A method for evaluating the sensitivity of oil well pipe to hydrogen sulfide stress corrosion

Through slow tensile test and fracture morphology observation, combined with step crack plane parameter analysis, the complexity and inaccuracy of the anti-stress corrosion detection of oil well pipes in the existing technology are solved, and fast and accurate stress corrosion performance is achieved Evaluation and guide the selection and equipment maintenance of oil well pipe materials.

CN115356199BActive Publication Date: 2024-12-03ANGANG STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210908043.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-29
Publication Date
2024-12-03
Estimated Expiration
2042-07-29

AI Technical Summary

Technical Problem

The existing test conditions for the anti-hydrogen sulfide stress corrosion of oil well pipes have harsh test conditions, long cycles, and the results can only provide information on failure and failure. It is impossible to accurately evaluate the resistance to hydrogen sulfide stress corrosion of the material, and the fracture morphology is complicated. Stress corrosion sensitivity cannot be accurately evaluated.

Method used

The slow tensile test is used to combine fracture morphology observation and step crack plane parameter analysis. By measuring the step crack area and shape, the stress corrosion sensitivity index is calculated, providing a fast and accurate evaluation method, shortening the test cycle and improving detection efficiency.

Benefits of technology

Quantitative evaluation of the stress corrosion resistance of hydrogen sulfide of oil well pipe materials is achieved, which can accurately reflect the actual stress corrosion resistance of the material, guide material selection and equipment maintenance, and reduce the test cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115356199B_ABST
    Figure CN115356199B_ABST
Patent Text Reader

Abstract

The present invention provides an evaluation method for the hydrogen sulfide stress corrosion sensitivity of oil well pipes, comprising: processing the sample into a set size and pre-treating the surface thereof; installing the sample on a stretching device in a reactor, adding an appropriate amount of test solution into the reactor, and sealing the reactor; adjusting the hydrogen sulfide concentration in the test solution, and rapidly stretching and pre-loading the sample to 50% to 80% of the yield strength value; starting a slow tensile loading test at a set strain rate after stabilization until the sample is broken, and recording the test results; taking out the broken tensile sample, observing the fracture morphology, and selecting the area of ​​the step crack plane with the largest area on the fracture to evaluate the stress corrosion resistance of the oil well pipe material. The step crack parameters on the fracture are used to accurately analyze the slow tensile test results, so as to achieve the purpose of quantitatively analyzing the stress corrosion resistance sensitivity of the oil well pipe material, shorten the test cycle, and improve the detection efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of corrosion testing, and in particular to a method for evaluating the sensitivity of oil well pipes to hydrogen sulfide stress corrosion. Background Art

[0002] In recent years, with the exploration and development of ultra-deep, ultra-high temperature, ultra-high corrosion and harsh environment oil and gas wells, the working environment of oil and gas wells generally has the characteristics of "high temperature, high pressure, high CO2, high H2S, high Cl-, and high mineralization". These complex and harsh working conditions, coupled with special operating processes, lead to stress corrosion cracking failure of oil well pipes, which seriously affects the normal production and operation of oil and gas fields. In particular, in the process of exploration and exploitation of sulfur-containing oil and gas resources, the oil well pipes used are prone to hydrogen sulfide stress corrosion cracking, which is a low-stress brittle fracture with fast crack propagation speed and sudden fracture. It has the highest risk factor and is prone to cause major accidents and casualties.

