminated by adding a polymerization terminator. As polymerization terminators, for example, there are thiodiphenylamine, 4-tert-butylcatechol, 2,2'-methylenebis-4-methyl-6-tert-butylphenol, etc. After the emulsion polymerization is completed, the unreacted monomers can be removed by conventional methods such as vacuum distillation.

[0078] To the chloroprene block copolymer latex obtained in the emulsion polymerization step 2, a freezing stabilizer, an emulsion stabilizer, a viscosity modifier, an antioxidant, a preservative, etc. may be optionally added after polymerization within a range not impairing the purpose of the present invention.

[0079] The chloroprene-based block copolymer preferably has a functional group having a structure represented by the following chemical formula (2) or chemical formula (3).

[0080]

Chemistry 2

[0081]

[0082]

Chemistry 3

[0083]

[0084] (In the chemical formula (2), R3 represents hydrogen, chlorine, substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted aryl, substituted or unsubstituted mercapto, or substituted or unsubstituted heterocyclic group.)

[0085] The terminal structure represented by the above chemical formula (2) or chemical formula (3) is introduced into the block copolymer by emulsion polymerization in the presence of a known RAFT agent. The compound into which the structure represented by the above chemical formula (2) is introduced is not particularly limited, and common compounds can be used, for example, dithiocarbamates and dithioesters. Specifically, benzyl-1-pyrrole dithiocarbamate (common name: benzyl 1-pyrrole dithiocarbamate), benzylphenyl dithiocarbamate, 1-benzyl-N,N-dimethyl-4-aminodithiobenzoate, 1-benzyl-4-methoxydithiobenzoate, 1-phenylethylimidazole dithiocarbamate (common name: 1-phenylethylimidazole dithiocarbamate), benzyl-1-(2-pyrrolidone) dithiocarbamate) (common name: benzyl-1-(2-pyrrolidone) dithiocarbamate), benzylphthalimido dithiocarbamate (common name: benzylphthalimido dithiocarbamate), 2-phenylethylimidazole dithiocarbamate (common name: benzyl ... -cyanopropan-2-yl-1-pyrrole dithiocarbamate (common name: 2-cyanopropan-2-yl-1-pyrrole dithiocarbamate), 2-cyanobutyl-2-yl-1-pyrrole dithiocarbamate (common name: 2-cyanobutyl-2-yl-1-pyrrole dithiocarbamate), benzyl-1-imidazole dithiocarbamate (common name: benzyl-1-imidazole dithiocarbamate), 2-cyanopropan-2-yl-N,N-dimethyl dithiocarbamate, benzyl-N,N-diethyl dithiocarbamate, cyanomethyl-1-(2-pyrrolidone) dithiocarbamate, 2-(ethoxycarbonylbenzyl)propan-2-yl-N,N- diethyl dithiocarbamate, 1-phenylethyl dithiobenzoate, 2-phenylpropan-2-yl dithiobenzoate, 1-acet-1-yl-ethyl dithiobenzoate, 1-(4-methoxyphenyl)ethyl dithiobenzoate, benzyl dithioacetate, ethoxycarbonylmethyl dithioacetate, 2-(ethoxycarbonyl)propan-2-yl dithiobenzoate, 2-cyanopropan-2-yl dithiobenzoate, tert-butyl dithiobenzoate, 2,4,4-trimethylpentan-2-yl dithiobenzoate, 2-(4-chlorophenyl)-propan-2-yl dithiobenzoate, 3-vinylbenzyl dithiobenzoate, 4-vinylbenzyl dithiobenzoate, benzyl diethoxyphosphinyl dithiocarboxylate, tert-butyl trithioperbenzoate, 2-phenylpropan-2-yl-4-chlorodithiobenzoate, 1-methyl-1-phenyl-ethyl naphthalene-1-carboxylate, 4-cyano-4-methyl-4-thiobenzylmercaptobutyric acid, dibenzyl tetrathioterephthalate, carboxymethyl dithiobenzoate, poly(ethylene oxide) having dithiobenzoate terminal groups, poly(ethylene oxide) having 4-cyano-4-methyl-4-thiobenzylmercaptobutyric acid terminal groups, 2-[(2-phenylethanesulfonyl)mercapto]propionic acid, 2-[(2-phenylethanesulfonyl)mercapto]succinic acid, 3,Potassium 5-dimethyl-1H-pyrazole-1-dithiocarboxylate, cyanomethyl-3,5-dimethyl-1H-pyrazole-1-dithiocarboxylate, cyanomethylmethyl-(phenyl)dithiocarbamate, benzyl-4-chlorodithiobenzoate, phenylmethyl-4-chlorodithiobenzoate, 4-nitrobenzyl-4-chlorodithiobenzoate, phenylpropan-2-yl-4-chlorodithiobenzoate, 1-cyano-1- Methyl 4-chlorodithiobenzoate, 3-chloro-2-butenyl-4-chlorodithiobenzoate, 2-chloro-2-butenyl dithiobenzoate, benzyl dithioacetate, 3-chloro-2-butenyl-1H-pyrrole-1-dithiocarboxylic acid, 2-cyanobutane-2-yl-4-chloro-3,5-dimethyl-1H-pyrazole-1-dithiocarboxylate, cyanomethylmethyl (phenyl)aminodithiocarboxylate. Among them, benzyl-1-pyrrole dithiocarboxylate and benzylphenyl dithiocarboxylate are particularly preferably used. The compound from which the structure represented by the above chemical formula (3) is derived is not particularly limited, and general compounds can be used, for example, 2-cyano-2-propyldodecyl trithiocarbonate, dibenzyl trithiocarbonate, butylbenzyl trithiocarbonate, 2-[[(butylthio)thiooxymethyl]thio]propionic acid, 2-[[(dodecylthio)thiooxymethyl]thio]propionic acid, 2-[[(butylthio)thiooxymethyl]thio]succinic acid, 2-[[(dodecylthio)thiooxymethyl]thio]succinic acid, 2-[[(dodecylthio)thiooxymethyl]thio]succinic acid, Trithiocarbonates such as [(tert-butyl)thio]thiooxymethyl]thio]-2-methylpropionic acid, 2,2′-[carbonylsulfonylbis(thio)]bis[2-methylpropionic acid], 2-amino-1-methyl-2-oxoethylbutyl trithiocarbonate, benzyl 2-[(2-hydroxyethyl)amino]-1-methyl-2-oxoethyl trithiocarbonate, 3-[[[(tert-butyl)thio]thiooxymethyl]thio]propionic acid, cyanomethyldodecyl trithiocarbonate, diethylaminobenzyl trithiocarbonate, and dibutylaminobenzyl trithiocarbonate are particularly preferably used. Among them, dibenzyl trithiocarbonate and butylbenzyl trithiocarbonate are particularly preferably used.