[0003] In view of the above situation, relevant standards have been formulated at home and abroad to reduce the risks brought by hydrogen sulfide stress corrosion cracking (SSCC), and strict testing and evaluation of oil well pipe resistance to SSCC have been carried out. NACE Standard TM0177-2005 "Indoor test of metal resistance to sulfide stress corrosion cracking and stress corrosion cracking in H2S environment" and GB / T4157-2006 "Laboratory test of metal resistance to special forms of environmental cracking in hydrogen sulfide environment" both stipulate the standard tensile test (method A), and determine its resistance to hydrogen sulfide stress corrosion by the fracture time within the test cycle. Products that do not fracture for more than 720 hours are qualified, and products that fracture within 720 hours are unqualified. The test results can only provide failure and non-failure information. Similarly, the four-point bending loading test in the ASTM G39-99 standard is also a common method for evaluating the stress corrosion resistance of oil well pipes. Using the A method standard solution, products that do not break within 720 hours are qualified, and products that break within 720 hours are unqualified. A 10x magnifying glass is used to observe whether there are cracks on the surface of the unbroken sample. The test results can only give failure and non-failure information. The above methods have harsh test conditions, long test cycles, and the test results can only give failure and non-failure information. For non-failed samples, it is impossible to evaluate their hydrogen sulfide stress corrosion resistance performance level. It is necessary to combine other experimental methods for comprehensive evaluation, which prolongs the test cycle and increases the test cost.

[0004] Therefore, it is necessary to find a new method that can quickly and accurately evaluate the hydrogen sulfide stress corrosion resistance of oil well pipe materials, shorten the test cycle, and reduce the test cost. The slow rate tensile test has been widely used by researchers because it is fast, accurate, highly reproducible, and obtains a lot of parameter information. It is currently one of the more mature and advanced standard methods for studying stress corrosion. When evaluating the hydrogen sulfide stress corrosion resistance of oil well pipes by slow tensile tests, fracture morphology and stress corrosion cracking sensitivity index are usually used for evaluation. If the fracture morphology is a brittle fracture feature, or the stress corrosion cracking sensitivity index is greater than a certain value (generally 25%), it is generally believed that the oil well pipe material has stress corrosion cracking sensitivity in the corresponding research system.

[0005] However, in the actual test process, it is often found that the fracture morphology is ductile fracture or mixed fracture mechanism, and the stress corrosion sensitivity index calculated by using the elongation after fracture, the shrinkage after fracture and the yield strength loss ratio is less than 25%. It is often believed that the material does not have stress corrosion sensitivity, but a step-shaped crack platform appears near the circumference of the fracture, indicating that the material actually has obvious stress corrosion sensitivity, which is inconsistent with the test results. In addition, even if the two materials have the same stress corrosion sensitivity index, the actual stress corrosion resistance is quite different, especially the step cracks perpendicular to the tensile direction in the fracture morphology, which are distributed along the circumferential direction, and their size and number are significantly different, which is not conducive to accurately evaluating the material's resistance to hydrogen sulfide stress corrosion.

[0006] Based on the above content, in order to accurately and quickly evaluate the hydrogen sulfide stress corrosion resistance of oil well pipe materials, the present invention is specially proposed. Summary of the invention

[0007] In order to overcome the shortcomings of the background technology, the present invention provides an evaluation method for the hydrogen sulfide stress corrosion resistance of oil well pipes, which can quickly and accurately evaluate the hydrogen sulfide stress corrosion resistance of oil well pipe materials, and use the step crack plane parameters on the fracture to accurately analyze the slow tensile test results, so as to achieve the purpose of quantitatively evaluating the stress corrosion resistance sensitivity of oil well pipe materials, shorten the test cycle, and improve the detection efficiency.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] A method for evaluating the sensitivity of oil well pipe to hydrogen sulfide stress corrosion, comprising the following steps:

[0010] Step 1: Process the sample into a set size and pre-treat its surface;

[0011] Step 2: Install the sample on the stretching device in the reactor, add an appropriate amount of test solution into the reactor, and seal the reactor;

[0012] Step 3: Adjust the concentration of hydrogen sulfide in the test solution and quickly stretch and preload the sample to 50% to 80% of the yield strength value;

[0013] Step 4: After stabilization, start the slow tensile loading test at the set strain rate until the sample is broken and record the test results;

[0014] Step 5: Finally, take out the broken tensile specimen, remove the corrosion products on the specimen surface and the fracture, observe the fracture morphology, and select the area of ​​the step crack plane with the largest area on the fracture to evaluate the stress corrosion resistance of the oil well pipe material.

[0015] Furthermore, the strain rate of the slow tensile loading test is 1×10 -7 ~5×10 -5 mm / s.