[0086] [Impregnation molding]

[0087] The dip molded article involved in this embodiment is obtained by dip molding the above-mentioned chloroprene block copolymer latex, and has low modulus, is soft, and has excellent mechanical properties such as tensile strength at break and elongation at break, and is also excellent in heat aging resistance. As the dip molded article, gloves, balloons and catheters are preferred. The dip molded article involved in one embodiment of the present invention can also be obtained by molding a chloroprene block copolymer latex composition containing the above-mentioned chloroprene block copolymer latex.

[0088] As a molding method when manufacturing the impregnation molded body of the present embodiment, a coagulation liquid impregnation method can be mentioned, for example, but it is not limited to this, and molding may be performed according to a conventional method.

[0089] The dip molded article of this embodiment may contain fillers or reinforcing agents, plasticizers, processing aids, lubricants, antioxidants, silane coupling agents, etc. within the range not impairing the purpose of the present invention. These additives can be appropriately selected according to the purpose and application.

[0090] The dip molded body of this embodiment may not contain a vulcanizing agent and / or a vulcanization accelerator. That is, the above-mentioned dip molded body includes a case where it contains a vulcanizing agent and does not contain a vulcanization accelerator; a case where it contains a vulcanizing agent and a vulcanization accelerator; a case where it does not contain a vulcanizing agent and a vulcanization accelerator. Whether to mix a vulcanizing agent and a vulcanization accelerator can be determined according to the target dip molded body. When the dip molded body involved in one embodiment of the present invention contains a vulcanizing agent and / or a vulcanization accelerator, when the dip molded body is set to 100% by mass, the total content of the vulcanizing agent and the vulcanization accelerator can be made to be less than 5% by mass, more preferably less than 1% by mass, and further preferably 0.1% by mass. The dip molded body involved in one embodiment of the present invention may also be free of a vulcanizing agent and a vulcanization accelerator from the viewpoint of reducing allergic reactions and reducing costs. Even if the dip molded body does not contain a vulcanizing agent and a vulcanization accelerator, it has sufficient mechanical strength.

[0091] Examples of the vulcanizing agent include sulfur, zinc oxide, and magnesium oxide.

[0092] Vulcanization accelerators are additives added to the raw rubber during vulcanization in order to interact with the vulcanizer to increase the vulcanization rate, shorten the vulcanization time, lower the vulcanization temperature, reduce the amount of vulcanizer, and improve the physical properties of the vulcanized rubber. They usually refer to additives that promote sulfur vulcanization reactions.

[0093] Examples of vulcanization accelerators generally used for vulcanization of chloroprene copolymer latex include thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthate-based, and thiazole-based vulcanization accelerators. These may be used alone or in combination of two or more as necessary.

[0094] The dip-molded article of the present embodiment can exhibit excellent mechanical properties regardless of whether a vulcanizing agent and a vulcanization accelerator are added. However, from the viewpoint of reducing allergic reactions and reducing costs, it is preferred that no vulcanizing agent and a vulcanization accelerator are contained.

[0095] As the anti-aging agent added to the dip molded body of the present embodiment, a primary anti-aging agent used in common rubber applications to prevent self-oxidation by capturing free radicals and a secondary anti-aging agent that renders hydroperoxide harmless can be added. These anti-aging agents can be added in an amount of 0.1% to 100 parts by mass of the rubber component in the chloroprene copolymer latex.The ratio of more than 1 mass part and less than 10 mass parts is added, preferably the scope of more than 2 mass parts and less than 5 mass parts. These anti-aging agents can be used alone or more than 2 kinds can be used in combination. It should be noted that as the primary anti-aging agent, phenolic anti-aging agent, amine anti-aging agent, acrylate anti-aging agent, imidazole anti-aging agent, carbamate metal salt, wax can be enumerated. In addition, as the secondary anti-aging agent, phosphorus anti-aging agent, sulfur anti-aging agent, imidazole anti-aging agent etc. can be enumerated. Examples of the antioxidant include, but are not particularly limited to, N-phenyl-1-naphthylamine, alkylated diphenylamine, octylated diphenylamine, 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, p-(p-toluenesulfonamide)diphenylamine, N,N'-di-2-naphthyl-p-phenylenediamine, N,N'-diphenyl-p-phenylenediamine, N-phenyl-N'-isopropyl-p-phenylenediamine, N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, N-phenyl-N'-(3-methacryloyloxy-2-hydroxypropyl)-p-phenylenediamine, 1,1 , 3-tris-(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 4,4'-butylenebis-(3-methyl-6-tert-butylphenol), 2,2-thiobis(4-methyl-6-tert-butylphenol), 7-octadecyl-3-(4'-hydroxy-3',5'-di-tert-butylphenyl)propionate, tetrakis-[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate]methane, pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], triethylene glycol-bis[3- (3-tert-butyl-5-methyl-4-hydroxyphenyl) propionate], 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], 2,4-bis(n-octylthio)-6-(4-hydroxy-3,5-di-tert-butylphenylamino)-1,3,5-triazine, tris-(3,5-di-tert-butyl-4-hydroxybenzyl)-isocyanurate, 2,2-thio-diethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], N,N'-hexamethylenebis(3,5-di- tert-butyl-4-hydroxy)-hydrocinnamic acid, 2,4-bis[(octylthio)methyl]-o-cresol, 3,5-di-tert-butyl-4-hydroxybenzyl-phosphonate-diethyl ester, tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane, octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and 3,9-bis[2-{3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5] undecane, tris(nonylphenyl)phosphite, tris(mixed mono- and di-nonylphenyl)phosphite, diphenyl mono(2-ethylhexyl)phosphite, diphenyl monotridecylphosphite, diphenyl isodecylphosphite, diphenyl isooctylphosphite, diphenyl nonylphenylphosphite, triphenylphosphite, tritridecylphosphite, triisodecylphosphite, tris(2-ethylhexyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, tetraphenyldipropylene glycol diphosphite, tetraphenyltetra(tridecyl)pentaerythritol tetraphosphite, 1,1,3-tris(2-methyl-4-di-tridecylphosphite-5-tert-butylphenyl)butane, 4,4 '-Butylenebis-(3-methyl-6-tert-butyl-di-tridecylphosphite), 2,2'-ethylenebis(4,6-di-tert-butylphenol)fluorophosphite, 4,4'-isopropylidene-diphenol alkyl (C12-C15)phosphite, cyclic neopentanetetraylbis(2,4-di-tert-butylphenylphosphite), cyclic neopentanetetraylbis(2,6-di-tert-butyl-4-phenylphosphite), cyclic neopentanetetraylbis(nonylphenylphosphite), bis(nonylphenyl)pentaerythritol diphosphite, dibutyl hydrogenphosphite, distearylpentaerythritol·diphosphite and hydrogenated bisphenol A pentaerythritol phosphite polymer, 2-mercaptobenzimidazole, butylation reaction product of p-cresol and dicyclopentadiene, etc.

[0096] [Example]

[0097] The present invention will be described below with reference to Examples and Comparative Examples, but these are merely illustrative and do not limit the contents of the present invention.

[0098] (Example 1)

[0099] (Polymerization Step 1) Synthesis of Polymer Block (A-1)

[0100] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a jacket for heating and cooling. 4666 g of pure water, 224 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 350 g of styrene monomer, and 6.07 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 3.82 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. 20 ml of the obtained latex was sampled and the physical properties were measured, and the remaining latex was used in the polymerization step 2.

[0101] The sampled latex was mixed with a large amount of methanol to precipitate the resin component, and the sample of the polymer block (A-1) was obtained by filtering and drying. The number average molecular weight, molecular weight distribution and glass transition temperature of the polymer block (A) were determined by analyzing the obtained sample. The analysis results are shown in Table 1. It should be noted that the determination methods of "number average molecular weight", "molecular weight distribution" and "glass transition temperature" will be described below.

[0102] (Polymerization Step 2) Synthesis of Chloroprene-Based Polymer Block (B-1)

[0103] After the polymerization step 1, when the internal temperature dropped to 45°C, 4480 g of chloroprene monomer and 91.4 g of 1,9-nonanediol dimethacrylate were slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reached 80%, a 10 wt % aqueous solution of a polymerization terminator N,N-diethylhydroxylamine was added to terminate the polymerization, and the unreacted chloroprene monomer was removed by reduced pressure distillation. 20 ml of the obtained latex was sampled and measured for physical properties, and the remaining latex was used to prepare a film for evaluation.

[0104] The average particle size of the latex and the mechanical stability of the latex were measured using a portion of the sampled latex. The analysis results are shown in Table 1. It should be noted that the measurement method will be described below. In addition, the sampled latex was mixed with a large amount of methanol to precipitate the resin components, and a sample of the chloroprene block copolymer was obtained by filtering and drying. The content (mass %) of the polymer block (A-1) and the chloroprene polymer block (B-1) of the chloroprene block copolymer was determined by analyzing the obtained sample. The analysis results are shown in Table 1. It should be noted that the measurement method will be described below.

[0105] (Example 2)

[0106] (Polymerization Step 1) Synthesis of Polymer Block (A-2)

[0107] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a heating and cooling jacket. 3333 g of pure water, 160 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 26.0 g of potassium hydroxide, 13.3 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 250 g of styrene monomer, and 4.33 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 2.73 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. 20 ml of the obtained latex was sampled and measured for physical properties, and the remaining latex was used in the polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-2) were determined by analysis in the same manner as in Example 1. Table 1 shows the analysis results.

[0108] (Polymerization Step 2) Synthesis of Chloroprene-Based Polymer Block (B-2)

[0109] After the polymerization step 1, when the internal temperature drops to 45°C, 5584 g of chloroprene monomer and 114.0 g of 1,9-nonanediol dimethacrylate are slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reaches 80%, a 10 wt% aqueous solution of the polymerization terminator N,N-diethylhydroxylamine is added to terminate the polymerization, and the unreacted chloroprene monomer is removed by vacuum distillation. 20 ml of the obtained latex is sampled to measure the physical properties, and the remaining latex is used to prepare an evaluation film. The average particle size of the latex, the mechanical stability of the latex, and the content (mass %) of the polymer block (A-2) of the chloroprene block copolymer and the chloroprene polymer block (B-2) are determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0110] (Example 3)

[0111] (Polymerization Step 1) Synthesis of Polymer Block (A-3)

[0112] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a heating and cooling jacket. 5733 g of pure water, 275 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 44.7 g of potassium hydroxide, 22.9 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 430 g of styrene monomer, and 7.45 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 4.69 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. 20 ml of the obtained latex was sampled and measured for physical properties, and the remaining latex was used in the polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-3) were determined by analysis in the same manner as in Example 1. Table 1 shows the analysis results.

[0113] (Polymerization Step 2) Synthesis of Chloroprene-Based Polymer Block (B-3)

[0114] After the polymerization step 1, when the internal temperature drops to 45°C, 3094 g of chloroprene monomer and 63.1 g of 1,9-nonanediol dimethacrylate are slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reaches 80%, a 10 wt% aqueous solution of the polymerization terminator N,N-diethylhydroxylamine is added to terminate the polymerization, and the unreacted chloroprene monomer is removed by vacuum distillation. 20 ml of the obtained latex is sampled to measure the physical properties, and the remaining latex is used to prepare an evaluation film. The average particle size of the latex, the mechanical stability of the latex, the content (mass %) of the polymer block (A-3) of the chloroprene block copolymer, and the chloroprene polymer block (B-3) are determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0115] (Example 4)

[0116] (Polymerization Step 1) Synthesis of Polymer Block (A-4)

[0117] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a heating and cooling jacket. 4666 g of pure water, 224 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 350 g of styrene monomer, and 6.07 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 3.82 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. 20 ml of the obtained latex was sampled and measured for physical properties, and the remaining latex was used in the polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-4) were determined by analysis in the same manner as in Example 1. Table 1 shows the analysis results.

[0118] (Polymerization Step 2) Synthesis of Chloroprene-Based Polymer Block (B-4)

[0119] After the polymerization step 1, when the internal temperature drops to 45°C, 4480 g of chloroprene monomer and 91.4 g of 1,9-nonanediol diacrylate are slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reaches 80%, a 10 wt% aqueous solution of the polymerization terminator N,N-diethylhydroxylamine is added to terminate the polymerization, and the unreacted chloroprene monomer is removed by vacuum distillation. 20 ml of the obtained latex is sampled to measure the physical properties, and the remaining latex is used to prepare an evaluation film. The average particle size of the latex, the mechanical stability of the latex, and the content (mass %) of the polymer block (A-4) and the chloroprene polymer block (B-4) of the chloroprene block copolymer are determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0120] (Example 5)

[0121] (Polymerization Step 1) Synthesis of Polymer Block (A-5)

[0122] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a heating and cooling jacket. 4666 g of pure water, 224 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 350 g of styrene monomer, and 6.07 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 3.82 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. 20 ml of the obtained latex was sampled and measured for physical properties, and the remaining latex was used in the polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-5) were determined by analysis in the same manner as in Example 1. Table 1 shows the analysis results.

[0123] (Polymerization Step 2) Synthesis of Chloroprene-Based Polymer Block (B-5)

[0124] After the polymerization step 1, when the internal temperature drops to 45°C, 4480 g of chloroprene monomer and 91.4 g of Light Ester EG (manufactured by Kyoeisha Chemical Co., Ltd.) as ethylene glycol diacrylate are slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reaches 80%, a 10 wt% aqueous solution of the polymerization terminator N,N-diethylhydroxylamine is added to terminate the polymerization, and the unreacted chloroprene monomer is removed by vacuum distillation. 20 ml of the obtained latex is sampled to measure the physical properties, and the remaining latex is used to prepare an evaluation film. The average particle size of the latex, the mechanical stability of the latex, and the content (mass %) of the polymer block (A-5) and the chloroprene polymer block (B-5) of the chloroprene block copolymer are determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0125] (Example 6)

[0126] (Polymerization Step 1) Synthesis of Polymer Block (A-6)

[0127] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a heating and cooling jacket. 4666 g of pure water, 224 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 350 g of styrene monomer, and 6.07 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 3.82 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. 20 ml of the obtained latex was sampled and measured for physical properties, and the remaining latex was used in the polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-6) were determined by analysis in the same manner as in Example 1. Table 1 shows the analysis results.