[0016] Furthermore, the strain rate of the rapid stretching is greater than or equal to 1×10 -4 mm / s.

[0017] Furthermore, the step 5 of evaluating the stress corrosion resistance of the oil well pipe material specifically includes the following:

[0018] 1) The crack propagation direction is along the step crack plane, extending from the outer surface of the specimen along the radius to the center and along the circumferential direction at the same time;

[0019] 2) The fracture morphology is observed using a laser confocal microscope with a magnification of 20-100. The fracture surface is uneven and a step crack appears in the circumferential direction. At the same time, the distance between the workbench and the lens is adjusted to ensure that the fracture morphology of the sample is clear and the step crack area is accurately measured;

[0020] 3) The step crack plane with the largest area on the fracture is selected to measure the step crack area;

[0021] 4) The step crack area is calculated by selecting the vertical projection area;

[0022] 5) The plane shape of the step crack is an ellipse, and the stress corrosion resistance is related to the maximum vertical projection area S of the step crack. The formula of its stress corrosion sensitivity R is simplified to R=K*r / b*S, where b is the minor axis length of the ellipse, that is, the radial crack extension depth, r is the radius of the slow tensile specimen test area, and K is a constant.

[0023] Furthermore, the slow tensile loading test is loaded along the length direction of the sample, and the tensile direction is parallel to the length direction of the sample.

[0024] Furthermore, the stretching direction of the slow tensile loading test is perpendicular to the step crack plane, and the stretching direction is perpendicular to the crack propagation direction, with a difference of 90°.

[0025] Furthermore, the test solution is Nace standard A solution, and the hydrogen sulfide concentration is 0 to 3500 ppm.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The present invention tests the stress corrosion resistance of oil well pipe materials in a service environment or a simulated actual environment, evaluates the stress corrosion resistance sensitivity of the oil well pipe materials by observing the fracture morphology and the area of ​​the step crack plane, and further evaluates the practicability of the oil well pipe materials in a specific working environment, thereby guiding material selection and equipment maintenance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a vertical projection diagram of the fracture sample of the embodiment of the present invention when the hydrogen sulfide concentration is zero.

[0029] Figure 2 This is a macroscopic three-dimensional morphology diagram of a fracture sample of an embodiment of the present invention when the hydrogen sulfide concentration is zero;

[0030] Figure 3 This is a vertical projection diagram of a fracture sample when the hydrogen sulfide concentration is 1000 ppm according to an embodiment of the present invention;

[0031] Figure 4 This is a macroscopic three-dimensional morphology diagram of a fracture sample when the hydrogen sulfide concentration is 1000 ppm according to an embodiment of the present invention;

[0032] Figure 5 This is a vertical projection diagram of a fracture sample when the hydrogen sulfide concentration is 3500 ppm according to an embodiment of the present invention;

[0033] Figure 6 This is a macroscopic three-dimensional morphology diagram of a fracture sample when the hydrogen sulfide concentration of an embodiment of the present invention is 3500ppm;

[0034] Figure 7 Graph showing the radial width b of the step crack plane and the elliptical vertical projection area S of an embodiment of the present invention. DETAILED DESCRIPTION

[0035] The specific implementation modes provided by the present invention are described in detail below with reference to the accompanying drawings.

[0036] A method for evaluating the sensitivity of oil well pipe to hydrogen sulfide stress corrosion, comprising the following steps:

[0037] Step 1: Process the sample into a set size and pre-treat its surface;

[0038] Step 2: Install the sample on the stretching device in the reactor, add an appropriate amount of test solution into the reactor, and seal the reactor; the test solution is Nace standard A solution, and the hydrogen sulfide concentration is 0 to 3500 ppm.

[0039] Step 3: Adjust the concentration of hydrogen sulfide in the test solution, and quickly stretch the preloaded sample to 50% to 80% of the yield strength value; the strain rate of the rapid stretching is greater than or equal to 1×10 -4 mm / s.