[0128] (Polymerization Step 2) Synthesis of Chloroprene-Based Polymer Block (B-6)

[0129] After the polymerization step 1, when the internal temperature drops to 45°C, 4480 g of chloroprene monomer and 93.3 g of divinylbenzene are slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reaches 80%, a 10 wt% aqueous solution of the polymerization terminator N,N-diethylhydroxylamine is added to terminate the polymerization, and the unreacted chloroprene monomer is removed by vacuum distillation. 20 ml of the obtained latex is sampled to measure the physical properties, and the remaining latex is used to prepare an evaluation film. The average particle size of the latex, the mechanical stability of the latex, and the content (mass %) of the polymer block (A-6) of the chloroprene block copolymer and the chloroprene polymer block (B-6) are determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0130] (Example 7)

[0131] (Polymerization Step 1) Synthesis of Polymer Block (A-7)

[0132] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a jacket for heating and cooling. 5450 g of pure water, 262 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 42.5 g of potassium hydroxide, 21.8 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 2500 g of styrene monomer, and 43.3 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 27.3 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. 20 ml of the obtained latex was sampled and the physical properties were measured, and the remaining latex was used in the polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-7) were determined by analysis in the same manner as in Example 1. Table 1 shows the analysis results.

[0133] (Polymerization Step 2) Synthesis of Chloroprene-Based Polymer Block (B-7)

[0134] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a jacket for heating and cooling. 2732 g of pure water, 131 g of potassium disproportionate rosin acid (produced by Harima Chemicals), 21.3 g of potassium hydroxide, 10.9 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (produced by Kao Corporation, trade name: Demol N), and 783 g of latex containing the polymer block (A-2) obtained in the polymerization step 1 were added, the internal temperature was set to 45°C, and the mixture was stirred at 200 rpm under a nitrogen stream. Thereafter, 3000 g of chloroprene monomer was slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reached 80%, a 10 wt% aqueous solution of a polymerization terminator N,N-diethylhydroxylamine was added to terminate the polymerization, and the unreacted chloroprene monomer was removed by distillation under reduced pressure. 20 ml of the obtained latex was sampled to measure the physical properties, and the remaining latex was used to prepare a membrane for evaluation. The average particle size of the latex, the mechanical stability of the latex, the content (mass %) of the polymer block (A-7) and the chloroprene polymer block (B-7) of the chloroprene block copolymer, and the toluene insoluble component were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0135] (Example 8)

[0136] (Polymerization Step 1) Synthesis of Polymer Block (A-8)

[0137] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a heating and cooling jacket. 4666 g of pure water, 224 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 350 g of styrene monomer, and 6.07 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 3.82 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. 20 ml of the obtained latex was sampled and measured for physical properties, and the remaining latex was used in the polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-8) were determined by analysis in the same manner as in Example 1. Table 1 shows the analysis results.

[0138] (Polymerization Step 2) Synthesis of Chloroprene-Based Polymer Block (B-8)

[0139] After the polymerization step 1, when the internal temperature drops to 45°C, 4480 g of chloroprene monomer and 91.4 g of triallyl isocyanurate are slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reaches 80%, a 10 wt% aqueous solution of the polymerization terminator N,N-diethylhydroxylamine is added to terminate the polymerization, and the unreacted chloroprene monomer is removed by vacuum distillation. 20 ml of the obtained latex is sampled to measure the physical properties, and the remaining latex is used to prepare an evaluation film. The average particle size of the latex, the mechanical stability of the latex, and the content (mass %) of the polymer block (A-8) of the chloroprene block copolymer and the chloroprene polymer block (B-8) are determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0140] (Example 9)

[0141] (Polymerization Step 1) Synthesis of Polymer Block (A-9)

[0142] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a heating and cooling jacket. 4666 g of pure water, 224 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 350 g of styrene monomer, and 6.07 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 3.82 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. 20 ml of the obtained latex was sampled and measured for physical properties, and the remaining latex was used in the polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-9) were determined by analysis in the same manner as in Example 1. Table 1 shows the analysis results.

[0143] (Polymerization Step 2) Synthesis of Chloroprene-Based Polymer Block (B-9)

[0144] After the polymerization step 1, when the internal temperature drops to 45°C, 4480 g of chloroprene monomer and 91.4 g of hydroxypyvalypivlate diacrylate (manufactured by Kyoeisha Chemical Co., Ltd.) are slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reaches 80%, a 10 wt% aqueous solution of the polymerization terminator N,N-diethylhydroxylamine is added to terminate the polymerization, and the unreacted chloroprene monomer is removed by vacuum distillation. 20 ml of the obtained latex is sampled to measure the physical properties, and the remaining latex is used to prepare an evaluation film. The average particle size of the latex, the mechanical stability of the latex, and the content (mass %) of the polymer block (A-9) and the chloroprene polymer block (B-9) of the chloroprene block copolymer are determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0145] (Example 10)

[0146] (Polymerization Step 1) Synthesis of Polymer Block (A-10)

[0147] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a jacket for heating and cooling. 4666 g of pure water, 224 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 350 g of styrene monomer, and 6.07 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 3.82 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. 20 ml of the obtained latex was sampled to measure the physical properties, and the remaining latex was used in the polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-10) were determined by analysis in the same manner as in Example 1. Table 1 shows the analysis results.

[0148] (Polymerization Step 2) Synthesis of Chloroprene-Based Polymer Block (B-10)

[0149] After the polymerization step 1, when the internal temperature drops to 45°C, 4480 g of chloroprene monomer and 91.4 g of trimethylolpropane triacrylate (produced by Kyoeisha Chemical Co., Ltd.) are slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reaches 80%, a 10 wt% aqueous solution of the polymerization terminator N,N-diethylhydroxylamine is added to terminate the polymerization, and the unreacted chloroprene monomer is removed by vacuum distillation. 20 ml of the obtained latex is sampled to measure the physical properties, and the remaining latex is used to prepare an evaluation film. The average particle size of the latex, the mechanical stability of the latex, and the content (mass %) of the polymer block (A-10) and the chloroprene polymer block (B-10) of the chloroprene block copolymer are determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0150] (Example 11)

[0151] (Polymerization Step 1) Synthesis of Polymer Block (A-11)

[0152] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a jacket for heating and cooling. 6667 g of pure water, 320 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 52.0 g of potassium hydroxide, 26.7 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 500 g of styrene monomer, and 6.50 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 4.09 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. 20 ml of the obtained latex was sampled and the physical properties were measured, and the remaining latex was used in the polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-11) were determined by analysis in the same manner as in Example 1. Table 1 shows the analysis results.

[0153] (Polymerization Step 2) Synthesis of Chloroprene-Based Polymer Block (B-11)

[0154] After the polymerization step 1, when the internal temperature drops to 45°C, 1607 g of chloroprene monomer and 32.8 g of 1,9-nonanediol dimethacrylate are slowly added over 2 hours for polymerization. When the polymerization rate of the chloroprene monomer reaches 80%, a 10 wt% aqueous solution of the polymerization terminator N,N-diethylhydroxylamine is added to terminate the polymerization, and the unreacted chloroprene monomer is removed by vacuum distillation. 20 ml of the obtained latex is sampled to measure the physical properties, and the remaining latex is used to prepare an evaluation film. The average particle size of the latex, the mechanical stability of the latex, and the content (mass %) of the polymer block (A-11) of the chloroprene block copolymer and the chloroprene polymer block (B-11) are determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0155] (Example 12)

[0156] (Polymerization Step 1) Synthesis of Polymer Block (A-12)

[0157] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a jacket for heating and cooling. 5450 g of pure water, 262 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 42.5 g of potassium hydroxide, 21.8 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 2500 g of styrene monomer, and 32.5 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 20.5 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. 20 ml of the obtained latex was sampled and the physical properties were measured, and the remaining latex was used in the polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-12) were determined by analysis in the same manner as in Example 1. Table 1 shows the analysis results.

[0158] (Polymerization Step 2) Synthesis of Chloroprene-Based Polymer Block (B-12)

[0159] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a jacket for heating and cooling. 1188 g of pure water, 57 g of potassium disproportionate rosin acid (produced by Harima Chemicals), 9.3 g of potassium hydroxide, 4.8 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (produced by Kao Corporation, trade name: Demol N), and 3147 g of latex containing the polymer block (A-12) obtained in the polymerization step 1 were added, the internal temperature was set to 45°C, and the mixture was stirred at 200 rpm under a nitrogen stream. Thereafter, 3000 g of chloroprene monomer was slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reached 80%, a 10 wt% aqueous solution of a polymerization terminator N,N-diethylhydroxylamine was added to terminate the polymerization, and the unreacted chloroprene monomer was removed by vacuum distillation. 20 ml of the obtained latex was sampled to measure the physical properties, and the remaining latex was used to prepare a membrane for evaluation. The average particle size of the latex, the mechanical stability of the latex, the content (mass %) of the polymer block (A-12) and the chloroprene polymer block (B-12) of the chloroprene block copolymer, and the toluene insoluble component were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0160] (Example 13)

[0161] (Polymerization Step 1) Synthesis of Polymer Block (A-13)

[0162] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a jacket for heating and cooling. 4666 g of pure water, 224 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 350 g of methyl methacrylate monomer, and 4.14 g of butyl-2-cyanoisopropyl trithiocarbonate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 2.87 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. 20 ml of the obtained latex was sampled to measure the physical properties, and the remaining latex was used in the polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-13) were determined by analysis in the same manner as in Example 1. Table 1 shows the analysis results.

[0163] (Polymerization Step 2) Synthesis of Chloroprene-Based Polymer Block (B-13)

[0164] After the polymerization step 1, when the internal temperature drops to 45°C, 4424 g of chloroprene monomer and 90.3 g of 1,9-nonanediol dimethacrylate are slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reaches 80%, a 10 wt% aqueous solution of the polymerization terminator N,N-diethylhydroxylamine is added to terminate the polymerization, and the unreacted chloroprene monomer is removed by vacuum distillation. 20 ml of the obtained latex is sampled to measure the physical properties, and the remaining latex is used to prepare an evaluation film. The average particle size of the latex, the mechanical stability of the latex, and the content (mass %) of the polymer block (A-13) of the chloroprene block copolymer and the chloroprene polymer block (B-13) are determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0165] (Comparative Example 1)

[0166] (Polymerization Step 1) Synthesis of Polymer Block (A-14)

[0167] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a jacket for heating and cooling. 3067 g of pure water, 147 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 23.9 g of potassium hydroxide, 12.3 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 230 g of styrene monomer, and 3.99 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 2.51 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. 20 ml of the obtained latex was sampled to measure the physical properties, and the remaining latex was used in the polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-14) were determined by analysis in the same manner as in Example 1. Table 1 shows the analysis results.

[0168] (Polymerization Step 2) Synthesis of Chloroprene-Based Polymer Block (B-14)

[0169] After the polymerization step 1, when the internal temperature drops to 45°C, 7278 g of chloroprene monomer and 148.5 g of 1,9-nonanediol dimethacrylate are slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reaches 80%, a 10 wt% aqueous solution of the polymerization terminator N,N-diethylhydroxylamine is added to terminate the polymerization, and the unreacted chloroprene monomer is removed by vacuum distillation. 20 ml of the obtained latex is sampled to measure the physical properties, and the remaining latex is used to prepare an evaluation film. The average particle size of the latex, the mechanical stability of the latex, and the content (mass %) of the polymer block (A-14) of the chloroprene block copolymer and the chloroprene polymer block (B-14) are determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0170] (Comparative Example 2)

[0171] (Polymerization Step 1) Synthesis of Polymer Block (A-15)

[0172] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a jacket for heating and cooling. 6667 g of pure water, 320 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 52.0 g of potassium hydroxide, 26.7 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 500 g of styrene monomer, and 4.27 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 2.69 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. 20 ml of the obtained latex was sampled to measure the physical properties, and the remaining latex was used in the polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-15) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0173] (Polymerization Step 2) Synthesis of Chloroprene-Based Polymer Block (B-15)

[0174] After the polymerization step 1, when the internal temperature drops to 45°C, 1607 g of chloroprene monomer and 32.8 g of 1,9-nonanediol dimethacrylate are slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reaches 80%, a 10 wt% aqueous solution of the polymerization terminator N,N-diethylhydroxylamine is added to terminate the polymerization, and the unreacted chloroprene monomer is removed by vacuum distillation. 20 ml of the obtained latex is sampled to measure the physical properties, and the remaining latex is used to prepare an evaluation film. The average particle size of the latex, the mechanical stability of the latex, and the content (mass %) of the polymer block (A-15) of the chloroprene block copolymer and the chloroprene polymer block (B-15) are determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0175] (Comparative Example 3)

[0176] Synthesis of copolymer containing only chloroprene polymer block (B-16)

[0177] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a heating and cooling jacket. 3600 g of pure water, 175 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 28.4 g of potassium hydroxide, 16.0 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 4000 g of chloroprene monomer, 81.6 g of 1,9-nonanediol dimethacrylate, and 4.72 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 45° C. and stirred at 200 rpm under a nitrogen stream. 2.96 g of 2,2′-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. When the polymerization rate of the chloroprene monomer reached 80%, a 10 wt% aqueous solution of a polymerization terminator N,N-diethylhydroxylamine was added to terminate the polymerization, and the unreacted chloroprene monomer was removed by vacuum distillation. 20 ml of the obtained latex was sampled for physical property measurement, and the remaining latex was used to prepare an evaluation film. The average particle size of the latex and the mechanical stability of the latex were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0178] (Comparative Example 4)

[0179] (Polymerization Step 1) Synthesis of Polymer Block (A-17)

[0180] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a heating and cooling jacket. 4616 g of pure water, 206 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 2.3 g of potassium hydroxide, 46.2 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 462 g of styrene monomer, and 9.2 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 6.0 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane]2-hydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. 20 ml of the obtained latex was sampled and measured for physical properties, and the remaining latex was used in the polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-17) were determined by analysis in the same manner as in Example 1. Table 1 shows the analysis results.