[0040] Step 4: After stabilization, start the slow tensile loading test at the set strain rate until the sample is broken, and record the test results; the strain rate of the slow tensile loading test is 1×10 -7 ~5×10 -5 mm / s.

[0041] Step 5: Finally, take out the broken tensile specimen, remove the corrosion products on the specimen surface and the fracture, observe the fracture morphology, and select the area of ​​the step crack plane with the largest area on the fracture to evaluate the stress corrosion resistance of the oil well pipe material.

[0042] The details include:

[0043] 1) The crack propagation direction is along the step crack plane, extending from the outer surface of the specimen along the radius to the center and along the circumferential direction at the same time;

[0044] 2) The fracture morphology is observed using a laser confocal microscope with a magnification of 20-100. The fracture surface is uneven and a step crack appears in the circumferential direction. At the same time, the distance between the workbench and the lens is adjusted to ensure that the fracture morphology of the sample is clear and the step crack area is accurately measured;

[0045] 3) The step crack plane with the largest area on the fracture is selected to measure the step crack area;

[0046] 4) The step crack area is calculated by selecting the vertical projection area;

[0047] 5) If Figure 7 As shown, the plane shape of the step crack is an ellipse, and the stress corrosion resistance is related to the maximum vertical projection area S of the step crack. The formula of its stress corrosion sensitivity R is simplified to R=K*r / b*S, where b is the minor axis length of the ellipse, that is, the radial crack extension depth, r is the radius of the slow tensile specimen test area, and K is a constant.

[0048] The fracture morphology is observed using a microscope with a magnification of 20-100. When the step crack is small, a larger magnification is used, and when the step crack is large, a smaller magnification is used to ensure that the fracture morphology of the sample is fully presented and the step crack area is accurately measured.

[0049] The slow tensile loading test is loaded along the length direction of the sample, and the tensile direction is parallel to the length direction of the sample. The tensile direction of the slow tensile loading test is perpendicular to the step crack plane, and the tensile direction is perpendicular to the crack extension direction, with a difference of 90°.

[0050] Example 1

[0051] The test material is 110 grade sulfur-resistant oil well pipe with a yield strength of 800 MPa. The method consists of Ⅰ sample processing, Ⅱ surface treatment, Ⅲ slow tensile loading test and Ⅳ fracture morphology observation and step crack area measurement.

[0052] The specimen processing in step I is to process the test material into a suitable cylindrical tensile specimen with a length of 72 mm, a test area diameter of 6.40 mm, and a surface finish of 0.3 μm;

[0053] The surface treatment in step II is to use ultrasonic cleaning to clean the sample in step I in acetone and anhydrous ethanol respectively, so as to remove the residue and grease on the surface of the sample;

[0054] The slow tensile loading test in step III is carried out using a slow strain rate tensile testing machine. The test temperature is room temperature. Nace standard A solution is injected into the reactor, the reactor is closed, and high-purity nitrogen is introduced for deoxygenation for 2 hours. The hydrogen sulfide concentration in the solution is 0. The sample is pre-loaded to 600Mpa and the sample is kept in the elastic stress deformation stage. Then, the sample is subjected to 5*10 -6 The slow tensile loading test was started at a strain rate of mm / s. After the test, the test results were recorded, the broken tensile specimens were taken out, and the corrosion products on the surface and fracture of the specimens were removed to ensure that the surface of the specimens presented a metallic luster and the fracture morphology was clear;

[0055] The fracture morphology observation and step crack area measurement in step IV were performed using a laser confocal microscope. The broken tensile specimen was placed vertically on the stage, with the tensile direction perpendicular to the stage plane. The distance between the fracture specimen and the lens was appropriately adjusted. The magnification was 100 times. The fracture morphology was photographed after clear focus. Figure 1-2 The fracture is cup-cone shaped, which is a ductile fracture. No stress corrosion occurs. The step crack area S is recorded as 0. Substituting into the stress corrosion sensitivity formula R=3r / b*S, the test results are shown in Table 1.

[0056] Example 2

[0057] The test material is 110 grade sulfur-resistant oil well pipe with a yield strength of 800 MPa. The method consists of Ⅰ sample processing, Ⅱ surface treatment, Ⅲ slow tensile loading test and Ⅳ fracture morphology observation and step crack area measurement.

[0058] The specimen processing in step I is to process the test material into a suitable cylindrical tensile specimen with a length of 72 mm, a test area diameter of 6.40 mm, and a surface finish of 0.3 μm;

[0059] The surface treatment in step II is to use ultrasonic cleaning to clean the sample in step I in acetone and anhydrous ethanol respectively, so as to remove the residue and grease on the surface of the sample;

[0060] The slow tensile loading test in step III is carried out using a slow strain rate tensile testing machine. The Nace standard A solution is injected into the reactor, and high-purity nitrogen is introduced for deoxygenation for 2 hours. An appropriate amount of analytical pure sodium sulfide is added. After sufficient reaction, the hydrogen sulfide concentration in the solution is ensured to be 1000ppm. The reactor is closed, and the sample is pre-loaded to 600Mpa to keep the sample in the elastic stress deformation stage. Then, the sample is subjected to 5*10 -6 The slow tensile loading test was started at a strain rate of mm / s. After the test, the test results were recorded, the broken tensile specimens were taken out, and the corrosion products on the surface and fracture of the specimens were removed to ensure that the surface of the specimens presented a metallic luster and the fracture morphology was clear;

[0061] The fracture morphology observation and step crack area measurement in step IV were performed using a laser confocal microscope. The broken tensile specimen was placed vertically on the stage, with the tensile direction perpendicular to the stage plane. The distance between the fracture specimen and the lens was appropriately adjusted. The magnification was 100 times. The fracture morphology was photographed after clear focus. Figure 3-4 , select the largest step crack plane, and calculate the radial width b and elliptical vertical projection area S (mm) of the step crack plane through the supporting software 2 ), put into the stress corrosion sensitivity formula R = 3r / b*S, the test results are shown in Table 1.

[0062] Example 3

[0063] The test material is 110 grade sulfur-resistant oil well pipe with a yield strength of 800 MPa. The method consists of Ⅰ sample processing, Ⅱ surface treatment, Ⅲ slow tensile loading test and Ⅳ fracture morphology observation and step crack area measurement.

[0064] The specimen processing in step I is to process the test material into a suitable cylindrical tensile specimen with a length of 72 mm, a test area diameter of 6.40 mm, and a surface finish of 0.3 μm;

[0065] The surface treatment in step II is to use ultrasonic cleaning to clean the sample in step I in acetone and anhydrous ethanol respectively, so as to remove the residue and grease on the surface of the sample;

[0066] The slow tensile loading test in step III is carried out using a slow strain rate tensile testing machine. The test temperature is room temperature. Nace standard A solution is injected into the reactor, the reactor is closed, high-purity nitrogen is introduced for deoxygenation for 2 hours, and then high-purity hydrogen sulfide gas (99.99%) is introduced until the solution is saturated. The concentration of hydrogen sulfide in the solution is 3500ppm at room temperature and atmospheric pressure. The sample is pre-loaded to 600Mpa to keep the sample in the elastic stress deformation stage. Then, the sample is subjected to 5*10 -6 The slow tensile loading test was started at a strain rate of mm / s. After the test, the test results were recorded, the broken tensile specimens were taken out, and the corrosion products on the surface and fracture of the specimens were removed to ensure that the surface of the specimens presented a metallic luster and the fracture morphology was clear;

[0067] The fracture morphology observation and step crack area measurement in step IV were performed using a laser confocal microscope. The broken tensile specimen was placed vertically on the stage, with the stretching direction perpendicular to the stage plane. The distance between the fracture and the lens was appropriately adjusted. The magnification was 100 times, and the fracture morphology was photographed after clear focus. Figure 5-6 , select the largest step crack plane, and calculate the radial width b and elliptical vertical projection area S (mm) of the step crack plane through the supporting software 2 ), put into the stress corrosion sensitivity formula R = 3r / b*S, the test results are shown in Table 1.