[0181] (Polymerization Step 2) Synthesis of Chloroprene-Based Polymer Block (B-17)

[0182] After the polymerization step 1, when the internal temperature drops to 45°C, 4154 g of chloroprene monomer is slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reaches 80%, a 10 wt% aqueous solution of the polymerization terminator N,N-diethylhydroxylamine is added to terminate the polymerization, and the unreacted chloroprene monomer is removed by vacuum distillation. 20 ml of the obtained latex is sampled to measure the physical properties, and the remaining latex is used to prepare an evaluation film. The average particle size of the latex, the mechanical stability of the latex, and the content (mass %) of the polymer block (A-17) and the chloroprene polymer block (B-17) of the chloroprene block copolymer are determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0183] (Comparative Example 5)

[0184] (Polymerization Step 1) Synthesis of Polymer Block (A-18)

[0185] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a heating and cooling jacket. 4616 g of pure water, 206 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 2.3 g of potassium hydroxide, 46.2 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 692 g of styrene monomer, and 9.2 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 6.0 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. 20 ml of the obtained latex was sampled and measured for physical properties, and the remaining latex was used in the polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-18) were determined by analysis in the same manner as in Example 1. Table 1 shows the analysis results.

[0186] (Polymerization Step 2) Synthesis of Chloroprene-Based Polymer Block (B-18)

[0187] After the polymerization step 1, when the internal temperature drops to 45°C, 3924 g of chloroprene monomer is slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reaches 80%, a 10 wt% aqueous solution of the polymerization terminator N,N-diethylhydroxylamine is added to terminate the polymerization, and the unreacted chloroprene monomer is removed by vacuum distillation. 20 ml of the obtained latex is sampled to measure the physical properties, and the remaining latex is used to prepare an evaluation film. The average particle size of the latex, the mechanical stability of the latex, and the content (mass %) of the polymer block (A-18) of the chloroprene block copolymer and the chloroprene polymer block (B-18) are determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0188] (Comparative Example 6)

[0189] Synthesis of triblock copolymers

[0190] (Synthesis of the first block)

[0191] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a heating and cooling jacket. 4613 g of pure water, 204.4 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 2.3 g of potassium hydroxide, 46.1 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 230 g of styrene monomer, and 9.2 g of benzyl-1-pyrrole dithiocarboate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 6.0 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane]2-hydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. 20 ml of the obtained latex was sampled to measure the physical properties, and the remaining latex was used in the subsequent polymerization step. The number average molecular weight, molecular weight distribution, and glass transition temperature of the first block were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 2.

[0192] (Synthesis of the Second Block)

[0193] After the synthesis of the first block, when the internal temperature dropped to 45°C, 4424 g of chloroprene monomer was added to carry out polymerization. When the polymerization rate of the chloroprene monomer reached 80%, a 10 wt % aqueous solution of a polymerization terminator N,N-diethylhydroxylamine was added to terminate the polymerization, and unreacted chloroprene monomer was removed by reduced pressure distillation. The obtained latex was used in the subsequent polymerization step.

[0194] (Synthesis of the third block)

[0195] After the synthesis of the second block, the internal temperature was raised to 80°C, 230 g of styrene monomer was added, and 6.0 g of 2,2'-azobis[2-(2-imidazoline-2-yl)propane]2-hydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate polymerization. After the polymerization, the polymerization was terminated by cooling to 25°C. 20 ml of the obtained latex was sampled to measure the physical properties, and the remaining latex was used to prepare an evaluation film. The average particle size of the latex, the mechanical stability of the latex, and the content (mass %) of the styrene blocks as the first block and the third block and the chloroprene block as the second block in the synthesized triblock copolymer were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 2.

[0196] (Comparative Example 7)

[0197] Production of a mixture of a homopolymer of a polymer block (A) and a homopolymer of a chloroprene-based polymer block (B)

[0198] (Synthesis of Homopolymer of Polymer Block (A))

[0199] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a jacket for heating and cooling. 4666 g of pure water, 224 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 36.4 g of potassium hydroxide, 18.7 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 350 g of styrene monomer, and 6.07 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 80° C. and stirred at 200 rpm under a nitrogen stream. 3.82 g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. When the polymerization rate of the styrene monomer reached 95%, a 10 wt% aqueous solution of a polymerization terminator N,N-diethylhydroxylamine was added to terminate the polymerization. 20 ml of the obtained latex was sampled and the physical properties were measured. The number average molecular weight, molecular weight distribution, and glass transition temperature of the homopolymer of the polymer block (A) were determined by analysis in the same manner as in Example 1. Table 3 shows the analysis results.

[0200] (Synthesis of Homopolymer of Chloroprene-Based Polymer Block (B))

[0201] The polymerization was carried out using an autoclave with a capacity of 10 L equipped with a stirrer and a heating and cooling jacket. 3960 g of pure water, 193 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 31.2 g of potassium hydroxide, 17.6 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N), 4400 g of chloroprene monomer, 89.8 g of 1,9-nonanediol dimethacrylate, and 5.19 g of butylbenzyl trithiocarbonate were added, and the internal temperature was set to 45° C. and stirred at 200 rpm under a nitrogen stream. 3.26 g of 2,2′-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: VA-044) was added as a polymerization initiator to initiate the polymerization. When the polymerization rate of the chloroprene monomer reached 80%, a 10 wt % aqueous solution of N,N-diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, and the unreacted chloroprene monomer was removed by distillation under reduced pressure.

[0202] (Mixture of homopolymer latex of polymer block (A) and homopolymer latex of chloroprene polymer block (B))

[0203] 4000 g of the homopolymer latex of the obtained polymer block (A) and 4000 g of the homopolymer latex of the chloroprene polymer block (B) were put into a 10 L autoclave equipped with a stirrer and a heating and cooling jacket, and the internal temperature was set to 45°C and stirred at 200 rpm. 20 ml of the obtained latex was sampled to measure the physical properties, and the remaining latex was used to prepare an evaluation film. The average particle size of the latex, the mechanical stability of the latex, and the content (mass %) of the homopolymer of the polymer block (A) and the homopolymer of the chloroprene polymer block (B) in the mixed polymer were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 3.

[0204] (Comparative Example 8)

[0205] Synthesis of Chloroprene Block Copolymer Latex by Forced Emulsification Method

[0206] (Polymerization Step 1) Synthesis of Polymer Block (A-19)

[0207] Use a 10L autoclave equipped with a stirrer and a heating and cooling jacket for polymerization. Add 4616g of tetrahydrofuran, 87.5g of styrene monomer, and 1.5g of benzylbutyl trithiocarbonate, set the internal temperature to 80°C, and stir at 200rpm under a nitrogen stream. Add 0.49g of azobisisobutyronitrile (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: AIBN) as a polymerization initiator to initiate the polymerization. Take a sample of 20ml from the resulting solution to measure the physical properties, and the remaining latex is used for subsequent polymerization steps. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-19) are determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 4.

[0208] (Polymerization Step 2) Synthesis of Chloroprene-Based Polymer Block (B-19)

[0209] After the polymerization step 1, when the internal temperature dropped to 45°C, 1120 g of chloroprene monomer and 22.8 g of 1,9-nonanediol dimethacrylate were slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reached 80%, a 10 wt % tetrahydrofuran solution of phenothiazine was added as a polymerization terminator to stop the polymerization, and the unreacted chloroprene monomer and tetrahydrofuran were removed by reduced pressure distillation to obtain a sample of a chloroprene block copolymer.

[0210] (Forced emulsification process)

[0211] Forced emulsification of chloroprene block copolymers

[0212] 350 g of the chloroprene block copolymer obtained in the polymerization step 2 was dissolved in 4200 g of benzene. 4725 g of pure water, 70 g of potassium disproportionate rosin acid (produced by Harima Chemicals), 0.78 g of potassium hydroxide, and 1.4 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (produced by Kao Corporation, trade name: Demol N) were added to the obtained solution, and forced emulsification was performed using a homogenizer. Benzene and water were removed by vacuum distillation in such a way that the solid content concentration of the obtained latex became 50%, thereby obtaining a chloroprene block copolymer latex. 20 ml of the obtained latex was sampled to measure the physical properties, and the remaining latex was used to prepare an evaluation film. The average particle size of the latex, the mechanical stability of the latex, and the content (mass %) of the polymer block (A-19) and the chloroprene polymer block (B-19) of the chloroprene block copolymer were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 4.

[0213] (Comparative Example 9)

[0214] Synthesis of triblock copolymer latex by forced emulsification method

[0215] (Synthesis of the first block)

[0216] Use a 10L autoclave with a stirrer and a heating and cooling jacket for polymerization. Add 4616g of tetrahydrofuran, 70g of styrene monomer, and 2.8g of benzyl-1-pyrrole dithiocarboxylate, set the internal temperature to 80°C, and stir at 200rpm under a nitrogen stream. Add 0.93g of azobisisobutyronitrile (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: AIBN) as a polymerization initiator to initiate the polymerization. Take a sample of 20ml from the resulting solution to measure the physical properties, and the remaining latex is used for subsequent polymerization steps. The number average molecular weight, molecular weight distribution, and glass transition temperature of the first block are determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 5.

[0217] (Synthesis of the Second Block)

[0218] After the polymerization step 1, when the internal temperature dropped to 45° C., 1346 g of chloroprene monomer was added to carry out polymerization. When the polymerization rate of the chloroprene monomer reached 80%, a 10 wt % tetrahydrofuran solution of phenothiazine was added as a polymerization terminator to stop the polymerization.

[0219] (Synthesis of the third block)

[0220] After the synthesis of the second block, the internal temperature was raised to 80°C, 70 g of styrene monomer was added, and 0.93 g of azobisisobutyronitrile (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: AIBN) was added as a polymerization initiator to initiate polymerization. After the polymerization, unreacted chloroprene monomer and tetrahydrofuran were removed by reduced pressure distillation to obtain a triblock copolymer.

[0221] (Forced Emulsification Step) Forced Emulsification of Triblock Copolymer

[0222] 350 g of the triblock copolymer obtained in the synthesis of the third block was dissolved in 4200 g of benzene. 4725 g of pure water, 70 g of potassium disproportionate rosin acid (manufactured by Harima Chemicals), 0.78 g of potassium hydroxide, and 1.4 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation, trade name: Demol N) were added to the obtained solution, and forced emulsification was performed using a homogenizer. Benzene and water were removed by vacuum distillation in such a way that the solid content concentration of the obtained latex became 50%, thereby obtaining a chloroprene block copolymer latex. 20 ml of the obtained latex was sampled to measure the physical properties, and the remaining latex was used to prepare an evaluation film. The average particle size of the latex, the mechanical stability of the latex, and the content (mass %) of the styrene block as the first block and the third block and the chloroprene block as the second block in the synthesized triblock copolymer were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 5.

[0223] [analyze]

[0224] (Determination of Number Average Molecular Weight and Molecular Weight Distribution of Polymer Block (A))

[0225] The molecular weight distribution of the number average molecular weight is a value in terms of polystyrene measured by gel permeation chromatography (GPC), and is a measured value under the following measurement conditions.

[0226] Device name: HLC-8320 (manufactured by Tosoh Corporation)

[0227] Column: 3 TSKgel GMHHR-H connected in series

[0228] Temperature: 40℃

[0229] Detection: Differential refractive index

[0230] Solvent: Tetrahydrofuran

[0231] Standard curve: drawn using standard polystyrene (PS).

[0232] (Glass transition temperature of polymer block (A))

[0233] The glass transition temperature was measured by the following method using a differential scanning calorimeter in accordance with JIS K 7121.

[0234] Device name: DSC1 (Mettler Toledo)

[0235] Steps: Heat to 120°C at a rate of 10°C / min under a nitrogen flow of 50 ml / min, maintain at 120°C for 10 minutes, then cool to -60°C, and then heat to 120°C at a rate of 10°C / min. According to the obtained DSC curve, the temperature of the intersection of the high-temperature side baseline extended to the straight line on the low-temperature side and the tangent drawn from the point with the largest gradient on the peak high-temperature side curve is taken as the glass transition temperature.

[0236] (Determination of Contents of Polymer Block (A) and Chloroprene Polymer Block (B) in Chloroprene Block Copolymer)

[0237] The measurement was performed by the following method using pyrolysis gas chromatography and 1H-NMR.

[0238] Pyrolysis gas chromatography device name: HP5890-II

[0239] Column: DB-5 0.25mmφ×30m (film thickness 1.0μm)

[0240] Column temperature: 50℃(5min)→10℃ / min→150℃→25℃ / min→300℃

[0241] Inlet temperature: 250℃

[0242] Detector temperature: 280°C

[0243] Detector: FID

[0244] 1H-NMR instrument name: JNM-ECX-400 (manufactured by JEOL Ltd.)