[0068] Table 1 Slow tensile test results of oil well pipes at different hydrogen sulfide concentrations

[0069]

[0070]

[0071] From the above test results, it can be seen that in Nace standard A solution, when the hydrogen sulfide concentration is zero, the oil well pipe material does not suffer from stress corrosion, the fracture is cup-cone shaped, which is a ductile fracture, and the stress corrosion sensitivity index is 0. With the increase of hydrogen sulfide concentration, the stress corrosion sensitivity index of the oil well pipe material increases from 56.75 to 86.37, and the fracture morphology shows step cracks, which has obvious stress corrosion characteristics, which is similar to the conventional stress corrosion sensitivity calculation results, such as elongation loss ratio and fracture time loss ratio. This method realizes the measurement of the hydrogen sulfide stress corrosion sensitivity index of the oil well pipe, and through the observation of the fracture morphology and the calculation of the step crack area, the stress corrosion resistance of the oil well pipe material is more accurately and comprehensively evaluated.

[0072] Example 4

[0073] The samples used in the test are two types of sulfur-resistant oil well pipes, A and B, and the two oil well pipes are two different oil well pipes (for example, oil well pipes with different materials or different rolling, heat treatment and other processes, the explanations here in the following embodiments are the same). The method consists of I sample processing, II surface treatment, III slow tensile loading test and IV fracture morphology observation and step crack area measurement.

[0074] The specimen processing in step I is to process the test material into a suitable cylindrical tensile specimen with a length of 72 mm, a test area diameter of 6.40 mm, and a surface finish of 0.3 μm;

[0075] The surface treatment in step II is to use ultrasonic cleaning to clean the sample in step I in acetone and anhydrous ethanol respectively, so as to remove the residue and grease on the surface of the sample;

[0076] The slow tensile loading test in step III is carried out using a slow strain rate tensile testing machine. The test temperature is room temperature. Nace standard A solution is injected into the reactor. The reactor is sealed and firstly high-purity nitrogen is introduced for deoxygenation for 2 hours. Then high-purity hydrogen sulfide gas (99.99%) is introduced until the solution is saturated. The concentration of hydrogen sulfide in the solution is 3500ppm at room temperature and atmospheric pressure. Then, the concentration of hydrogen sulfide in the solution is 1*10 -7 The slow tensile loading test was started at a strain rate of mm / s. After the test, the test results were recorded, the broken tensile specimens were taken out, and the corrosion products on the surface and fracture of the specimens were removed to ensure that the surface of the specimens presented a metallic luster and the fracture morphology was clear;

[0077] The fracture morphology observation and step crack area measurement in step IV were carried out using a laser confocal microscope. The broken tensile specimen was placed vertically on the stage, with the stretching direction perpendicular to the stage plane. The distance between the fracture and the lens was appropriately adjusted. The magnification was 80 times. After the fracture morphology was focused clearly, the largest step crack plane was selected. The radial width b and the elliptical vertical projection area S (mm) of the step crack plane were calculated using the supporting software. 2 ), substitute the stress corrosion sensitivity formula R=3r / b*S, and the test results are shown in Table 2. Analysis shows that the order of stress corrosion sensitivity from high to low is: B>A.

[0078] Table 2 Slow tensile test results of oil well pipe

[0079]

[0080] Example 5

[0081] The samples used in the test are two types of sulfur-resistant oil well pipes, A and B, and the two oil well pipes are two different oil well pipes (for example, oil well pipes with different materials or different rolling, heat treatment and other processes, the explanations here in the following embodiments are the same). The method consists of I sample processing, II surface treatment, III slow tensile loading test and IV fracture morphology observation and step crack area measurement.