[0245] Steps: A chloroprene block copolymer composed of a polymer block (A) and a chloroprene polymer block (B) not containing a multifunctional monomer unit is measured by pyrolysis gas chromatography, and a standard curve is drawn based on the area ratio of the peak derived from the polymer block (A) to the peak derived from the chloroprene polymer block (B) and the content of the polymer block (A) and the chloroprene polymer block (B) in the chloroprene block copolymer obtained by measuring 1H-NMR. The sampled latex is mixed with methanol and the sample of the chloroprene block copolymer precipitated is measured by pyrolysis gas chromatography, and the content of the polymer block (A) and the chloroprene polymer block (B) in the chloroprene block copolymer is calculated using the above-drawn standard curve based on the area ratio of the peak derived from the polymer block (A) to the peak derived from the chloroprene polymer block (B).

[0246] (Measurement of average particle size of latex)

[0247] 0.1 g of the sampled latex was dissolved in 50 g of pure water to prepare a sample, and the sample was measured by a dynamic light scattering method using ELSZ-2 manufactured by Otsuka Electronics Co., Ltd., and the average particle size of the latex was calculated by a photon correlation method.

[0248] (Determination of mechanical stability of latex)

[0249] The mechanical stability of the latex was measured according to the following method using a MARON mechanical stability tester in accordance with JIS K 6392.

[0250] Steps: After filtering the sampled latex with a metal mesh to remove impurities, adjust the filtered latex to 20°C and weigh 50g in a test container. Install the test container in the testing machine and measure for 10 minutes under a load of 10kg. Filter the sample in the test container after the measurement with an 80-mesh metal mesh that has been dried at 125°C for 1 hour and cooled in a desiccant. After drying the 80-mesh metal mesh and the precipitate in a dryer at 125°C for 1 hour, cool in a desiccant, and weigh the 80-mesh metal mesh and the precipitate. In addition, calculate the total solid content of the sampled latex (unit: %) according to JIS K 6387. Then use the following formula to calculate the coagulation rate of the latex (unit: mass %).

[0251] [(weight of the 80-mesh metal mesh and the precipitate after drying (unit: g))-(weight of the 80-mesh metal mesh (unit: g))] / [50×((total solid content of latex (unit: mass %)) / 100)]×100

[0252] The obtained coagulation rate of the latex was defined as the mechanical stability of the latex. A mechanical stability of the latex of 1% by mass or less was considered to be an acceptable level.

[0253] [Preparation of samples for tensile test]

[0254] (Preparation of latex containing chloroprene block copolymer)

[0255] 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (trade name "NOCRAC PBK", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) as an antioxidant, 0.3 parts by mass of sodium lauryl sulfate (trade name "EMAR 10", manufactured by Kao Corporation) and water were added to 100 parts by mass (in terms of solid content) of the chloroprene block copolymer in the latex obtained in the polymerization step 2 to prepare a complex having a solid content concentration of 30% by mass, and the mixture was mixed at 20° C. for 16 hours using a ceramic ball mill.

[0256] (Film Production)

[0257] A ceramic cylinder with an outer diameter of 50 mm was immersed in a coagulation solution mixed with 62 parts by mass of water, 35 parts by mass of potassium nitrate tetrahydrate and 3 parts by mass of calcium carbonate for 1 second and then taken out. After drying for 4 minutes, it was immersed in the latex prepared above for 2 minutes. Thereafter, it was washed with running water at 45°C for 1 minute and heated at 130°C for 30 minutes to remove moisture, thereby preparing a film for tensile testing (140×150 mm, thickness: 0.2 mm).

[0258] [Evaluation of tensile properties]

[0259] The produced film was heat treated at 130°C for 30 minutes, and then the 500% elongation modulus, tensile strength at break, and elongation at break were measured according to JIS K 6251. A 500% elongation modulus of 3.0 MPa or less, a tensile strength at break of 17 MPa or more, and an elongation at break of 900% or more were considered acceptable levels.

[0260] [Evaluation of thermal aging characteristics]

[0261] The prepared film was subjected to a heat aging test in a forced cycle type heat aging tester at 100°C for 22 hours, and then the 500% elongation modulus, tensile strength at break and elongation at break were measured according to JIS K 6251. The film was considered acceptable if the 500% elongation modulus was 3.0 MPa or less, the tensile strength at break was 17 MPa or more, and the elongation at break was 900% or more.

[0262]

Table 1

[0263]

[0264]

[0265]

Table 2

[0266]

[0267]

Table 3

[0268]

[0269]

Table 4

[0270]

[0271]

Table 5

[0272]

[0273] In Examples 1 to 13, the mechanical stability of the latex is all below 1% by mass, and the mechanical stability of the latex is excellent. In addition, even without using a vulcanizing agent and a vulcanization accelerator, the 500% elongation modulus of the film is below 3.0 MPa, the flexibility is excellent, the tensile strength at break is above 17 MPa, the elongation at break is above 900%, and the tensile properties are excellent. In addition, the 500% elongation modulus after the heat aging test is below 3.0 MPa, the flexibility is excellent, the tensile strength at break is above 17 MPa, the elongation at break is above 900%, and the heat aging resistance is also excellent. On the other hand, in Comparative Examples 1 to 8, any of the physical properties of the mechanical stability of the latex, the softness of the film, the tensile properties, and the heat aging resistance are not good.

[0274] Industrial Applicability

[0275] The dip-molded article obtained from the chloroprene block copolymer latex of the present invention has excellent flexibility, tensile properties, and heat aging resistance, and can be applied to surgical gloves, gloves, balloons, catheters, etc. In addition, the chloroprene block copolymer latex of the present invention can be applied to coatings, adhesives, and the like.

Claims

1. A chloroprene block copolymer latex, comprising a chloroprene block copolymer, wherein the chloroprene block copolymer comprises: 5 to 10% by mass of a polymer block (A) derived from a monomer which, when homopolymerized, yields a polymer having a glass transition temperature of 80° C. or higher; and The chloroprene-based polymer block (B) containing chloroprene monomer units is 85 to 95% by mass, The number average molecular weight of the polymer block (A) is 10,000 or more, The film obtained by dip-molding the chloroprene block copolymer latex is heat-treated at 130° C. for 30 minutes, and the tensile strength at break measured according to JIS K 6251 is 17 MPa or more, and the elongation at break is 900% or more.

2. The chloroprene block copolymer latex according to claim 1, wherein The average particle size of the chloroprene block copolymer latex measured by dynamic light scattering method is less than 300 nm.

3. The chloroprene block copolymer latex according to claim 1 or 2, wherein The chloroprene polymer block (B) comprises a chloroprene monomer unit and a polyfunctional monomer unit. The chloroprene block copolymer latex according to claim 1 or 2, which is used for impregnation of a molded article.