[0082] The specimen processing in step I is to process the test material into a suitable cylindrical tensile specimen with a length of 72 mm, a test area diameter of 6.40 mm, and a surface finish of 0.3 μm;

[0083] The surface treatment in step II is to use ultrasonic cleaning to clean the sample in step I in acetone and anhydrous ethanol respectively, so as to remove the residue and grease on the surface of the sample;

[0084] The slow tensile loading test in step III is carried out using a slow strain rate tensile testing machine. Nace standard A solution is injected into the reactor, high-purity nitrogen is introduced for deoxygenation for 2 hours, and an appropriate amount of analytical pure sodium sulfide is added. After sufficient reaction, the hydrogen sulfide concentration in the solution is ensured to be 1000ppm. The reactor is then closed and then heated for 5*10 -5 The slow tensile loading test was started at a strain rate of mm / s. After the test, the test results were recorded, the broken tensile specimens were taken out, and the corrosion products on the surface and fracture of the specimens were removed to ensure that the surface of the specimens presented a metallic luster and the fracture morphology was clear;

[0085] The fracture morphology observation and step crack area measurement in step IV were carried out using a laser confocal microscope. The broken tensile specimen was placed vertically on the stage, with the stretching direction perpendicular to the stage plane. The distance between the fracture and the lens was appropriately adjusted. The magnification was 80 times. After the fracture morphology was focused clearly, the largest step crack plane was selected. The radial width b and the elliptical vertical projection area S (mm) of the step crack plane were calculated using the supporting software. 2 ), substitute the stress corrosion sensitivity formula R=3r / b*S, and the test results are shown in Table 3. Analysis shows that the order of stress corrosion sensitivity from high to low is: B>A.

[0086] Table 3 Slow tensile test results of oil well pipe

[0087]

[0088] The above embodiments are implemented based on the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the above embodiments. The methods used in the above embodiments are conventional methods unless otherwise specified.

Claims

1. A method for evaluating the sensitivity of oil well pipe to hydrogen sulfide stress corrosion, characterized in that: The steps include: Step 1: Process the sample into a set size and pre-treat its surface; Step 2: Install the sample on the tensile device in the reactor, add the test solution into the reactor, and seal the reactor; Step 3: Adjust the concentration of hydrogen sulfide in the test solution and quickly stretch and preload the specimen to 50%~80% of the yield strength value; Step 4: After stabilization, start the slow tensile loading test at the set strain rate until the sample is broken and record the test results; Step 5: Finally, take out the broken tensile specimen, remove the corrosion products on the specimen surface and the fracture, observe the fracture morphology, and select the step crack plane with the largest area on the fracture to evaluate the stress corrosion resistance of the oil well pipe material; The step 5 of evaluating the stress corrosion resistance of the oil well pipe material specifically includes the following steps: 1) The crack propagation direction is along the step crack plane, extending from the outer surface of the specimen along the radius to the center and along the circumferential direction at the same time; 2) The fracture morphology is observed using a laser confocal microscope with a magnification of 20-100. The fracture surface is uneven and presents a step crack plane in the circumferential direction. At the same time, the distance between the workbench and the lens is adjusted to ensure that the fracture morphology of the sample is clear and the step crack area is accurately measured; 3) The step crack plane is selected to measure the step crack with the largest area on the fracture surface; 4) The step crack area is calculated by selecting the vertical projection area; 5) The plane shape of the step crack is an ellipse, and the stress corrosion resistance is related to the maximum vertical projection area S of the step crack. The formula of its stress corrosion sensitivity R is simplified to R=K*r / b*S, where b is the minor axis length of the ellipse, that is, the radial crack extension depth, in mm, r is the radius of the slow tensile specimen test area, in mm, K is 3; S is in mm 2 ; The slow tensile loading test is performed in a direction parallel to the length of the sample. The tensile direction of the slow tensile loading test is perpendicular to the step crack plane, and the tensile direction is perpendicular to the crack propagation direction, with a difference of 90°.

2. The method for evaluating the sensitivity of oil well pipe to hydrogen sulfide stress corrosion according to claim 1, characterized in that: The strain rate of the slow tensile loading test is 1×10 -7 ~ 5×10 -5 mm / s.

3. The method for evaluating the sensitivity of oil well pipe to hydrogen sulfide stress corrosion according to claim 1, characterized in that: The strain rate of the rapid stretching is greater than or equal to 1×10 -4 mm / s.